Organometallic compounds and their purification methods
Organometallic compounds are used for depositing high-purity tin oxide films with high conformality and etch selectivity, addressing the challenges of immersion lithography by enhancing semiconductor device performance and yield through CVD and ALD processes combined with multi-stage distillation.
Patent Information
- Application Number
- JP2022194698
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-08-02
- Filing Date
- 2022-12-06
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2038-07-31
AI Technical Summary
The semiconductor industry faces challenges in maintaining high-density, high-yield semiconductor device performance due to the need for transparent resist protective layers that can withstand immersion lithography processes without chemical damage and ensure adequate etch selectivity and conformality, while conventional resist compositions are not suitable for immersion lithography.
The use of organometallic compounds for the deposition of high-purity tin oxide films through chemical vapor deposition (CVD) and atomic layer deposition (ALD) at low temperatures, which exhibit high conformality, etch selectivity, and optical transparency, along with multi-stage distillation for purification to achieve ultra-high purity.
The resulting tin oxide films provide improved hermetic properties, reduced metallic impurities, and enhanced device performance with low defect density, high device density, and improved yield, meeting stringent industry requirements.
Smart Images

Figure 0007577104000002 
Figure 0007577104000003 
Figure 0007577104000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to organometallic compounds useful for the deposition of high purity tin oxide and the purification of such organometallic compounds. [Background technology]
[0002] The semiconductor industry continues to produce components with increasingly smaller geometries. The production of such semiconductor devices presents new design and manufacturing challenges to maintain or improve semiconductor device performance. There are also challenges in producing semiconductor interconnect stacks that provide high density, high yield, good signal integrity, and adequate power delivery.
[0003] Lithography is a major pattern transfer technology and is widely used in the fabrication of various electronic devices containing fine structures, such as semiconductor devices and liquid crystal devices. As device structures become smaller, the masking patterns used in the lithography process also need to be optimized for precise pattern transfer to the underlying layers.
[0004] Multiple patterning lithography refers to a variety of techniques developed for photolithography to increase the structural density of semiconductor devices. Double patterning, a type of multiple patterning, uses multiple masks and photolithography steps to produce semiconductor devices at a certain level. Double patterning changes the relationship between semiconductor device wiring parameters and the quality of the wiring to maintain performance, with benefits such as reduced spacing and smaller diameter wiring.
[0005] Recently, immersion lithography methods have been proposed to address some of the problems in the industry.
[0006] By adopting immersion lithography, resist patterns with improved resolution and depth of focus can be formed at low cost using lenses installed in existing exposure systems, which has led to immersion lithography attracting a great deal of attention.
[0007] With the move to immersion lithography and multi-patterning, a new class of conformally deposited materials is needed to build up on top of photoresist, BARC, and other traditional masking layers. These new conformally deposited layers can accomplish two main functions: 1) It can act as a transparent protective layer (or "mask") to prevent chemical attack by immersion lithography fluids. In this case, the conformal layer must be transparent so that it can be applied to the lithography process without adverse patterning and exposure problems. 2) It has a higher etch selectivity than conventional films such as prior art and amorphous carbon, which become less transparent with increasing thickness. For example, a multi-patterning process may require a thicker (>10,000A) and therefore less transparent amorphous carbon layer to provide sufficient etch protection. A metal oxide conformal film can remain transparent while maintaining the necessary etch selectivity during the plasma etch process to provide similar etch resistance.
[0008] Objectives such as smoothness, etching and deposition characteristics, 100% step coverage / conformity requirements, and other requirements dictate that the reactive gases used in these processes be of high purity to achieve stable chemical structures.
[0009] The films must also be made with high purity because they are used as resist protection layers during etching or litho immersion processing. Impurities in the films can undergo harmful chemical or optical reactions that can lead to pattern degradation or adversely affect the critical dimensions of device features, reducing the performance of the integrated devices.
[0010] Conventional resist compositions are not necessarily usable in immersion lithography processes for various reasons. For example, in immersion lithography processes, the resist film is in direct contact with a refractive index liquid (immersion liquid) during exposure, and the resist film is susceptible to chemical damage by this liquid. Resist compositions suitable for use in immersion lithography processes must also be transparent to the exposure light. Furthermore, even if conventional resist compositions are effective in lithography in which exposure is performed through an air layer, in immersion lithography, sufficient resolution of the pattern may not be achieved because the characteristics change depending on the liquid.
[0011] Therefore, there remains a need for improved transparent resist protection layers that can meet increasingly stringent industry requirements. Furthermore, as outlined, more selective ALD films are required for multi-patterning. Summary of the Invention
[0012] Disclosed herein are compounds useful for the deposition of high purity tin oxide films that exhibit high conformality, high etch selectivity, high hardness and elastic modulus, and are optically transparent.
[0013] The compounds include those of Formula I below: R x -Sn-A 4-x Formula I During the ceremony, A is selected from the group consisting of (YaR'z) and 3- to 7-membered nitrogen-containing heterocyclic groups; each R group is independently selected from the group consisting of alkyl or aryl groups having 1 to 10 carbon atoms; each R' group is independently selected from the group consisting of alkyl, acyl, or aryl groups having 1 to 10 carbon atoms; x is an integer from 0 to 4; a is an integer from 0 to 1, Y is selected from the group consisting of N, O, S, and P; z is 1 when Y is O or S or is absent, and is 2 when Y is N or P.
[0014] The compounds of formula I enable low temperature chemical vapor deposition (CVD) and atomic layer deposition (ALD) of tin oxide to produce films of high purity tin oxide that are low in metallic impurities, have high hardness and elastic modulus, and provide greater than 99% step coverage (i.e., high conformality) to device structures and topography.
[0015] Further disclosed is the purification of the compound of formula I by multi-stage distillation. This purification results in a so-called "ultra-pure" compound, which has a significantly lower concentration of metallic impurities compared to compounds purified by conventional means. The use of the ultra-pure compounds in the processes disclosed herein produces membranes with improved properties compared to those known in the prior art. For example, these membranes have improved sealing properties, reduced metallic impurities, and improved yield loss and long-term reliability problems due to such metallic impurities. Multi-stage distillation may be performed by packaged multiple columns, staged distillation columns using multiple trays, multiple distillation columns, or other types of multi-stage distillation formats.
[0016] The tin oxide films produced in this way exhibit high etch selectivity compared to conventional masking conformal layers used in multi-layer patterning integration techniques, thereby enabling thinner film requirements to be met compared to conventional films such as amorphous carbon, boron-doped carbon, etc.
[0017] In one embodiment, in the organometallic compound of formula I, A is selected from the group consisting of a (NR'2) group and a 3- to 7-membered nitrogen-containing heterocyclic group. In one embodiment, A is a (NR'2) group. In one embodiment, A is a 3- to 7-membered nitrogen-containing heterocyclic group. In one embodiment, A is a pyrrolidinyl group. In one embodiment, A is a 3- to 7-membered nitrogen-containing heterocyclic group. 4-x is (NMe2)2 or (NEtMe)2.
[0018] In another embodiment, the R and R' groups are independently selected alkyl groups having 1 to 10 carbon atoms. It is contemplated that each R and R' group may be an independently selected alkyl group having 1 to 6 carbon atoms. In some embodiments, each R and R' group is an independently selected alkyl group having 1 to 4 carbon atoms. In some embodiments, R and R' are independently selected from the group consisting of methyl, ethyl, propyl, isopropyl, tert-butyl, isobutyl, and n-butyl. In some embodiments, R and R' represent different alkyl groups.
[0019] In one embodiment, the compound of formula I is selected from the group consisting of Me2Sn(NMe2)2, Me2Sn(NEtMe)2, t-BuSn(NEtMe)3, i-PrSn(NEtMe)3, n-Pr(NEtMe)3, EtSN(NEtMe)3, i-BuSn(NEtMe)3, Et2Sn(NEtMe)2, Me2Sn(NEtMe)2, Sn(NEtMe)4, Bu2Sn(NEtMe)2, Et2Sn(NMe2)2, Me2Sn(NEt2)2, Sn(pyrrolidinyl)4, and Bu2Sn(pyrrolidinyl)2.
[0020] In some embodiments, the compound of formula I is selected from the group consisting of Me2Sn(NMe2)2, Me2Sn(NEtMe)2, Et2Sn(NMe2)2, Me2Sn(NEt2)2, Sn(pyrrolidinyl)4, and Bu2Sn(pyrrolidinyl)2.
[0021] In some embodiments, the compound of formula I is selected from the group consisting of Me2Sn(NEtMe)2 and Me2Sn(NMe2)2.
[0022] In some embodiments, the compound of formula I is Me2Sn(NMe2)2.
[0023] In some embodiments, a composition is provided that includes an organometallic compound that is any of the compounds disclosed above and another organometallic compound that contains Sn. The other organometallic compound can be a compound of formula I.
[0024] In various embodiments, the further organometallic compound is selected from the group consisting of MeSn(NMe2)3 and Sn(NMe2)4.
[0025] In one embodiment, a method for purifying organometallic compounds using multi-stage distillation is disclosed. In one embodiment, 2 to 20 stages are required to reduce metal contamination to less than 1 ppm. In one embodiment, 2 to 20 stages are required to reduce metal contamination to less than 100 ppb. In one embodiment, 2 to 20 stages are required to reduce metal contamination to less than 10 ppb. In one embodiment, 2 to 20 stages are required to reduce metal contamination to 1 ppb or less.
[0026] The foregoing and other features and advantages of the present invention will become more apparent in the light of the following detailed description of the preferred embodiment, as illustrated in the accompanying drawings. As will be understood, the present invention is capable of modification in various respects without departing from the invention. Accordingly, the drawings and description are to be regarded as illustrative in nature and not restrictive. [Brief description of the drawings]
[0027] FIG. 1 shows the NMR spectrum of Me3SnNMe2.
[0028] FIG. 2 shows the NMR spectrum of Sn(NMe2)4.
[0029] FIG. 3 shows the NMR spectrum of Me2Sn(NEtMe)2.
[0030] FIG. 4 shows the NMR spectrum of Bu2Sn(NMe2)2.
[0031] FIG. 5 shows the NMR spectrum of Me2SnEt2.
[0032] FIG. 6 shows the NMR spectrum of Me4Sn.
[0033] FIG. 7 shows the NMR spectrum of Bu2Sn(OMe)2.
[0034] FIG. 8 shows the NMR spectrum of Bu2Sn(OAc)2.
[0035] FIG. 9 shows the NMR spectrum of Et2Sn(NMe2)2.
[0036] FIG. 10 shows the NMR spectrum of Me2Sn(NEt2)2.
[0037] FIG. 11 shows the NMR spectrum of Sn(pyrrolodinyl)4.
[0038] FIG. 12 shows the NMR spectrum of Bu2Sn(pyrrolodinyl)2.
[0039] FIG. 13 shows the NMR spectrum of Et2Sn(pyrrolodinyl)2.
[0040] FIG. 14 shows the NMR spectrum of Me2Sn(NMe2)2.
[0041] FIG. 15 shows the NMR spectrum of tBuSn(NMe2)3.
[0042] FIG. 16 shows the NMR of the reaction of (NMe2)4Sn with ethanol.
[0043] FIG. 17 shows the NMR of the reaction of Me3SnNMe2 with water.
[0044] FIG. 18 shows the NMR of the reaction of Bu2Sn(OAc)2 with methanol.
[0045] FIG. 19 shows the NMR of the reaction of Bu2Sn(OMe)2 with acetic acid.
[0046] FIG. 20 shows the NMR of the reaction of Bu2Sn(NMe2)2 with methanol.
[0047] FIG. 21 shows the NMR of Me4Sn before and after heating at 200° C.
[0048] FIG. 22 shows the NMR of Et2Sn(NMe2)2 before and after heating at 200 °C.
[0049] FIG. 23 shows the NMR of Me2Sn(NMe2)2 before and after heating at 150 °C.
[0050] FIG. 24 shows the decomposition temperatures of exemplary compounds of Formula I.
[0051] FIG. 25 shows a schematic diagram of a multi-stage distillation apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0052] Organometallic compounds of Formula I are disclosed: R x -Sn-A 4-x Formula I During the ceremony, A is (Y a R' z ) and 3- to 7-membered nitrogen-containing heterocyclic groups; each R group is independently selected from the group consisting of alkyl or aryl groups having 1 to 10 carbon atoms; each R' group is independently selected from the group consisting of alkyl, acyl, or aryl groups having 1 to 10 carbon atoms; x is an integer from 0 to 4; a is an integer from 0 to 1, Y is selected from the group consisting of N, O, S, and P; z is 1 when Y is O or S or is absent, and is 2 when Y is N or P.
[0053] Compounds of formula I include those in which R is selected from the group consisting of alkyl and aryl groups having 1 to 10 carbon atoms. Particular compounds are those in which R is selected from the group consisting of alkyl and aryl groups having 1 to 6 carbon atoms. More particular are those in which R is selected from the group consisting of alkyl and aryl groups having 1 to 4 carbon atoms. Examples of such compounds include those in which R is a methyl, ethyl, or butyl group.
[0054] Compounds of formula I include those in which R' is selected from the group consisting of alkyl, acyl, and aryl groups having 1 to 10 carbon atoms. Particular compounds are those in which R' is selected from the group consisting of alkyl, acyl, and aryl groups having 1 to 6 carbon atoms. More particular are those in which R' is selected from the group consisting of alkyl, acyl, and aryl groups having 1 to 4 carbon atoms. Examples of such compounds include those in which R' is a methyl, ethyl, or acetyl group.
[0055] Compounds of formula I include those where Y is selected from the group consisting of N, O, S, and P. Particular compounds are those where Y is selected from the group consisting of N and O.
[0056] Compounds of formula I include those where x is an integer from 0 to 4. In certain embodiments, x is an integer from 1 to 3. More preferably, x is 2.
[0057] Compounds of formula I include those where A is a 3- to 7-membered nitrogen-containing heterocyclic group such as aziridinyl, pyrrolidinyl, and piperidinyl. Particular compounds are those where A is a pyrrolidinyl or piperidinyl group.
[0058] Compounds of formula I include those in which R is an alkyl group and A is an NR' group and R' is an alkyl group. Particular compounds are those in which R and R' represent different alkyl groups.
[0059] Compounds of formula I exhibit good reactivity and also good thermal stability. Thus, the compounds can be fed into the deposition chamber without decomposition, which would result in non-uniform deposited films. The excellent stability and reactivity profile of the compounds of the present invention also means that less material can be fed into the growth chamber (less material is more economical) and shorter cycle times can be achieved (because less material remains in the chamber and is pumped out at the end of the process). Thus, thicker films can be deposited in less time, thus increasing throughput. Furthermore, ALD can be carried out at much lower temperatures (or over a wider temperature range) using compounds of formula I than in the art processes. Thermal stability also means that the materials are much easier to purify and handle after synthesis.
[0060] Such compounds are useful for sealing and protecting resist layers used in immersion lithography (i.e., functioning as a "mask"). Thus, the compounds disclosed herein can be used to protect underlying layers during immersion lithography in the production of transparent tin oxide films that have suitable properties for deposition over photoresist or other organic masking layers. This allows the production of devices with improved semiconductor device performance for industry requirements such as low defect density, improved device reliability, high device density, high yield, good signal integrity, adequate power supply, etc.
[0061] Additionally, the use of compounds of formula I in the methods disclosed herein enables low temperature chemical vapor deposition (CVD) and atomic layer deposition (ALD) of tin oxide to produce films of high purity tin oxide with low metallic impurities and greater than 99% step coverage (i.e., high conformality) to device features and topography.
[0062] Compounds of formula I can be prepared by processes known in the art. The following examples are illustrative of such processes but are not intended to be limiting. Example 1: Me 3 Sn(NMe 2 Synthesis of
[0063] 20 mL of 2.5 M butyllithium in hexane and 50 mL of anhydrous hexane were charged into a 250 mL flask. Me2NH gas was bubbled through the solution until the reaction proceeded sufficiently, and the reaction mixture was stirred for 2 hours. A solution of 10 g of Me3SnCl in 100 mL of anhydrous hexane was added to this, and the mixture was stirred for 12 hours. Filtration was performed to remove the solids. The solvent was removed under reduced pressure. The resulting liquid product was purified by distillation under reduced pressure. The product was identified as Me3SnNMe2 by NMR, as shown in Figure 1. Example 2: Sn(NMe 2 ) 4 Synthesis of
[0064] A 250 mL flask was charged with 80 mL of 2.5 M butyllithium in hexane and 50 mL of anhydrous hexane. Me2NH gas was passed through the solution until the reaction proceeded sufficiently, and the reaction mixture was stirred for 2 hours. To this was added a solution of 13 g of SnCl4 in 100 mL of anhydrous benzene, and the mixture was stirred for 4 hours. After cooling, filtration was performed to remove the solids. The solvent was removed under reduced pressure. The resulting liquid product was purified by distillation under reduced pressure. The product was identified as Sn(NMe2)4 by NMR, as shown in Figure 2. Example 3: Me 2 Sn(NEtMe) 2 Synthesis of
[0065] Under inert atmosphere, 25.00 mL of 2.5 M butyllithium in hexane and 200 mL of anhydrous hexane were charged to a 1 L round bottom flask, followed by slow addition of 5.40 mL of HNEtMe in 100 mL of anhydrous hexane. The reaction mixture was stirred at room temperature for 1 hour. A solution of 6.70 g of Me2SnCl2 in 200 mL of anhydrous benzene was added to the flask (cooled in an ice bath) and the reaction mixture was stirred at room temperature overnight. The solvent was removed from the filtrate under reduced pressure. The resulting liquid product was concentrated under reduced pressure (80 °C, 9.8 × 10 -2 The product was identified as Me2Sn(NEtMe)2 by NMR spectroscopy, as shown in Figure 3. 1) nBuLi + HNEtMe → LiNEtMe + butane Equation II 2)Me2SnCl2+2LiNEtMe→Me2Sn(NEtMe)2+2LiCl Formula III Example 4: Bu 2 Sn(NMe 2 ) 2 Synthesis of
[0066] 24 mL of 2.5 M butyllithium in hexane and 100 mL of anhydrous hexane were charged to a 250 mL flask. Me2NH gas was bubbled through the solution until the reaction proceeded sufficiently, and the reaction mixture was stirred for 2 hours. To this was added a solution of 9.11 g of Bu2SnCl2 in 100 mL of anhydrous benzene, and the mixture was stirred for 4 hours. Filtration was performed to remove the solids. The solvent was removed under reduced pressure. The resulting liquid product was purified by distillation under reduced pressure. The product was identified as Bu2Sn(NMe2)2 by NMR, as shown in Figure 4. Example 5: Me 2 SnEt 2 Synthesis of
[0067] 6.59 g of Me2SnCl2 was dissolved in 100 mL of anhydrous ether and 30 mL of 3M EtMgBr was added under N2. After stirring for 4 h, the mixture was treated with 0.1 M HCl solution and the organic layer was collected. The collected organic layer was further treated with saturated NaHCO3 solution and the organic layer was collected. Distillation was performed under N2 to remove the ether. Purification was performed by distillation under reduced pressure. The product was confirmed as Me2SnEt2 by NMR as shown in Figure 5. Example 6: Me 4 Synthesis of Sn
[0068] To a solution of 23.5 g SnCl4 in ether was added 150 mL of 3 M MeMgI under N2. After stirring for 4 h, the mixture was treated with 0.1 M HCl solution and the organic layer was collected. The collected organic layer was further treated with saturated NaHCO3 solution and the organic layer was collected. Fractional distillation was performed to remove the ether. Purification was performed by distillation under reduced pressure. NMR confirmed the product as Me4Sn, as shown in Figure 6. Example 7: Bu 2 Sn(OMe) 2 Synthesis of
[0069] 20 g of Bu2SnCl2 and 20 mL of anhydrous methanol were charged in a 250 mL flask, followed by 7 g of sodium methoxide dissolved in 30 mL of anhydrous methanol. The mixture was refluxed for 12 hours. Filtration was performed to remove the solids. The solvent was removed under reduced pressure. The resulting liquid product was purified by distillation under reduced pressure. The product was identified as Bu2Sn(OMe)2 by NMR, as shown in Figure 7. Example 8: Bu 2 Sn(OAc) 2 Synthesis of
[0070] First, sodium acetate was generated by adding 6 g of acetic acid to a solution of 5.4 g of sodium methoxide in 30 mL of anhydrous methanol. This was then added to a mixture of 30 g of Bu2SnCl2 in 30 mL of anhydrous methanol. The resulting mixture was refluxed for 4 hours. Filtration was performed to remove the solids. The solvent was removed under reduced pressure. The resulting liquid product was purified by distillation under reduced pressure. The product was identified as Bu2Sn(OAc)2 by NMR as shown in Figure 8. Example 9: Et 2 Sn(NMe 2 ) 2 Synthesis of
[0071] 22 mL of 2.5 M butyllithium in hexane and 400 mL of anhydrous hexane were charged into a 1 L flask. Me2NH gas was bubbled through the resulting solution and the reaction mixture was stirred for 1 h. To this was added a solution of 6.71 g of Et2SnCl2 in 100 mL of anhydrous benzene and the mixture was stirred for 4 h. Filtration was performed to remove the solid product. The solvent was removed from the resulting filtrate under reduced pressure. The resulting liquid product was purified by distillation under reduced pressure. The product was identified as Et2Sn(NMe2)2 by NMR as shown in Figure 9. Example 10: Me 2 Sn(NEt 2 ) 2 Synthesis of
[0072] 24 mL of 2.5 M butyllithium in hexane and 50 mL of anhydrous hexane were charged to a 250 mL flask, followed by the addition of 4.39 g of Et2NH. The reaction mixture was stirred for 2 hours. To this was added a solution of 6.59 g of Me2SnCl2 in 100 mL of anhydrous ether, and the mixture was stirred for 4 hours. Filtration was performed to remove the solids. The solvent was removed under reduced pressure. The resulting liquid product was purified by distillation under reduced pressure. The product was identified as Me2Sn(NEt2)2 by NMR, as shown in Figure 10. Example 11: Sn(pyrrolidinyl) 4 Synthesis of
[0073] Under an inert atmosphere, 0.5 mL of Sn(NMe2)4 and 25 mL of anhydrous hexane were charged to a 100 mL round bottom flask, followed by the dropwise addition of 1.1 mL of pyrrolidine. The reaction mixture was stirred at room temperature for 2 hours, after which the solvent was removed by distillation under reduced pressure. The residue in the reaction flask was identified as Sn(pyrrolodinyl)4 by NMR spectroscopy, as shown in Figure 11. Example 12: Bu 2 Sn(pyrrolodinyl) 2 Synthesis of
[0074] Under inert atmosphere, 25 mL of 2.5 M butyllithium in hexane and 200 mL of anhydrous hexane were charged to a 1 L round bottom flask, followed by slow addition of 5.3 mL of pyrrolidine in 25 mL of anhydrous hexane. The reaction mixture was stirred at room temperature for 1 hour and then placed in an ice bath. A solution of 9.46 g of Bu2SnCl2 in 50 mL of anhydrous hexane was added to the flask and the reaction mixture was stirred at room temperature for 2 hours. Filtration was performed to remove the solid product. The solvent was removed from the resulting filtrate under reduced pressure. The product was identified as Bu2Sn(pyrrolodinyl)2 by NMR spectroscopy, as shown in Figure 12. Example 13: Et 2 Sn(pyrrolodinyl) 2 Synthesis of
[0075] Under an inert atmosphere, 5.3 mL of pyrrolidine and 200 mL of anhydrous pentane were charged into a 1 L round bottom flask. The reaction flask was once placed in an ice bath and 25 mL of 2.5 M butyllithium in hexane was slowly added to the reaction flask with vigorous stirring. The reaction mixture was stirred at room temperature for 1 hour and again placed in an ice bath. A solution of 7.7 g of Et2SnCl2 in 100 mL of anhydrous pentane and 20 mL of anhydrous benzene were added to the flask and the reaction mixture was stirred at room temperature overnight. Filtration was performed to remove the solid product. The solvent was removed from the resulting filtrate under reduced pressure. The final product was purified by vacuum distillation. The product was identified as Et2Sn(pyrrolodinyl)2 by NMR spectroscopy as shown in Figure 13. Example 14: Me 2 Sn(NMe 2 ) 2 Synthesis of
[0076] Under an inert atmosphere, 25 mL of 2.5 M butyllithium in hexane and 400 mL of anhydrous hexane were charged to a 1 L flask. The reaction flask was placed in an ice bath and Me2NH gas was passed through the solution until a white sherbet-like solution was obtained (approximately 15 min). The reaction mixture was then stirred at room temperature for 1 h. The reaction flask was again placed in an ice bath and a solution of 6.7 g Me2SnCl2 in 100 mL of anhydrous benzene was slowly added and the mixture was stirred at room temperature overnight. Filtration was performed to remove the solid product. The solvent was removed from the resulting filtrate under reduced pressure. The resulting liquid product was purified by distillation under reduced pressure. The product was identified as Me2Sn(NMe2)2 by NMR spectroscopy as shown in Figure 14. Example 15: tBuSn(NMe 2 ) 3 Synthesis of
[0077] Sn(NMe2)4+tBuLi→tBuSn(NMe2)3+LiNMe2 Equation IV
[0078] Under inert atmosphere, 100 mL of Sn(NMe2)4 and approximately 3 L of anhydrous hexane were charged to a 5 L round bottom flask. The mixture was stirred by mechanical stirrer and placed in an ethylene glycol bath at -15 °C. In a glove box, 200 mL of 1.7 M tert-butyllithium solution in anhydrous hexane and approximately 200 mL of anhydrous hexane were charged to a 1 L flask. The tBuLi solution was slowly added to the reaction flask. The resulting reaction mixture was stirred at room temperature for 3 hours. After that, the stirring was stopped and the salt was allowed to precipitate from the reaction mixture overnight. The liquid was cannulated into another 5 L round bottom flask. The resulting solvent was removed by distillation and 62 g of the final product was obtained by elution under reduced pressure (120 °C, 6.2 × 10 -2 The product was isolated by distillation at 1000 rpm (1000 Torr). The product was confirmed as tBuSn(NMe2)3 by NMR spectroscopy, as shown in Figure 15. It was 90% tBuSn(NMe2)3 and 10% tBu2Sn(NMe2)2.
[0079] Similarly, complexes of type RSn(NEtMe)3 can be synthesized by reacting Sn(NEtMe)4 with RLi (where R = Et, iPr, iBu, nPr) following the procedure described above. Sn(NEtMe)4+RLi→RSn(NEtMe)3+LiNEtMe Formula V where R = Et, iPr, iBu, nPr Example 16: Sn(NEtMe) 4 +EtLi→EtSn(NEtMe) 3 +LiNEtMe
[0080] Under inert atmosphere, 100 g of Sn(NEtMe)4 and approximately 2.5 L of anhydrous hexane were charged in a 5 L round bottom flask. The mixture was stirred by mechanical stirrer and placed in an ethylene glycol bath at -15°C. In a glove box, 655 mL of 0.5 M ethyllithium solution in anhydrous benzene and approximately 200 mL of anhydrous benzene were charged in a 1 L flask. The EtLi solution was slowly added to the reaction flask. The resulting reaction mixture was stirred at room temperature for 3 hours. After that, the stirring was stopped and the salt was allowed to precipitate from the reaction mixture overnight. The liquid was cannulated into another 5 L round bottom flask. The resulting solvent was removed by distillation and the final product was isolated by distillation under reduced pressure. Example 17: Sn(NEtMe) 4 +iPrLi → iPrSn(NEtMe) 3 +LiNEtMe
[0081] Under inert atmosphere, 100 g of Sn(NEtMe)4 and approximately 2.5 L of anhydrous hexane were charged in a 5 L round bottom flask. The mixture was stirred by mechanical stirrer and placed in an ethylene glycol bath at -15°C. In a glove box, 468 mL of 0.7 M isopropyl lithium solution in anhydrous pentane and approximately 200 mL of anhydrous hexane were charged in a 1 L flask. The iPrLi solution was slowly added to the reaction flask. The resulting reaction mixture was stirred at room temperature for 3 hours. After that, the stirring was stopped and the salt was allowed to precipitate from the reaction mixture overnight. The liquid was cannulated into another 5 L round bottom flask. The resulting solvent was removed by distillation and the final product was isolated by distillation under reduced pressure. Example 18: Sn(NEtMe) 4 +iBuLi→iBuSn(NEtMe) 3 +LiNEtMe
[0082] Under inert atmosphere, 100 g of Sn(NEtMe)4 and approximately 3 L of anhydrous hexane were charged in a 5 L round bottom flask. The mixture was stirred by mechanical stirrer and placed in an ethylene glycol bath at -15°C. In a glove box, 193 mL of 1.7 M isobutyllithium solution in anhydrous heptane and approximately 200 mL of anhydrous hexane were charged in a 1 L flask. The iBuLi solution was slowly added to the reaction flask. The resulting reaction mixture was stirred at room temperature for 3 hours. After that, the stirring was stopped and the salt was allowed to precipitate from the reaction mixture overnight. The liquid was cannulated into another 5 L round bottom flask. The resulting solvent was removed by distillation and the final product was isolated by distillation under reduced pressure. Example 19: Sn(NEtMe) 4 +nPrLi→nPrSn(NEtMe) 3 +LiNEtMe
[0083] Under inert atmosphere, 100 g of Sn(NEtMe)4 and approximately 3 L of anhydrous hexane were charged in a 5 L round bottom flask. The mixture was stirred by mechanical stirrer and placed in an ethylene glycol bath at -15°C. In a glove box, 193 mL of 1.7 M n-propyl lithium solution in anhydrous heptane and approximately 200 mL of anhydrous hexane were charged in a 1 L flask. The nPrLi solution was added slowly to the reaction flask. The resulting reaction mixture was stirred at room temperature for 3 hours. After that, the stirring was stopped and the salt was allowed to precipitate from the reaction mixture overnight. The liquid was cannulated into another 5 L round bottom flask. The resulting solvent was removed by distillation and the final product was isolated by distillation under reduced pressure. Example 20: Comparative reactivity test
[0084] a) Water was added to Sn(NMe2)4. The reaction occurred spontaneously. The clear Sn(NMe2)4 became cloudy and a white solid was formed. Absolute ethanol was added to Sn(NMe2)4. The mixture was heated and NMR confirmed that the -NMe2 groups were completely replaced by -OEt groups. More ethanol was added and NMR further confirmed that the reaction was complete (Figure 16).
[0085] b) Water was added to Me3SnNMe2. NMR did not show any reaction occurring. The mixture was heated at 50°C for 1 hour. NMR showed that a reaction occurred (Figure 17). Anhydrous methanol was added to Me3SnNMe2. NMR did not indicate any reaction had occurred. The mixture was heated at 50°C for 1 hour. The clear solution became cloudy. NMR confirmed that a reaction had occurred.
[0086] c) Water was added to Bu2Sn(OAc)2. The reaction was spontaneous. The clear Bu2Sn(OAc)2 became cloudy and a white solid was formed. Anhydrous methanol was added to ·Bu2Sn(OAc)2. NMR did not indicate any reaction occurred (Figure 18).
[0087] d) Water was added to Bu2Sn(OMe)2. The reaction was spontaneous. The clear Bu2Sn(OMe)2 became cloudy and a white solid was formed. Acetic acid was added to ·Bu2Sn(OMe)2. NMR showed that some of the -OMe groups were replaced by -OAc groups (Figure 19).
[0088] e) Water was added to Bu2Sn(NMe2)2. The reaction occurred spontaneously. The clear Bu2Sn(NMe2)2 became cloudy and a white solid was formed. Methanol was added to ·Bu2Sn(NMe2)2. NMR showed that some of the -NMe2 groups were replaced by -OMe groups (Figure 20). Example 21: Thermal stability test
[0089] Thermal stability testing of the compound of formula I was performed in a closed glass ampoule heated at a set temperature for 1 hour. NMR was performed to determine whether any thermal decomposition occurred. Additionally, visual inspection was performed to determine whether solids formed after heat treatment. Figure 21 shows the NMR of Me4Sn before and after heating at 200°C. Both NMR and visual inspection confirmed no significant changes after heating at 200°C for 1 hour.
[0090] Figure 22 shows the NMR of Et2Sn(NMe2)2 before and after heating at 200° C. Both NMR and visual observation confirmed no significant changes after heating at 200° C. for 1 hour.
[0091] Figure 23 shows the NMR of Me2Sn(NMe2)2 before and after heating at 150° C. Both NMR and visual observation confirmed no significant changes after heating at 150° C. for 24 hours.
[0092] FIG. 24 shows the decomposition temperatures of exemplary compounds of Formula I.
[0093] These results demonstrate that the compounds of formula I are thermally stable, demonstrating that the compounds can be delivered to the deposition chamber without observable decomposition. Multi-Stage Distillation
[0094] Various multi-stage distillations are known in the chemical manufacturing industry, but have not previously been used to purify organometallic materials, including tetramethyltin or other compounds of formula I.
[0095] Multiple effect or multi-stage distillation (MED) is a distillation process often used to desalinate seawater, as shown in the schematic diagram in Figure 25. The process consists of several stages or "effects". (In the schematic diagram in Figure 25, the first stage is shown at the top. The pink areas are steam, the light blue areas are liquid feed, and the turquoise areas are condensate. How the feed enters the stages other than the first is not shown, but is easily understood. F is the feed inlet, S is the heating steam inlet, C is the heating steam outlet, W is the purified material (condensate) outlet, R is the waste material outlet, O is the coolant inlet, P is the coolant outlet, and VC is the cooling section of the last stage.) In each stage, the feed is heated by steam in the tubes. Some of the feed is evaporated, and this steam flows into the tubes of the next stage to further heat and evaporate the distillate. Each stage essentially reuses the energy from the previous stage.
[0096] The plant can be viewed as a series of closed volumes separated by the walls of tubes, each with a heat source at one end and a heat sink at the other. Each volume has two communicating subspaces: the outside of the nth tube and the inside of the n+1th tube. Each volume has a lower temperature and pressure than the previous volume, and the tube walls are at a temperature intermediate between the temperatures of the fluids on either side of it. The pressure in each volume cannot equilibrate with the temperatures of the walls of both subspaces, and so has an intermediate pressure. As a result, the first subspace has a lower pressure or higher temperature, and the feed material evaporates. The second subspace has a higher pressure or lower temperature, and the vapor condenses. This causes the energy of evaporation to flow from the warm first subspace to the cold second subspace, where energy flows by conduction through the tube walls to the next colder volume.
[0097] As shown in Table 1 below, purification of SnMe4 by multi-stage distillation results in a compound with significantly lower levels of impurities than that purified by conventional means. [Table 1]
[0098] In the context of this description (particularly in the context of the claims which follow), the use of the singular form "a," "an," "an," or "the" is to be construed as covering both the singular and the plural, unless otherwise specified herein or clearly contradicted by context. The terms "comprising," "having," "including," and "containing" are to be construed as open-ended terms (i.e., meaning "including but not limited to"), unless otherwise specified. The term "connected" is to be construed as partly or wholly contained within, attached to, or connected to, with or without intervening material.
[0099] References to numerical ranges recited herein are merely intended to serve as a shorthand method of referring individually to each individual value within that range, unless otherwise stated herein, and each individual value is incorporated herein as if it were individually referred to herein.
[0100] All methods described herein may be performed in any suitable order unless otherwise specified herein or clearly contradicted by context. The use of any and all examples or exemplary language (e.g., "etc.") provided herein is intended only to better illustrate embodiments of the present invention and does not impose limitations on the scope of the present invention unless otherwise claimed. Various embodiments and components may be interchanged or combined as appropriate.
[0101] No language in the specification should be construed as indicating any non-claimed element essential to the practice of the invention.
[0102] It will be apparent to those skilled in the art that various modifications and variations can be made to the present invention without departing from the spirit and scope of the present invention. It is not intended to limit the present invention to the specific forms disclosed, but rather, the present invention is intended to cover all modifications, alternative constructions, and equivalents that are within the spirit and scope of the present invention as defined in the appended claims. Therefore, it is intended that the present invention cover the modifications and variations of the present invention provided they come within the scope of the appended claims and their equivalents.
Claims
1. 1. A method for purifying an organometallic compound, comprising the steps of: A) In the first stage distillation of organometallic compounds The organometallic compound is Me 3 Sn(NMe 2 ), Sn(NMe 2 ) 4、 Me 2 Sn(NEtMe) 2、 B 2 Sn(NMe 2 ) 2, Et 2 Sn(NMe 2 ) 2、 Me 2 Sn(NEt 2 ) 2、 Sn(pyrrolidinyl) 4、 B 2 Sn (pyrrolodinyl) 2、 Et 2 Sn (pyrrolodinyl) 2、 Me 2 Sn(NMe 2 ) 2、 tBuSn(NMe 2 ) 3 is selected from the group consisting of In the first stage distillation, i) feeding a feed material comprising a first organometallic compound to a first distillation space under a first reduced pressure; ii) heating the first distillation space to a first temperature to vaporize a portion of the feed material; iii) removing a vaporized portion of the feed from the first distillation space to form a distillate; B) distilling the distillate from the previous stage in at least one other stage subsequent to the first stage, i) feeding distillate from a previous stage to a distillation space subsequent to the first distillation space under a reduced pressure subsequent to the first reduced pressure; ii) heating a distillation space subsequent to the first distillation space to a temperature subsequent to the first temperature to vaporize a portion of the distillate from the previous stage; iii) removing the evaporated portion of the distillate from the previous stage from the distillation space subsequent to the first distillation space to form a distillate subsequent to the distillate formed in the first stage; C) removing a final distillate from the last stage subsequent to the first stage, A method for purifying an organometallic compound, comprising repeating step B a sufficient number of times to obtain an organometallic compound in a final distillate having a high purity.
2. In each step after the first step, the distillation space has a lower pressure than the preceding stage, and / or 2. The method for purifying organometallic compounds according to claim 1, wherein the temperature of each of the distillation spaces is lower than the temperature of the preceding space.
3. In each stage, the distillation space is heated by steam in the tubes; 2. The method of claim 1, wherein in each stage after the first stage, the vapor in the tubes is a vaporized portion of the feed or a distillate from the previous stage of the respective stage.
4. 2. The method of claim 1, wherein step B is repeated a sufficient number of times to reduce metal contamination to less than 1 ppm.
Citation Information
Patent Citations
CZ00218093B6
Preparation of alkyl-tin compounds
GB871730A
JP1973005571B
Production of tin alkoxide
JP1986205289A
Dialkyltin alkoxide
JP2005298433A