Method for producing bioabsorbable cotton-like material
The method of melt spinning polyglycolide threads and applying woolly processing addresses the challenge of creating bioabsorbable cotton-like materials with high water absorption for surgical use, ensuring effective fluid absorption and safety.
Patent Information
- Application Number
- JP2021022640
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-16
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-02-16
AI Technical Summary
Conventional bioabsorbable medical supplies are difficult to make into cotton-like materials and have low water absorption, posing safety and effectiveness issues in surgical applications.
A method involving melt spinning of polyglycolide into threads and applying woolly processing to create a bioabsorbable flocculent with high water absorption, mimicking the properties of cotton.
The produced bioabsorbable flocculent exhibits high water absorption and safety by being fully absorbed into the body, effectively absorbing body fluids during surgical operations.
Smart Images

Figure 0007577561000002 
Figure 0007577561000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a bioabsorbable cotton-like material, which is capable of producing a bioabsorbable cotton-like material having high water absorbency. [Background technology]
[0002] In the medical field, bioabsorbable materials are sometimes used as materials for surgical tools. By using bioabsorbable materials, they are absorbed into the body and disappear after fulfilling their role, so there is no need to perform another surgery to remove them, and safety can be improved. Specifically, nonwoven fabrics made of bioabsorbable materials such as those disclosed in Patent Document 1 are used as substrates to prevent leakage of body fluids and air. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-315561 Summary of the Invention [Problem to be solved by the invention]
[0004] Meanwhile, cotton is routinely used in the medical field for a variety of purposes. For example, cotton is used in surgical procedures to absorb bodily fluids. Since the cotton used in such surgical procedures may be forgotten to be removed, there is an increasing demand for cotton made of bioabsorbable materials to ensure safety in the event that the cotton is forgotten to be removed. However, most medical supplies made of conventional bioabsorbable materials are in the form of flat nonwoven fabrics or solids, and there is a problem that they are difficult to make into a cotton-like form. In addition, medical supplies made of conventional bioabsorbable materials have a problem of low water absorption, making it even more difficult to obtain a highly water-absorbent bioabsorbable cotton-like body.
[0005] In view of the above problems, an object of the present invention is to provide a method for producing a bioabsorbable cotton-like material, which is capable of producing a bioabsorbable cotton-like material with high water absorbency. [Means for solving the problem]
[0006] The present invention is a method for producing a bioabsorbable cotton-like material for medical use, which includes a step of forming polyglycolide into thread by melt spinning and a step of subjecting the thread to a woolly process. The present invention will be described in detail below.
[0007] As a result of extensive research, the present inventors discovered that a bioabsorbable material can be made cotton-like by subjecting thread made of polyglycolide to a woolly process, and thus completed the present invention.
[0008] The method for producing a bioabsorbable cotton-like material of the present invention first involves a step of forming polyglycolide into threads by melt spinning. By using polyglycolide as a material, it is possible to impart bioabsorbability to the resulting cotton-like material. In addition, since polyglycolide decomposes relatively quickly, it can be absorbed into the body in a short period of time. Furthermore, by using polyglycolide, it is possible to achieve physical properties closer to those of cotton. Note that the cotton-like material referred to here is a material in which fibers are entangled to form a lightweight mass with low density.
[0009] The thickness of the thread is not particularly limited, but is preferably 1.0 μm or more and 30 μm or less. By setting the thickness of the thread within the above range, the handleability of the obtained cotton-like material can be improved and the physical properties can be made closer to those of cotton. The thickness of the thread is more preferably 5 μm or more and more preferably 20 μm or less.
[0010] The melt spinning method is not particularly limited, and any conventionally known method and conditions can be used without particular limitation.
[0011] The weight average molecular weight of the polyglycolide is not particularly limited, but is preferably 30,000 or more and 200,000 or less. The strength of the obtained bioabsorbable cotton-like material can be increased by making the weight-average molecular weight of polyglycolide 30,000 or more, and the decomposition rate can be increased by making the weight-average molecular weight of polyglycolide 200,000 or less. The weight-average molecular weight of the polyglycolide is more preferably 50,000 or more, and more preferably 150,000 or less.
[0012] The method for producing a bioabsorbable cotton-like material of the present invention then includes a step of subjecting the thread to a woolly finish. Woolly processing refers to a process in which fibers are twisted, heated, and then untwisted. Woolly processing causes the fibers to shrink and become bulky, so by applying woolly processing to threads made of polyglycolide and bundling them together, the shape can be made cotton-like.
[0013] The heating temperature in the woolly processing is preferably 50°C or higher and 200°C or lower. By setting the heating temperature within the above range, the yarn can be sufficiently crimped, and the physical properties of the resulting cotton-like material can be made closer to those of cotton. The heating temperature is more preferably 70°C or higher and more preferably 150°C or lower.
[0014] The bioabsorbable cotton-like material obtained by the method for producing a bioabsorbable cotton-like material of the present invention is used in the medical field. The bioabsorbable cotton-like material obtained by the present invention has excellent water absorption properties, and is therefore very effective in applications such as packing it around an affected area in a surgical operation to absorb bodily fluids. Since the bioabsorbable cotton-like material obtained by the present invention is bioabsorbable, even if it remains in the body, it will eventually be absorbed and disappear, making it highly safe. Effect of the Invention
[0015] According to the present invention, there is provided a method for producing a bioabsorbable cotton-like material, which is capable of producing a bioabsorbable cotton-like material with high water absorbency. [Brief description of the drawings]
[0016] [Figure 1] 1 is a photograph comparing the bioabsorbable cotton-like materials of Example 1 and Comparative Example 1, the polyester cotton of Reference Example 1, and the organic cotton of Reference Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The following describes the embodiments of the present invention in more detail, but the present invention is not limited to these embodiments.
[0018] Example 1 A melt spinning method was used to obtain threads made of polyglycolide with a weight-average molecular weight of 200,000. The obtained polyglycolide was then subjected to woolly processing using a friction tester at a twist number of 2,000 T / m and a set temperature of 140°C, and the threads were cut at regular intervals and then bundled together to obtain bioabsorbable cotton-like materials.
[0019] Comparative Example 1 A bioabsorbable cotton-like material was obtained in the same manner as in Example 1, except that the woolly processing was not carried out.
[0020] (Reference example 1) Polyester cotton (100% polyester cotton, Craft Cotton (SW-300) manufactured by Kiyohara Co., Ltd.) was used as is.
[0021] (Reference example 2) Cotton (100% organic cotton) was used as is.
[0022] <Physical Properties> The following measurements were carried out on the bioabsorbable cotton-like materials obtained in the Examples and the cotton of the Reference Examples. The results are shown in Table 1.
[0023] (Measurement of specific volume) The specific volume, compressibility and recovery rate of the bioabsorbable cotton-like material and cotton were measured according to the method of JIS L 1097. The results are shown in Table 1. Specifically, the obtained bioabsorbable cotton-like material or cotton was first cut into a sample of 20 x 20 cm, and stacked until the mass reached about 40 g to obtain a test piece. The obtained test piece was then left for 1 hour and weighed. Next, a 14 g thick plate was placed on the test piece, and a 63 g weight A was placed on it for 30 seconds, after which the weight A was removed and the test piece was left for 30 seconds. This operation was repeated three times, and the heights of the four corners of the test piece after the third operation were measured to obtain the average value. Based on the average value of the heights of the four corners obtained, the specific volume was calculated from the following formula. The test was performed on three test pieces, and the average of the three measured values was expressed. Specific volume (cm3 / g)=(5×5×(h0 / 10)) / W h0: Average height of the four corners of the test piece after weight A is removed (mm) W: Mass of the test piece (g)
[0024] (Measurement of compression rate and recovery rate) The heights of the four corners of the test piece were measured in the same manner as in the measurement of the specific volume, and then a 126g weight B was placed on the test piece for 30 seconds, and the heights of the four corners of the test piece were measured. The weight B was then removed, and the heights of the four corners of the test piece were measured 3 minutes later. The measured heights of the four corners were averaged, and the compression ratio and recovery ratio were calculated from the three average values according to the following formula. The test was performed on three test pieces, and the averages of the three measurements were used. Compression ratio (%) = (h0-h1) / h0*100 Recovery rate (%)=(h2-h1) / (h0-h1)*100 h1: Average height of the four corners of the test piece when weight B is placed on it (mm) h2: Average height of the four corners of the test piece after weight B is removed (mm)
[0025] (Water retention measurement) The water retention of the bioabsorbable cotton-like material and cotton was measured according to a method in accordance with JIS L 1912-1997, and the water absorbency was evaluated. Specifically, first, the initial weight of the sample in the standard state was measured, and the sample was placed under the water for 180 seconds in a container filled with water. The sample was then removed from the water, hung vertically for 120 seconds, and the weight was measured after the test. Based on the weight obtained, the water retention rate was calculated using the following formula. The results are shown in Table 1. Note that no measurement was performed for Reference Example 2, as it was not degreased. W A =(M N -M K ) / M K ×100 W A :Water retention rate (%) M K : Initial weight (g) (average value of 5 times) M N Weight after test (g) (average of 5 tests)
[0026] [Table 1]
[0027] From Table 1, it can be seen that the bioabsorbable cotton-like materials of the Examples have similar properties to cotton and can be used as a substitute for cotton. Also, Fig. 1 shows photographs comparing the bioabsorbable cotton-like materials of Example 1 and Comparative Example 1 with the polyester cotton of Reference Example 1 and the organic cotton of Reference Example 2. As can be seen from Fig. 1, the fibers of Example 1 are more densely entangled than those of Comparative Example 1, and are closer to cotton. [Industrial Applicability]
[0028] According to the present invention, there is provided a method for producing a bioabsorbable cotton-like material, which is capable of producing a bioabsorbable cotton-like material with high water absorbency.
Claims
1. A method for producing a bioabsorbable cotton-like material for medical use, comprising the steps of forming polyglycolide into thread by melt spinning, and subjecting the thread to a woolly process.
2. 2. The method for producing a bioabsorbable cotton-like material according to claim 1, wherein the heating temperature in the woolly processing is 50° C. or higher and 200° C. or lower.
Citation Information
Patent Citations
Manufacture of semiconductor device
JP1993315561A
Regeneration medical base material
JP2009050623A
Highly porous self-cohered web material with hemostatic properties
JP2009502330A
Base material for finger joint cartilage
JP2021010552A