Rubber composite and method for producing the rubber composite
A rubber composite with a plated steel wire featuring a Cu-rich adhesive layer and Zn-rich film layer addresses adhesive deterioration and corrosion issues, ensuring strong adhesion and durability in corrosive conditions.
Patent Information
- Application Number
- JP2023548493
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-14
- Filing Date
- 2022-09-14
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2042-09-14
AI Technical Summary
Existing rubber composites face issues with adhesive deterioration and corrosion-induced separation between steel wires and rubber due to environmental factors, leading to reduced durability and adhesion strength.
A rubber composite is formed with a plated steel wire having a specific Cu and Zn plating composition, including a Cu-rich adhesive layer and a Zn-rich film layer, which are formed without heat treatment to maintain wire drawability and enhance adhesion and corrosion resistance.
The composite exhibits strong adhesion and resistance to adhesive deterioration even in corrosive environments, maintaining durability and reducing separation between steel wires and rubber.
Smart Images

Figure 0007578896000004 
Figure 0007578896000005 
Figure 0007578896000006
Abstract
Description
[Technical field]
[0001] The present disclosure relates to rubber composites and methods for making rubber composites. [Background technology]
[0002] Rubber products such as tires and hose wires are strengthened with reinforcing materials, which exert their reinforcing effect by adhering to the rubber. For this reason, the surface of reinforcing materials such as steel wires is usually plated with brass (Cu-Zn alloy), which has adhesive properties with rubber. The brass plating on the surface of plated steel wire adheres to the vulcanized rubber through the coating of unvulcanized rubber and the vulcanization process, and also has lubricating properties during the wire drawing process.
[0003] On the other hand, it is known that the adhesive strength between the reinforcing material and rubber decreases due to environmental influences during use, so that plated steel wires used as rubber reinforcing materials are required to suppress the deterioration of adhesiveness. Furthermore, if a rubber product is damaged (the rubber part is cut) and moisture penetrates, the steel reinforcing material corrodes, losing its adhesion to the rubber and causing separation between the steel and rubber.For this reason, rubber reinforcing materials are required to adhere firmly to the rubber with minimal deterioration in adhesive strength, as well as to suppress separation, which is the loss of adhesion to the rubber caused by corrosion of the reinforcing material within the rubber.
[0004] The adhesion between rubber and brass plating is achieved by the reaction of Cu in the brass plating with S in the rubber during vulcanization, forming a dense adhesive layer. On the other hand, the deterioration of adhesion due to the influence of temperature and humidity is thought to be caused by the excessive reaction of Cu in the brass plating with S in the rubber.
[0005] In order to suppress deterioration of the adhesion between rubber and plated steel wire, techniques relating to control of the adhesive layer between the rubber and the plating layer have been disclosed. Patent Document 1 discloses a technique for forming needle-shaped Cu-S-based reaction products at the adhesive interface between brass and rubber. Patent Document 2 discloses a metal cord-rubber composite in which the surface of the metal cord is treated with triazole so that the N atoms on the surface of the metal cord are 2 to 60 atomic % and the ratio of (S atomic %) / (sulfur content in the rubber compound) in the adhesive layer is 6 or more, in order to obtain a metal cord-rubber composite with excellent initial adhesion, heat-resistant adhesion, and durability.
[0006] There have also been various proposals regarding the composition of brass plating to suppress deterioration of adhesion. For example, Patent Document 3 discloses a steel wire having a brass plating in which the Cu content in the brass plating is reduced to suppress adhesion deterioration, and the Cu content in the brass plating is 35 to 55 wt % of simple gamma phase. Patent Document 4 discloses a steel wire in which the brass plating on the surface of the steel wire has a copper ratio of 35 to 50 mass % and the copper ratio in a 5 nm thick region of the brass plating is 15 to 30 atomic % in order to improve durable adhesion to rubber. Furthermore, Patent Document 5 discloses a method for improving wire drawability by applying a Cu plating having a thickness of 0.005 μm or more and less than 0.02 μm to a brass plating surface layer having a Cu ratio of 50 to 60%. Patent Documents 6 to 8 also disclose rubber composites in which plated steel wires are covered with rubber.
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 2004-263336 Patent Document 2: JP 2017-14338 A Patent Document 3: JP 2013-227629 A Patent Document 4: JP 2003-313788 A Patent Document 5: JP 2003-96594 A Patent Document 6: JP 2005-314808 A Patent Document 7: International Publication No. 2019 / 159531 Patent Document 8: JP 2012-167381 A Summary of the Invention [Problem to be solved by the invention]
[0008] The technology disclosed in Patent Document 1 requires a preheat treatment before vulcanization in order to generate needle-like crystals, which has the problem of increasing production costs. In addition, it is not expected to improve the corrosion resistance of the plated steel wire, and it is thought that peeling from the rubber due to corrosion will not be improved. In the technology disclosed in Patent Document 2, even if the metal cord is treated with a triazole compound, the corrosion resistance of the metal cord is not improved, and therefore peeling from the rubber due to corrosion is not considered to be improved. The low Cu brass plating disclosed in Patent Document 3 or Patent Document 4 has a problem that the plating layer becomes hard and wire drawability decreases. In addition, the corrosion resistance of the plated steel wire is not improved, so it is considered that peeling between the plated steel wire and rubber in a corrosive environment cannot be suppressed. When the composition of only the brass plating surface layer disclosed in Patent Document 5 is made to have good processability, the wire drawability is improved, but it is considered that it is not possible to suppress peeling between the plated steel wire and the rubber, that is, separation, caused by corrosion of the steel when moisture penetrates into the rubber.
[0009] An object of the present disclosure is to provide a rubber composite in which a steel wire and vulcanized rubber are firmly bonded to each other and a decrease in the adhesive strength between the steel wire and the vulcanized rubber is suppressed even in a corrosive environment due to moisture, and a method for manufacturing the rubber composite. [Means for solving the problem]
[0010] Means for solving the above problems include the following aspects. <1> A rubber composite comprising a plated steel wire having a plating layer formed on a surface of the steel wire and a vulcanized rubber coating the plated steel wire, When a cross section perpendicular to the longitudinal direction of the rubber composite is observed using a backscattered electron image obtained by a field emission scanning electron microscope, the rubber composite includes a coating layer between the vulcanized rubber and the steel wire, the coating layer being in contact with the steel wire, and an adhesive layer between the vulcanized rubber and the coating layer, the adhesive layer has a mass ratio of Cu of 15 to 75 and a mass ratio of Cu to S (Cu mass ratio / S mass ratio) of 1.0 to 4.0 when the total mass of Cu, Zn, and S in the adhesive layer is 100; The coating layer has a mass ratio of Zn of more than 65 to 90 when the total mass of Cu, Zn, and S in the coating layer is 100. Rubber composite. <2> The adhesive layer has a thickness of 50 to 500 nm; The thickness of the coating layer is 100 to 500 nm. <1> The rubber composite according to claim 1. <3> A plated steel wire manufacturing process for manufacturing a two-layer plated steel wire by the following method A or the following method B; a rubber composition coating step of coating a surface of the two-layer plated steel wire with a rubber composition; a vulcanization step of vulcanizing the rubber composition coated on the surface of the two-layer plated steel wire to bond the vulcanized rubber and the two-layer plated steel wire; Including, The method A includes a Zn plating step of forming a Zn plating layer on the surface of a drawn wire material to obtain a Zn-plated drawn wire material, a Cu plating step of forming a Cu plating layer on the surface of the Zn-plated drawn wire material to obtain a two-layer plated drawn wire material, and a wire drawing step of wet drawing the two-layer plated drawn wire material without heating to obtain the two-layer plated steel wire, Method B is a method for producing a rubber composite, comprising a Zn plating step of forming a Zn plating layer on the surface of a drawn wire material to obtain a Zn-plated drawn wire material, a wiredrawing step of wet-drawing the Zn-plated drawn wire material to obtain a Zn-plated steel wire, and a Cu plating step of forming a Cu plating layer on the surface of the Zn-plated steel wire to obtain the two-layer plated steel wire. <4> In the plated steel wire manufacturing process, the two-layer plated steel wire is manufactured by the method A. <3> A method for producing a rubber composite according to claim 1. <5> In the plated steel wire manufacturing process, the two-layer plated steel wire is manufactured by the method B. <3> A method for producing a rubber composite according to claim 1. Effect of the Invention
[0011] According to the present disclosure, there is provided a rubber composite in which a steel wire and a vulcanized rubber are firmly bonded to each other and a decrease in the adhesive strength between the steel wire and the vulcanized rubber is suppressed even in a corrosive environment due to moisture, and a method for manufacturing the rubber composite. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic diagram illustrating an example of a method for making a rubber composite of the present disclosure. [Diagram 2] FIG. 2 is a schematic diagram illustrating another example of a method for making a rubber composite according to the present disclosure. [Diagram 3] FIG. 2 is a schematic diagram showing a manufacturing process of a plated steel wire in an example. [Figure 4] FIG. 2 is a schematic diagram showing an adhesion test sample in an example. [Diagram 5] FIG. 2 is a diagram showing an example of a backscattered electron image near a surface layer in a cross section of a rubber composite. [Figure 6] FIG. 2 is a schematic diagram showing positions at which compositions of an adhesive layer and a coating layer were analyzed by EDS (energy dispersive X-ray spectroscopy). [Figure 7] FIG. 1 shows an example of the results of a line analysis from rubber to steel by EDS. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, embodiments of a rubber composite comprising a plated steel wire and vulcanized rubber in the present disclosure, a plated steel wire that can be suitably used for producing the rubber composite, and a method for producing the rubber composite will be described in detail. In this specification, a numerical range expressed with "~" means a range including the numerical values before and after "~" as the lower and upper limits. However, if the lower limit is marked "more than" or the upper limit is marked "less than," those numerical values are not included. In the numerical ranges described in stages in this specification, the upper limit value of a certain numerical range may be replaced by the upper limit value of another numerical range described in stages or a value shown in an example, and the lower limit value of a certain numerical range may be replaced by the lower limit value of another numerical range described in stages or a value shown in an example. "%" indicating the content of an element means "mass %" unless otherwise specified. The term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved. In this specification, "steel wire" means a steel material as a base material in a plated steel wire, "plated steel wire" means a steel material including a steel wire and a plating layer applied to the steel wire, and "drawn wire material" means a material before final wiredrawing to manufacture a plated steel wire, that is, a steel material before or after plating. In addition, in this specification, the term "Cu plating layer" refers to a plating layer that contains Cu and may contain elements other than Cu. The same applies to the term "Zn plating layer."
[0014] The embodiments of the present disclosure do not limit the present disclosure. The components of the embodiments of the present disclosure include those that are replaceable and easy for a person skilled in the art, or those that are substantially the same. Furthermore, various forms included in the embodiments of the present disclosure can be arbitrarily combined within the scope of obvious to a person skilled in the art.
[0015] The inventors of the present disclosure have intensively studied the adhesion and corrosion behavior of vulcanized rubber (sometimes referred to as "coated rubber" or simply "rubber" in the present disclosure) in a rubber composite and a plated steel wire as a reinforcing material. As a result, they have found that at the interface between the steel wire, which is the base material of the plated steel wire, and the rubber, an adhesive layer containing Cu and S is formed in contact with the rubber, which originates from the rubber and the plated layer, and a coating layer containing Zn is formed in contact with the steel (steel wire) of the plated steel wire to prevent corrosion of the steel wire, thereby firmly bonding the steel wire and rubber and suppressing adhesion deterioration in a corrosive environment. They have also found that by appropriately adjusting the composition of the adhesive layer and the coating layer formed between the rubber and the steel wire, respectively, adhesion deterioration between the rubber and the steel wire is suppressed, and adhesion peeling (separation) with the rubber is suppressed even in an environment where moisture penetrates into the rubber and the steel wire is prone to corrosion, and the durability of the rubber composite can be improved.
[0016] Furthermore, the inventors of the present disclosure have discovered that, in order to prevent a decrease in wiredrawability even when the Cu ratio in the entire plating layer of the plated steel wire contained in this rubber composite decreases, by performing the wiredrawing process without heating and diffusing after plating, the wiredrawability does not decrease even with low Cu (high Zn) plating, and by optimizing the plating composition and plating adhesion amount, high adhesive strength to the rubber and high corrosion resistance can be obtained, which has led to the completion of the invention of the present disclosure.
[0017] [Rubber composite] The rubber composite according to the present disclosure is a rubber composite including a plated steel wire having a plating layer formed on the surface of the steel wire, and vulcanized rubber coating the plated steel wire, and when a cross section perpendicular to the longitudinal direction of the rubber composite is observed using a backscattered electron image obtained by a field emission scanning electron microscope, the rubber composite includes a coating layer in contact with the steel wire between the vulcanized rubber and the steel wire, and an adhesive layer interposed between the vulcanized rubber and the coating layer. In the adhesive layer, when the total mass of Cu, Zn, and S in the adhesive layer is taken as 100, the mass ratio of Cu is 15 to 75, and the mass ratio of Cu to the mass ratio of S (Cu mass ratio / S mass ratio) is 1.0 to 4.0. In the coating layer, the mass ratio of Zn is more than 65 and is in the range of 90 to 100 when the total mass of Cu, Zn, and S in the coating layer is taken as 100. In this disclosure, the "mass ratio" of each element of Cu, Zn, or S in an "adhesive layer" or a "coating layer" means the mass ratio of each element when the total mass of Cu, Zn, and S in each layer is taken as 100. The steel wire, the vulcanized rubber (coating rubber), the adhesive layer, and the coating layer will be specifically described below.
[0018] <Steel wire> The steel material components (chemical composition of the steel wire) of the rubber composite of the present disclosure are not particularly limited, but in order to reduce weight and increase the reinforcing effect, it is preferable that the wire diameter is small and the strength is high. For this reason, the C content of the steel wire is preferably 0.80% or more, and in order to reinforce the rubber product (rubber composite) with a steel wire of higher strength, the C content is preferably 0.92% or more. To further increase the strength, a steel material component containing 1.02% or more of C is preferable. The steel wire may contain components such as Si and Mn in addition to Fe and C, and may contain about 0.2% Cr as necessary, for example, to increase strength. The diameter and structure of the steel wire depend on the application of the rubber composite, but for example, the wire diameter is 0.1 mm to 0.4 mm, and the structure is preferably mainly composed of pearlite.
[0019] <Vulcanized rubber> The vulcanized rubber (coated rubber) in the rubber composite of the present disclosure is formed by vulcanizing a rubber composition that coats a plated steel wire. The rubber composition may contain, in addition to the rubber component, sulfur (vulcanizing agent), cobalt or cobalt-containing compound (adhesion promoter), etc.
[0020] The rubber component of the rubber composition used for the coating rubber is not particularly limited, but for example, natural rubber and / or synthetic polyisoprene rubber (IR) is preferable, and natural rubber is more preferable. Other synthetic rubbers include polybutadiene rubber (BR) and styrene-butadiene copolymers. (SBR), styrene-isoprene copolymer (SIR), acrylonitrile-butadiene Examples of the rubber components include diene rubbers such as copolymer rubber, ethylene-propylene copolymer rubber, ethylene-propylene-diene rubber, butyl rubber, halogenated butyl rubber, alkylated chlorosulfonated polyethylene rubber, isobutylene-isoprene copolymer rubber, polychloroprene rubber, etc. These rubber components may be used alone or in combination of two or more.
[0021] The vulcanizing agent sulfur is preferably blended in an amount of 8.0 parts by mass or less per 100 parts by mass of the rubber component. In particular, the amount is in the range of 3.0 to 8.0 parts by mass, and more preferably in the range of 4.0 to 6.0 parts by mass. Blending 8.0 parts by mass or less of sulfur can suitably prevent deterioration of the aging resistance of the coating rubber composition. Blending 3.0 parts by mass or more of sulfur is more preferable because it improves initial adhesion.
[0022] Cobalt or a cobalt-containing compound is preferably blended in an amount of 0.1 to 0.4 parts by mass in terms of the amount of cobalt per 100 parts by mass of the rubber component. When the amount of cobalt or a cobalt-containing compound is 0.4 parts by mass or less in terms of the amount of cobalt, the deterioration of the aging resistance of the coating rubber composition can be suitably prevented, and when the amount of cobalt or a cobalt-containing compound is 0.1 parts by mass or more in terms of the amount of cobalt, the initial adhesion is improved, which is more preferable. Examples of the cobalt- or gout-containing compound that can be used include cobalt (simple substance), cobalt salts of organic acids, and cobalt salts of inorganic acids. Examples of the cobalt- or gout-containing compound that can be used include cobalt chloride, cobalt nitrate, cobalt sulfate, cobalt acetate, cobalt citrate, cobalt gluconate, cobalt naphthenate, cobalt neodecanoate, cobalt stearate, cobalt rosinate, cobalt versatate, cobalt tall oil acid, cobalt neodecanoate borate, and cobalt acetylacetonate. Also, a complex salt in which a part of the organic acid is replaced with boric acid or the like may be used.
[0023] In addition to the compounding agents described above, the coating rubber composition in the rubber composite of the present disclosure may contain other compounding agents, such as vulcanization activators such as zinc oxide and organic acids (e.g., stearic acid), vulcanization accelerators, inorganic fillers such as carbon black and silica, antioxidants, antiozonants, and softeners.
[0024] For example, the rubber may contain, per 100 parts by mass of rubber, organic acid cobalt (1 to 5 parts by mass) as an adhesion promoter, sulfur (3 to 8 parts by mass) as a vulcanizing agent, carbon black (50 to 65 parts by mass) as a reinforcing agent, and other organic and inorganic additives.
[0025] <Interface structure between steel wire and vulcanized rubber> The rubber composite of the present disclosure contains Cu sulfide produced by reaction of S in the rubber with Cu in the plating at the interface between the steel wire and the vulcanized rubber, and includes an adhesive layer (Cu sulfide layer) in contact with the rubber, and a Zn-rich coating layer in contact with the steel wire.
[0026] (adhesive layer) The adhesive layer contains S and is in contact with the rubber to contribute to adhesion to the rubber. The adhesive layer is a layer that is newly formed mainly from S in the rubber layer and Cu in the Cu-plated layer during the process of vulcanizing the rubber composition coated on the Cu-plated layer when producing the rubber composite of the present disclosure. The adhesive layer contains Cu such that the mass ratio of Cu is 15-75 when the total mass of Cu, Zn, and S in the adhesive layer is taken as 100. By making the mass ratio of Cu in the adhesive layer 15 or more, the adhesive strength (initial adhesion) between the steel wire and the vulcanized rubber can be increased. On the other hand, if the mass ratio of Cu in the adhesive layer exceeds 75, adhesion deterioration in a high temperature and high humidity environment increases, so the upper limit of the mass ratio of Cu in the adhesive layer is 75. The mass ratio of Cu in the adhesive layer is preferably 20-70.
[0027] In addition, the mass ratio of Cu to the mass ratio of S in the adhesive layer (Cu mass ratio / S mass ratio, hereinafter sometimes referred to as "Cu / S") is 1.0 to 4.0. When the Cu / S in the adhesive layer is 1.0 or more, a dense adhesive layer is formed, and higher adhesive strength is obtained. On the other hand, if Cu / S exceeds 4.0, Cu reacts excessively, resulting in a coarse adhesive layer, which reduces adhesive strength. From this viewpoint, Cu / S in the adhesive layer is preferably 1.5 to 3.0.
[0028] The thickness of the adhesive layer is not particularly limited, but if the adhesive layer is too thin, the adhesive strength with the rubber may be insufficient, and if the adhesive layer is too thick, the adhesive layer may peel off from the adhesive layer. Therefore, the thickness of the adhesive layer is preferably 30 to 600 nm, more preferably 50 to 500 nm, and even more preferably 60 to 250 nm. The adhesive layer may contain elements other than Cu, Zn, and S, such as Fe, Co, Ni, P, and Bi, but the content of other elements in the adhesive layer is preferably 0.5% or less.
[0029] (Coating layer) The coating layer is a layer derived from the plating layer of the plated steel wire when the rubber composite of the present disclosure is produced. The coating layer is located inside the adhesive layer (on the steel wire side) and has the function of preventing corrosion of the steel wire by contacting the steel wire. In the coating layer, the mass ratio of Zn is more than 65 and is in the range of 90 to 100 when the total mass of Cu, Zn, and S in the coating layer is taken as 100. When the mass ratio of Zn in the coating layer is more than 65, the coating layer can exhibit corrosion protection effect for steel. On the other hand, if the mass ratio of Zn in the coating layer exceeds 90, a Zn oxide layer is formed due to corrosion of the coating, and the adhesive strength decreases significantly. Therefore, the mass ratio of Zn in the coating layer is greater than 65 and less than 90, and preferably 80-90.
[0030] The thickness of the coating layer is not particularly limited, but if the coating layer is too thin, the function of preventing corrosion of the steel wire may be insufficient, and if the coating layer is too thick, adhesion deterioration may increase. From this viewpoint, the thickness of the coating layer is preferably 100 to 500 nm, and more preferably 150 to 200 nm. The coating layer may contain elements other than Cu, Zn, and S, such as Fe, Co, Ni, P, and Bi, but the content of other elements in the coating layer is preferably 0.5% or less.
[0031] (Observation of the rubber / steel wire interface) The interface between the steel wire and the vulcanized rubber in the rubber composite can be observed as follows to measure the contents of S, Cu, and Zn. A sample of the steel wire pulled out from the rubber in the rubber composite is cut perpendicular to the length direction with a CP (Cross Section Polisher: registered trademark, manufactured by JEOL Ltd.) and the C-section (cross section perpendicular to the length direction) is observed with a FE-SEM (field emission scanning electron microscope), and the rubber layer, sulfide layer (adhesive layer), coating layer, and base steel (steel wire) are identified using backscattered electron images.The composition of each layer is then analyzed with EDS (energy dispersive X-ray spectroscopy). The SEM acceleration voltage is set to 15 kV, and spot analysis is performed at a magnification of 30,000 times. When measuring the thickness of each layer, the measurement can be performed using software having a function for measuring length of SEM images (for example, Smile View (registered trademark) manufactured by JEOL Ltd.). Analysis of each layer and measurement of thickness are performed at three locations on one cross section, and the average value is calculated by measuring three cross sections.
[0032] The method for identifying each layer of the rubber composite of the present disclosure and the method for analyzing the composition will now be described more specifically. In the rubber composite of the present disclosure, the rubber layer, adhesive layer, coating layer, and base steel (steel wire) can be identified and specified by the contrast of the reflected electron image when a cross section (C cross section) perpendicular to the longitudinal direction is observed with an FE-SEM. The C cross section of an integrated body (rubber composite) of rubber-coated plated steel wire and rubber is processed with a CP, and a COMPO (reflected electron composition image) is observed with an FE-SEM with a Schottky field emission electron gun at an accelerating voltage of 15 kV and a magnification of 30,000. Figure 5 shows an example of a backscattered electron image near the surface layer in the cross section of a rubber composite. The adhesive layer is between the rubber part and the plating layer (coating layer), and is a compound layer containing copper and sulfur; it is in contact with the rubber and is observed with a contrast that is brighter than the rubber layer and darker than the plating layer. The coating layer is a plating layer on the surface of the steel wire, which exists closer to the steel wire than the adhesive layer, and is the area with brighter contrast than the adhesive layer in the COMPO image. The coating layer is a layer that exists in contact with the steel wire to suppress the corrosion of steel through the sacrificial corrosion protection action of Zn.
[0033] Next, we will explain the composition analysis of the adhesive layer and coating layer using EDS (energy dispersive X-ray spectroscopy). Figure 6 shows a schematic diagram of the positions of composition analysis by EDS for each layer identified by the COMPO image. Between the steel wire 2 and the rubber part 8, a coating layer 4 as the first layer and an adhesive layer 6 as the second layer are laminated from the steel wire 2 side. The dashed lines in Figure 6 indicate the positions at half the thickness of each of the adhesive layer 6 and the coating layer 4, and + on the lines indicates the analysis points. The adhesive layer 6 and the coating layer 4 are each analyzed at three points. As shown in Fig. 6, EDS analysis is performed by point analyzing the central parts of the thickness direction of the adhesive layer 6 and the coating layer 4 in the COMPO image, selecting CuKα, ZnKα, and SKα radiation, and obtaining simplified quantitative values using ZAF quantitative correction. In this case, even if the X-ray penetrates the inside of the analysis target and detects C, Fe, and other elements, the concentration of each of these three elements is calculated by setting the total of Cu, Zn, and S to 100. Figure 7 shows an example of the results of a line analysis (arrow) of the interface from the rubber to the steel at the position of arrow L in the COMPO image shown in Figure 5, with each element (Cu, Zn, S, Fe, C) traced with a different line type. If each layer is explained in terms of composition changes, the adhesive layer is the region between the rubber and the steel wire, where the S intensity increases from the rubber side toward the steel wire surface and then drops rapidly, and where the Cu intensity is 50% or more of the maximum intensity. The coating layer is the region between the adhesive layer and the steel wire, where the S intensity drops rapidly from the adhesive layer toward the steel wire surface, the Fe intensity increases, and then becomes almost constant, and where the Zn intensity is 50% or more of the maximum intensity.
[0034] [Method of manufacturing rubber composite] Next, a method for producing a rubber composite according to the present disclosure will be described. The method for producing the rubber composite according to the present disclosure is not particularly limited, but the rubber composite can be suitably produced by coating a plated steel wire having a plating layer with a predetermined composition with a rubber composition and then vulcanizing the coated rubber. A preferred method for producing a rubber composite according to the present disclosure includes a plated steel wire production process for producing a two-layer plated steel wire, a rubber composition coating step of coating a surface of the two-layer plated steel wire with a rubber composition; and a vulcanization step of vulcanizing the rubber composition coated on the surface of the two-layer plated steel wire to bond the vulcanized rubber to the two-layer plated steel wire. Here, the method for producing the double-layer plated steel wire may be the following Method A or Method B. (A method) The method includes a Zn plating step of forming a Zn plating layer on the surface of a drawn wire material to obtain a Zn-plated drawn wire material, a Cu plating step of forming a Cu plating layer on the surface of the Zn-plated drawn wire material to obtain a two-layer plated drawn wire material, and a wire drawing step of wet drawing the two-layer plated drawn wire material without heating to obtain the two-layer plated steel wire. (Method B) The method includes a Zn plating step of forming a Zn plating layer on the surface of a drawn wire material to obtain a Zn-plated drawn wire material, a wire drawing step of wet-drawing the Zn-plated drawn wire material to obtain a Zn-plated steel wire, and a Cu plating step of forming a Cu plating layer on the surface of the Zn-plated steel wire to obtain a two-layer plated steel wire. That is, in both methods A and B, a two-layer plated steel wire is produced without alloying by heating after forming a Zn plating layer and a Cu plating layer on the surface of a drawn wire material or a steel wire, and then the two-layer plated steel wire is coated with a rubber composition and vulcanized to bond the vulcanized rubber and the two-layer plated steel wire. By vulcanization, an adhesive layer derived from the rubber and the Cu plating and a coating layer derived from the Zn plating are formed between the vulcanized rubber and the steel wire, and the rubber composite according to the present disclosure can be produced. 1 and 2 each show a schematic diagram of an example of a method for producing a rubber composite according to the present disclosure.
[0035] <Plated steel wire> A plated steel wire that can be suitably used in producing a rubber composite according to the present disclosure will now be described. The plated steel wire in the present disclosure is a steel wire having a Zn plating layer containing Zn and a Cu plating layer containing Cu formed on the surface thereof (in the present disclosure, this may be referred to as a "two-layer plated steel wire", a "Zn-Cu plated steel wire", or simply a "plated steel wire"). The steel composition of the steel wire which is the base material of the plated steel wire is as described above, and the description thereof will be omitted here.
[0036] (Plating layer) The plating layer of the plated steel wire in the present disclosure preferably has a Zn content of more than 65 to 95 mass % in the entire plating layer. If the Zn content in the entire plating layer is more than 65%, the Zn ratio in the coating layer does not decrease too much when it is vulcanized and bonded to rubber, the corrosion-inhibiting effect of the steel wire is not likely to decrease, the plated steel wire is not likely to corrode when moisture penetrates into the rubber, and peeling from the rubber is not likely to occur. On the other hand, when the Zn content in the entire plating layer is 95% or less, the initial adhesion to the rubber is less likely to decrease, and further, a significant decrease in adhesion strength after deterioration is suppressed. In addition, Zn corrosion is less likely to progress, thick and brittle Zn corrosion products are less likely to form, and adhesion peeling from the rubber is less likely to progress. From this viewpoint, the Zn content in the entire plating layer is preferably more than 65 and 95 mass %, and more preferably 80 to 90 mass %. For example, when a Zn plating layer and a Cu plating layer are laminated on the surface of a steel wire as a plating layer, the Zn content in the entire plating layer is the Zn content as the average composition in the entire plating layer including the Zn plating layer and the Cu plating layer. The plating layer may contain elements other than Cu and Zn, such as Fe, Co, Ni, P, and Bi, but the content of other elements in the plating layer is preferably 0.5 mass% or less.
[0037] When the total content of Cu and Zn in the surface layer from the surface of the plating layer to a depth of 50 nm is taken as 100 atomic %, the Cu content is preferably 20 to 80 atomic %. If the Cu content in the surface layer of the plating layer is less than 20 atomic %, the adhesion deteriorates significantly, and separation due to peeling from the rubber may easily occur. On the other hand, if the Cu content in the surface layer of the plating layer exceeds 80 atomic %, both the initial adhesion and the adhesion strength after deterioration decrease, and separation may become more likely to occur. From this viewpoint, the Cu content in the surface layer of the plating layer is preferably 20 to 80 atomic %, more preferably 30 to 60 atomic %, and further preferably 30 to 50 atomic %. For example, when a Zn plating layer and a Cu plating layer are laminated on the surface of a steel wire as a plating layer, the Cu content (Cu atomic %) in the surface layer of the plating layer is the Cu atomic % as the average composition in a region of the surface layer of 50 nm. The thickness of the plating layer is preferably, for example, 150 to 500 nm in the entire plating layer from the viewpoint of forming an adhesive layer and a coating layer by vulcanization treatment after coating with the rubber composition.
[0038] (Plating weight) If the plating layer becomes too thick, the fatigue strength may decrease, so the plating weight is preferably 9.5 g or less per kg of steel. On the other hand, if the coating weight is too small, the plating thickness will be locally thin, which may cause poor formation of an adhesive layer with the rubber and reduce wire drawability. Therefore, it is preferable that the coating weight is 2.0 g or more per kg of steel. From this viewpoint, the coating weight is more preferably 3.0 g / kg to 8.0 g / kg per 1 kg of steel.
[0039] (Analysis of plating layer) The average composition of the plating layer can be analyzed as follows. Approximately 10 g of plated steel wire is collected and immersed in 100 ml of a 70% concentration ammonia solution to dissolve the plating layer, and the amount of plating attached per 1 kg of steel can be calculated from the change in mass. The amount of Zn in the ammonia aqueous solution in which the plating layer has been dissolved is quantified in g / l using ICP (Inductively Coupled Plasma). This is then converted into 100 ml of analysis solution, and the average Zn mass% in the plating layer can then be calculated by converting it into the Zn concentration relative to the total mass of the dissolved plating layer. Similarly, the amount of Cu is quantified, and the average plating thickness can be calculated from the plating composition (Zn and Cu ratio as the average plating density) and plating weight.
[0040] The composition of the surface layer of the plated steel wire was measured by measuring the depth profile from the surface of the plated steel wire using XPS (X-ray photoelectron spectroscopy). 2 The atomic percentages of Cu and Zn are calculated in 5 nm increments and the average value is calculated for 10 points over a surface layer of 50 nm.
[0041] The coating weight, average composition, and surface layer composition of plated steel wire are similarly measured three times in the longitudinal direction and the average values (averages of three locations out of 10 at each measurement position) are used.
[0042] <Method of manufacturing plated steel wire> An example of a method for producing a plated steel wire in the present disclosure will be specifically described with reference to Figures 1 and 2. It is needless to say that the method for producing a plated steel wire in the present disclosure is not limited to the method described below. For example, a hot rolled wire rod is subjected to a first wire drawing to produce a first drawn wire rod having a wire diameter of about 1.0 mm to 2.0 mm, and then isothermally transformed by heat treatment to produce a pearlite structure. Next, the drawn wire is sequentially electroplated with Zn and then with Cu (FIG. 1(A)) to form a Zn-plated layer and a Cu-plated layer on the surface of the base steel (steel wire), to produce a two-layer plated drawn wire. The coating weight after plating is, for example, 2.0 to 8.9 g / kg Zn, 0.5 to 1.0 g / kg Cu, and 2.5 to 9.4 g / kg Zn+Cu. Next, the two-layer plated drawn wire material is wet drawn without heating to a wire diameter in the range of 0.1 mm to 0.4 mm (FIG. 1(B)). In this manufacturing process, by controlling the thickness of the Zn plating layer and the thickness of the Cu plating layer thereover, it is possible to control the adhesion weight of the plating layer, the composition of the entire plating layer, and the plating composition of the surface layer, thereby making it possible to manufacture the plated steel wire according to the present disclosure.
[0043] In the plated steel wire of the present disclosure, the Zn plating and Cu plating are formed separately, and then the plated steel wire is not heated to form an alloy, so that the average composition of the plated layer can be freely set from a low Cu range to a high Cu range, and workability is not affected. Therefore, the productivity of the wire drawing process to obtain the plated steel wire is good, and the wire can be manufactured with the same productivity as that of normal brass plating (60 to 70% Cu brass). Good productivity in the wire drawing process to obtain the plated steel wire means that there is little productivity inhibition due to wire breakage during drawing or a decrease in wire drawing speed, and it means that the productivity is the same as that of normal brass plated steel wire.
[0044] As another method for producing a plated steel wire in the present disclosure, for example, a first drawn wire material having a wire diameter of 1.0 to 2.0 mm is subjected to heat treatment in the same manner as above, and then the Zn-plated drawn wire material having a Zn plating of 2.0 to 8.9 g / kg is wet-drawn (FIGS. 2(A) and (B)). The wire is drawn to a wire diameter of 0.1 to 0.4 mm to obtain a Zn-plated steel wire, and then passed through a Cu plating bath to form a plating layer on the surface of the Zn-plated steel wire with a Cu plating amount of, for example, 0.5 to 1.0 g / kg and a total amount of Zn+Cu of 2.5 to 9.4 g / kg (FIG. 2(C)). At this time, the Cu plating can be electrolytic plating by passing current through the wire, but since a thin Cu film is sufficient, it is preferable to perform Cu displacement plating by passing the wire through a copper pyrophosphate bath for a short time in order to perform the plating more simply. The Cu concentration of the plating solution and the treatment time can be adjusted to the target plating composition and plating amount. The Cu plating on the surface of the Zn-plated steel wire can be applied not only to the single wire but also to the stranded wire.
[0045] Even when a Zn-plated drawn wire material having a single Zn-plated layer is further drawn, the drawing process can be performed without peeling of the plating during drawing, wire breakage, or a decrease in the drawing speed. Therefore, the plated steel wire of the present disclosure can be obtained by forming a Cu-plated layer on the surface of the Zn-plated steel wire after wiredrawing.
[0046] <Formation of vulcanized rubber> The rubber composite of the present disclosure can be produced by coating the plated steel wire (two-layer plated steel wire) produced as described above with a rubber composition and vulcanizing the wire to produce a vulcanized rubber. For example, a plated steel wire is coated with a rubber composition produced by kneading each component of the rubber composition by a conventional method, and the wire is molded into a desired shape, and then vulcanized to produce the rubber composite shown in FIG. 1(C) or FIG. 2(D). The vulcanization conditions are not particularly limited, but the pressure is preferably 2 MPa to 25 MPa, and the temperature is preferably 120 to 200° C. The vulcanization time is not particularly limited, but is preferably 10 minutes to 60 minutes.
[0047] Vulcanization produces a sulfide layer (adhesive layer) at the interface between the plating layer and the vulcanized rubber through a reaction. The sulfide layer is formed when Cu from the plating layer diffuses into the rubber and reacts, and depending on the reaction speed and the composition of the plating layer, a significantly thicker adhesive layer may be produced. As a result, the adhesive layer + coating layer may be significantly thicker than the thickness of the two plating layers. For example, if a plating layer with a high Cu concentration is formed at the interface between the steel wire and the vulcanized rubber, a thick adhesive layer with low density may be produced by vulcanization. On the other hand, depending on the reaction speed during vulcanization, the composition of the plating layer, and local variations in the circumferential and longitudinal directions, the sum of the thickness of the sulfide layer and the thickness of the coating layer may be thinner than the thickness of the plating layer.
[0048] The rubber composite of the present disclosure can also be produced by forming a plated steel wire into a strand, coating the strand with a rubber composition, and then vulcanizing the strand. In this case, it is sufficient that the adhesive layer and coating layer described above are formed between the strand and the vulcanized rubber (at the interface).
[0049] By using the plated steel wire according to the present disclosure, a rubber composite can be produced that has high initial adhesive strength and is inhibited from decreasing in adhesive strength and from peeling off from the rubber even after deterioration treatment. The adhesion properties of the plated steel wire and rubber composite in the present disclosure can be evaluated, for example, by the following adhesion test method.
[0050] (Adhesion test method) As shown in FIG. 4, a plated steel wire is embedded in a rubber composition 20 according to the ASTM D1871A method, and within one week after vulcanization, the plated steel wire 10 exposed from the rubber 20 is chucked and the pull-out force from the rubber 20 is measured to determine the initial adhesive strength. The rubber part of the adhesive test piece S in FIG. 4 is immersed in distilled water at 80° C. for 7 days, and then the pull-out force is measured in the same manner to determine the adhesive strength after adhesive deterioration. During the deterioration treatment, the part embedded in the rubber 20 (the plated steel wire part shown by the dashed line) undergoes adhesion deterioration due to the high temperature and high humidity environment. During the deterioration treatment, distilled water penetrates into the rubber from the immersed rubber end 11, so corrosion progresses from the immersed rubber end 11, causing peeling (separation) between the plated steel wire 10 and the rubber 20. As a result, the occurrence of separation can be evaluated by measuring the length of peeling from the rubber due to corrosion from the appearance of the plated steel wire pulled out after deterioration. Applications of the rubber composite according to the present disclosure are not limited, and examples include rubber products reinforced with steel cords, such as tires and conveyor belts. EXAMPLES
[0051] The rubber composite and the plated steel wire for a rubber composite of the present disclosure will be described in more detail below with reference to examples. However, the rubber composite and the plated steel wire for a rubber composite of the present disclosure are not limited to these examples. Each step in the examples (inventive example and comparative example) is shown in Fig. 3. (A) is a step in a conventional example (comparative example), and (B) and (C) are steps in the inventive examples of the present disclosure.
[0052] The raw material was a hot-rolled wire rod having a wire diameter of 5.5 mm and having the steel composition shown in Table 1. The wire rod was pickled, lime-coated, and dry-drawn to a wire diameter of 1.39 mm. The wire was then heated at 975°C for 35 seconds and then heat-treated to undergo isothermal transformation at a temperature in the range of 580 to 610°C for 6 seconds.
[0053] [Table 1]
[0054] After that, Zn plating and Cu plating were applied sequentially to the surface of the steel material (drawn wire material) by electrolytic plating (electrolytic two-layer plating), and the wire was drawn by wet wire drawing to a wire diameter of 0.2 mm at a wire speed of 500 m / min without performing heat treatment after plating. By changing the Zn plating thickness and Cu plating thickness during plating, plated steel wires (two-layer plated steel wires) with different plating compositions and plating adhesion amounts were manufactured (Fig. 3(A)). In addition, after the above heat treatment, the steel surface was electrolytically plated with Zn to obtain Zn-plated drawn wire, which was then wet-drawn and passed through a Cu pyrophosphate bath to produce plated steel wire with displacement Cu plating (post-Cu plating) on the Zn plating (Figure 3(B)).
[0055] For the comparative material, following the above heat treatment, a Zn plating was applied over the Cu plating so that the Cu content was 64 mass%, and the material was heated at 450°C for 9 s to form a brass alloy, after which it was drawn (Figure 3(C)).
[0056] The plating properties were evaluated by immersing a plated steel wire in a 70% ammonia solution and determining the amount of plating applied per 1 kg of steel from the change in mass before and after immersion. The mass % of Zn in the plating was calculated by quantifying the Zn concentration in the plating solution using ICP (Inductively Coupled Plasma) and determining the mass of Zn relative to the total mass of the plating. XPS analysis of plated steel wire surface to a depth of 50 nm (SiO 2 The atomic percentages of Cu and Zn (calculated as percent) were measured every 5 nm and the average of 10 points was calculated. Similarly, the Cu concentration in the plating solution was quantified, the plating composition was obtained, the average density was calculated from the plating composition (Cu, Zn), and the average plating thickness was calculated from the plating adhesion weight. This measurement was performed at three points in the longitudinal direction for one plated steel wire, and the average value (the average of the three points out of the 10 points at each measurement position) was determined.
[0057] The adhesion between the plated steel wire and rubber was evaluated by stranding the drawn plated steel wire into a 1+6 structure (six plated steel wires arranged around one central steel wire) and embedding it in a rubber composition having the compounding amount (phr: parts per hundred rubber) shown in Table 2 according to the ASTM D1871A method, and vulcanizing it at 150°C for 30 minutes at a press pressure of 25 MPa to prepare sample S (rubber composite) for the adhesion test (pull-out test) as shown in Figure 4. 10 is the plated steel wire and 20 is the vulcanized rubber.
[0058] [Table 2]
[0059] Nocrac 810NA: Anti-aging agent, manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Noccela CZ: Vulcanization accelerator manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0060] <Pull-out test> In the pull-out test, the portion of the plated steel wire 10 protruding from the vulcanized rubber 20 of the test sample S was chucked, and the pull-out load of the portion embedded in the rubber 20 (the portion indicated by the dashed line) was measured, and the average of the maximum and minimum pull-out loads was taken as the pull-out force.
[0061] (Initial adhesive strength) The pull-out strength of the test sample left at room temperature within one week after vulcanization was taken as the initial adhesive strength.
[0062] (Adhesive strength after deterioration) The adhesive strength after deterioration treatment was evaluated by immersing the test sample in distilled water at 80°C for 7 days, then removing it and conducting a pull-out test within one day.
[0063] (Detachment length after corrosion) The length of the portion of the plated steel wire that was not covered with rubber from the corroded end 11 of the plated steel wire that was pulled out after the deterioration test was measured, and the peeling length of the plated steel wire from the rubber due to corrosion (peeling length after corrosion, separation length) was calculated.
[0064] The initial adhesive strength and adhesive strength after deterioration were evaluated using an index with the initial adhesive strength value of test sample (No. 15) using diffusion brass-plated steel wire with a Cu concentration of 64% set as 100, and the peel length from the rubber after deterioration was evaluated using an index with the value of test sample (No. 15) using diffusion brass-plated steel wire with a Cu concentration of 64% set as 100. An initial bond strength index of less than 90 was judged as "poor," 90 to 110 was judged as "equal," and over 110 was judged as "good." If the adhesive strength index after deterioration was less than 50, the adhesive deterioration was judged to be significant. The peel length from the rubber was judged based on No. 15 as "good" if the peel length was less than 70, "same" if it was 70 to 130, and "poor" if it was over 130.
[0065] <Observation of the rubber / steel wire interface> The state of the interface between the rubber and the steel wire in the rubber composite was observed as follows. The cross section of the plated steel wire pulled out of the rubber test sample was processed with a CP and observed at 30,000x magnification with an SEM. The backscattered electron image identified the sulfide layer (adhesive layer) in contact with the rubber and the coating layer in contact with the base steel (steel wire). Figure 5 shows an example of a backscattered electron image. Each layer was spot analyzed by EDS to quantify Cu, Zn, and S.
[0066] The steel material, coating layer, adhesive layer, plating layer, and evaluation results are shown in Table 3.
[0067] [Table 3]
[0068] <Example of the present invention> The adhesive properties of all rubber composites using the plated steel wire in this disclosure were equivalent to those of the rubber composite using the brass-plated steel wire of the comparative material No. 15, with respect to both initial adhesive strength and adhesive strength after deterioration. The peeling length of the rubber after corrosion was reduced by almost half, and separation from the rubber was suppressed. No. 5 had a high Zn content in the coating layer, so its adhesion deterioration strength was equivalent to that of the standard No. 15, but the peeling length after corrosion was improved. Nos. 9 and 10 have a thick adhesive layer, so the adhesive strength after deterioration treatment is equivalent to that of the standard No. 15, but the peeling length after corrosion has been improved.
[0069] <Comparative Example> No. 15 is a rubber composite using diffusion brass-plated steel wire, and was assigned an initial adhesive strength of 100. The peel length after corrosion was also assigned a standard of 100, but the adhesive strength after corrosion decreased to 50. Nos. 16 to 19, 22, 24, and 25 all have different Zn and Cu compositions in the plating layer, but all are diffusion brass plating, and the Zn content of the coating layer in the rubber composite was low, resulting in a large peeling length from the rubber after corrosion. No. 17 is an example in which the Zn ratio of the coating layer was low, resulting in a long peeling length after corrosion. No. 18 is an example in which the Zn ratio of the coating layer was even lower, resulting in low adhesive strength after deterioration and significant peeling after corrosion. No. 19 is a diffusion brass plating with a low Cu content, and the plating layer peeled off during wire drawing, resulting in a large decrease in adhesive strength with the rubber and peeling after corrosion. No. 20 is a Cu-plated material, and is an example in which the initial adhesion and adhesive strength decreased after deterioration. No. 21 is a Zn-plated material, and is an example in which the adhesive strength after deterioration was significantly reduced due to corrosion of the Zn layer, and peeling from the rubber after corrosion became significantly large. No. 22 is a diffusion brass plated product, but the Cu content in the plating was high, resulting in a decrease in strength after adhesion deterioration and significant peeling from the rubber after corrosion. No. 23 is a thick diffusion plating with a high Zn ratio. The Cu content of the adhesive layer is low, which reduces the adhesive strength. Furthermore, due to deterioration treatment and corrosion, the oxidation of Zn has progressed, resulting in increased adhesive strength after deterioration and peeling from the rubber due to corrosion. No.24 is a copper-plated brass surface, and the copper on the surface reacted excessively, reducing the initial adhesion and the adhesive strength after deterioration, and causing significant peeling from the rubber after corrosion. In other words, the adhesive layer had a high Cu / S ratio, the copper reaction proceeded, and the coating layer was thin, causing significant peeling from the rubber after corrosion. No. 25 is an example in which the plating thickness was thin, the film became thin, and the film had low corrosion resistance, resulting in significant peeling from the rubber after corrosion.
[0070] The disclosure of Japanese Patent Application No. 2021-149713, filed on September 14, 2021, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated herein by reference. [Explanation of symbols]
[0071] 2. Steel Wire 4. Coating Layer 6 Adhesive layer 8 Rubber part 10. Galvanized steel wire 11 Rubber end with embedded galvanized steel wire 20 Vulcanized rubber S Test sample (rubber composite)
Claims
1. A rubber composite comprising a plated steel wire having a plating layer formed on a surface of the steel wire and a vulcanized rubber coating the plated steel wire, When a cross section perpendicular to the longitudinal direction of the rubber composite is observed using a backscattered electron image obtained by a field emission scanning electron microscope, the rubber composite includes a coating layer between the vulcanized rubber and the steel wire, the coating layer being in contact with the steel wire, and an adhesive layer between the vulcanized rubber and the coating layer, In the adhesive layer, when the total mass of Cu, Zn, and S in the adhesive layer is taken as 100, a mass ratio of Cu to a mass ratio of S (Cu mass ratio / S mass ratio) is 1.0 to 4.0; The coating layer has a mass ratio of Zn of more than 65 to 90 when the total mass of Cu, Zn, and S in the coating layer is 100; Rubber composite.
2. The adhesive layer has a thickness of 50 to 500 nm; The thickness of the coating layer is 100 to 500 nm; The rubber composite of claim 1.
3. A plated steel wire manufacturing process for manufacturing a two-layer plated steel wire by the following method A or the following method B; a rubber composition coating step of coating a surface of the two-layer plated steel wire with a rubber composition; a vulcanization step of vulcanizing the rubber composition coated on the surface of the two-layer plated steel wire to bond the vulcanized rubber and the two-layer plated steel wire; Including, The method A includes a Zn plating step of forming a Zn plating layer on a surface of a drawn wire material to obtain a Zn-plated drawn wire material, a Cu plating step of forming a Cu plating layer on the surface of the Zn-plated drawn wire material to obtain a two-layer plated drawn wire material, and a wire drawing step of wet drawing the two-layer plated drawn wire material without heating to obtain the two-layer plated steel wire, The method B is a method for producing a rubber composite, which includes a Zn plating step of forming a Zn plating layer on the surface of a drawn wire material to obtain a Zn-plated drawn wire material, a wire drawing step of wet-drawing the Zn-plated drawn wire material to obtain a Zn-plated steel wire, and a Cu plating step of forming a Cu plating layer on the surface of the Zn-plated steel wire to obtain the two-layer plated steel wire.
4. The method for producing a rubber composite according to claim 3, wherein the two-layer plated steel wire is produced by the method A in the plated steel wire production step.
5. The method for producing a rubber composite according to claim 3, wherein the two-layer plated steel wire is produced by the B method in the plated steel wire production step.
Citation Information
Patent Citations
Radial tire bead wire containing surface coating and preparation method of radial tire bead wire
CN113005494A
Reinforcement for rubber
JP1986287932A
Method for manufacturing brass-plated steel wire, steel cord, and tire
JP2008200729A