Method for producing rubber composition, rubber composition produced by said method, and tire produced using said rubber composition
By dispersing polybutene in water-based emulsions with ESBR rubber, the method addresses uniform dispersion issues, resulting in rubber compositions with improved grip and wear performance, suitable for tire manufacturing.
Patent Information
- Application Number
- JP2021106457
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-15
- Filing Date
- 2021-06-28
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2041-06-28
AI Technical Summary
Existing rubber manufacturing processes using ESBR and natural rubber face challenges in achieving uniform dispersion of hydrophobic resins and oils in water-based solutions, leading to suboptimal physical properties in final products like tires and shoe soles.
A method involving the dispersion of polybutene in water-based emulsions with ESBR rubber, using a hydrophobic extender oil and polybutene emulsion, followed by salting out and acid precipitation to create a uniformly mixed rubber composition, which is then dried and molded, enhancing the physical properties of the final product.
The resulting rubber composition exhibits improved grip, reduced rolling resistance, and enhanced wear performance, while maintaining environmental friendliness and cost-effectiveness by utilizing existing equipment and processes.
Smart Images

Figure 0007579214000001 
Figure 0007579214000002 
Figure 0007579214000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a rubber composition, a rubber composition produced by the method, and a tire produced using the same. [Background technology]
[0002] In general, products using ESBR and natural rubber include tires, soles, belts, hoses, sheets, sealants, and adhesives that require excellent adhesion, all of which must have excellent durability. To complete these products, it is common to mix the raw rubber and processing aids, including reinforcing materials and additives, directly into a compounder to produce a bulk state, or to mix them together after producing a masterbatch to produce the final rubber composite product. Patent Document 1 (Korean Patent Publication No. 10-2020-0031529) presents the results of improving the performance of rubber composites by dispersing hydrocarbon traction resin in ESBR. However, the types of resins that are extended include coumarone-indene resins, petroleum-based resins, terpene polymers, α-methylstyrene resins, and mixtures thereof, all of which have a glass transition temperature (Tg) exceeding 30°C. These generally dissolve well in organic solvents, so rubbers manufactured by solution polymerization, such as solution styrene butadiene rubber (SSBR), styrene-butadiene-styrene rubber (SBS), styrene-ethylene-butadiene-styrene rubber (SEBS), butadiene rubber (BR), butyl rubber (IR), isoprene-isobutylene rubber (IIR), ethylene propylene rubber (EPM), ethylene propylene diene rubber (EPDM) and polyolefin elastomer (POE), can be easily manufactured into solidified products by dissolving the resin in an organic solvent, extending it in the solution phase, and then removing the solvent.
[0003] However, in order to manufacture ESBR, which is a product that uses water as a solvent during rubber manufacturing, and to extend hydrophobic oil and resin for functionality to natural rubber latex obtained from nature to produce a solidified ESBR product, uniform dispersion is possible only when the oil and resin to be extended are dispersed in water using an emulsifier on SBR latex polymer from which unreacted monomers such as styrene and butadiene have been removed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Korean Patent Publication No. 10-2020-0031529 Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention relates to a method for producing a polybutene (PIB) extended rubber composition that uses water as a solvent and can improve the physical properties of synthetic rubber and natural rubber, a rubber composition produced by the method, and a tire produced using the same. [Means for solving the problem]
[0006] In order to achieve the object of the present invention, the present invention provides a method for producing a rubber composition in which polybutene is dispersed in a solution state in rubber (PIB extended rubber); the rubber is emulsion styrene butadiene rubber (ESBR), and the aromatic content in the oil is 5 to 25 wt %; NaphtheneThe method includes the steps of dispersing a hydrophobic extender oil having a paraffin content of 25 to 45% by weight and a paraffin content of 35 to 65% by weight and polybutene in water to prepare an extender oil / polybutene emulsion (1); adding the extender oil / polybutene emulsion (1) to an ESBR rubber composition (2) in the form of a latex and dispersing it uniformly in a solution state to prepare an ESBR rubber / extender oil / polybutene composition; and solidifying the ESBR rubber / extender oil / polybutene composition in the form of a latex through salting out and acid precipitation, drying and molding the composition. The polybutene is a highly reactive polybutene having a number average molecular weight of 150 to 3,000 g / mol, in which the carbon-carbon double bonds are mainly located at the terminals of the polybutene PIB. A method for making a rubber composition is provided.
[0010] According to one embodiment, the latex form ESBR The rubber composition (2) is preferably produced by including a step of recovering residual monomers after emulsion polymerization of a composition containing monomers, water, an emulsifier and additives.
[0011] According to an embodiment, the monomer for preparing the rubber composition is preferably at least one selected from the group consisting of styrene, α-methylstyrene, butadiene, isoprene, acrylonitrile, methyl methacrylate, methyl methacrylic acid, and chloroprene.
[0012] According to an embodiment, the polybutene has a number average molecular weight of 300 to 3,000 g / mol, and is preferably added in an amount of 1 to 10 wt % based on the rubber content.
[0013] According to an embodiment of the present invention, the rubber composition prepared according to the present invention is preferably used as a rubber composition for tire treads, a rubber composition for shoe soles, a rubber composition for belts, or a rubber composition for asphalt additives.
[0014] In order to achieve yet another object of the present invention, the present invention provides a rubber composition for a tire tread, which comprises the rubber composition produced according to the present invention.
[0015] In order to achieve still another object of the present invention, there is provided a tire manufactured using the rubber composition for tire tread according to the present invention.
[0016] According to one embodiment of the present invention, the polybutene is a C4 polymer using isobutylene as a main monomer, has a number average molecular weight of 300 to 3,000 g / mol, and can be added in an amount of 0.1 to 27.3 wt% based on the rubber content, and preferably is added in an amount of 1 to 10 wt%. Effect of the Invention
[0017] The rubber composition produced according to the present invention can improve the physical properties of the final rubber product. In addition, a tire produced from the rubber composition produced according to the present invention has improved grip (ground contact on wet roads), fuel efficiency, and wear performance. In addition, the method for producing the rubber composition according to the present invention can use existing equipment while dramatically improving the physical properties of the rubber product, thereby significantly reducing the unit price, and is environmentally friendly by utilizing polybutene, an environmentally friendly resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will now be described in more detail, but this is for the purpose of explaining the present invention and is not intended to limit the scope of the present invention.
[0019] The present invention provides a method for producing a polybutene-dispersed rubber composition in which polybutene is dispersed in rubber in the form of a solution (PIB extended rubber), comprising the steps of: dispersing a hydrophobic extender oil and polybutene in water to produce an extender oil / polybutene emulsion (1); adding the extender oil / polybutene emulsion (1) to a rubber composition in the form of a latex and dispersing it uniformly in the form of a solution to produce a rubber / extender oil / polybutene composition; and solidifying the rubber / extender oil / polybutene composition in the form of a latex through salting out and acid precipitation, drying and molding.
[0020] <Extender oil / polybutene solution and commercialization> The advantage of the present invention is that a rubber composition that can provide rubber with desired excellent physical properties can be produced by simply changing the process of producing an extender oil emulsion by adding polybutene without changing the raw materials and process in the existing extender oil emulsion production process.
[0021] It is essential to change the existing process of dispersing hydrophobic extender oil in water to produce an emulsion by dispersing polybutene together with extender oil in water to produce an extender oil / polybutene emulsion.
[0022] According to the present invention, such a process has the advantage that existing equipment can be utilized, and the physical properties of the rubber obtained by such a process change show unexpected and surprising effects.
[0023] In addition, in the present invention, it is necessary to go through an intermediate step of adding the polybutene emulsion to a rubber composition in the form of a latex to prepare a rubber / extender oil / polybutene composition in a homogeneous mixture.
[0024] Here, the "latex-form rubber composition" as used herein refers to a synthetic rubber composition produced by emulsion polymerization in a form in which micelles containing rubber particles are dispersed in an aqueous solution, and has a milk-like form, and includes natural rubber latex.
[0025] The rubber / extender oil / polybutene composition is solidified into a latex form through salting out and acid precipitation, and then dried and molded to produce a rubber composition in which polybutene is uniformly dispersed. Only by using the rubber composition thus produced can rubber with the desired final properties be obtained.
[0026] Here, the final physical properties may vary depending on the type of rubber product. For example, when the final rubber product is a tire tread, excellent braking properties and low fuel consumption properties are required, so durability, grip, and low rolling resistance are important.
[0027] Therefore, in the present invention, when a tire tread is to be manufactured, a rubber composition for manufacturing the tire tread must be manufactured, and when the rubber composition for the tire tread is manufactured, a step must be included in which the rubber used is mixed with a rubber latex intermediate from which unreacted monomers have been removed after the preparation of a polybutene (PIB) emulsion, solidified through salting out and acid precipitation, and then dried and molded to manufacture an ESBR rubber composition. The rubber that can be used when manufacturing the tire tread can be synthetic rubber, natural rubber, or a mixture of natural rubber and synthetic rubber.
[0028] The natural rubber may be a general natural rubber or a modified natural rubber. Any general natural rubber known as natural rubber may be used, and the place of origin is not limited. The natural rubber mainly contains cis-1,4-polyisoprene, but may contain trans-1,4-polyisoprene depending on the required characteristics. Therefore, the natural rubber may include natural rubber mainly containing trans-1,4-isoprene, such as balata, a type of rubber of the Sapotaceae family found in South America, in addition to natural rubber mainly containing cis-1,4-polyisoprene.
[0029] The modified natural rubber means a rubber obtained by modifying or refining the general natural rubber. For example, the modified natural rubber may be epoxidized natural rubber (ENR), deproteinized natural rubber (DPNR), hydrogenated natural rubber, etc.
[0030] Synthetic rubbers include styrene butadiene rubber (ESBR, SSBR), modified styrene butadiene rubber, butadiene rubber (BR), modified butadiene rubber, chlorosulfonated polyethylene rubber, epichlorohydrin rubber, silicone rubber, nitrile rubber, hydrogenated nitrile rubber, nitrile butadiene rubber (NBR), modified nitrile butadiene rubber, styrene-butadiene-styrene rubber (SBS), styrene ethylene butylene styrene (SEBS) rubber, ethylene propylene rubber (EPM), ethylene propylene diene (EPDM) rubber, hypalon rubber, chloroprene rubber, ethylene vinyl acetate rubber, acrylic rubber, hydrin rubber, vinylbenzyl chloride styrene butadiene rubber, bromomethylstyrene butyl rubber, maleic acid styrene butadiene rubber, carboxylic acid styrene butadiene rubber, epoxy isoprene rubber, maleic acid ethylene propylene rubber, carboxylic acid nitrile butadiene rubber, brominated polyisobutyl isoprene-coparamethylstyrene, BIMS), and combinations thereof.
[0031] The polybutene (PIB) , high As the reactive polybutene (HRPIB), a polybutene having a number average molecular weight of 150 to 3,000 g / mol, preferably 300 to 3,000 g / mol, can be used. In the highly reactive polybutene (PIB), the carbon-carbon double bonds are mainly located at the terminals of the polybutene (PIB), so that the bonding with the raw rubber increases during the reaction, and the bonding strength is improved compared to the conventional polybutene (CPIB). * This is because it has an advantageous effect compared to polybutenes having an α-double bond content of less than 40%. Thus, polybutenes can also be used in different ways depending on the desired physical properties of the final rubber product.
[0032] According to one embodiment of the present invention, polybutene is a C4 polymer having a number average molecular weight of 300 to 3,000 g / mol, and can be added in an amount of 0.1 to 27.3 wt% of the rubber content, and preferably 1 to 10 wt%.
[0033] If the polymer is contained in an amount less than 1 wt% relative to the rubber content, the physical properties of the final rubber product will not be significantly improved, whereas if it is contained in an amount more than 10 wt%, the inherent physical properties of the rubber may not be exhibited.
[0034] For example, the ratio of extender oil contained in commercially produced oil-extended rubber is mostly 37.5 phr. Therefore, in order to include 1 wt% polybutene (1.4 phr relative to rubber) in the rubber that extends the extender oil / polybutene, the extender oil / polybutene ratio in the extender oil / polybutene emulsion is 173 / 7 (TDAE 346g / polybutene 14g) to extend 1 wt% polybutene in the rubber. In this case, the concentration of the extender oil / polybutene produced is adjusted by adding water.
[0035] The latex-form rubber composition is preferably produced by emulsion polymerization of a composition containing monomers, water, an emulsifier, and additives, and then recovering residual monomers.
[0036] According to an embodiment of the present invention, the monomer for preparing the rubber composition is preferably at least one selected from the group consisting of styrene, α-methylstyrene, butadiene, isoprene, acrylonitrile, methyl methacrylate, methyl methacrylic acid, and chloroprene.
[0037] According to an embodiment of the present invention, the rubber composition is preferably used as a rubber composition for tire treads, industrial belts, and the like.
[0038] In order to achieve yet another object of the present invention, there is provided a rubber composition for a tire tread, which comprises the ESBR rubber composition produced according to the present invention.
[0039] The rubber composition for tire treads according to one embodiment of the present invention may contain, in addition to the raw rubber and highly reactive polybutene (HRPIB) described above, rubber compounding ingredients that are generally used in rubber compositions for tire treads, such as silica and / or carbon black as reinforcing fillers, process oil as a softener, sulfur as a vulcanizing agent, CBS and 1,3-diphenylguanidine (DPG) as vulcanization accelerators, zinc oxide and stearic acid as vulcanization activators, a coupling agent for improving dispersibility, and an antioxidant.
[0040] The type of silica that can be used as a reinforcing filler in the present invention is not particularly limited, but it is preferably silica having a surface area of 175±5 m 2 / g, a moisture content of 6.0±0.5 wt.%, and a silicon dioxide (SiO2) content of 90 wt.% or more.
[0041] The carbon black used in the present invention is not particularly limited in type, but preferably has a BET (Brunauer-Emmett-Teller) specific surface area of 80 to 90 m 2 It is preferable that the carbon black has a molecular weight of 100 to 110 g / 100 g, a DBP (Di-n-bibutyl Phthalate) adsorption value of 100 to 110 g / 100 g, and an iodine adsorption value of 90 to 120 mg / g. It is preferable to use 40 to 100 parts by weight of the carbon black per 100 parts by weight of raw rubber, but if the amount used is less than 40 parts by weight, it is not preferable because a sufficient reinforcing effect is not exhibited, and if the amount used exceeds 100 parts by weight, it is not preferable because heat generation and wear resistance effects are not exhibited.
[0042] The extender oil acts as a softener and has an aromatic content of 5 to 25% by weight. Naphthene The content of the paraffinic component is preferably 25 to 45% by weight, and the content of the paraffinic component is preferably 35 to 65% by weight. The various additives used in the present invention are general components used in rubber compositions for tire treads, and the detailed content thereof will be omitted.
[0043] As described above, the rubber composition for tire treads according to the present invention does not affect various basic physical properties of tires, and improves the grip, fuel economy and wear performance of the tread portion of automobile tires, while enabling these properties to be sustained.
[0044] In order to achieve still another object of the present invention, there is provided a tire manufactured using the rubber composition for tire tread according to the present invention.
[0045] The present invention will be described in more detail below with reference to specific examples and comparative examples, which are merely for the purpose of making the present invention easier to understand and are not intended to limit the scope of the present invention. EXAMPLES
[0046] <Production Example 1: Production of ESBR latex> In a 10L pressure reactor equipped with a mechanical stirrer at 5℃, 3200mL of deionized water, 46g of potassium rosinate, 74g of potassium fatty acid, 7.0g of potassium chloride, 560g of styrene, 1440g of butadiene, 1.0g of EDTA, 1.0g of sodium hydrosulfite, 0.2g of iron sulfate, 0.6g of sodium formaldehyde sulfonate, 2.0g of tert-dodecyl mercaptan, and 1.2g of methane hydroperoxide were added and stirred for 8 hours. 2.0g of diethylhydroxyamine was added to stop the reaction. Thereafter, the unreacted butadiene was removed by increasing the temperature of the reactor to 20°C while stirring, and the unreacted styrene was removed by distillation under reduced pressure to produce a styrene-butadiene latex with a weight average molecular weight of 1,058,000g / mol, MWD of 4.2, a styrene content of 23.6%, and a total solid content (TSC) of 25%.
[0047] <Production Example 2: Production of extender oil / polybutene emulsion> In a 1L glass reactor equipped with a mechanical stirrer, 46ml of water from which cations have been removed at 60℃, 3.1ml of 25wt% caustic soda water (NaOH aqueous solution), and 7.1g of distilled tall oil (DTO) are added and stirred until complete saponification. After confirming that the DTO is completely emulsified in the water, 360g of TDAE oil heated to 60℃, 4.2g of antioxidant K-13, and 180ml of water are added and stirred vigorously for 30 minutes to produce an emulsion of the extender oil. An emulsion containing extender oil / polybutene is produced by replacing a certain portion of the extender oil with polybutene at the extension oil addition stage. The extender oil / polybutene can be extended into rubber by adjusting the ratio of extender oil / polybutene contained in the extender oil / polybutene emulsion. At this time, the concentration of the produced extender oil / polybutene is adjusted by adding additional water.
[0048] <Production Example 3: Extending Oil / Production of Polybutene-Extended ESBR> Polymerization was carried out in a 4L wide-mouth glass reactor equipped with a mechanical stirrer while maintaining the temperature at 60°C, and then 800g of styrene-butadiene latex (latex-shaped rubber composition) prepared in Preparation Example 1 was added and heated to 60°C. 200g of 60°C extender oil / polybutene emulsion prepared in Preparation Example 2 was added to the heated latex and stirred for 10 minutes. Then, 500ml of 60°C saturated aqueous sodium chloride solution was added to salt out, and dilute sulfuric acid was added until the pH reached 4, and an acidification process was carried out stepwise to produce ESBR rubber particles in which the extender oil / polybutene was extended in a water-like state. The rubber particles were separated and washed three times with cation-removed water at 60°C, and the particles were separated and dried in a hot air dryer at 100°C to produce an ESBR sample in which the extender oil / polybutene was extended by 37.5phr.
[0049] <Comparative Manufacturing Example 1> An extended oil emulsion was produced in the same manner as in Production Example 2, except that only TDAE oil was used.
[0050] <Comparative Example 1: ESBR extended with TDAE oil only> An ESBR sample was produced in the same manner as in Production Example 3 using the ESBR latex of Production Example 1 and the extended oil emulsion produced using only the TDAE oil of Comparative Production Example 1.
[0051] Example 1: Oil-extended ESBR containing 1 wt% PIB The ESBR latex of Production Example 1 was subjected to the method of Production Example 2, except that the extender oil (TDAE) was 346 g / polybutene (HRPIB470 * An ESBR sample was produced in the same manner as in Production Example 3 using the extender oil / polybutene emulsion produced by adding 14 g of 1,2-dichlorophenyl ether.
[0052] *Polybutene: Hanwha Total Co., Ltd. HRPIB470 HRPIB470:high reactive PIB(Mn 1,300g / mol)
[0053] Example 2: Oil-extended ESBR containing 3 wt% PIB The method of Preparation Example 2 was applied to the ESBR latex of Preparation Example 1. However, an ESBR sample was produced in the same manner as Preparation Example 3 using an extender oil / polybutene emulsion produced by adding 320 g of extender oil (TDAE) / 40 g of polybutene (HRPIB470).
[0054] Example 3: Oil-extended ESBR containing 5 wt% PIB The same method as in Preparation Example 2 was applied to the ESBR latex of Preparation Example 1. However, an ESBR sample was produced in the same manner as in Preparation Example 3 using an extender oil / polybutene emulsion produced by adding 294 g of extender oil (TDAE) / 66 g of polybutene (HRPIB470).
[0055] Example 4: Oil-extended ESBR containing 10 wt% PIB The same method as in Preparation Example 2 was applied to the ESBR latex of Preparation Example 1. However, an ESBR sample was produced in the same manner as in Preparation Example 3 using an extender oil / polybutene emulsion produced by adding 228 g of extender oil (TDAE) / 132 g of polybutene (HRPIB470).
[0056] The extender oil / polybutene contents of the ESBR samples prepared in the Examples and Comparative Examples are shown in Table 1.
[0057] [Table 1]
[0058] <Composition Evaluation: Comparative Example 1 and Examples 1 to 4> A composite material before crosslinking was produced using the composition in Table 2 using Moriyama's MIX-LABO (mixing capacity: 0.5 liter, main motor: 15 HP).
[0059] [Table 2]
[0060] The compounding was carried out in two stages. In the first mixing, a 0.5 L compounder was filled to 75% by volume, and the rubber composition, filler (silica), zinc oxide (ZnO), stearic acid, and silane coupling agent (Si-69) were added with the rotor rotating at 70 rpm to obtain the primary rubber composition.
[0061] In the second mixing, the mixture was cooled to room temperature, and sulfur, DPG (diphenyl guanidine), CBS (N-cyclohexyl-2-benzothiazole sulfonamide), and an antioxidant (6-PPD) were added at 90°C or less, and the mixture was mixed at 50 rpm for 2 minutes.
[0062] To crosslink the compounded rubber composites, the vulcanization characteristics were measured using a Rubber Process Analyzer (RPA) at 160°C, 40 minutes, and a deformation rate of 1%, and each rubber composite was crosslinked in a high-temperature press at 160°C for a time period equal to 90 seconds added to the T90 time obtained by adding 10 seconds to the T90 time, to produce test pieces of rubber composites for tire treads.
[0063] As other additives, 3 parts by weight of zinc oxide (ZnO), 2 parts by weight of stearic acid (St-A), 50 parts by weight of silica (VN3, Evonik), and 4 parts by weight of silica coupling agent (SI-69) were added to 100 parts by weight of rubber composition containing SBR, BR, and PIB to prepare a first compound (silica master batch, SMB). Depending on the content of polybutene, 1.5 to 2.0 parts by weight of sulfur, 1.8 parts by weight of vulcanization accelerator diphenyl guanidine (DPG), 1.8 parts by weight of cyclohexyl benzothiazole sulfenamide (CBS), and 0.2 parts by weight of antioxidant (6PPD) were further added to the first compound to prepare a second compound (final master batch, FMB).
[0064] <Experimental Example> The test pieces of each rubber composite material prepared in the comparative examples and examples were measured for physical properties according to the relevant ASTM regulations as follows, and the results are shown in Table 3 below.
[0065] (1) Mixed viscosity (Mooney viscosity, MV): Using a Mooney viscometer (MV2000, Alpha Technology), the Mooney viscosity was measured by measuring and interpreting the value from 1 minute of preheating with a large rotor at 100°C until 4 minutes after the rotor was started.
[0066] (2) Crosslink density: For crosslinking of compounded rubber composite material, it was measured by subtracting the minimum value from the maximum value of the torque value during measuring crosslinking characteristics under the conditions of 160℃, 40 minutes, and 1% deformation rate using a Rubber Process Analyzer (RPA).
[0067] (3) Hardness: The hardness test was carried out in accordance with JIS K6253 (2001) to measure the spring hardness HA (Shore-A hardness).
[0068] (4) Modulus: The modulus was measured by cutting the test piece into a dumbbell shape and using a tensile tester manufactured by Instron Corp. The 100% and 200% moduli refer to the stress acting on the test piece when the test piece is elongated by 100% and 200%, respectively.
[0069] (5) Tensile strength: For the tensile strength, a No. 3 dumbbell test piece as specified in JIS K6251 (2001) was prepared by punching a vulcanized rubber sheet. Using this test piece, a tensile test was carried out according to the method specified in JIS K6251 at a measurement temperature of 25°C and a tensile speed of 500 mm / min, and the 100% modulus (M100), 200% modulus (M200), the stress at tensile break TB, and the elongation at tensile break EB were measured.
[0070] (6) Elongation: Measured as the deformation rate (%) up to the breaking point when measuring tensile strength.
[0071] (7) Viscoelasticity: Viscoelasticity is measured using dynamic mechanical analysis (DMA). 0°C Tan δ is used as a proxy for tire braking performance on wet roads, with a higher value indicating better performance. 60°C Tan δ is used as a proxy for tire rolling resistance, with a lower value indicating better rolling resistance and improved fuel efficiency.
[0072] (8) Abrasion: Abrasion is measured by applying a load of 5N using a DIN abrasion tester in accordance with the ASTM D5963 method to measure the weight lost due to abrasion. The weight loss is expressed as a relative index. The higher the index value, the better the abrasion performance.
[0073] [Table 3]
[0074] As shown in Table 3, ESBR rubber with PIB extension has improved durability, grip, and low rolling resistance compared to rubber without PIB, resulting in excellent braking characteristics, fuel efficiency, and wear performance. [Industrial Applicability]
[0075] INDUSTRIAL APPLICABILITY The present invention can be used in a method for producing a rubber composition, a rubber composition produced by the method, and a tire produced using the same.
Claims
1. A method for producing a polybutene-dispersed rubber composition in which polybutene is dispersed in a solution state in rubber (PIB extended rubber), comprising the steps of: the rubber is emulsion styrene butadiene rubber (ESBR); A step of dispersing a hydrophobic extender oil having an aromatic content of 5-25 wt%, a naphthene content of 25-45 wt%, and a paraffin content of 35-65 wt% in the oil and polybutene in water to prepare an extender oil / polybutene emulsion (1); The extender oil / polybutene emulsion (1) is added to an ESBR rubber composition (2) in the form of a latex, and uniformly dispersed in a solution state to produce an ESBR rubber / extender oil / polybutene composition; and The ESBR rubber / extender oil / polybutene composition is solidified in a latex state through salting out and acid precipitation, and then dried and molded; The method for producing a rubber composition is characterized in that the polybutene is a highly reactive polybutene in which carbon-carbon double bonds are mainly located at the terminals of polybutene PIB and the number average molecular weight is 150 to 3,000 g / mol.
2. The method for producing a rubber composition according to claim 1, wherein the ESBR rubber composition (2) in the form of a latex is produced by emulsion polymerization of a composition containing a monomer, water, an emulsifier and an additive, and then recovering the residual monomer.
3. The method for producing a rubber composition according to claim 1, wherein the highly reactive polybutene has a number average molecular weight of 300 to 3,000 g / mol, and is added in an amount of 1 to 10 wt % based on the rubber content.
4. The method for producing a rubber composition according to any one of claims 1 to 3, wherein the rubber composition is used as a rubber composition for tire treads, a rubber composition for shoe soles, a rubber composition for belts, or a rubber composition for asphalt additives.
5. A rubber composition for a tire tread, comprising the rubber composition produced by the method according to any one of claims 1 to 3.
6. A tire produced using the rubber composition for a tire tread according to claim 5.
Citation Information
Patent Citations
Image processing method of computer graphics
JP1986020949A
Manufacturing method of rubber composition
JP2007297416A
Rubber composition for tire tread and pneumatic tire having tread produced by using the same
JP2008255168A
Unvulcanized rubber composition for inner liner and pneumatic tire
JP2016098296A
Rubber composition for tire tread and tire manufactured using the same
JP2020029555A