Device and manufacturing method thereof

By using a polymer-bound inorganic particle insulating layer with a 10% thickness variation coefficient, the issues of uneven thickness and high leakage current in capacitors and FETs are addressed, enhancing device performance and yield.

JP7578010B2Active Publication Date: 2024-11-06TORAY INDUSTRIES INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021016320
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-26
Filing Date
2021-02-04
Publication Date
2024-11-06
Estimated Expiration
2041-02-04

AI Technical Summary

Technical Problem

Existing methods for manufacturing electronic devices such as capacitors and field-effect transistors (FETs) using insulating layers with added inorganic compounds result in uneven thickness, leading to increased leakage current, particularly in capacitors with large lower electrodes.

Method used

The development of an insulating layer composed of a polymer bound to inorganic particles, ensuring a film thickness variation coefficient of 10% or less, which reduces leakage current and maintains a high dielectric constant.

Benefits of technology

The solution achieves a uniform thickness in the insulating layer near the electrodes, resulting in devices with both high dielectric constant and low leakage current, improving yield and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578010000010
    Figure 0007578010000010
  • Figure 0007578010000011
    Figure 0007578010000011
  • Figure 0007578010000012
    Figure 0007578010000012
Patent Text Reader

Abstract

To provide an element, such as a capacitor or a field effect transistor, including an insulating layer with a high dielectric constant and reduced leak current, and a manufacturing method for the same.SOLUTION: A field effect transistor (FET) 1 is an element in which at least a patterned lower electrode (gate electrode 11), an insulating layer (gate insulating layer 12), and a patterned upper electrode (source electrode 13 and drain electrode 15) are stacked on an insulating base material 100. The insulating layer contains polymer coupled with an inorganic particle. The variation coefficient of the film thickness of a part of the insulating layer formed on the lower electrode that is not covered with the upper electrode is within 10%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an element and a manufacturing method thereof, and more particularly to an element such as a capacitor or a field effect transistor and a manufacturing method thereof. [Background technology]

[0002] In recent years, technologies that use coating methods to manufacture electronic devices such as electronic paper, flexible sensors, and RFID (Radio Frequency IDentification) tags have been investigated. Coating methods can be used to avoid vacuum and high-temperature processes, making it possible to manufacture electronic devices at low cost.

[0003] Electronic devices contain elements such as field-effect transistors (FETs) and capacitors, which require an insulating layer to insulate the upper and lower electrodes.

[0004] The insulating layer in a FET is the gate insulating layer that separates the semiconductor layer, source electrode, and drain electrode from the gate electrode. The electrical characteristics, surface smoothness, and film thickness of the gate insulating layer have a significant effect on FET characteristics such as leakage current value and FET ON / OFF current value.

[0005] The insulating layer in a capacitor is a dielectric film that separates the upper and lower electrodes and accumulates the electric charge generated by the electric field applied between the upper and lower electrodes. The electrical properties, surface smoothness, and film thickness of the dielectric film have a significant effect on the capacitor properties such as leakage current value and accumulated charge amount.

[0006] As materials for the insulating layer, organic materials that are soluble in organic solvents, such as organic polymers, have been actively studied. These can be formed into thin films at low cost using coating methods such as slit coating, and can be formed into thin films on film substrates such as polyethylene terephthalate using low-temperature processes. In particular, the addition of inorganic compounds to the insulating layer has been actively studied in order to increase the dielectric constant of the insulating layer.

[0007] Known examples of insulating layers in which an inorganic compound is added to an organic polymer include a gate insulating layer containing polysiloxane chemically bonded to inorganic particles (see, for example, Patent Document 1) and a gate insulating layer containing a polymer and inorganic oxide particles (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2019 / 065561 [Patent Document 2] JP 2013-115162 A Summary of the Invention [Problem to be solved by the invention]

[0009] However, it has become clear that the technology described in Patent Document 1 has a problem in that the unevenness in the thickness of the insulating layer in the vicinity of the lower electrode becomes large, and the leakage current of the element becomes large. Furthermore, Patent Document 1 does not mention capacitors, and it has been found that the above problem is particularly prominent in capacitors with a large lower electrode area.

[0010] Furthermore, when the inventors studied the technology of Patent Document 2, they found that although the unevenness in the thickness of the insulating layer was small, the formation of conductive paths by some of the aggregated inorganic particles caused an increase in the leakage current of the capacitor.

[0011] The present invention has been made in view of the above-mentioned problems, and has an object to provide an element for an electronic device having an insulating layer with a high dielectric constant and reduced leakage current. [Means for solving the problem]

[0012] The present invention is an element having at least (1) a patterned lower electrode, (2) an insulating layer, and (3) a patterned upper electrode laminated on a substrate, the insulating layer containing a polymer (A) bonded to inorganic particles, and the insulating layer formed on the lower electrode has a film thickness variation coefficient of 10% or less in a portion not covered by the upper electrode. Effect of the Invention

[0013] According to the element of the present invention, by having an insulating layer with a high uniformity in thickness near and on the electrode, it is possible to obtain an element in which the insulating layer has both a high dielectric constant and a low leakage current. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a field-effect transistor according to an embodiment of the present invention; [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of a field-effect transistor according to an embodiment of the present invention; [Diagram 3] FIG. 1 is a schematic cross-sectional view showing an example of a field-effect transistor according to an embodiment of the present invention; [Figure 4] FIG. 1 is a schematic cross-sectional view showing an example of a field-effect transistor according to an embodiment of the present invention; [Diagram 5] FIG. 1 is a schematic cross-sectional view showing an example of a field-effect transistor according to an embodiment of the present invention; [Figure 6] FIG. 1 is a schematic cross-sectional view showing an example of a field-effect transistor according to an embodiment of the present invention; [Figure 7] FIG. 1 is a schematic cross-sectional view showing an example of a capacitor according to an embodiment of the present invention; [Figure 8] FIG. 1 is a schematic cross-sectional view showing an example of a circuit obtained by using the electronic device element of the present invention. [Figure 9] FIG. 1 is a schematic cross-sectional view showing an example of a circuit obtained by using the electronic device element of the present invention. [Figure 10] FIG. 1 is a schematic cross-sectional view showing an example of a circuit obtained by using the electronic device element of the present invention. [Figure 11] FIG. 1 is a block diagram showing an example of a wireless communication device using a field-effect transistor according to the present invention. [Figure 12] FIG. 1 is a schematic cross-sectional view showing an example of a capacitor according to an embodiment of the present invention; [Figure 13] FIG. 1 is a schematic cross-sectional view showing an example of a field-effect transistor according to an embodiment of the present invention; [Figure 14] FIG. 1 is a schematic cross-sectional view showing an example of a circuit obtained by using the electronic device element of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Preferred embodiments of the element according to the present invention will be described in detail below. However, the present invention is not limited to the following embodiments and can be modified in various ways depending on the purpose and application.

[0016] <Element> An element according to an embodiment of the present invention is an element having at least (1) a patterned lower electrode, (2) an insulating layer, and (3) a patterned upper electrode laminated on a substrate, the insulating layer containing a polymer (A) bonded to inorganic particles, and the insulating layer having a coefficient of variation in thickness in a portion on the lower electrode that is not covered by the upper electrode, within 10%.

[0017] Examples of the element include a field effect transistor (FET) and a capacitor.

[0018] An example of a FET is an element having a gate electrode, a gate insulating layer, a source electrode, a drain electrode, and a semiconductor layer in contact with the source electrode and the drain electrode.

[0019] The capacitor includes an element having a lower electrode, an upper electrode, and a dielectric film between the lower electrode and the upper electrode.

[0020] The insulating layer in the present invention functions as a gate insulating layer in the above-mentioned FET, and as a dielectric film in the capacitor.

[0021] In the present invention, the film thickness of the insulating layer on the lower electrode and not covered by the upper electrode refers to the arithmetic mean (average film thickness) of the film thickness at 15 randomly selected locations among the locations in the insulating layer that correspond to the above-mentioned location. The first measurement method is a measurement using an optical interference spectroscopic film thickness measuring device. The second measurement method is a measurement method in which the cross section of the insulating layer is observed using a scanning electron microscope (SEM) or a transmission electron microscope (TEM) and the height of the cross section is measured and calculated. If the first measurement method is not possible, the second measurement method is used. If both the first measurement method and the second measurement method are possible, the value measured by the first measurement method is adopted. The standard deviation of the film thickness at the 15 locations divided by the average film thickness is used as the variation coefficient of the film thickness of the insulating layer.

[0022] [Embodiment 1: FET] Fig. 1 is a schematic cross-sectional view showing a FET which is an element according to a first embodiment of the present invention. This FET 1 has an insulating substrate 100, a gate electrode 11, a gate insulating layer 12, a source electrode 13, a drain electrode 15, and a semiconductor layer 14 in contact with the source electrode and the drain electrode. The semiconductor layer and the gate electrode are electrically separated by the gate insulating layer. In the FET 1 shown in Fig. 1, there is no overlap between the gate electrode 11 and the source electrode 13 / drain electrode 15, and the width of the semiconductor layer 14 and the width of the gate electrode are the same.

[0023] In the first embodiment, the gate electrode 11 is the "patterned lower electrode", the gate insulating layer 12 is the "insulating layer", and the source electrode 13 and the drain electrode 15 are the "patterned upper electrodes".

[0024] 2 to 6 are schematic cross-sectional views showing modifications of the FET according to the first embodiment.

[0025] In the FET 2 according to the first modification shown in FIG. 2, the gate electrode 11 overlaps with the source electrode 13 and the drain electrode 15 .

[0026] In a FET 3 according to the second modification shown in FIG. 3, there is no overlap between the gate electrode 11 and the source electrode 13 / drain electrode 15, and the width of the semiconductor layer 14 is larger than the width of the gate electrode.

[0027] In a FET 4 according to a third modification shown in FIG. 4, the gate electrode 11 and the source electrode 13 overlap, and in a FET 5 according to a fourth modification shown in FIG.

[0028] 1 to 5 show examples of a bottom gate structure, whereas a FET 6 according to Modification 5 shown in Fig. 6 has a top gate structure, in which the gate electrode 11 does not overlap with the source electrode 13 and the drain electrode 15. In Modification 5, the source electrode 13 and the drain electrode 15 are "patterned lower electrodes", and the gate electrode 11 is "patterned upper electrode".

[0029] (Gate insulation layer) The FET according to the embodiment of the present invention contains a polymer (A) bonded to inorganic particles in the gate insulating layer, which will be described later. In such a case, the thickness of the gate insulating layer generally becomes uneven around the lower electrode or on the lower electrode. In a portion where the gate insulating layer is thin, the element may not operate due to the occurrence of leakage current. On the other hand, in a portion where the gate insulating layer is thick, the on-current tends to become small. Thus, when the thickness of the gate insulating layer is large, the FET characteristics are deteriorated. Furthermore, in a substrate having a plurality of FETs, the thickness of the gate insulating layer becomes uneven, and the FET characteristics of each FET in the substrate become uneven.

[0030] In the FET according to the embodiment of the present invention, the coefficient of variation of the thickness of the gate insulating layer is 10% or less. This indicates that the thickness unevenness of the gate insulating layer is small. This reduces the leakage current and improves the yield of device formation. The coefficient of variation of the thickness of the gate insulating layer is more preferably 8% or less, and further preferably 5% or less.

[0031] Methods for making the coefficient of variation of the thickness of the gate insulating layer 10% or less include a method of making the gate insulating layer contain a specific surface modifier, a method of making the gate insulating layer contain a specific polymer (B), etc. The details of these will be described later.

[0032] The thickness of the gate insulating layer on the lower electrode is preferably 10 nm or more, more preferably 25 nm or more, and particularly preferably 50 nm or more, and is preferably 1000 nm or less, more preferably 750 nm or less, and particularly preferably 500 nm or less.

[0033] The gate insulating layer is composed of a single layer or multiple layers. In the case of multiple layers, a plurality of preferable gate insulating layers described below may be laminated, or the preferable gate insulating layer may be laminated with a known gate insulating layer.

[0034] The relative dielectric constant of the gate insulating layer is preferably 4 or more, more preferably 7 or more, even more preferably 8.5 or more, and particularly preferably 10 or more. By having the relative dielectric constant in the above range, the on-current of the FET can be increased. In addition, the relative dielectric constant is preferably 20 or less, more preferably 15 or less, even more preferably 13.5 or less, and particularly preferably 12 or less. By having the relative dielectric constant in the above range, excessive dielectric loss due to the gate insulating layer can be prevented, and in particular, an FET driven by radio waves in a high frequency band of 100 MHz or more can operate accurately. The relative dielectric constant ε of the gate insulating layer r can be calculated using the following formula (a).

[0035] ε r =C D / (S ε0) (a) where C(F) is the capacitance of the gate insulating layer, D(m) is the thickness of the gate insulating layer, and S(m 2 ) is the area of ​​the electrodes sandwiching the gate insulating layer, and ε0 is the dielectric constant of vacuum (8.85×10 -12 F / m).

[0036] (Inorganic particles) The inorganic particles used in the FET according to the embodiment of the present invention are not particularly limited as long as they are particles made of an inorganic substance. Since the inorganic particles have a small shrinkage rate during thermal curing, the occurrence of shrinkage stress can be suppressed. Therefore, the crack resistance of the electronic device element of the present invention can be improved, and the leakage current can be reduced.

[0037] As the inorganic particles, particles made of a metal compound or a semi-metal compound are preferred, and from the viewpoint of reactivity with the polymer, inorganic oxide particles are particularly preferred.

[0038] Examples of the metal or metalloid include elements selected from the group consisting of silicon, magnesium, calcium, strontium, barium, lanthanum, cerium, tin, titanium, zirconium, hafnium, yttrium, niobium, tantalum, and aluminum. The inorganic particles are preferably particles of a compound containing one or more elements selected from the above group. Examples of the metal compound or metalloid compound include halides, oxides, nitrides, hydroxides, carbonates, sulfates, nitrates, or metasilicates of the above metals or metalloids.

[0039] Examples of inorganic oxide particles used in the present invention include known ones such as those described in International Publication No. 2019 / 065561. Among them, from the viewpoint of high dielectric constant of the cured film, inorganic particles selected from tin oxide-titanium oxide composite particles, silicon oxide-titanium oxide composite particles, titanium oxide particles, zirconium oxide particles, hafnium oxide particles, yttrium oxide particles, niobium oxide particles, tantalum oxide particles, tin oxide particles, tin oxide-zirconium oxide composite particles, silicon oxide-zirconium oxide composite particles, aluminum oxide particles, barium titanate particles, strontium titanate particles, barium titanate-strontium titanate composite particles, lead zirconate titanate particles, lanthanum lead zirconate titanate particles, strontium niobate bismuth particles, strontium niobate titanate bismuth particles, and strontium tantalate bismuth particles are more preferable, and from the viewpoint of availability, titanium oxide-containing particles such as tin oxide-titanium oxide composite particles, silicon oxide-titanium oxide composite particles, and titanium oxide particles are particularly preferable. By improving the dielectric constant of the insulating layer, the element characteristics of the element for electronic devices of the present invention are improved. For example, in the case of a FET, when the FET is driven (on) at a certain gate voltage value, the current flowing through the circuit increases.

[0040] There are no particular limitations on the shape of the inorganic particles, but in order to maintain a smooth surface of the insulating layer, a shape with a low aspect ratio is preferred, and a spherical shape is more preferred.

[0041] From the viewpoint of improving the pattern processability of the insulating layer and reducing leakage current by improving crack resistance, the number average particle size of the inorganic particles is preferably 1 nm or more, more preferably 5 nm or more, even more preferably 15 nm or more, and particularly preferably 20 nm or more.On the other hand, the number average particle size is preferably 100 nm or less, more preferably 70 nm or less, even more preferably 60 nm or less, and particularly preferably 50 nm or less.When the number average particle size is within the above range, the pattern processability of the cured film can be improved.

[0042] Here, the number average particle size of inorganic particles can be determined by the following measurement using a scanning electron microscope (SEM) or a transmission electron microscope (TEM). The cross section of the cured film is observed at a magnification of 50,000 to 200,000 times. If the inorganic particles are spherical, the diameter of the sphere is measured and used as the particle size of the particle. If the inorganic particles are not spherical, the longest diameter (hereinafter, "major axis diameter") and the longest diameter in a direction perpendicular to the major axis diameter (hereinafter, "minor axis diameter") are measured, and the biaxial average diameter obtained by averaging the major axis diameter and the minor axis diameter is used as the particle size of the particle. This particle size measurement is performed on 20 or more randomly selected particles, and the arithmetic average is used as the number average particle size.

[0043] The content of the inorganic particles in the gate insulating layer is preferably 5 vol% or more, more preferably 8 vol% or more, and particularly preferably 10 vol% or more, in terms of volume fraction, and is preferably 50 vol% or less, more preferably 30 vol% or less, even more preferably 20 vol% or less, and particularly preferably 18 vol% or less.

[0044] (Bonding of inorganic particles and polymers) The "bond" in the "polymer bonded to inorganic particles" is a bond selected from a covalent bond, an ionic bond, a coordinate bond, a metallic bond, a hydrogen bond, a bond based on pi-pi interactions, a bond based on ion-dipole interactions, a bond based on dipole-dipole interactions, a bond based on dipole-induced dipole interactions, a bond based on hydrophobic interactions, a bond based on charge transfer complex formation, a bond based on metal-ligand complex formation, a bond based on London dispersion forces, and a bond based on van der Waals forces.

[0045] The inorganic particles have functional groups, such as hydroxyl groups, on their surfaces that can react with polymers, and the inorganic particles react with the polymers at these functional groups, resulting in the inorganic particles being incorporated into the polymers. When the inorganic particles are bonded to the polymer, the aggregation of the inorganic particles in a solution state is suppressed compared to when the inorganic particles are mixed with the polymer. Furthermore, when the inorganic particles are bonded to the polymer, the alkali solubility of the inorganic particles is improved, so that when the insulating layer constituting the element of the present invention is formed by alkaline development, the deterioration of pattern processability due to the generation of residues can be suppressed. It is preferable that the "bond" is a covalent bond from the viewpoints of aggregation suppression and pattern processability.

[0046] The presence or absence of bonding between inorganic particles and polymers is 13 C-NMR, 29 It can be confirmed by combining analytical methods such as Si-NMR and IR. For example, 13 C-NMR or 29 Using Si-NMR, the spectrum of the inorganic particles, the spectrum of the polymer, and the spectrum of the polymer to which the inorganic particles are bonded are compared. The peaks derived from the C or Si atoms bonded to the inorganic particles in the polymer to which the inorganic particles are bonded are peaks with chemical shifts that do not exist in the spectrum of the polymer, so it is possible to confirm the presence or absence of bonding between the inorganic particles and the polymer.

[0047] Similarly, in IR, the peaks derived from C or Si atoms in a polymer to which inorganic particles are bonded have a different wavenumber from the spectrum of the polymer, making it possible to confirm whether or not the inorganic particles are bonded to the polymer.

[0048] (Polymer with inorganic particles attached) In the polymer (A) to which inorganic particles are bonded, the polymer is preferably soluble in a solvent. The polymer skeleton may be linear, cyclic, or branched. It is also preferable that a crosslinkable functional group, a polar functional group, or a functional group that controls various properties of the polymer is introduced into the side chain. By using a polymer with these controlled properties, for example, coatability, surface flatness, solvent resistance, transparency, and good wettability with other inks can be obtained in the process of producing an element for an electronic device. Furthermore, a good element having excellent durability and stability after the formation of the element for an electronic device can be obtained.

[0049] The polymer (A) used in the present invention is not particularly limited as long as it exhibits insulation to the extent that the FET functions normally, and for example, polysiloxane, polyamide, polyamideimide, polyimide, polybenzimidazole, polyvinyl alcohol, polyvinylphenol, polyacetal, polycarbonate, polyarylate, polyphenylene sulfide, polyethersulfone, polyetherketone, polyphthalamide, polyethernitrile, polymethyl methacrylate, polymethacrylamide, polyvinylidene fluoride, polytetrafluoroethylene, polystyrene, polyester, aromatic polyether, novolac resin, phenol resin, acrylic resin, olefin resin, alicyclic olefin resin, vinyl chloride resin, epoxy resin, melamine resin, urea resin, etc. can be used. In addition, it is also possible to use a copolymer or mixture of these polymers with other polymers. Among these, polysiloxane is preferably used from the viewpoint of improving the on-current of the FET and reducing the leakage current.

[0050] Specific examples of polysiloxanes include known polysiloxanes such as those described in WO 2019 / 065561.

[0051] (Surface conditioner) The technique of using a surface conditioner to set the coefficient of variation of the thickness of the gate insulating layer to 10% or less is particularly effective when the gate insulating layer is formed by a coating method using an insulating layer-forming coating liquid.

[0052] The surface conditioner used in the present invention may be, for example, polyether-modified polydimethylsiloxane. It is presumed that the polyether-modified polydimethylsiloxane reduces the surface tension of the coating liquid for forming the insulating layer and improves the stability of the coating liquid for forming the insulating layer.

[0053] Examples of polyether-modified polydimethylsiloxanes include BYK-333, BYK-331, BYK-307 (manufactured by BYK Japan Co., Ltd.), Borchi Gol LA2, and Borchi Gol LA50 (manufactured by Bochers Co., Ltd.).

[0054] (Polymer B) The polymer (B) used in the present invention includes a polymer that is not bonded to inorganic particles, has a structure different from that of the polymer (A), and has a functional group capable of hydrogen bonding with the hydroxyl group on the surface of the inorganic particles contained in the polymer (A).Specific examples of the polymer (B) include polysiloxane, polyamide, polyamideimide, polyimide, polybenzimidazole, polyvinyl alcohol, polyhydroxystyrene, polyacetal, polycarbonate, polyarylate, polyphenylene sulfide, polyethersulfone, polyetherketone, polyphthalamide, polyethernitrile, polymethyl methacrylate, polymethacrylamide, aromatic polyether, novolac resin, phenolic resin, acrylic resin, epoxy resin, melamine resin, urea resin, and various other polymers can be used.In addition, these polymers can be copolymerized or mixed with other polymers.

[0055] The polymer (B) is preferably a polymer having at least one functional group selected from the group consisting of a carboxyl group, a sulfo group, a phosphoric acid group, a mercapto group, a hydroxyl group, an epoxy group, and derivatives thereof, and is particularly preferably at least one selected from the group consisting of polysiloxanes having a structural unit represented by formula (1), resins having a phenolic hydroxyl group, polyesters having a carboxylic acid residue represented by formula (2), and polymaleic acid and derivatives thereof.

[0056] [ka]

[0057] The polysiloxane having a structural unit represented by general formula (1) can also be expressed as a polysiloxane having a structural unit represented by general formula (5).

[0058] [ka]

[0059] In the general formulas (1) and (5), R 5 R represents a hydrogen atom, an alkyl group, a cycloalkyl group, a heterocyclic group, an aryl group, a heteroaryl group, or an alkenyl group. 6 represents a hydrogen atom, an alkyl group, a cycloalkyl group, or a silyl group. n represents 0 or 1. A 2 represents an organic group containing at least one of a carboxyl group, a sulfo group, a thiol group, a phenolic hydroxyl group, an epoxy group, or a derivative thereof. However, when the derivative is a cyclic condensation structure of any two of the carboxyl group, the sulfo group, the thiol group, and the phenolic hydroxyl group, A 2 represents an organic group having at least one cyclic condensed structure.

[0060] [ka]

[0061] In the general formula (2), R 7 represents a hydrogen atom, an alkyl group, a cycloalkyl group, a heterocyclic group, an aryl group, a heteroaryl group, an alkenyl group, or an organic group represented by general formula (3). In general formula (2), the residues of the carboxyl groups at the 1-position and 1'-position are the sites provided for ester bonds in the polyester.

[0062] [ka]

[0063] In the general formula (3), R 8 represents a hydroxyl group, an alkoxy group, or a functional group represented by general formula (4).

[0064] [ka]

[0065] In the general formula (4), R 9 R represents a functional group represented by an alkylene group or an oxyalkylene group. However, the alkylene group or the oxyalkylene group may contain at least one ester bond, amide bond, or urethane bond. 10 represents a hydrogen atom or a methyl group.

[0066] The weight ratio of the polymer (A) in the total polymer components contained in the gate insulating layer is not particularly limited, but is preferably 94% by weight or less from the viewpoint of improving the unevenness of the insulating layer thickness on and around the electrode, while being 50% by weight or more from the viewpoint of maintaining the high dielectric property derived from the inorganic particles contained in the polymer (A).

[0067] By being within these ranges, it is possible to obtain a contrast between the exposed and unexposed parts during photolithography while maintaining a high dielectric constant of the insulating layer. "It is possible to obtain a contrast between the exposed and unexposed parts" means, for example, in the case of a positive photosensitive material, that there is no residual film in the exposed parts and the solubility of the unexposed parts in a developer is suppressed, resulting in an insulating layer of a desired thickness.

[0068] The content of the inorganic particles relative to 100 parts by weight of the total of polymer A and polymer B is not particularly limited, but from the viewpoint of increasing the dielectric constant of the insulating layer, it is preferably 15 parts by weight or more, and particularly preferably 30 parts by weight or more, while from the viewpoint of dispersibility of polymer A in a solution state, it is preferably 80 parts by weight or less.

[0069] The presence of polymer (A) and polymer (B) in the gate insulating layer was confirmed by FT-IR and 1 H-NMR, 13 C-NMR, 29 Analysis can be performed by combining analytical techniques such as Si-NMR, pyrolysis GC-MS, and LC-MS.

[0070] (Other Ingredients) The gate insulating layer may contain a viscosity modifier, a surfactant, a stabilizer, etc., as necessary. The insulating layer in the present invention may further contain a photosensitive organic component. Examples of the photosensitive organic component include a radical polymerizable compound having an ethylenically unsaturated double bond group, a photopolymerization initiator that generates radicals by bond cleavage and / or reaction upon irradiation with UV light, a chain transfer agent, a polymerization inhibitor, and a photoacid generator that generates acid by light.

[0071] From the viewpoint of reducing hysteresis in FET devices, it is preferable to use a photoacid generator that does not generate radicals that cause charge trapping in the gate insulating layer. By reducing charge trapping in the gate insulating layer, low hysteresis can be achieved.

[0072] The photoacid generator is not particularly limited, but examples thereof include onium salt compounds, halogen-containing compounds, diazoketone compounds, diazomethane compounds, sulfone compounds, sulfonic acid ester compounds, and sulfonimide compounds. Specific examples of diazoketone compounds include 1,3-diketo-2-diazo compounds, diazobenzoquinone compounds, and diazonaphthoquinone compounds. Among them, diazonaphthoquinone compounds are preferred from the viewpoint of the pattern processing accuracy and crack resistance of the insulating layer. Preferred diazoketone compounds include esters of 1,2-naphthoquinone diazide-4-sulfonic acid and 2,2,3,4,4'-pentahydroxybenzophenone, and esters of 1,2-naphthoquinone diazide-4-sulfonic acid and 1,1,1-tris(4-hydroxyphenyl)ethane.

[0073] (Semiconductor layer) The semiconductor layer in the present invention is not particularly limited as long as it has semiconducting properties, and inorganic semiconductors such as silicon semiconductors and oxide semiconductors, organic semiconductors such as pentacene and polythiophene derivatives, and carbon semiconductors such as carbon nanotubes (CNTs) and graphene can be used. Among these, CNTs are superior in that they have high carrier mobility and can be applied to a simple coating process at low cost.

[0074] Furthermore, a CNT composite having a conjugated polymer attached to at least a portion of the CNT surface is particularly preferred because it has excellent dispersion stability in a solution and can obtain low hysteresis. The state in which a conjugated polymer is attached to at least a portion of the CNT surface means that a part or the entire CNT surface is covered with the conjugated polymer.

[0075] Preferred examples of CNTs and organic semiconductors include known CNTs and organic semiconductors such as those described in International Publication No. 2019 / 065561.

[0076] The FET according to the embodiment of the present invention may also have an orientation layer between the gate insulating layer and the semiconductor layer. As the material for the orientation layer, known materials such as silane compounds, titanium compounds, organic acids, and heteroorganic acids can be used, and organic silane compounds are particularly preferred.

[0077] The FET according to the embodiment of the present invention may have a second insulating layer on the opposite side of the gate insulating layer with respect to the semiconductor layer. Here, the opposite side of the gate insulating layer with respect to the semiconductor layer refers to the lower side of the semiconductor layer, for example, when the gate insulating layer is on the upper side of the semiconductor layer. This makes it possible to reduce the threshold voltage and hysteresis, and to obtain a high-performance FET. Examples of the second insulating layer and its manufacturing method that are preferably used include known ones such as those described in International Publication No. 2019 / 065561.

[0078] (substrate) The material used for the substrate may be any material as long as at least the surface on which the electrodes (gate electrode or source / drain electrodes) are disposed is insulating. For example, inorganic materials such as silicon wafer, glass, sapphire, and sintered alumina, and organic materials such as polyimide, polyvinyl alcohol, polyvinyl chloride, polyethylene terephthalate, polyethylene naphthalate, polyvinylidene fluoride, polysiloxane, polyvinylphenol (PVP), polyester, polycarbonate, polysulfone, polyethersulfone, polyethylene, polyphenylene sulfide, and polyparaxylene are preferably used.

[0079] Alternatively, the substrate may be a laminate of multiple materials, such as a PVP film formed on a silicon wafer, or an acrylic resin, polyester resin, or polysiloxane formed on polyethylene terephthalate as an adhesion improver for the lower electrode.

[0080] Among these, from the viewpoints of element flexibility and manufacturing costs, polyethylene terephthalate (PET) is preferred as the substrate material, and from the viewpoint of the smoothness of the substrate surface in particular, a film in which a coating layer containing silica nanoparticles is formed on the surface of a PET film to which no filler such as silica particles has been added is preferred.

[0081] Regular PET film contains silica particles, which gives the substrate a low surface smoothness, and when devices are fabricated using this film, leakage is likely to occur in the gate insulating layer at the convex parts. On the other hand, a film in which a coating layer containing silica nanoparticles is formed on the surface of a PET film to which no fillers such as silica particles have been added has a high surface smoothness. Therefore, devices fabricated using this film are less likely to experience leakage in the gate insulating layer.

[0082] (electrode) Examples of materials used for the gate electrode, source electrode, and drain electrode include conductive metal oxides such as tin oxide, indium oxide, and indium tin oxide (ITO); metals such as platinum, gold, silver, copper, iron, tin, zinc, aluminum, indium, chromium, lithium, sodium, potassium, cesium, calcium, magnesium, palladium, molybdenum, amorphous silicon, and polysilicon, and alloys thereof; inorganic conductive substances such as copper iodide and copper sulfide; polythiophene, polypyrrole, and polyaniline; complexes of polyethylenedioxythiophene and polystyrenesulfonic acid; conductive polymers whose conductivity has been improved by doping with iodine or the like; and conductors such as carbon materials. These materials may be used alone, or a plurality of materials may be stacked or mixed for use.

[0083] It is preferable to use metal particles as the conductor. The use of metal particles has the effect of improving the bending resistance of the element. This is thought to be because unevenness is formed on the surface of the conductive film, and the gate insulating layer penetrates into the unevenness, resulting in an anchor effect that improves the adhesion between the conductive film and the gate insulating layer.

[0084] Specifically, the metal particles are preferably metal particles containing at least one of gold, silver, copper, platinum, lead, tin, nickel, aluminum, tungsten, molybdenum, ruthenium oxide, chromium, titanium, carbon, or indium. These metal particles can be used alone, as an alloy, or as mixed particles. Among these, gold, silver, copper, or platinum particles are preferred from the viewpoint of electrical conductivity. Among these, silver particles are more preferred from the viewpoint of cost and stability. Furthermore, it is even more preferred to contain carbon black from the viewpoint of reducing the electrical resistivity of the conductive film.

[0085] At least one of the gate electrode and the source electrode / drain electrode preferably contains an organic component. By containing an organic component, the adhesion between the electrode and the gate insulating layer is improved. In addition, by containing a photosensitive organic component in the organic component, the electrode can be patterned by photolithography without using a resist, and productivity can be further improved. From the viewpoint of further enhancing these effects, it is preferable that both the gate electrode and the source electrode / drain electrode contain an organic component.

[0086] The organic component is not particularly limited, but may be a monomer, an oligomer, or a polymer. The oligomer or polymer is not particularly limited, and may be an acrylic resin, an epoxy resin, a novolac resin, a phenolic resin, a polyimide precursor, or a polyimide, but from the viewpoint of crack resistance when bent, an acrylic resin is preferred. This is presumably because the glass transition temperature of the acrylic resin is 100°C or less, and it softens when the conductive film is thermally cured, strengthening the bond between the conductive particles.

[0087] The photosensitive organic component includes a monomer, oligomer, polymer and / or an addition reaction product thereof having a polymerizable unsaturated group in the molecule.

[0088] As a monomer having a polymerizable unsaturated group in the molecule, a compound having an active carbon-carbon unsaturated double bond can be used. As a functional group, a monofunctional compound having a group selected from a vinyl group, an allyl group, an acrylate group, a methacrylate group, and an acrylamide group and a polyfunctional compound can be used. One or more of these can be used.

[0089] The above monomer is preferably contained in the range of 1 mass % to 15 mass % and more preferably in the range of 2 mass % to 10 mass % based on the total mass of the electrode material. An oligomer or polymer having a polymerizable unsaturated group in the molecule can be obtained by adding the polymerizable unsaturated group to a side chain or a molecular end of an oligomer or polymer.

[0090] The polymerizable unsaturated group is preferably an ethylenically unsaturated group, such as a vinyl group, an allyl group, an acryl group, or a methacryl group.

[0091] Methods for adding such side chains to an oligomer or polymer include known methods, such as those described in WO 2019 / 065561.

[0092] The electrode material preferably contains a photopolymerization initiator for photocuring. The photopolymerization initiator is selected depending on the light source used for photocuring, and a photoradical polymerization initiator, a photocationic polymerization initiator, or the like can be used.

[0093] The photopolymerization initiator is preferably contained in the range of 0.05% by mass to 10% by mass, more preferably 0.1% by mass to 10% by mass, based on the total mass of the electrode material. If the amount of the photopolymerization initiator is too small, photocuring may be insufficient, and if the amount of the photopolymerization initiator is too large, compatibility may be poor.

[0094] By using a sensitizer together with a photopolymerization initiator, the sensitivity can be improved and the wavelength range effective for the reaction can be expanded. When the electrode material contains a sensitizer, the content is preferably 0.05% by mass to 10% by mass, more preferably 0.1% by mass to 10% by mass, based on the photosensitive organic component. If the amount of the sensitizer is too small, the effect of improving photocuring cannot be exhibited, and if the amount of the sensitizer is too large, compatibility may be poor.

[0095] The amount of the conductor in the conductive film is preferably within a range of 70 to 95 wt % of the conductive film, more preferably 80 wt % or more as the lower limit and 90 wt % or less as the upper limit, respectively. By being within this range, the resistivity value and the probability of disconnection of the conductive film can be reduced.

[0096] Examples of methods for forming the electrodes include methods using known techniques such as resistance heating deposition, electron beam, sputtering, plating, CVD, ion plating coating, inkjet, and printing, and methods in which a paste containing the organic component and a conductor is applied onto an insulating substrate by known techniques such as spin coating, blade coating, slit die coating, screen printing, bar coater, casting, print transfer, and immersion and pulling, and then dried using an oven, a hot plate, infrared rays, etc. There are no particular limitations as long as electrical continuity can be obtained.

[0097] When the electrodes are formed by applying a paste, the paste may contain an organic solvent for forming the paste. By using an organic solvent, the viscosity of the paste can be adjusted and the surface smoothness of the applied film can be improved.

[0098] The width, thickness and spacing of the electrodes are arbitrary. It is preferable that the electrode width is 5 μm to 1 mm, the thickness is 0.01 μm to 100 μm, and the spacing between the electrodes is 1 μm to 500 μm, but is not limited to these.

[0099] As a method for forming the electrodes in a pattern, the electrode thin film prepared by the above method may be patterned into a desired shape by a known photolithography method, or the electrode, wiring, and connection material may be patterned through a mask of a desired shape during deposition or sputtering. Alternatively, the pattern may be directly formed by inkjet or printing.

[0100] The electrode patterns may be formed by processing each separately, or at least two of them may be processed together to form the electrode patterns. From the viewpoint of reducing the processing steps and connecting the patterns, it is preferable to process the electrode patterns together.

[0101] (FET manufacturing method) A method for manufacturing the FET shown in Fig. 1 will be described below, although the manufacturing method is not limited to the following.

[0102] (Step 1) A step of forming a conductive pattern that will become the lower electrode on a substrate First, a conductive pattern that will become the gate electrode 11 is formed on the substrate 100. Examples of the formation method include known methods such as metal deposition, spin coating, blade coating, slit die coating, screen printing, bar coating, mold method, print transfer method, immersion and pulling method, and inkjet method. In addition, when forming the conductive pattern, the pattern may be directly formed using a mask or the like, or the gate electrode may be patterned by applying a resist onto the formed gate electrode, exposing and developing the resist film into a desired pattern, and then etching it. Furthermore, when a conductive paste having a photosensitive organic component is used, the gate electrode can be patterned by photolithography without using a resist.

[0103] (Step 2) Step of forming a gate insulating layer Next, a gate insulating layer 12 is formed on the substrate on which the conductive pattern is formed. The gate insulating layer 12 can be formed by applying at least a solution containing a polymer to which inorganic particles are bonded onto the substrate, drying the substrate to obtain a coating film, and then heating and curing the coating film. In addition, in forming a circuit in which FETs are combined, the coating film can be patterned to obtain electrical continuity from the conductive pattern present under the insulating layer.

[0104] Examples of a method for applying a solution containing a polymer to which inorganic particles are bonded include known application methods such as spin coating, blade coating, slit die coating, screen printing, bar coating, casting, print transfer, immersion and pulling, and inkjet printing.

[0105] (Step 3) forming a conductive pattern that will become an upper electrode on the gate insulating layer Next, a conductive pattern that becomes the source electrode 13 and the drain electrode 15 is formed on the gate insulating layer. As with the gate electrode 11, the method of forming the source electrode 13 and the drain electrode 15 includes known methods such as metal deposition, spin coating, blade coating, slit die coating, screen printing, bar coating, casting, printing transfer, immersion and pulling, and inkjet. In addition, when forming the conductive pattern, a pattern may be formed directly using a mask or the like, or the source electrode and the drain electrode may be patterned by applying a resist onto the formed electrode, exposing and developing the resist film into a desired pattern, and then etching it. Furthermore, when a conductive paste having a photosensitive organic component is used, it is also possible to pattern the gate electrode by photolithography using only the conductive paste without using a resist.

[0106] After (step 3), a semiconductor layer 14 is formed on the gate insulating layer on which the source electrode and drain electrode are formed, thereby obtaining a FET. Although a dry method such as resistance heating deposition, electron beam, sputtering, and CVD can be used as a method for forming the semiconductor layer 14, it is preferable to use a coating method from the viewpoint of manufacturing cost and adaptability to a large area. Examples of the coating method include known coating methods such as spin coating, blade coating, slit die coating, screen printing, bar coating, casting, printing transfer, immersion and pulling, and inkjet. The coating method can be selected according to the coating film characteristics to be obtained, such as coating film thickness control and orientation control. Using these methods, the semiconductor layer is formed so that the semiconductor layer and the conductive pattern that becomes the source electrode 13 and the drain electrode 15 are in contact with each other. The source electrode and the drain electrode may be formed after forming the semiconductor layer.

[0107] In particular, when forming a semiconductor layer containing CNTs, it is preferable to apply a solution containing CNTs onto the gate insulating layer. In this case, there is no particular limitation on the application method, but the use of an inkjet method is superior in that it reduces the amount of solution used and increases productivity. The solution containing CNTs can be prepared by stirring CNTs in a solvent through a stirring process using a known dispersion device such as an ultrasonic homogenizer.

[0108] A step of forming an orientation layer between the gate insulating layer 12 and the semiconductor layer 14 by a method similar to the method of forming a coating film of the above-mentioned gate insulating layer material may be added. Also, a step of forming a second insulating layer on the opposite side of the semiconductor layer 14 to the gate insulating layer 12 by a method similar to that of the semiconductor layer 14 may be added.

[0109] [Embodiment 2: Capacitor] 7 is a schematic cross-sectional view showing a capacitor as an element according to embodiment 2 of the present invention. Capacitor 7 has insulating base material 200, lower electrode 21, dielectric film 22 covering part of lower electrode 21, and upper electrode 23 covering part of dielectric film 22.

[0110] Regarding the materials and manufacturing methods of the insulating substrate, the dielectric film, the upper electrode and the lower electrode, the same points as those for the insulating substrate, the gate insulating layer and the gate electrode in the above-mentioned FET are applied.

[0111] The capacitor according to the embodiment of the present invention contains the polymer (A) bonded to the inorganic particles in the insulating layer, but in such a case, the thickness of the insulating layer formed around the lower electrode and on the lower electrode generally becomes uneven. In particular, since the area of ​​the lower electrode in a capacitor is large, if the thickness of the insulating layer on the electrode becomes uneven, leakage occurs at the thin part of the film, and the yield of the capacitor formation is significantly reduced. Furthermore, the unevenness in the film thickness causes a large variation in the capacitor characteristics such as the capacitance value in the substrate.

[0112] In the capacitor according to the embodiment of the present invention, the coefficient of variation of the thickness of the insulating layer is 10% or less, so that the leakage current is reduced and the yield of the element formation is improved. The coefficient of variation of the thickness of the insulating layer is more preferably 8% or less, and further preferably 5% or less.

[0113] The variation coefficient of the insulating layer thickness can be set to 10% or less by the same method as that used for the gate insulating layer of the FET according to the first embodiment described above.

[0114] The material and composition constituting this insulating layer and the manufacturing method thereof are the same as those for the gate insulating layer of the FET according to the first embodiment described above.

[0115] <Circuit> A circuit can be configured by combining the above FET and capacitor. There are no particular limitations on the circuit, and examples include, but are not limited to, a rectifier circuit, a modulation circuit, a memory circuit, a power supply circuit, a reference voltage / current circuit, a data converter circuit, and an operational amplifier. In addition, these may be used alone or in combination of two or more types.

[0116] FIG. 8 is an example of a rectifier circuit including a FET 301 and a capacitor element 302. In the structure of FIG. 8, a capacitor 302 consisting of a lower electrode 32, an upper electrode 37, and an insulating layer (dielectric film) 33b, a FET 301 consisting of a gate electrode 31, an insulating layer 33a (gate insulating layer), a source electrode 35, a drain electrode 36, and a semiconductor layer 34, a wiring 38, and a via 39 are provided on an insulating substrate 300. In FIG. 8, the dielectric film of the capacitor 302 and the gate insulating layer of the FET 301 are made common and made of the same material. In FIG. 8, a structure in which the drain electrode 36 and the upper electrode 37 are electrically connected via the wiring 38 are illustrated, but the drain electrode 36 and the lower electrode 32 may be electrically connected via the wiring 38 and the via 39. In addition, although a FET having a bottom gate structure is shown in FIG. 8, a FET having a top gate structure may also be used. Furthermore, while FIG. 8 shows a circuit in which the dielectric film of capacitor 302 and the gate insulating layer of FET 301 are made of a common material, as shown in FIGS. 9 and 10, insulating layers 33A and 33B made of different materials may also be used.

[0117] The insulating substrate, dielectric film, gate electrode, upper electrode, and lower electrode can be made of the same materials and manufactured by the same methods as those used in the first and second embodiments. The vias and wiring can be made of the same materials and manufactured by the same methods as those used in the lower electrode and upper electrode.

[0118] (Applicability of the element) The element of the present invention is applicable to ICs for various electronic devices, wireless communication devices such as RFID tags, wireless power supply devices, TFT arrays for displays, sensors, and tamper detection systems.

[0119] <Wireless communication device> The element of the present invention and a circuit having the same can be applied to a wireless communication device. This wireless communication device is a device that performs electrical communication by receiving a carrier wave transmitted from an antenna mounted on a reader / writer, such as an RFID (Radio Frequency IDentification) tag, which is a non-contact tag such as a product tag, an anti-shoplifting tag, various tickets, and a smart card. In concrete terms, for example, a wireless signal transmitted from an antenna mounted on a reader / writer is received by an antenna of the RFID tag, which is converted to a direct current by a rectifier circuit, and the RFID tag is energized. Next, the energized RFID tag receives a command from the wireless signal and performs an operation according to the command. After that, a response to the command is transmitted as a wireless signal from the antenna of the RFID tag to the antenna of the reader / writer. The operation according to the command is executed by a demodulation circuit, a control circuit, a modulation circuit, and the like.

[0120] A more specific configuration of a wireless communication device having at least the element of the present invention and an antenna, for example, as shown in FIG. 11, includes a power supply generating unit 45 that rectifies a modulated wave signal received from an external source by an antenna 40 and supplies power to each unit, a demodulation circuit 41 that demodulates the modulated wave signal and sends it to a control circuit, a modulation circuit 43 that modulates data sent from the control circuit and sends it to the antenna, and a control circuit 42 that writes the data demodulated by the demodulation circuit 41 to a memory circuit 44 and reads data from the memory circuit 44 and transmits it to the modulation circuit 43, and the respective circuit units are electrically connected to each other. At least one of the power supply generating unit, demodulation circuit, control circuit, modulation circuit, and memory circuit includes the above-mentioned element, and may further include a capacitor, a resistive element, a diode, etc. The memory circuit may further include a read-only memory unit in which information is written during manufacturing, or a non-volatile rewritable memory unit such as an EEPROM (Electrically Erasable Programmable Read-Only Memory) or a FeRAM (Ferroelectric Random Access Memory). The power supply generating unit is composed of a capacitor and a diode.

[0121] The antenna, capacitor, resistor, diode, and non-volatile rewritable memory unit may be any commonly used material and may have any shape. The material electrically connecting each of them may be any commonly used conductive material. The connection method may be any method that can provide electrical continuity, and the width and thickness of the connection part may be any method.

[0122] <Product tag> A product tag using the wireless communication device will now be described. This product tag has, for example, a base and the wireless communication device covered by the base.

[0123] The base is formed of a non-metallic material such as paper formed into a flat plate shape. For example, the base has a structure in which two flat sheets of paper are pasted together, and the wireless communication device is disposed between the two sheets of paper. Individual identification information for identifying individual products, for example, is stored in advance in a memory circuit of the wireless memory device.

[0124] Wireless communication is performed between this product tag and a reader / writer. A reader / writer is a device that wirelessly reads and writes data to product tags, and exchanges data with product tags during the product distribution process and at the time of payment. Publicly known reader / writers can be used, including, for example, portable types and fixed types installed at cash registers.

[0125] Specifically, the product tag has an identification information return function that wirelessly returns the stored individual identification information in response to a command from a specific reader / writer that requests the transmission of individual identification information. This makes it possible to simultaneously identify multiple products without contact at a product checkout register, for example, and makes payment processing easier and faster than identification using barcodes.

[0126] For example, when paying for a product, the reader / writer reads the product information from the product tag and sends it to a POS (Point of Sale System) terminal, which then registers the sale of the product identified by that product information. EXAMPLES

[0127] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0128] (1) Insulation layer thickness measurement The thickness of the insulating layer formed on the lower electrode and not covered by the upper electrode was measured using an optical interference spectroscopic film thickness measuring instrument (OPTM-A2, manufactured by Otsuka Electronics Co., Ltd.) The film thickness was measured at 15 points for each part, and the arithmetic mean and standard deviation were obtained. The standard deviation was divided by the arithmetic mean to calculate the coefficient of variation, and the film thickness was evaluated according to the following criteria. A (very good): Coefficient of variation is 5% or less B (Good): Coefficient of variation is greater than 5% and less than 8% C (Acceptable): Coefficient of variation is greater than 8% and less than 10% D (Fail): The coefficient of variation is greater than 10%.

[0129] (2) Measurement of the dielectric constant of the insulating layer The insulating solution shown in Table 1 was spin-coated (800 rpm x 10 seconds) onto an aluminum substrate, and then heat-treated at 110°C for 2 minutes, followed by heat-treatment at 150°C for 30 minutes in a drying oven to form a cured film with a thickness of 400 nm. Next, a circular aluminum electrode with a diameter of 5 mm was formed by vapor deposition on the cured film. The electrostatic capacitance of this film was measured at 25°C and 1 MHz using a precision impedance analyzer (Agilent, Model 4294A). Based on the above conditions and measured values, the relative dielectric constant ε of the cured film was calculated according to equation (a). r asked for.

[0130] ε r =C D / (S ε0) (a) where C(F) is the capacitance of the insulating layer, D(m) is the thickness of the insulating layer, and S(m 2 ) is the area of ​​the electrodes sandwiching the insulating layer, and ε0 is the dielectric constant of vacuum (8.85×10 -12 F / m).

[0131] (3) Making the capacitor The capacitor shown in FIG. 12 was fabricated. Copper was vacuum-deposited to a thickness of 100 nm on a 50 μm-thick PET film (trade name "U48", manufactured by Toray Industries, Inc.) 500 by resistance heating, and a photoresist (trade name "LC140-10cP", manufactured by Rohm and Haas Co., Ltd.) was spin-coated (1000 rpm x 20 seconds) on top of the copper, and dried by heating at 100°C for 10 minutes. The fabricated photoresist film was pattern-exposed through a mask using a parallel light mask aligner (PLA-501F, manufactured by Canon Inc.), and then shower-developed for 60 seconds with ELM-D (trade name, manufactured by Mitsubishi Gas Chemical Co., Ltd.), a 2.38 mass% TMAH aqueous solution, using an automatic developing device (AD-2000, manufactured by Takizawa Sangyo Co., Ltd.), and then washed with water for 30 seconds. After that, it was etched for 2 minutes with Cu-03 (trade name, manufactured by Kanto Chemical Co., Ltd.), and then washed with water for 30 seconds. The resist was peeled off by immersing the film in JELK-101 (trade name, manufactured by Kanto Chemical Co., Ltd.) for 2 minutes, and then washed with water for 30 seconds, followed by drying by heating at 120°C for 20 minutes to form the lower electrode 51. Next, the insulating material solution described in each example and comparative example was spin-coated (800 rpm x 10 seconds) on the PET film on which the lower electrode 51 was formed, and then heat-treated at 110°C for 2 minutes, followed by heating at 150°C for 30 minutes using a drying oven to form a dielectric film 52 with a thickness of 400 nm. Next, the conductive paste of Preparation Example 2 was applied with a bar coater, and pre-baked at 100°C for 10 minutes in a drying oven. Thereafter, the film was exposed to light using an exposure device "PEM-8M", and then immersed and developed in a 0.5% Na2CO3 solution for 30 seconds, rinsed with ultrapure water, and cured in a drying oven at 140°C for 30 minutes to form the upper electrode 53.

[0132] (4) Fabrication of FET The FET shown in FIG. 13 was fabricated. Copper was vacuum-deposited to a thickness of 100 nm on a PET film (trade name "U48", manufactured by Toray Industries, Inc.) 600 with a thickness of 50 μm by resistance heating, and a photoresist (trade name "LC140-10cP", manufactured by Rohm and Haas Co., Ltd.) was spin-coated (1000 rpm x 20 seconds) on top of the copper, and dried by heating at 100°C for 10 minutes. The fabricated photoresist film was pattern-exposed through a mask using a parallel light mask aligner (PLA-501F, manufactured by Canon Inc.), and then shower-developed for 60 seconds with ELM-D (trade name, manufactured by Mitsubishi Gas Chemical Co., Ltd.), a 2.38 mass% TMAH aqueous solution, using an automatic developing device (AD-2000, manufactured by Takizawa Sangyo Co., Ltd.), and then washed with water for 30 seconds. The film was then etched for 2 minutes with Cu-03 (trade name, manufactured by Kanto Chemical Co., Ltd.), and then washed with water for 30 seconds. The resist was peeled off by immersing the film in JELK-101 (trade name, manufactured by Kanto Chemical Co., Ltd.) for 2 minutes, and then washed with water for 30 seconds, followed by drying by heating at 120°C for 20 minutes to form a gate electrode 61. Next, the insulating material solution described in each example and comparative example was spin-coated (800 rpm x 10 seconds) on the PET film on which the gate electrode 61 was formed, and then heat-treated at 110°C for 2 minutes, followed by heating at 150°C for 30 minutes using a drying oven to form a gate insulating layer 62 with a film thickness of 400 nm. Next, the semiconductor solution of Preparation Example 1 was inkjet-coated on the gate insulating layer 62, and then heat-treated at 150°C for 30 minutes in the atmosphere to form a semiconductor layer 63. Next, the conductive paste of Preparation Example 2 was applied with a bar coater, and pre-baked in a drying oven at 100°C for 10 minutes. After that, the film was exposed to light using a “PEM-8M” exposure device, then developed by immersion in a 0.5% Na2CO3 solution for 30 seconds, rinsed with ultrapure water, and cured in a drying oven at 140°C for 30 minutes to form a source electrode 64 and a drain electrode 65.

[0133] (5) Making a rectifier circuit A rectifier circuit consisting of a FET 701 and a capacitor 702 shown in FIG. 14 was fabricated. Copper was vacuum-deposited to a thickness of 100 nm on a PET film (trade name "U48", manufactured by Toray Industries, Inc.) 700 with a thickness of 50 μm by a resistance heating method, and a photoresist (trade name "LC140-10cP", manufactured by Rohm and Haas Co., Ltd.) was spin-coated (1000 rpm x 20 seconds) thereon and dried by heating at 100° C. for 10 minutes. The fabricated photoresist film was pattern-exposed through a mask using a parallel light mask aligner (PLA-501F, manufactured by Canon Inc.), and then shower-developed for 60 seconds with ELM-D (trade name, manufactured by Mitsubishi Gas Chemical Co., Ltd.), which is a 2.38 mass % TMAH aqueous solution, using an automatic developing device (AD-2000, manufactured by Takizawa Sangyo Co., Ltd.), and then washed with water for 30 seconds. Then, the film was etched with Cu-03 (trade name, manufactured by Kanto Chemical Co., Ltd.) for 2 minutes, and then washed with water for 30 seconds. The resist was peeled off by immersing the film in JELK-101 (trade name, manufactured by Kanto Chemical Co., Ltd.) for 2 minutes, washed with water for 30 seconds, and then heated and dried at 120°C for 20 minutes to form the gate electrode 71 of the FET element and the lower electrode 72 of the capacitor element. Next, the insulating material solution described in each example and comparative example was spin-coated (800 rpm x 10 seconds) on the PET film on which the gate electrode 71 and the lower electrode 72 were formed, and then heat-treated at 110°C for 2 minutes. After that, the film was exposed to light using an exposure device "PEM-8M", and then immersed and developed in a TMAH solution for 30 seconds, and rinsed with ultrapure water to form a hole pattern in the area where the via 79 was to be formed. Then, the film was heated at 150°C for 30 minutes using a drying oven to form an insulating layer 73 having a thickness of 400 nm, which also serves as the gate insulating layer of the FET element and the dielectric layer of the capacitor element. Next, the semiconductor solution of Preparation Example 1 was inkjet coated on the insulating layer 73, and heat-treated at 150°C for 30 minutes in the atmosphere to form a semiconductor layer 74. Next, the conductive paste of Preparation Example 2 was coated with a bar coater, and pre-baked in a drying oven at 100°C for 10 minutes. After that, it was exposed to light using an exposure device "PEM-8M", immersion developed in a 0.5% Na2CO3 solution for 30 seconds, rinsed with ultrapure water, and cured in a drying oven at 140°C for 30 minutes to form a source electrode 75 and a drain electrode 76 of the FET element, an upper electrode 77 of the capacitor element, wiring 78, and a via 79.

[0134] (6) Evaluation of short circuit rate of capacitor The interelectrode current (Ie) was measured for 100 capacitors fabricated with different applied voltages (Ve). The measurements were performed using a Semiconductor Characterization System 4200-SCS (Keithley Instruments, Inc.) in the atmosphere (temperature 20°C, humidity 35%). The electrode area was 1 mm 2 For the element, Ie at Ve=10V is 10 -8 Elements rated A or higher were considered short-circuited elements and were evaluated according to the following criteria. A (very good): Fewer than 1 out of 100 elements were shorted. B (Good): The number of elements with short circuits was between 2 and 5 out of 100. C (Acceptable): The number of elements with short circuits is between 5 and 20 out of 100. D (Fail): 20 or more short-circuited elements out of 100.

[0135] (7) Evaluation of FET leakage rate The source-drain current (Id)-source-drain voltage (Vsd) characteristics were measured for 100 fabricated FETs when the gate voltage (Vg) was changed. The measurements were performed using a Semiconductor Characterization System Model 4200-SCS (Keithley Instruments, Inc.) in the atmosphere (temperature 20°C, humidity 35%). The on-current was calculated from the drain current value at Vg = -20V. Furthermore, when the gate-source current (Vgs) at Vg = 20V was 10 -8 Elements rated A or higher were considered to be leak elements and were evaluated according to the following criteria. A (very good): The number of elements that leaked was 1 or less out of 100. B (Good): The number of elements showing leakage is between 2 and 5 out of 100. C (Acceptable): The number of elements showing leakage is between 5 and 20 out of 100. D (Fail): Leaks were observed in 20 or more of 100 elements.

[0136] (8) Yield evaluation of rectifier circuits In the 100 rectifier circuits thus produced, when an AC current was input to the source electrode 75, the DC current output to the drain electrode 76 was measured, and the yield of the rectifier circuits was evaluated according to the following criteria. A (very good): The number of non-operating circuits is 1 or less in 100. B (Good): The number of non-operating circuits is between 2 and 5 out of 100. C (Acceptable): The number of non-operating circuits is between 5 and 20 out of 100. D (Not acceptable): The number of non-operating circuits is 20 or more out of 100.

[0137] Synthesis Example 1: Synthesis of polysiloxane with inorganic particles (PS-01) Into a three-neck flask, 10.90 g (0.08 mol) of methyltrimethoxysilane (MeSi), 5.25 g (0.02 mol) of 3-trimethoxysilylpropylsuccinic anhydride (SucSi), 24.84 g (0.10 mol) of 1-naphthyltrimethoxysilane (NapSi), and 20.6 mass% titanium oxide-silicon oxide composite particle methanol dispersion liquid "Optlake (registered trademark)" TR-550 (JGC Catalyst Co., Ltd.) were added. 133.68g (100 parts by mass of particle content per 100 parts by mass of organosilane (27.54g) when fully condensed) manufactured by Kasei Co., Ltd.) and 102.28g of diacetone alcohol (DAA, boiling point 168°C) were charged, and an aqueous phosphoric acid solution in which 0.205g of phosphoric acid (0.50% by mass relative to the charged monomer) was dissolved in 11.16g of water was added over 10 minutes while stirring at room temperature. After that, the flask was immersed in a 40°C oil bath and stirred for 60 minutes, and the oil bath was heated to 115°C over 30 minutes. One hour after the start of the temperature rise, the internal temperature of the solution reached 100°C, and the solution was heated and stirred for 2 hours (internal temperature was 100-110°C). The resin solution obtained by heating and stirring was cooled in an ice bath, and then anion exchange resin and cation exchange resin were added at 2% by weight each relative to the resin solution and stirred for 12 hours. After stirring, the anion exchange resin and cation exchange resin were removed by filtration to obtain a solution of polysiloxane (PS-01) with inorganic particles bonded thereto. Nitrogen was flowed at 0.05 liters per minute during the temperature increase and heating and stirring. A total of 121.19 g of by-products, methanol and water, were distilled out during the reaction. The solids concentration of the resulting solution of polysiloxane with inorganic particles bonded thereto, PS-01, was 33 mass%.

[0138] Synthesis Example 2: Synthesis of polysiloxane (PS-02) 10.90g (0.08mol) of methyltrimethoxysilane (MeSi), 5.25g (0.02mol) of 3-trimethoxysilylpropylsuccinic anhydride (SucSi), and 24.84g (0.10mol) of 1-naphthyltrimethoxysilane (NapSi) were dissolved in 64.26g of propylene glycol monobutyl ether (boiling point 170°C), and 11.16g of water and 0.205g of phosphoric acid were added thereto while stirring. The resulting solution was heated at a bath temperature of 105°C for 2 hours, and the internal temperature was raised to 70°C, and the components mainly consisting of by-product methanol were distilled out. Next, the solution was heated at a bath temperature of 130°C for 2.0 hours, and the internal temperature was raised to 110°C, and the components mainly consisting of water and propylene glycol monobutyl ether were distilled out. The resin solution obtained by heating and stirring was cooled in an ice bath, and then 2% by weight of anion exchange resin and cation exchange resin were added to the resin solution and stirred for 12 hours. After stirring, the anion exchange resin and cation exchange resin were removed by filtration to obtain a polysiloxane solution with a solid concentration of 36.0 wt%.

[0139] Synthesis Example 3: Synthesis of polysiloxane (PS-03) 61.29g (0.09 mol) of methyltrimethoxysilane, 12.31g (0.01 mol) of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 99.15g (0.10 mol) of phenyltrimethoxysilane were dissolved in 48.84g of propylene glycol monobutyl ether (boiling point 170°C), and 10.98g of water and 0.173g of phosphoric acid were added thereto while stirring. The resulting solution was heated at a bath temperature of 105°C for 2 hours, and the internal temperature was raised to 90°C, and a component mainly consisting of by-product methanol was distilled out. The solution was then heated at a bath temperature of 130°C for 2.0 hours, and the internal temperature was raised to 118°C, and a component mainly consisting of water and propylene glycol monobutyl ether was distilled out. The resin solution obtained by heating and stirring was cooled in an ice bath, and then anion exchange resin and cation exchange resin were added at 2% by weight each relative to the resin solution, and stirred for 12 hours. After stirring, the anion exchange resin and cation exchange resin were removed by filtration to obtain a polysiloxane solution with a solids concentration of 36.0 wt %.

[0140] Synthesis Example 4: Synthesis of naphthoquinone diazide compound (QD-01) Under a dry nitrogen stream, 15.32 g (0.05 mol) of Ph-cc-AP-MF (trade name, manufactured by Honshu Chemical Industry Co., Ltd.) and 37.62 g (0.14 mol) of 5-naphthoquinone diazide sulfonyl chloride were dissolved in 450 g of 1,4-dioxane and brought to room temperature. 15.58 g (0.154 mol) of triethylamine mixed with 50 g of 1,4-dioxane was added dropwise so that the temperature in the system did not exceed 35°C. After the addition, the mixture was stirred at 30°C for 2 hours. The triethylamine salt was filtered, and the filtrate was poured into water. The precipitate was then collected by filtration. The precipitate was dried in a vacuum dryer to obtain a quinone diazide compound (QD-01) having the following structure.

[0141] Synthesis Example 5: Compound P1 (Polymerizable component: polymer having a polymerizable unsaturated group) Copolymerization ratio (by weight): ethyl acrylate (hereinafter, "EA") / 2-ethylhexyl methacrylate (hereinafter, "2-EHMA") / styrene (hereinafter, "St") / glycidyl methacrylate (hereinafter, "GMA") / acrylic acid (hereinafter, "AA") = 20 / 40 / 20 / 5 / 15.

[0142] In a reaction vessel in a nitrogen atmosphere, 150 g of diethylene glycol monoethyl ether acetate (hereinafter, "DMEA") was charged, and the temperature was raised to 80°C using an oil bath. A mixture consisting of 20 g of EA, 40 g of 2-EHMA, 20 g of St, 15 g of AA, 0.8 g of 2,2'-azobisisobutyronitrile, and 10 g of DMEA was added dropwise over 1 hour. After the dropwise addition was completed, the polymerization reaction was carried out for another 6 hours. Then, 1 g of hydroquinone monomethyl ether was added to stop the polymerization reaction. Subsequently, a mixture consisting of 5 g of GMA, 1 g of triethylbenzylammonium chloride, and 10 g of DMEA was added dropwise over 0.5 hours. After the dropwise addition was completed, the addition reaction was carried out for another 2 hours. The obtained reaction solution was purified with methanol to remove unreacted impurities, and further dried in vacuum for 24 hours to obtain compound P1.

[0143] Synthesis Example 6: Compound P2 (Polymerizable component: polymer having a polymerizable unsaturated group) Copolymerization ratio (by weight): bifunctional epoxy acrylate monomer (Epoxy Ester 3002A; manufactured by Kyoeisha Chemical Co., Ltd.) / bifunctional epoxy acrylate monomer (Epoxy Ester 70PA; manufactured by Kyoeisha Chemical Co., Ltd.) / GMA / St / AA=20 / 40 / 5 / 20 / 15.

[0144] In a reaction vessel in a nitrogen atmosphere, 150g of DMEA was charged and heated to 80°C using an oil bath. A mixture consisting of 20g of epoxy ester 3002A, 40g of epoxy ester 70PA, 20g of St, 15g of AA, 0.8g of 2,2'-azobisisobutyronitrile and 10g of DMEA was added dropwise over 1 hour. After completion of the dropwise addition, the polymerization reaction was carried out for another 6 hours. Then, 1g of hydroquinone monomethyl ether was added to stop the polymerization reaction. Subsequently, a mixture consisting of 5g of GMA, 1g of triethylbenzylammonium chloride and 10g of DMEA was added dropwise over 0.5 hours. After completion of the dropwise addition, the addition reaction was carried out for another 2 hours. The obtained reaction solution was purified with methanol to remove unreacted impurities, and further dried in vacuum for 24 hours to obtain compound P2.

[0145] Synthesis Example 7: Compound P3, which is a urethane-modified compound of compound P2 (polymerizable component: polymer having a polymerizable unsaturated group) In a reaction vessel under a nitrogen atmosphere, 100 g of diethylene glycol monoethyl ether acetate (hereinafter, "DMEA") was charged, and the temperature was raised to 80°C using an oil bath. To this, a mixture consisting of 10 g of photosensitive component P2, 3.5 g of n-hexyl isocyanate, and 10 g of DMEA was added dropwise over 1 hour. After the dropwise addition was completed, the reaction was allowed to proceed for an additional 3 hours. The resulting reaction solution was purified with methanol to remove unreacted impurities, and further vacuum dried for 24 hours to obtain compound P3 having a urethane bond.

[0146] Synthesis Example 8: Synthesis of inorganic particle-bonded polysiloxane (PS-04) A three-neck flask was charged with 4.36g (0.032mol) of methyltrimethoxysilane, 4.20g (0.016mol) of 3-trimethoxysilylpropylsuccinic anhydride, 22.21g (0.11mol) of phenyltrimethoxysilane, 145.72g of 20.6% by mass titanium oxide-silicon oxide composite particle methanol dispersion, and 116.74g of diacetone alcohol. An aqueous phosphoric acid solution in which 0.154g of phosphoric acid was dissolved in 8.93g of water was added over 10 minutes while stirring at room temperature. After that, the flask was immersed in a 40°C oil bath and stirred for 60 minutes, and the oil bath was heated to 115°C over 30 minutes. One hour after the start of the temperature increase, the internal temperature of the solution reached 100°C, and it was heated and stirred for 2 hours from there (internal temperature was 100-110°C). The resin solution obtained by heating and stirring was cooled in an ice bath, and then 2% by weight of anion exchange resin and cation exchange resin were added to the resin solution, followed by stirring for 12 hours. After stirring, the anion exchange resin and cation exchange resin were removed by filtration, yielding a solution of polysiloxane (PS-04) bound to inorganic particles. During the temperature increase and heating and stirring, nitrogen was passed through at 0.05 liters per minute. A total of 121.85 g of by-products, methanol and water, were distilled out during the reaction. The solids concentration of the resulting solution of polysiloxane bound to inorganic particles, PS-04, was 31% by mass.

[0147] Synthesis Example 9: Synthesis of polysiloxane with inorganic particles (PS-05) A solution of polysiloxane (PS-05) with inorganic particles bonded thereto was obtained in the same manner as in Synthesis Example 8, except that 3.27 g (0.024 mol) of methyltrimethoxysilane, 3.15 g (0.012 mol) of 3-trimethoxysilylpropylsuccinic anhydride, 16.66 g (0.084 mol) of phenyltrimethoxysilane, 170.012 g of a 20.6 mass% titanium oxide-silicon oxide composite particle methanol dispersion, 116.74 g of diacetone alcohol, 6.70 g of water, and 0.115 g of phosphoric acid were used. A total of 134.78 g of by-products, methanol and water, were distilled out during the reaction. The solids concentration of the resulting solution of polysiloxane with inorganic particles bonded thereto, PS-05, was 31 mass%.

[0148] Synthesis Example 10: Synthesis of inorganic particle-bonded polysiloxane (PS-06) A solution of polysiloxane (PS-06) with inorganic particles bonded thereto was obtained in the same manner as in Synthesis Example 8, except that 2.72 g (0.02 mol) of methyltrimethoxysilane, 2.62 g (0.01 mol) of 3-trimethoxysilylpropylsuccinic anhydride, 13.88 g (0.07 mol) of phenyltrimethoxysilane, 242.87 g of a 20.6 mass% titanium oxide-silicon oxide composite particle methanol dispersion, 145.93 g of diacetone alcohol, 5.58 g of water, and 0.096 g of phosphoric acid were used. A total of 184.63 g of by-products, methanol and water, were distilled out during the reaction. The solids concentration of the resulting solution of polysiloxane with inorganic particles bonded thereto, PS-06, was 31 mass%.

[0149] Preparation Example 1: Preparation of semiconductor solution 1.0 mg of CNT (CNI, single-walled CNT, purity 95%) was added to a 10 ml solution of 2.0 mg of poly(3-hexylthiophene) (P3HT) (Aldrich Corporation), and the mixture was subjected to ultrasonic stirring at 20% output for 4 hours using an ultrasonic homogenizer (Tokyo Rikakikai Co., Ltd., VCX-500) while cooling on ice, to obtain CNT dispersion A (CNT composite concentration relative to solvent: 0.96 g / l).

[0150] Next, a semiconductor solution for forming a semiconductor layer was prepared. The above CNT dispersion A was filtered using a membrane filter (pore size 10 μm, diameter 25 mm, Millipore Omnipore Membrane) to remove CNT composites with a length of 10 μm or more. 5 ml of o-dichlorobenzene (Wako Pure Chemical Industries, Ltd.) was added to the obtained filtrate, and then a rotary evaporator was used to distill off chloroform, which is a low boiling point solvent, and the solvent was replaced with o-dichlorobenzene to obtain CNT dispersion B. 3 mL of o-dichlorobenzene was added to 1 ml of CNT dispersion B to obtain a semiconductor solution (CNT composite concentration relative to the solvent: 0.03 g / l).

[0151] Preparation Example 2: Preparation of conductive paste In a 100 ml clean bottle, 1.6 g of compound P1, 0.4 g of compound P3, 0.4 g of photopolymerization initiator OXE-01 (manufactured by BASF Japan Ltd.), 0.06 g of acid generator SI-110 (manufactured by Sanshin Chemical Industry Co., Ltd.), and 38 g of diacetone alcohol (manufactured by Sankyo Chemical Co., Ltd.) were added and mixed with a rotation-revolution vacuum mixer "Awatori Rentaro" (registered trademark) (ARE-310; manufactured by Thinky Co., Ltd.) to obtain 40.86 g of photosensitive resin solution (solid content 4.0 wt%). 20.0 g of the obtained photosensitive resin solution was mixed with 5.0 g of Ag particles having a volume average particle diameter of 0.5 μm, and kneaded using a three-roller "EXAKT M-50" (trade name, manufactured by EXAKT Co., Ltd.) to obtain 25 g of conductive paste.

[0152] Example 1 16.36 g of a solution of polysiloxane bonded to inorganic particles (PS-01, polymer (A)), 0.60 g of Arastar 700 (manufactured by Arakawa Chemical Industries, Ltd., polymer (B), styrene-maleic acid half ester copolymer) (mixture weight ratio of polymer (A) to polymer (B) is 90:10), 0.54 g of quinone diazide compound (QD-01), 300 ppm of BYK-333 (polysiloxane surfactant, polyether modified polydimethylsiloxane, manufactured by BYK Japan Co., Ltd.), and 33.04 g of DAA were mixed and stirred under yellow light to obtain a uniform solution, and then filtered through a 0.20 μm filter to obtain an insulating material solution (solid concentration 12 mass%).

[0153] Using the obtained insulator solution, the relative dielectric constant of the insulating layer was measured by the method described in (2). In addition, a capacitor was fabricated by the method described in (3), the thickness of the dielectric film (insulating layer) was evaluated by the method described in (1), and the short circuit rate was evaluated by the method described in (6). In addition, a FET was fabricated by the method described in (4), the thickness of the gate insulating layer was evaluated by the method described in (1), and the FET leakage rate was evaluated by the method described in (7).

[0154] In addition, a rectifier circuit was fabricated by the method described in (5), the thickness of the insulating layer was evaluated by the method described in (1), and the yield of the rectifier circuit was evaluated by the method described in (8). The results are shown in Tables 1 to 4.

[0155] Example 2 An insulating material solution (solid concentration 12% by mass) was obtained in the same manner as in Example 1, except that 1.67 g of the polysiloxane solution (PS-02, polymer (B)) synthesized in Synthesis Example 2 was used instead of Alastar 700, the amount of the polysiloxane solution bonded to inorganic particles (PS-01) was changed to 18.00 g, and the amount of DAA was changed to 30.33 g (the mixing weight ratio of polymer (A) to polymer (B) was 90:10).

[0156] The obtained insulating solution was used for evaluation in the same manner as in Example 1. The results are shown in Tables 1 to 4. Table 2 shows the evaluation results for the capacitor, Table 3 shows the evaluation results for the FET, and Table 4 shows the evaluation results for the rectifier circuit.

[0157] Example 3 An insulator solution (solid concentration 12% by mass) was obtained in the same manner as in Example 1, except that 1.67 g of the polysiloxane solution (PS-03, polymer (B)) synthesized in Synthesis Example 3 was used instead of Alastar 700, the amount of the polysiloxane solution bonded to inorganic particles (PS-01) was changed to 18.00 g, and the amount of DAA was changed to 30.33 g (the mixture weight ratio of polymer (A) and polymer (B) was 90:10).

[0158] The obtained insulating solution was used for evaluation in the same manner as in Example 1. The results are shown in Tables 1 to 4.

[0159] Example 4 An insulating material solution (solid concentration 12 mass%) was obtained in the same manner as in Example 3, except that the amount of the polysiloxane solution (PS-01) bonded to inorganic particles was changed to 13.64 g, the amount of the polysiloxane solution (PS-03) was changed to 4.17 g, and the amount of DAA was changed to 32.20 g (the mixture weight ratio of polymer (A) and polymer (B) was 75:25).

[0160] Using the obtained insulator solution, the relative dielectric constant of the insulating layer was measured by the method described in (2). In addition, a capacitor was fabricated by the method described in (3), the thickness of the dielectric film (insulating layer) was evaluated by the method described in (1), and the short circuit rate was evaluated by the method described in (6). The results are shown in Tables 1 and 2.

[0161] Example 5 An insulating material solution (solid concentration 12 mass%) was obtained in the same manner as in Example 3, except that the amount of the polysiloxane solution (PS-01) bonded to inorganic particles was changed to 9.09 g, the amount of the polysiloxane solution (PS-03) was changed to 8.33 g, and the amount of DAA was changed to 32.58 g (the mixture weight ratio of polymer (A) and polymer (B) was 50:50).

[0162] The obtained insulating solution was used for evaluation in the same manner as in Example 4. The results are shown in Tables 1 and 2.

[0163] Example 6 An insulating material solution (solid concentration 12 mass%) was obtained in the same manner as in Example 3, except that the amount of the polysiloxane solution (PS-01) bonded to inorganic particles was changed to 17.27 g, the amount of the polysiloxane solution (PS-03) was changed to 0.83 g, and the amount of DAA was changed to 31.89 g (the mixing weight ratio of polymer (A) and polymer (B) was 95:5).

[0164] The obtained insulating solution was used for evaluation in the same manner as in Example 4. The results are shown in Tables 1 and 2.

[0165] Example 7 18.18 g of a solution of polysiloxane bonded to inorganic particles (PS-01), 0.54 g of a quinone diazide compound (QD-01), 300 ppm of BYK-333 (a polysiloxane surfactant, manufactured by BYK Japan Co., Ltd.), and 31.82 g of DAA were mixed and stirred under a yellow light to obtain a homogeneous solution, which was then filtered through a 0.20 μm filter to obtain an insulating material solution (solid concentration 12 mass%).

[0166] The obtained insulating solution was used for evaluation in the same manner as in Example 1. The results are shown in Tables 1 to 4.

[0167] Example 8 An insulating solution was prepared in the same manner as in Example 7, except that BYK-331 (polysiloxane-based surfactant, polyether-modified polydimethylsiloxane, manufactured by BYK-Chemie Japan Co., Ltd.) was used instead of BYK-333. Using the obtained insulating solution, evaluations were performed in the same manner as in Example 4. The results are shown in Tables 1 and 2.

[0168] Example 9 An insulating material solution (solid concentration 12 mass%) was obtained in the same manner as in Example 7, except that 19.20 g of the inorganic particle-bonded polysiloxane solution (PS-04) was used instead of the inorganic particle-bonded polysiloxane solution (PS-01), and the amount of DAA was changed to 32.50 g. The obtained insulating solution was used to perform the same evaluation as in Example 1. The results are shown in Tables 1 to 4.

[0169] Example 10 An insulator solution was prepared in the same manner as in Example 7, except that the solution of polysiloxane bonded to inorganic particles (PS-05) was used instead of the solution of polysiloxane bonded to inorganic particles (PS-04). Using the obtained insulator solution, evaluations were performed in the same manner as in Example 1. The results are shown in Tables 1 to 4.

[0170] Example 11 An insulator solution was prepared in the same manner as in Example 7, except that the solution of polysiloxane bonded to inorganic particles (PS-06) was used instead of the solution of polysiloxane bonded to inorganic particles (PS-04). Using the obtained insulator solution, evaluations were performed in the same manner as in Example 1. The results are shown in Tables 1 to 4.

[0171] Example 12 An insulating material solution (solid concentration 12 mass%) was obtained in the same manner as in Example 3, except that 17.30 g of a polysiloxane solution (PS-06) with inorganic particles bonded thereto was used instead of the polysiloxane solution with inorganic particles bonded thereto (PS-01), the amount of DAA was changed to 32.90 g, and the amount of polysiloxane solution (PS-03, polymer (B)) was changed to 1.66 g. The obtained insulating solution was used to perform the same evaluation as in Example 1. The results are shown in Tables 1 to 4.

[0172] Comparative Example 1 An insulating solution was prepared in the same manner as in Example 7, except that DFX-18 (a fluorine-containing surfactant, manufactured by Neos Co., Ltd.) was used instead of BYK-333.

[0173] The obtained insulator solution was used for evaluation in the same manner as in Example 1. The results are shown in Tables 1 to 4. Since the coefficient of variation of the insulating layer exceeded 10%, the short circuit rate evaluation of the capacitor, the FET leakage rate evaluation, and the yield evaluation of the rectifier circuit were all poor.

[0174] Comparative Example 2 An insulator solution was prepared in the same manner as in Example 7, except that the amount of DFX-18 added was 900 ppm. Using the obtained insulator solution, evaluations were performed in the same manner as in Example 4. The results are shown in Tables 1 and 2. Since the coefficient of variation of the insulating layer exceeded 10%, the short circuit rate evaluation of the capacitor was poor.

[0175] Comparative Example 3: Preparation of Insulator Solution An insulator solution was prepared in the same manner as in Example 1, except that polystyrene (manufactured by SigmaAldrich) was used instead of Alastar 700. However, titanium oxide particles precipitated, and a homogeneous solution could not be obtained.

[0176] [Table 1]

[0177] [Table 2]

[0178] [Table 3]

[0179] [Table 4] [Explanation of symbols]

[0180] 1, 2, 3, 4, 5, 6 FETs 11, 31, 61, 71 Gate electrode 12, 62 Gate insulating layer 13, 35, 64, 75 Source electrode 14, 34, 63, 74 Semiconductor layer 15, 36, 65, 76 Drain electrode 38, 78 Wiring 39, 79 Via 100, 200, 300, 400, 500, 600, 700 Insulating substrate 301, 701 FET elements 302, 702 Capacitor element 21, 32, 51, 72 Lower electrode 22, 52 Dielectric film 23, 37, 53, 77 upper electrode 33, 33A, 33B, 73 Insulation layer 40 Antenna 41 Demodulation circuit 42 Control circuit 43 Modulation Circuit 44 Memory circuit 45 Power generation section

Claims

1. An element comprising at least (1) a patterned lower electrode, (2) an insulating layer, and (3) a patterned upper electrode laminated on a substrate, the insulating layer contains a polymer (A) covalently bonded to inorganic particles, the insulating layer further comprises a polymer (B) which is not covalently bonded to the inorganic particles, has a structure different from that of the polymer (A), and has a functional group capable of forming a hydrogen bond with a hydroxy group on the surface of the inorganic particles contained in the polymer (A); A device characterized in that the coefficient of variation in thickness of said insulating layer in a portion on said lower electrode that is not covered by said upper electrode is 10% or less.

2. 2. The element according to claim 1, wherein the inorganic particles are particles of a compound containing one or more elements selected from the group consisting of silicon, magnesium, calcium, strontium, barium, lanthanum, cerium, tin, titanium, zirconium, hafnium, yttrium, niobium, tantalum and aluminum.

3. The element according to claim 1 or 2, further comprising a polyether-modified polydimethylsiloxane in the insulating layer.

4. 4. The element according to claim 1, wherein the weight ratio of the polymer (A) to all polymer components contained in the insulating layer is 50% by weight or more and 94% by weight or less.

5. The element according to claim 1 , wherein the number average particle size of the inorganic particles contained in the insulating layer is within a range of 1 nm or more and 100 nm or less.

6. 6. The element according to claim 1, wherein the content of the inorganic particles contained in the insulating layer is 5 vol % or more and 50 vol % or less in terms of volume fraction.

7. 7. The element according to claim 1, wherein the average thickness of the insulating layer on the lower electrode is within the range of 10 nm to 1000 nm.

8. The element according to any one of claims 1 to 7, wherein the substrate is a film.

9. A device according to any preceding claim, wherein the bottom electrode is copper.

10. 10. The element of claim 1, wherein the element is a capacitor.

11. The device according to claim 1 , wherein the device is a field effect transistor.

12. The device of claim 11 further comprising a semiconductor film comprising carbon nanotubes.

13. A method for producing an element according to any one of claims 1 to 12, comprising the steps of forming a conductive pattern to be a lower electrode on a substrate, forming an insulating layer on the conductive pattern, and forming a conductive pattern to be an upper electrode on the insulating layer, wherein the step of forming the insulating layer comprises applying a solution containing a polymer (A) covalently bonded to inorganic particles, drying the solution to obtain a coating film, and then heating and curing the coating film.

14. A wireless communication device comprising an element according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Photosensitive resin composition and semiconductor device using the same

    JP2006309202A

  • Organic thin-film transistor using gate insulation layer containing metal oxide nanoparticles in photocurable transparent polymer by sol-gel and photocuring reaction, and manufacturing method for them

    JP2009182329A

  • Field effect organic transistor

    JP2011258894A

  • Field effect transistor

    JP2013115162A

  • Ferroelectric memory element, method for producing same, memory cell using ferroelectric memory element, and radio communication device using ferroelectric memory element