Liquid crystal polyester fiber and its manufacturing method
By employing specific metal elements as catalysts in solid-phase polymerization, the liquid crystal polyester fibers achieve enhanced mechanical properties and heat aging resistance through low-temperature and short-time heat treatment, addressing the limitations of conventional catalysts.
Patent Information
- Application Number
- JP2022565239
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-25
- Filing Date
- 2021-11-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-11-15
AI Technical Summary
Existing liquid crystal polyester fibers face challenges in achieving high mechanical properties and heat aging resistance due to the thermal decomposition of conventional polymerization catalysts during melt spinning and the promotion of side reactions, which reduce strength and flexibility.
The use of specific metal elements from Groups 8 to 11 of the periodic table, such as copper, cobalt, and palladium, as catalysts in solid-phase polymerization to promote desired reactions while suppressing side reactions, allowing for low-temperature and short-time heat treatment.
The resulting liquid crystal polyester fibers exhibit excellent mechanical properties and heat aging resistance, with increased strength and reduced deterioration in high-temperature environments.
Smart Images

Figure 0007577129000001 
Figure 0007577129000002 
Figure 0007577129000003
Abstract
Description
Related Applications
[0001] This application claims priority to Patent Application No. 2020-195469, filed in Japan on November 25, 2020, the entire contents of which are incorporated herein by reference. [Technical field]
[0002] The present invention relates to a liquid crystal polyester fiber and a method for producing the same. [Background technology]
[0003] Liquid crystal polyester fiber is a chemical fiber made of a polymer having a rigid molecular structure, and can be obtained by melt spinning liquid crystal polyester. Liquid crystal polyester fiber can exhibit very high mechanical properties by increasing the molecular weight of the polymer through solid-phase polymerization of the raw spun yarn obtained by melt spinning through heat treatment. Heat treatment in the solid-phase polymerization process requires high temperature and long time, but in order to improve productivity, many techniques have been studied to promote the polymerization reaction, such as increasing the molecular weight of liquid crystal polyester at low temperature and in a short time.
[0004] Regarding the polymerization of liquid crystal polyester, for example, Patent Document 1 (JP 2013-67779 A) describes a method for producing liquid crystal polyester in which a specific heteroaromatic compound is added as a catalyst in melt polycondensation of a monomer mixture containing at least one monomer selected from the group consisting of terephthalic acid, terephthalic acid derivatives, 2,6-naphthalenedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid derivatives, and it is described that such a production method allows the reaction to proceed at a low temperature in a short time.
[0005] Furthermore, Patent Document 2 (WO 2017 / 68867) describes a method for producing a wholly aromatic polyester by carrying out polymerization using a fatty acid metal salt (specifically, potassium acetate) as a polymerization catalyst. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-67779 A [Patent Document 2] WO 2017 / 68867 Summary of the Invention [Problem to be solved by the invention]
[0007] Thus, Patent Documents 1 and 2 describe polymerization catalysts used during melt polymerization in the production of liquid crystal polyester, but none of them describe catalysts used in solid-phase polymerization after molding (e.g., melt spinning) the liquid crystal polyester obtained by melt polymerization.
[0008] Specifically, basic organic catalysts such as the heteroaromatic compounds described in Patent Document 1 are thermally decomposed during melt spinning of the liquid crystal polyester at temperatures above 250°C, and therefore cannot be used in the subsequent solid-state polymerization.
[0009] In addition, the alkali metal ion catalyst described in Patent Document 2 has drawbacks such as a decrease in ultimate strength and a decrease in heat aging resistance of the fiber after the solid-state polymerization process, possibly because the catalyst has a function of promoting side reactions such as depolymerization reactions as the molecular weight increases.
[0010] In the solid-state polymerization process, other side reactions besides the polymerization reaction can occur, which result in a decrease in strength, as well as phenomena such as the softening of the fiber surface causing the fibers to fuse together and lose flexibility. Therefore, a technology is needed that selectively promotes only the polymerization reaction that contributes to improving mechanical properties at the lowest possible temperature and in the shortest possible time.
[0011] The present invention has been made in view of the above problems, and an object of the present invention is to provide a liquid crystalline polyester fiber which can exhibit excellent mechanical properties by a heat treatment at a low temperature for a short time and which is excellent in heat aging resistance. [Means for solving the problem]
[0012] The inventors of the present invention have conducted extensive research to achieve the above object, and have found that the polymerization catalysts that have been used in the past for melt polymerization cannot selectively promote the reaction in solid-state polymerization, possibly because the reaction mechanism of solid-state polymerization is different from that of melt polymerization. As a result of further research into catalysts suitable for solid-state polymerization, they have found that (i) by using a catalyst containing a specific metal element, excellent mechanical properties can be achieved by low-temperature and short-time heat treatment, and (ii) the progress of side reactions that cause strength reduction other than the polymerization reaction can be suppressed to some extent, and the heat aging resistance of the heat-treated yarn obtained after the solid-state polymerization process can be improved, leading to the completion of the present invention.
[0013] That is, the present invention can be configured in the following manner. [Aspect 1] A liquid crystal polyester fiber comprising at least one metal element selected from the group consisting of metal elements of Groups 8 to 11 of the periodic table (preferably at least one metal element selected from the group consisting of copper, cobalt, and palladium). [Aspect 2] The liquid crystal polyester fiber according to aspect 1, wherein the total content of the metal elements is 1 to 1000 ppm by weight (preferably 3 to 500 ppm by weight, more preferably 5 to 200 ppm by weight, and further preferably 10 to 100 ppm by weight). [Aspect 3] The liquid crystalline polyester fiber according to aspect 1 or 2, wherein the metal element is contained as a metal compound, and the melting point of the metal compound is a melting point of the liquid crystalline polyester + 30°C or less (preferably a melting point of the liquid crystalline polyester + 20°C or less). Aspect 4 A liquid crystalline polyester fiber according to any one of aspects 1 to 3, having a strength of 18 cN / dtex or more (preferably 20 cN / dtex or more, more preferably 23 cN / dtex or more). Aspect 5 The liquid crystal polyester fiber according to any one of aspects 1 to 4, wherein the total amount of one end is 20 meq / kg or less (preferably 3 to 15 meq / kg, more preferably 5 to 13 meq / kg). Aspect 6 The liquid crystal polyester fiber according to any one of aspects 1 to 5, wherein the liquid crystal polyester fiber has a ketone bond amount of 0.05 mol % or less (preferably 0.04 mol % or less, more preferably 0.02 mol % or less). Aspect 7 A method for producing the liquid crystalline polyester fiber according to any one of aspects 1 to 6, comprising melt spinning a resin composition containing a liquid crystalline polyester and at least one metal element selected from the group consisting of metal elements in Groups 8 to 11 of the periodic table (preferably at least one metal element selected from the group consisting of copper, cobalt, and palladium). Aspect 8 The method for producing a liquid crystal polyester fiber according to aspect 7, wherein the content of the metal elements in the resin composition is 1 to 1000 ppm by weight in total (preferably 3 to 500 ppm by weight, more preferably 5 to 200 ppm by weight, and further preferably 10 to 100 ppm by weight). Aspect 9 A method for producing a liquid crystalline polyester fiber according to aspect 7 or 8, wherein the metal element is contained in the resin composition as a compound having a melting point that is 30°C or lower above the melting point of the liquid crystalline polyester (preferably 20°C or lower above the melting point of the liquid crystalline polyester). Aspect 10 A method for producing a liquid crystalline polyester fiber according to any one of aspects 7 to 9, comprising heat-treating the raw spun yarn obtained by the melt spinning. Aspect 11 A method for producing a liquid crystal polyester fiber according to embodiment 10, wherein the total carboxy terminal amount (total CEG amount) of the raw spinning yarn is 5.0 meq / kg or less (preferably 4.0 meq / kg or less, more preferably 3.0 meq / kg or less, even more preferably 2.5 meq / kg or less, and still more preferably 2.0 meq / kg or less). Aspect 12 A fiber structure at least partially comprising the liquid crystal polyester fiber according to any one of the first to sixth aspects.
[0014] In this specification, the term "liquid crystal polyester fiber" refers to a fiber composed of a liquid crystal polyester, and is a concept including both a raw spun yarn obtained by melt spinning and a heat-treated yarn obtained by heat-treating the raw spun yarn.
[0015] It should be noted that any combination of at least two elements disclosed in the claims and / or the specification is included in the present invention. In particular, any combination of two or more of the claims described in the claims is included in the present invention. Effect of the Invention
[0016] The liquid crystal polyester fiber of the present invention can exhibit excellent mechanical properties by a heat treatment at a low temperature for a short time, and the liquid crystal polyester fiber after the heat treatment has excellent heat aging resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] [Liquid crystal polyester fiber] The liquid crystal polyester fiber of the present invention is composed of liquid crystal polyester. The liquid crystal polyester is composed of repeating structural units derived from, for example, aromatic diol, aromatic dicarboxylic acid, aromatic hydroxycarboxylic acid, etc., and the structural units derived from aromatic diol, aromatic dicarboxylic acid, and aromatic hydroxycarboxylic acid are not particularly limited in terms of their chemical structure as long as they do not impair the effects of the present invention. In addition, the liquid crystal polyester may contain structural units derived from aromatic diamine, aromatic hydroxyamine, or aromatic aminocarboxylic acid, as long as they do not impair the effects of the present invention. For example, examples of preferred structural units are shown in Table 1.
[0018] [Table 1]
[0019] In the structural units in Table 1, m is an integer of 0 to 2, and Y in the formula, in the range of 1 to the maximum number of possible substitution, each independently represents a hydrogen atom, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), an alkyl group (e.g., an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, an isopropyl group, a t-butyl group, etc.), an alkoxy group (e.g., a methoxy group, an ethoxy group, an isopropoxy group, a n-butoxy group, etc.), an aryl group (e.g., a phenyl group, a naphthyl group, etc.), an aralkyl group (e.g., a benzyl group (phenylmethyl group), a phenethyl group (phenylethyl group), etc.), an aryloxy group (e.g., a phenoxy group), an aralkyloxy group (e.g., a benzyloxy group), etc.).
[0020] More preferred structural units include the structural units described in Examples (1) to (18) in Tables 2, 3, and 4. When a structural unit in the formula is a structural unit that can exhibit multiple structures, two or more of such structural units may be combined and used as a structural unit that constitutes a polymer.
[0021] [Table 2]
[0022] [Table 3]
[0023] [Table 4]
[0024] In the structural units of Tables 2, 3 and 4, n is an integer of 1 or 2, and each structural unit n=1, n=2 may exist alone or in combination, and Y1 and Y2 may each independently be a hydrogen atom, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), an alkyl group (e.g., an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, an isopropyl group, a t-butyl group, etc.), an alkoxy group (e.g., a methoxy group, an ethoxy group, an isopropoxy group, an n-butoxy group, etc.), an aryl group (e.g., a phenyl group, a naphthyl group, etc.), an aralkyl group (e.g., a benzyl group (phenylmethyl group), a phenethyl group (phenylethyl group), etc.), an aryloxy group (e.g., a phenoxy group, etc.), an aralkyloxy group (e.g., a benzyloxy group, etc.), etc. Among these, a hydrogen atom, a chlorine atom, a bromine atom, or a methyl group is preferred.
[0025] Furthermore, examples of Z include substituents represented by the following formulas.
[0026] [ka]
[0027] The liquid crystal polyester may preferably be a combination having a naphthalene skeleton as a structural unit. It is particularly preferable to include both a structural unit (A) derived from hydroxybenzoic acid and a structural unit (B) derived from hydroxynaphthoic acid. For example, the structural unit (A) may be the following formula (A), and the structural unit (B) may be the following formula (B). From the viewpoint of improving melt moldability, the ratio of the structural unit (A) to the structural unit (B) may be preferably in the range of 9 / 1 to 1 / 1, more preferably 7 / 1 to 1 / 1, and even more preferably 5 / 1 to 1 / 1.
[0028] [ka]
[0029] [ka]
[0030] The total of the structural units (A) and the structural units (B) may be, for example, 65 mol % or more, more preferably 70 mol % or more, and even more preferably 80 mol % or more, based on the total structural units. In particular, liquid crystal polyesters in which the structural units (B) account for 4 to 45 mol % of the polymer are preferred.
[0031] The liquid crystal polyester may contain a structural unit derived from 4-hydroxybenzoic acid as an aromatic hydroxycarboxylic acid, and may contain a structural unit derived from an aromatic dicarboxylic acid and a structural unit derived from an aromatic diol. For example, at least one selected from the group consisting of the following formula (C) and the following formula (D) may be used as the structural unit derived from an aromatic dicarboxylic acid, and at least one selected from the group consisting of the following formula (E) and the following formula (F) may be used as the structural unit derived from an aromatic diol. Preferably, the liquid crystal polyester may include a structural unit (A) (above formula (A)) derived from 4-hydroxybenzoic acid, a structural unit (C) (below formula (C)) derived from terephthalic acid as an aromatic dicarboxylic acid, a structural unit (D) (below formula (D)) derived from isophthalic acid, and a structural unit (E) (below formula (E)) derived from 4,4'-dihydroxybiphenyl as an aromatic diol; a liquid crystal polyester may include a structural unit (A) (above formula (A)) derived from 4-hydroxybenzoic acid, a structural unit (C) (below formula (C)) derived from terephthalic acid as an aromatic dicarboxylic acid, a structural unit (D) (below formula (D)) derived from isophthalic acid, a structural unit (E) (below formula (E)) derived from 4,4'-dihydroxybiphenyl as an aromatic diol, and a structural unit (F) (below formula (F)) derived from hydroquinone.
[0032] [ka]
[0033] [ka]
[0034] [ka]
[0035] [ka]
[0036] The liquid crystal polyester may contain a constitutional unit derived from 4-hydroxybenzoic acid, preferably 50 mol% or more, more preferably 53 mol% or more, and even more preferably 60 mol% or more. The upper limit of the content of the constitutional unit derived from 4-hydroxybenzoic acid in the liquid crystal polyester is not particularly limited, but may be, for example, 90 mol% or less, preferably 88 mol% or less, and more preferably 85 mol% or less.
[0037] The melting point (hereinafter sometimes referred to as Mp0) of the liquid crystal polyester suitably used in the present invention is preferably in the range of 250 to 380°C, more preferably 255 to 370°C, even more preferably 260 to 360°C, and even more preferably 260 to 330°C. The melting point here is the main absorption peak temperature observed when measured with a differential scanning calorimeter (DSC; Mettler "TA3000") in accordance with the JIS K 7121 test method. Specifically, 10 to 20 mg of a sample is taken and sealed in an aluminum pan in the DSC device, and the endothermic peak is measured when nitrogen is flowed as a carrier gas at 100 mL / min and the temperature is raised at 20°C / min. If no clear peak appears in the first run of DSC measurement due to the type of polymer, the polymer should be heated at 50°C / min to a temperature 50°C higher than the expected flow temperature, completely melted at that temperature for 3 minutes, then cooled to 50°C at a rate of 80°C / min, and then the endothermic peak should be measured at a heating rate of 20°C / min.
[0038] The liquid crystal polyester may contain thermoplastic polymers such as polyethylene terephthalate, modified polyethylene terephthalate, polyolefin, polycarbonate, polyamide, polyphenylene sulfide, polyether ether ketone, fluororesin, etc., within the scope of not impairing the effects of the present invention. In addition, the liquid crystal polyester may contain various additives such as inorganic substances such as titanium oxide, kaolin, silica, barium oxide, etc., colorants such as carbon black, dyes, pigments, etc., antioxidants, ultraviolet absorbers, light stabilizers, etc.
[0039] The liquid crystal polyester fiber of the present invention contains at least one metal element selected from the group consisting of metal elements of Groups 8 to 11 of the periodic table. Preferably, at least one metal element is selected from the group consisting of metal elements of Periods 4 to 6 and Groups 8 to 11 of the periodic table, and specifically, at least one metal element may be selected from the group consisting of iron, ruthenium, osmium, cobalt, rhodium, iridium, nickel, palladium, platinum, copper, silver, and gold. Since the progress of the reaction in solid-phase polymerization can be promoted by the catalytic action of a specific metal element, the liquid crystal polyester fiber spinning raw yarn containing such a metal element as a solid-phase polymerization catalyst can exhibit excellent mechanical properties by low-temperature and short-time heat treatment. In addition, these metal elements can selectively promote the polymerization reaction and can suppress to some extent the progress of side reactions that cause a decrease in strength other than the polymerization reaction, so that the heat-treated yarn of the liquid crystal polyester fiber containing such a metal element has excellent heat aging resistance, that is, even if it is kept in a high-temperature environment for a long time, the decrease in mechanical properties can be suppressed.
[0040] From the viewpoint of promoting the polymerization reaction in solid-state polymerization, the metal element contained in the liquid crystal polyester fiber of the present invention may more preferably be at least one metal element selected from the group consisting of copper, cobalt, and palladium, and further preferably be copper.
[0041] The above metal elements may be contained as metal compounds having a structure in which a metal atom is bonded to a nonmetallic atom. Examples of metal compounds include formates, acetates, propionates, butyrates, valerates, capronates, enanthates, caprylates, pelargonates, caprates, laurates, myristates, palmitates, stearates, naphthenates, benzoates, oxalates, malonates, succinates, adipates, terephthalates, isophthalates, phthalates, salicylates, tartrates, citrates, fluoroacetates, chloroacetates, bromoacetates, fluoropropionates, chloropropionates, bromopropionates, and other organic acid salts; sulfates, carbonates, nitrates, and other inorganic acid salts; fluorides, chlorides, bromides, iodides, and other halides; hydroxides; oxides; sulfides, and the like. These metal compounds may be used alone or in combination of two or more. Among these metal compounds, for example, organic acid salts, inorganic acid salts, halides, and hydroxides are preferred from the viewpoint of having a low melting point and being able to improve dispersibility in the fibers.
[0042] The metal compound is not particularly limited as long as it acts as a solid-phase polymerization catalyst, but may be a metal compound that acts as a catalyst for decarboxylation of aromatic carboxylic acid, and may be a metal complex compound in which a metal atom is coordinated with a ligand from the viewpoint of promoting the polymerization reaction in solid-phase polymerization. The ligand is not particularly limited as long as it is a ligand that can be coordinated to a metal atom in the metal compound, but examples of the ligand include nitrogen-based ligands, oxygen-based ligands, carbon-based ligands, phosphorus-based ligands, and sulfur-based ligands. In the metal compound, an organic acid corresponding to the organic acid salt, an inorganic acid corresponding to the inorganic acid salt, or a halogen corresponding to the halide may be coordinated to the metal atom as a ligand.
[0043] The nitrogen-based ligand is not particularly limited as long as it has a nitrogen atom capable of being coordinated to the metal atom. Examples of the nitrogen-based ligand include ammine (NH3), aniline, diisopropylamine, triethylamine, triphenylamine, hexamethyldisilazane, diazabicycloundecene, ethylenediamine (en), 2,3-butanediamine, N,N,N',N'-tetramethylethylenediamine, ethylenediaminetetraacetic acid (edta), diethylenetriamine, N,N,N',N'',N''-pentamethyldiethylenetriamine, 1,4,7-triazacyclononane, triethylenetetramine, tris(2-aminoethyl)amine, hexamethylenetetramine, etc. Amine ligands; nitrogen-containing heteroaromatic ligands such as pyrrole, pyridine (py), dimethylpyridine, bipyridine (bpy), terpyridine, imidazole, pyrazole, pyrazine, pyrimidine, triazole, quinoline, isoquinoline, acridine, 1,8-naphthyridine, phenanthroline (phen), 2,9-dimethyl-1,10-phenanthroline, 4,7-diphenyl-1,10-phenanthroline, 2,9-diphenyl-1,10-phenanthroline, 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline, dimethylaminopyridine, and porphyrin; nitrile ligands such as acetonitrile and benzonitrile; cyanide (CN - );isothiocyanide (NCS - ); nitrosyl (NO), etc.
[0044] The oxygen-based ligand is not particularly limited as long as it has an oxygen atom capable of being coordinated to the metal atom. Examples of the oxygen-based ligand include ether-based ligands such as dimethyl ether, diethyl ether, tetrahydrofuran, 1,4-dioxane, and 1,2-dimethoxyethane; alcohol-based ligands such as methanol, ethanol, phenol, and 1,1'-binaphthalene-2,2'-diol; carboxylate (RCOO) ligands; - ), oxalate (ox 2- ), acetylacetonate (acac), and other acyl ligands; aqua (HO); hydroxide (OH - );Oxo(O 2- ) etc.
[0045] The carbon-based ligand is not particularly limited as long as it is a ligand having a carbon atom capable of being coordinated to the metal atom, and examples thereof include alkyl-based ligands such as methyl; aryl-based ligands such as phenyl; vinyl-based ligands; alkynyl-based ligands; carbene-based ligands such as N-heterocyclic carbene; alkene-based ligands such as ethylene and dibenzylideneacetone (dba); alkyne-based ligands such as acetylene and 2-phenylethynylbenzene; cyclopentadiene-based ligands such as cyclopentadiene and pentamethylcyclopentadiene; diene-based ligands such as 1,3-butadiene and 1,5-cyclooctadiene (cod); cyclic polyene-based ligands such as benzene and cyclooctatetraene; isocyanide-based ligands such as cyanomethylisocyanide and phenylisocyanide; carbonyl (CO), and the like.
[0046] The phosphorus-based ligand is not particularly limited as long as it is a ligand having a phosphorus atom capable of being coordinated to the above-mentioned metal atom, and examples thereof include triphenylphosphine, tris(2-methylphenyl)phosphine, tris(2-methoxyphenyl)phosphine, di-tert-butylphenylphosphine, trimethylphosphine, tri-tert-butylphosphine, tricyclohexylphosphine, bis(diphenylphosphino)methane (dppm), 1,2-bis(diphenylphosphino)ethane (dppe), 1,3-bis(diphenylphosphino)propane (dppp), 2,2'-bis(diphenylphosphino)methane (dppe), 1,3-bis(diphenylphosphino)propane (dppp), 2,2'-bis(diphenylphosphino)methane (dppm), 2,2'-bis(diphenylphosphino)propane (dppp), 2,2'-bis(diphenylphosphino)methane (dppe), 2,2'-bis(diphenylphosphino)propane (dppp ... and phosphine-based ligands such as phosphine(diphenylphosphino)-1,1'-binaphthyl (BINAP), 2-dicyclohexylphosphino-2',6'-dimethoxybiphenyl (SPhos), 2-dicyclohexylphosphino-2',4',6'-triisopropylbiphenyl (XPhos), 2-dicyclohexylphosphino-2'-methylbiphenyl (MePhos), 2-dicyclohexylphosphino-2'-(N,N-dimethylamino)biphenyl (DavePhos), and 2-(di-tert-butylphosphino)biphenyl (JohnPhos).
[0047] The sulfur-based ligand is not particularly limited as long as it has a sulfur atom capable of being coordinated to the metal atom. Examples of the sulfur-based ligand include thiol-based ligands; sulfoxide-based ligands such as dimethyl sulfoxide (DMSO); sulfur-containing heteroaromatic ligands such as thiophene, dibenzothiophene, and thiopyran; thiocyanide (SCN) - );Sulfide (S 2- ) etc.
[0048] The preferred ligand varies depending on the type of metal atom. In the case of copper, from the viewpoint of promoting the polymerization reaction in solid-phase polymerization, it is preferable that a nitrogen-based ligand is coordinated, more preferably that a nitrogen-containing heteroaromatic ligand or a nitrogen-based chelate ligand is coordinated, and even more preferably that a nitrogen-containing heteroaromatic chelate ligand is coordinated. Here, the chelate ligand is a ligand having two or more coordination sites in the molecule, and the multiple coordination sites are located at positions where they can be coordinated simultaneously with one metal atom. Examples of the nitrogen-based chelate ligand include ethylenediamine, diethylenetriamine, triethylenetetramine, tris(2-aminoethyl)amine, hexamethylenetetramine, bipyridine, terpyridine, phenanthroline, and derivatives thereof.
[0049] The valence of copper in the copper compound may be zero, monovalent, or divalent. From the viewpoint of avoiding aggregation or localization during melt spinning, it is preferably monovalent or divalent, and from the viewpoint of promoting the polymerization reaction in solid-state polymerization, it is more preferably monovalent.
[0050] In the case of cobalt, from the viewpoints of stability in the atmosphere during use and promotion of the polymerization reaction in solid-phase polymerization, it is preferable that an oxygen-based ligand is coordinated, and more preferably an acyl-based ligand is coordinated.
[0051] In the case of palladium, from the viewpoints of stability in the atmosphere during use and promotion of the polymerization reaction in solid-phase polymerization, it is preferable that an oxygen-based ligand is coordinated, and it is more preferable that an acyl-based ligand (e.g., carboxylato (preferably, acetato, trifluoroacetato)) is coordinated.
[0052] The liquid crystal polyester fiber of the present invention can appropriately set the content of the metal element according to the type of the metal element, but for example, from the viewpoint of achieving a good balance between the promotion of polymerization reaction in solid-state polymerization and the suppression of side reactions, the above metal elements may be contained in a total of 1 to 1000 ppm by weight, preferably 3 to 500 ppm by weight, more preferably 5 to 200 ppm by weight, and even more preferably 10 to 100 ppm by weight. The content of the metal element indicates the ratio of the total weight of the above metal element to the total weight of the liquid crystal polyester fiber, and when the metal element is contained as the above-mentioned metal compound, it indicates the content in terms of metal atom. Here, the above content of the metal element may be the content of the metal element in the components constituting the fiber itself, excluding components attached to the fiber surface such as oils.
[0053] In the liquid crystal polyester fiber of the present invention, the content of alkali metals and alkaline earth metals may be less than 100 ppm by weight in total, preferably 10 ppm by weight or less, more preferably 5 ppm by weight or less, and even more preferably 1 ppm by weight or less, from the viewpoint of suppressing side reactions in solid-phase polymerization. Here, the content of alkali metals and alkaline earth metals may be the content of alkali metals and alkaline earth metals in the components constituting the fiber itself, excluding components attached to the fiber surface such as oils. In this specification, alkali metals refer to lithium, sodium, potassium, rubidium, cesium, and francium, and alkaline earth metals refer to beryllium, magnesium, calcium, strontium, barium, and radium.
[0054] Furthermore, the liquid crystal polyester fiber of the present invention may contain 50% by weight or more of liquid crystal polyester, preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 95% by weight or more, and even more preferably 99.9% by weight or more.
[0055] The liquid crystal polyester fiber spinning raw yarn of the present invention may have a total carboxy terminal amount (total CEG amount) of 5.0 meq / kg or less. Although the relationship between the carboxy group present at the molecular end of the liquid crystal polyester and the reaction in solid-phase polymerization is not clear, it is considered that reducing the amount of carboxy groups at the molecular end is one of the factors that activate the reaction in solid-phase polymerization, and it is considered that a spinning raw yarn with a small total carboxy terminal amount can exhibit excellent mechanical properties by heat treatment at a low temperature and for a short time. The total carboxy terminal amount (total CEG amount) of the liquid crystal polyester fiber spinning raw yarn may be preferably 4.0 meq / kg or less, more preferably 3.0 meq / kg or less, even more preferably 2.5 meq / kg or less, and even more preferably 2.0 meq / kg or less. The total carboxy terminal amount (total CEG amount) is a value measured by the method described in the examples described later, and is the amount of carboxy groups present at the molecular ends of the molecules that mainly constitute the liquid crystal polyester fiber in 1 kg of fiber. For example, the carboxy group present at the polymer end in the liquid crystal polyester may be a carboxy group that remains unreacted in a structural unit present at such a polymer end, the structural unit being derived from a monomer having a carboxy group, such as an aromatic hydroxycarboxylic acid or an aromatic dicarboxylic acid.
[0056] The liquid crystal polyester fiber of the present invention may have a total one-terminal amount of 50 meq / kg or more, preferably 55 meq / kg or more, more preferably 60 meq / kg or more. It may also be 200 meq / kg or less, preferably 100 meq / kg or less. The total one-terminal amount indicates the number of polymer chains and is used as an index for evaluating the molecular weight. The larger the total one-terminal amount, the smaller the molecular weight, and the smaller the total one-terminal amount, the larger the molecular weight. Considering that it is difficult to quantify all types of terminals in liquid crystal polyester depending on the composition, in the present invention, the total one-terminal amount is defined as a numerical value obtained by dividing the total amount (meq / kg) of carboxyl group terminals derived from hydroxycarboxylic acid and terminals from which carbon dioxide has been eliminated by decarboxylation reaction in the carboxyl group derived from hydroxycarboxylic acid per 1 kg of liquid crystal polyester fiber by the molar ratio of the structural unit derived from hydroxycarboxylic acid in the liquid crystal polyester, and is a value measured by the method described in the examples below. By heat treating the spinning raw yarn having a relatively large total one-terminal amount as described above, solid-phase polymerization proceeds and the total one-terminal amount can be reduced (i.e., the molecular weight can be increased).
[0057] The liquid crystal polyester fiber spinning raw yarn of the present invention can exhibit excellent mechanical properties by heat treatment at a low temperature and for a short time. In general, heat treatment of the liquid crystal polyester fiber spinning raw yarn requires a long time (for example, about 20 hours) to improve the mechanical properties, and even when the heat treatment time is to be shortened, it is necessary to gradually increase the heat treatment temperature and perform heat treatment at a high temperature above the melting point of the spinning raw yarn, taking advantage of the fact that the melting point of the liquid crystal polyester fiber increases with the progress of solid-phase polymerization. In the present invention, when the strength of the liquid crystal polyester fiber spinning raw yarn is, for example, 12 cN / dtex or less, a heat-treated yarn with a strength of 18 cN / dtex or more can be obtained by heat treatment at a low temperature and for a short time. The low temperature and short time conditions vary depending on the heat treatment method and the amount of the raw spinning yarn subjected to the heat treatment, but for example, in a batch-type heat treatment, the strength of the heat-treated yarn may be 18 cN / dtex or more, preferably 20 cN / dtex or more, and more preferably 23 cN / dtex or more, by heat-treating the liquid crystal polyester fiber at a temperature lower than the melting point (Mp) of the raw spinning yarn for 3 hours or less. In the present invention, the liquid crystal polyester fiber may be regarded as a raw spinning yarn when the strength is 12 cN / dtex or less, and may be regarded as a heat-treated yarn when the strength exceeds 12 cN / dtex.
[0058] The heat-treated yarn of the liquid crystal polyester fiber of the present invention may have a strength of 18 cN / dtex or more, preferably 20 cN / dtex or more, more preferably 23 cN / dtex or more. The upper limit of the strength is not particularly limited, but may be, for example, about 40 cN / dtex. In the present invention, the strength of the liquid crystal polyester fiber refers to the tensile strength, and is a value measured by the method described in the examples below.
[0059] The heat-treated yarn of the liquid crystal polyester fiber of the present invention preferably has a high molecular weight from the viewpoint of improving mechanical properties such as strength, and for example, the total amount of one terminal may be 20 meq / kg or less, preferably 15 meq / kg or less, more preferably 13 meq / kg or less. The lower limit of the total amount of one terminal is not particularly limited, but may be, for example, 3 meq / kg or more, preferably 5 meq / kg or more.
[0060] From the viewpoint of improving mechanical properties such as strength, the heat-treated yarn of the liquid crystal polyester fiber of the present invention may have a ketone bond amount of 0.05 mol% or less, preferably 0.04 mol% or less, more preferably 0.02 mol% or less. In the present invention, the ketone bond amount means the ratio of the molar amount of the ketone bond to the total molar amount of the ester bond and the ketone bond, and is a value measured by the method described in the examples below. If the ketone bond amount is too large, the strength of the liquid crystal polyester fiber tends to decrease, possibly due to a decrease in the linearity of the polymer. The lower limit of the ketone bond amount is not particularly limited, but may be, for example, 0.005 mol% or more.
[0061] The heat-treated liquid crystal polyester fiber of the present invention may have a melting point of 290 to 400° C., preferably 300 to 380° C., and more preferably 305 to 350° C. The melting point of the liquid crystal polyester fiber is increased from the melting point (Mp) of the raw spinning yarn by solid-phase polymerization. The melting point of the liquid crystal polyester fiber is a value measured by the method described in the examples below.
[0062] The heat-treated yarn of the liquid crystal polyester fiber of the present invention has excellent heat aging resistance, and the strength retention rate when heated at 250°C for 100 hours may be 70% or more, preferably 80% or more, more preferably 85% or more. In addition, the strength retention rate when heated at 250°C for 300 hours may be 50% or more, preferably 60% or more, more preferably 65% or more. Since the heat-treated yarn preferably has a sufficiently high strength due to solid-phase polymerization, the strength retention rate when heated at 250°C for 100 hours or 300 hours may be 100% or less. The strength retention rate of the heat-treated yarn is a value measured by the method described in the examples below.
[0063] The single fiber fineness of the liquid crystal polyester fiber of the present invention can be appropriately selected depending on the application, etc., and may be, for example, 0.5 to 50 dtex, preferably 1.0 to 35 dtex, more preferably 1.0 to 15 dtex, and further preferably 1.5 to 10 dtex.
[0064] The liquid crystal polyester fiber of the present invention may be a monofilament or a multifilament. In the case of a multifilament, the number of filaments can be appropriately selected depending on the application, etc. For example, the number of filaments may be 5 to 5,000, preferably 10 to 4,000, and more preferably 30 to 3,000.
[0065] The total fineness of the liquid crystal polyester fiber of the present invention can be appropriately selected depending on the application, etc., and may be, for example, 10 to 50,000 dtex, preferably 15 to 30,000 dtex, more preferably 25 to 10,000 dtex.
[0066] [Method of manufacturing liquid crystal polyester fiber] The method for producing a liquid crystal polyester fiber of the present invention may include at least a step of melt spinning a resin composition containing a liquid crystal polyester and at least one metal element selected from the group consisting of metal elements of Groups 8 to 11 of the periodic table.
[0067] The resin composition may contain the liquid crystal polyester and at least one metal element selected from the group consisting of metal elements in Groups 8 to 11 of the periodic table. The form in which the metal element is contained is not particularly limited, and the metal element may be contained as the metal compound described above.
[0068] From the viewpoint of achieving both favorable acceleration of polymerization reaction in solid-state polymerization and suppression of side reactions, the resin composition may contain, for example, 1 to 1000 ppm by weight of the above metal elements in total, preferably 3 to 500 ppm by weight, more preferably 5 to 200 ppm by weight, and further preferably 10 to 100 ppm by weight. The content of the metal elements in the resin composition indicates the ratio of the total weight of the added metal elements to the total weight of the resin composition including the liquid crystal polyester and the added metal elements, and when the metal elements are contained as the above-mentioned metal compounds, the content is expressed in terms of metal atoms.
[0069] From the viewpoint of promoting the polymerization reaction in the solid-state polymerization, the metal compound may be the above-mentioned metal complex compound. In this case, the metal compound may be mixed into the resin composition in such a manner that the metal complex compound already has a ligand coordinately bonded thereto, or the metal compound and the compound that forms the ligand may be added separately to the resin.
[0070] The metal compound may be a compound having a melting point of the liquid crystal polyester (Mp0)+30°C or less from the viewpoint of improving the long-term operation of melt spinning and improving the dispersibility in the resin. In the melt spinning process, the resin composition is heated and melted at a temperature equal to or higher than the melting point (Mp0) of the liquid crystal polyester, but since the reaction related to solid-phase polymerization can be progressed to some extent even at this stage due to the catalytic action of the metal element in the resin composition, it is preferable to melt the metal compound together with the liquid crystal polyester in the resin composition to promote the reaction. The upper limit of the melting point of the metal compound is preferably Mp0+20°C or less. From the viewpoint of processability, the melting point of the metal compound is preferably 400° C. or less, and more preferably 350° C. or less. The lower limit of the melting point of the metal compound is not particularly limited, but from the viewpoint of handleability in the vicinity of a melt spinning machine, it is preferably 100° C. or more.
[0071] Melt spinning can be carried out by a known or conventional method. For example, the resin composition is melted in an extruder, extruded from a nozzle at a predetermined spinning temperature, and wound up by a godet roller or the like.
[0072] The method for producing the liquid crystal polyester fiber of the present invention may further include a solid-phase polymerization step of heat-treating the raw spun yarn obtained by melt spinning. Since the raw spun yarn of the liquid crystal polyester fiber of the present invention can promote the reaction in the solid-phase polymerization due to the catalytic action of a specific metal element, the heat treatment in the solid-phase polymerization step can be performed at a low temperature for a short time.
[0073] From the viewpoint of promoting the polymerization reaction in the solid-phase polymerization, the raw spun yarn to be subjected to the solid-phase polymerization step may have a total carboxy terminal amount (total CEG amount) of 5.0 meq / kg or less, preferably 4.0 meq / kg or less, more preferably 3.0 meq / kg or less, even more preferably 2.5 meq / kg or less, and even more preferably 2.0 meq / kg or less. In the above melt spinning step, when the resin composition is heated and melted at a temperature equal to or higher than the melting point (Mp0) of the liquid crystal polyester, the amount of the carboxy groups at the molecular terminals of the liquid crystal polyester can be reduced by desorbing carbon dioxide from the carboxy groups at the molecular terminals, possibly because the metal elements in the resin composition act as a catalyst for the decarboxylation reaction.
[0074] The method of heat treatment in the solid-state polymerization step is not particularly limited, and may be, for example, a batch-type heat treatment or a continuous heat treatment by conveying.
[0075] For example, in the case of a batch-type heat treatment, the heat treatment may be performed in a state where the material is wound around a bobbin in a packaged form, or in a skein or tow form, and it is preferable to perform the heat treatment in a packaged form in terms of simplifying the equipment and improving productivity. The bobbin must be able to withstand the temperature of the solid-state polymerization, and is preferably made of a metal such as aluminum, brass, iron, or stainless steel.
[0076] In the case of continuous heat treatment by conveyance, the conveyance method may be either contact conveyance (for example, conveyor system, support roll system, heat treatment system using heated rollers) or non-contact conveyance (roll-to-roll system). The treatment path does not have to be a straight line, and turning rollers or guides may be arranged in the device to appropriately change the length, angle, curvature, etc. of the treatment path for heat treatment.
[0077] The solid-state polymerization step can be carried out by a known method, such as atmospheric heating, contact heating, etc. The atmosphere is preferably air, an inert gas (e.g., nitrogen, argon), or a combination thereof. The solid-state polymerization can also be carried out under reduced pressure.
[0078] In the solid-state polymerization step, the heat treatment temperature may be 230°C or higher, and from the viewpoint of efficient strength improvement, it may be preferably 240°C or higher, more preferably 250°C or higher. The heat treatment temperature may be lower than the melting point (Mp) of the raw spun yarn to be subjected to the solid-state polymerization step in order to prevent melting. For example, in the range of 230°C or higher, it may be Mp-80°C or higher and lower than Mp°C, preferably Mp-50°C or higher and lower than Mp°C, more preferably Mp-30°C or higher and lower than Mp°C. In the present invention, excellent mechanical properties can be exhibited at a low heat treatment temperature, but since the melting point of the liquid crystal polyester fiber increases as the solid-state polymerization proceeds, it is sufficient to set the initial heat treatment temperature in the solid-state polymerization step lower than the melting point (Mp) of the raw spun yarn, and from the viewpoint of efficient strength improvement, the heat treatment temperature may be increased stepwise according to the progress of the solid-state polymerization, and heat treatment may be performed at a temperature higher than the melting point (melting point of the raw spun yarn) at the time of subjecting to the solid-state polymerization step.
[0079] In the present invention, excellent mechanical properties can be exhibited by a short heat treatment, but the heat treatment time of the solid-phase polymerization step can be appropriately set according to the heat treatment method and heat treatment temperature. The heat treatment time is not particularly limited as long as the desired mechanical properties can be exhibited, but can be set, for example, within the range of 15 minutes to 15 hours, preferably 30 minutes to 10 hours, more preferably 1 to 8 hours, and the short heat treatment time can be, for example, 15 minutes to 3 hours. The heat treatment time here refers to the retention time at a predetermined heat treatment temperature.
[0080] In the method for producing the liquid crystal polyester fiber of the present invention, the strength ratio of the liquid crystal polyester fiber before and after the solid-state polymerization process may be 1.5 times or more, preferably 1.8 times or more, and more preferably 2.0 times or more. The upper limit of the strength ratio of the liquid crystal polyester fiber before and after the solid-state polymerization process is not particularly limited, but may be, for example, 10 times or less. Here, the strength ratio before and after the solid-state polymerization process refers to the value obtained by dividing the tensile strength of the liquid crystal polyester fiber after the solid-state polymerization process by the tensile strength of the liquid crystal polyester fiber (raw spinning yarn) before the solid-state polymerization process.
[0081] In the method for producing a liquid crystal polyester fiber of the present invention, for example, in order to improve the bundling property of the fiber or to prevent fusion during heat treatment, a known oil agent may be added before or after the solid-phase polymerization step, and a compound containing an alkali metal or an alkaline earth metal may be added as described above.
[0082] The liquid crystal polyester fiber of the present invention can be suitably used for various fiber structures. Examples of the fiber structures include one-dimensional structures such as ropes and mixed yarns, and highly processed products such as two-dimensional structures such as woven fabrics, knitted fabrics, and nonwoven fabrics, and can be used as various fiber products such as tension members (electric wires, optical fibers, heater wire core threads, cords for various electrical products such as earphone cords), sail cloths, ropes, sling belts, ropes, land nets, lifelines, fishing lines, fishing nets, and longlines. The fiber structures may be composed of the liquid crystal polyester fiber alone, or may contain other components within a range that does not impair the effects of the present invention. EXAMPLES
[0083] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. In the following examples and comparative examples, various physical properties were measured by the following methods.
[0084] (Total fineness, single fiber fineness) Based on JIS L 1013:2010 8.3.1 A method, the liquid crystal polyester fiber was wound into a skein of 1m per turn x 100 turns (total 100m) using a measuring device "Wrap Reel by Motor Driven" manufactured by Daiei Scientific Instruments Co., Ltd., and the weight (g) was multiplied by 100 to perform measurements twice per level, and the average value was taken as the total fineness (dtex) of the liquid crystal polyester fiber obtained. The quotient obtained by dividing this value by the number of filaments was taken as the single fiber fineness (dtex).
[0085] (Melting point of fiber and resin chips (granular moldings)) The melting point was determined as the main absorption peak temperature observed by measuring using a differential scanning calorimeter (DSC; Mettler, "TA3000") in accordance with JIS K 7121. Specifically, 10 to 20 mg of a sample was placed in an aluminum pan and sealed in the DSC device, and nitrogen was passed as a carrier gas at a flow rate of 100 mL / min, and the endothermic peak derived from the liquid crystal polyester was measured when the temperature was raised from 25°C at a rate of 20°C / min.
[0086] (Melting point of metal compounds) The measurement was performed using the same equipment and pan as in the measurement of the melting point of the fiber described above. However, in order to eliminate peaks due to hydration water and residual solvent, nitrogen was flowed as a carrier gas at a flow rate of 100 mL / min, the temperature was raised from 25°C to 150°C at 20°C / min, held for 1 minute, then cooled to 25°C at -20°C / min, and the endothermic peak that appeared at the lowest temperature was measured when the temperature was raised again from 25°C at 20°C / min.
[0087] (Metal element content) A liquid for analysis was prepared by the "microwave decomposition" described below, and the metal element content (ppm by weight) was determined by ICP-MS measurement. Microwave digestion Microwave decomposition was performed using a microwave decomposition device "ETHOS-1" manufactured by Milestone General Co., Ltd. 0.1 g of liquid crystal polyester fiber sample was weighed into a quartz insert, and 6 mL of nitric acid (1.42 mol / L) was added. The quartz insert was placed in a decomposition vessel containing 5 mL of water and 2 mL of hydrogen peroxide (concentration 30-36 wt%), sealed, and microwave decomposition was performed. After cooling, the volume was adjusted to 50 mL, and the filtrate was filtered through a 0.45 μm pore size filter and subjected to ICP-MS measurement. ICP-MS measurement The metal element content of the sample solution prepared by the microwave digestion was analyzed using an ICP-MS analyzer "Agirent 7900" manufactured by Agilent Technologies. The same sample solution was measured three times in comparison with XSTC-622 (standard solution manufactured by SPEX) under the conditions of a carrier gas flow rate of 0.7 L / min and RF output of 1500 W, and the content of each metal element was determined from the average value. In addition, when a sample has oil on it, such as a fiber, and there is concern about the influence of metal elements contained in the oil, it is recommended to remove the oil using the following method before performing microwave digestion. · Oil removal A liquid crystal polyester fiber sample of 100 g or less was placed in an aqueous solution in which 2 g of a nonionic surfactant (Actinol F-9, manufactured by Matsumoto Yushi Seiyaku Co., Ltd.) was dissolved in 1 L of ion-exchanged water, and the temperature was adjusted to 60 to 90 ° C., followed by shaking for 40 minutes. The liquid crystal polyester fiber sample was removed and rinsed twice for 40 minutes with 1 L of ion-exchanged water adjusted to 60 to 90 ° C. The liquid crystal polyester fiber sample was removed and dried in an air atmosphere at 80 ° C. for 3 hours or more using a hot air dryer "DN63HI" manufactured by Yamato Scientific Co., Ltd., to obtain a liquid crystal polyester fiber sample from which the oil agent had been removed.
[0088] (Tensile strength) With reference to JIS L 1013:2010 8.5.1, a tensile test was performed six times for one yarn sample using an autograph "AGS-100B" manufactured by Shimadzu Corporation under conditions of a test length of 10 cm and a tensile speed of 10 cm / min. The average tensile strength (cN) was divided by the total fineness (dtex) measured by the above-mentioned method to calculate the tensile strength (cN / dtex).
[0089] (Total CEG amount) The liquid crystal polyester fiber sample was frozen and crushed to d90 = 100 μm or less, and a large excess of n-propylamine was added to the crushed sample, which was then heated and stirred at 40 ° C for 90 minutes to decompose the sample. In this case, the ester bond present inside the polymer chain was decomposed into carboxylic acid n-propylamide and a hydroxy group, and the carboxy group (CEG) and hydroxy group present at the end of the polymer chain did not change from the carboxy group and hydroxy group, so the decomposition products were separated by HPLC, and the amount of carboxy terminals (meq / kg) derived from each monomer was quantified by comparing the peak area of the decomposition products having carboxy groups with the calibration curves created by HPLC analysis of each standard. For example, the amount of CEG derived from monovalent carboxylic acids such as 4-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid was determined by quantifying 4-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid as they are, and the amount of terephthalic acid, isophthalic acid, 2, The amount of CEG derived from divalent carboxylic acids such as 6-naphthalenedicarboxylic acid can be determined by quantifying substances in which one of the carboxy groups is amidated, such as terephthalic acid mono-n-propylamide, isophthalic acid mono-n-propylamide, and 2,6-naphthalenedicarboxylic acid mono-n-propylamide. The sum of all the carboxyl terminal amounts contained in each sample was taken as the total carboxyl terminal amount (total CEG amount) (meq / kg) of that sample.
[0090] (Total end amount) As in the measurement of the total CEG amount, the liquid crystal polyester fiber sample was decomposed using n-propylamine, and the total amount (meq / kg) of the carboxyl end amount derived from hydroxycarboxylic acid and the end amount generated by the decarboxylation reaction of the carboxyl group at the end derived from hydroxycarboxylic acid was quantified. For example, the amount of end derived from 4-hydroxybenzoic acid was determined by quantifying 4-hydroxybenzoic acid and phenol, and the amount of end derived from 6-hydroxy-2-naphthoic acid was determined by quantifying 6-hydroxy-2-naphthoic acid and 2-naphthol. In order to take into account the amount of end derived from diols and dicarboxylic acids other than hydroxycarboxylic acid, the total amount of end derived from hydroxycarboxylic acid was divided by the molar ratio of the structural unit derived from hydroxycarboxylic acid in the liquid crystal polyester of the sample, and the total amount of end from one end of the sample was determined.
[0091] (Ketone binding amount) The amount of ketone bonds was calculated by pyrolysis gas chromatography described in Polymer Degradation and Stability, 76, 85-94 (2002). Specifically, a liquid crystal polyester fiber sample was heated in the presence of tetramethylammonium hydroxide (TMAH) using a pyrolysis apparatus (Frontier Labs, Inc., "PY2020iD") to generate gas by pyrolysis / methylation. This gas was analyzed using gas chromatography (Agilent Technologies, Inc., "GC-6890N"), and the amount of ketone bonds (mol%) was calculated from the peak area derived from the ketone bonds and the peak area derived from the ester bonds.
[0092] (Heat aging resistance) After applying 80T / m twist in the Z direction to the yarn sample, the liquid crystal polyester fiber was wound into a skein of 1m x 50 skeins (total of 50m) using a measuring device "Wrap Reel by Motor Driven" manufactured by Daiei Scientific Precision Manufacturing Co., Ltd. The liquid crystal polyester fiber was heated at 250°C in an air atmosphere using a hot air dryer "DN63HI" manufactured by Yamato Scientific Co., Ltd. Two skeins were made for each sample, one of which was heated for 100 hours and the other for 300 hours. During heating, the skein was hung on a metal bar placed near the top of the furnace so that there was no contact other than the contact point with the metal bar. The average tensile strength (cN) of the heated sample was measured using the method described above using the parts other than the contact point with the metal bar. The ratio of this value divided by the average tensile strength (cN) before heating in the heat aging resistance test and multiplied by 100 was used as the strength retention rate (%) at 250°C for 100 hours and 300 hours.
[0093] [Example 1] The constituent units (A) and (B) shown in the formula below are (A) / (B)=73 / 27 (molar ratio), and the content of alkali metals and alkaline earth metals is 10 ppm by weight or less in total. Copper acetate (I) (manufactured by Fujifilm Wako Chemical Co., Ltd., melting point 271 ° C.) powder was added as a polymerization catalyst to a chip (granular molded body) of liquid crystal polyester resin (α) (Mp0: 281 ° C.) so that the copper atom equivalent was 50 ppm by weight (copper element content relative to the total amount of resin chips and polymerization catalyst), and the mixture was mixed well with a shaker. The blend of resin chips and polymerization catalyst thus obtained was dried with hot air at 120 ° C. for more than 4 hours, and then melt extruded at a heater temperature of 300 ° C. with a Φ15 mm twin-screw extruder (manufactured by Technovel Co., Ltd., "KZW15TW-45MG-NH (-700)"), and the resin composition was supplied to the spinning head while being metered with a gear pump. At this time, a vacuum pump (Orion Machinery Co., Ltd. dry pump, "KRF40A-V-01B") was connected to a vent part in the middle of the twin-screw extruder via a metal tube, and the space not filled with the resin composition in the twin-screw extruder was decompressed to 60 kPa. The temperature of the spinning head from the extruder outlet was set to 310°C. The spinning head was equipped with a spinneret with a hole diameter of 0.125 mmφ, a land length of 0.175 mm, and 50 holes, and the resin composition was discharged at a discharge rate of 28 g / min and wound around a bobbin at a winding speed of 1000 m / min to obtain a liquid crystal polyester fiber spinning raw yarn. At this time, a 2 wt% aqueous solution of sodium dodecyl phosphate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Wako First Grade) was applied to the spinning raw yarn from an oiling guide arranged directly under the spinning raw yarn. The amount of this aqueous solution applied was 1.4 g / min, and the adhesion ratio of sodium dodecyl phosphate to the spinning raw yarn was calculated to be 0.1 wt%.
[0094] [ka]
[0095] Next, 4 kg of the obtained raw spinning yarn was wound at a winding density of 0.6 g / cm 3The fiber was then rewound onto an aluminum bobbin so that the fiber length was 10 mm, and the fiber was heated from 25° C. to 250° C. in a nitrogen atmosphere in a closed oven over a period of 2 hours, heat-treated at 250° C. for 3 hours, and cooled from 250° C. to 25° C. over a period of 2 hours to obtain a heat-treated liquid crystal polyester filament fiber. The analytical results of the obtained liquid crystal polyester fiber (raw spun fiber and heat-treated fiber) are shown in Table 5.
[0096] [Example 2] Two types of reagents, copper iodide (Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent) and an equimolar amount of 1,10-phenanthroline (Fujifilm Wako Chemical Co., Ltd.) were added to 5 L of acetonitrile (Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent) per mole of copper iodide (I), and the suspension was stirred for 1 hour, filtered, and dried at 100°C for 3 hours to obtain an orange solid (melting point 300°C). Except for using this solid as a polymerization catalyst in place of copper (I) acetate so as to have a copper atom equivalent concentration of 50 ppm by weight, a liquid crystal polyester fiber raw spun yarn and a heat-treated yarn were obtained in the same manner as in Example 1. The analytical results of the obtained liquid crystal polyester fiber (raw spun yarn and heat-treated yarn) are shown in Table 5.
[0097] [Example 3] A liquid crystal polyester fiber raw spun yarn and heat-treated yarn were obtained in the same manner as in Example 1, except that copper (II) acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Wako Grade 1, melting point 115°C) was added as a polymerization catalyst instead of copper (I) acetate to a concentration of 50 ppm by weight in terms of copper atoms. The analytical results of the obtained liquid crystal polyester fiber (raw spun yarn and heat-treated yarn) are shown in Table 5.
[0098] [Example 4] Two types of reagents, copper(II) sulfate pentahydrate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., special grade reagent) and 2 times the molar amount of 1,10-phenanthroline (manufactured by FUJIFILM Wako Chemical Co., Ltd.) relative to copper(II) sulfate pentahydrate, were added to 5 L of acetonitrile (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., special grade reagent) per mole of copper(II) sulfate pentahydrate, and the suspension was stirred for 1 hour, filtered, and dried at 100°C for 3 hours to obtain a blue solid (melting point 294°C). Except for using this solid as a polymerization catalyst in place of copper (I) acetate so as to have a copper atom equivalent concentration of 50 ppm by weight, a liquid crystal polyester fiber raw spun yarn and a heat-treated yarn were obtained in the same manner as in Example 1. The analytical results of the obtained liquid crystal polyester fiber (raw spun yarn and heat-treated yarn) are shown in Table 5.
[0099] [Example 5] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 1, except that cobalt (II) acetate tetrahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Wako special grade, melting point 194°C) was added as a polymerization catalyst instead of copper (I) acetate to a concentration of 50 ppm by weight in terms of cobalt atoms. The analytical results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0100] [Example 6] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 1, except that palladium acetate (II) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Wako special grade, melting point 205°C) was added as a polymerization catalyst instead of copper acetate (I) to a concentration of 50 ppm by weight in terms of palladium atoms. The analytical results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0101] [Example 7] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 1, except that the weight ratio of copper acetate (I) added to the resin was 5 ppm by weight in terms of copper atom. The analysis results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0102] [Example 8] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 1, except that the weight ratio of copper acetate (I) added to the resin was 500 ppm by weight in terms of copper atom. The analysis results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0103] [Example 9] To the chips (granular molded body) of the liquid crystal polyester resin (α) described in Example 1, copper acetate (I) powder (manufactured by Fujifilm Wako Chemical Co., Ltd., melting point 271 ° C.) was added as a polymerization catalyst to 500 ppm by weight in terms of copper atoms, and mixed well with a shaker. The blend of the resin chips and polymerization catalyst thus obtained was dried with hot air at 120 ° C. for 4 hours or more, and then melt extrusion was performed at a heater temperature of 300 ° C. with a Φ15 mm twin-screw extruder (manufactured by Technovel Co., Ltd., "KZW15TW-45MG-NH (-700)"), and the resin composition was supplied to the tip die while being metered with a gear pump. At this time, a vacuum pump (dry pump manufactured by Orion Machinery Co., Ltd., "KRF40A-V-01B") was connected via a metal tube from the vent part in the middle of the twin-screw extruder, and the resin composition non-filled space in the twin-screw extruder was depressurized to 60 kPa. The temperature from the extruder outlet to the tip die at this time was 310 ° C. At the tip die, the resin was extruded in a rod shape from a circular hole of φ3 mm at a discharge rate of 28 g / min, and while taking up this at a winding speed of 5 m / min, the rod-shaped resin composition was cut with a rotary cutter so that the major axis was 5 mm or less to obtain a resin composition chip. The resin composition chip thus obtained (containing 500 ppm by weight of copper) and the liquid crystal polyester resin (α) chip were mixed in a weight ratio of 1:9, mixed well with a shaker, and dried with hot air at 120 ° C for 4 hours or more. The blend of the two types of chips thus obtained was melt-extruded at a heater temperature of 300 ° C with a φ15 mm twin-screw extruder (manufactured by Technovel Co., Ltd., "KZW15TW-45MG-NH (-700)"), and the resin composition was supplied to the spinning head while being metered with a gear pump. At this time, a vacuum pump (Orion Machinery Co., Ltd. dry pump, "KRF40A-V-01B") was connected to a vent part in the middle of the twin-screw extruder via a metal pipe, and the space not filled with the resin composition in the twin-screw extruder was decompressed to 60 kPa. The temperature of the spinning head from the extruder outlet was 310°C. The spinning head was equipped with a spinneret with a hole diameter of 0.125 mmφ, a land length of 0.175 mm, and 50 holes, and the resin composition was discharged at a discharge rate of 28 g / min and wound around a bobbin at a winding speed of 1000 m / min to obtain a liquid crystal polyester fiber spinning raw yarn.At this time, a 2 wt% aqueous solution of sodium dodecyl phosphate (Wako First Grade, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was applied to the raw spinning yarn from an oiling guide arranged directly under the spinneret. The amount of this aqueous solution applied was 1.4 g / min, and the deposition ratio of sodium dodecyl phosphate to the raw spinning yarn was calculated to be 0.1 wt%. Next, 4 kg of the obtained raw spinning yarn was wound at a winding density of 0.6 g / cm 3 The fiber was then rewound onto an aluminum bobbin so that the fiber length was 10 mm, and the fiber was heated from 25° C. to 250° C. in a nitrogen atmosphere in a closed oven over a period of 2 hours, heat-treated at 250° C. for 3 hours, and cooled from 250° C. to 25° C. over a period of 2 hours to obtain a heat-treated liquid crystal polyester filament fiber. The analytical results of the obtained liquid crystal polyester fiber (raw spun fiber and heat-treated fiber) are shown in Table 5.
[0104] [Example 10] A spinning raw yarn was obtained in the same manner as in Example 1, except that a spinneret with a hole diameter of 0.100 mmφ, a land length of 0.140 mm, and 100 holes was used. Then, a heat treatment was performed in the same manner as in Example 1 to obtain a heat-treated yarn. The analysis results of the obtained liquid crystal polyester fiber (spinning raw yarn and heat-treated yarn) are shown in Table 5.
[0105] [Example 11] A spinning raw yarn was obtained in the same manner as in Example 1, except that a spinneret with a hole diameter of 0.150 mmφ, a land length of 0.210 mm, and 20 holes was used. Then, heat treatment was performed in the same manner as in Example 1 to obtain a heat-treated yarn. The analysis results of the obtained liquid crystal polyester fiber (spinning raw yarn and heat-treated yarn) are shown in Table 5.
[0106] [Example 12] A spinning raw yarn was obtained in the same manner as in Example 1, except that a spinneret with a hole diameter of 0.125 mmφ, a land length of 0.175 mm, and 20 holes was used, the resin composition was discharged at a discharge rate of 11.0 g / min, and the amount of sodium dodecyl phosphate aqueous solution applied from the oiling guide was 0.55 g / min. Then, heat treatment was performed in the same manner as in Example 1 to obtain a heat-treated yarn. The analysis results of the obtained liquid crystal polyester fiber (spinning raw yarn and heat-treated yarn) are shown in Table 5.
[0107] [Example 13] Instead of the liquid crystal polyester resin (α) described in Example 1, a liquid crystal polyester resin (β) (Mp0: 348 ° C.) having a molar ratio of each constituent unit shown in the following formula (A) / (C) / (D) / (E) = 65 / 10 / 5 / 20 and a total content of alkali metals and alkaline earth metals of 10 weight ppm or less was used, and the extruder heater temperature during melt extrusion was 360 ° C., and the temperature of the spinning head from the extruder outlet was 360 ° C., except that the spinning raw yarn was obtained in the same manner as in Example 1. Thereafter, the heat treatment temperature of the spinning raw yarn using a closed oven was 290 ° C., and a heat-treated yarn was obtained in the same manner as in Example 1. The analysis results of the obtained liquid crystal polyester fiber (spinning raw yarn and heat-treated yarn) are shown in Table 5.
[0108] [ka]
[0109] [Example 14] Instead of the liquid crystal polyester resin (α) described in Example 1, a liquid crystal polyester resin (γ) (Mp0: 315 ° C.) having a molar ratio of each constituent unit shown in the following formula of (A) / (C) / (D) / (E) / (F) = 54 / 15 / 8 / 16 / 7 and a total content of alkali metals and alkaline earth metals of 10 weight ppm or less was used, and the extruder heater temperature during melt extrusion was 340 ° C., and the temperature of the spinning head from the extruder outlet was 350 ° C., except that the spinning raw yarn was obtained in the same manner as in Example 1. Thereafter, the heat treatment temperature of the spinning raw yarn using a closed oven was set to 260 ° C., and a heat-treated yarn was obtained in the same manner as in Example 1. The analysis results of the obtained liquid crystal polyester fiber (spinning raw yarn and heat-treated yarn) are shown in Table 5.
[0110] [ka]
[0111] [Example 15] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 2, except that the weight ratio of the orange solid (copper (I) iodide, 1,10-phenanthroline) added to the resin was 10 ppm by weight in terms of copper atom. The analysis results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0112] [Example 16] The weight ratio of the orange solid (copper (I) iodide, 1,10-phenanthroline) added to the resin is calculated in terms of copper atoms. 20 Except for using ppm by weight, the liquid crystal polyester fiber raw spun yarn and heat-treated yarn were obtained in the same manner as in Example 2. The analysis results of the obtained liquid crystal polyester fiber (raw spun yarn and heat-treated yarn) are shown in Table 5.
[0113] [Example 17] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 2, except that the weight ratio of the orange solid (copper (I) iodide, 1,10-phenanthroline) added to the resin was 30 ppm by weight in terms of copper atom. The analysis results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0114] [Example 18] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 2, except that the weight ratio of the orange solid (copper (I) iodide, 1,10-phenanthroline) added to the resin was 70 ppm by weight in terms of copper atoms. The analysis results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0115] [Example 19] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 2, except that the weight ratio of the orange solid (copper (I) iodide, 1,10-phenanthroline) added to the resin was 100 ppm by weight in terms of copper atoms. The analysis results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0116] [Example 20] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 2, except that the weight ratio of the orange solid (copper (I) iodide, 1,10-phenanthroline) added to the resin was 150 ppm by weight in terms of copper atoms. The analysis results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0117] [Comparative Example 1] Except for not mixing a polymerization catalyst and using only the chips of the liquid crystal polyester resin (α) as a raw material for spinning, the same procedure as in Example 1 was followed to obtain a liquid crystal polyester fiber raw spun yarn and a heat-treated yarn. The analysis results of the obtained liquid crystal polyester fiber (raw spun yarn and heat-treated yarn) are shown in Table 5.
[0118] [Comparative Example 2] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 1, except that potassium acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent) was added as a polymerization catalyst instead of copper (I) acetate to a concentration of 50 ppm by weight in terms of potassium atom. The analysis results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0119] [Comparative Example 3] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 1, except that N,N-dimethyl-4-aminopyridine (DMAP) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Wako special grade) was added at a weight ratio of 1 wt% as a polymerization catalyst instead of copper (I) acetate. The analysis results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0120] [Comparative Example 4] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 13, except that potassium acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent) was added as a polymerization catalyst instead of copper (I) acetate so as to be 50 ppm by weight in terms of potassium atom. The analysis results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0121] [Comparative Example 5] A liquid crystal polyester fiber raw yarn and a heat-treated yarn were obtained in the same manner as in Example 14, except that potassium acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent) was added as a polymerization catalyst instead of copper (I) acetate so as to be 50 ppm by weight in terms of potassium atom. The analysis results of the obtained liquid crystal polyester fiber (raw yarn and heat-treated yarn) are shown in Table 5.
[0122] [Table 5]
[0123] As shown in Table 5, the raw spinning yarns of Examples 1 to 20 contain specific metal elements, and the catalytic action of these elements allows high-strength heat-treated yarns to be obtained by heat treatment at low temperatures for a short period of time. Furthermore, the specific metal elements used in Examples 1 to 20 can selectively promote reactions in solid-state polymerization and suppress the progression of side reactions that reduce strength, so the resulting heat-treated yarns have excellent heat aging resistance.
[0124] On the other hand, since the raw spun yarn of Comparative Example 1 does not contain a catalyst, solid-state polymerization does not proceed sufficiently by heat treatment at a low temperature for a short time, and a heat-treated yarn with high strength is not obtained. On the other hand, in the heat aging resistance test, solid-state polymerization proceeds due to heating in the test, and the strength is increased.
[0125] The raw spun yarn of Comparative Example 3 contains an organic catalyst used as a polymerization catalyst for synthesizing liquid crystal polyester, but perhaps due to thermal decomposition during melt spinning, solid-state polymerization does not proceed sufficiently in a low-temperature, short-time heat treatment, and a high-strength heat-treated yarn is not obtained, as in Comparative Example 1, which does not contain a catalyst. On the other hand, in the heat aging resistance test, solid-state polymerization proceeds due to heating in the test, and strength increases.
[0126] Comparative Examples 2, 4, and 5 contain alkali metals, and high-strength heat-treated yarns can be obtained by heat treatment at low temperatures and for a short period of time. However, as a catalyst, they not only promote the reaction in solid-state polymerization but also promote side reactions, and therefore in the heat aging resistance test, the strength of these yarns is significantly reduced compared to the heat-treated yarns of Examples 1 to 20, and their heat aging resistance is inferior. [Industrial Applicability]
[0127] The liquid crystal polyester fiber of the present invention can be used for various fiber products such as ropes, nets, fishing nets, sling belts, and tension members.
[0128] As described above, the preferred embodiments of the present invention have been described. However, various additions, modifications, and omissions can be made without departing from the spirit of the present invention, and such additions, modifications, and omissions are also included within the scope of the present invention.
Claims
1. A liquid crystal polyester fiber containing at least one metal element selected from the group consisting of metal elements of Groups 8 to 11 of the periodic table, having a strength of 12 cN / dtex or less, and being subjected to a heat treatment.
2. A liquid crystal polyester fiber containing at least one metal element selected from the group consisting of metal elements in groups 8 to 11 of the periodic table and having a strength of 18 cN / dtex or more.
3. 3. The liquid crystal polyester fiber according to claim 2, wherein the total amount of terminal ends is 20 meq / kg or less.
4. 4. The liquid crystal polyester fiber according to claim 2, wherein the ketone bond amount is 0.05 mol % or less.
5. The liquid crystal polyester fiber according to any one of claims 1 to 4, wherein the total content of the metal elements is 1 to 1000 ppm by weight.
6. The liquid crystal polyester fiber according to any one of claims 1 to 5, wherein the metal element is contained as a metal compound, and the melting point of the metal compound is a melting point of the liquid crystal polyester + 30 ° C or less.
7. A liquid crystal polyester fiber described in any one of claims 1 to 6, wherein the total content of alkali metals and alkaline earth metals is less than 100 ppm by weight.
8. A liquid crystal polyester fiber described in any one of claims 1 to 7, wherein the liquid crystal polyester contained in the liquid crystal polyester fiber is composed of a combination of structural units represented by any one of the following formulas (1) to (16) and (18). [Table 1] [Table 2] [Table 3] In the formula, n is an integer of 1 or 2, and each of the structural units n=1 and n=2 may exist alone or in combination, Y 1 and Y 2 are each independently a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, an aryl group, an aralkyl group, a phenethyl group, an aryloxy group, or an aralkyloxy group, and Z is any of the substituents represented by the following formula: [Formula 1]
9. A method for producing the liquid crystal polyester fiber according to any one of claims 1 to 8, comprising melt-spinning a resin composition containing a liquid crystal polyester and at least one metal element selected from the group consisting of metal elements in Groups 8 to 11 of the periodic table.
10. A method for producing a liquid crystal polyester fiber according to any one of claims 2 to 4 and claims 5 to 8 when dependent on any one of claims 2 to 4, comprising melt spinning a resin composition containing a liquid crystal polyester and at least one metal element selected from the group consisting of metal elements in groups 8 to 11 of the periodic table, and heat treating the raw spun yarn obtained by the melt spinning.
11. The method for producing a liquid crystal polyester fiber according to claim 10, wherein the total amount of carboxy terminals (total amount of CEG) of the raw spinning yarn is 5.0 meq / kg or less.
12. The method for producing a liquid crystal polyester fiber according to any one of claims 9 to 11, wherein the content of the metal elements in the resin composition is 1 to 1000 ppm by weight in total.
13. The method for producing a liquid crystal polyester fiber according to any one of claims 9 to 12, wherein the metal element is contained in the resin composition as a compound having a melting point of the liquid crystal polyester + 30 ° C or less.
14. A fiber structure comprising at least a part of the liquid crystal polyester fiber according to any one of claims 1 to 8.
Citation Information
Patent Citations
Method for producing liquid crystal polyester, and liquid crystal polyester
JP2013067779A
Liquid crystal polymer and resin molded article made of resin composition containing the liquid crystal polymer
JP2020105397A
Polymerization catalyst for polyester, polyester produced with the same, and process for producing polyester
WO2002022707A1
Fully aromatic polyester, and production method therefor
WO2017068867A1
Wholly aromatic polyester and polyester resin composition
WO2020204124A1
Cited By
JPWO2023058563A1