Method for manufacturing a sensor element

By using a covering material during co-firing to stabilize Au concentration, the method addresses Au evaporation and scattering issues, ensuring accurate gas detection in sensors.

JP7577586B2Active Publication Date: 2024-11-05NGK CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021051704
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-25
Publication Date
2024-11-05
Estimated Expiration
2041-03-25

AI Technical Summary

Technical Problem

Existing methods for forming electrodes with Au in gas sensors result in Au evaporation and scattering, leading to contamination of other parts and instability in Au concentration, which affects the performance and accuracy of gas detection.

Method used

A method involving the use of a covering material with a porosity of 60% or less, placed on the electrode during co-firing to suppress Au evaporation and scattering, ensuring at least 30% coverage of the electrode surface.

Benefits of technology

This approach stabilizes the Au concentration, preventing contamination and maintaining the sensitivity and accuracy of gas detection, particularly in multi-gas sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577586000002
    Figure 0007577586000002
  • Figure 0007577586000003
    Figure 0007577586000003
  • Figure 0007577586000004
    Figure 0007577586000004
Patent Text Reader

Abstract

To provide a manufacturing method of a sensor element that suitably forms an electrode containing Au as a metal component and suppressing disperses scattering of Au to other places.SOLUTION: A manufacturing method of a sensor element for a gas sensor provided with an electrode containing Au on a surface includes: a thin film forming step in which a first paste film that will become an electrode containing Au by firing is formed on the surface of an element body that will become the sensor element by firing; a covering material placing step in which a covering material made of ceramics and having a porosity of 60% or less is placed on the paste film so that at least part of the first paste film is covered with a coverage of 30% or more; and a co-firing step in which the element body containing the first paste film is fired together with the covering material at a temperature of 1200°C or higher and 1500°C or lower.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a sensor element of a gas sensor, and more particularly to the formation of an electrode containing Au as a metal component. [Background technology]

[0002] Gas sensors that detect a specific gas component in a gas to be measured and determine its concentration include various types, such as semiconductor type, catalytic combustion type, oxygen concentration difference detection type, limiting current type, and mixed potential type. Some of these types use a sensor element whose main component is a ceramic solid electrolyte such as zirconia. Among these, a mixed potential type gas sensor in which the metal component of the detection electrode provided in the sensor element is a Pt-Au alloy is already known (see, for example, Patent Document 1 and Patent Document 2).

[0003] The gas sensor disclosed in Patent Document 1 detects unburned hydrocarbons, but Au has low ammonia oxidation activity and good ammonia detection sensitivity, so it can also be used as a material for the ammonia detection electrode. For example, Patent Document 2 mentions a mixed potential type gas sensor using a Pt-Au alloy for the detection electrode, which is used as an ammonia gas sensor. In addition, in the case of a detection electrode whose metal component is a Pt-Au alloy, it is preferable to make the surface of the metal particle an Au-enriched region where Au is concentrated, in order to ensure detection sensitivity.

[0004] However, because Au has a relatively low melting point of 1064° C., even when the detection electrode is formed with Pt, which has a high melting point of 1768° C., evaporation (detachment) of Au may occur from the paste film that will ultimately become the detection electrode during co-firing with the solid electrolyte, which is performed at, for example, about 1200° C. to 1500° C. In addition, detachment of Au from the detection electrode may occur during use of the gas sensor, in which the sensor element is heated to high temperatures.

[0005] In consideration of these points, Patent Document 1 discloses an embodiment in which an element body that will become a sensor element after sintering is surrounded by a sheath material made of dense alumina, for example, and the element body is sintered in a state in which the element body is placed in a space that is sufficiently narrow compared to the internal volume of a sintering furnace, with the aim of suppressing the detachment of Au during the formation of the detection electrode and maintaining the Au-enriched region during subsequent use.

[0006] In this case, Au evaporates (desorbs) from the paste film formed on the surface of the element body, which becomes the detection electrode by firing, but since the element body is surrounded by the sheath material, an Au-excess atmosphere is created near the paste film inside the sheath material even if only a relatively small amount of Au atoms evaporates. As a result, Au is less likely to evaporate from the paste film, and as firing progresses to form the detection electrode, a state is created in which the Au atoms present in the paste film are unevenly distributed on the surfaces of the Pt-Au alloy particles, and an Au-enriched region is ultimately formed.

[0007] Patent Document 2 also discloses an embodiment in which an electrode evaporation prevention film having the same alloy composition as the detection electrode or a composition richer in Au than that is provided on the surface of the sensor element (for example, the same surface as the detection electrode), and when the gas sensor is used, Au is evaporated from the electrode evaporation prevention film, which is heated to a high temperature together with the sensor element, to form an Au saturated vapor field in the vicinity of the detection electrode, thereby suppressing the evaporation of Au from the detection electrode. When providing the electrode evaporation prevention film on the same surface as the detection electrode, it is also disclosed that an insulating layer is first formed on the surface of the sensor element, and then the electrode evaporation prevention film is formed on the insulating layer.

[0008] Meanwhile, a gas sensor is also already known in which a single sensor element, whose main constituent material is an oxygen-ion conductive solid electrolyte, is provided with an NH3 gas sensor section equipped with a mixed potential cell and capable of detecting ammonia, and a NOx sensor section equipped with a plurality of electrochemical pump cells including a measurement pump cell, and the concentration of NH3 gas can be determined based on the output of the former, and the NOx concentration can be determined based on the output values ​​of both (see, for example, Patent Document 3). [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 5938133 [Patent Document 2] Patent No. 6655515 [Patent Document 3] JP 2018-40746 A Summary of the Invention [Problem to be solved by the invention]

[0010] The methods for suppressing Au evaporation disclosed in Patent Document 1 and Patent Document 2 each form an Au-excess atmosphere around the element body or sensor element, which can lead to the problem of Au poisoning, in which Au evaporated from the detection electrode itself or the electrode evaporation suppression film adheres to other parts of the element or other electrodes.

[0011] In particular, as in the gas sensor disclosed in Patent Document 3, when a detection electrode, which is one of the components of the mixed potential cell in the NH3 gas sensor section and contains a Pt-Au alloy as a metal component, and an outer pump electrode, which is one of the components of the electrochemical pump cell in the NOx sensor section and contains Pt as a metal component, are provided on the surface of a single sensor element, adhesion of Au to the outer pump electrode or the lead pattern connected to it is undesirable because it degrades the performance of the electrochemical pump cell and ultimately degrades the measurement accuracy of the NOx concentration.

[0012] In addition, the methods disclosed in Patent Documents 1 and 2 are effective in forming and maintaining an Au-enriched region in the detection electrode, but do not necessarily contribute to stabilizing the Au content in the detection electrode. Furthermore, these methods require the use of separate members or processes and materials for providing extra components that do not directly contribute to the function of the gas sensor, which complicates the process and increases costs.

[0013] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a manufacturing method for a sensor element that can suitably form an electrode containing Au as a metal component while suppressing the scattering of Au to other locations. [Means for solving the problem]

[0014] In order to solve the above problems, a first aspect of the present invention is a method for manufacturing a sensor element of a gas sensor having an electrode containing Au on a surface thereof, the method comprising the steps of: forming a first paste film, which becomes the electrode containing Au when fired, on a surface of an element body which becomes the sensor element when fired; 1. The method includes a second film formation process for forming a protective layer film, which becomes a surface protective layer by firing, on the element body that has undergone the film formation process; a covering material placement process for placing a covering material made of ceramics and having a porosity of 60% or less on the protective layer film so that at least a portion of the first paste film is covered with a coverage rate of 30% or more; and a co-firing process for firing the element body including the first paste film and the protective layer film together with the covering material at a temperature of 1200°C or higher and 1500°C or lower, and the covering material is removed after the co-firing process.

[0015] A second aspect of the present invention is a manufacturing method for a sensor element according to the first aspect, further comprising a sheath arrangement process for arranging a plurality of element bodies on which the first paste film is formed in a sintered sheath so that the first paste films are arranged in a row, and is characterized in that in the covering material placement process, a rod-shaped covering material is placed on top of the row of first paste films.

[0016] A third aspect of the present invention is a manufacturing method for a sensor element according to the first aspect, further comprising a sheath arrangement process for arranging one or more element bodies on which the first paste film is formed in a sintered sheath, and is characterized in that in the covering material placement process, a plate-shaped covering material is placed on each of the first paste films of the one or more element bodies.

[0017] A fourth aspect of the present invention is a method for manufacturing a sensor element according to any one of the first to third aspects, characterized in that the covering material has a thickness of 1 mm or more and 10 mm or less.

[0018] A fifth aspect of the present invention is a method for manufacturing a sensor element according to any one of the first to fourth aspects, characterized in that the covering material is made of alumina.

[0019] A sixth aspect of the present invention is a method for manufacturing a sensor element according to any one of the first to fifth aspects, characterized in that the Au-containing electrode is an NH3 detection electrode containing a Pt-Au alloy as a metal component and having catalytic activity against NH3 gas disabled, and the sensor element has a base portion made of an oxygen ion conductive solid electrolyte, and is provided with an NH3 gas sensor portion having a mixed potential cell composed of the NH3 detection electrode, a reference electrode provided inside the sensor element, and a solid electrolyte between the NH3 detection electrode and the reference electrode.

[0020] A seventh aspect of the present invention is a method for manufacturing a sensor element according to the sixth aspect, wherein the sensor element comprises at least one internal space into which a gas to be measured is introduced from an external space, a NOx measurement electrode formed facing the at least one internal space, and an outer pump electrode formed on a surface of the sensor element, and further comprises a NOx sensor portion including a measurement pump cell which is an electrochemical pump cell, the measurement electrode, the outer pump electrode, and a solid electrolyte between the NOx measurement electrode and the outer pump electrode, 1.In the film forming process, a second paste film is further formed which becomes the outer pump electrode by firing, and in the covering material placing process, the covering material is positioned so that at least the side of the first paste film which is closer to the second paste film is covered.

[0021] An eighth aspect of the present invention is a manufacturing method for a sensor element according to the seventh aspect, characterized in that in the covering material placing step, the covering material is positioned so that in addition to at least a portion of the first paste film, at least a portion of the area between the first paste film and the second paste film is covered. Effect of the Invention

[0022] According to the first to eighth aspects of the present invention, the evaporation and scattering of Au during co-firing is suppressed by the placement of the covering material, so that weight loss and a decrease in the concentration of Au in the Au-containing electrode of the sensor element are suppressed.

[0023] In particular, according to the sixth to eighth aspects, deterioration of the sensitivity characteristics when detecting NH3 gas using the sensor element is suppressed.

[0024] In particular, according to the seventh and eighth aspects, when the sensor element is used in a multi-gas sensor, deterioration in the accuracy of NOx detection caused by Au adhering or being adsorbed to the external pump electrode is more reliably suppressed. [Brief description of the drawings]

[0025] [Figure 1] 1 is a diagram illustrating an example of the configuration of a gas sensor 100, including a vertical cross-sectional view along the longitudinal direction of a sensor element 101. FIG. [Diagram 2] 1 is a top view of the sensor element 101 taken along the longitudinal direction. [Diagram 3] 3 is a diagram showing a process flow for manufacturing the sensor element 101. FIG. [Figure 4] FIG. 1 is a side view diagrammatically illustrating a method for suppressing the evaporation and scattering of Au. [Diagram 5]1 is a diagram showing an example of arrangement of an element body 101α relative to a sintered sheath S. FIG. [Figure 6] 13 is an enlarged view of a main portion showing an example in which a covering material C is placed on an element body 101α placed in a sintered sheath S. FIG. [Figure 7] 13 is an enlarged view of a main portion showing an example in which a covering material C is placed on an element body 101α placed in a sintered sheath S. FIG. [Figure 8] 13 is an enlarged view of a main portion showing an example in which a covering material C is placed on an element body 101α placed in a sintered sheath S. FIG. [Figure 9] 13 is an enlarged view of a main portion showing an example in which a covering material C is placed on an element body 101α placed in a sintered sheath S. FIG. [Figure 10] 13 is an enlarged view of a main portion showing an example in which a covering material C is placed on an element body 101α placed in a sintered sheath S. FIG. [Figure 11] FIG. 13 is a diagram showing an example of the arrangement of load bars. [Figure 12] 13A and 13B are diagrams showing modified examples of the arrangement of the covering material. [Figure 13] 13 is a graph in which the Au residual rate is plotted against the coverage rate for each sensor element 101 manufactured using covering materials C having the same porosity. [Figure 14] 13 is a graph in which the Au concentration is plotted against the coverage for each sensor element 101 manufactured using covering material C having the same porosity. [Figure 15] 1 is a graph in which the output value of the mixed potential cell 61 is plotted against the concentration of NH 3 gas in the model gas for each gas sensor 100 having the same coverage rate when the sensor element 101 is co-fired. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] <Outline of gas sensor configuration> First, a schematic configuration of a gas sensor 100 will be described, including an example of a configuration of a sensor element manufactured by applying a manufacturing method according to the present embodiment. Fig. 1 is a schematic diagram showing an example of the configuration of the gas sensor 100, including a vertical cross-sectional view along the longitudinal direction of a sensor element 101, which is a main component of the gas sensor 100. Fig. 2 is a top view along the longitudinal direction of the sensor element 101. However, the sizes and ratios of the components in both figures are not necessarily the same as the actual ones.

[0027] The sensor element 101 has a structure in which six layers, namely, a first substrate layer 1, a second substrate layer 2, a third substrate layer 3, a first solid electrolyte layer 4, a spacer layer 5, and a second solid electrolyte layer 6, each of which is made of an oxygen ion conductive solid electrolyte layer such as zirconia (ZrO2), are laminated in this order from the bottom as viewed in the drawing. The solid electrolyte forming these six layers is dense and airtight. The sensor element 101 is manufactured, for example, by laminating ceramic green sheets corresponding to each layer after performing a predetermined processing and printing a circuit pattern, and further sintering them to integrate them. Hereinafter, the part of the sensor element 101 made of the solid electrolyte is also referred to as a base part.

[0028] At one tip of the sensor element 101, between the lower surface of the second solid electrolyte layer 6 and the upper surface of the first solid electrolyte layer 4, a gas inlet 10, a first diffusion rate-controlling section 11, a buffer space 12, a second diffusion rate-controlling section 13, a first internal space 20, a third diffusion rate-controlling section 30, and a second internal space 40 are formed adjacent to each other and communicated with each other in this order.

[0029] The gas inlet 10, the buffer space 12, the first internal space 20, and the second internal space 40 are spaces inside the sensor element 101 provided in a manner penetrating the spacer layer 5, and each is bounded at its upper part by the lower surface of the second solid electrolyte layer 6, at its lower part by the upper surface of the first solid electrolyte layer 4, and at its sides by the spacer layer 5.

[0030] The first diffusion rate-controlling section 11, the second diffusion rate-controlling section 13, and the third diffusion rate-controlling section 30 are each provided as two horizontally elongated slits (with the openings extending in the direction perpendicular to the drawing). The portion extending from the gas inlet 10 to the second internal space 40 is also referred to as a gas flow section.

[0031] Further, at a position farther from the tip side than the gas flow section, a reference gas introduction space 43 is provided between the upper surface of the third substrate layer 3 and the lower surface of the spacer layer 5, and at a position defined at the side by the side surface of the first solid electrolyte layer 4. Air is introduced into the reference gas introduction space 43 as a reference gas.

[0032] The air introduction layer 48 is a layer made of porous alumina, and air as a reference gas is introduced into the air introduction layer 48 through the reference gas introduction space 43. In addition, the air introduction layer 48 is formed so as to cover the reference electrode 42.

[0033] Reference electrode 42 is an electrode formed in a manner to be sandwiched between the upper surface of third substrate layer 3 and first solid electrolyte layer 4, and as described above, is surrounded by air introduction layer 48 which is connected to reference gas introduction space 43. In addition, as will be described later, it is possible to measure the oxygen concentration (oxygen partial pressure) in first internal space 20 and second internal space 40 using reference electrode 42.

[0034] Although not shown in Fig. 1, as shown in Fig. 2, a plurality of terminal electrodes 77 are provided on the upper surface (i.e., the upper surface of the second solid electrolyte layer 6) of the other end portion (the end portion opposite to the tip portion provided with the gas flow portion) of the sensor element 101. Fig. 2 illustrates an example in which four terminal electrodes 77 (77a to 77d) are provided. Furthermore, a heater electrode 71 and terminal electrodes 77, which will be described later, are also provided on the lower surface (i.e., the lower surface of the first substrate layer 1) of the other end portion.

[0035] In the gas flow section, the gas inlet 10 is a portion that opens to the outside space, and the measurement gas is introduced into the sensor element 101 from the outside space through the gas inlet 10 .

[0036] The first diffusion rate-controlling portion 11 is a portion that applies a predetermined diffusion resistance to the measurement gas taken in through the gas inlet 10.

[0037] The buffer space 12 is a space provided for guiding the measurement gas introduced from the first diffusion rate-controlling portion 11 to the second diffusion rate-controlling portion 13 .

[0038] The second diffusion rate-controlling portion 13 is a portion that imparts a predetermined diffusion resistance to the measurement gas introduced from the buffer space 12 into the first internal space 20 .

[0039] When the measurement gas is introduced from the outside of the sensor element 101 into the first internal space 20, the measurement gas is suddenly taken into the sensor element 101 from the gas inlet 10 due to pressure fluctuations of the measurement gas in the external space (exhaust pressure pulsations if the measurement gas is automobile exhaust gas), but is not introduced directly into the first internal space 20, but is introduced into the first internal space 20 after the concentration fluctuations of the measurement gas are cancelled out through the first diffusion rate-controlling section 11, buffer space 12, and second diffusion rate-controlling section 13. As a result, the concentration fluctuations of the measurement gas introduced into the first internal space 20 become almost negligible.

[0040] The first internal space 20 is provided as a space for adjusting the oxygen partial pressure in the measurement gas introduced through the second diffusion rate-controlling part 13. The oxygen partial pressure is adjusted by the operation of the main pump cell 21.

[0041] The main pump cell 21 is an electrochemical pump cell including an inner pump electrode 22 having a ceiling electrode portion 22a provided on almost the entire lower surface of the second solid electrolyte layer 6 facing the first internal space 20, an outer pump electrode 23 provided in a region corresponding to the ceiling electrode portion 22a on the upper surface of the second solid electrolyte layer 6 so as to be exposed to the external space, and the second solid electrolyte layer 6 sandwiched between these electrodes.

[0042] The inner pump electrode 22 is formed across the upper and lower solid electrolyte layers (the second solid electrolyte layer 6 and the first solid electrolyte layer 4) that define the first internal space 20, and the spacer layer 5 that provides the side walls. Specifically, a ceiling electrode portion 22a is formed on the lower surface of the second solid electrolyte layer 6 that provides the ceiling surface of the first internal space 20, and a bottom electrode portion 22b is formed on the upper surface of the first solid electrolyte layer 4 that provides the bottom surface. Side electrode portions (not shown) are formed on the side wall surfaces (inner surfaces) of the spacer layer 5 that constitute both side wall portions of the first internal space 20 so as to connect the ceiling electrode portion 22a and the bottom electrode portion 22b, and are arranged in a tunnel-shaped structure at the positions where the side electrode portions are arranged.

[0043] The inner pump electrode 22 and the outer pump electrode 23 are formed as porous cermet electrodes (for example, a cermet electrode of Pt containing 1% Au and ZrO2). The inner pump electrode 22, which comes into contact with the measurement gas, is formed using a material with a weakened ability to reduce the NOx component in the measurement gas.

[0044] In the main pump cell 21, by applying a desired pump voltage Vp0 between the inner pump electrode 22 and the outer pump electrode 23 by a variable power supply 24 and flowing a pump current Ip0 in a positive or negative direction between the inner pump electrode 22 and the outer pump electrode 23, it is possible to pump oxygen in the first internal space 20 out to the external space, or to pump oxygen from the external space into the first internal space 20.

[0045] In addition, in order to detect the oxygen concentration (oxygen partial pressure) in the atmosphere in the first internal space 20, an electrochemical sensor cell, i.e., an oxygen partial pressure detection sensor cell 80 for controlling the main pump, is configured by the inner pump electrode 22, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, and the reference electrode 42.

[0046] By measuring the electromotive force V0 in the oxygen partial pressure detection sensor cell 80 for controlling the main pump, the oxygen concentration (oxygen partial pressure) in the first internal space 20 can be determined.

[0047] Furthermore, the pump current Ip0 is controlled by feedback controlling Vp0 so that the electromotive force V0 is constant, thereby keeping the oxygen concentration in the first inner space 20 at a predetermined constant value.

[0048] The third diffusion rate-controlling section 30 is a section that applies a predetermined diffusion resistance to the measurement gas whose oxygen concentration (oxygen partial pressure) has been controlled by the operation of the main pump cell 21 in the first internal space 20, and guides the measurement gas to the second internal space 40.

[0049] The second internal space 40 is provided as a space for performing a process for identifying the concentration of nitrogen oxides (NOx) in the measurement gas introduced through the third diffusion-controlling part 30. The NOx concentration is mainly identified in the second internal space 40 in which the oxygen concentration is adjusted by the auxiliary pump cell 50, and further by operating the measurement pump cell 41.

[0050] In the second internal space 40, the oxygen concentration (oxygen partial pressure) is adjusted in advance in the first internal space 20, and then the oxygen partial pressure of the measurement gas introduced through the third diffusion rate-controlling part is further adjusted by the auxiliary pump cell 50. This makes it possible to keep the oxygen concentration in the second internal space 40 constant with high accuracy, and therefore makes it possible to specify the NOx concentration with high accuracy in the gas sensor 100.

[0051] The auxiliary pump cell 50 is an auxiliary electrochemical pump cell that is composed of an auxiliary pump electrode 51 having a ceiling electrode portion 51a provided on almost the entire lower surface of the second solid electrolyte layer 6 facing the second internal space 40, an outer pump electrode 23 (not limited to the outer pump electrode 23, but a sensor element 101 and an appropriate outer electrode will suffice), and the second solid electrolyte layer 6.

[0052] The auxiliary pump electrode 51 is disposed in the second internal space 40 in a tunnel-shaped structure similar to that of the inner pump electrode 22 provided in the first internal space 20. That is, a ceiling electrode portion 51a is formed on the second solid electrolyte layer 6 providing the ceiling surface of the second internal space 40, a bottom electrode portion 51b is formed on the first solid electrolyte layer 4 providing the bottom surface of the second internal space 40, and side electrode portions (not shown) connecting the ceiling electrode portion 51a and the bottom electrode portion 51b are formed on both wall surfaces of the spacer layer 5 providing the side walls of the second internal space 40, forming a tunnel-shaped structure.

[0053] Like the inner pump electrode 22, the auxiliary pump electrode 51 is also made of a material with a reduced ability to reduce the NOx component in the measurement gas.

[0054] In the auxiliary pump cell 50, by applying a desired voltage Vp1 between the auxiliary pump electrode 51 and the outer pump electrode 23, it is possible to pump oxygen in the atmosphere within the second internal space 40 out to the external space or pump oxygen from the external space into the second internal space 40.

[0055] In addition, in order to control the oxygen partial pressure in the atmosphere within the second internal space 40, an electrochemical sensor cell, i.e., an oxygen partial pressure detection sensor cell 81 for controlling the auxiliary pump, is constituted by the auxiliary pump electrode 51, the reference electrode 42, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, and the third substrate layer 3.

[0056] The auxiliary pump cell 50 performs pumping using a variable power supply 52 whose voltage is controlled based on the electromotive force V1 detected by the auxiliary pump control oxygen partial pressure detection sensor cell 81. As a result, the oxygen partial pressure in the atmosphere in the second internal space 40 is controlled to a low partial pressure that does not substantially affect the detection of NOx.

[0057] In addition, the pump current Ip1 is used to control the electromotive force of the main pump control oxygen partial pressure detection sensor cell 80. Specifically, the pump current Ip1 is input as a control signal to the main pump control oxygen partial pressure detection sensor cell 80, and the electromotive force V0 is controlled so that the gradient of the oxygen partial pressure in the measurement gas introduced from the third diffusion rate-controlling part 30 into the second internal space 40 is always constant. When used as a NOx sensor, the oxygen concentration in the second internal space 40 is kept at a constant value of about 0.001 ppm by the action of the main pump cell 21 and the auxiliary pump cell 50.

[0058] The measurement pump cell 41 detects NOx in the measurement gas in the second internal space 40. The measurement pump cell 41 is an electrochemical pump cell including a NOx measurement electrode (hereinafter simply referred to as the measurement electrode) 44 provided on the upper surface of the first solid electrolyte layer 4 facing the second internal space 40 and spaced apart from the third diffusion rate-controlling section 30, the outer pump electrode 23, the second solid electrolyte layer 6, the spacer layer 5, and the first solid electrolyte layer 4.

[0059] The measurement electrode 44 is a porous cermet electrode. The measurement electrode 44 also functions as a NOx reduction catalyst that reduces NOx present in the atmosphere in the second internal space 40. Furthermore, the measurement electrode 44 is covered with a fourth diffusion rate-controlling part 45.

[0060] The fourth diffusion rate-controlling part 45 is a film made of a porous body mainly composed of alumina (Al2O3). The fourth diffusion rate-controlling part 45 serves to limit the amount of NOx flowing into the measurement electrode 44, and also functions as a protective film for the measurement electrode 44 (measurement electrode protective layer).

[0061] In the measurement pump cell 41, oxygen produced by decomposition of nitrogen oxides in the atmosphere surrounding the measurement electrode 44 is pumped out, and the amount of oxygen produced can be detected as a pump current Ip2.

[0062] In order to detect the oxygen partial pressure around the measurement electrode 44, an electrochemical sensor cell, i.e., an oxygen partial pressure detection sensor cell 82 for controlling the measurement pump, is configured by the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, the measurement electrode 44, and the reference electrode 42. The variable power supply 46 is controlled based on the electromotive force V2 detected by the oxygen partial pressure detection sensor cell 82 for controlling the measurement pump.

[0063] The measurement gas introduced into the second internal space 40 reaches the measurement electrode 44 through the fourth diffusion rate-controlling part 45 under conditions in which the oxygen partial pressure is controlled. Nitrogen oxides in the measurement gas around the measurement electrode 44 are reduced (2NO → N2 + O2) to generate oxygen. The generated oxygen is then pumped by the measurement pump cell 41, and the voltage Vp2 of the variable power supply 46 is controlled so that the control voltage V2 detected by the measurement pump control oxygen partial pressure detection sensor cell 82 is kept constant. The amount of oxygen generated around the measurement electrode 44 is proportional to the concentration of nitrogen oxides in the measurement gas, so that the nitrogen oxide concentration in the measurement gas can be calculated using the pump current Ip2 in the measurement pump cell 41.

[0064] Furthermore, by combining the measurement electrode 44, the first solid electrolyte layer 4, the third substrate layer 3 and the reference electrode 42 to form an oxygen partial pressure detection means as an electrochemical sensor cell, it is possible to detect an electromotive force corresponding to the difference between the amount of oxygen generated by reduction of the NOx components in the atmosphere around the measurement electrode 44 and the amount of oxygen contained in the reference atmosphere, thereby making it possible to determine the concentration of the NOx components in the measured gas.

[0065] In addition, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, the outer pump electrode 23, and the reference electrode 42 constitute an electrochemical sensor cell 83, and the electromotive force Vref obtained by this sensor cell 83 makes it possible to detect the oxygen partial pressure in the measurement gas outside the sensor.

[0066] As described above, the portion of the sensor element 101 extending from the gas inlet 10 to the second internal space 40 in the longitudinal direction of the element, as well as the electrodes, pump cell, sensor cell, etc. provided in that portion, are primarily related to the measurement of NOx concentration, and therefore in this embodiment, these portions are also referred to as the NOx sensor portion of the sensor element 101.

[0067] Furthermore, the sensor element 101 includes an NH3 detection electrode (hereinafter, simply the detection electrode) 60 on the upper surface of the second solid electrolyte layer 6. The detection electrode 60 is formed as a porous cermet electrode of Pt containing Au at a predetermined ratio, that is, a Pt-Au alloy, and zirconia. In the sensor element 101, the detection electrode 60, the reference electrode 42, and the solid electrolyte layer present between the two electrodes form a mixed potential cell 61. That is, the concentration of NH3 in the measurement gas is obtained by utilizing the fact that a potential difference occurs due to the difference in the concentration of NH3 near the two electrodes based on the principle of mixed potential. In this embodiment, the part of the sensor element 101 that forms the mixed potential cell 61 is also referred to as an NH3 gas sensor part. In addition, the reference electrode 42 is also referred to as a common reference electrode because it is used not only in the NH3 gas sensor part but also in the NOx sensor part as described above.

[0068] Specifically, the detection electrode 60 is made inactive for NH3 gas in a predetermined concentration range by appropriately determining the composition of the Pt-Au alloy that is the constituent material of the detection electrode 60. In other words, the decomposition reaction of NH3 gas in the detection electrode 60 is suppressed. As a result, in the gas sensor 100, the potential of the detection electrode 60 is made to selectively vary (have a correlation) with the concentration of NH3 gas in the concentration range. In other words, the detection electrode 60 is provided so as to have the characteristics that the potential is highly dependent on the concentration of NH3 gas in the concentration range, while the potential is less dependent on the concentration of other components of the measured gas.

[0069] The distance between the detection electrode 60 and the outer pump electrode 23 may be set appropriately depending on the size of the sensor element 101, the desired performance, etc. Fig. 2(a) illustrates an example in which the distance between them is smaller than the size of the detection electrode 60 in the longitudinal direction of the element, and Fig. 2(b) illustrates an example in which the distance between them is larger than the size of the detection electrode 60 in the longitudinal direction of the element.

[0070] More specifically, in the sensor element 101, the detection electrode 60 is provided so that the dependence of the potential on the NH3 gas concentration is significant by suitably determining the degree of Au concentration on the surface of the Pt-Au alloy particles that constitute the detection electrode 60.

[0071] In this specification, the Au enrichment degree refers to the area ratio of the portion of the surface of the precious metal particle constituting the detection electrode 60 that is covered with Au. In this specification, the Au enrichment degree is calculated by using the peak intensity values ​​of the detection peaks for Au and Pt obtained by performing XPS (X-ray photoelectron spectroscopy) analysis on the surface of the precious metal particle, Au concentration (%) = 100 × Au intensity value / (Au intensity value + Pt intensity value) (1) The Au concentration is calculated using the following formula:

[0072] In the case where the surface protective layer 90 described below is not present and the detection electrode 60 is exposed, the XPS measurement can be performed by measuring the precious metal particles present on the surface of the detection electrode 60. If the detection electrode 60 is not exposed, the detection electrode 60 can be broken and the surface of the precious metal particles present on the broken surface can be measured.

[0073] Furthermore, when the Au concentration calculated by formula (1) is 10% or more, it can be considered that Au is concentrated on the surface of the precious metal particles constituting the detection electrode 60. In other words, it can be considered that an Au-concentrated region is formed on the surface of the precious metal particle. In this embodiment, the Au concentration of the detection electrode 60 is 15% or more.

[0074] The Au concentration can also be calculated from the detection values ​​for Au and Pt in an Auger spectrum obtained by performing AES (Auger electron spectroscopy) analysis on the surface of the precious metal particle. The Au concentration value obtained by this method and the Au concentration value calculated by formula (1) based on the results of XPS analysis can be considered to be substantially the same.

[0075] On the other hand, as described above, the periphery of the reference electrode 42 is covered with the air introduction layer 48 that is connected to the reference gas introduction space 43, so that the periphery of the reference electrode 42 is constantly filled with air (oxygen) when the gas sensor 100 is in use. Therefore, when the gas sensor 100 is in use, the reference electrode 42 always has a constant potential.

[0076] As a result, when the gas sensor 100 is in use, in the mixed potential cell 61, a potential difference EMF corresponding to the concentration of NH3 gas in the measured gas is generated between the detection electrode 60 and the reference electrode 42, at least over the NH3 gas concentration range of 0 ppm to 500 ppm.

[0077] Furthermore, the sensor element 101 includes a heater section 70 that adjusts the temperature by heating and keeping the sensor element 101 warm in order to increase the oxygen ion conductivity of the solid electrolyte. The heater section 70 includes a heater electrode 71, a heater 72, a through hole 73, a heater insulating layer 74, and a pressure release hole 75. The heater electrode 71 is an electrode formed in such a manner that it is in contact with the lower surface of the first substrate layer 1. By connecting the heater electrode 71 to an external power source, it is possible to supply power to the heater section 70 from the outside.

[0078] The heater 72 is an electrical resistor sandwiched between the second substrate layer 2 and the third substrate layer 3. The heater 72 is connected to a heater electrode 71 via a through hole 73, and generates heat when power is supplied from the outside through the heater electrode 71, thereby heating and keeping warm the solid electrolyte that forms the sensor element 101.

[0079] Moreover, the heater 72 is embedded throughout the entire area from the first internal space 20 to the second internal space 40, and is capable of adjusting the temperature of the entire sensor element 101 to a temperature at which the solid electrolyte is activated.

[0080] The heater insulating layer 74 is an insulating layer made of an insulator such as alumina and formed on the upper and lower surfaces of the heater 72. The heater insulating layer 74 is formed for the purpose of obtaining electrical insulation between the second substrate layer 2 and the heater 72, and between the third substrate layer 3 and the heater 72.

[0081] The pressure relief hole 75 is a portion that penetrates the third substrate layer 3 and is provided so as to communicate with the reference gas introduction space 43, and is formed for the purpose of mitigating the increase in internal pressure that accompanies an increase in temperature within the heater insulation layer 74.

[0082] In the gas sensor 100, when the concentration of NOx is determined, the heater 72 generates heat, so that each part of the sensor element 101 is heated to a temperature suitable for operation and kept warm. Therefore, the pump cells, the sensor cell, and the mixed potential cell 61 are also heated to a temperature suitable for each of them. However, the temperature ranges in which each of them operates suitably are different. Specifically, the NOx sensor part (more specifically, the tip side (left side in FIG. 1) of the third diffusion rate-controlling part 30, which includes the main pump cell 21 including the inner pump electrode 22 and the outer pump electrode 23, etc.) is heated to a predetermined temperature (first temperature) of 600° C. to 900° C., and the NH3 gas sensor part (more specifically, the mixed potential cell 61 and its vicinity) is heated to a predetermined temperature (second temperature) of 400° C. to 650° C., which is lower than the first temperature.

[0083] In the gas sensor 100, the arrangement position of each cell, the range in which the heater is present, and the heating mode by the heater 72 are determined so that these temperature conditions are suitably realized.

[0084] Furthermore, the sensor element 101 includes a surface protection layer 90 provided on the upper surface of the second solid electrolyte layer 6 in a manner to cover the outer pump electrode 23 and the detection electrode 60. The surface protection layer 90 is provided for the purpose of preventing poisonous substances contained in the measured gas from adhering to the outer pump electrode 23 and the detection electrode 60. A suitable example of the surface protection layer 90 is formed of porous alumina. However, the surface protection layer 90 is provided so as to have a pore diameter and a pore size that do not limit the flow of gas between the outer pump electrode 23 and the detection electrode 60 and the outside of the element.

[0085] 1 shows the surface protective layer 90 extending to the other end (the right end as viewed in the drawing) of the sensor element 101, but in reality, the terminal electrode 77 (not shown) is exposed without being covered by the surface protective layer 90. Alternatively, the surface protective layer 90 may be provided so as to cover only the outer pump electrode 23 and the detection electrode 60, rather than extending to the other end.

[0086] The operation of each part of the gas sensor 100, such as the application of a voltage to the pump cell by the variable power supply and heating by the heater 72, is controlled by a controller (control means) 110 electrically connected to each part. In addition, the controller 110 determines the NOx concentration in the measurement gas based on the potential difference EMF generated in the mixed potential cell 61 of the sensor element 101 and the pump current Ip2 flowing through the measurement pump cell 41. In addition, the NH3 concentration can also be determined during the NOx concentration calculation. That is, the controller 110 also functions as a concentration determination means for determining the NOx concentration and further the NH3 concentration.

[0087] 1, only the potential difference EMF and the pump current Ip2 are connected to the controller 110 by arrows, but this is merely for convenience of illustration, and it goes without saying that other potential difference values ​​and pump current values ​​are also provided to the controller 110. A general-purpose personal computer can be used as the controller 110.

[0088] Also, for convenience of illustration, Fig. 1 shows only conceptually the electrical connections between the electrodes constituting each pump cell and the variable power source, and the electrical connections in the mixed potential cell 61 and each sensor cell. In the actual gas sensor 100, for example, as shown in Fig. 2, the outer pump electrode 23 is connected to a terminal electrode 77a, which is one of the terminal electrodes 77, by a lead wire 23L, the detection electrode 60 is connected to a terminal electrode 77c, which is another one of the terminal electrodes 77, by a lead wire 60L, and the other electrodes are also connected to the other one of the terminal electrodes 77 by a lead wire (not shown) provided inside the sensor element 101. The sensor element 101 is inserted into a connector (not shown) that provides electrical connection between the sensor element 101 and the outside, and the terminal electrode 77 is brought into contact with a connection terminal of the connector, thereby realizing connections between the various cells provided in the sensor element 101 and the outside.

[0089] In the gas sensor 100 having the above configuration, the concentration of NH3 gas in the measurement gas can be accurately determined based on the potential difference EMF generated between the detection electrode 60 and the reference electrode 42 in the mixed potential cell 61. In addition, the NOx concentration determined based on the value of the pump current Ip2 flowing through the measurement pump cell 41 is corrected based on the potential difference EMF, so that the NOx concentration can be measured even in the presence of NH3 gas. In other words, the gas sensor 100 functions as a multi-gas sensor that can simultaneously measure the concentrations of NH3 and NOx in parallel.

[0090] <Sensor element manufacturing process> Next, a process for manufacturing the sensor element 101 shown in Fig. 1 will be described. In summary, the sensor element 101 shown in Fig. 1 is manufactured by forming a laminate made of green sheets containing an oxygen ion conductive solid electrolyte such as zirconia as a ceramic component, and cutting and firing the laminate. An example of the oxygen ion conductive solid electrolyte is yttria partially stabilized zirconia (YSZ), in which 3 mol % or more of yttria is added to zirconia.

[0091] FIG. 3 is a diagram showing a process flow when the sensor element 101 is produced. When the sensor element 101 is produced, first, blank sheets (not shown) that are green sheets on which no pattern is formed are prepared (step S1). Specifically, six blank sheets corresponding to the first substrate layer 1, the second substrate layer 2, the third substrate layer 3, the first solid electrolyte layer 4, the spacer layer 5, and the second solid electrolyte layer 6 are prepared. The blank sheets are provided with a plurality of sheet holes used for positioning during printing and lamination. The sheet holes are formed in advance by a punching process using a punching device or the like. In addition, in the case of a green sheet in which the corresponding layer forms an internal space, a through portion corresponding to the internal space is also provided in advance by a similar punching process or the like. In addition, the thicknesses of the blank sheets corresponding to each layer of the sensor element 101 do not all need to be the same.

[0092] Once blank sheets corresponding to each layer are prepared, a pattern printing and drying process is performed to form various patterns on each blank sheet (step S2). Specifically, electrode patterns such as the pump electrodes, detection electrode 60, terminal electrode 77, heater electrode 71, etc., a pattern for the heater 72, an air introduction layer 48, and wiring patterns such as lead wires 23L, 60L, and internal wiring (not shown) are formed. Furthermore, a pattern for the surface protection layer 90 is also printed. Note that cut marks are also printed on the first substrate layer 1, which serve as a reference for the cutting position when cutting the laminate in a later process.

[0093] Each pattern is printed by applying a pattern-forming paste prepared according to the characteristics required for each object to a blank sheet using a known screen printing technique. For drying after printing, known drying means can be used.

[0094] After the pattern printing is completed, the green sheets corresponding to each layer are laminated and bonded to each other by printing and drying the adhesive paste (step S3). A known screen printing technique can be used to print the adhesive paste, and a known drying method can be used to dry the green sheets after printing.

[0095] Next, the green sheets coated with the adhesive are stacked in a predetermined order, and pressed under predetermined temperature and pressure conditions to form a laminate (step S4). Specifically, the green sheets to be laminated are stacked and held in a predetermined lamination jig (not shown) while being positioned by the sheet holes, and heated and pressed together with the lamination jig by a lamination machine such as a known hydraulic press. The pressure, temperature, and time for heating and pressing depend on the lamination machine used, but appropriate conditions may be determined so that good lamination can be achieved. Note that a surface protection layer 90 may be formed on the laminate obtained in this manner.

[0096] After the laminate is obtained as described above, the laminate is cut at a plurality of locations to cut out individual units (referred to as element bodies) of the sensor element 101 (step S5). The cut-out element bodies are fired under predetermined conditions to produce the sensor element 101 as described above (step S6). That is, the sensor element 101 is produced by integral firing (co-firing) of the solid electrolyte layer and the electrodes. The firing temperature at that time is preferably 1200° C. or higher and 1600° C. or lower (for example, 1400° C.). By performing the co-firing in this manner, each electrode in the sensor element 101 has sufficient adhesion strength. This contributes to improving the durability of the sensor element 101.

[0097] Moreover, in this embodiment, by adopting a measure described later, the evaporation and scattering of Au from the pattern (printed film) that will ultimately become the detection electrode 60 during co-firing is suitably suppressed.

[0098] The sensor element 101 thus obtained is accommodated in a predetermined housing and assembled into the main body of the gas sensor 100 (not shown).

[0099] <Prevention of evaporation and scattering of Au from the detection electrode during co-firing> As described above, in this embodiment, the screen printing technique is used to form the electrodes provided on the sensor element 101, and the element body is fired together with the paste films for forming the electrodes formed by printing, thereby completing the sensor element 101. In this case, the detection electrode 60 contains a Pt-Au alloy containing Au, which has a melting point lower than the co-firing temperature, as a metal component, and is provided on the upper surface of the sensor element 101. Therefore, although the porous surface protection layer 90 is provided on the upper surface of the detection electrode 60, evaporation and scattering of Au from the paste film that becomes the detection electrode 60 may occur during co-firing.

[0100] Such evaporation and scattering of Au is undesirable because it not only reduces the weight of the detection electrode, but also causes problems such as contamination of other parts by the scattered Au and a lower than expected coverage (concentration) of Au on the surface of the detection electrode 60. In particular, when other electrodes and lead patterns connected thereto are provided in the vicinity of the detection electrode 60, such as the outer pump electrode 23 of the sensor element 101 according to this embodiment, if Au scattered from the paste film that becomes the detection electrode 60 adheres to those electrodes and lead patterns, the electrode may not be able to perform the expected function.

[0101] In this embodiment, the Au residual rate calculated by the following formula is used as an index of the weight loss in the detection electrode 60.

[0102] Au residual rate (%) = 100 × {(weight ratio of Au to the total metal components in the detection electrode) / (weight ratio of Au to the total metal components in the detection electrode paste)} (2) Here, the weight ratio of Au to the total metal components in each of the detection electrode 60 and the detection electrode paste provided in the sensor element 101 can be obtained as the weight ratio of Au to the total weight of Au and Pt when composition analysis is performed by EPMA on each of the detection electrode and the detection electrode paste.

[0103] After the preparation of the detection electrode paste, no Pt or Au is supplied to the detection electrode 60 until the detection electrode 60 is obtained by co-firing when producing the sensor element 101 in the above-mentioned manufacturing process. Therefore, the fact that the Au weight ratio in the detection electrode 60 is lower than the Au weight ratio in the detection electrode paste means that Au has evaporated during co-firing.

[0104] 4 is a side view that shows a schematic diagram of a method for suppressing the evaporation and scattering of Au during co-firing to obtain the sensor element 101 in this embodiment in order to avoid the occurrence of the above-mentioned problems. In FIG. 4, the left-right direction in the drawing corresponds to the longitudinal direction of the element, as in FIG. 1.

[0105] 4(a) to 4(e), the pump electrode film 23α and the detection electrode film 60α, which are paste films formed by screen printing using a predetermined paste, are provided on the upper surface of the element body 101α that will become the sensor element 101 after co-firing, and a protective layer film 90α, which is also formed by screen printing using a predetermined paste, is provided so as to cover them. The pump electrode film 23α, the detection electrode film 60α, and the protective layer film 90α are paste films that will become the outer pump electrode 23, the detection electrode 60, and the porous surface protective layer 90, respectively, after co-firing.

[0106] In this embodiment, prior to co-firing, for example, as shown in FIG. 4(a) and FIG. 4(b), a covering material C is placed on the upper surface of the protective layer film 90α and above the detection electrode film 60α. Then, the covering material C and the covering material C are co-firing. The covering material C is a rod-shaped or plate-shaped member made of ceramics with a porosity of 60% or less, at least the bottom surface (the surface in contact with the protective layer film 90α) being substantially flat. Alumina is exemplified as the ceramic used for the covering material C, but other materials may be used as long as the ceramics can withstand the above-mentioned co-firing temperature of 1200°C or more. The covering material C has an appropriate thickness selected from the range of 1 mm to 10 mm depending on its shape, porosity, etc.

[0107] By placing the covering material C, the path of evaporation and scattering of Au during the process of firing the detection electrode film 60α to become the detection electrode 60 is blocked, thereby suppressing the adhesion and adsorption of Au to other parts, and suppressing the weight loss of the detection electrode 60 in the final sensor element 101 and the decrease in the concentration of Au on the metal particle surface.

[0108] In any of the cases of Fig. 4(a) to Fig. 4(e), the length of the covering material C in the short-side direction of the element (not shown) is equal to or greater than the length of the sensing electrode film 60α in the short-side direction of the element.

[0109] For example, Fig. 4(a) and Fig. 4(b) show a case where a covering material C (C1) having a size L1 in the element longitudinal direction equal to the size L0 of the detection electrode film 60α in the element longitudinal direction is placed on the detection electrode film 60α via a protective layer 90α. That is, the state where the entire upper surface of the detection electrode film 60α is covered with the covering material C1 is shown.

[0110] When the covering material C1 is placed in this manner, the evaporation and scattering of Au is suppressed more effectively than when the covering material C1 is not provided.

[0111] 4(c) shows a case where a covering material C (C2) having a size L2 in the element longitudinal direction larger than the size L0 of the detection electrode film 60α in the element longitudinal direction is placed on the detection electrode film 60α via a protective layer film 90α. In this case, the entire upper surface of the detection electrode film 60α is covered with the covering material C2. Furthermore, the entire area between the detection electrode film 60α and the pump electrode film 23α and the pump electrode film 23α are also covered with the covering material C2.

[0112] In the case where the covering material C2 is placed in this manner, the evaporation and scattering of Au is also effectively suppressed. In addition, compared to the case where the covering material C1 shown in Fig. 4(b) is placed, the adhesion and adsorption of Au to the outer pump electrode 23 is more reliably suppressed. This more reliably suppresses the deterioration of the detection accuracy of NOx caused by such adhesion and adsorption.

[0113] 4(d) shows a case where a covering material C (C3) having a size L3 in the element longitudinal direction that is half the size L0 of the detection electrode film 60α in the element longitudinal direction is placed on the detection electrode film 60α via a protective layer 90α. More specifically, the half of the detection electrode film 60α close to the pump electrode film 23α is covered by the covering material C3.

[0114] When the covering material C3 is placed in this manner, the half of the detection electrode film 60α farther from the pump electrode film 23α is not covered by the covering material C3, so that although it is possible that Au may evaporate and scatter from this side through the surface protective layer 90, such evaporation and scattering is suppressed compared to the case where co-firing is performed without placing the covering material C3. Moreover, because the covering material C3 is placed on the side closer to the pump electrode film 23α, adhesion and adsorption of Au to the outer pump electrode 23 is suitably suppressed. In other words, deterioration of the NOx detection accuracy caused by such adhesion and adsorption is suppressed.

[0115] Figure 4(e) shows a case in which the same covering material C1 as that placed on the detection electrode film 60α in Figure 4(b) is shifted toward the pump electrode film 23α side more than in the case shown in Figure 4(b) so as to cover the detection electrode film 60α by a width L3 that is half the size L0 of the detection electrode film 60α in the element longitudinal direction.

[0116] 4(d), the half of the detection electrode film 60α farther from the pump electrode film 23α is not covered by the covering material C3, and therefore, although Au may evaporate and scatter from this side through the surface protective layer 90, such evaporation and scattering is suppressed compared to the case where co-firing is performed without placing the covering material C1. Moreover, since the covering material C1 is placed so as to cover a part of the region between the detection electrode film 60α and the pump electrode film 23α, the adhesion and adsorption of Au to the outer pump electrode 23 is suppressed more effectively than in the case shown in FIG. 4(d).

[0117] As shown in Figures 4(d) and 4(e), even if the detection electrode film 60α is partially covered during co-firing, the evaporation and scattering of Au from the detection electrode film 60α is suppressed, and the weight loss of the detection electrode 60 in the final sensor element 101 and the decrease in the concentration of Au on the metal particle surfaces are suppressed.

[0118] Specifically, when the coverage is defined as the ratio of the planar area of ​​the portion of the detection electrode film 60α covered by the covering material C to the planar area of ​​the entire detection electrode film 60α, arranging the covering material C so that the coverage is 30% or more can suitably suppress the weight loss of the detection electrode 60 in the sensor element 101 and the decrease in the Au concentration on the metal particle surface. For example, an Au concentration of 15% or more, which is required for the dependency of the potential difference EMF on the NH3 gas concentration in the mixed potential cell 61 to become significant, can be suitably ensured.

[0119] <Examples of covering material shapes and arrangements> Next, various examples of the specific shape of the covering material C and the arrangement during co-firing will be described in order. Fig. 5 is a diagram showing an example of the arrangement of the element body 101α relative to the sintered sheath S, which is the premise of the above. Figs. 6 to 10 are enlarged views of the main part showing various examples of placing the covering material C on the element body 101α arranged in the sintered sheath S. Note that the protective layer film 90α is omitted in Figs. 5 to 10.

[0120] In the example shown in Fig. 5, a total of 44 element bodies 101α having the electrode arrangement illustrated in Fig. 2(a) are arranged in two rows with the pump electrode film 23α, the detection electrode film 60α, the lead wire film 23Lα, the lead wire film 60Lα, and the terminal electrode film 77α facing upward, and are arranged in a firing sheath S so that the ends of the pump electrode film 23α and the detection electrode film 60α of the element bodies 01α belonging to each row GL and row GR face each other in the left-right direction as viewed in the drawing. The lead wire film 23Lα, the lead wire film 60Lα, and the terminal electrode film 77α are paste films that become the lead wire 23L, the lead wire 60L, and the terminal electrode film 77α after co-firing, respectively. The 22 element bodies 01α belonging to each row GL and row GR are arranged so that 11 of them are spaced apart from each other in the vertical direction as viewed in the drawing.

[0121] In each of the 22 elements 01α belonging to each of the rows GL and GR, the positions of the detection electrode films 60α in the left-right direction in the drawing are the same as each other. In other words, the detection electrode films 60α of the individual elements 101α are arranged in a row along the up-down direction in the drawing.

[0122] FIG. 6 shows an example in which a rod-shaped covering material C (Ca) having a width La equal to the size L0 of the detection electrode film 60α in the element longitudinal direction is arranged on the row of the detection electrode film 60α along the vertical direction as viewed in the drawing in each of the rows GL and GR. In this case, the covering material Ca is arranged so as to be perpendicular to the longitudinal direction of each element body 101α. In this case, in each element body 101α, the entire upper surface of the detection electrode film 60α is covered by the covering material Ca as in the case shown in FIG. 4(b). That is, the coverage rate is 100%.

[0123] FIG. 7 shows an example in which a rod-shaped or plate-shaped covering material C (Cb) having a width Lb larger than the size L0 of the detection electrode film 60α in the element longitudinal direction is arranged on the row of the detection electrode film 60α in each of the rows GL and GR. In this case, in each element body 101α, the entire upper surface of the detection electrode film 60α is covered by the covering material Cb as in the case shown in FIG. 4(c). That is, the coverage rate is 100%. In addition, in FIG. 4(c), the entire pump electrode film 23α is also covered by the covering material Cb.

[0124] FIG. 8 shows an example of the arrangement of the covering material C which differs between row GL and row GR.

[0125] In the row GL, a rod-shaped covering material C (Cc) having a width Lc of 50% of the size L0 of the detection electrode film 60α in the element longitudinal direction is arranged on the row of the detection electrode films 60α. In this example, the half of each detection electrode film 60α close to the pump electrode film 23α is covered by the covering material Cc, and the opposite half is exposed.

[0126] In row GR, an example is shown in which the same covering material Ca as shown in Figure 6 is shifted toward the pump electrode film 23α and placed over the row of detection electrode films 60α so that each detection electrode film 60α is exposed by 50% of the size L0 in the longitudinal direction of the element.

[0127] The former corresponds to the case of Fig. 4(d), and the latter corresponds to the case of Fig. 4(e). In either case, half of the planar area S0 of the detection electrode film 60α is covered, and the remaining half is exposed, so the coverage rate is 50%. Note that this embodiment in which the covering materials C are arranged differently in the left and right columns is merely for the purpose of explanation, and the same covering materials C are usually arranged in the same way.

[0128] Figure 9 shows an example in which the same covering material C (Cd) is arranged in different manners for four element groups: element group GL1 at the upper side of the row GL as viewed in the drawing, element group GL2 at the lower side of the row GL as viewed in the drawing, and element group GR1 at the upper side of the row GR as viewed in the drawing, and element group GR2 at the lower side of the row GR as viewed in the drawing.

[0129] The covering material Cd has a plate shape (chip shape) having the same planar shape as the detection electrode film 60.alpha.. In Fig. 9, each detection electrode film 60.alpha. is covered with an individual covering material Cd.

[0130] A covering material Cd is disposed on the detection electrode film 60α of each element 101α belonging to the element group GL1 so as to completely cover the detection electrode film, which corresponds to the case shown in FIG. 4(b), and the coverage rate is 100%.

[0131] The covering material Cd is arranged so that the detection electrode film 60α of each element body 101α belonging to the element group GL2 is entirely covered in the element short-side direction, while in the element long-side direction, 70% of the size L0 is exposed on the side closer to the pump electrode film 23α. In this case, the coverage rate is 30%.

[0132] The covering material Cd is arranged so that the detection electrode film 60α of each element body 101α belonging to the element group GR1 is entirely covered in the element short-side direction, while in the element long-side direction, 70% of the size L0 is exposed on the side farther from the pump electrode film 23α. In this case, the coverage rate is also 30%.

[0133] The covering material Cd is arranged on the detection electrode film 60α of each element body 101α belonging to the element group GR2 so that a part of the detection electrode film 60α is exposed in both the short-side direction and the long-side direction of the element. In this case, 70% of the planar area S0 of the detection electrode film 60α is exposed, so that the coverage rate is 30%.

[0134] As in the case shown in FIG. 8, the arrangement of the covering material C in a different manner as shown in FIG. 9 is merely for illustrative purposes.

[0135] 6 to 8, the embodiment using the rod-shaped covering material C has the advantage that it can be placed on multiple detection electrode films 60α at once. However, from the viewpoint of handling, it is somewhat difficult to make the thickness of the covering material C thin, and in light of the purpose of covering the detection electrode films 60α, there may be parts of the covering material C that are essentially unnecessary, so that when the covering material C is placed on the detection electrode films 60α, the load acting on the detection electrode films 60α may become large.

[0136] On the other hand, in the case of covering each detection electrode film 60α individually with a plate-shaped covering material C as shown in Figure 9, although the arrangement becomes complicated when there are a large number of target element bodies 101α, it is relatively easy to make the material thin and it can be arranged in the minimum necessary area, so that it is possible to reduce the load acting on the detection electrode film 60α compared to the case where a rod-shaped covering material C is used.

[0137] Figure 10 shows an example of the arrangement of covering materials C which differs between rows GL and GR in a case where a total of 44 element bodies 101α having the electrode arrangement illustrated in Figure 2(b) are arranged in a sintered sheath S in rows GL and GR, unlike the cases shown in Figures 5 to 9.

[0138] In the row GL, an example is shown in which the covering material Ca is disposed on the row of the detection electrode films 60α aligned in the vertical direction as viewed in the drawing, similarly to Fig. 6. In this case, the coverage rate is 100%.

[0139] 8, the covering material Ca is shifted toward the pump electrode film 23α and disposed on the row of the sensing electrode films 60α so that each sensing electrode film 60α is exposed by 50% of the size L0 in the element longitudinal direction. In this case, the coverage is 50%.

[0140] As shown in Figures 6 to 10, there are various embodiments for the shape, size, and arrangement of the covering material C that is placed on the detection electrode film 60α during co-firing. However, as long as the covering material C made of a ceramic with a porosity of 60% or less is placed on the detection electrode film 60α with a coverage rate of 30% or more, the evaporation and scattering of Au that occurs during co-firing is suppressed, thereby suppressing the adhesion and adsorption of Au to other parts, and thus suppressing the weight loss of the detection electrode 60 in the final sensor element 101 and the decrease in the concentration of Au on the metal particle surfaces.

[0141] As described above, according to this embodiment, when a gas sensor element having a base material made of a solid electrolyte and a detection electrode containing Au as a metal component on its surface is manufactured by co-firing, a covering material is placed on the electrode film so that 30% or more of the electrode film that becomes the detection electrode by firing is covered, thereby suppressing the evaporation and scattering of Au during co-firing. This suppresses the adhesion and adsorption of Au to other parts, and suppresses the weight loss of the detection electrode in the finally obtained sensor element and the decrease in the concentration of Au on the metal particle surface. Furthermore, when the detection electrode is an NH3 detection electrode that constitutes a mixed potential cell, the sensitivity characteristic to NH3 is suitably secured. Furthermore, when an external pump electrode that constitutes an electrochemical pump cell for detecting NOx is further provided on the surface of the sensor element, the adhesion and adsorption of Au to the external pump electrode is suitably suppressed.

[0142] <Modification> In the above embodiment, the gas sensor 100 including the sensor element 101 is a multi-gas sensor capable of simultaneously measuring the concentrations of NH3 and NOx in parallel, but this is not a required aspect. As long as a sensor element having a detection electrode containing Au as a metal component on its surface is manufactured by co-firing, the effect of suppressing the evaporation and scattering of Au during co-firing, as well as the weight loss of the detection electrode and the decrease in the concentration of Au, can be obtained by using a covering material as in the above embodiment, even when a sensor element having a different configuration is manufactured. For example, the use of a covering material is also effective in manufacturing a sensor element having only a mixed potential cell 61.

[0143] Furthermore, in the above-described embodiment, NH3 is detected by the mixed potential cell, but other gas species such as hydrocarbon gases may be detected.

[0144] When multiple elements 101α are placed in the firing sheath S and co-fired in the manner shown in Fig. 5, multiple load rods may be placed to suppress deformation of the elements 101α. The load rods are placed at predetermined intervals in the longitudinal direction of the elements 101α so as to extend in a direction perpendicular to the longitudinal direction of each element 101α. When rod-shaped covering materials C are placed as shown in Figs. 6 to 8 and 10, the load rods and covering materials C are placed approximately parallel to each other.

[0145] Alternatively, the load rod may be disposed on the element body 101α in parallel to the element body 101α. Fig. 11 is a diagram showing an example of such a load rod arrangement. However, for simplicity of illustration, the pump electrode film 23α, the detection electrode film 60α, the lead wire film 23Lα, the lead wire film 60Lα, and the terminal electrode film 77α are shown only in some of the element bodies 101α, and the others are omitted.

[0146] In Fig. 11, the elements 101α are aligned in a sintered sheath S in the same manner as in Fig. 5. For the element group GL1 on the upper left side in the drawing, a rod-shaped covering material C (Ce) is arranged on the row of detection electrode films 60α aligned in the vertical direction in the drawing, and for each of the elements 101α belonging to the element group GL2 on the lower left side in the drawing, a chip-shaped covering material C (Cf) is arranged on each detection electrode film 60α.

[0147] In addition, in most of the area toward the rear end side (terminal electrode film 77α side) of the arrangement positions of the covering materials Ce, Cf, a load bar W is arranged on top of and parallel to each element body 101α belonging to element groups GL1 and GL2.

[0148] Alternatively, the covering material may also function as a load rod. Fig. 12 is a diagram showing an example of the arrangement of such covering materials. In Fig. 12, the element bodies 101α are aligned in the sintered sheath S in the same manner as in Fig. 5. However, in Fig. 12, the pump electrode film 23α, the detection electrode film 60α, the lead wire film 23Lα, the lead wire film 60Lα, and the terminal electrode film 77α are shown only in some of the element bodies 101α, and the rest are omitted, as in Fig. 11.

[0149] In the case shown in Figure 12, a rod-shaped covering material C (Cg) is arranged on each element 101α belonging to the element group GL1 on the upper left side of the drawing, parallel to the element 101α and in a manner covering most of the area of ​​the element 101α.

[0150] Furthermore, a rod-shaped covering material C(Ch) which is even longer than the covering material Cg is arranged in a straight line in such a manner as to cover most of the area of ​​each of the pairs of element body 101α belonging to element group GL2 on the lower left side of the drawing and element body 101α belonging to element group GR2 on the lower right side of the drawing.

[0151] Moreover, if the width Lb of the covering material Cb shown in FIG. 7 is increased to be approximately equal to the length of the element body 101α, the plate-like covering material Cb will also function as a load rod. EXAMPLES

[0152] (Confirmation of the effect on Au residual rate and Au concentration) The sensor elements 101 were manufactured by varying the combination of the porosity of the covering material C and the coverage of the sensing electrode film 60α, and the Au residual rate and the Au concentration degree in the sensing electrode were evaluated.

[0153] Specifically, the porosity of the alumina covering material C was varied to four levels: 1%, 10%, 40%, and 60%, and the coverage of the detecting electrode film 60α with each covering material C when placed on the detecting electrode film 60α was varied to seven levels: 10%, 30%, 50%, 70%, 100%, 150%, and 200%. The co-firing temperature was 1400°C. For comparison, co-firing without a covering material was also performed.

[0154] The Au retention rate was calculated based on equation (2), and the Au concentration was calculated based on equation (1).

[0155] In addition, a coverage rate of 150% or 200% means that the entire detection electrode film 60α in each element body 101α is covered by the covering material C, and the area covered by the covering material C is 150% or 200% of the planar area of ​​the detection electrode film 60α.

[0156] Fig. 13 is a graph in which the Au residual rate is plotted against the coverage rate for each sensor element 101 manufactured using covering materials C with the same porosity. Also, Fig. 14 is a graph in which the Au concentration is plotted against the coverage rate for each sensor element 101 manufactured using covering materials C with the same porosity.

[0157] It can be seen from Figure 13 that when covering material C is not used, the Au residual rate remains at a few percent, whereas when covering material C is used, the Au residual rate tends to increase as the coverage rate increases. It can also be seen that, although the Au residual rate value differs depending on the porosity when the coverage rate exceeds 30%, the difference is at most about 10%.

[0158] 14, it is confirmed that the Au concentration remains at a few percent when the covering material C is not used, whereas the Au concentration tends to increase as the coverage rate increases when the covering material C is used. In addition, it is considered that the NH3 gas can be suitably detected in the mixed potential cell 61 including the detection electrode 60 if the Au concentration is 15% or more, and it is confirmed from FIG. 12 that the requirement is met if the coverage rate is 30% or more.

[0159] However, when the coverage rate exceeds 30%, the Au enrichment value differs depending on the porosity. When the porosity of covering material C is 60%, even when the coverage rate is 200%, it is confirmed that the Au enrichment rate is approximately 15% lower when the porosity is 10% or less.

[0160] The above results show that the greater the coverage of the detection electrode film 60α by the covering material, the more effective it is in suppressing the weight loss and the reduction in the Au concentration of the detection electrode 60. Furthermore, it shows that by performing co-firing in a state where the detection electrode film 60α is covered with a covering material C having a porosity of at least 60% at a coverage rate of 30% or more, the weight loss of Au can be suppressed compared to the case where a covering material is not used, and a degree of Au concentration of 15% or more can be achieved, which enables the mixed potential cell 61 including the detection electrode to suitably detect NH3 gas.

[0161] (Confirmation of scattering suppression) The presence or absence of Au adhesion when the sensor element 101 was produced by co-firing was examined by performing XPS analysis at two points A and B in FIG. 2(b) for both the case where the covering material C was used and the case where it was not used. Table 1 shows the results. Point A is on the outer pump electrode 23, and point B is on the terminal electrode 77. In addition, as the covering material C, an alumina covering material with a porosity of 10% was prepared, and the covering material was arranged so as to have a coverage rate of 200% and co-firing was performed. The co-firing temperature was 1400°C. The amount of Au is shown as a relative value when the intensity value of the Au and Pt detection peaks in the XPS analysis results are used and the intensity value of Pt is set to 100.

[0162] [Table 1]

[0163] As can be seen from Table 1, when no covering material was used, Au was detected at point A, but when a covering material was used, Au was not detected at either point A or point B. This result indicates that the use of a covering material is particularly effective in suppressing the scattering of Au in the vicinity of the detection electrode 60.

[0164] (Checking sensitivity characteristics) Using alumina covering material C with a porosity of 1%, sensor elements 101 were fabricated with different covering rates during co-firing, and each was used to fabricate a gas sensor 100. The detection sensitivity of each gas sensor was evaluated using a model gas with a known concentration of NH3 gas.

[0165] Specifically, the coverage was varied to five levels: 10%, 30%, 50%, 100%, and 200%. For comparison, a gas sensor having a sensor element fabricated without using a covering material during co-firing was also prepared.

[0166] The concentration of NH3 gas in the model gas was varied to four levels: 1 ppm, 10 ppm, and 1000 ppm. In addition to NH3, each model gas contained 10% O2, 6% H2O, and the remainder was N2.

[0167] Then, each gas sensor 100 was driven in a model gas atmosphere, and the potential difference EMF generated in the mixed potential cell 61 was obtained as an output value.

[0168] 15 is a diagram in which the output value of each gas sensor 100 is plotted against the concentration of NH3 gas in the model gas. The gas sensors 100 are distinguished by the coverage (at the time of co-firing) when the sensor element 101 included therein is produced.

[0169] 15 confirms that there is no dependency on the concentration of NH3 gas in the range exceeding 10 ppm for the gas sensor 100 in which the coverage during co-firing in producing the sensor element 101 was 10% or less. Considering this result together with the result shown in FIG. 14, it is determined that good sensitivity characteristics can be obtained in the mixed potential cell 61 in the gas sensor 100 in which the coverage during co-firing is 30% or more and thus the Au concentration in the detection electrode 60 is 15% or more. [Explanation of symbols]

[0170] 1~3 1st~3rd substrate layer 4 First solid electrolyte layer 5 Spacer layer 6 Second solid electrolyte layer 10 Gas inlet 11 First diffusion-controlled section 12 Buffer space 13 Second diffusion-controlled section 20 1st internal void 21 Main pump cell 22 Inner pump electrode 23 Outer pump electrode 23α Pump electrode membrane 23L, 60L lead wire 23Lα, 60Lα Lead wire film 30 Third diffusion-controlled section 40 Second internal void 41 Measuring pump cell 42 Reference electrode 44 Measuring electrode 45 4th diffusion-controlled section 50 Auxiliary pump cell 60 Detection electrode 60α Detection electrode film 61 Mixed Potential Cell 70 Heater section 71 Heater electrode 77 Terminal electrode 77α Terminal electrode film 90 Surface protective layer 90α protective layer film 100 Gas Sensor 101 Sensor element 101α element body S firing sheath

Claims

1. A method for manufacturing a sensor element of a gas sensor having an electrode containing Au on a surface thereof, comprising the steps of: a first film formation step of forming a first paste film, which will become the Au-containing electrode upon firing, on a surface of an element body which will become the sensor element upon firing; a second film formation step of forming a protective layer film which becomes a surface protective layer by firing on the element body which has been subjected to the first film formation step; a covering material placing step of placing a covering material made of ceramics and having a porosity of 60% or less on the protective layer film so that at least a portion of the first paste film is covered with a coverage rate of 30% or more; a co-firing step of firing the element body including the first paste film and the protective layer film together with the covering material at a temperature of 1200° C. or more and 1500° C. or less; Equipped with The covering material is removed after the co-firing step. A method for manufacturing a sensor element.

2. A method for manufacturing the sensor element according to claim 1, comprising the steps of: a sheath arrangement step of arranging the plurality of element bodies on which the first paste film is formed in a firing sheath so that the first paste films are arranged in a row; Further equipped with In the covering material placing step, the rod-shaped covering material is placed on the row of the first paste films. A method for manufacturing a sensor element.

3. A method for manufacturing the sensor element according to claim 1, comprising the steps of: a sheath arrangement step of arranging one or more element bodies on which the first paste film is formed into a sintered sheath; Further equipped with In the covering material placement step, a plate-shaped covering material is placed on each of the first paste films of the one or more element bodies. A method for manufacturing a sensor element.

4. A method for manufacturing a sensor element according to any one of claims 1 to 3, comprising the steps of: The thickness of the covering material is 1 mm or more and 10 mm or less. A method for manufacturing a sensor element.

5. A method for manufacturing a sensor element according to any one of claims 1 to 4, comprising the steps of: The covering material is made of alumina. A method for manufacturing a sensor element.

6. A method for manufacturing a sensor element according to any one of claims 1 to 5, comprising the steps of: The Au-containing electrode contains a Pt-Au alloy as a metal component, and NH 3 NH gas whose catalytic activity against the gas is disabled 3 A sensing electrode, The sensor element has a base portion made of an oxygen ion conductive solid electrolyte, and the NH 3 A detection electrode, a reference electrode provided inside the sensor element, and the NH 3 a mixed potential cell including a sensing electrode and a solid electrolyte between the sensing electrode and the reference electrode; 3 The gas sensor unit is provided. A method for manufacturing a sensor element.

7. A method for manufacturing a sensor element according to claim 6, comprising the steps of: The sensor element is At least one internal space into which a gas to be measured is introduced from an external space; A NOx measuring electrode formed facing the at least one internal cavity; an outer pump electrode formed on a surface of the sensor element; a NOx sensor portion including a measurement pump cell which is an electrochemical pump cell, the measurement pump cell being constituted by the NOx measurement electrode, the outer pump electrode, and a solid electrolyte between the NOx measurement electrode and the outer pump electrode; The present invention further comprises: In the first film forming step, a second paste film is further formed, the second paste film being fired to become the outer pump electrode; In the covering material placing step, the covering material is arranged so as to cover at least a side of the first paste film close to the second paste film. A method for manufacturing a sensor element.

8. A method for manufacturing a sensor element according to claim 7, comprising the steps of: In the covering material placement step, the covering material is disposed so as to cover at least a portion of the first paste film and at least a portion of the region between the first paste film and the second paste film. A method for manufacturing a sensor element.

Citation Information

Patent Citations

  • Triple joint type propeller shaft

    JP1984038133A

  • Gas sensor detection electrode, gas sensor and production method of gas sensor

    JP2017090405A

  • Ammonia gas sensor, manufacturing method of conductive paste, and manufacturing method of gas sensor

    JP2017116371A

  • Gas sensor and gas concentration measurement method employing gas sensor

    JP2018031732A

  • Gas sensor

    JP2018040746A