Semiconductor element forming method and substrate processing apparatus
By forming a coating layer and selectively etching recesses in semiconductor substrates, the method addresses uneven etching in high-aspect-ratio features, ensuring consistent diameters and uniform electrical characteristics of memory elements.
Patent Information
- Application Number
- JP2020213627
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-23
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-12-23
AI Technical Summary
The challenge in semiconductor manufacturing is the variation in electrical characteristics of memory elements due to uneven etching in recesses with high aspect ratios, such as memory holes and trenches, leading to inconsistent diameters throughout the recess, which is exacerbated by the difficulty of etching solutions reaching the lower parts effectively.
A method involving the formation of a coating layer that selectively covers the surface side of recesses, followed by etching the deep part with a chemical solution to widen the diameter, using a filling layer, partially removing it with a removal liquid, and applying a water repellent to adjust the recess diameter uniformly.
This approach ensures consistent diameters of recesses across their depth, maintaining uniform electrical characteristics of memory elements and enhancing manufacturing precision.
Smart Images

Figure 0007578483000001 
Figure 0007578483000002 
Figure 0007578483000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a semiconductor device forming method and a substrate processing apparatus. [Background technology]
[0002] Substrate processing apparatuses for processing substrates are used, for example, in the formation of semiconductor elements. In recent years, in order to manufacture fine memory elements of semiconductor elements, the memory elements have been formed by stacking them on a semiconductor substrate (see Patent Document 1). In the semiconductor memory element of Patent Document 1, holes with a large aspect ratio, so-called memory holes, are formed in the stacked structure of the semiconductor substrate in the direction perpendicular to the base material. A large number of memory elements are arranged in the holes. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-117894 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the semiconductor memory element of Patent Document 1, the diameter of the lower part of the memory hole is smaller than the diameter of the upper part of the memory hole. This is because the etching solution is less likely to reach the lower part of the memory hole than the upper part of the memory hole. In this case, there is a risk of variation in the electrical characteristics of the memory element formed in the memory hole. The aspect ratio of the memory hole (the ratio of the height to the width of the memory hole) is increasing year by year, and in recent years, there are memory holes with an aspect ratio of more than 50. In memory holes with such a high aspect ratio, it is not easy to align the diameter of the upper part of the memory hole with the diameter of the lower part of the memory hole.
[0005] In addition, with the recent trend toward miniaturization of elements or three-dimensionalization of element structures, similar problems occur not only in the memory holes described above, but also in recesses such as holes or trenches with large aspect ratios. That is, the etching solution does not penetrate as easily below the recess compared to above it, and liquid replacement does not progress easily, so the lower part of the recess is etched differently from the upper part of the recess. Thus, in recesses such as holes and trenches with a relatively large aspect ratio (hereinafter referred to as recesses), the diameter of the recess may not be constant within the recess.
[0006] The present invention has been made in consideration of the above-mentioned problems, and its object is to provide a semiconductor element forming method and a substrate processing apparatus that are capable of adjusting the diameter of a recess provided in a layered structure of a substrate by selectively etching the recess. [Means for solving the problem]
[0007] According to one aspect of the present invention, a method for forming a semiconductor device includes the steps of forming a covering layer that selectively covers a portion of a recess provided in a laminate structure supported by a substrate, the portion being located on a surface side, and etching the deep portion of the recess with a chemical solution so as to increase the diameter of the portion of the recess deeper than the covering layer. The step of forming the covering layer includes the steps of forming a filling layer that fills the recess, and, after forming the filling layer, heating the filling layer while in contact with an aqueous solution to partially remove the portion of the filling layer located on the surface side, thereby forming a partial filling layer that partially fills the deep portion of the recess. a step of supplying a water repellent agent after forming the partial filling layer; and a step of supplying the water repellent agent, forming the coating layer on the recess surface side, and then removing the partial filling layer and the water repellent agent. Includes.
[0009] In one embodiment, removing the partial filling layer includes supplying a removal liquid to dissolve the partial filling layer.
[0010] In one embodiment, the step of partially removing the filling layer includes the step of supplying a removal liquid that removes the filling layer.
[0011] In one embodiment, in the etching step, the chemical solution contains any one of hydrofluoric acid, water, and phosphoric acid.
[0012] In one embodiment, a plurality of storage elements are formed in the recess.
[0013] In one embodiment, the laminate structure includes the recess. As multiple The recess The recess Every The difference in top diameter is less than 5%.
[0014] In one embodiment, the Multiple Recess is In the laminate structure rules Targeted There are.
[0015] In one embodiment, an etch stop layer is disposed between the substrate and the layered structure.
[0016] In one embodiment, in the step of forming the partially filled layer, an acidic aqueous solution is supplied as the aqueous solution.
[0017] According to another aspect of the present invention, a substrate processing apparatus includes a processing liquid supply unit, a water repellent supply unit, a chemical liquid supply unit, an aqueous solution supply unit, a heating mechanism, and a control unit. The processing liquid supply unit supplies a processing liquid. The water repellent supply unit supplies a water repellent. The chemical liquid supply unit supplies the chemical liquid. The aqueous solution supply unit supplies an aqueous solution. The heating mechanism heats a filling layer formed from the processing liquid. The control unit controls the processing liquid supply unit, the water repellent supply unit, the chemical liquid supply unit, the aqueous solution supply unit, and the heating mechanism. The control unit controls the processing liquid supply unit, the water repellent supply unit, the chemical liquid supply unit, the aqueous solution supply unit, and the heating mechanism so as to (1) supply the processing liquid to form a filling layer that fills a recess provided in a laminated structure supported by a substrate, (2) after forming the filling layer, heat the filling layer with the heating mechanism while the filling layer is in contact with the aqueous solution supplied from the aqueous solution supply unit, thereby partially removing a portion of the filling layer located on the surface side and forming a partial filling layer that partially fills a deeper portion of the recess, (3) supply the water repellent to form a coating layer that selectively covers a portion of the recess located on the surface side that is not covered by the partial filling layer, and (4) supply the chemical liquid to expand the diameter of a portion of the recess deeper than the coating layer.
[0018] In one embodiment, the heating mechanism heats the packed bed with heat or light.
[0019] In one embodiment, the heating mechanism includes a heater.
[0020] In one embodiment, the heating mechanism includes a lamp.
[0021] In one embodiment, the heating mechanism includes a heat medium supplying unit that supplies a heat medium, and the heat medium includes heated nitrogen gas.
[0022] In one embodiment, the aqueous solution supply unit supplies an acidic aqueous solution as the aqueous solution. Effect of the Invention
[0023] According to the present invention, the diameter of the recess provided in the laminated structure of the substrate can be adjusted. [Brief description of the drawings]
[0024] [Figure 1] 1 is a schematic diagram of a substrate processing apparatus according to an embodiment of the present invention; [Diagram 2] 1 is a schematic diagram of a substrate processing apparatus according to an embodiment of the present invention; [Diagram 3] 1 is a block diagram of a substrate processing apparatus according to an embodiment of the present invention; [Figure 4] 1A is a schematic side view of a semiconductor element manufactured using the substrate processing apparatus of this embodiment, FIG. 1B is a schematic top view of the semiconductor element, and FIG. 1C is an enlarged view of a portion of FIG. [Diagram 5] 1(a) to 1(e) are schematic views for explaining the semiconductor element forming method of the present embodiment. [Figure 6] 1(a) to 1(g) are schematic views for explaining the semiconductor element forming method of the present embodiment. [Figure 7] FIG. 2 is a flow diagram of a semiconductor device forming method according to the present embodiment. [Figure 8] FIG. 2 is a flow diagram of a semiconductor device forming method according to the present embodiment. [Figure 9] 1 is a schematic diagram of a substrate processing apparatus according to an embodiment of the present invention; [Figure 10] FIG. 2 is a flow diagram of a semiconductor device forming method according to the present embodiment. [Figure 11] 1 is a schematic diagram of a substrate processing apparatus according to an embodiment of the present invention; [Figure 12] FIG. 2 is a flow diagram of a semiconductor device forming method according to the present embodiment. [Figure 13] 1 is a schematic diagram of a substrate processing apparatus according to an embodiment of the present invention; [Figure 14] FIG. 2 is a flow diagram of a semiconductor device forming method according to the present embodiment. [Figure 15] 1 is a schematic diagram of a substrate processing apparatus according to an embodiment of the present invention; [Figure 16] FIG. 2 is a flow diagram of a semiconductor device forming method according to the present embodiment. [Figure 17]1 is a schematic diagram of a substrate processing apparatus according to an embodiment of the present invention; [Figure 18] FIG. 2 is a flow diagram of a semiconductor device forming method according to the present embodiment. [Figure 19] 1 is a schematic diagram of a substrate processing apparatus according to an embodiment of the present invention; [Figure 20] 1 is a schematic diagram of a semiconductor element formed by the semiconductor element forming method of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Hereinafter, an embodiment of a semiconductor device forming method and a substrate processing apparatus according to the present invention will be described with reference to the drawings. In the drawings, the same or corresponding parts are denoted by the same reference numerals and will not be described repeatedly. In this specification, mutually orthogonal X-axis, Y-axis, and Z-axis may be described in order to facilitate understanding of the invention. Typically, the X-axis and Y-axis are parallel to the horizontal direction, and the Z-axis is parallel to the vertical direction. In addition, in this specification, mutually orthogonal x-axis, y-axis, and z-axis may be described in order to facilitate understanding of the invention. Typically, the x-axis and y-axis extend parallel to the main surface of the substrate or base material, and the z-axis extends in a direction perpendicular to the main surface of the substrate or base material.
[0026] First, an embodiment of a substrate processing apparatus 100 according to the present invention will be described with reference to Fig. 1. Fig. 1 is a schematic plan view of the substrate processing apparatus 100 of the present embodiment.
[0027] The substrate processing apparatus 100 processes a substrate W. The substrate processing apparatus 100 processes the substrate W by performing at least one of etching, surface treatment, property imparting, treatment film formation, removal of at least a portion of a film, and cleaning on the substrate W.
[0028] The substrate W is used as a semiconductor substrate. The substrate W includes a semiconductor wafer. For example, the substrate W has a substantially circular disk shape. Here, the substrate processing apparatus 100 processes the substrates W one by one.
[0029] 1, the substrate processing apparatus 100 includes a plurality of chambers 110, a fluid cabinet 100A, a fluid box 100B, a plurality of load ports LP, an indexer robot IR, a center robot CR, and a controller 101. The controller 101 controls the load ports LP, the indexer robot IR, and the center robot CR. The controller 101 includes a control unit 102 and a memory unit 104.
[0030] Each of the load ports LP accommodates a plurality of stacked substrates W. The indexer robot IR transports the substrates W between the load port LP and the center robot CR. The center robot CR transports the substrates W between the indexer robot IR and the chambers 110. Each of the chambers 110 discharges liquid onto the substrate W to process the substrate W. The liquid includes a processing liquid, a removing liquid, a water repellent agent and / or a chemical liquid. The fluid cabinet 100A accommodates a liquid. The fluid cabinet 100A may also accommodate a gas.
[0031] Specifically, the multiple chambers 110 form multiple towers TW (four towers TW in FIG. 1) arranged to surround the center robot CR in a plan view. Each tower TW includes multiple chambers 110 (three chambers 110 in FIG. 1) stacked vertically. Each fluid box 100B corresponds to a multiple tower TW. The liquid in the fluid cabinet 100A is supplied to all the chambers 110 included in the tower TW corresponding to the fluid box 100B via any of the fluid boxes 100B. Also, the gas in the fluid cabinet 100A is supplied to all the chambers 110 included in the tower TW corresponding to the fluid box 100B via any of the fluid boxes 100B.
[0032] The control device 101 controls various operations of the substrate processing apparatus 100 .
[0033] The control device 101 includes a control unit 102 and a storage unit 104. The control unit 102 has a processor. The control unit 102 has, for example, a central processing unit (CPU). Alternatively, the control unit 102 may have a general-purpose computer.
[0034] The storage unit 104 stores data and computer programs. The data includes recipe data. The recipe data includes information indicating a plurality of recipes. Each of the plurality of recipes defines the processing content and processing procedure for the substrate W.
[0035] The storage unit 104 includes a main storage device and an auxiliary storage device. The main storage device is, for example, a semiconductor memory. The auxiliary storage device is, for example, a semiconductor memory and / or a hard disk drive. The storage unit 104 may include a removable medium. The control unit 102 executes a computer program stored in the storage unit 104 to perform a substrate processing operation.
[0036] Next, the substrate processing apparatus 100 of this embodiment will be described with reference to Fig. 2. Fig. 2 is a schematic diagram of the substrate processing apparatus 100.
[0037] The substrate processing apparatus 100 includes a chamber 110, a substrate holding unit 120, and a liquid supply unit 130. The chamber 110 accommodates a substrate W. The substrate holding unit 120 holds the substrate W.
[0038] The chamber 110 is substantially box-shaped with an internal space. The chamber 110 accommodates the substrate W. Here, the substrate processing apparatus 100 is a single-wafer type that processes the substrates W one by one, and the chamber 110 accommodates the substrates W one by one. The substrate W is accommodated in the chamber 110 and is processed in the chamber 110. The chamber 110 accommodates at least a part of each of the substrate holder 120 and the liquid supply unit 130.
[0039] The substrate holding part 120 holds the substrate W. The substrate holding part 120 holds the substrate W horizontally so that the top surface (front surface) Wa of the substrate W faces upward and the back surface (bottom surface) Wb of the substrate W faces vertically downward. The substrate holding part 120 also rotates the substrate W while holding it. The top surface Wa of the substrate W is provided with a layered structure in which a recess is formed, as will be described in detail later. The substrate holding part 120 rotates the substrate W while holding it.
[0040] For example, the substrate holding unit 120 may be of a clamping type that clamps an end of the substrate W. Alternatively, the substrate holding unit 120 may have any mechanism that holds the substrate W from the back surface Wb. For example, the substrate holding unit 120 may be of a vacuum type. In this case, the substrate holding unit 120 holds the substrate W horizontally by adsorbing the central portion of the back surface Wb of the substrate W, which is the non-device formation surface, to the upper surface. Alternatively, the substrate holding unit 120 may combine a clamping type that brings multiple chuck pins into contact with the peripheral edge surface of the substrate W with a vacuum type.
[0041] For example, the substrate holding unit 120 includes a spin base 121, a chuck member 122, a shaft 123, an electric motor 124, and a housing 125. The chuck member 122 is provided on the spin base 121. The chuck member 122 chucks the substrate W. Typically, the spin base 121 is provided with a plurality of chuck members 122.
[0042] The shaft 123 is a hollow shaft. The shaft 123 extends vertically along the rotation axis Ax. The spin base 121 is coupled to the upper end of the shaft 123. The substrate W is placed above the spin base 121.
[0043] The spin base 121 is disk-shaped and horizontally supports the substrate W. The shaft 123 extends downward from the center of the spin base 121. The electric motor 124 applies a rotational force to the shaft 123. The electric motor 124 rotates the shaft 123 in a rotational direction, thereby rotating the substrate W and the spin base 121 about the rotation axis Ax. The housing 125 surrounds the shaft 123 and the electric motor 124.
[0044] The liquid supply unit 130 supplies liquid to the substrate W. Typically, the liquid supply unit 130 supplies liquid to the upper surface Wa of the substrate W.
[0045] The liquid supply unit 130 includes a processing liquid supply unit 132, a removal liquid supply unit 134, a water repellent agent supply unit 136, and a chemical liquid supply unit 138. At least a portion of the processing liquid supply unit 132, the removal liquid supply unit 134, the water repellent agent supply unit 136, and the chemical liquid supply unit 138 are accommodated within the chamber 110.
[0046] The processing liquid supply unit 132 supplies a processing liquid to the upper surface Wa of the substrate W. For example, the processing liquid contains a solute and a volatile solvent. After the processing liquid is supplied to the upper surface Wa of the substrate W, the solvent evaporates, forming a filling layer from the solute. The filling layer is a solid film made of a solute component. The filling layer can hold particles remaining in the recesses of the substrate W. When the filling layer is formed, particles adhering to the upper surface Wa of the substrate W are detached from the substrate W and held in the filling layer.
[0047] Here, "solidification" refers to the solidification of a solute due to forces acting between molecules or atoms, for example, as a result of the evaporation of a solvent. "Hardening" refers to the solidification of a solute due to chemical changes, such as polymerization or crosslinking. Therefore, "solidification or hardening" refers to the "solidification" of a solute due to various factors. Note that the treatment liquid only needs to be solidified or hardened to an extent that it can hold particles, and the solvent does not need to be completely volatilized. In addition, the "solute component" that forms the filling layer may be the solute itself contained in the treatment liquid, or may be something derived from the solute, for example, something obtained as a result of a chemical change.
[0048] As the solute, various resins can be used which are soluble in any solvent and which, when solidified or cured, can form a filling layer in a state in which particles adhering to the upper surface of the substrate W are separated from the substrate W and held thereon. For example, as the solute, a resin (hereinafter sometimes referred to as a "heat-sensitive water-soluble resin") which is poorly soluble or insoluble in water before being heated to a predetermined alteration temperature or higher, and which is altered to become water-soluble when heated to the alteration temperature or higher, may be used.
[0049] The heat-sensitive water-soluble resin may be, for example, a resin that is decomposed by heating to a predetermined alteration temperature or higher (for example, 200° C. or higher) to expose a polar functional group and become water-soluble. When heated to the alteration temperature or higher, the heat-sensitive water-soluble resin becomes water-soluble.
[0050] However, the temperature of the heat-sensitive water-soluble resin may be kept below the alteration temperature to form the filling layer while maintaining its poor solubility or insolubility in the aqueous liquid. When forming the filling layer, the temperature of the processing liquid is set below the alteration temperature of the heat-sensitive water-soluble resin, so that a filling layer that is poorly soluble or insoluble in the aqueous liquid is formed on the upper surface of the substrate W without altering the heat-sensitive water-soluble resin to be water-soluble. In this case, the filling layer that maintains its clump state can be removed from the substrate W without causing particles to fall off from the filling layer. Therefore, particles can be removed at a high removal rate.
[0051] In addition to the heat-sensitive water-soluble resin, the solute contained in the treatment liquid may be, for example, an acrylic resin, a phenolic resin, an epoxy resin, a melamine resin, a urea resin, an unsaturated polyester resin, an alkyd resin, a polyurethane, a polyimide, a polyethylene, a polypropylene, a polyvinyl chloride, a polystyrene, a polyvinyl acetate, a polytetrafluoroethylene, an acrylonitrile butadiene styrene resin, an acrylonitrile styrene resin, a polyamide, a polyacetal, a polycarbonate, a polyvinyl alcohol, a modified polyphenylene ether, a polybutylene terephthalate, a polyethylene terephthalate, a polyphenylene sulfide, a polysulfone, a polyether ether ketone, a polyamide imide, or the like.
[0052] The solvent preferably has a higher volatility than water. As the solvent, PGEE (propylene glycol monoethyl ether) is preferably used.
[0053] The treatment liquid may also contain a sublimable substance. As the sublimable substance, various substances that have a high vapor pressure at 5°C to 35°C and change from a solid phase to a gas phase without passing through a liquid phase are used. As the sublimable substance, for example, hexamethylenetetramine, 1,3,5-trioxane, 1-pyrrolidinecarbodithioic acid ammonium, metaldehyde, paraffin having about 20 to 48 carbon atoms, t-butanol, paradichlorobenzene, naphthalene, L-menthol, fluorohydrocarbon compounds, etc. can be used. In particular, as the sublimable substance, fluorohydrocarbon compounds can be used.
[0054] As the fluorohydrocarbon compound, for example, one or more of the following compounds (A) to (E) can be used. Compound (A): Fluoroalkane having 3 to 6 carbon atoms or a derivative thereof Compound (B): Fluorocycloalkane having 3 to 6 carbon atoms, or a derivative thereof Compound (C): fluorobicycloalkane having 10 carbon atoms or a derivative thereof Compound (D): Fluorotetracyanoquinodimethane or its derivative Compound (E): Fluorocyclotriphosphazene or its derivative
[0055] The compound (A) may be a fluoroalkane having 3 to 6 carbon atoms represented by the formula (1) or a derivative thereof. C m H n F2 m+2-n (1) (In the formula, m is a number from 3 to 6, and n is a number in the range of 0≦n≦2m+1.)
[0056] It is particularly preferable to use 1,1,2,2,3,3,4-heptafluorocyclopentane as the sublimable substance. This compound has a vapor pressure of about 8266 Pa at 20°C, a melting point (freezing point) of 20.5°C, and a boiling point of 82.5°C. When mixing a sublimable substance in a molten state, a solvent that is compatible with the sublimable substance in a molten state is preferable. When dissolving a sublimable substance as a solute, a solvent that is soluble in the sublimable substance is preferable.
[0057] In addition, when a sublimable substance in a molten state is mixed, the solvent is preferably a solvent that is compatible with the sublimable substance in a molten state. In addition, when a sublimable substance as a solute is dissolved, the solvent is preferably a solvent that is soluble in the sublimable substance.
[0058] The solvent may be, for example, at least one selected from the group consisting of DIW, pure water, aliphatic hydrocarbons, aromatic hydrocarbons, esters, alcohols, ethers, and the like. Specifically, for example, DIW, pure water, methanol, ethanol, IPA, butanol, ethylene glycol, propylene glycol, NMP (N-methyl-2-pyrrolidone), DMF (N,N-dimethylformamide), DMA (dimethylacetamide), DMSO (dimethylsulfoxide), hexane, toluene, PGMEA (propylene glycol monomethyl ether acetate), PGME (propylene glycol monomethyl ether), PGPE (propylene glycol monopropyl ether), PGEE (propylene glycol monoethyl ether), GBL (γ-butyrolactone), acetylacetone, 3-pentanone, 2-heptanone, ethyl lactate, cyclohexanone, dibutyl ether, HFE (hydrofluoroether), ethyl nonafluoroisobutyl ether, ethyl nonafluorobutyl ether, and at least one selected from the group consisting of m-xylene hexafluoride.
[0059] Further, examples of solutes contained in the treatment liquid other than those mentioned above include polymers containing a protecting group that is dissociated by an acid. Copolymers having acrylate as a structural unit are also suitable.
[0060] The processing liquid supply unit 132 includes a pipe 132a, a valve 132b, and a nozzle 132n. The nozzle 132n ejects the processing liquid onto the upper surface Wa of the substrate W. The nozzle 132n is connected to the pipe 132a. The processing liquid is supplied to the pipe 132a from a supply source. The valve 132b opens and closes a flow path in the pipe 132a. The nozzle 132n is preferably configured to be movable relative to the substrate W.
[0061] The removing liquid supply unit 134 supplies a removing liquid to the upper surface Wa of the substrate W. The removing liquid can remove a filling layer formed from a solute of the processing liquid. By controlling the time for which the removing liquid is supplied, the filling layer can be selectively removed from the substrate W.
[0062] As the removing liquid, any solvent that dissolves any resin can be used. As the removing liquid, for example, organic solvents such as thinner, toluene, acetates, alcohols, and glycols, and acidic liquids such as acetic acid, formic acid, and hydroxyacetic acid can be used. In particular, it is preferable to use a solvent that is compatible with water-based liquids. For example, it is preferable to use isopropyl alcohol (IPA) as the removing liquid. Furthermore, an alkaline aqueous solution can be used as the removing liquid. For example, as the alkaline aqueous solution, inorganic alkalis such as sodium hydroxide, potassium hydroxide, sodium carbonate, and sodium silicate, organic amines such as ammonia, ethylamine, propylamine, diethylamine, diethylaminoethanol, and triethylamine, and quaternary amines can be used.
[0063] The removing liquid supply unit 134 includes a pipe 134a, a valve 134b, and a nozzle 134n. The nozzle 134n ejects the removing liquid onto the upper surface Wa of the substrate W. The nozzle 134n is connected to the pipe 134a. The removing liquid is supplied to the pipe 134a from a supply source. The valve 134b opens and closes a flow path in the pipe 134a. The nozzle 134n is preferably configured to be movable relative to the substrate W.
[0064] The water repellent agent supplying section 136 supplies a liquid water repellent agent to the upper surface Wa of the substrate W. A water repellent layer is formed on the upper surface Wa of the substrate W by the supply of the water repellent agent.
[0065] For example, the water repellent agent includes a compound having a methyl group or a silyl group at its terminal. Typically, hydroxyl groups (OH groups) are present on the surface of the recess, but the water repellent agent replaces the hydroxyl groups on the surface of the substrate W with methyl groups or silyl groups. It is preferable that the water repellent agent does not change the properties of the filling layer.
[0066] For example, the water repellent is a water repellent that makes silicon (Si) itself and compounds containing silicon hydrophobic. Typically, the water repellent is a silane coupling agent. In one example, the silane coupling agent includes at least one of HMDS (hexamethyldisilazane), TMS (tetramethylsilane), fluorinated alkylchlorosilane, alkyldisilazane, and non-chloro water repellent. The non-chloro water repellent includes at least one of dimethylsilyldimethylamine, dimethylsilyldiethylamine, hexamethyldisilazane, tetramethyldisilazane, bis(dimethylamino)dimethylsilane, N,N-dimethylaminotrimethylsilane, N-(trimethylsilyl)dimethylamine, and organosilane compound.
[0067] The water repellent agent supplying unit 136 includes a pipe 136a, a valve 136b, and a nozzle 136n. The nozzle 136n ejects the water repellent agent onto the upper surface Wa of the substrate W. The nozzle 136n is connected to the pipe 136a. The water repellent agent is supplied from a supply source to the pipe 136a. The valve 136b opens and closes a flow path in the pipe 136a. The nozzle 136n is preferably configured to be movable relative to the substrate W.
[0068] The chemical liquid supply unit 138 supplies a chemical liquid to the upper surface Wa of the substrate W. The upper surface Wa of the substrate W can be chemically processed by chemical processing using the chemical liquid. By chemical processing, it is possible to perform any one of etching, surface treatment, imparting properties, forming a processed film, and removing at least a part of a film on the substrate W. Typically, the chemical liquid is an etching liquid used in the etching process of the substrate W.
[0069] The chemical solution includes hydrofluoric acid. For example, the hydrofluoric acid may be heated to 40° C. or higher and 70° C. or lower, or may be heated to 50° C. or higher and 60° C. or lower. However, the hydrofluoric acid does not have to be heated. The chemical solution may also include water or phosphoric acid.
[0070] The chemical solution may further include hydrogen peroxide. The chemical solution may also include SC1 (ammonia hydrogen peroxide mixture), SC2 (hydrochloric acid hydrogen peroxide mixture), or aqua regia (a mixture of concentrated hydrochloric acid and concentrated nitric acid).
[0071] The chemical liquid supply unit 138 includes a pipe 138a, a valve 138b, and a nozzle 138n. The nozzle 138n ejects the chemical liquid onto the upper surface Wa of the substrate W. The nozzle 138n is connected to the pipe 138a. The chemical liquid is supplied from a supply source to the pipe 138a. The valve 138b opens and closes a flow path in the pipe 138a. The nozzle 138n is preferably configured to be movable relative to the substrate W.
[0072] As described above, the nozzles 132n, 134n, 136n, and 138n of the processing liquid supply unit 132, the removal liquid supply unit 134, the water repellent agent supply unit 136, and the chemical liquid supply unit 138 may be movable. The nozzles 132n, 134n, 136n, and 138n can move horizontally and / or vertically according to a movement mechanism controlled by the control unit 102. Note that in this specification, the movement mechanism is omitted to avoid overly complicating the drawings.
[0073] The substrate processing apparatus 100 further includes a cup 180. The cup 180 collects liquid scattered from the substrate W. The cup 180 moves up and down. For example, the cup 180 moves up vertically to the side of the substrate W during the period in which the liquid supply unit 130 supplies liquid to the substrate W. In this case, the cup 180 collects liquid scattered from the substrate W due to the rotation of the substrate W. Furthermore, when the period in which the liquid supply unit 130 supplies liquid to the substrate W ends, the cup 180 moves down vertically from the side of the substrate W.
[0074] As described above, the control device 101 includes the control unit 102 and the memory unit 104. The control unit 102 controls the substrate holder 120, the processing liquid supply unit 132, the removal liquid supply unit 134, the water repellent agent supply unit 136, and / or the cup 180. In one example, the control unit 102 controls the electric motor 124, and the valves 132b, 134b, 136b, and / or 138b.
[0075] The substrate processing apparatus 100 of this embodiment is suitable for use in the manufacture of a semiconductor device having a semiconductor. Typically, in a semiconductor device, a conductive layer and an insulating layer are laminated on a base material. The substrate processing apparatus 100 is suitable for use in cleaning and / or processing (e.g., etching, changing characteristics, etc.) the conductive layer and / or insulating layer during the manufacture of the semiconductor device.
[0076] Next, a substrate processing apparatus 100 according to the present embodiment will be described with reference to Figures 1 to 3. Figure 3 is a block diagram of the substrate processing apparatus 100.
[0077] 3, the control device 101 controls various operations of the substrate processing apparatus 100. The control device 101 controls the indexer robot IR, the center robot CR, the substrate holding unit 120, and the liquid supply unit 130. Specifically, the control device 101 controls the indexer robot IR, the center robot CR, the substrate holding unit 120, and the liquid supply unit 130 by transmitting control signals to the indexer robot IR, the center robot CR, the substrate holding unit 120, and the liquid supply unit 130.
[0078] Specifically, the control unit 102 controls the indexer robot IR to transfer the substrate W by the indexer robot IR.
[0079] The control unit 102 controls the center robot CR to transfer the substrate W by the center robot CR. For example, the center robot CR receives an unprocessed substrate W and carries the substrate W into any one of the multiple chambers 110. The center robot CR also receives a processed substrate W from the chamber 110 and carries the substrate W out.
[0080] The control unit 102 controls the substrate holding unit 120 to start rotation of the substrate W, change the rotation speed, and stop the rotation of the substrate W. For example, the control unit 102 can control the substrate holding unit 120 to change the rotation speed of the substrate holding unit 120. Specifically, the control unit 102 can change the rotation speed of the substrate W by changing the rotation speed of the electric motor 124 of the substrate holding unit 120.
[0081] The control unit 102 can individually control the valves 132b, 134b, 136b, 138b of the liquid supply unit 130 to switch the states of the valves 132b, 134b, 136b, 138b between an open state and a closed state. Specifically, the control unit 102 can control the valves 132b, 134b, 136b, 138b of the liquid supply unit 130 to open the valves 132b, 134b, 136b, 138b, thereby allowing the processing liquid, removal liquid, water repellent, and chemical liquid flowing through the pipes 132a, 134a, 136a, 138a to pass toward the nozzles 132n, 134n, 136n, 138n. Furthermore, the control unit 102 can control the valves 132b, 134b, 136b, and 138b of the liquid supply unit 130 to close the valves 132b, 134b, 136b, and 138b, thereby stopping the supply of the processing liquid, the removal liquid, the water repellent, and the chemical liquid flowing through the pipes 132a, 134a, 136a, and 138a toward the nozzles 132n, 134n, 136n, and 138n, respectively.
[0082] The substrate processing apparatus 100 of this embodiment is preferably used for forming semiconductor elements. For example, the substrate processing apparatus 100 is preferably used for processing a substrate W used as a semiconductor element having a stacked structure. The semiconductor element is a so-called 3D structure memory (storage device). As an example, the substrate W is preferably used as a NAND type flash memory.
[0083] Next, with reference to Fig. 4, a substrate W fabricated as a semiconductor element 300 using the substrate processing apparatus 100 of this embodiment will be described. Fig. 4(a) is a schematic side view of the semiconductor element 300 fabricated by processing the substrate W using the substrate processing apparatus 100, Fig. 4(b) is a schematic top view of the semiconductor element 300, and Fig. 4(c) is a partially enlarged view of Fig. 4(b). In Fig. 4, the direction perpendicular to the main surface of the base material S of the substrate W is indicated as the z direction, and the directions perpendicular to the z direction are indicated as the x direction and the y direction.
[0084] As shown in FIG. 4(a), the substrate W has a base material S and a layered structure L. The base material S is a thin film extending in the xy plane. The layered structure L is formed on the upper surface of the base material S. The base material S supports the layered structure L. The layered structure L is formed to extend in the z direction from the upper surface of the base material S.
[0085] The substrate W shown in FIG. 4(a) further includes an etching stop layer Es between the base material S and the laminated structure L. The etching stop layer Es is made of, for example, alumina (Al 2 O 3 As will be described in detail later, the stacked structure L is partially removed by etching to form the recess R. The progress of the etching is stopped by the etching stop layer Es.
[0086] The laminated structure L has an insulating layer N and a conductive layer M. The insulating layer N and the conductive layer M are laminated alternately. For example, the insulating layer N is made of a silicon oxide film. The conductive layer M is made of a metal. For example, the conductive layer M contains tungsten (W).
[0087] Each of the multiple insulating layers N extends parallel to the upper surface of the substrate S. A multiple number of conductive layers M are provided between two adjacent insulating layers N. The two adjacent insulating layers N are supported by the conductive layers M.
[0088] For example, the thickness (length along the z direction) of the insulating layer N is 1 nm or more and 50 nm or less, and for example, the thickness (length along the z direction) of the conductive layer M is 1 nm or more and 50 nm or less.
[0089] The sum of the thickness of one insulating layer N and the thickness of one conductive layer M is 20 nm to 100 nm. The laminated structure L includes 10 to 100 insulating layers N and 10 to 100 conductive layers M.
[0090] The laminated structure L is provided with a recess R. The recess R extends in a direction perpendicular to the main surface of the substrate S. The recess R extends between the surface La of the laminated structure L and the etching stop layer Es.
[0091] The diameter of the recess R is on the nano-order. For example, the diameter of the recess R is 20 nm or more and 300 nm or less. The diameter of the recess R may be 50 nm or more and 200 nm or less.
[0092] Ideally, the recesses R are formed perpendicular to the main surface of the substrate S. The diameter (top diameter Wt) of the surface portion of the recesses R is 20 nm or more and 300 nm or less, and is 50 nm or more and 200 nm or less.
[0093] For example, the aspect ratio of the recess R is 10 or more. Also, it has been reported so far that a memory hole with a height of about 1 μm can be formed with an aspect ratio of 40 to 50, and it is expected that the aspect ratio will further increase in the future. For example, the upper limit of the aspect ratio of the recess R may be 100 or 200.
[0094] In the semiconductor element 300 shown in FIG. 4(a), a cylindrical charge retention layer H is disposed in a recess R of a substrate W. A cylindrical channel layer Ch is disposed inside the charge retention layer H. For example, the channel layer Ch is made of polysilicon. A cylindrical dielectric layer D is disposed inside the channel layer Ch. The dielectric layer D is made of a silicon oxide film.
[0095] The charge retention layer H may have a three-layer structure. For example, the charge retention layer H includes a cylindrical inner layer H1, a cylindrical middle layer H2, and a cylindrical outer layer H3. The outer layer H3 contacts the laminated structure L. The middle layer H2 is disposed inside the outer layer H3. The inner layer H1 is disposed inside the middle layer H2. The inner layer H1 contacts the channel layer Ch. Therefore, from the center of the recess R of the laminated structure L, the dielectric layer D, the channel layer Ch, the inner layer H1, the middle layer H2, and the outer layer H3 are disposed.
[0096] For example, the inner layer H1 is made of a silicon oxide film. The inner layer H1 is also called a tunnel layer.
[0097] For example, the intermediate layer H2 is formed of a silicon nitride film. The intermediate layer H2 accumulates electric charges. The intermediate layer H2 is also called a charge accumulation layer.
[0098] For example, the outer layer H3 is formed of a silicon oxide film. The outer layer H3 is also called a blocking layer.
[0099] When a voltage is applied to the conductive layer M and the channel layer Ch, charges are stored in the corresponding intermediate layer H2. As shown in Fig. 4(a), a memory element Se is formed corresponding to the conductive layer M. Therefore, in one recess R, the number of memory elements Se formed corresponds to the number of conductive layers M.
[0100] As shown in FIG. 4(b), a plurality of recesses R are formed in the substrate W, and the recesses R are regularly arranged in the substrate W. A charge retention layer H, a channel layer Ch, and a dielectric layer D are arranged in each recess R. The plurality of recesses R are designed to have the same diameter and height. For example, the difference in the top diameter Wt of each recess R may be 5% or less, or may be 3% or less.
[0101] Typically, the recess R is formed by performing dry etching on the stacked structure L. When the stacked structure L is dry etched to form the recess R, the diameter of the deep portion of the recess R may become smaller than the diameter of the surface side of the recess R. In particular, when the height of the stacked structure and / or the number of layers in the stacked structure increases, the diameter of the deep portion of the recess R tends to become smaller than the diameter of the surface side of the recess R. In addition, the shorter the processing period of the dry etching is in order to improve the throughput, the more likely the diameter of the deep portion of the recess R tends to become smaller than the diameter of the surface side of the recess R.
[0102] As shown in FIG. 4(a), a plurality of memory elements Se are formed in the recess R. For this reason, it is preferable that the diameter of the recess R is constant from the surface side portion to the deep portion. However, when the recess R is formed in the stacked structure L, the diameter of the recess R may not be constant. If the diameter of the recess R is different, when the memory elements are formed in the recess R, the electrical characteristics of the memory elements may not be constant, and the characteristics of the memory elements may not be uniform.
[0103] Generally, the smaller the diameter of the recess R, the more memory elements can be formed in the substrate, so a smaller diameter of the recess R is preferable in order to increase memory capacity. However, if the diameter of the recess R is small, the flow of the etching fluid for etching the recess R is likely to be insufficient. For this reason, when the recess R is etched, etching tends to be uneven depending on the position of the recess R. Specifically, the surface side portion of the recess R is relatively easily etched, whereas the deeper portion of the recess R is relatively difficult to etch.
[0104] Although details will be described later, according to this embodiment, even if the diameter of the recess R is small, the deep portion Rf of the recess R can be selectively etched. This makes it possible to suppress non-uniformity in the diameter of the recess R.
[0105] Next, the semiconductor device forming method of this embodiment will be described with reference to Fig. 5. A part of the semiconductor device forming method of this embodiment is performed using the substrate processing apparatus 100 described above with reference to Figs.
[0106] As shown in FIG. 5(a), the substrate W has a base material S and a laminated structure L. The base material S is a thin film extending in the xy plane. The laminated structure L is formed on the upper surface of the base material S. The laminated structure L is formed so as to extend in the z direction from the upper surface of the base material S. For example, the laminated structure L is formed of a silicon oxide film and a silicon nitride film. The laminated structure L has a surface La.
[0107] The laminated structure L has an insulating layer N and a sacrificial layer Sa. The insulating layers N and the sacrificial layers Sa are alternately laminated. Each of the insulating layers N extends parallel to the upper surface of the substrate S. A plurality of sacrificial layers Sa are provided between two adjacent insulating layers N. The two adjacent insulating layers N are supported by the sacrificial layers Sa. The sacrificial layers Sa are replaced with the conductive layers M shown in FIG. 4 in the process of fabricating the semiconductor element 300.
[0108] For example, the thickness (length along the z direction) of the insulating layer N is 1 nm or more and 50 nm or less. The insulating layer N is made of a silicon oxide film.
[0109] Furthermore, for example, the thickness (length along the z direction) of the sacrificial layer Sa is 1 nm or more and 50 nm or less. For example, the sacrificial layer Sa is made of a material that is etched when an etching solution that does not substantially etch the insulating layer N is used. In one example, the sacrificial layer Sa is made of a silicon nitride film. For example, when phosphoric acid is used as the etching solution, the sacrificial layer Sa can be etched without substantially etching the insulating layer N.
[0110] As shown in FIG. 5(b), a recess R is formed in the laminated structure L. Typically, the recess R is formed by dry etching. Ideally, the diameter (length in the xy plane) of the recess R formed by dry etching is constant from the surface side to the deep part, but in reality, the diameter of the recess R may not be constant from the surface side to the deep part. In particular, when the processing time of the dry etching is shortened to improve the throughput of the substrate W, it is difficult for the diameter of the recess R to be constant from the surface side to the deep part. In this case, the diameter of the deep part Rf of the recess R is smaller than the diameter of the surface side part Rn of the recess R.
[0111] As shown in FIG. 5(c), the recess R of the substrate W is deformed. For example, the diameter of the deep portion Rf of the recess R is selectively made larger than the diameter of the deep portion Rf of the recess R after dry etching. In one example, the diameter of the deep portion Rf of the recess R is expanded over a length of less than 10 nm along the xy plane. This allows the diameter of the recess R of the substrate W to be uniform from the surface side to the deep portion.
[0112] As shown in FIG. 5(d), a charge retention layer H is formed inside the recess R of the laminated structure L.
[0113] 5(e), a channel layer Ch and a dielectric layer D are formed inside the charge retention layer H. Thereafter, the sacrificial layer Sa is replaced with a conductive layer M. In this manner, the semiconductor element 300 shown in FIG. 4 can be formed.
[0114] In Fig. 5(b), in order to avoid overly complicated explanation, the diameter of the recess R is shown to change linearly from the surface side to the depth, but this embodiment is not limited to this. Due to the bowing phenomenon, the diameter of the recess R may be largest near the center.
[0115] Next, the semiconductor device forming method of this embodiment will be described with reference to Figs. 1 to 3 and 6. Figs. 6(a) to 6(g) are schematic diagrams for explaining the semiconductor device forming method of this embodiment. The semiconductor device forming method shown in Figs. 6(a) to 6(g) is suitably used as a part of the semiconductor device forming method described above with reference to Fig. 5. For example, the semiconductor device forming method shown in Figs. 6(a) to 6(g) is performed for the modification of the recess R shown in Fig. 5(c). The semiconductor device forming method of this embodiment is performed using the substrate processing apparatus 100 described above with reference to Figs. 1 to 3.
[0116] As shown in Fig. 6(a), a recess R is provided in the laminated structure L. For example, the recess R is formed in the laminated structure L by etching the substrate W. Here, the recess R is formed in the insulating layer N and the sacrificial layer Sa. The recess R reaches the etching stop layer Es.
[0117] As shown in FIG. 6(b), the recess R is filled with a filling layer F. The filling layer F is, for example, an organic material (carbon-based material). In one example, the filling layer F is a polymer. The filling layer F may be formed of a resist. For example, after the processing liquid supply unit 132 supplies the processing liquid to the substrate W, the solvent is volatilized from the processing liquid, and the filling layer F is formed from the solute of the processing liquid. Here, the filling layer F fills from the deep portion Rf of the recess R to the surface side portion Rn.
[0118] The processing liquid preferably changes to a solid state after being applied to the substrate W. The processing liquid itself is in a liquid state, but after the processing liquid is applied to the substrate W, the solvent evaporates, and the solute changes to a solid state to form a filling layer F.
[0119] As shown in FIG. 6(c), a removing liquid Ds is applied to the substrate W. The removing liquid Ds dissolves the filling layer F. Here, the removing liquid Ds partially dissolves the filling layer F filled in the recess R. As a result, the surface side portion Rn of the recess R is replaced with the removing liquid Ds while the deep portion Rf of the recess R remains filled with the filling layer F. As a result, a partial filling layer Fp that partially fills the deep portion Rf of the recess R is formed from the filling layer F.
[0120] For example, the removing liquid supply unit 134 supplies the removing liquid Ds to the substrate W. The removing liquid supply unit 134 supplies the removing liquid Ds for a time and in an amount that is set so that the filling layer F is partially dissolved but not completely dissolved. For example, the removing liquid Ds contains isopropyl alcohol (IPA).
[0121] Typically, more than half of the depth of the recess R is replaced with the removal liquid Ds, and less than half of the filling layer F remains in the depth of the recess R to become the partial filling layer Fp. For example, the depth of the partial filling layer Fp (length in the z-axis direction) is ⅓ or less of the depth of the recess R.
[0122] 6(d), a water repellent agent P is supplied. For example, the water repellent agent supplying unit 136 supplies the water repellent agent P to the substrate W. The partial filling layer Fp is not affected by the water repellent agent P, and the removing liquid Ds is replaced with the water repellent agent P. As a result, the removing liquid Ds in the surface side portion Rn of the recess R is replaced with the water repellent agent P, while the deep portion Rf of the recess R remains filled with the partial filling layer Fp.
[0123] Although the deep portion Rf of the recess R is covered with the partial filling layer Fp, the surface side portion Rn of the recess R is not covered with the partial filling layer Fp. Therefore, when the water repellent P is supplied, the surface of the laminated structure L reacts with the water repellent P in the surface side portion Rn of the recess R to form a coating layer Ps.
[0124] As shown in FIG. 6(e), the partial filling layer Fp and the water repellent P are removed. In this case, a part of the water repellent P on the surface side of the recess R is removed together with the partial filling layer Fp in the deep portion Rf of the recess R. At this time, it is preferable to also remove particles that are residues when the recess R is formed (e.g., during dry etching). By removing the partial filling layer Fp, the insulating layer N and the sacrificial layer Sa are exposed in the deep portion Rf of the recess R. Meanwhile, the surface side portion Rn of the recess R remains covered with the covering layer Ps.
[0125] For example, a removal liquid may be applied to remove the partial filling layer Fp and the water repellent agent P. In one example, the removal liquid includes IPA. For example, the removal liquid supply unit 134 supplies the removal liquid Ds to the substrate W. The removal liquid supply unit 134 supplies the removal liquid for a time and in an amount set so that the partial filling layer Fp is completely dissolved.
[0126] Alternatively, the substrate W may be heated to remove the partial filling layer Fp and the water repellent agent P. For example, if the partial filling layer Fp is formed from a sublimable substance, the partial filling layer Fp may be sublimated by heating.
[0127] As shown in FIG. 6(f), the recess R is etched with a chemical solution C. Typically, the chemical solution C contains hydrofluoric acid. For example, the chemical solution C contains hydrofluoric acid diluted in the range of 1:100 to 1:2000. Alternatively, the chemical solution C may contain water or deionized water (DIW). Alternatively, the chemical solution C may contain phosphoric acid.
[0128] The deep portion Rf of the recess R is etched by the chemical solution C because the insulating layer N and the sacrificial layer Sa are exposed therein. On the other hand, the surface side portion Rn of the recess R is not etched by the chemical solution C because it is covered by the covering layer Ps. Therefore, as shown in FIG. 6(f), the region Re located in the deep portion Rf of the recess R is removed by the chemical solution C, and the diameter of the recess R is enlarged. The diameter of the deep portion Rf of the recess R may be enlarged so as to be equal to the diameter (top diameter) just before the recess R.
[0129] As shown in FIG. 6(g), the chemical solution C and the coating layer Ps are removed. The chemical solution C and the coating layer Ps may be removed by ultraviolet irradiation or heating. At this time, it is preferable that the residue from the dry etching is also removed. The chemical solution C and the coating layer Ps may be removed in an apparatus other than the substrate processing apparatus 100.
[0130] In this manner, the diameter of the recess R of the laminated structure L can be adjusted. In Fig. 6(e), Fig. 6(f) and Fig. 6(g), the diameter of the deep portion Rf of the recess R is illustrated as being equal to the top diameter (aperture) of the recess R, while the diameter of the deep portion Rf of the recess R is larger than the diameter of the central portion of the recess R, so that the change in the shape of the recess R can be easily understood. However, it should be noted that this is merely an example. The diameter of the deep portion Rf of the recess R may be enlarged so that the diameter of the deep portion Rf of the recess R is equal to the diameter of the central portion of the recess R. Alternatively, the recess R may be deformed so that the diameter of the deep portion Rf of the recess R is equal to the top diameter and the diameter of the central portion of the recess R.
[0131] In FIG. 6(c), the filling layer F is partially replaced with the removing liquid Ds by applying the removing liquid Ds. When the diameter of the recess R is small, it takes a relatively long time for the removing liquid Ds to remove the entire filling layer F. For this reason, the removal process of the filling layer F by the removing liquid Ds is interrupted halfway through the time it takes for the removing liquid Ds to remove the entire filling layer F, so that the filling layer F can be partially removed. Also, as shown in FIG. 6(c), by adjusting the amount of the removing liquid Ds, the processing time, etc., it is possible to leave a partial filling layer Fp that covers an appropriate portion.
[0132] 6(c), the partial filling layer Fp is formed from the filling layer F by the removal liquid Ds, but this embodiment is not limited to this. When the filling layer F is made of a sublimable substance, the partial filling layer Fp may be formed from the filling layer F by heating. In this case, too, the partial filling layer Fp that partially fills the deep portion Rf of the recess R may be formed from the filling layer F by adjusting the heating time and temperature.
[0133] The substrate W is preferably used as a memory having a plurality of memory elements Se. Typically, when the substrate W is used as a memory, the substrate W is provided with a plurality of recesses R designed to have a uniform diameter and height. Therefore, a plurality of recesses used in a memory having a large storage capacity can be simultaneously deformed by the same process.
[0134] When forming the recess R in the laminated structure L, the diameter of the recess R may be largest near the center due to the bowing phenomenon. In this case, it is preferable that the covering layer Ps covers the center. The diameter of the deep portion Rf of the recess R may be enlarged by etching so as to be equal to the largest diameter of the recess R at the center.
[0135] In the above description with reference to Fig. 6, the coating layer Ps is formed by supplying the liquid water repellent P to the filled recess R of the partial filling layer Fp, but this embodiment is not limited to this. The coating layer Ps may be formed by a gas.
[0136] Next, a semiconductor device forming method of the present embodiment will be described with reference to Figures 1 to 3, 6, and 7. Figure 7 is a flow diagram of the semiconductor device forming method. The semiconductor device forming method of the present embodiment is suitably performed by the substrate processing apparatus 100 described above with reference to Figures 1 to 3.
[0137] First, in step S10, the recess R is partially covered with the laminated structure L. Typically, the surface side portion Rn of the recess R is selectively covered. For example, a covering layer Ps is formed on the surface side portion Rn of the recess R. The covering layer Ps selectively covers the surface side portion Rn of the recess R, but does not cover the deep portion Rf of the recess R. Therefore, the laminated structure L is exposed in the deep portion Rf of the recess R.
[0138] In step S20, the diameter of the deep portion Rf of the recess R is expanded. By applying the chemical solution C to the recess R, the diameter of the deep portion Rf of the recess R can be expanded. Since the recess R is partially covered with the coating layer Ps, the diameter of the deep portion Rf of the recess R that is not covered with the coating layer Ps is partially expanded. This allows the diameter of the deep portion Rf of the recess R to be expanded, and therefore the diameter of the recess R can be adjusted.
[0139] Next, a semiconductor device forming method of the present embodiment will be described with reference to Figures 1 to 3 and 6 to 8. Figure 8 is a flow diagram of the semiconductor device forming method. The semiconductor device forming method of the present embodiment is suitably performed using the substrate processing apparatus 100 described above with reference to Figures 1 to 3.
[0140] First, in step Sa, the substrate W is carried into the substrate processing apparatus 100. Here, the substrate W has a base material S and a laminated structure L, and the laminated structure L has a recess R provided therein.
[0141] In step S10, the recesses R are partially covered in the laminate structure L. Here, the partial coverage of the recesses R in step S10 is performed by forming a filling layer F in step S12, partially removing the filling layer F (forming a partial filling layer Fp) in step S14, supplying a water repellent agent in step S16, and removing the partial filling layer Fp in step S18.
[0142] In step S12, the recess R is filled with a filling layer F. The processing liquid supply unit 132 supplies the processing liquid to the substrate W. As a result, the filling layer F is filled into the recess R of the substrate W. Typically, after the processing liquid is supplied, the substrate holding unit 120 increases the rotation speed of the substrate W to shake off the processing liquid remaining in excess on the surface of the substrate W to the outside of the substrate W.
[0143] In step S14, a portion of the filling layer F is removed. For example, the removing liquid supply unit 134 supplies the removing liquid to the substrate W for a predetermined period of time. The removing liquid Ds is applied to the filling layer F in the recess R, thereby partially dissolving the filling layer F and forming a partial filling layer Fp in the recess R. The time for applying the removing liquid Ds is set so as to partially remove the filling layer F in the recess R. At this time, the filling layer F in the surface side portion Rn of the recess R is removed, while the partial filling layer Fp remains in the deep portion Rf of the recess R.
[0144] Alternatively, the filling layer F may be heated for a predetermined period of time to form a partial filling layer Fp in the recess R. For example, when the filling layer F contains a sublimable substance, the filling layer F can be heated for a predetermined period of time to sublimate a part of the filling layer F to form the partial filling layer Fp in the recess R.
[0145] In step S16, a water repellent is supplied to the substrate W. The water repellent supplying unit 136 supplies the water repellent to the substrate W. By applying the water repellent to the recess R in which the partial filling layer Fp is formed in the deep portion Rf, the water repellent is filled in the surface side portion Rn of the recess R where the partial filling layer Fp is not formed, and a water repellent layer is formed. At this time, the characteristics of the surface side portion Rn of the recess R are changed by the water repellent, and a coating layer Ps is formed on the surface side portion Rn of the recess R. In this way, by supplying the water repellent, a coating layer Ps is formed as a part of the water repellent layer on the surface side portion Rn of the recess R.
[0146] In step S18, the partial filling layer Fp is removed. Here, the portion of the water-repellent layer formed from the water-repellent agent other than the coating layer Ps is removed, and the partial filling layer Fp is also removed. For example, the removing liquid supply unit 134 supplies a removing liquid to the substrate W to dissolve the partial filling layer Fp and replace the portion of the water-repellent layer other than the coating layer Ps. At this time, the surface side portion Rn of the recess R is covered with the coating layer Ps, while the laminated structure L is exposed in the deep portion Rf of the recess R.
[0147] Alternatively, the partial filling layer Fp may be removed by heating the partial filling layer Fp for a predetermined period of time. For example, when the filling layer F contains a sublimable substance, the filling layer F can be heated to sublimate a part of the filling layer F, thereby removing the partial filling layer Fp from the recess R.
[0148] Next, in step S20, the diameter of the deep portion Rf of the recess is expanded. For example, the chemical solution supply unit 138 supplies a chemical solution to the substrate W. As a result, the deep portion Rf of the recess R that is not covered by the covering layer Ps is partially etched, and the recess diameter is expanded.
[0149] In step Sb, the substrate W is unloaded from the substrate processing apparatus 100. Thereafter, the covering layer Ps is removed as necessary. The covering layer Ps may be removed by ashing the covering layer Ps by irradiation with ultraviolet light or heat treatment. In this manner, the substrate W in which the variation in the recess diameter is suppressed can be formed.
[0150] In the above description with reference to FIG. 8, the etching in step S20 is performed with one type of etching solution, but this embodiment is not limited to this. The etching in step S20 may be performed with multiple types of etching solutions. For example, with one type of etching solution, the etching amount of the insulating layer N may not be equal to the etching amount of the sacrificial layer Sa. In this case, it is preferable to perform the etching in step S20 with multiple types of etching solutions.
[0151] Next, a semiconductor device forming method of this embodiment will be described with reference to Figures 1 to 3, 6, 9, and 10. Figure 9 is a schematic diagram of a substrate processing apparatus 100 of this embodiment. The substrate processing apparatus 100 of Figure 9 has a similar configuration to the substrate processing apparatus 100 shown in Figure 2, except that the liquid supply unit 130 further includes a rinsing liquid supply unit 137 and the chemical liquid supply unit 138 includes a first chemical liquid supply unit 138A and a second chemical liquid supply unit 138B, and therefore, to avoid redundancy, repeated descriptions will be omitted.
[0152] In the substrate processing apparatus 100, the liquid supply unit 130 further includes a rinsing liquid supply unit 137. The rinsing liquid supply unit 137 supplies the substrate W with a rinsing liquid.
[0153] The rinsing liquid supply unit 137 supplies a rinsing liquid to the upper surface Wa of the substrate W. A rinsing process using the rinsing liquid can wash away chemicals, impurities, and the like adhering to the upper surface Wa of the substrate W. The rinsing liquid supplied from the rinsing liquid supply unit 137 may include any of deionized water (DIW), carbonated water, electrolytic ionized water, ozone water, ammonia water, hydrochloric acid water with a diluted concentration (for example, about 10 ppm to 100 ppm), or reduced water (hydrogen water).
[0154] The rinsing liquid supply unit 137 includes a pipe 137a, a valve 137b, and a nozzle 137n. The nozzle 137n ejects the rinsing liquid onto the upper surface Wa of the substrate W. The nozzle 137n is connected to the pipe 137a. The rinsing liquid is supplied to the pipe 137a from a supply source. The valve 137b opens and closes a flow path in the pipe 137a. The nozzle 137n is preferably configured to be movable relative to the substrate W.
[0155] In the substrate processing apparatus 100, the chemical liquid supply unit 138 includes a first chemical liquid supply unit 138A and a second chemical liquid supply unit 138B. The first chemical liquid supply unit 138A supplies a first chemical liquid to the substrate W. The second chemical liquid supply unit 138B supplies a second chemical liquid to the substrate W.
[0156] The first chemical liquid supply unit 138A supplies a first chemical liquid to the upper surface Wa of the substrate W. The upper surface Wa of the substrate W can be chemically processed by chemical processing using the first chemical liquid. The first chemical liquid supply unit 138A includes a pipe 138a, a valve 138b, and a nozzle 138n. The nozzle 138n ejects the first chemical liquid onto the upper surface Wa of the substrate W. The nozzle 138n is connected to the pipe 138a. The first chemical liquid is supplied from a supply source to the pipe 138a. The valve 138b opens and closes a flow path in the pipe 138a. The nozzle 138n is preferably configured to be movable relative to the substrate W.
[0157] The second chemical liquid supply unit 138B supplies the second chemical liquid to the upper surface Wa of the substrate W. The upper surface Wa of the substrate W can be chemically processed by chemical processing using the second chemical liquid. The second chemical liquid supply unit 138B includes a pipe 138c, a valve 138d, and a nozzle 138m. The nozzle 138m ejects the second chemical liquid onto the upper surface Wa of the substrate W. The nozzle 138m is connected to the pipe 138c. The second chemical liquid is supplied to the pipe 138c from a supply source. The valve 138d opens and closes a flow path in the pipe 138c. It is preferable that the nozzle 138m is configured to be movable relative to the substrate W.
[0158] The etching selectivity of the first chemical liquid for the sacrificial layer Sa relative to the insulating layer N is different from the etching selectivity of the second chemical liquid for the sacrificial layer Sa relative to the insulating layer N. For example, when the etching ratio of the first chemical liquid for the sacrificial layer Sa relative to the insulating layer N is high, the etching ratio of the second chemical liquid for the sacrificial layer Sa relative to the insulating layer N is low. In one example, when the first chemical liquid contains hydrofluoric acid, it is preferable that the second chemical liquid contains water or phosphoric acid. In this way, by using the first chemical liquid and the second chemical liquid having different etching selectivities of the sacrificial layer Sa relative to the insulating layer N, the etching amount of the insulating layer N can be made equal to the etching amount of the sacrificial layer Sa.
[0159] The control unit 102 can switch the states of the valves 137b, 138b, 138d between an open state and a closed state by separately controlling the valves 137b, 138b, 138d of the liquid supply unit 130. Specifically, the control unit 102 can pass the rinsing liquid, the first chemical liquid, and the second chemical liquid flowing through the pipes 137a, 138a, 138c toward the nozzles 137n, 138n, 138m by controlling the valves 137b, 138b, 138d of the liquid supply unit 130 to open the valves 137b, 138b, 138d. In addition, the control unit 102 can control the valves 137b, 138b, and 138d of the liquid supply unit 130 to close the valves 137b, 138b, and 138d, thereby stopping the supply of the rinsing liquid, the first chemical liquid, and the second chemical liquid flowing through the pipes 137a, 138a, and 138c toward the nozzles 137n, 138n, and 138m, respectively.
[0160] Fig. 10 is a flow diagram of the semiconductor element forming method of the present embodiment. The flow diagram of Fig. 10 is similar to the flow diagram of Fig. 8 except that etching of the deep portion Rf of the recess R is performed with a plurality of etching solutions, and therefore, to avoid redundancy, overlapping descriptions are omitted.
[0161] In this embodiment, the etching in step S20 includes a first etching in step S20a, a rinse liquid supply in step S20b, and a second etching in step S20c. The first etching and the second etching have different etching selectivities of the sacrificial layer Sa to the insulating layer N. For example, when the etching ratio of the sacrificial layer Sa to the insulating layer N is high in the first etching, it is preferable that the etching ratio of the sacrificial layer Sa to the insulating layer N is low in the second etching.
[0162] In step S20a, the first etching selectively etches one of the insulating layer N and the sacrificial layer Sa. For example, the first chemical liquid supply unit 138A supplies the first chemical liquid to the upper surface Wa of the substrate W. When selectively etching the insulating layer N of the insulating layer N and the sacrificial layer Sa, it is preferable to use hydrofluoric acid as the first chemical liquid. When selectively etching the sacrificial layer Sa of the insulating layer N and the sacrificial layer Sa, it is preferable to use hot water or phosphoric acid as the first chemical liquid.
[0163] Thereafter, in step S20b, a rinsing process is performed. The rinsing liquid supply unit 137 supplies a rinsing liquid to the upper surface Wa of the substrate W.
[0164] In step S20c, the second etching selectively etches the other of the insulating layer N and the sacrificial layer Sa. For example, the second chemical liquid supply unit 138B supplies the second chemical liquid to the upper surface Wa of the substrate W. When one of the insulating layer N and the sacrificial layer Sa is selectively etched in the first etching, the other of the insulating layer N and the sacrificial layer Sa is selectively etched in the second etching. As described above, by performing two etchings with different selectivity, the amount of etching of the insulating layer N can be made equal to the amount of etching of the sacrificial layer Sa.
[0165] 2, 6, and 7, the processing liquid supply unit 132 supplies the processing liquid to the substrate W, thereby forming the filling layer F. When the processing liquid contains a solute and a volatile solvent, it is preferable to heat the processing liquid after the processing liquid supply unit 132 supplies the processing liquid to the substrate W. By heating the processing liquid, the filling layer F can be formed quickly.
[0166] Next, the semiconductor device forming method of this embodiment will be described with reference to Figures 11 and 12. Figure 11 is a schematic diagram of a substrate processing apparatus 100 of this embodiment. The substrate processing apparatus 100 of Figure 11 has the same configuration as the substrate processing apparatus 100 shown in Figure 2, except that it further includes a heat medium supply unit 140, a gas supply unit 142, and a shielding member 150, and therefore duplicated descriptions will be omitted to avoid redundancy.
[0167] The substrate processing apparatus 100 further includes a heat medium supplying unit 140, a gas supplying unit 142, and a shielding member 150. The heat medium supplying unit 140 supplies a heat medium to the substrate W. The gas supplying unit 142 supplies a gas to the substrate W. The shielding member 150 shields the substrate W from the vertically upper side.
[0168] The processing liquid supply unit 132 supplies a processing liquid containing a solute and a volatile solvent. The filling layer F is formed from the solute component.
[0169] The heat medium supplied by the heat medium supply unit 140 may be either liquid or gas. For example, the heat medium is hot water. While or after the processing liquid supply unit 132 supplies the processing liquid to the upper surface Wa of the substrate W, the heat medium supply unit 140 heats the substrate W held by the spin base 121 and the chuck member 122 from the rear surface Wb side of the substrate W to form a filling layer on the upper surface Wa of the substrate W.
[0170] While the substrate W is rotating, the heat medium supplying unit 140 supplies the heat medium toward the center position of the back surface Wb of the substrate W. The supplied heat medium spreads over substantially the entire back surface Wb of the substrate W by the action of centrifugal force. As a result, the processing liquid on the substrate W and the upper surface Wa of the substrate W is heated, and the solvent is volatilized from the processing liquid to quickly form a filling layer.
[0171] The heat medium supply unit 140 includes a pipe 140a, a valve 140b, and a nozzle 140n. The nozzle 140n faces the back surface Wb of the substrate W. The nozzle 140n ejects the heat medium onto the back surface Wb of the substrate W. The nozzle 140n is connected to the pipe 140a. The heat medium is supplied to the pipe 140a from a supply source. The valve 140b opens and closes a flow path in the pipe 140a.
[0172] The gas supply unit 142 supplies a gas to the upper surface Wa of the substrate W. The gas supplied by the gas supply unit 142 preferably contains an inert gas. The inert gas contains nitrogen gas.
[0173] The gas supply unit 142 includes a pipe 142a and a valve 142b. A gas is supplied from a supply source to the pipe 142a. The valve 142b opens and closes a flow path in the pipe 142a.
[0174] The shielding member 150 is located above the substrate holding part 120. The shielding member 150 faces the substrate W. Here, the outer diameter of at least a part of the shielding member 150 in the horizontal direction is substantially equal to the outer diameter of the substrate W.
[0175] The shielding member 150 moves relative to the substrate W between a proximity position and a retracted position. When the shielding member 150 is located at the proximity position, the shielding member 150 descends and approaches the upper surface of the substrate W at a predetermined distance. At the proximity position, the shielding member 150 covers the surface of the substrate W and shields the area above the substrate W. When the shielding member 150 is located at the retracted position, the shielding member 150 is located at a position vertically above the proximity position. When the shielding member 150 moves from the proximity position to the retracted position, the shielding member 150 rises and moves away from the substrate W.
[0176] The shielding member 150 includes a shielding plate 152, a support shaft 154, and a nozzle 156. The support shaft 154 is located on the line of the rotation axis Ax of the shaft 123. The shielding plate 152 extends in the horizontal direction from the support shaft 154. Here, the shielding plate 152 has a shape that extends in the horizontal direction. For example, the shielding plate 152 is substantially disk-shaped.
[0177] A pipe 134a of the removing liquid supply unit 134 and a pipe 142a of the gas supply unit 142 are connected to the nozzle 156. The nozzle 156 functions as a nozzle for the removing liquid supply unit 134 and the gas supply unit 142.
[0178] The control unit 102 can control the valves 140b, 142b separately to switch the states of the valves 140b, 142b between an open state and a closed state. Specifically, the control unit 102 can control the valves 140b, 142b to open the valves 140b, 142b to allow the heat medium and gas flowing through the pipes 140a, 142a toward the nozzles 140n, 156 to pass. The control unit 102 can also control the valves 140b, 142b to close the valves 140b, 142b to stop the supply of the heat medium and gas flowing through the pipes 140a, 142a toward the nozzles 140n, 156.
[0179] Furthermore, the control unit 102 controls the shielding member 150 to move the shielding member 150 relative to the substrate W between the approach position and the retracted position.
[0180] Fig. 12 is a flow diagram of the semiconductor device forming method of the present embodiment. The flow diagram of Fig. 12 is similar to the flow diagram of Fig. 8 except that the formation of the filling layer F is performed in multiple steps, and therefore, to avoid redundancy, overlapping descriptions are omitted.
[0181] The formation of the filling layer F in step S12 includes supplying a treatment solution in step S12a, spinning off in step S12b, and heating in step S12c.
[0182] In step S12a, the processing liquid is supplied by the processing liquid supply unit 132 onto the upper surface Wa of the substrate W. At this time, the rotation speed of the substrate W is 10 rpm to 100 rpm.
[0183] In step S12b, after supplying the processing liquid, the substrate holder 120 increases the rotation speed of the substrate W to spin off the processing liquid from the upper surface Wa of the substrate W. For example, the rotation speed of the substrate W is increased to 300 rpm to 1500 rpm.
[0184] In step S12c, the heat medium supplying unit 140 supplies a heat medium to the back surface Wb of the substrate W. For example, after the processing liquid is spun off, the rotation speed of the substrate W is reduced to 100 rpm to 1000 rpm. By heating the processing liquid on the upper surface Wa of the substrate W, a filling layer F can be quickly formed from the processing liquid.
[0185] 11 and 12, the processing liquid is heated by the heat medium supplied from the heat medium supply unit 140, but this embodiment is not limited to this. A heat source such as a lamp or an electric heater may be provided in the substrate processing apparatus 100, and the processing liquid may be heated by utilizing heat from the heat source.
[0186] It is preferable to supply a stripping liquid to the substrate W before supplying the removal liquid for removing the filling layer F and / or the partial filling layer Fp.
[0187] Next, the semiconductor element forming method of this embodiment will be described with reference to Figures 6, 13, and 14. Figure 13 is a schematic diagram of a substrate processing apparatus 100 of this embodiment. The substrate processing apparatus 100 of Figure 13 has the same configuration as the substrate processing apparatus 100 shown in Figure 11, except that the liquid supply unit 130 further includes a rinsing liquid supply unit 137 and a stripping liquid supply unit 160, and therefore, to avoid redundancy, repeated descriptions will be omitted.
[0188] In the substrate processing apparatus 100 of this embodiment, the liquid supply unit 130 further includes a rinsing liquid supply unit 137 and a stripping liquid supply unit 160. The rinsing liquid supply unit 137 supplies a rinsing liquid to the substrate W. The stripping liquid supply unit 160 supplies a stripping liquid to the substrate W.
[0189] The rinsing liquid supply unit 137 supplies a rinsing liquid to the substrate W. The rinsing liquid supply unit 137 includes a pipe 137a and a valve 137b. The rinsing liquid is supplied from a supply source to the pipe 137a. The valve 137b opens and closes a flow path in the pipe 137a.
[0190] A pipe 137a of a rinsing liquid supply unit 137 is connected to the nozzle 156 of the shielding member 150. The nozzle 156 functions as a nozzle of the rinsing liquid supply unit 137.
[0191] The remover liquid supply unit 160 supplies a remover liquid to the upper surface Wa of the substrate W. The remover liquid has a remover property with respect to the filling layer F. By supplying the remover liquid, the filling layer F can be easily removed thereafter. For example, the remover liquid includes at least one of DIW and SC1. By controlling the concentration and processing time of the remover liquid supplied by the remover liquid supply unit 160, a partial filling layer Fp can be appropriately formed from the filling layer F.
[0192] Here, the stripping liquid supply unit 160 includes a first stripping liquid supply unit 162 and a second stripping liquid supply unit 164. The first stripping liquid supply unit 162 supplies a first stripping liquid to the upper surface Wa of the substrate W. The second stripping liquid supply unit 164 supplies a second stripping liquid to the upper surface Wa of the substrate W. The first stripping liquid supply unit 162 supplies a stripping liquid different from the second stripping liquid supply unit 164 to the upper surface Wa of the substrate W.
[0193] The first stripping liquid supply unit 162 includes a pipe 162a and a valve 162b. The first stripping liquid is supplied from a supply source to the pipe 162a. The valve 162b opens and closes a flow path in the pipe 162a.
[0194] The second stripping liquid supply unit 164 includes a pipe 164a and a valve 164b. The second stripping liquid is supplied from a supply source to the pipe 164a. The valve 164b opens and closes a flow path in the pipe 164a.
[0195] The stripping liquid supply unit 160 further includes a pipe 160a and a nozzle 160n. The pipe 160a is connected to the pipe 162a and the pipe 164a. The nozzle 160n discharges the stripping liquid onto the upper surface Wa of the substrate W. The nozzle 160n is connected to the pipe 160a. The nozzle 160n is preferably configured to be movable relative to the substrate W.
[0196] The control unit 102 can separately control the valves 162b and 164b of the stripping liquid supply unit 160 to switch the states of the valves 162b and 164b between an open state and a closed state. Specifically, the control unit 102 can control the valves 162b and 164b of the stripping liquid supply unit 160 to open the valve 162b or 164b, thereby allowing the first stripping liquid and the second stripping liquid flowing through the pipe 160a and the pipe 162a or 164a toward the nozzle 160n to pass. The control unit 102 can also control the valves 162b and 164b of the stripping liquid supply unit 160 to close the valves 162b and 164b, thereby stopping the supply of the first stripping liquid and the second stripping liquid flowing through the pipe 160a and the pipe 162a or 164a toward the nozzle 160n.
[0197] When the processing liquid contains a heat-sensitive water-soluble resin as a solute, in order to make the temperature of the heat-sensitive water-soluble resin lower than the deterioration temperature when the processing liquid is heated, it is preferable to use a heat medium whose boiling point is lower than the deterioration temperature. For example, in the case of a heat-sensitive water-soluble resin whose deterioration temperature is 180° C., DIW (boiling point: 100° C.) or the like can be used as the heat medium. It is more preferable that the temperature of the heat medium is lower than the boiling point of the solvent. By making the temperature of the processing liquid lower than the boiling point of the solvent, the solvent can be left in the filling layer. Then, the interaction between the solvent remaining in the filling layer and the stripping liquid makes it easier to strip the filling layer from the upper surface of the substrate W.
[0198] Fig. 14 is a flow diagram of the semiconductor device forming method of this embodiment. The flow diagram of Fig. 14 is similar to the flow diagram of Fig. 12 except that a removing liquid is supplied to remove the filling layer and the partial filling layer, and a stripping liquid is supplied before the supply of the removing liquid, and therefore, to avoid redundancy, overlapping descriptions are omitted.
[0199] After the substrate W is heated in step S12c, a first remover liquid is supplied in step S13a. The first remover liquid supply unit 162 supplies the first remover liquid to the substrate W. For example, the first remover liquid supply unit 162 supplies DIW as the first remover liquid.
[0200] In step S13b, the second remover liquid is supplied. The second remover liquid supply unit 164 supplies the second remover liquid to the substrate W. For example, the second remover liquid supply unit 164 supplies SC1 as the second remover liquid.
[0201] In step S13c, a rinsing liquid is supplied. For example, the rinsing liquid supply unit 137 supplies the rinsing liquid to the upper surface Wa of the substrate W.
[0202] Thereafter, in step S14a, the filling layer F is partially dissolved by the removing liquid to form a partial filling layer Fp. The removing liquid supply unit 134 supplies the removing liquid to the substrate W for a predetermined period of time. The removing liquid Ds is applied to the filling layer F in the recess R, thereby partially dissolving the filling layer F to form a partial filling layer Fp in the recess R. By controlling the concentrations and processing times of the first remover liquid, the second remover liquid, and the removing liquid supplied by the first remover liquid supply unit 162, the second remover liquid supply unit 164, and the remover liquid supply unit 134, the partial filling layer Fp can be appropriately formed from the filling layer F.
[0203] Moreover, after the water repellent is supplied in step S16, a remover is supplied in step S18a to remove the water repellent P except for the coating layer Ps and the partial filling layer Fp. The subsequent processing is similar.
[0204] In the flow diagram shown in FIG. 14, the first and second stripping liquids are supplied before the filling layer F is partially dissolved by the removal liquid, but this embodiment is not limited to this. The first and second stripping liquids may be supplied not only before the filling layer F is partially dissolved, but also before the partial filling layer Fp is dissolved. Alternatively, the first and second stripping liquids may be supplied not only before the filling layer F is partially dissolved, but also before the partial filling layer Fp is dissolved.
[0205] 14, the first and second stripping liquids are supplied, but this embodiment is not limited to this. Only one of the first and second stripping liquids may be supplied before dissolving the filling layer F and / or the partial filling layer Fp.
[0206] In the above description with reference to Fig. 13 and Fig. 14, the filling layer F and / or the partial filling layer Fp are removed by a stripping solution and a removing solution, but this embodiment is not limited to this. The filling layer F and / or the partial filling layer Fp may be removed by heating.
[0207] Next, the semiconductor device forming method of this embodiment will be described with reference to Fig. 6, Fig. 15, and Fig. 16. Fig. 15 is a schematic diagram of a substrate processing apparatus 100 of this embodiment. The substrate processing apparatus 100 of Fig. 15 has a similar configuration to the substrate processing apparatus 100 shown in Fig. 11, except that the processing liquid contains a sublimable substance and the filling layer formed from the processing liquid is cooled, and therefore, to avoid redundancy, duplicated descriptions will be omitted.
[0208] In this embodiment, the processing liquid supply unit 132 supplies the processing liquid containing the sublimable substance to the upper surface Wa of the substrate W. When mixing the sublimable substance in a molten state, the solvent is preferably a solvent that is compatible with the sublimable substance in a molten state. When dissolving the sublimable substance as a solute, the solvent is preferably a solvent that is soluble in the sublimable substance.
[0209] The substrate processing apparatus 100 further includes a coolant supplying unit 144. The coolant supplying unit 144 supplies a coolant whose temperature is lower than room temperature to the substrate W. The coolant is, for example, DIW cooled to a temperature lower than room temperature.
[0210] The coolant supplied by the coolant supply unit 144 may be either liquid or gas. After the processing liquid supply unit 132 supplies the processing liquid to the upper surface Wa of the substrate W, the coolant supply unit 144 cools the substrate W held by the spin base 121 and the chuck member 122 from the back surface Wb side of the substrate W.
[0211] While the substrate W is rotating, the coolant supply unit 144 supplies the coolant toward the center position of the back surface Wb of the substrate W. The supplied coolant spreads over substantially the entire back surface Wb of the substrate W by the action of centrifugal force. As a result, the processing liquid on the substrate W and the upper surface Wa of the substrate W is cooled and solidified, and a filling layer can be quickly formed from the processing liquid.
[0212] The coolant supply unit 144 includes a pipe 144a and a valve 144b. A coolant is supplied to the pipe 144a from a supply source. The valve 144b opens and closes a flow path in the pipe 144a. The pipe 144a is connected to a pipe 140a of the heat medium supply unit 140. The coolant is supplied to the back surface Wb of the substrate W from a nozzle 140n of the heat medium supply unit 140.
[0213] The substrate processing apparatus 100 includes a heat medium supplying unit 140 in addition to the coolant supplying unit 144. The heat medium supplying unit 140 supplies the heat medium to the rear surface Wb of the substrate W until just before the coolant supplying unit 144 supplies the coolant to the rear surface Wb of the substrate W, whereby the filling layer F can be formed thin. This allows the internal stress generated in the filling layer F to be reduced.
[0214] Fig. 16 is a flow diagram of the semiconductor device forming method of this embodiment. The flow diagram of Fig. 16 is similar to the flow diagram of Fig. 8 except that the treatment liquid contains a sublimable substance and is heated when removing the partial filling layer, and therefore, to avoid redundancy, overlapping descriptions are omitted.
[0215] In step S12, a filling layer F is formed. The processing liquid supply unit 132 supplies a processing liquid to the substrate W. Here, the processing liquid contains a sublimable substance. The processing liquid supply unit 132 supplies the processing liquid containing a sublimable substance to the upper surface Wa of the substrate W.
[0216] When forming the filling layer F, the coolant supply unit 144 supplies the coolant to the back surface Wb of the substrate W. This causes the processing liquid to solidify and form the filling layer F. The coolant supplied to the back surface Wb of the substrate W spreads over substantially the entire back surface Wb of the substrate W due to the action of centrifugal force. This starts cooling the processing liquid on the upper surface Wa of the substrate W.
[0217] Furthermore, when removing the partial filling layer Fp in step S18b, the supply of the refrigerant by the refrigerant supply unit 144 is stopped, and the supply of the heat medium by the heat medium supply unit 140 is started. This causes the partial filling layer Fp to sublimate, and therefore the partial filling layer Fp can be removed.
[0218] Next, the method for forming a semiconductor device according to this embodiment will be described with reference to Figures 17 and 18. Figure 17 is a schematic diagram of a substrate processing apparatus 100 according to this embodiment. The substrate processing apparatus 100 in Figure 17 has the same configuration as the substrate processing apparatus 100 shown in Figure 2, except that it further includes an aqueous solution supply unit 200 and a heating mechanism 210, and therefore, redundant description will be omitted to avoid redundancy.
[0219] The aqueous solution supplying unit 200 supplies the aqueous solution to the upper surface Wa of the substrate W. The supplied aqueous solution comes into contact with the surface of the formed filling layer.
[0220] The aqueous solution may be an acidic aqueous solution, such as an aqueous solution containing acetic acid, formic acid, hydroxyacetic acid, or sulfonic acid.
[0221] The aqueous solution supply unit 200 includes a pipe 200a, a valve 200b, and a nozzle 200n. The nozzle 200n ejects the aqueous solution onto the upper surface Wa of the substrate W. The nozzle 200n is connected to the pipe 200a. The aqueous solution is supplied to the pipe 200a from a supply source. The valve 200b opens and closes a flow path in the pipe 200a. The nozzle 200n is preferably configured to be movable relative to the substrate W.
[0222] The substrate processing apparatus 100 further includes a heating mechanism 210. The heating mechanism 210 heats the substrate W. The heating mechanism 210 heats the substrate W when the recess R of the substrate W is filled with the filling layer F. Here, the heating mechanism 210 is disposed above the spin base 121.
[0223] The heating mechanism 210 can increase or decrease the energy applied to the substrate W by increasing or decreasing the power supplied to the heating mechanism 210. The amount of heat applied to the substrate W increases or decreases corresponding to the increase or decrease in energy. The heating mechanism 210 is in the form of a circular plate, and the diameter of the heating mechanism 210 is larger than the radius of the substrate W. Furthermore, when the heating mechanism 210 is used together with the shielding member 150, the diameter of the heating mechanism 210 may be smaller than the radius of the shielding plate 152 (FIG. 15). Due to this shape, the heating mechanism 210 can heat the entire substrate W uniformly.
[0224] The heating mechanism 210 has a heating unit. For example, the heating unit heats the filling layer with light or heat. The heating unit may be any of a heater, a lamp, and an LED, and is not limited to these as long as it has a heating function. The heating units may be uniformly arranged in a concentric or lattice pattern in the heating mechanism 210. With this arrangement, the heating mechanism 210 can uniformly heat the entire substrate W. Furthermore, the heating mechanism 210 may heat the substrate W surface differently depending on the region. For example, the heating mechanism 210 can separate the substrate W into a central portion, a middle portion, and an outer periphery in a triple concentric circle shape, and heat the central portion, the middle portion, and the outer periphery to different temperatures. Note that the regions separated as different temperature regions in the substrate W are not limited to concentric circles, and may be changed as appropriate.
[0225] While or after the processing liquid supply unit 132 supplies the processing liquid to the upper surface Wa of the substrate W, the heating mechanism 210 heats the substrate W held by the spin base 121 and the chuck member 122 from the back surface Wb side of the substrate W to form a filling layer on the upper surface Wa of the substrate W. The heating mechanism 210 has a lifting mechanism (not shown) and is spaced vertically downward from the substrate W, and moves up and down between a standby position where the lifting mechanism waits, a contact position where it contacts the substrate W, and an approach position between the standby position and the contact position.
[0226] Furthermore, while or after the aqueous solution supply unit 200 is supplying the aqueous solution to the upper surface Wa of the substrate W, the heating mechanism 210 heats the substrate W held by the spin base 121 and the chuck member 122 from the back surface Wb side of the substrate W to dissolve or modify a part of the filling layer F on the upper surface Wa of the substrate W. This may form a partial filling layer Fp on the upper surface Wa of the substrate W. The heating mechanism 210 has a lifting mechanism (not shown) and is separated vertically downward from the substrate W, and lifts and lowers between a standby position where the lifting mechanism waits, a contact position where it contacts the substrate W, and an approach position between the standby position and the contact position.
[0227] In this embodiment, the heating mechanism 210 heats the substrate W from the back surface Wb side of the substrate W, but the heating mechanism 210 may heat the substrate W from the top surface Wa side of the substrate W. In this case, the heating mechanism 210 moves vertically upward away from the substrate W and moves up and down between a standby position where the lifting mechanism waits, a contact position where the lifting mechanism contacts the substrate W, and an approach position between the standby position and the contact position.
[0228] While the substrate W is rotating, the heating mechanism 210 is moved from the standby position to the contact position by the lifting mechanism. The heating mechanism 210 may be stationary between the standby position and the contact position. Even if the heating mechanism 210 does not move from the standby position, the output of the heating mechanism 210 may be increased to increase the amount of heat.
[0229] Fig. 18 is a flow diagram of the semiconductor device forming method of the present embodiment. The flow diagram of Fig. 18 is similar to the flow diagram of Fig. 8 except that an aqueous solution is supplied to remove a part of the filling layer and heating is performed after the aqueous solution is supplied, and therefore, to avoid redundancy, overlapping descriptions are omitted.
[0230] In step S14, a portion of the filling layer F is removed. An aqueous solution is supplied to the filling layer F, the filling layer F in contact with the aqueous solution is heated, and then a removing liquid is applied to the filling layer F in the recess R, whereby the filling layer F is partially dissolved to form a partial filling layer Fp in the recess R. The partial removal of the filling layer F in step S14 includes supplying the aqueous solution in step S14b, heating in step S14c, and supplying the removing liquid in step S14d.
[0231] In step S14b, the aqueous solution is supplied from the aqueous solution supply unit 200 to the substrate W for a predetermined period of time. The aqueous solution comes into contact with the filling layer F in the recess R, and penetrates or permeates into the filling layer F.
[0232] In step S14c, the substrate W is heated for a predetermined period of time by the heating mechanism 210. The heating causes the acid contained in the filling layer F to diffuse, and the part of the filling layer F into which the acid has diffused is partially dissolved and / or denatured. At this time, a partial filling layer Fp may be formed in the recess R. By controlling the heating time and heating temperature by the heating mechanism 210, and the distance between the heating mechanism 210 and the substrate W, it is possible to control the region of the filling layer F to be removed, and it is possible to appropriately form a partial filling layer Fp by partially removing the part of the filling layer F located on the surface side of the filling layer F.
[0233] In step S14d, the removing liquid is supplied for a predetermined period of time from the removing liquid supply unit 134 to the substrate W. By applying the removing liquid to the region of the filling layer F into which the acid has diffused, the filling layer F is partially dissolved and a partial filling layer Fp is formed in the recess R.
[0234] The removal liquid for partially removing the portion located on the surface side of the filling layer F from the filling layer F may be the same as or different from the removal liquid for the partial filling layer Fp.
[0235] In the description with reference to Figs. 17 and 18, the substrate W during or after the aqueous solution is supplied is heated by a heating mechanism such as a lamp or an electric heater, but this embodiment is not limited to this. A heat medium supplying unit may be provided as a heating mechanism in the substrate processing apparatus 100, and the substrate W during or after the aqueous solution is supplied may be heated by using a heat medium supplied from the heat medium supplying unit. The heat medium may be, for example, heated high-temperature nitrogen (N 2 ) gas.
[0236] 1 to 18, the substrate processing apparatus 100 is of a single-wafer type and processes the substrates W one by one, but the present invention is not limited to this. The substrate processing apparatus may be of a batch type.
[0237] Next, the substrate processing apparatus 100 of this embodiment will be described with reference to Fig. 19. Fig. 19 is a schematic diagram of the substrate processing apparatus 100. The substrate processing apparatus 100 can process a plurality of substrates W collectively.
[0238] The substrate processing apparatus 100 includes a substrate holding unit 120 and a liquid supply unit 130. The liquid supply unit 130 includes a processing liquid supply unit 132, a removing liquid supply unit 134, a water repellent agent supply unit 136, and a chemical liquid supply unit 138. The processing liquid supply unit 132, the removing liquid supply unit 134, the water repellent agent supply unit 136, and the chemical liquid supply unit 138 each store a liquid.
[0239] The processing liquid supply unit 132 includes a processing liquid storage tank 132t. The processing liquid is stored in the processing liquid storage tank 132t. A filling layer is formed from the processing liquid. For example, the processing liquid includes a solute and a volatile solvent. Alternatively, the processing liquid includes a sublimable substance.
[0240] The removing liquid supply unit 134 includes a removing liquid storage tank 134t. The removing liquid storage tank 134t stores a removing liquid. The removing liquid can remove the filling layer formed from the processing liquid. By controlling the time for supplying the removing liquid, the filling layer can be selectively removed from the substrate W.
[0241] The removal liquid may be any solvent that dissolves any of the resins, such as organic solvents such as thinner, toluene, acetates, alcohols, and glycols, and acidic liquids such as acetic acid, formic acid, and hydroxyacetic acid.
[0242] The water repellent supply unit 136 includes a water repellent storage tank 136t. A liquid water repellent is stored in the water repellent storage tank 136t. A water repellent layer is formed on the substrate W by the water repellent. The water repellent is a water repellent that hydrophobicizes silicon (Si) itself and compounds containing silicon. The water repellent is, for example, a silane coupling agent. The silane coupling agent includes, for example, at least one of HMDS (hexamethyldisilazane), TMS (tetramethylsilane), fluorinated alkylchlorosilane, alkyldisilazane, and a non-chloro water repellent. The non-chloro water repellent includes, for example, at least one of dimethylsilyldimethylamine, dimethylsilyldiethylamine, hexamethyldisilazane, tetramethyldisilazane, bis(dimethylamino)dimethylsilane, N,N-dimethylaminotrimethylsilane, N-(trimethylsilyl)dimethylamine, and an organosilane compound.
[0243] The chemical supply unit 138 includes a chemical storage tank 138t. A chemical is stored in the chemical storage tank 138t. The chemical can be processed by a chemical process using the chemical. The chemical process can perform any one of etching, surface treatment, imparting properties, forming a processed film, and removing at least a part of a film on the substrate W. Typically, the chemical is an etching solution used in the etching process of the substrate W.
[0244] The chemical solution includes hydrofluoric acid. For example, the hydrofluoric acid may be heated to 40° C. or higher and 70° C. or lower, or may be heated to 50° C. or higher and 60° C. or lower. However, the hydrofluoric acid does not have to be heated. The chemical solution may also include water or phosphoric acid.
[0245] The chemical solution may further include hydrogen peroxide. The chemical solution may also include SC1 (ammonia hydrogen peroxide mixture), SC2 (hydrochloric acid hydrogen peroxide mixture), or aqua regia (a mixture of concentrated hydrochloric acid and concentrated nitric acid).
[0246] The substrate holding part 120 holds a substrate W. The normal direction of the main surface of the substrate W held by the substrate holding part 120 is parallel to the Y direction. The substrate holding part 120 moves the substrates W while holding a plurality of substrates W. For example, the substrate holding part 120 moves vertically upward or vertically downward while holding the substrates W. Alternatively, the substrate holding part 120 may move horizontally while holding the substrates W.
[0247] The substrate holding part 120 includes a main body plate 122b and a holding rod 124b. The main body plate 122b is a plate extending in the vertical direction (Z direction). The holding rod 124b extends in the horizontal direction (Y direction) from one main surface of the main body plate 122b. Here, two holding rods 124b extend in the Y direction from one main surface of the main body plate 122b. The multiple substrates W are arranged in the front-rear direction of the page, and the lower edge of each substrate W is abutted by the multiple holding rods 124b to be held in an upright position (vertical position).
[0248] The substrate processing apparatus 100 further includes a control device 101. The control device 101 includes a control unit 102 and a storage unit 104. The control unit 102 controls the substrate holding unit 120.
[0249] In the substrate processing apparatus 100 of this embodiment, the control unit 102 can adjust the diameter of the recess provided in the stack structure L of the substrate W by treating the substrate W held by the substrate holding unit 120 with different liquids, in the same manner as in the single-wafer processing system, as described with reference to Figures 6 to 16 for the single-wafer processing system.
[0250] 1 to 19, the memory element Se is disposed in the recess R of the substrate W, but this embodiment is not limited to this. A dummy memory element having a similar configuration to the memory element Se but not used as a memory element may be formed in the recess R of the substrate W. Alternatively, a contact plug for electrically connecting to the memory element Se may be formed in the recess R of the substrate W.
[0251] Next, a semiconductor element 300 formed by the semiconductor element forming method of the present embodiment will be described with reference to Fig. 20. Fig. 20 is a schematic diagram of the semiconductor element 300.
[0252] The semiconductor element 300 is provided with a plurality of recesses R. The recesses R include a memory recess Rs in which the memory element Se is disposed, and a contact recess Rc in which the contact plug Cp is disposed. The contact recess Rc is electrically connected to the conductive layer M.
[0253] According to the semiconductor element forming method of the present embodiment, the diameter of not only the memory recess Rs but also the contact recess Rc can be made uniform from the surface portion to the depth portion, so that the strength with which the contact recess Rc supports the semiconductor element can be made uniform.
[0254] The embodiments of the present invention have been described above with reference to the drawings. However, the present invention is not limited to the above embodiments, and can be implemented in various aspects without departing from the gist of the present invention. In addition, various inventions can be formed by appropriately combining multiple components disclosed in the above embodiments. For example, some components may be deleted from all components shown in the embodiments. Furthermore, components across different embodiments may be appropriately combined. The drawings are mainly shown schematically for ease of understanding, and the thickness, length, number, spacing, etc. of each component shown in the drawings may differ from the actual ones due to the convenience of drawing. In addition, the material, shape, dimensions, etc. of each component shown in the above embodiments are examples and are not particularly limited, and various changes are possible within a range that does not substantially deviate from the effects of the present invention. [Industrial Applicability]
[0255] The present invention can be suitably used in a semiconductor device forming method and a substrate processing apparatus. [Explanation of symbols]
[0256] 100 Substrate processing apparatus 110 Chamber 120 Board holding part 130 Liquid supply section 132 Processing liquid supply unit 134 Removal liquid supply section 136 Water repellent supply unit 138 Chemical Solution Supply Unit W substrate
Claims
1. forming a coating layer that selectively covers a portion of a recess located on a surface side of the recess provided in a laminate structure supported by a substrate; etching the deep portion of the recess with a chemical solution so as to increase the diameter of the portion of the recess that is deeper than the coating layer; Inclusive of The step of forming the coating layer includes: forming a filling layer to fill the recess; a step of forming the filling layer, and then heating the filling layer while the filling layer is in contact with an aqueous solution to partially remove a portion of the filling layer located on a surface side thereof, thereby forming a partial filling layer that partially fills a deep portion of the recess; supplying a water repellent agent after forming the partial filling layer; a step of supplying the water repellent agent to form the coating layer on the surface side of the recess, and then removing the partial filling layer and the water repellent agent; A method for forming a semiconductor device comprising the steps of:
2. 2. The method of claim 1, wherein the step of removing the partial filling layer includes the step of supplying a removing liquid to dissolve the partial filling layer.
3. 3. The method of claim 2, wherein the step of partially removing the filling layer includes the step of supplying a remover that removes the filling layer.
4. 4. The method of claim 1, wherein in the etching step, the chemical solution contains any one of hydrofluoric acid, water, and phosphoric acid.
5. The method of claim 1 , wherein a plurality of memory elements are formed in the recess.
6. The laminated structure has a plurality of recesses as the recess, 6. The method of claim 1, wherein a difference in top diameter between the recesses is 5% or less.
7. The method for forming a semiconductor device according to claim 1 , further comprising the step of: providing an etching stop layer between the substrate and the laminated structure.
8. 8. The method for forming a semiconductor device according to claim 1, wherein an acidic aqueous solution is supplied as the aqueous solution in the step of forming the partial filling layer.
9. a processing liquid supply unit that supplies a processing liquid; a water repellent supply unit for supplying a water repellent; A chemical supply unit that supplies a chemical; an aqueous solution supply unit for supplying an aqueous solution; a heating mechanism for heating the packed bed formed from the treatment liquid; a control unit that controls the treatment liquid supply unit, the water repellent agent supply unit, the chemical liquid supply unit, the aqueous solution supply unit, and the heating mechanism; Equipped with The control unit is (1) supplying the treatment liquid to form a filling layer that fills a recess provided in a laminate structure supported by a substrate; (2) After the filling layer is formed, the filling layer is heated by the heating mechanism while being in contact with the aqueous solution supplied from the aqueous solution supply unit, thereby partially removing a portion of the filling layer located on the surface side, and forming a partial filling layer that partially fills a deep portion of the recess; (3) supplying the water repellent to form a coating layer that selectively covers a portion of the recess that is located on the surface side and is not covered by the partial filling layer; (4) Supplying the chemical solution to increase the diameter of a portion of the recess deeper than the coating layer; the processing liquid supply unit, the water repellent agent supply unit, the chemical liquid supply unit, the aqueous solution supply unit, and the heating mechanism are controlled in such a manner as described above.
10. The substrate processing apparatus according to claim 9 , wherein the heating mechanism heats the filling layer with heat or light.
11. The substrate processing apparatus according to claim 9 , wherein the heating mechanism includes a heater.
12. The substrate processing apparatus according to claim 9 , wherein the heating mechanism includes a lamp.
13. The heating mechanism includes a heat medium supply unit that supplies a heat medium, The substrate processing apparatus according to claim 9 , wherein the heat medium includes heated nitrogen gas.
14. The substrate processing apparatus according to claim 9 , wherein the aqueous solution supply unit supplies an acidic aqueous solution as the aqueous solution.
Citation Information
Patent Citations
Semiconductor device and its manufacture
JP2000223563A
Method for fabricating deep trench capacitor storage electrode
JP2001144265A
Method of manufacturing semiconductor device, and the semiconductor device
JP2011159760A
Semiconductor device and manufacturing method of the same
JP2012174790A
Semiconductor storage device
JP2019117894A