All-solid-state lithium secondary battery and method for producing same
The integration of graphitized platelet carbon nanofibers and silver nanoparticles in the negative electrode layer of all-solid-state lithium secondary batteries addresses lithium ion reduction and dendrite formation, improving efficiency and lifespan while maintaining energy density and reducing silver usage.
Patent Information
- Application Number
- JP2023524813
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-28
- Filing Date
- 2022-05-27
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2042-05-27
AI Technical Summary
All-solid-state lithium secondary batteries face issues with lithium ion reduction during charging, leading to reduced storage capacity, dendrite formation, and decreased lifespan due to voids between the solid electrolyte and metal layer, and excessive volume increase when external pressure is applied to prevent void formation.
Incorporating a negative electrode active material layer composed of graphitized platelet carbon nanofibers and silver nanoparticles, which enhance lithium ion mobility and storage, reducing the need for high external pressure while maintaining battery stability and energy density.
The solution improves initial charge/discharge efficiency, extends battery life, and maintains energy density by effectively storing and transferring lithium ions, even with a lower content of silver nanoparticles, thus enhancing the cost-competitiveness of the battery.
Smart Images

Figure 0007578329000003 
Figure 0007578329000004 
Figure 0007578329000005
Abstract
Description
[Technical field]
[0001] The present invention relates to an all-solid-state lithium secondary battery and a method for producing the same. [Background technology]
[0002] Secondary batteries have been mainly applied to small fields such as mobile devices and notebook computers, but recently their application has expanded to medium and large fields, for example, fields requiring high energy and high output such as energy storage systems (ESS) and electric vehicles (EV).
[0003] Meanwhile, interest in all-solid lithium secondary batteries has been growing recently. The all-solid lithium secondary battery is a secondary battery that uses a non-flammable inorganic solid electrolyte instead of a liquid electrolyte, and has been drawing attention in that it has higher thermal stability than a lithium secondary battery that uses a liquid electrolyte, and is very unlikely to explode due to leakage during overcharging, and does not require additional equipment to prevent such an explosion.
[0004] However, since all-solid-state lithium secondary batteries use a solid electrolyte that is somewhat large in volume, there have been many attempts to improve the energy density of the battery. For this purpose, a metal layer capable of forming an alloy with lithium, such as lithium metal, is used as the negative electrode active material layer. However, when such a metal layer is used, as the lithium deposited on the metal layer is ionized and dissolved, voids are generated between the solid electrolyte and the metal layer, adversely affecting the operation of the battery. In addition, when the all-solid-state lithium secondary battery is discharged, lithium metal is deposited in a dendrite shape from the surface of the metal layer, thereby reducing the life and stability of the all-solid-state lithium secondary battery.
[0005] In order to solve this problem, a method of applying a high external pressure by disposing end plates on the positive and negative electrodes to prevent the generation of voids has been used in the past. However, when end plates that apply external pressure are used, the volume of the all-solid-state lithium secondary battery increases excessively, resulting in a problem of a decrease in the energy density of the all-solid-state lithium secondary battery.
[0006] Therefore, there is a need for new methods that can improve the life and stability of all-solid-state lithium secondary batteries. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide an all-solid-state lithium secondary battery in which lithium ions can be reduced during charging to effectively store lithium metal, thereby improving initial charge / discharge efficiency and life characteristics.
[0008] Another problem to be solved by the present invention is to provide a cost-competitive all-solid-state lithium secondary battery by reducing the content of silver nanoparticles used.
[0009] Still another problem to be solved by the present invention is to provide a method for producing the above-mentioned all-solid-state lithium secondary battery. [Means for solving the problem]
[0010] According to one embodiment of the present invention, there is provided an all-solid-state lithium secondary battery including a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, wherein the negative electrode active material layer includes graphitized platelet carbon nanofibers (GPCNF) and silver nanoparticles.
[0011] According to another embodiment of the present invention, there is provided a method for manufacturing an all-solid-state lithium secondary battery, the method including: a first step of reducing silver ions in a mixture of silver ions and graphitized platelet carbon nanofibers to form a dry mixed powder including the graphitized platelet carbon nanofibers and silver nanoparticles disposed on the graphitized platelet carbon nanofibers; and a second step of forming a negative electrode active material layer on a negative electrode current collector via a negative electrode mixture including the dry mixed powder. Effect of the Invention
[0012] In the all-solid-state lithium secondary battery according to the present invention, the negative electrode active material layer includes the graphitized platelet carbon nanofibers and the silver nanoparticles, and thus, during charging, lithium ions are reduced and precipitated by the negative electrode active material layer, and can be effectively stored in the negative electrode. During discharging, the stored lithium can be dissolved in the form of lithium ions and transferred to the positive electrode. The graphitized platelet carbon nanofibers can increase the mobility of the lithium ions, thereby improving the initial charge / discharge efficiency and life characteristics of the battery. Furthermore, by using the graphitized platelet carbon nanofibers, the above-mentioned lithium ion transfer can be effectively performed even when a low content of silver nanoparticles is used, and the price competitiveness of the manufactured all-solid-state lithium secondary battery can be improved. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a schematic diagram for illustrating the graphitized platelet carbon nanofiber referred to in the present invention. [Diagram 2] FIG. 2 is a schematic diagram for explaining the platelet carbon nanofiber referred to in the present invention. [Diagram 3] FIG. 2 is a schematic diagram for illustrating the graphitized platelet carbon nanofiber referred to in the present invention. [Figure 4] FIG. 1 is a schematic diagram illustrating an all-solid-state lithium secondary battery according to an embodiment of the present invention. [Diagram 5] FIG. 1 is a schematic diagram illustrating an all-solid-state lithium secondary battery according to an embodiment of the present invention. [Figure 6] 1 is a TEM photograph of the platelet carbon nanofibers referred to in the present invention. [Figure 7] 1 is a TEM photograph of the graphitized platelet carbon nanofibers referred to in the present invention. [Figure 8] 1 is a TEM image of graphitized platelet carbon nanofibers containing silver nanoparticles used in an all-solid-state lithium secondary battery according to one embodiment of the present invention. [Figure 9] 4 is a TEM image of platelet carbon nanofibers containing silver nanoparticles used in an all-solid-state lithium secondary battery according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0015] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless it has a clearly different meaning in the context.
[0016] In this specification, the terms "comprise", "comprise", "have" and the like are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, but are not intended to preclude the presence or additional possibility of one or more other features, numbers, steps, components, or combinations thereof.
[0017] In this specification, the "specific surface area" is measured by the BET method, and specifically, it can be calculated from the amount of nitrogen gas adsorbed at liquid nitrogen temperature (77K) using a BELSORP-mini II manufactured by BEL Japan.
[0018] In the present specification, the graphitized platelet carbon nanofiber may mean a carbon structure having a fibrous shape in which graphene sheets are laminated. Referring to FIG. 1, the graphitized platelet carbon nanofiber may mean a carbon nanofiber having a structure in which a hexagonal mesh plane of carbon is arranged perpendicular to a fiber axis L. The length of the graphitized platelet carbon nanofiber means the length of a line or curve that appears when one end and the other end of the graphitized platelet carbon nanofiber are connected along the graphitized platelet carbon nanofiber, and may mean, for example, the distance between the one end and the other end along the fiber axis of the graphitized platelet carbon nanofiber when the graphitized platelet carbon nanofiber is stretched in a straight line. In addition, the diameter of the graphitized platelet carbon nanofiber means the width of the graphitized platelet carbon nanofiber in the direction of a short axis D that is perpendicular to the fiber axis L of the graphitized platelet carbon nanofiber and parallel to the plane of the graphene sheet or the hexagonal mesh plane of carbon.
[0019] 2 and 3 are schematic diagrams for explaining the side S of the carbon nanofiber in FIG. 1. Referring to FIG. 2 and FIG. 3, the difference between the platelet carbon nanofiber and the graphitized platelet carbon nanofiber can be seen. The platelet carbon nanofiber has the same form as described in the above paragraph. However, the side of the platelet carbon nanofiber is a form in which the edge plane (E in FIG. 2) of the graphene sheet (black line segment in FIG. 2 and FIG. 3) is exposed, whereas the side of the graphitized platelet carbon nanofiber is a form in which the basal plane (B in FIG. 3) is exposed. Such a difference is also clearly seen in the TEM photographs of the platelet carbon nanofiber in FIG. 6 and the graphitized platelet carbon nanofiber in FIG. 7.
[0020] Specifically, the graphitized platelet carbon nanofiber has a shape in which a plurality of graphene sheets are stacked in the growth direction of the graphitized platelet carbon nanofiber, and the graphitized platelet carbon nanofiber includes a bent portion protruding toward a side of the graphitized platelet carbon nanofiber, and the bent portion corresponds to a basal surface of the graphene sheet. The bent portion is formed by one graphene sheet extending and connecting with another graphene sheet, and exposes the basal surface from the side of the graphitized platelet carbon nanofiber to the outside as shown in FIG. 3 and FIG. 7. More specifically, the basal surface may have a closed loop shape and be present in a bent state at the side of the graphitized platelet carbon nanofiber. The loop shape may appear periodically along the growth direction of the graphitized platelet carbon nanofiber.
[0021] The graphitized platelet carbon nanofibers may be formed by graphitizing the platelet carbon nanofibers through heat treatment at high temperature. Specifically, the graphitized platelet carbon nanofibers may be formed by heat treating the platelet carbon nanofibers at a temperature of 2,000° C. or higher, for example, 2,000° C. to 3,500° C. The heat treatment time may be 10 minutes to 24 hours.
[0022] In this specification, the method of measuring the X-ray diffraction (XRD) of the graphitized platelet carbon nanofiber and the platelet carbon nanofiber is as follows. The XRD analysis can be performed using a Bruker AXS d4 Endeavor XRD (voltage: 40 kV, current: 40 mA) under the condition of Cu Kα radiation (wavelength: 1.54 Å) at a scanning speed of 87.5 seconds per 0.02° from 2θ (Theta) 10° to 90°. Among the measurement results, the full width at half-maximum (FWHM) of the (002) crystal peak appearing at 2θ in the vicinity of 20° to 30° can be measured, and the d(002) value and Lc(002) value can be calculated according to the Scherrer formula.
[0023] I of this specification D / I G The ratio can be measured from the wavelength-peak graph during Raman spectrum measurement. Specifically, a baseline is set and the graph is fitted so that the D peak and G peak can be distinguished, and then the D peak intensity is divided by the G peak intensity to obtain the ratio I. D / I G (Using built-in software, NRS-2000B, Jasco) -1 The G peak near the carbon sp 2 E in Bond 2g This is due to the vibration mode at 1350cm -1The D peak near the sp 2 It appears when there is a defect in the bond.
[0024] In this specification, the average diameter of the graphitized platelet carbon nanofibers (or platelet carbon nanofibers) corresponds to the average value of the diameters of the top 50 graphitized platelet carbon nanofibers (or platelet carbon nanofibers) and the bottom 50 graphitized platelet carbon nanofibers (or platelet carbon nanofibers) in order of diameter when the negative electrode active material layer is observed with an SEM at a magnification of ×20,000.
[0025] In this specification, the average length of the graphitized platelet carbon nanofibers (or platelet carbon nanofibers) corresponds to the average value of the lengths of the top 50 graphitized platelet carbon nanofibers (or platelet carbon nanofibers) and the bottom 50 graphitized platelet carbon nanofibers (or platelet carbon nanofibers) in order of length when the negative electrode active material layer is observed with an SEM at a magnification of ×20,000.
[0026] In this specification, the average particle size of silver nanoparticles corresponds to the average value of the particle sizes of the top 50 largest silver nanoparticles and the bottom 50 largest silver nanoparticles when the platelet carbon nanofiber containing the produced silver nanoparticles or the platelet carbon nanofiber containing silver nanoparticles of the negative electrode active material layer is observed by TEM at a magnification of ×1,000,000.
[0027] The present invention will be specifically described below.
[0028] All-solid-state lithium secondary battery An all-solid-state lithium secondary battery according to an embodiment of the present invention includes a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, and the negative electrode active material layer may include graphitized platelet carbon nanofibers (GPCNFs) and silver nanoparticles.
[0029] (1) Negative electrode active material layer The all-solid-state lithium secondary battery may include a negative electrode active material layer. Specifically, the all-solid-state lithium secondary battery may include a negative electrode, and the negative electrode may include a negative electrode current collector and a negative electrode active material layer.
[0030] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, the negative electrode current collector may be made of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. Specifically, a transition metal that easily adsorbs carbon, such as nickel or stainless steel metal, may be used as the negative electrode current collector.
[0031] 4, the negative electrode active material layer 100 may be disposed on at least one surface of the negative electrode current collector 110. Specifically, the negative electrode active material layer 100 may be disposed on one surface of the negative electrode current collector 110, or may be disposed on both surfaces of the negative electrode current collector (not shown).
[0032] The negative electrode active material layer may include graphitized platelet carbon nanofibers and silver nanoparticles. Specifically, the negative electrode active material layer may be composed of graphitized platelet carbon nanofibers and silver nanoparticles.
[0033] 1) Graphitized platelet carbon nanofibers The graphitized platelet carbon nanofibers may act as a migration path for allowing lithium ions transferred from the positive electrode active material layer to be easily deposited and stored on the negative electrode current collector.
[0034] The graphitized platelet carbon nanofiber includes a bent portion protruding toward a side surface of the graphitized platelet carbon nanofiber, and the bent portion corresponds to a basal surface of the graphene sheet. That is, the basal surface is exposed from the side surface of the graphitized platelet carbon nanofiber toward the outside. More specifically, the basal surface may have a closed loop shape and be bent at the side surface of the graphitized platelet carbon nanofiber. The loop shape may appear periodically along the growth direction of the graphitized platelet carbon nanofiber. Lithium ions may rapidly move on the basal surface, and the graphitized platelet carbon nanofiber may play a role in inducing rapid movement of lithium ions. As a result, the irreversible capacity for initial lithium ion absorption may be reduced.
[0035] When the graphitized platelet carbon nanofiber is subjected to XRD measurement, d(002) of the graphitized platelet carbon nanofiber can be 0.330 nm to 0.350 nm, specifically 0.330 nm to 0.345 nm, more specifically 0.330 nm to 0.340 nm. When the above range is satisfied, the crystallinity of the graphitized platelet carbon nanofiber is high, the electrical conductivity is greatly improved, and it is also advantageous for the absorption and migration of lithium ions.
[0036] When XRD measurement is performed on the platelet carbon nanofiber, the Lc(002) of the platelet carbon nanofiber may be 20 nm to 200 nm, specifically 20 nm to 150 nm, more specifically 20 nm to 100 nm, for example, 35 nm to 100 nm. When the above range is satisfied, the graphitization degree of the graphitized platelet carbon nanofiber is excellent, the electrical conductivity is improved, and the crystalline defects in the length direction of the graphitized platelet carbon nanofiber are small, so that the mechanical strength of the material itself can be excellent. Therefore, in the process of dispersing and using the graphitized platelet carbon nanofiber, the phenomenon of the graphitized platelet carbon nanofiber being cut can be reduced, and the deterioration of the battery due to defects in the graphitized platelet carbon nanofiber during charging and discharging of the battery can be minimized.
[0037] When performing Raman spectroscopy on the graphitized platelet carbon nanofibers, the I D / I G can be 0.1 to 1.0, specifically 0.1 to 0.5, and more specifically 0.1 to 0.3. When the above range is satisfied, the crystallinity of the graphitized platelet carbon nanofiber is high, the electrical conductivity is greatly improved, and it is also advantageous for the absorption and migration of lithium ions.
[0038] The average length of the graphitized platelet carbon nanofibers may be 0.1 μm to 5 μm, specifically 0.1 μm to 2.5 μm, more specifically 0.1 μm to 1 μm. When the above range is satisfied, a conductive path can be effectively formed in the negative electrode active material layer, and the efficiency of the all-solid-state lithium secondary battery can be improved. In addition, even when the silver nanoparticles react with lithium ions to change the volume, the structural collapse of the negative electrode active material layer can be effectively suppressed.
[0039] The graphitized platelet carbon nanofibers may have an average diameter of 10 nm to 500 nm, specifically 10 nm to 400 nm, more specifically 10 nm to 300 nm. When the average diameter satisfies the above range, even if lithium ions are absorbed and transferred through the graphitized platelet carbon nanofibers, the mechanical structure of the graphitized platelet carbon nanofibers can be effectively maintained.
[0040] The specific surface area of the graphitized platelet carbon nanofiber is 5 m 2 / g~10m 2 / g, specifically 5m 2 / g~80m 2 / g, more specifically 5m 2 / g~60m 2 When the above range is satisfied, the silver nanoparticles can be stably arranged on the surface of the graphitized platelet carbon nanofibers, and the absorption and migration of lithium ions can be effectively performed.
[0041] The graphitized platelet carbon nanofibers may be included in the negative electrode active material layer at 50 wt% to 98 wt%, specifically 60 wt% to 95 wt%, more specifically 70 wt% to 90 wt%. When the above range is satisfied, the reduction in the energy density of the all-solid-state lithium secondary battery can be minimized and the mobility of lithium ions can be effectively improved, thereby improving the initial charge / discharge efficiency and life characteristics of the all-solid-state lithium secondary battery.
[0042] 2) Silver nanoparticles The silver nanoparticles have a lithophilic property and can easily form an alloy with lithium ions, and thus the silver nanoparticles can form an alloy with the lithium ions transferred from the positive electrode active material layer to promote the absorption and diffusion of the lithium ions into the negative electrode active material layer.
[0043] The silver nanoparticles may include silver (Ag). Furthermore, the silver nanoparticles may further include at least one selected from the group consisting of gold, platinum, palladium, silicon, aluminum, bismuth, tin, indium, and zinc. Alternatively, the silver nanoparticles may be made of silver. The silver nanoparticles may be in a solid phase.
[0044] The silver nanoparticles may be disposed on the surface of the graphitized platelet carbon nanofibers. Specifically, the silver nanoparticles may be formed by reducing silver ions in a silver ion aqueous solution on the surface of the graphitized platelet carbon nanofibers, and thus the silver nanoparticles may be disposed on the surface of the graphitized platelet carbon nanofibers. Alternatively, a powder of silver nanoparticles and the platelet carbon nanofibers may be mixed in a powder state, and the silver nanoparticles may be disposed on the surface of the platelet carbon nanofibers.
[0045] The average particle size of the silver nanoparticles may be 1 nm to 100 nm, specifically 1 nm to 50 nm, more specifically 1 nm to 30 nm, for example, 1 nm to 2 nm. When the above range is satisfied, the silver nanoparticles can be effectively dispersed in the negative electrode active material layer, and even if the content of the silver nanoparticles is at a low level, lithium ions can be easily absorbed and diffused. In addition, the initial efficiency and life characteristics of the battery can be improved.
[0046] In the negative electrode active material layer, the silver nanoparticles may be included in an amount of 1 wt% to 40 wt% based on the total weight of the graphitized platelet carbon nanofibers and the silver nanoparticles, specifically 3 wt% to 30 wt%, more specifically 5 wt% to 20 wt%, for example 7 wt% to 10 wt%. When the above range is satisfied, the lithium ions transferred to the positive electrode active material layer can be effectively alloyed with the silver nanoparticles, so that the electrochemical characteristics of the all-solid-state lithium secondary battery can be improved. In addition, since a somewhat low content of silver nanoparticles is used, the energy density and price competitiveness of the all-solid-state lithium secondary battery can be improved.
[0047] In particular, the content of the silver nanoparticles can be 10% by weight or less, specifically 7% to 10% by weight, because the negative electrode active material layer contains the graphitized platelet carbon nanofibers. The lithium ions transferred from the positive electrode active material layer are alloyed with the silver nanoparticles having lithium affinity, and the lithium ions are absorbed and diffused to the negative electrode. In particular, the layered structure on the platelet carbon nanofibers described in the present invention can further accelerate the absorption and diffusion of the lithium ions. Therefore, the speed at which lithium metal is deposited and stored on the negative electrode active material layer and the negative electrode current collector can be improved. In addition, since the side of the graphitized platelet carbon nanofiber has a closed loop shape at a predetermined period, the silver nanoparticles can be effectively dispersed and arranged along the curved surface, and the aggregation of the silver nanoparticles can be effectively suppressed even during repeated charging and discharging of the battery. As a result, even with a small content of silver nanoparticles, the capacity and initial charge / discharge efficiency of the all-solid-state lithium secondary battery can be sufficiently improved.
[0048] In the negative electrode active material layer, the weight ratio of the graphitized platelet carbon nanofibers to the silver nanoparticles may be 99:1 to 60:40, specifically 97:3 to 70:30, more specifically 95:5 to 80:20, for example, 95:5 to 88:12. When this is satisfied, the capacity and initial charge / discharge efficiency of the all-solid-state lithium secondary battery can be more effectively improved.
[0049] The loading amount of the negative electrode active material layer is 0.1 mg / cm 2 ~2.0mg / cm 2 Specifically, it can be 0.3 mg / cm 2 ~1.8mg / cm 2 , more specifically 0.5 mg / cm 2 ~1.6mg / cm 2 When the above range is satisfied, the energy density is not hindered due to an increase in the thickness of the negative electrode, and the effects of improving the initial efficiency and lifespan of the battery can be maximized.
[0050] The thickness of the negative electrode active material layer may be 1 μm to 100 μm, specifically 1 μm to 50 μm, and more specifically 1 μm to 20 μm. When the thickness is within this range, the energy density is not hindered due to an increase in the thickness of the negative electrode, and the effect of improving the initial efficiency and life of the battery can be maximized.
[0051] 3) Negative electrode binder The negative electrode active material layer may further include a negative electrode binder, which may include at least one selected from the group consisting of polyvinylidene fluoride (PVdF), polyvinyl alcohol (PVA), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, polyvinylpyrrolidone, polytetrafluoroethylene (PTFE), polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), styrene-butadiene rubber (SBR), and fluororubber.
[0052] The negative electrode binder may be included in the negative electrode active material layer in an amount of 1 wt % to 20 wt %, specifically 1 wt % to 15 wt %, more specifically 1 wt % to 10 wt %. When the amount is within the above range, the resistance of the negative electrode can be maintained at a low level, the mechanical properties of the negative electrode can be improved, and the absorption and diffusion of lithium ions can be further promoted.
[0053] Depending on the case, the negative electrode active material layer may further include at least one of lithium ions, lithium, and an alloy of lithium and silver nanoparticles. Specifically, when the all-solid-state lithium secondary battery is in operation, at least one of lithium ions, lithium, and an alloy of lithium and silver nanoparticles may be present in the negative electrode active material layer due to lithium ions transferred from the positive electrode active material layer.
[0054] (2) Positive electrode active material layer The all-solid-state lithium secondary battery may include a positive electrode active material layer. Specifically, the all-solid-state lithium secondary battery may include a positive electrode, and the positive electrode may include or consist of a positive electrode active material layer.
[0055] The positive electrode may include a positive electrode current collector. The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the positive electrode or the battery and has high conductivity, and may include at least one selected from the group consisting of stainless steel, copper, aluminum, nickel, titanium, and calcined carbon, and may specifically include aluminum. The positive electrode current collector may further include a primer layer that includes a carbon-based conductive material and a binder and is coated on the surface of the positive electrode current collector. This can greatly improve the binding strength and electrical conductivity between the positive electrode active material layer and the current collector.
[0056] The positive electrode active material layer may be disposed on at least one surface of the positive electrode current collector. Specifically, the positive electrode active material layer may be disposed on one or both surfaces of the positive electrode current collector.
[0057] The positive electrode active material layer may include a positive electrode active material.
[0058] The positive electrode active material is a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; 1+x Mn 2-x Lithium manganese oxides, including LiMnO4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMn2O4, LiMnO2, etc.; lithium copper oxide (Li2CuO2); vanadium oxides, such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; and the chemical formula LiNi 1-x M x Lithium nickel oxide with Ni site represented by the chemical formula LiMnO2 (where M=Co, Mn, Al, Cu, Fe, P, Mg, Ca, Zr, Ti, Ru, Nb, W, B, Si, Na, K, Mo, V or Ga, and x=0.01 to 0.3); 1-x M x Lithium manganese composite oxide represented by Li2Mn3MO8 (wherein M=Co, Ni, Fe, Cr, Zn or Ta, and x=0.01 to 0.1) or Li2Mn3MO8 (wherein M=Fe, Co, Ni, Cu or Zn); LiNi x Mn 2-x Lithium manganese oxides with spinel structure represented by O4; LiMn2O4 in which part of the Li in the chemical formula is replaced by an alkaline earth metal ion; disulfide compounds; LiMn x Fe 1-x PO4(0≦x≦0.9); Fe2(MoO4)3, etc., but are not limited to these.
[0059] The positive electrode active material is Li 1+x M y O 2+zcan include, and M can be at least one element selected from the group consisting of Ni, Co, Mn, Fe, P, Al, Mg, Ca, Zr, Zn, Ti, Ru, Nb, W, B, Si, Na, K, Mo, and V, and 0 ≦ x ≦ 5, 0 < y ≦ 2, 0 ≦ z ≦ 2 can hold. Specifically, the said Li 1+x M y O 2+z can include at least one selected from the group consisting of LiCoO2, LiNiO2, LiMnO2, Li[Ni 0.5 C o0.3 Mn 0.2 O2, Li[Ni 0.6 Co 0.2 Mn 0.2 O2, Li[Ni 0.7 Co 0.1 Mn 0.2 O2, Li[Ni 0.8 Co 0.1 Mn 0.1 O2, Li[Ni 0.9 Co 0.05 Mn 0.05 O2, LiMn2O4, LiFePO 4、0.5 Li2MnO3·0.5Li[Mn 0.4 Ni 0.3 Co 0.3 O2. Preferably, the said Li 1+x M y O 2+z can include any one of the said Li[Ni 0.6 Co 0.2 Mn 0.2 O2, Li[Ni 0.7 Co 0.1 Mn 0.2 O2, Li[Ni 0.8 Co 0.1 Mn 0.1 O2, Li[Ni 0.9 Co 0.05 Mn 0.05 O2. Since the positive electrode active material includes Li 1+x M y O 2+z lithium can be sufficiently supplied to the negative electrode, and Li 1+x M y O 2+zdoes not cause a decrease in the overall performance of the battery and is electrochemically active after the first cycle, thus eliminating the loss of battery capacity due to the irreversible capacity of the negative electrode. 1+x M y O 2+z may be in the form of secondary particles formed by combining or granulating primary particles, or alternatively, may be in the form of a single particle.
[0060] The positive electrode active material may be contained in the positive electrode active material layer in an amount of 50% by weight to 95% by weight, specifically 60% by weight to 90% by weight.
[0061] The positive electrode active material layer may further include a solid electrolyte.
[0062] Specifically, the solid electrolyte can include at least one selected from the group consisting of polymer solid electrolytes, oxide-based solid electrolytes, sulfide-based solid electrolytes, and halide-based solid electrolytes.
[0063] The polymer solid electrolyte may be a composite of a lithium salt and a polymer resin. Specifically, the polymer solid electrolyte may be formed by adding a polymer resin to a solvated lithium salt. Specifically, the ionic conductivity of the polymer solid electrolyte is about 1×10 -7 S / cm or more, preferably about 1×10 -3 S / cm or more.
[0064] The polymer resin may include at least one of polyether polymers, polycarbonate polymers, acrylate polymers, polysiloxane polymers, phosphazene polymers, polyethylene derivatives, alkylene oxide derivatives such as polyethylene oxide, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymers containing ionic dissociation groups. The polymer solid electrolyte may include at least one of branched copolymers in which amorphous polymers such as PMMA, polycarbonate, polysiloxane (pdms) and / or phosphazene are copolymerized with a comonomer on a PEO (poly ethylene oxide) main chain, comb-like polymers, and crosslinked polymers.
[0065] The lithium salt is ionizable, Li + X - The anion of such a lithium salt is not particularly limited, but may be represented by F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3- , CF3CO2 - , CH3CO2 - , SCN - , (CF3CF2SO2)2N - The following can be exemplified:
[0066] The oxide-based solid electrolyte may contain oxygen (O) and have the ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table. Non-limiting examples of the oxide-based solid electrolyte include LLTO-based compounds, Li6La2CaTa2O 12 , Li6La2ANb2O 12 (A is Ca or Sr), Li2Nd3TeSbO 12 , LiBO 2.5 N 0.5 , Li9SiAlO8, LAGP compounds, LATP compounds, Li 1+x Ti 2-x Al x S y (PO4) 3-y (where 0≦x≦1, 0≦y≦1), LiAl x Zr 2-x (PO4)3 (where 0≦x≦1, 0≦y≦1), LiTi x Zr 2-x (PO4)3 (where 0≦x≦1, 0≦y≦1), LISICON-based compounds, LIPON-based compounds, Perovskite-based compounds, Nasicon-based compounds, and LLZO-based compounds may be included, but are not limited thereto.
[0067] The sulfide-based solid electrolyte contains sulfur (S) and has ion conductivity of a metal belonging to Group 1 or Group 2 of the periodic table, and may include Li-PS-based glass or Li-PS-based glass ceramic. Non-limiting examples of such sulfide-based solid electrolytes include Li6PS5Cl, Li6PS5Br, Li6PS5I, Li2S-P2S5, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2, Li2S-GeS2-ZnS, and the like, and may include one or more of these. However, it is not particularly limited to this.
[0068] The halide-based solid electrolyte may include at least one of Li3YCl6 and Li3YBr6, but is not limited thereto.
[0069] The solid electrolyte may be contained in the positive electrode active material layer in an amount of 5% by weight to 50% by weight, specifically 10% by weight to 30% by weight.
[0070] The positive electrode active material layer may further include a positive electrode conductive material.
[0071] The positive electrode conductive material is not particularly limited as long as it does not cause a chemical change in the positive electrode or the battery and has conductivity, and for example, the positive electrode conductive material may include one or a mixture of two or more conductive materials selected from graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; graphene; conductive fibers such as carbon nanofibers and carbon nanotubes; carbon fluoride; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives.
[0072] The positive electrode conductive material may be contained in the positive electrode active material layer in an amount of 1% by weight to 30% by weight.
[0073] The positive electrode active material layer may further include a positive electrode binder.
[0074] The positive electrode binder is not particularly limited as long as it is a component that is useful for binding the positive electrode active material, the conductive material, etc., and for binding to the current collector. Specifically, the positive electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride (PVdF), polyvinyl alcohol (PVA), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, polyvinylpyrrolidone, polytetrafluoroethylene (PTFE), polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), styrene-butadiene rubber (SBR), and fluororubber.
[0075] The positive electrode binder may be included in the positive electrode active material layer in an amount of 1% by weight to 30% by weight.
[0076] The positive electrode active material layer may contain one or more additives such as an oxidation stabilizing additive, a reduction stabilizing additive, a flame retardant, a heat stabilizer, and an antifogging agent, if necessary.
[0077] (3) Solid electrolyte layer The all-solid-state lithium secondary battery may include a solid electrolyte layer.
[0078] The solid electrolyte layer can act as an insulating layer and an ion-conducting channel in an all-solid-state lithium secondary battery.
[0079] Referring to FIG. 4, the solid electrolyte layer 300 may be disposed between the negative electrode active material layer 100 and the positive electrode active material layer 200 .
[0080] The solid electrolyte layer 300 includes the solid electrolyte. Specifically, the solid electrolyte may include at least one selected from the group consisting of a polymer solid electrolyte, an oxide-based solid electrolyte, and a sulfide-based solid electrolyte.
[0081] The polymer solid electrolyte may be a composite of a lithium salt and a polymer resin. Specifically, the polymer solid electrolyte may be formed by adding a polymer resin to a solvated lithium salt. Specifically, the ionic conductivity of the polymer solid electrolyte is about 1×10 -7 S / cm or more, preferably about 1×10 -3 S / cm or more.
[0082] The polymer resin may include at least one of polyether polymers, polycarbonate polymers, acrylate polymers, polysiloxane polymers, phosphazene polymers, polyethylene derivatives, alkylene oxide derivatives such as polyethylene oxide, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymers containing ionic dissociation groups. The polymer solid electrolyte may include at least one of branched copolymers in which amorphous polymers such as PMMA, polycarbonate, polysiloxane (pdms) and / or phosphazene are copolymerized with a comonomer on a PEO (poly ethylene oxide) main chain, comb-like polymers, and crosslinked polymers.
[0083] The lithium salt is ionizable, Li + X - The anion of such a lithium salt is not particularly limited, but may be represented by F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4- , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , (CF3CF2SO2)2N - The following can be exemplified:
[0084] The oxide-based solid electrolyte may contain oxygen (O) and have the ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table. Non-limiting examples of the oxide-based solid electrolyte include LLOP-based compounds, Li6La2CaTa2O 12 , Li6La2ANb2O 12 (A is Ca or Sr), Li2Nd3TeSbO 12 , LiBO 2.5 N 0.5 , Li9SiAlO8, LAGP compounds, LATP compounds, Li 1+x Ti 2-x Al x S y (PO4) 3-y (where 0≦x≦1, 0≦y≦1), LiAl x Zr 2-x (PO4)3 (where 0≦x≦1, 0≦y≦1), LiTi x Zr 2-x(PO4)3 (where 0≦x≦1, 0≦y≦1), LISICON-based compounds, LIPON-based compounds, Perovskite-based compounds, Nasicon-based compounds, and LLZO-based compounds may be included, but are not limited thereto.
[0085] The sulfide-based solid electrolyte contains sulfur (S) and has ion conductivity of a metal belonging to Group 1 or Group 2 of the periodic table, and may include Li-PS-based glass or Li-PS-based glass ceramic. Non-limiting examples of such sulfide-based solid electrolytes include Li6PS5Cl, Li6PS5Br, Li6PS5I, Li2S-P2S5, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2, Li2S-GeS2-ZnS, and the like, and may include one or more of these. However, it is not particularly limited to this.
[0086] The solid electrolyte layer may further include a binder for the solid electrolyte layer. The binder for the solid electrolyte layer may be introduced for bonding between solid electrolytes and between the solid electrolyte layer and battery elements (e.g., positive and negative electrodes) laminated on both sides of the solid electrolyte layer.
[0087] The material of the binder for the solid electrolyte layer is not particularly limited, and can be appropriately selected from the range of components used as binders for solid electrolytes in all-solid-state lithium secondary batteries. Specifically, the binder for the solid electrolyte layer can include at least one selected from the group consisting of polyvinylidene fluoride (PVdF), polyvinyl alcohol (PVA), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), styrene-butadiene rubber (SBR), styrene-butadiene styrene block copolymer (SBS), nitrile butadiene rubber (NBR), fluororubber, and acrylic binders.
[0088] The thickness of the solid electrolyte layer may be 10 μm to 90 μm, specifically 20 μm to 80 μm, taking into consideration ion conductivity, physical strength, energy density of the applied battery, etc. The tensile strength of the solid electrolyte layer may be 500 kgf / cm 2 ~2,000kgf / cm 2 The porosity of the solid electrolyte layer 300 may be 15% or less, or about 10% or less.
[0089] The all-solid-state lithium secondary battery may further include a metal layer. Referring to Fig. 5, the all-solid-state lithium secondary battery 10 may further include a negative electrode current collector 110, and may further include a metal layer 120 located between the negative electrode active material layer 100 and the negative electrode current collector 110 in a charged state. The metal layer 120 may include lithium, and may be made of lithium.
[0090] The metal layer may refer to a layer formed by storing lithium ions transferred from the positive electrode active material layer, via the negative electrode active material layer, on the negative electrode current collector and the negative electrode active material layer when the all-solid-state lithium secondary battery is charged. Therefore, the metal layer clearly appears during charging.
[0091] The metal layer is observed during the discharge process, but theoretically may not be observed during full discharge.
[0092] The present invention is significant in all-solid-state lithium secondary batteries, but may not be so significant in lithium secondary batteries using liquid electrolytes. For example, when a liquid electrolyte is used, the lithium stored in the negative electrode (for example, in the form of a metal layer) may continue to be exposed to the liquid electrolyte, making it difficult to completely store lithium in the negative electrode.
[0093] Manufacturing method for all-solid-state lithium secondary battery A method for manufacturing an all-solid-state lithium secondary battery according to another embodiment of the present invention may include a first step of reducing silver ions in a mixture of silver ions and graphitized platelet carbon nanofibers to form a dry mixed powder including the graphitized platelet carbon nanofibers and silver nanoparticles disposed on the graphitized platelet carbon nanofibers, and a second step of forming a negative electrode active material layer on a negative electrode current collector via a negative electrode slurry including the dry mixed powder. Here, the all-solid-state lithium secondary battery may be the same as the all-solid-state lithium secondary battery of the above-mentioned embodiment. Also, the negative electrode active material layer may be the same as the negative electrode active material layer of the above-mentioned embodiment.
[0094] (1) First step In the first step, a dry mixed powder is formed, which includes the graphitized platelet carbon nanofibers and silver nanoparticles disposed on the graphitized platelet carbon nanofibers. The dry mixed powder may be prepared by mixing powdered silver nanoparticles and powdered graphitized platelet carbon nanofibers. Alternatively, the dry mixed powder may be prepared by mixing the graphitized platelet carbon nanofibers in a silver ion solution and then reducing the silver nanoions. The silver nanoparticles can be reduced by a variety of methods, including chemical reduction, electrochemical reduction, photochemical reduction, laser reduction, ultrasonic reduction, and sputtering, and preferably by a chemical reduction method using a polyol process or a microwave-assisted polyol method using microwaves.
[0095] In the polyol process, the silver ion solution may contain a solvent and a stabilizer together with the silver ions. The solvent may be ethylene glycol, and the stabilizer may be polyvinylpyrrolidone, but is not limited thereto.
[0096] The molar concentration of silver ions in the silver ion solution may be 1 mM to 1,000 mM, specifically 1 mM to 500 mM, and more specifically 1 mM to 300 mM. When the molar concentration range is satisfied, the content and size of the formed silver nanoparticles can be adjusted to an appropriate level, and the capacity, initial charge / discharge efficiency, and life characteristics of the all-solid-state lithium secondary battery can be effectively adjusted.
[0097] In the first step, reducing the silver ions may include reacting the mixed solution at 100°C to 500°C, specifically, at 100°C to 300°C. That is, the reaction can be performed by heat treatment at the above-mentioned temperature. This allows the silver ions to be appropriately reduced, and silver nanoparticles having a suitable size can be obtained. In addition, in the process, the silver nanoparticles can be arranged on the surface of the graphitized platelet carbon nanofibers.
[0098] The reduction of the silver ions may include adjusting the pH of the mixed solution. Specifically, the mixed solution may be adjusted to have an acidity of pH 8 to pH 14, more specifically pH 9 to pH 13. This allows the silver ions to be appropriately reduced, and silver nanoparticles having a suitable size to be obtained.
[0099] Next, the solid content of the mixed solution can be washed and then dried to obtain the dry mixed powder.
[0100] In the dry mixed powder, the weight ratio of the graphitized platelet carbon nanofibers to the silver nanoparticles may be 99:1 to 60:40, specifically 97:3 to 70:30, more specifically 95:5 to 80:20. When this is satisfied, the capacity and initial charge / discharge efficiency of the all-solid-state lithium secondary battery can be more effectively improved.
[0101] (2) Second step In the second step, a negative electrode active material layer may be formed on a negative electrode current collector by a negative electrode slurry including the dry mixed powder. The negative electrode slurry may include a dry mixed powder and a solvent for the negative electrode slurry.
[0102] The solvent for the negative electrode slurry may be selected from the group consisting of water, N-methylpyrrolidone, etc., but is not necessarily limited thereto.
[0103] The negative electrode slurry may further include a negative electrode binder. The negative electrode binder may be the same as the negative electrode binder in the above embodiment.
[0104] In the second step, the negative electrode slurry may be coated on a negative electrode current collector and dried to form the negative electrode active material layer. If necessary, a pressing process may be performed together with the coating and drying processes.
[0105] The present invention also provides a battery module including the all-solid-state lithium secondary battery as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source. Specific examples of the device include, but are not limited to, a power tool operated by a battery-type motor, electric vehicles including electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), etc., electric two-wheeled vehicles including electric bicycles (E-bikes) and electric scooters (E-scooters), electric golf carts, urban air mobility (UAM), and power storage systems.
[0106] The present invention will be further described below with reference to examples. However, the following examples are intended to illustrate the present invention, and the scope of the present invention is not limited to these examples.
[0107] Examples and Comparative Examples Example 1: Manufacture of all-solid-state lithium secondary battery (1) Manufacturing of negative electrodes The platelet carbon nanofibers were heat-treated in an Ar atmosphere at a temperature of 2800°C for 6 hours to produce graphitized platelet carbon nanofibers.
[0108] Graphitized platelet carbon nanofibers, AgNO3, and polyvinylpyrrolidone were mixed in an ethylene glycol solvent, and the pH was adjusted to a range of 8 to 14 using NaOH pellets, and then the mixture was stirred for 24 hours to produce a mixed solution. The mixed solution was subjected to Ar bubbling using an ultrasonic device, and was repeatedly heated and cooled using a microwave reactor (LG Electronics) in Continuous Wave Mode (2.45 GHz, 500 W) for 10 seconds, 20 seconds, 30 seconds, 1 minute, 2 minutes, and 5 minutes. As a result, silver ions were reduced, and silver nanoparticles were arranged on the graphitized platelet carbon nanofibers. Next, the mixture was filtered and washed with an acetone solution, and dried in a vacuum oven at 100 °C for 24 hours to obtain a dry mixed powder containing graphitized platelet carbon nanofibers and silver nanoparticles arranged on the graphitized platelet carbon nanofibers (see FIG. 8). The content of the silver nanoparticles (based on the total weight of the graphitized platelet carbon nanofibers and the silver nanoparticles) was 10 wt %, and the average particle size of the silver nanoparticles was 2 nm.
[0109] The dry mixed powder and polyvinylidene fluoride were added to a solvent, N-methylpyrrolidone (NMP), and stirred to form a negative electrode slurry, in which the weight ratio of the dry mixed powder to the polyvinylidene fluoride was 93:7.
[0110] The negative electrode slurry was applied to a stainless steel current collector (thickness: 15 μm), dried in a vacuum oven at 100° C. for 12 hours, and then rolled using a roll press to manufacture a negative electrode including a stainless steel current collector and a negative electrode active material layer positioned on the stainless steel current collector. The negative electrode active material layer had a thickness of 10 μm and a loading amount of 1 mg / cm. 2 It was.
[0111] (2) Manufacturing of positive electrodes As a positive electrode active material, Li[Ni 0.82 Co0.14 Mn 0.04 ]O2, Li6PS6Cl as a solid electrolyte, carbon nanofiber (VGCF, Showa Denko) as a conductive material, and polytetrafluoroethylene as a binder were sequentially added to the container in a weight ratio of 77:20:1:2. After each addition, the mixture was mixed 10 times at 10,000 RPM for 30 seconds using a Lab Blender to prepare a positive electrode mixture. The mixture was subjected to high shear mixing for 5 minutes at 100 rpm at 100 °C using a Twin Screw Kneader (LG Electronics) to apply shear force. The positive electrode mixture was then processed into a free-standing film having a thickness of 200 μm using a Two Roll Mill (Inoue) at 100 °C. Next, the film was placed on one side of a primer-coated aluminum current collector (thickness: 20 μm), and the film was bonded to the current collector using a lamination roll maintained at 120° C. to prepare a positive electrode.
[0112] (3) Manufacturing of all-solid-state lithium secondary batteries The solid electrolyte Li6PS6Cl and nitrile butadiene rubber (NBR) were mixed in the xylene solvent, and then mixed with a zirconia ball in a Thinky Mixer at 2,000 RPM for 10 times for 1 minute each to produce a solid electrolyte slurry. This was coated on a PET film release paper and dried in a vacuum oven at 45°C for 6 hours to prepare a solid electrolyte layer. Here, the weight ratio of the solid electrolyte Li6PS6Cl and nitrile butadiene rubber (NBR) was 95:5 by weight, and the thickness of the solid electrolyte layer produced was 100μm.
[0113] The solid electrolyte layer was disposed between the negative electrode and the positive electrode to prepare an assembly, and the assembly was then sealed in a pouch. The pouch was then fixed onto an Al plate and subjected to a pressure treatment at 500 MPa for 30 minutes in a warm isostatic pressure device to prepare the all-solid-state lithium secondary battery of Example 1.
[0114] Examples 2 to 5: Production of all-solid-state lithium secondary batteries An all-solid-state lithium secondary battery was manufactured in the same manner as in Example 1, except that the silver nanoparticle content and average particle size were adjusted as shown in Tables 1 and 2 by controlling the weight ratio of graphitized platelet carbon nanofiber, AgNO3, and polyvinylidene pyrrolidone, pH value, reaction conditions in a microwave reactor, etc.
[0115] Comparative Examples 1-2: Production of all-solid-state lithium secondary batteries (1) Manufacturing of negative electrodes An all-solid-state lithium secondary battery was manufactured in the same manner as in Example 1, except that carbon black (PRINTEX, manufactured by Orion Engineered Carbons) was used instead of the graphitized platelet carbon nanofiber in Example 1, and the weight ratio of carbon black, AgNO3, and polyvinylidene pyrrolidone, pH value, reaction conditions in a microwave reactor, etc. were controlled to adjust the content and average particle size of silver nanoparticles as shown in Tables 1 and 2.
[0116] Comparative Example 3: Manufacture of lithium secondary battery (1) Manufacturing of negative and positive electrodes A negative electrode and a positive electrode were produced in the same manner as in Example 1.
[0117] (3) Manufacture of lithium secondary batteries Next, a monocell was prepared by disposing a 15 μm-thick polyethylene separator between the prepared negative and positive electrodes, and then an electrolyte (ethylene carbonate (EC) / ethyl methyl carbonate (EMC)=1 / 2 (volume ratio), lithium hexafluorophosphate (LiPF61 mol)) was injected into the monocell to prepare a lithium secondary battery.
[0118] Comparative Example 4: Manufacture of lithium secondary battery A lithium secondary battery was manufactured in the same manner as in Comparative Example 3, except that the weight ratio of graphitized platelet carbon nanofiber, AgNO3, and polyvinylidene pyrrolidone, pH value, reaction conditions in a microwave reactor, etc. were controlled to adjust the content and average particle size of silver nanoparticles as shown in Table 1.
[0119] Comparative Example 5: Manufacture of Lithium Secondary Battery Except for using non-graphitized platelet carbon nanofibers instead of graphitized platelet carbon nanofibers, an all-solid-state lithium secondary battery was manufactured in the same manner as in Example 1. Figure 9 is a TEM image of the dry mixed powder containing silver nanoparticles arranged on the platelet carbon nanofibers.
[0120] Meanwhile, the fabricated negative electrodes were observed, and the graphitized platelet carbon nanofibers of Examples 1 to 5 and Comparative Examples 3 and 4 had d(002) of 0.335 nm and Lc(002) of 41 nm. The XRD analysis of the graphitized platelet carbon nanofibers was performed using a Bruker AXS D4 Endeavor XRD (voltage: 40 kV, current: 40 mA). Under the condition of Cu Kα radiation (wavelength: 1.54 Å), measurements were performed at a scanning speed of 87.5 seconds per 0.02° from 2θ (Theta) 10° to 90°. Among the measurement results, the full width at half-maximum (FWHM) of the (002) crystal peak appearing at 2θ in the vicinity of 20° to 30° was measured, and the d(002) value and Lc(002) value were calculated according to the Scherrer formula. The I D / I G The ratio was 0.24. D / I G The ratio was measured from a wavelength-peak graph during Raman spectrum measurement.
[0121] The platelet carbon nanofibers were also evaluated in the same manner.
[0122] [Table 1]
[0123] The platelet carbon nanofibers and the graphitized platelet carbon nanofibers had an average length of 1 μm and an average diameter of 200 nm. The average diameter corresponds to the average value of the diameters of the top 50 graphitized platelet carbon nanofibers and the bottom 50 graphitized platelet carbon nanofibers (or platelet carbon nanofibers) in descending order of average diameter when the negative electrode active material layer is observed by SEM at a magnification of ×20,000. The average length corresponds to the average value of the lengths of the top 50 graphitized platelet carbon nanofibers (or platelet carbon nanofibers) and the bottom 50 graphitized platelet carbon nanofibers (or platelet carbon nanofibers) in descending order of average length when the negative electrode active material layer is observed by SEM at a magnification of ×20,000.
[0124] Experimental example 1: Evaluation of initial charge / discharge efficiency Each of the batteries of the examples and comparative examples was mounted on a pressure jig, and the bolts / nuts located at the four corners were tightened with the same pressure of 1 N m to prepare a monocell. The batteries were charged and discharged once at 60°C under the following conditions, and the initial charge / discharge efficiency was evaluated as the ratio of the first discharge capacity to the first charge capacity (see Table 2).
[0125] Charging conditions: 0.1C CC charging up to 4.25V, then CV charging with 4.25V 0.05C cut-off Discharge conditions: 0.1C CC discharge to 3.0V
[0126] Experimental Example 2: Evaluation of Capacity Retention Rate The batteries of the examples and comparative examples were each charged and discharged at 60° C. under the following conditions, and then the capacity retention rate (%) after 50 cycles was evaluated. The discharge capacity at the first charge / discharge was set as 100%.
[0127] Charging conditions: 0.5C CC charging up to 4.25V, 0.5C cut-off Discharge conditions: 0.33C CC discharge to 3.0V
[0128] [Table 2]
[0129] The average particle size of the silver nanoparticles corresponds to the average value of the particle sizes of the top 50 silver nanoparticles and the bottom 50 silver nanoparticles when the graphitized platelet carbon nanofibers containing the silver nanoparticles in the negative electrode active material layer are observed by TEM at a magnification of ×1,000,000. The GPCNF is a graphitized platelet carbon nanofiber, the PCNF is a non-graphitized platelet carbon nanofiber, and the CB is carbon black.
[0130] The content of the silver nanoparticles refers to the content based on the total weight of the platelet carbon nanofibers and the silver nanoparticles in the negative electrode active material layer.
Claims
1. a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer; the negative electrode active material layer comprises graphitized platelet carbon nanofibers and silver nanoparticles.
2. The graphitized platelet carbon nanofiber has a structure in which a plurality of graphene sheets are stacked in the growth direction of the graphitized platelet carbon nanofiber, the graphitized platelet carbon nanofiber includes a bend protruding toward a side of the graphitized platelet carbon nanofiber; The all-solid-state lithium secondary battery according to claim 1 , wherein the bent portion corresponds to a basal surface of the graphene sheet.
3. 2. The all-solid-state lithium secondary battery of claim 1, wherein the silver nanoparticles are disposed on a surface of the graphitized platelet carbon nanofibers.
4. When performing XRD measurement on the graphitized platelet carbon nanofibers, 2. The all-solid-state lithium secondary battery of claim 1, wherein the graphitized platelet carbon nanofibers have a d(002) of 0.330 nm to 0.350 nm.
5. When performing XRD measurement on the graphitized platelet carbon nanofibers, 2. The all-solid-state lithium secondary battery of claim 1, wherein the Lc(002) of the graphitized platelet carbon nanofiber is 20 nm to 200 nm.
6. I of the graphitized platelet carbon nanofibers D / I G The all-solid-state lithium secondary battery according to claim 1, wherein is 0.1 to 1.
0.
7. 2. The all-solid-state lithium secondary battery of claim 1, wherein the graphitized platelet carbon nanofibers have an average diameter of 10 nm to 500 nm.
8. 2. The all-solid-state lithium secondary battery of claim 1, wherein the graphitized platelet carbon nanofibers have an average length of 0.1 μm to 5 μm.
9. The specific surface area of the graphitized platelet carbon nanofiber is 5 m 2 / g to 100m 2 The all-solid-state lithium secondary battery according to claim 1, wherein the total mass of the lithium ion exchange layer is 1000 vol. / g.
10. 2. The all-solid-state lithium secondary battery according to claim 1, wherein the graphitized platelet carbon nanofibers are contained in the negative electrode active material layer at 50% by weight to 98% by weight.
11. 2. The all-solid-state lithium secondary battery according to claim 1, wherein the average particle size of the silver nanoparticles is 1 nm to 100 nm.
12. In the negative electrode active material layer, 2. The all-solid-state lithium secondary battery according to claim 1, wherein the silver nanoparticles are contained in an amount of 1% by weight to 40% by weight based on the total weight of the graphitized platelet carbon nanofibers and the silver nanoparticles.
13. 2. The all-solid-state lithium secondary battery of claim 1, wherein the weight ratio of the graphitized platelet carbon nanofibers to the silver nanoparticles is 99:1 to 60:
40.
14. The all-solid-state lithium secondary battery according to claim 1 , wherein the negative electrode active material layer further comprises a negative electrode binder.
15. 2. The all-solid-state lithium secondary battery according to claim 1, wherein the negative electrode active material layer has a thickness of 1 μm to 100 μm.
16. Further comprising a negative electrode current collector, The negative electrode further includes a metal layer located between the negative electrode active material layer and the negative electrode current collector in a charged state, The all-solid-state lithium secondary battery according to claim 1 , wherein the metal layer contains lithium.
17. a first step of reducing silver ions in a mixture of silver ions and graphitized platelet carbon nanofibers to form a dry mixed powder comprising the graphitized platelet carbon nanofibers and silver nanoparticles disposed on the graphitized platelet carbon nanofibers; and a second step of forming a negative electrode active material layer on a negative electrode current collector via the negative electrode mixture containing the dry mixed powder.
Citation Information
Patent Citations
Negative electrode material, negative electrode using the same, and lithium ion battery and lithium polymer battery using the negative electrode
JP2009059713A
Polymer electrolyte, secondary battery, and method of manufacturing secondary battery
JP2011181463A
Composite carbon fiber
JP2014177722A
Negative electrode active material for lithium ion secondary battery
JP2019021503A
Non-aqueous electrolyte for battery and lithium secondary battery
JP2021048006A