Electrode manufacturing method and all-solid-state battery manufacturing method

The method of using hardened electrode materials with dispersion promoting components addresses the short pot life issue in bulk type all-solid-state batteries, enhancing productivity and slurry formation efficiency.

JP7578645B2Active Publication Date: 2024-11-06TOYOTA JIDOSHA KK +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022105794
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-06-30
Publication Date
2024-11-06
Estimated Expiration
2042-06-30

AI Technical Summary

Technical Problem

Bulk type all-solid-state batteries face challenges in mass production due to the short pot life of slurry containing a large amount of liquid, leading to solids settlement and difficulty in regenerating a homogeneous slurry, and the need for hard kneading which is labor-intensive.

Method used

A method involving the preparation of hardened electrode materials with a dispersion promoting component, such as a styrene-butadiene rubber binder or imidazoline compound, to facilitate easy slurry formation after storage, using a solvent like tetralin to maintain stability during storage.

Benefits of technology

Improves productivity by allowing for easier and faster slurry formation post-storage, maintaining homogeneity, and reducing the need for extensive manual labor in the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578645000003
    Figure 0007578645000003
  • Figure 0007578645000004
    Figure 0007578645000004
  • Figure 0007578645000001
    Figure 0007578645000001
Patent Text Reader

Abstract

To improve the productivity.SOLUTION: A first electrode material is prepared by kneading an active material, a solid electrolyte, and a solvent. A second electrode material is prepared by adding a dispersion promoting component to the first electrode material. A slurry containing a second electrode material is provided. An electrode is manufactured by applying the slurry to the surface of a base material. A composite is formed by adhering the solid electrolyte to the surface of the active material. The dispersion promoting component promotes the dispersion of the solid electrolyte in the solvent.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing an electrode and a method for producing an all-solid-state battery. [Background technology]

[0002] JP 2020-053307 A discloses preparing a paste by adding a solvent to a kneaded electrode material. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-053307 A Summary of the Invention [Problem to be solved by the invention]

[0004] Bulk-type all-solid-state batteries are being studied. Bulk-type all-solid-state batteries can be manufactured by stacking powder layers. A wet process is a promising method for forming the powder layer. In the wet process, a slurry containing an active material, a solid electrolyte, and the like is prepared. The slurry is applied to the surface of a substrate to manufacture a powder layer (electrode).

[0005] In mass production, it may be necessary to temporarily store the electrode work-in-progress. For example, it is possible to store the slurry. However, since the slurry contains a large amount of liquid, the pot life tends to be short. That is, the solids may settle in a relatively short time. If the settled solids harden, it is difficult to regenerate the slurry.

[0006] Usually, slurries are produced through kneading and dilution. "Kneading" refers to the process of kneading a fluid that is as hard as a solid. In kneading, materials are mixed in a state where the solid content is high. In kneading, a large shear force is generated, which can break down the agglomeration of powder. By breaking down the agglomeration of powder, it is expected that different types of powder will be well dispersed and mixed together.

[0007] Hereinafter, the work-in-process after kneading is also referred to as "kneaded material". The kneaded material can be diluted with a solvent (liquid) and stirred to form a slurry. For example, it is possible to store the kneaded material. Kneaded materials tend to have a longer pot life than slurries. Kneading is an operation that requires many steps. By preparing and storing a large amount of kneaded material and diluting it to produce a slurry as needed, it is expected that productivity will improve.

[0008] In a thick kneaded material, liquid is held between the solid particles. During storage, the liquid may seep out over time, causing the solid particles to adhere tightly to each other. In other words, the solid and the liquid may separate. If the solid and the liquid separate, it is difficult to form a homogeneous slurry in a short time.

[0009] The objective of the present disclosure is to improve productivity. [Means for solving the problem]

[0010] The technical configuration and effects of the present disclosure will be described below. However, the mechanism of action in this specification includes assumptions. The mechanism of action does not limit the technical scope of the present disclosure.

[0011] 1. A method for producing an electrode includes the following steps (a) to (d): (a) A first electrode material is prepared by kneading an active material, a solid electrolyte, and a solvent. (b) preparing a second electrode material by adding a dispersion promoting component to the first electrode material; (c) preparing a slurry containing a second electrode material; (d) The slurry is applied to the surface of a substrate to produce an electrode. In the above (a), the solid electrolyte is attached to the surface of the active material to form a composite. The dispersion-promoting component promotes the dispersion of the solid electrolyte in the solvent.

[0012] The first electrode material and the second electrode material are in-process products after being thick-kneaded, that is, the first electrode material and the second electrode material are thick-kneaded materials.

[0013] According to the new findings of the present disclosure, the addition of a specific component to the kneaded material can facilitate the formation of a slurry after storage. That is, a dispersion-promoting component is added to the kneaded material. The dispersion-promoting component can promote the dispersion of the solid electrolyte in the solvent. The solid electrolyte and the active material form a complex. It is expected that the action of the dispersion-promoting component promotes the dispersion of the complex, and a homogeneous slurry can be formed in a short time.

[0014] 2. In the method for producing an electrode according to the above item "1," (b) may include storing the second electrode material.

[0015] The second electrode material to which the dispersion promoting component has been added is suitable for storage because it is easy to form a slurry even after storage.

[0016] 3. In the method for producing an electrode according to the above item "1" or "2," the solid electrolyte may include, for example, a sulfide solid electrolyte, and the dispersion-promoting component may include, for example, a styrene-butadiene rubber-based binder.

[0017] Hereinafter, "solid electrolyte" may be abbreviated as "SE". For example, sulfide solid electrolyte may be abbreviated as "sulfide SE". Sulfide SE has both high ionic conductivity and excellent moldability. Sulfide SE is suitable for bulk-type all-solid-state batteries. Styrene butadiene (SBR)-based binders may promote the dispersion of sulfide SE.

[0018] 4. In the method for producing an electrode according to any one of the above items 1 to 3, the solid electrolyte may include, for example, a sulfide solid electrolyte, and the dispersion-promoting component may include, for example, an imidazoline-based compound.

[0019] The imidazoline-based compound can act as a dispersant for the solid content of the slurry, and can impart good dispersibility to the sulfide SE in particular.

[0020] 5. In the method for producing an electrode according to any one of the above items 1 to 4, the solid electrolyte may include, for example, a sulfide solid electrolyte, and the solvent may include, for example, tetralin.

[0021] Tetralin is also written as 1,2,3,4-Tetrahydronaphthalene (THN). THN tends to be less likely to degrade sulfides SE. Furthermore, THN can have a high viscosity. When a solvent contains THN, it tends to be less likely to separate into solid and liquid forms during storage.

[0022] 6. A method for producing an all-solid-state battery includes the following (e): (e) An all-solid-state battery is manufactured, the battery including the electrode according to any one of the above items "1" to "5".

[0023] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the present embodiment do not limit the technical scope of the present disclosure. The present embodiment and the present embodiment are illustrative in all respects. The present embodiment and the present embodiment are non-restrictive. The technical scope of the present disclosure encompasses all modifications within the meaning and scope equivalent to the description of the claims. For example, it is originally intended that any configuration may be extracted from the present embodiment and the present embodiment, and that they may be arbitrarily combined. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 is a schematic flow chart of the manufacturing method according to the present embodiment. [Diagram 2] FIG. 2 is a conceptual diagram of the all-solid-state battery in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] <Terms and definitions> The words "comprise," "include," "have," and variations thereof (e.g., "consisting of") are open-ended. The open-ended form may or may not include additional elements in addition to the required elements. The words "consisting of" are closed-ended. However, the closed form does not exclude additional elements that are normally associated with the technology or that are unrelated to the technology disclosed. The words "consisting essentially of..." are semi-closed. The semi-closed form allows for the addition of elements that do not substantially affect the basic and novel characteristics of the technology disclosed.

[0026] "At least one of A and B" includes "A or B" as well as "A and B." "At least one of A and B" can also be written as "A and / or B."

[0027] Expressions such as "may" and "may" are used in the permissive sense, meaning "to have the possibility," rather than in the obligatory sense, meaning "to have to."

[0028] Unless otherwise specified, the order of execution of the steps, operations, and the like included in various methods is not limited to the order described. For example, the steps may proceed simultaneously. For example, the steps may be performed in sequence.

[0029] Elements expressed in the singular form include the plural form unless otherwise specified. For example, a "particle" can mean not only "one particle" but also "an aggregate of particles (powder, powder, particle group)."

[0030] For example, a numerical range such as "m to n%" includes an upper limit and a lower limit. That is, "m to n%" indicates a numerical range of "m% or more and n% or less." Furthermore, "m% or more and n% or less" includes "more than m% and less than n%." Furthermore, a numerical value arbitrarily selected from within the numerical range may be set as a new upper limit or lower limit. For example, a new numerical range may be set by arbitrarily combining a numerical value within the numerical range with a numerical value described in another part of this specification, in a table, in a figure, or the like.

[0031] All numerical values ​​are modified by the term "about." The term "about" may mean, for example, ±5%, ±3%, ±1%, etc. All numerical values ​​may be approximations that may vary depending on the application of the disclosed technology. All numerical values ​​may be expressed with significant figures. Measurements may be average values ​​of multiple measurements. The number of measurements may be three or more, five or more, or ten or more. In general, the more measurements are taken, the more reliable the average value is expected to be. Measurements may be rounded off based on the number of significant figures. Measurements may include errors associated with, for example, the detection limits of the measuring device.

[0032] When a compound is expressed by a stoichiometric composition formula (e.g., "LiCoO2", etc.), the stoichiometric composition formula is merely a representative example of the compound. The compound may have a non-stoichiometric composition. For example, when lithium cobalt oxide is expressed as "LiCoO2", unless otherwise specified, the lithium cobalt oxide is not limited to the composition ratio of "Li / Co / O=1 / 1 / 2" and may contain Li, Co, and O in any composition ratio. Furthermore, doping, substitution, etc. with trace elements may also be allowed.

[0033] "Semi-metals" include B, Si, Ge, As, Sb, and Te. "Metals" refers to elements from Groups 1 to 16 of the periodic table, other than "H, B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se." When an inorganic compound contains at least one of a semi-metal and a metal and F, the semi-metal and the metal may have a positive (+) oxidation number.

[0034] "Electrode" is a general term for a positive electrode or a negative electrode. The electrode may be a positive electrode or a negative electrode.

[0035] A "hollow particle" refers to a particle in which the area of ​​the cavity in the center is 30% or more of the cross-sectional area of ​​the entire particle in a cross-sectional image of the particle (e.g., a cross-sectional SEM image, etc.). A "solid particle" refers to a particle in which the area of ​​the cavity in the center is less than 30% of the cross-sectional area of ​​the entire particle in a cross-sectional image of the particle.

[0036] "D50" refers to the particle size at which the cumulative frequency of the smaller particle sizes reaches 50% in a volume-based particle size distribution. D50 can be measured using a laser diffraction particle size distribution analyzer.

[0037] The "average Feret diameter" is measured in a two-dimensional image of a particle (e.g., a SEM image, etc.). The arithmetic mean of the maximum Feret diameters of 20 or more particles is the "average Feret diameter".

[0038] "Solid content concentration" refers to the ratio of the total mass of the components other than the solvent to the total mass of the mixture. The solid content concentration is expressed as a percentage.

[0039] <Manufacturing method> FIG. 1 is a schematic flow chart of the manufacturing method according to the present embodiment. Hereinafter, the "manufacturing method in this embodiment" may be abbreviated as "this manufacturing method." This manufacturing method includes "an electrode manufacturing method" and "an all-solid-state battery manufacturing method." The electrode manufacturing method includes "(a) thick kneading," "(b) addition of a dispersion-promoting component," "(c) preparation of a slurry," and "(d) manufacturing of an electrode." The all-solid-state battery manufacturing method further includes "(e) manufacturing of an all-solid-state battery" in addition to (a) to (d).

[0040] (a) Thick kneading The method includes preparing a first electrode material by kneading a mixture of an active material, a solid electrolyte, and a solvent.

[0041] The kneading may be performed by any mixing device. For example, a rotation-revolution mixer, a kneader, or the like may be used. These devices may be suitable for the kneading operation (kneading operation). For example, in a kneader, the contents are kneaded while compressive and shear forces are applied to the contents in the gap between the inner wall of the mixing vessel and the blade. For example, a planetary mixer, or the like may be used.

[0042] For example, the active material and SE are supplied to the mixing device in a predetermined blending amount. Furthermore, a solvent is added so as to obtain a predetermined solid content concentration. The solid content concentration in the kneading may be, for example, 72% or more. When the solid content concentration is 72% or more, the solvent is easily retained inside the powder, and kneading tends to be easy to carry out. The solid content concentration may be, for example, 74% or more, 75.5%, 76% or more, or 78% or more. When the solid content concentration is 76% or more, the solid and liquid are less likely to separate during mixing, and kneading tends to be easy to stabilize. The solid content concentration in the kneading may be, for example, 90% or less. When the solid content concentration is 90% or less, the mixture is easily moistened, and kneading tends to be easy to stabilize. The solid content concentration may be, for example, 88% or less, 85% or less, 83% or less, or 82% or less. The solid content concentration may be, for example, 76 to 83%. Within this range, dispersion tends to be easily promoted. By promoting dispersion, for example, it is expected that output will be improved.

[0043] The kneading may be performed so that the active material and the SE are uniformly mixed. The kneading treatment time may be, for example, 0.5 hours or more, 1 hour or more, 2 hours or more, or 3 hours or more. The kneading treatment time may be, for example, 8 hours or less, or 4 hours or less. If the kneading is not stable, for example, the solid and the liquid may separate during the treatment, and therefore, sufficient treatment time may not be ensured. If the treatment time is not sufficient, a uniform dispersion state may not be achieved.

[0044] A first electrode material is formed by kneading. The first electrode material is in a wet state. The first electrode material may be, for example, in the form of granules, powder, clay, etc. The first electrode material includes a complex.

[0045] (Complex) The composite is formed by attaching the SE to the surface of the active material. For example, the active material may be coated with the SE. For example, the SE may cover a part of the surface of the active material. For example, the SE may cover the entire surface of the active material.

[0046] (active material) The active material is particulate. The active material may be, for example, secondary particles. The secondary particles are an aggregate of primary particles. The D50 of the secondary particles may be, for example, 1 to 30 μm, 3 to 20 μm, or 5 to 15 μm. The average Feret diameter of the primary particles may be, for example, 0.01 to 3 μm.

[0047] The active material may have any shape. For example, the active material may be spherical, ellipsoidal, flaky, fibrous, etc. The active material may be solid or hollow particles.

[0048] The active material can cause an electrode reaction. The active material may be, for example, a positive electrode active material. The positive electrode active material may contain any component. The positive electrode active material may contain, for example, at least one selected from the group consisting of LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(NiCoMn)O2, Li(NiCoAl)O2, Li(NiCoMnAl)O2, and LiFePO4. For example, "(NiCoMn)" in "Li(NiCoMn)O2" indicates that the sum of the composition ratios in parentheses is 1. As long as the sum is 1, the amount of each component is arbitrary. Li(NiCoMn)O2 is, for example, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.4 Co 0.3 Mn 0.3 O2, LiNi 0.5 Co 0.2 Mn0.3 O2, LiNi 0.5 Co 0.3 Mn 0.2 O2, LiNi 0.5 Co 0.4 Mn 0.1 O2, LiNi 0.5 Co 0.1 Mn 0.4 O2, LiNi 0.6 Co 0.2 Mn 0.2 O 2、 LiNi 0.6 Co 0.3 Mn 0.1 O 2、 LiNi 0.6 Co 0.1 Mn 0.3 O 2、 LiNi 0.7 Co 0.1 Mn 0.2 O 2、 LiNi 0.7 Co 0.2 Mn 0.1 O 2、 LiNi 0.8 Co 0.1 Mn 0.1 O 2、 and LiNi 0.9 Co 0.05 Mn 0.05 Li(NiCoAl)O2 may contain at least one selected from the group consisting of LiNi 0.8 Co 0.15 Al 0.05 It may contain O2 etc.

[0049] The positive electrode active material may be represented, for example, by the following formula (1). Li 1-y Ni x M 1-x O2…(1) 0.5≦x≦1 -0.5≦y≦0.5 In the above formula (1), M may include at least one selected from the group consisting of Co, Mn, and Al, and x may be, for example, 0.6 or more, 0.7 or more, 0.8 or more, or 0.9 or more.

[0050] The positive electrode active material may contain additives, for example. The additives may be, for example, substitutional solid solution atoms or interstitial solid solution atoms. The additives may be deposits adhering to the surface of the positive electrode active material (primary particles). The deposits may be, for example, simple substances, oxides, carbides, nitrides, halides, etc. The addition amount may be, for example, 0.01 to 0.1, 0.02 to 0.08, or 0.04 to 0.06. The addition amount indicates the ratio of the amount of the additive to the amount of the positive electrode active material [unit: mol]. The additives may contain at least one selected from the group consisting of B, C, N, halogens, Sc, Ti, V, Cu, Zn, Ga, Ge, Se, Sr, Y, Zr, Nb, Mo, In, Sn, W, and lanthanoids.

[0051] The active material may be, for example, a negative electrode active material. The negative electrode active material may contain any components. The negative electrode active material may be, for example, natural graphite, artificial graphite, soft carbon, hard carbon, Si, SiO x (0 < x < 2), Si-based alloys, Sn, SnO x (0 < x < 2), Li, Li-based alloys, and Li4Ti5O 12 and may contain at least one selected from the group consisting of. SiO x (0 < x < 2) may be doped with, for example, Mg or the like. A composite material may be formed by supporting an alloy-based active material (such as Si, etc.) on a carbon-based active material (such as graphite, etc.).

[0052] (Buffer layer) A buffer layer may be formed on the surface of the active material. The buffer layer covers at least a part of the surface of the active material. Sulfide SE tends to deteriorate when in direct contact with the active material. The buffer layer can reduce the direct contact between the active material and the sulfide SE. The buffer layer may have a thickness of, for example, 5 to 500 nm. The buffer layer may be formed, for example, by a mechanochemical treatment. As an example of a mechanochemical treatment apparatus, for example, "Nobilta NOB-MINI" manufactured by Hosokawa Micron Corporation, etc. can be mentioned.

[0053] (Oxide solid electrolyte) The buffer layer may contain, for example, an oxide SE. The buffer layer may contain, for example, LiNbO3, Li3PO4, etc.

[0054] (Fluoride solid electrolyte) The buffer layer may contain, for example, a fluoride SE. The fluoride SE tends to have a less increase in reaction resistance during durability compared to the oxide SE. The fluoride SE can have any composition as long as it contains F. The fluoride SE may contain, for example, Li and F.

[0055] The fluoride SE may be represented by, for example, the following formula (2). Li 6-nx M x F6…(2) In the above formula (2), x satisfies 0 < x < 2. M is at least one selected from the group consisting of a semi-metal atom and a metal atom other than Li. n indicates the oxidation number of M.

[0056] In the above formula (2), M may consist of a single atom or a plurality of types of atoms. When M consists of a plurality of types of atoms, n indicates the weighted average of the oxidation numbers of each atom. For example, when M contains Ti (oxidation number = +4) and Al (oxidation number = +3), the molar ratio of Ti to Al is "Ti / Al = 3 / 7", and x = 1, n becomes 3.3 according to the formula "n = 0.3×4 + 0.7×3".

[0057] In the above formula (2), x may satisfy, for example, 0.1 ≦ x ≦ 1.9, 0.2 ≦ x ≦ 1.8, 0.3 ≦ x ≦ 1.7, 0.4 ≦ x ≦ 1.6, 0.5 ≦ x ≦ 1.5, 0.6 ≦ x ≦ 1.4, 0.7 ≦ x ≦ 1.3, 0.8 ≦ x ≦ 1.2, or 0.9 ≦ x ≦ 1.1.

[0058] M may contain, for example, an atom having an oxidation number of +4. M may contain, for example, an atom having an oxidation number of +3. M may contain, for example, an atom having an oxidation number of +4 and an atom having an oxidation number of +3.

[0059] In the above formula (2), M may, for example, include at least one selected from the group consisting of Ca, Mg, Al, Y, Ti, and Zr. M may, for example, include at least one selected from the group consisting of Al, Y, and Ti. M may, for example, include at least one selected from the group consisting of Al and Ti.

[0060] The fluoride SE may be represented, for example, by the following formula (3): Li 3-x Ti x Al 1-x F6…(3) In the above formula (3), x may satisfy, for example, 0≦x≦1, 0.1≦x≦0.9, 0.2≦x≦0.8, 0.3≦x≦0.7, or 0.4≦x≦0.6.

[0061] (solid electrolyte) The SE is particulate. The SE may have a smaller D50 than the active material. The SE may have a D50 of, for example, 0.01 to 1 μm, 0.01 to 0.95 μm, or 0.1 to 0.9 μm. The amount of SE to be blended is arbitrary. For example, the amount of SE may be 1 to 10 parts by mass per 100 parts by mass of the active material. The SE may include, for example, at least one selected from the group consisting of sulfide SE, fluoride SE, and oxide SE.

[0062] (Sulfide solid electrolyte) The sulfide SE may exhibit high ionic conductivity. The sulfide SE may have any composition as long as it contains S (sulfur). The sulfide SE may contain, for example, Li, P, and S. The sulfide SE may further contain, for example, O, Ge, Si, etc. The sulfide SE may further contain, for example, halogens, etc. The sulfide SE may further contain, for example, I, Br, etc. The sulfide SE may be, for example, a glass ceramic type or an argyrodite type. Sulfides SE include, for example, LiI-LiBr-Li3PS4, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2O-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-GeS2-P2S5, Li2S-P2S5, Li4P2S6, Li7P3S 11 and Li3PS4.

[0063] For example, "LiI-LiBr-Li3PS4" indicates a sulfide SE produced by mixing LiI, LiBr, and Li3PS4 in any molar ratio. For example, the sulfide SE may be produced by a mechanochemical method. "Li2S-P2S5" includes Li3PS4. Li3PS4 may be produced, for example, by mixing Li2S and P2S5 in "Li2S / P2S5=75 / 25 (molar ratio)". The molar ratio may be specified by adding a number before LiI, etc. For example, "10LiI-15LiBr-75Li3PS4" indicates that LiI / LiBr / Li3PS4 are mixed in "10 / 15 / 75 (molar ratio)".

[0064] (solvent) The solvent is a liquid. The solvent can promote adhesion between the active material and the sulfide SE during kneading. The solvent can function as a dispersion medium in the slurry. The solvent can contain any component. The solvent may contain at least one selected from the group consisting of aromatic hydrocarbons, esters, alcohols, ketones, and lactams. The solvent may contain at least one selected from the group consisting of THN, butyl butyrate, heptane, and N-methyl-2-pyrrolidone (NMP).

[0065] Butyl butyrate is expected to be less likely to degrade sulfide SE than, for example, NMP, etc. THN is expected to be less likely to degrade sulfide SE than, for example, butyl butyrate and NMP, etc. By including THN in the solvent, for example, it is expected to reduce initial resistance.

[0066] Furthermore, THN can have a high viscosity. It is expected that the solvent containing THN will be less likely to separate into solid and liquid forms during storage.

[0067] (b) Addition of Dispersion-Promoting Components The method includes providing a second electrode material by adding a dispersion enhancing component to a first electrode material.

[0068] The second electrode material is formed by adding a dispersion promoting component to the first electrode material. After the second electrode material is formed, the second electrode material may be lightly stirred. The second electrode material may be, for example, in the form of granules, powder, clay, liquid, etc. The solid content concentration of the second electrode material may be, for example, 50 to 80%, 60 to 80%, 70 to 80%, 72 to 78.5%, or 75 to 78.5%.

[0069] (Dispersion promoting component) The dispersion-promoting component can promote the dispersion of the SE in the solvent. The dispersion-promoting component can include any component as long as the dispersion of the SE can be promoted. The dispersion-promoting component may include, for example, at least one selected from the group consisting of an imidazoline-based compound and an SBR-based binder.

[0070] (Imidazoline compounds) The dispersion-promoting component may include, for example, an imidazoline-based compound. The imidazoline-based compound may impart good dispersibility, particularly to sulfide SE. The imidazoline-based compound has an imidazoline skeleton. The imidazoline skeleton includes a nitrogen-containing heterocyclic structure. The imidazoline skeleton may be derived from imidazole. The imidazoline-based compound may be represented, for example, by the following formula (4).

[0071] [ka]

[0072] In the above formula (4), R 1 R may be, for example, an alkyl group or a hydroxyalkyl group. 1 may have, for example, a carbon number of 1 to 22. In the hydroxyalkyl group, for example, a hydroxyl group may be bonded to the terminal carbon atom opposite to the carbon atom bonded to N (nitrogen atom).

[0073] In the above formula (4), R 2 R may be, for example, an alkyl or alkenyl group. 2 may have, for example, a carbon number of 10 to 22. In the alkenyl group, the position and number of double bonds are optional.

[0074] The imidazoline compound may include, for example, 1-hydroxyethyl-2-alkenylimidazoline, etc. The dispersion-promoting component may include one type of imidazoline compound alone, or may include two or more types of imidazoline compounds.

[0075] The amount of the imidazoline-based compound blended is arbitrary. For example, the amount of the imidazoline-based compound blended per 100 parts by mass of the active material may be 0.01 to 10 parts by mass, 0.05 to 5 parts by mass, or 0.05 to 0.1 parts by mass.

[0076] (SBR binder) The dispersion-promoting component may include an SBR-based binder. The SBR-based binder may impart dispersibility to the sulfide SE. "SBR-based binder" refers to a binder that includes an SBR-derived component. The SBR-based binder may be made of SBR. The SBR-based binder may be a copolymer of an SBR-derived component and other components. The SBR-based binder may be a polymer blend of an SBR-derived component and other components. The SBR-based binder may be a polymer alloy of an SBR-derived component and other components. The SBR-based binder may include, for example, 10% or more of an SBR-derived component, 30% or more of an SBR-derived component, 50% or more of an SBR-derived component, 70% or more of an SBR-derived component, or 90% or more of an SBR-derived component, by mass fraction.

[0077] The SBR binder may have thermoplastic properties. The SBR binder may have a softening point suitable for hot press processing. When an electrode containing the SBR binder is subjected to hot press processing, the SBR binder may be liquefied and then resolidified. As a result, the electrode is expected to become dense. When the electrode is dense, the battery characteristics (e.g., input / output characteristics, etc.) are expected to be improved.

[0078] The affinity between various materials can be evaluated by the distance (Ra) in the Hansen space. The "Hansen space" is a three-dimensional space represented by the Hansen solubility parameter (HSP). In the Hansen space, the smaller the distance (Ra) between two materials, the higher the affinity between the two materials is considered to be. The distance (Ra) between the sulfide SE and the imidazoline compound is smaller than the distance (Ra) between the sulfide SE and the SBR binder. When the dispersion-promoting component contains both the imidazoline compound and the SBR binder, the imidazoline compound can be preferentially adsorbed to the sulfide SE compared to the SBR binder, and it is expected that the imidazoline compound and the SBR binder will act synergistically to enhance the dispersion effect.

[0079] For example, the distance between the sulfide SE and the fluorine-based binder (such as PVDF) tends to be small. When an imidazoline compound and a fluorine-based binder coexist, the fluorine-based binder may preferentially adsorb to the sulfide SE. As a result, a synergistic dispersion effect may not be obtained. However, any binder may be used as long as the dispersion effect of the dispersion-promoting component is obtained. An example of calculating the distance in the Hansen space is shown below.

[0080] Distance between sulfide SE and imidazoline compound (Ra) = 10.7 MPa 0.5 Distance between sulfide SE and SBR binder (Ra) = 11.6 MPa 0.5 Distance between sulfide SE and fluorine-based binder (Ra) = 3.8 MPa 0.5

[0081] The amount of the SBR binder to be added is arbitrary. For example, the amount of the SBR binder to be added may be 0.1 to 5 parts by mass, or 1 to 3 parts by mass, per 100 parts by mass of the active material.

[0082] (Addition of solvent) A solvent may be added to the second electrode material. It is expected that the interaction between the additional solvent and the dispersion promoting component will facilitate subsequent slurry formation. For example, THN may be added to the second electrode material.

[0083] (storage) The manufacturing method may include storing the second electrode material. The second electrode material may be stored, for example, indoors. The storage temperature may be, for example, 25±10° C. The relative humidity of the storage location may be, for example, 50% or less. The storage period may be, for example, 1 day or more, 3 days or more, 7 days or more, 14 days or more, or 21 days or more. The storage period may be, for example, 28 days or less, or 21 days or less. The high degree of freedom in the storage period is expected to improve productivity.

[0084] The second electrode material may be stored in a container. Storage in a container is expected to facilitate management of the storage environment (e.g., the surrounding atmosphere). The storage container may be made of a material that does not deteriorate upon contact with the second electrode material. Examples of deterioration include dissolution, swelling, and decomposition. The storage container may contain at least one material selected from the group consisting of glass materials, metal materials (e.g., aluminum, stainless steel, etc.), resin materials, and carbon materials (e.g., carbon fibers, etc.).

[0085] The storage container may be sealed. The second electrode material includes a liquid. By sealing the storage container, a change in composition due to volatilization of the liquid can be reduced.

[0086] The storage container may have a low dew point atmosphere. The second electrode material may include a sulfide SE. The low dew point atmosphere in the storage container may reduce deterioration of the sulfide SE due to moisture. The dew point in the storage container may be, for example, −30° C. or lower, −40° C. or lower, or −60° C. or lower. The lower the dew point, the less deterioration of the sulfide SE is expected.

[0087] (c) Preparation of slurry The present manufacturing method includes preparing a slurry containing a second electrode material. For example, the second electrode material may be subjected to a dispersion treatment to form the slurry. In the present manufacturing method, any dispersion device may be used. For example, an ultrasonic homogenizer or the like may be used. During the dispersion treatment, a solvent may be added. The final solid content concentration of the slurry may be, for example, 50 to 70%, 50 to 60%, or 60 to 70%. During the dispersion treatment, an electronic conductive material or an ion conductive material may be added.

[0088] (Electronic Conductive Material) The electronic conductive material can form an electronic conductive path in the electrode. The amount of the electronic conductive material is arbitrary. The amount of the electronic conductive material may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the active material. The electronic conductive material may contain any component. The electronic conductive material may contain, for example, at least one selected from the group consisting of carbon black (CB), vapor grown carbon fiber (VGCF), carbon nanotube (CNT) and graphene flake (GF). The CB may contain, for example, at least one selected from the group consisting of acetylene black (AB), Ketjen Black (registered trademark), and furnace black.

[0089] (Ion Conductive Material) The ion conductive material can form an ion conductive path in the electrode. The ion conductive material may be particulate. The ion conductive material may have a D50 of, for example, 0.01 to 1 μm, 0.01 to 0.95 μm, or 0.1 to 0.9 μm. The amount of the ion conductive material is arbitrary. The amount of the ion conductive material may be, for example, 1 to 200 parts by volume, 50 to 150 parts by volume, or 50 to 100 parts by volume, relative to 100 parts by volume of the active material. The ion conductive material may contain, for example, a sulfide SE, a fluoride SE, or the like. The sulfide SE and fluoride SE contained in the ion conductive material may be the same type as or different from the sulfide SE and fluoride SE contained in the second electrode material.

[0090] (d) Manufacture of electrodes The method includes applying the slurry to a surface of a substrate to produce an electrode. Any coating device may be used in the method. For example, a die coater, a roll coater, or the like may be used.

[0091] The substrate may be conductive. The substrate may function as a current collector. The substrate may be, for example, sheet-like or mesh-like. The substrate may have a thickness of, for example, 5 to 50 μm. The substrate may include, for example, a metal foil, a metal mesh, a porous metal body, or the like. The substrate may include, for example, at least one selected from the group consisting of Al, Cu, Ni, Cr, Ti, and Fe. The substrate may include, for example, an Al foil, an Al alloy foil, a Ni foil, a Cu foil, a Cu alloy foil, a Ti foil, a stainless steel foil, or the like. The surface of the metal foil may be covered with a carbon layer. The carbon layer may include, for example, a conductive carbon material (for example, AB, etc.).

[0092] The slurry is dried on the surface of the substrate to form an active material layer. In this manufacturing method, any drying device can be used. For example, a hot plate, a hot air dryer, an infrared dryer, etc. may be used.

[0093] After drying the slurry, the electrode may be subjected to a press process. For example, cold press process may be performed, or hot press process may be performed. In the present manufacturing method, any press device may be used. For example, a roll press device or the like may be used. When hot press process is performed, the press temperature may be adjusted depending on, for example, the type of binder. The press temperature may be, for example, 80 to 180°C. After press process, the active material layer may have a thickness of, for example, 10 to 200 μm. After press process, the active material layer may have a density of, for example, 2 to 4 g / cm. 3 may be also possible.

[0094] (e) Manufacturing of all-solid-state batteries The method may include producing an all-solid-state battery including the electrode obtained above.

[0095] FIG. 2 is a conceptual diagram of the all-solid-state battery in this embodiment. For example, a power generating element 150 may be formed. The power generating element 150 may be formed by stacking a positive electrode 110, a separator layer 130, and a negative electrode 120. At least one of the positive electrode 110 and the negative electrode 120 is the electrode obtained above. The separator layer 130 is disposed between the positive electrode 110 and the negative electrode 120. The separator layer 130 includes, for example, an ion conductive material and a binder. The separator layer 130 may be formed, for example, by applying a slurry to the surface of at least one of the positive electrode 110 and the negative electrode 120.

[0096] After the power generating element 150 is formed, the power generating element 150 may be subjected to hot pressing. It is expected that the power generating element 150 will become dense through the hot pressing.

[0097] For example, a lead tab, an external terminal, or the like may be connected to the power generating element 150. The power generating element 150 is housed in an exterior body (not shown). The exterior body may be sealed. By housing the power generating element 150 in the exterior body, the all-solid-state battery 200 can be completed.

[0098] The exterior body may have any shape. For example, the exterior body may be a pouch made of a metal foil laminated film. For example, the exterior body may be a case made of a metal. For example, the exterior body may contain Al or the like. The exterior body may house a single power generating element 150 alone, or may house a plurality of power generating elements 150. The plurality of power generating elements 150 may form a series circuit or a parallel circuit. EXAMPLES

[0099] <Sample preparation> Samples No. 1 to 5 were prepared as follows.

[0100] No.1 The following materials were prepared: Active material: LiNi 0.8 Co 0.15 Al 0.05 O2 Fluoride SE:Li2.7 Ti 0.3 Al 0.7 F6 Sulfide SE:Li3PS4 SBR binder Imidazoline compound: 1-hydroxyethyl-2-alkenyl imidazoline (manufactured by BYK-Chemie "DISPERBYK (registered trademark)-109") Solvent:THN

[0101] A "Nobilta NOB-MINI" manufactured by Hosokawa Micron Corporation was prepared. In the device, 48.7 parts by mass of active material and 1.3 parts by mass of fluoride SE were mixed to form a buffer layer on the surface of the active material. The buffer layer contained fluoride SE. The mixing conditions were as follows:

[0102] Power: 12W per gram of material Rotational speed: 6000 rpm Processing time: 30 minutes

[0103] A dispersion liquid was prepared by dispersing 98.4 parts by mass of sulfide SE and 229.6 parts by mass of the solvent using an ultrasonic homogenizer.

[0104] A glove box was prepared. The dew point in the glove box was controlled to -70°C or less. A planetary mixer was placed in the glove box. 1000 parts by mass of the active material (having a buffer layer) and the dispersion obtained above were charged into the mixing vessel of the planetary mixer. The mixture was kneaded at 70 revolutions for 10 minutes. 34 parts by mass of the solvent were added, and the mixture was kneaded at 100 revolutions for 10 minutes. 37 parts by mass of the solvent were added, and the mixture was kneaded at 100 revolutions for 10 minutes. Finally, the solvent was added so that the solid concentration was 78.5%, and the mixture was kneaded at 100 revolutions for 4 hours. This formed a kneaded material.

[0105] The mixture was transferred to a sealed container (made of stainless steel). A solvent was then added to the mixture so that the solids concentration was 75%. The mixture was lightly stirred to liquefy the mixture. Dispersion-promoting components (SBR binder and imidazoline compound) were then added to the mixture. This formed the sample. The sample was stirred for 30 minutes.

[0106] No.2 A sample was prepared similar to No. 1, except that no SBR binder was added to the stiff mix.

[0107] No.3 A sample was prepared similar to No. 1, except that no imidazoline-based compound was added to the mix.

[0108] No.4 The No. 1 stiff material was used as the sample as is.

[0109] No.5 A sample was prepared similarly to No. 1, except that no SBR binder or imidazoline compound was added to the thickened mix.

[0110] "evaluation" A 15g sample was stored for 14 days. After storage, the sample was stirred. The time required for the sample to be stirred to form a slurry was measured. After the slurry was formed, the dispersion state was visually confirmed. In Table 1 below, "P (pass)" in the "Slurry dispersion state" column indicates that the slurry was homogeneous. "F (fail)" indicates that the slurry was inhomogeneous.

[0111] [Table 1]

[0112] In Table 1 above, it can be seen that by including a dispersion-promoting component in a sample, the time required for slurry formation after storage is shortened and the dispersion state of the slurry tends to improve. [Explanation of symbols]

[0113] 110 positive electrode, 120 negative electrode, 130 separator layer, 150 power generating element, 200 solid-state battery.

Claims

1. (a) preparing a first electrode material by kneading an active material, a solid electrolyte, and a solvent; (b) preparing a second electrode material by adding a dispersion promoting component to the first electrode material; (c) providing a slurry including the second electrode material; and (d) applying the slurry to a surface of a substrate to produce an electrode. Including, In the step (a), the solid electrolyte is attached to a surface of the active material to form a composite, the dispersion-promoting component promotes dispersion of the solid electrolyte in the solvent, The solid electrolyte includes a sulfide solid electrolyte; and The dispersion-promoting component includes a styrene-butadiene rubber-based binder. A method for manufacturing an electrode.

2. The dispersion-promoting component includes an imidazoline-based compound. A method for producing the electrode according to claim 1 .

3. (a) preparing a first electrode material by kneading an active material, a solid electrolyte, and a solvent; (b) preparing a second electrode material by adding a dispersion promoting component to the first electrode material; (c) providing a slurry including the second electrode material; and (d) applying the slurry to a surface of a substrate to produce an electrode. Including, In the step (a), the solid electrolyte is attached to a surface of the active material to form a composite, the dispersion-promoting component promotes dispersion of the solid electrolyte in the solvent, The solid electrolyte includes a sulfide solid electrolyte; and The dispersion-promoting component includes an imidazoline compound. A method for manufacturing an electrode.

4. (b) includes storing the second electrode material; A method for producing the electrode according to any one of claims 1 to 3.

5. The solvent comprises tetralin. A method for producing the electrode according to any one of claims 1 to 3.

6. (e) manufacturing an all-solid-state battery comprising the electrode according to any one of claims 1 to 3. Including, How solid-state batteries are manufactured.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery manufacturing method and nonaqueous electrolyte secondary battery

    JP2014011075A

  • All-solid-state battery

    JP2020053307A

  • Battery material, battery, and method for producing battery material