Aqueous adhesive for producing laminated cellulose board containing single-layer graphene oxide, laminated cellulose board obtained using the same, and method for producing the same

A water-based adhesive with graphene oxide nanoplates improves the mechanical and adhesive properties of laminated cellulose boards, addressing recyclability and environmental friendliness, and enhances stability under varying conditions.

JP7577354B2Active Publication Date: 2024-11-05GRAPHENEA SA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022515486
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-09
Filing Date
2020-09-09
Publication Date
2024-11-05
Estimated Expiration
2040-09-09

AI Technical Summary

Technical Problem

Existing adhesives for laminated cellulose boards face challenges in providing recyclability, environmental friendliness, and maintaining adhesive performance, while also ensuring stability under varying environmental conditions.

Method used

A water-based adhesive comprising 20.0% to 40.0% starch, optionally up to 10% natural or synthetic polymers, and 0.1% to 10% graphene oxide nanoplates as an adhesive enhancer, along with additional components like fungicides and stabilizers, is used to enhance adhesive properties.

Benefits of technology

The adhesive exhibits improved mechanical properties and reduced drying time, leading to increased productivity and enhanced resistance to peeling and moisture, with graphene oxide enhancing the adhesive properties and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577354000003
    Figure 0007577354000003
  • Figure 0007577354000004
    Figure 0007577354000004
  • Figure 0007577354000005
    Figure 0007577354000005
Patent Text Reader

Abstract

The present invention relates to a water-based adhesive for the production of laminated cellulose boards, the adhesive comprising single-phase graphene oxide as a glue enhancer. The present invention also relates to a laminated cellulose board obtained therefrom and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of water-based adhesives, and in particular to a method for producing a single-use adhesive for such adhesives. layer The water-based adhesive of the present invention is suitable for the manufacture of laminated cellulose boards, such as cardboard or paper laminates (e.g. cardboard blanks). [Background technology]

[0002] Adhesives are substances that are widely used in many industries for the manufacture of articles and / or materials, and in many cases, adhesives are essential for the successful manufacture of the articles and / or materials.

[0003] Examples of industries requiring adhesives are the paper industry and the production of laminated cellulose boards. Although both industries concern paper, they are essentially different and have different needs with regard to the adhesives used: in the former, cellulose fibres are attached to one another, whereas in the latter, sheets of paper or cardboard are attached to one another. In the paper industry, cellulosic materials are used as raw materials (wood fibres, but also rags, flax, cotton linters, bagasse, etc.) to produce cellulosic products such as pulp, paper, paperboard, etc., whereby adhesives are used to bond the cellulosic fibres. In the production of laminated cellulose boards, such as cardboard, plies of cardboard are usually attached to one another by such adhesives to give multiple layers. However, not only must the plies be attached to one another to give a cardboard blank, but they must also be attached in such a way that the resulting cardboard blank will withstand handling by the user and weather phenomena such as humidity, rain, low and high temperatures. That is to say, the cardboard blank needs to be reliable, and adhesives are highly relevant from this point of view.

[0004] Graphene has been used in many different articles and materials, often because it makes it possible to enhance the functionality or properties of said article or material. In the prior art, several attempts have been disclosed to incorporate graphene oxide into paper pulp to improve some of the properties of the paper, or graphene into cardboard to improve the adhesive properties of the adhesives used in its production.

[0005] For example, US Pat. No. 5,399,633 discloses a water-based adhesive product that can be used to bond various powders, fibers, soils, etc., i.e., for example, in the paper industry. The problem to be solved is to provide a recyclable and environmentally friendly adhesive, while at the same time maintaining good performance. As can be seen in the Examples section, the adhesive materials are mainly synthetic adhesives such as acrylamide, methyl acrylate, potassium acrylate, N,N'-bis(acryloyl)cystamine, and N,N-methylenebisacrylamide, which may be supplemented with polysaccharide materials, which include water-soluble starch. The water-based adhesive further contains a graphite material, which is a simple graphite material. layer It may be selected from graphite oxide, multi-layer graphene oxide, or exfoliated graphite. No specific properties are imposed on the graphite material, and the exemplified adhesive is used only to bond powdered soil, and no paper or cellulosic fibers are disclosed in the examples, much less bonding cellulose boards.

[0006] Patent Document 2 discloses a method for producing weather-resistant, water-resistant, and high-quality specialty printing paper, which includes preparing a pulp, producing paper therewith, and applying an adhesive layer thereto. In the step of preparing the pulp, a solubilizer composition is added, which contains all of graphene quantum dots, nano-silica, and nano-titanium dioxide. The graphene quantum dots are monolithic nanoparticles prepared by a microwave stripping method. layer Graphene oxide quantum dots. layerIt is disclosed that graphene oxide quantum dots provide good surface modification effect, while silica can effectively improve the adhesion of papermaking fibers and improve the folding resistance and mechanical properties of paper.

[0007] Patent document 3 instead discloses an adhesive for the production of laminates of cellulose products, i.e. for the production of laminated cellulose boards. The adhesive is produced by adding graphene nanofilaments to a mixture of water and starch. The added nanofilaments have a diameter in the range of 1 to 100 nanometers and a length of more than 30 micrometers. Such nanofilaments, however, do not mix well with water or aqueous solutions. Therefore, the mixture is not really stable and has to be used within a short time after preparation, and the adhesive properties of the adhesive to which they are added are not significantly improved, probably due to insufficient mixing with water. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] China Patent Application Publication No. 106381104 [Patent Document 2] China Patent Application Publication No. 108914675 [Patent Document 3] European Patent Application Publication No. 2886621 Summary of the Invention [Problem to be solved by the invention]

[0009] Therefore, there remains an interest in providing adhesives that can overcome the shortcomings of prior art solutions and that are useful in producing laminated cellulose boards. [Means for solving the problem]

[0010] The present invention relates to a water-based adhesive for the manufacture of laminated cellulose boards, comprising: 1) Water, 2) 20.0% by weight to 40.0% by weight of starch; 3) optionally up to 10% by weight of at least one additional polymer selected from natural polymers or soluble synthetic polymers; 4) A paste strengthening agent that is dissolved in water and layer The water-based adhesive contains 0.1% by weight to 10 -7 Weight percent layer A sizing agent comprising an amount of graphene oxide, 5) at least one further component, which, depending on the polymer, is selected from fungicides and biocides and / or stabilizers, gelling agents, thickeners, defoamers, tackifiers, moisture-proof resins, rheology agents, The present invention relates to a water-based adhesive comprising: [Brief description of the drawings]

[0011] To complete this specification and to provide a better understanding of the invention, a series of drawings are provided. Said drawings form an integral part of this specification and illustrate embodiments of the invention, which should not be construed as limiting the scope of the invention, but merely as examples of how the invention can be practiced. The drawings include the following figures:

[0012] [Figure 1] FIG. 1 shows a laminated cellulose cardboard containing five layers. [Diagram 2] FIG. 1 shows a laminated cellulose cardboard comprising three layers. [Diagram 3] Figure 3 shows the results of a dry peel test carried out with samples: Figure 3 corresponds to a dry peel test carried out with cardboard prepared with an adhesive without a glue enhancer according to the invention. [Figure 4]Figure 4 shows the results of a dry peel test carried out with different samples than in Figure 3. Figure 4 corresponds to a dry peel test carried out with cardboard prepared with an adhesive containing a glue enhancer according to the invention. [Diagram 5] 1A-1D are schematic illustrations of adhesives obtained by some of the different preparation methods mentioned above. [Figure 6a] FIG. 2 is a schematic diagram showing the steps of the Steinhall process described above. [Figure 6b] FIG. 2 is a schematic diagram showing the steps of the Steinhall process described above. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] According to a first aspect, the present invention relates to a water-based adhesive for the manufacture of laminated cellulose boards, comprising: 1) Water, 2) 20.0% by weight to 40.0% by weight of starch; 3) optionally up to 10% by weight of at least one additional polymer selected from natural polymers or soluble synthetic polymers; 4) A paste strengthening agent that is dissolved in water and layer The water-based adhesive contains 0.1% by weight to 10 -7 Weight percent layer A sizing agent comprising an amount of graphene oxide, 5) at least one component selected from mildewcides and biocides, and / or stabilizers, gelling agents, thickeners, defoamers, tackifiers, moisture-proof resins, and rheology agents, depending on the polymer; The present invention relates to a water-based adhesive comprising:

[0014] According to a particular embodiment, the starch may be present in the water-based adhesive in an amount of 20-32% by weight, such as 25-30% by weight.

[0015] The starch may be, for example, corn starch, wheat starch, potato starch, pea starch, tapioca starch, or one of their mixtures.

[0016] The starch may be chemically modified to enable the starch to perform properly under conditions frequently encountered during processing or storage, such as high heat, high shear, low pH, freeze / thaw, and cooling.

[0017] The at least one component 5) may be, for example, borax powder and a mixture of calcium hydroxide and sodium carbonate, which when dissolved in water gives caustic soda (sodium hydroxide). Sodium hydroxide promotes the penetration of the glue into the paper and reduces the gel time. Borax powder stabilizes the glue by reacting with cooked starch and improves the adhesiveness of the glue and its penetration into the paper. Borax powder further helps to give an optimal rheology. The concentration of sodium hydroxide in the adhesive may be 1.5-3.0% by weight and the concentration of borax in the adhesive may be 1-2% by weight.

[0018] Other additional components 5) may be, for example, at least one of urea-formaldehyde to improve moisture resistance, polyvinyl alcohol or polyvinyl acetate to improve cold water resistance, or a biocide to inhibit mold growth.

[0019] In the water-based adhesive defined above, the natural polymer is selected from vegetable, protein or animal sources, in particular from dextrin, starch or albumin, or from any polymer extracted from casein, blood, fish, soybean, hide or bone, and the soluble synthetic polymer is selected from polyvinyl alcohol, cellulose ethers, methylcellulose, carboxymethylcellulose, polyvinylpyrrolidone, urea-formaldehyde blends and melamine-formaldehyde blends.

[0020] The water-based adhesive may comprise just one additional polymer or a mixture of two or more polymers.

[0021] The remainder to 100% by weight is water.

[0022] The above single layer Graphene oxide was synthesized according to the method disclosed in EP15382123, which is incorporated herein by reference for its method of preparation of graphene oxide. Generally speaking, the procedure is based on a modified Hummers process, where the oxidation reaction and post-exfoliation process are carried out using a high shear mixer. This method exfoliates graphene oxide simultaneously with the reaction, improving the yield, oxygen content, and simple structure. layer The content is higher than that obtained using the standard stirring method. layer Graphene oxide is in the form of nanoplates as defined in ISO / TR18401:2017. Therefore, the single graft used to prepare the adhesive of the present invention layer Graphene oxide is a form of such a nanoplate. The referenced ISO standards provide definitions and classifications of nano-articles based on their size and shape. Nano-articles are typically described or classified with respect to dimensions constrained to the nanoscale. As such, if one dimension is nanoscale but the other two dimensions are larger than nanoscale, the article is known as a nanoplate. If two dimensions are nanoscale, the article is known as a nanofiber, which includes nanotubes. If all three dimensions are nanoscale, the article is known as a nanoparticle or quantum dot.

[0023] The moisture resistant resin may be, for example, ketone-formaldehyde, urea-formaldehyde, or resorcinol.

[0024] In the aqueous adhesive according to the present invention, layer Graphene oxide is used as an adhesive enhancer. Thus, a further aspect of the present invention is layerThe use of graphene oxide as an adhesive enhancer for water-based adhesives for the manufacture of laminated cellulose boards. layer Graphene oxide is a form of nanoplates as defined in ISO / TR18401:2017.

[0025] Preferred components 5) are caustic soda and / or borax. The preferred amount of caustic soda is 1.5-3% by weight relative to the weight of starch, and the preferred amount of borax is 1-2% by weight relative to the weight of starch.

[0026] A third aspect of the present invention is a method for producing a water-based adhesive for the manufacture of a laminated cellulose board of the present invention as defined above, the method comprising the steps of mixing starch, water and a glue enhancer, the glue enhancer being present in a concentration of 0.1% by weight to 0.001% by weight. layer The graphene oxide is suspended in water. layer The graphene oxide is preferably in the form of nanoplates as defined in ISO / TR18401:2017.

[0027] For example, the method comprises: a) mixing starch into a first aqueous solution under stirring and at a temperature between 20.0°C and 30.0°C to obtain a first mixture containing 20.0% to 40.0% by weight of starch; b) adding a paste enhancer to the first mixture under stirring, the paste enhancer being a single component of 0.1% by weight to 0.001% by weight. layer A second water-based composition containing graphene oxide, whereby the composition contains 0.1% by weight to 10 -7 Weight percent layer Producing a second mixture comprising graphene oxide; Includes.

[0028] The second mixture may be used directly as a water-based adhesive.

[0029] The single unit in the second mixture layer The concentration of graphene oxide in the mixture was layer In order to reduce the cost of graphene oxide, it is preferable to use a graphene oxide concentration of 0.001% by weight to 10 -7 % by weight, and even more preferably 10 -5 Weight%~10 -7 As indicated above, the single layer The graphene oxide is preferably in the form of nanoplates as defined in ISO / TR18401:2017.

[0030] According to a further embodiment, the temperature in step a) is between 24.0°C and 26.0°C, preferably between 24.5°C and 25.5°C.

[0031] Further embodiments provide for stirring the first mixture in step a) for at least 20 minutes and / or stirring the second mixture in step b) for at least 10 minutes.

[0032] Said adhesives may be prepared by different methods known in the state of the art.

[0033] For example, it may be prepared by the method known as "Steinhall", which provides a two-phase adhesive consisting of a starch solution in which a raw, uncooked starch, i.e., a second starch, is suspended in a first starch, called the carrier. The carrier is prepared by the combined action of heat and caustic soda on the starch slurry. This provides the necessary viscosity to retain the water necessary for the gelatinization of the second starch, and controls the absorption into the paper as well as the initial adhesive strength.

[0034] A further preparation method that may be used is the "no carrier" process. This process provides a single phase adhesive. Most of the starch granules are partially swollen and the mixture is sufficiently viscous to prevent settling. The starch slurry gradually swells when exposed to precise heat and alkali conditions, and the swelling reaction is stopped with boric acid at the required viscosity.

[0035] Minocar is a further process that may be used. The Minocar process is an extension of the no-carrier process, which provides a two-phase adhesive, in which raw, uncooked starch is suspended in a first portion of mostly partially swollen granules.

[0036] A further adhesive to which the glue enhancer according to the invention may be added is "one bag mix" (OBM) starch, which is a blend of several components that when mixed with water form Steinhall glue. The main components are: a pre-gelatinized (cooked and dried) starch which dissolves in water to form a first carrier component of the paste; a native starch that has not been heat treated, the starch being the second starch portion of the paste; a mixture of calcium hydroxide and sodium carbonate which forms sodium hydroxide (caustic soda) when dissolved in water; Borax powder, It is.

[0037] The primary reason for using OBM is its ease of use, especially in situations where preparation facilities are limited.

[0038] A further process is the Steinhall process, which gives a two-phase adhesive consisting of a starch solution in which a second starch, which is a raw, uncooked starch (approximately 80-90% by weight of the total starch), called the carrier, is suspended in a first starch (approximately 10-20% by weight of the total starch). The carrier is prepared by the combined action of heat and caustic soda (approximately 1.4-3% by weight) on the starch slurry. Approximately 1-2% by weight of borax is generally added.

[0039] The adhesive of the invention as defined or obtained above may be used, for example, in the manufacture of laminated cellulose boards.

[0040] The added single layer Graphene oxide surprisingly and unexpectedly enhances the adhesive properties obtained from polymers, such as starch, and therefore enhances the adhesive properties of the adhesive produced. Furthermore, the presence of oxygen groups in graphene oxide appears to make it possible to disperse graphene oxide within the adhesive, improving its adhesive properties.

[0041] The resulting adhesives exhibit reduced drying times compared to the drying times of adhesives without graphene oxide, which in turn leads to increased productivity since articles with such adhesives require less time to manufacture.

[0042] The mechanical properties of the products to which the adhesive is applied, such as single-walled cardboard, simple-walled cardboard, double-walled cardboard, etc., are also improved due to the adhesive. Some mechanical properties have been determined by FEFCO test method no. 9 (https: / / find-k.ru / images / FEFCO%209.pdf), i.e., a method for determining the water resistance of glue bonds of laminated cellulose corrugated boards by immersion. Dry peeling, i.e., resistance to detachment of the cellulose layer, was also tested using a dynamometer. Details are given in the examples and figures.

[0043] Besides standard laminated cellulose boards, other products can also be produced with the adhesive according to the invention, such as semi-chemical and plastic papers.

[0044] The main component for the production of corrugated board is paper. Depending on the type of application and their characteristics, papers used in corrugated board production are divided into two groups: Paper for the flat layer, i.e., liner, and Paper for corrugated layers, i.e. fluting, It can be divided into: Depending on their manufacturing process and composition, liners are divided into two main groups: Kraftliner, and Test liner, It belongs to one of the following. Kraft liners have the best strength parameters of all liners. They are composed of cellulose pulp with a small addition of recycled fibers. The overcoat is usually better sized and has a higher smoothness.

[0045] Topliner (white kraft liner) is a grade of kraft liner. The overcoat is often made of bleached kraft pulp, while the bottom layer is made of unbleached stock. For more advanced imprints, white coated kraft liners are used, and the overcoat is often coated with a pigment coating.

[0046] Testliners are two-ply papers, most often made from 100% recycled paper. Testliners are a combination of two layers. This construction allows the use of kraft pulp for the top layer and recycled fibers for the bottom layer. Due to the price relationship between expensive cellulose mass and cheap papermaking stock, there is a continuous increase of the latter in testliner formulations. They are increasingly made entirely from recycled fibers. In such cases, the top layer is dyed to limit the color of the kraft pulp. As with kraft liners, testliners are produced with a white top layer of similar whiteness. For a more sophisticated print, coated testliners are produced, where the top layer is most often coated with a pigment coating.

[0047] In addition to the above-mentioned plain paper, special papers having special properties are also applicable. Wet strength (modified after wetting to ensure strength properties are maintained (PN-P-50000:1992)); Fat Tite papers (high resistance to penetration by grease and oil, some of these papers are particularly resistant to penetration by the substances mentioned above (PN-P-50000:1992)), Barrier coated paper (having a protective layer, e.g. of polyethylene (PE), covering one or both sides of the paper (PN-EN26590-1:1993)); Fireproof paper (flame-resistant and / or ignition-resistant (PN-P-500000:1992)) Examples include: The papers for fluting in corrugated board are divided into two groups: Waste-Based Fluting (WBF), and Semi-chemical fluting (SC) It can be divided into: WBF is made exclusively from recycled fibers. To improve the mechanical properties of such fluting, starch is added to the structure. This process is commonly described as bonding. It can be done "in stock" (i.e. sizing, where starch is introduced into waste paper pulp) or starch can additionally be applied on the paper surface (surface sizing).

[0048] The semi-chemical fluting contains about 70% semi-chemical pulp, which is produced from hardwood (mostly birch) during the pulping process. The remainder of the pulp consists mostly of waste paper.

[0049] The adhesive according to the present invention may also be applied to any of the papers mentioned above.

[0050] A further aspect of the present invention is a method for producing a laminated cellulose board comprising the steps of: i) providing at least two cellulose plies; ii) a cellulose ply having a single layer on at least a portion of its surface; layer applying an adhesive of the present invention comprising graphene oxide; iii) contacting a surface of a further cellulose ply with a surface of the first cellulose ply of step ii); iv) optionally repeating steps ii) and iii) one or more times to obtain a laminated cellulose board; The method includes:

[0051] In the above method, step iii) may further comprise applying to at least a part of a surface of the further cellulose ply an adhesive according to any one of claims 1 to 4. That is to say, the adhesive is applied to at least a part of both surfaces to be joined together. Methods for applying the adhesive to the cellulose ply are known in the art, a preferred method being roll coating.

[0052] The cellulosic ply, according to one embodiment, may be a paper or cardboard ply.

[0053] The present invention also relates to a laminated cellulose board obtainable by the above-mentioned method.

[0054] The present invention further relates to a laminated cellulose board comprising at least two cellulose plies attached to one another, said at least two cellulose plies being bonded to one another with an adhesive according to the present invention, i.e. layer The present invention relates to laminated cellulose boards, characterized in that they are attached to one another by an adhesive comprising graphene oxide.

[0055] In the above laminated cellulose board, at least one of the cellulose plies may be a corrugated ply, thus providing a laminated corrugated cellulose board.

[0056] In the above laminated cellulose board, at least one of the cellulose plies may be a laminate paper.

[0057] FIG. 1 shows a laminated cellulose corrugated board having a number of plies, in particular five plies, numbered 25 to 29, which plies are coated with an adhesive, for example an adhesive according to the invention, i.e. layer They are attached to each other by an adhesive that includes graphene oxide.

[0058] The laminated cellulose corrugated board comprises a first planar ply 25, a first wavy ply 26 attached below the first planar ply 25, a second planar ply 27 attached below the first wavy ply 26, a second wavy ply 28 attached below the second planar ply 27, and a third planar ply 29 attached below the second wavy ply 28. In this particular embodiment, the first wavy ply 26 has smaller fluting than the fluting of the second wavy ply 28. This should not be considered as a limitation of the invention in any case, since the fluting of the different wavy plies may be the same or different.

[0059] One of the two main surfaces of the first and third planar plies 25 and 29 (i.e., outer liners) is attached by adhesive to the main surfaces of the first and second wavy plies 26 and 28, respectively. Each of the second planar ply 27, the first wavy ply 26, and the second wavy ply 28 has its two main surfaces attached by adhesive to the main surface of another ply. Depending on the properties of the adhesive, the plies are glued together with more or less adhesiveness. The adhesive and adhesiveness affect the mechanical properties of the laminated cellulose corrugated board 20, since the resistance of a ply can be increased by the resistance of the other plies, which depends, among other characteristics, on how strongly the plies are glued together.

[0060] It is readily apparent that other laminated cellulose boards (both corrugated and non-corrugated) are possible within the scope of the present invention, for example, laminated cellulose corrugated boards having a first flat ply and a first wavy ply, or having a first flat ply, a first wavy ply and a second flat ply, or having additional flat and / or wavy plies, etc. Furthermore, the fluting of the wavy plies may be the same or different. It is also readily apparent that laminated cellulose boards may be prepared using different types of paper or cardboard, such as semi-chemical paper, kraft paper, or plastic paper.

[0061] FIG. 2 shows a laminated cellulose corrugated board including three plies, specifically a first flat ply, a wavy ply attached underneath the first flat ply, and a second flat ply attached underneath the wavy ply.

[0062] Figure 3 shows a laminated cellulose corrugated board having three plies as described with reference to Figure 2, which are glued with an adhesive without a glue enhancer according to the invention. As can be observed, the first flat ply separates very simply from the wavy ply without delamination of the plies, which is due to the weak adhesion of the plies to each other.

[0063] In figure 4 a laminated cellulose corrugated board having three plies as described with reference to figure 2 is shown, the plies being glued with an adhesive comprising a glue enhancer according to the invention. As can be observed, the first flat ply delaminates in this case (i.e. both the flat and the corrugated ply break), due to the strong adhesion resulting from the glue enhancer according to the invention contained in the adhesive used to attach the plies to each other. EXAMPLES

[0064] In the following, the present invention will be further illustrated by examples and comparative examples. In any case, the examples should not be construed as limiting the scope of the present invention, but merely as illustrative of the present invention.

[0065] Example 1: Preparation of adhesive according to the present invention The adhesive is prepared as follows: 1800 L of water is provided, the volume of water is heated to 25.0° C., 550 kg of modified starch is added, the mixture is stirred for 20 minutes, 1.5 L of glue enhancer is added to the mixture, and the solvent is water and 0.01% by weight of a simple glycerol. layer The resulting mixture is stirred for 10 minutes. The resulting exemplary adhesive thus contains approximately 0.0000064% by weight of graphene oxide. layer It has graphene oxide.

[0066] <Example 2: Dry peel test> With and without the adhesive according to the invention, i.e. layer Several samples of laminated cellulose corrugated board, with and without graphene oxide, were subjected to dry peel tests in which two plies glued together were pulled apart. The average load required to separate the two plies over the length of the specimen was recorded and expressed in N.

[0067] In particular, the dry peel test was carried out on a board comprising three layers as shown in Figure 2. The three layers are: Top ply: Flat ply: T14; Paper type: Test, grammage 140g Middle ply: wavy ply, fluting SQ15; Paper type: semi-chemical, grammage 150g Lower ply: T14; Paper type: Test, grammage 140g.

[0068] Sample 1 is a laminated cellulose corrugated board according to the above, prepared with a glue or adhesive that does not contain a glue enhancer according to the invention.

[0069] Sample 2 is a laminated cellulose corrugated board according to the above, prepared with a glue or adhesive containing a glue enhancer according to the invention.

[0070] The results of the tests are shown in Table 1, where two rows of values ​​are shown, the first row corresponding to the dry peel between the upper flat ply and the middle corrugated ply, and the second row corresponding to the dry peel between said corrugated ply and the lower flat ply.

[0071] [Table 1]

[0072] In sample 2, i.e. the sample with the glue booster according to the invention, the dry peel between the top flat ply and the wavy ply results in delamination (see FIG. 4). The delamination is the result of the high strength of the adhesive, and both the flat and wavy plies break.

[0073] In contrast, for sample 1, ie, the sample without the glue enhancer according to the present invention, the measured dry peel force between the upper plain ply and the corrugated ply was 7.93N.

[0074] In a dry peel test between the corrugated ply and the underlying flat ply, Sample 2 required a force of 4.74 N for dry peeling, which was greater than the force for dry peeling of Sample 1 (2.13 N).

[0075] Thus, in both cases, the resistance to dry peel of sample 2 (with glue enhancer) is greater than that of sample 1 (without glue enhancer) (see Figure 4 vs. Figure 3, delamination vs. peel without delamination).

[0076] <Example 3: Determination of water resistance of glue bond: FEFCO test method #9> The water resistance of the glue bonds of laminated cellulose corrugated boards made with and without adhesives containing the glue enhancer of the present invention by immersion is also tested according to FEFCO test method #9. The water resistance of the corrugated board glue is expressed by the length of time that a given combination of glue lines immersed in water will withstand the pull of a suspended weight (having a mass of 250 grams) in a plane perpendicular to the glue lines and perpendicular to the axis of the cellulose board.

[0077] In particular, the dry peel test was carried out on a board comprising five layers according to Figure 1. The five layers, listed from top to bottom, were: Top outer flat ply: T200; Paper type: Test, grammage 200g 1st wavy ply: small fluting, SQ150; Paper type: semi-chemical, grammage 150g Middle ply (middle liner): T140; Paper type: Test, grammage 140g Second wavy ply: large fluting, SQ150; Paper type: semi-chemical, grammage 150g Lower outer flat ply: T200; Paper type: Test, grammage 200g.

[0078] Sample 3 is a laminated cellulose corrugated board according to the above, prepared with a glue or adhesive that does not contain a glue enhancer according to the invention.

[0079] Sample 4 is a laminated cellulose corrugated board according to the above, prepared with a glue or adhesive containing a glue enhancer according to the present invention.

[0080] It can be seen in Table 2 that sample 4 (having an adhesive containing a glue enhancer according to the invention) is characterized by a longer time until it breaks compared to sample 3 (having an adhesive without a glue enhancer), in which the water resistance between each pair of plies is measured and the standard deviation of the measured times in the different tests is also shown.

[0081] [Table 2]

[0082] In this context, although terms such as first, second, etc. are used herein to describe certain substances or elements, it will be understood that these substances or elements should not be limited by these terms, as these terms are only used to distinguish one substance or element from another substance or element.

[0083] In this context, the term "comprise" and its derivatives (such as "comprising") should not be understood in an exclusive sense, i.e., these terms should not be interpreted as excluding the possibility that what is described and defined may include further elements, steps, etc.

[0084] On the other hand, the present invention is obviously not limited to the particular embodiments described herein, but also encompasses any variations (e.g., regarding the selection of materials, dimensions, components, configurations, etc.) that may be conceived by a person skilled in the art within the general scope of the invention as defined in the claims.

Claims

1. 1. A water-based adhesive for the manufacture of laminated cellulose boards, comprising: 1) Water; 2) 20.0% to 40.0% by weight of starch; 3) optionally up to 10% by weight of at least one additional polymer selected from natural polymers or soluble synthetic polymers; 4) A glue enhancer, comprising: a single-layer graphene oxide in water; and a water-based adhesive having a viscosity of 0.1% by weight to 10% by weight. -7 % by weight of monolayer graphene oxide; and 5) at least one further component, which, depending on the polymer, is selected from fungicides and biocides and / or stabilizers, gelling agents, thickeners, defoamers, tackifiers, moisture-proof resins, rheology agents; A water-based adhesive comprising:

2. 2. The water-based adhesive according to claim 1, characterized in that the at least one further component 5) is borax and NaOH or a mixture of calcium hydroxide and sodium carbonate.

3. 3. The water-based adhesive according to claim 1 or 2, characterized in that the starch is corn starch, wheat starch, potato starch, pea starch, tapioca starch or a mixture thereof.

4. 4. The water-based adhesive according to claim 1, wherein the at least one further polymer is a natural polymer selected from vegetable, protein or animal sources, preferably selected from dextrin, starch or albumin, or from any polymer extracted from casein, blood, fish, soy, hide or bone.

5. 5. The water-based adhesive according to claim 1, wherein the at least one further polymer is a soluble synthetic polymer selected from polyvinyl alcohol, cellulose ethers, methyl cellulose, carboxymethyl cellulose, polyvinylpyrrolidone, urea-formaldehyde blends and melamine-formaldehyde blends.

6. The water-based adhesive according to any one of claims 1 to 5, characterized in that the single-layer graphene oxide is in the form of nanoplates as defined in ISO / TR18401:2017.

7. 6. Use of monolayer graphene oxide as a glue enhancer for a water-based adhesive for the manufacture of laminated cellulose boards, characterized in that the water-based adhesive comprises starch and optionally at least one further polymer, the at least one polymer being selected from natural polymers or soluble synthetic polymers, and the water-based adhesive is as defined in any one of claims 1 to 5.

8. 8. The use of single-layer graphene oxide according to claim 7, characterized in that the single-layer graphene oxide is in the form of nanoplates as defined in ISO / TR18401:2017.

9. 7. A method for producing a water-based adhesive according to any one of claims 1 to 6, comprising the steps of mixing starch, water and a glue enhancer, characterized in that the glue enhancer is a suspension of 0.1 wt.% to 0.001 wt.% of single layer graphene oxide in water.

10. 10. The method of claim 9, a) mixing starch in water under stirring and at a temperature between 20.0°C and 30.0°C to obtain a first mixture comprising 20.0% to 40.0% by weight of starch; b) adding a glue booster to the first mixture under stirring, the glue booster being a suspension of 0.1 wt. % to 0.001 wt. % single layer graphene oxide in water, whereby 0.1 wt. % to 10 -7 producing a second mixture comprising: A method comprising:

11. 11. The method of claim 10, wherein in step a) the first mixture is stirred for at least 20 minutes and in step b) the second mixture is stirred for at least 10 minutes.

12. 1. A method for producing a laminated cellulose board, comprising: i) providing at least two cellulose plies; ii) applying to at least a portion of a surface of the cellulose ply an adhesive according to any one of claims 1 to 6; iii) contacting a surface of a further cellulose ply with the first cellulose ply of step ii); iv) optionally repeating steps ii) and iii) one or more times to obtain a laminated cellulose board; A method comprising:

13. The method according to claim 12, characterized in that step iii) further comprises applying an adhesive according to any one of claims 1 to 6 to at least a part of a surface of the further cellulose ply.

14. 14. The method of claim 12 or 13, characterized in that the cellulose ply is a paper or cardboard ply.

15. A laminated cellulose board comprising at least two cellulose plies attached to one another, characterized in that the at least two cellulose plies are attached to one another by an adhesive according to any one of claims 1 to 6.

16. A laminated cellulose board according to claim 15 or obtainable by the method according to any one of claims 12 to 14, wherein at least one of the cellulose plies is a corrugated ply.

17. A laminated cellulose board according to any one of claims 15 and 16 or obtainable by the method according to any one of claims 12 to 14, wherein at least one of the cellulose plies is a laminate paper.

Citation Information

Patent Citations

  • Water-based adhesive and preparation method thereof

    CN106381104A

  • Manufacturing method of weather-resistant, waterproof and high-quality special paper for printing

    CN108914675A

  • Adhesive for the manufacture of laminates of cellulose products and manufacturing procedures of laminates of cellulose products

    EP2886621A1

  • Manufacture of corrugated cardboard

    JP1982056242A

  • High solid adhesive for corrugated cardboard

    JP1989110579A