Polymer electrolytes for improved performance lithium metal polymer batteries
A crosslinked copolymer of poly(alkylene oxide) and lithium polystyrene-sulfonyl(trifluoromethylsulfonyl)imide addresses mechanical and conductivity issues in lithium metal polymer batteries, enhancing performance and safety by reducing dendrite formation and allowing operation at lower temperatures.
Patent Information
- Application Number
- JP2021524185
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-11-27
- Filing Date
- 2019-11-25
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2039-11-25
AI Technical Summary
Lithium metal polymer batteries face issues with mechanical stability and low ionic conductivity due to poly(ethylene oxide) (PEO)-based electrolytes, leading to poor performance at elevated temperatures and potential dendrite formation, which can cause short circuits.
A crosslinked copolymer comprising poly(alkylene oxide) and lithium polystyrene-sulfonyl(trifluoromethylsulfonyl)imide (PSTFSILi) units, with controlled polymerization to achieve high cation transference number, improved mechanical strength, and enhanced ionic conductivity.
The crosslinked copolymer provides excellent mechanical strength, high ionic conductivity, and reduced dendrite formation, enabling safe and efficient operation of lithium metal polymer batteries at lower temperatures.
Smart Images

Figure 0007579246000022 
Figure 0007579246000023 
Figure 0007579246000024
Abstract
Description
[Technical field]
[0001] The present invention relates to a crosslinked copolymer comprising at least repeating units of poly(alkylene oxide) and at least repeating units of lithium polystyrene-sulfonyl(trifluoromethylsulfonyl)imide (PSTFSILi); a solid polymer electrolyte comprising said crosslinked copolymer, and the use of said crosslinked copolymer for the preparation of a battery (e.g., a lithium metal polymer (LMP) comprising said solid polymer electrolyte).
[0002] The invention finds application typically, but not exclusively, in the field of lithium metal polymer batteries, in particular in the manufacture of electric vehicles; and / or in the storage of intermittent energy of the solar and / or wind type.
[0003] Currently available lithium metal polymer batteries are in the form of several thin films wound or stacked together, with a thickness of the order of about 100 micrometers, and contain: a negative electrode (anode) that ensures the supply of lithium ions during discharge; a positive electrode (cathode) that acts as a receptacle into which the lithium ions are inserted; a lithium ion-conducting solid polymer electrolyte located between the positive and negative electrodes; and a current collector connected to the positive electrode to ensure electrical connection.
[0004] The negative electrode is usually made of a sheet of metallic lithium or a lithium alloy; the solid polymer electrolyte is usually made of a poly(ethylene oxide) (PEO)-based polymer and at least one lithium salt; the positive electrode usually comprises a metal oxide-based or phosphate-based electrode active material, for example of the LiMPO4 type (where M represents a metal cation selected from the group of Fe, Mn, Co, Ni, Ti and a combination of these cations, and optionally carbon); and the current collector is usually made of a metal sheet. Ionic conductivity is ensured by dissolving the lithium salt in the PEO.
[0005] However, at the temperatures (60 - 80 °C) typically used in LMP batteries, PEO becomes a viscous liquid and loses its dimensional stability, so it does not have sufficient mechanical strength.
[0006] Other PEO-based (co)polymers such as poly(ethylene oxide-stat-propylene oxide) type (i.e., PEO-stat-PPO) statistical copolymers; polystyrene-b-PEO type (i.e., PS-b-PEO) block copolymers; crosslinked PEO or copolymers containing acrylate or methacrylate chains, which are branched PEOs especially for strengthening mechanical properties, are described. It has also been proposed to add PEO-based polymer inorganic or organic particles, optionally on the nanometer scale, such as particles of aluminum oxide, titanium oxide or cellulose nanofibrils.
[0007] However, the ionic conductivity at 60 °C of electrolytes based on such polymers remains low. Only the use of a positive electrode with a low active material reference weight (low surface capacity) and a low current (<C / 15) makes it possible to recover the capacity at this temperature. Therefore, currently, the operating temperature for obtaining the performance corresponding to the intended use of batteries on the market is 80 °C.
[0008] Furthermore, mechanical properties deteriorated in tests to improve the conductivity of PEO by adding plasticizers.
[0009] Finally, in solid polymer electrolytes composed of lithium salts dissolved in a polyether polymer matrix such as PEO doped with lithium salts, the electrical performance is limited by the strong interaction between lithium cations and PEO chains, so the proportion of the charge carried by lithium ions (also called cation transference number) becomes low (on the order of 0.2). The value of the cation transference number determines the amount of current transported by cations.
[0010] A low cationic transport number leads to the formation of a salt concentration gradient across the electrolyte thickness during battery operation, which can lead to salt depletion at the electrodes, increasing electrolyte resistance, reducing power performance, promoting the formation of lithium dendrites, leading to reduced faradaic efficiency, and ultimately causing short circuits.
[0011] To solve this problem, US Pat. No. 5,999,366 describes diblock copolymers of the AB type or triblock copolymers of the BAB type. The A blocks are unsubstituted poly(ethylene oxide) chains with a number average molecular weight of less than or equal to 100 kDa. The B blocks are anionic polymers that can be prepared from one or more monomers selected from vinyl monomers and derivatives, said monomers being substituted with the anion of a lithium sulfonyl(trifluoromethylsulfonyl)imide (TFSILi) salt of the following formula:
[0012] [ka]
[0013] In the formula, * represents the attachment point of the anion of the salt to the monomer via a covalent bond or a linear alkyl chain having 1-5 carbon atoms. However, the aforementioned PEO-based AB-type diblock copolymers or BAB-type triblock copolymers have lower ionic conductivity than PEO alone, despite the transference number being equal to 1. Moreover, their mechanical strength is not optimized. [Prior art documents] [Patent documents]
[0014] [Patent Document 1] International Publication No. 2013 / 034848 Summary of the Invention
[0015] The object of the present invention is to overcome all or part of the aforementioned drawbacks of the prior art and to provide a polymeric material that can be used in batteries, in particular LMP batteries, in particular in solid polymer electrolytes, said polymeric material having good properties in terms of ionic conductivity, cationic transport number and mechanical strength, in particular at temperatures above 60° C.
[0016] It would also be desirable to reduce or eliminate dendritic growth in batteries, especially LMP batteries, to ensure good electrochemical performance, especially in terms of cycling behavior, faradaic efficiency, and to ensure that said batteries are completely safe to use.
[0017] These objectives are achieved by the invention described below.
[0018] A first subject of the present invention is a crosslinked copolymer, characterized in that it comprises at least recurring units of lithium polystyrene-sulfonyl(trifluoromethylsulfonyl)imide (PSTFSILi) and recurring units of a poly(alkylene oxide) chosen from the group consisting of poly(ethylene oxide) units, poly(propylene oxide) units, poly(ethylene and propylene) oxide units and mixtures thereof, said crosslinked copolymer being obtained by crosslinking a triblock copolymer of the BAB type:
[0019] - the A block is a crosslinkable poly(alkylene oxide) obtained from: * at least one monomer selected from ethylene glycol, propylene glycol, and mixtures thereof, or at least one poly(alkylene oxide) oligomer selected from one of poly(ethylene oxide), poly(propylene oxide), poly(ethylene and propylene) oxides, and mixtures thereof; and, * at least one compound containing at least one crosslinkable alkene or alkyne functional group; and,
[0020] Each B block is an anionic polystyrene substituted with the anion of sulfonyl(trifluoromethylsulfonyl)imide lithium salt (TFSILi) and corresponds to the following formula (I):
[0021] [ka]
[0022] In the formula, n represents the number of lithium styrene-sulfonyl(trifluoromethylsulfonyl)imide moieties in each B block.
[0023] Due to the combination of poly(alkylene oxide) repeating units and lithium polystyrene-sulfonyl(trifluoromethylsulfonyl)imide repeating units and crosslinking, the crosslinked copolymer has good properties in terms of cationic transport number, ionic conductivity, and mechanical strength, and can be used in solid polymer electrolytes and / or composite electrodes, especially for LMP batteries.
[0024] According to the invention, each B block preferably contains 4 to 31 moieties of lithium styrene-sulfonyl(trifluoromethylsulfonyl)imide (STFSILi), and even more preferentially 5 to 12 moieties of STFSILi. A very particularly preferred value is 8 moieties of STFSILi for each B block.
[0025] The number average molecular weight of the B block is preferentially in the range of 1.6 to 3.8 kDa.
[0026] The lithium salt LiTFSI is directly grafted onto polystyrene, so Li + The cationic transport number can be made to be 1, while, in particular, the cross-linking and the presence of poly(alkylene oxide) uniformly distributed in the copolymer ensure good mechanical strength and good ionic conductivity.
[0027] The crosslinked copolymer may contain about 10-50% by weight PSTFSILi, preferably about 13-28% by weight PSTFSILi, based on the total weight of the crosslinked copolymer.A particularly preferred value is about 22% by weight PSTFSILi.
[0028] The number average molecular weight of the A block is preferentially in the range from 10 to 50 kDa, even more preferentially in the range from 15 to 30 kDa, with a particularly preferred value of 20 kDa.
[0029] The A block preferably has a number average molecular weight of 25 kDa or less.
[0030] According to the invention, the A block preferably contains 227 to 1136 alkylene oxide moieties, and even more preferentially 340 to 681 alkylene oxide moieties. A very particularly preferred value is 454 alkylene oxide moieties.
[0031] The A blocks are preferably poly(ethylene oxide) or poly(ethylene and propylene) oxides, more preferably poly(ethylene oxide).
[0032] The A block preferably comprises a functional polymer of formula (II):
[0033] [ka]
[0034] In the formula, R 1is a substituent containing at least one crosslinkable alkene or alkyne functional group; CoA is a poly(alkylene oxide) chain selected from one of a poly(ethylene oxide) chain, a poly(propylene oxide) chain, a poly(ethylene and propylene) oxide chain, and a mixture thereof, preferably selected from a poly(ethylene oxide) chain, and a poly(ethylene and propylene) oxide chain, more preferably selected from a poly(ethylene oxide) chain; and p is 10-50, preferably 6-33, more preferably 12-15.
[0035] Thus, the A blocks contain crosslinkable functional groups uniformly distributed within said A blocks.
[0036] The poly(alkylene oxide) CoA chain is preferably linear.
[0037] Substituent R 1 can be selected from alkyl radicals containing at least one alkene or alkyne functional group, and the substituent R 1 contains 4 to 10 carbon atoms, preferably 4 to 6 carbon atoms.
[0038] According to a preferred embodiment of the invention, the functional polymer of formula (II) corresponds to the following formula (II-a):
[0039] [ka]
[0040] In the formula, y is 11 to 91, preferably 17 to 75, and more preferably 23 to 45. And, p is as defined in the present invention.
[0041] According to a particularly preferred embodiment of the invention, the A block corresponds to the following formula (II-b):
[0042] [ka]
[0043] wherein y and p are as defined in the present invention; M is a substituent containing a radical initiator capable of initiating the polymerization of the lithium styrene-sulfonyl(trifluoromethylsulfonyl)imide monomer of the B block and enabling the formation of a covalent bond between the A block and the B block.
[0044] The radical initiator of the substituent M can be selected from alkoxyamines and nitroxide-mediated radical initiators.
[0045] For example, radical initiators of the alkoxyamine type ensure the polymerization of the lithium styrene-sulfonyl(trifluoromethylsulfonyl)imide monomer in a controlled manner, thus making it possible to form a B block while combining it with an A block.
[0046] The substituent M can be selected from alkoxyamines. The CO alkoxyamine bond can be homolytically cleaved under the action of temperature to generate a nitroxide that acts as a mediator in the polymerization reaction and an initiator radical that adds to the monomer.
[0047] In particular, the substituent M corresponds to the following formula (III):
[0048] [ka]
[0049] where * indicates the point of attachment of M to the terminal oxygen of the A block of formula (II-b) and SG1 indicates a nitroxide radical of the formula:
[0050] [ka]
[0051] wherein ** indicates the point of attachment of SG1 to the -CH- radical of M in formula (III).
[0052] In the crosslinked copolymer according to the invention, the ratio of the number of moles of alkylene oxide to the number of moles of STFSILi (AO / Li) [the ratio of the number of moles of ethylene oxide to the number of moles of STFSILi (EO / Li)] is preferably in the range of 7 to 65, more preferably in the range of 10 to 50 and very particularly preferably in the range of 15 to 25.
[0053] The compound containing a crosslinkable alkene or alkyne functional group may be selected from compounds of formula (IV):
[0054] [ka]
[0055] In the formula, R' 1 is an alkyl group containing at least one alkene or alkyne functional group, said alkyl group containing 4 to 10 carbon atoms, preferably 4 to 6 carbon atoms; X and X' are the same or different and are independently selected from halogen, carboxylic acid, acyl chloride, ester and aldehyde functional groups.
[0056] X and X' are preferably the same.
[0057] According to a particularly preferred embodiment, X and X' are halogens, more preferably chlorine atoms.
[0058] As an example, compounds containing crosslinkable alkene or alkyne functional groups include 3-chloro-2-chloro Methyl -1-propene.
[0059] The A block may be obtained starting from at least one monomer selected from ethylene glycol, propylene glycol, and mixtures thereof, or at least one poly(alkylene oxide) oligomer selected from poly(ethylene oxide), poly(propylene oxide), poly(ethylene and propylene) oxides, and mixtures thereof, and at least one compound containing at least one crosslinkable alkene or alkyne functional group, preferably by polycondensation.
[0060] Poly(alkylene oxide) oligomers can be hydroxyl (-OH), thiol (-SH), primary amine (-NH2) or secondary amine (-NHR 2 ,R 2 =-CH3 or -C2H5), preferably containing end groups of the hydroxyl or primary amine type.
[0061] The alkylene oxide oligomers may have a molar mass up to about 5000 g / mol, preferably in the range of about 700 to 4000 g / mol, even more preferably in the range of about 1000 to 2000 g / mol.
[0062] According to one embodiment of the present invention, the alkylene oxide oligomer is selected from oligomers of the following formula: * H-[O-(CH2) x ] y’ -OH (wherein 2≦x≦4, preferably x=2; 10≦y′≦91, preferably 17≦y′≦75, more preferably 23≦y′≦45); * H-[O-CH2-CHR 3 ] y’’ -OH(in the formula, R 3 is an alkyl group having 1 to 3 carbon atoms, preferably a methyl group; 7≦y″≦69, preferably 10≦y″≦34, more preferably 17≦y″≦27;
[0063] * H-[O-(CH2) z -O-(CH2-CHR 4 ) u ]w -OH (wherein 1≦z≦4, preferably z=1 or 2; 1≦u≦2, preferably u=1; w is the molecular weight of the oligomer in the range of about 700 to 4000 g / mol, preferably about 1000 to 2000 g / mol, more preferably 2≦w≦23; R 4 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, preferably a hydrogen atom or a methyl group; -(CH2) z - and - (CH2-CHR 3 ) u - is understood to mean a different aliphatic chain);
[0064] *NH2-CHR 5 -CH2-[O-CH2-CHR 5 ] w’ -NH2(wherein, R 5 is an alkyl group having 1 to 3 carbon atoms, preferably a methyl group; 5≦w′≦69, preferably 12≦w′≦52, more preferably 17≦w′≦35; these oligomers are 5 When is methyl, it may be sold under the name Jeffamines™ in a wide range of
[0065] *NH2-CHR 6 -CH2-O-[CH2-CH2-O] w’’ -CH2-CHR 6 -NH2(wherein, R 6 is an alkyl group having 1 to 3 carbon atoms, preferably a methyl group; 7≦w″≦91, preferably 17≦w″≦68, more preferably 23≦w″≦45).
[0066] The alkylene oxide oligomer preferably has the formula H-[O-(CH2-CH2)] as defined in the present invention. y’ The monomer is selected from the group consisting of oligomers of -OH.
[0067] The alkylene oxide oligomer is preferably an ethylene oxide oligomer, in particular having a molar mass in the range of about 750 to 4000 g / mol, more preferably in the range of about 1000 to 2000 g / mol.
[0068] The crosslinked copolymer according to the present invention can be prepared by a method comprising the following steps: i) preparing a crosslinkable poly(alkylene oxide) as defined in the present invention; and ii) copolymerizing the crosslinkable poly(alkylene oxide) of step i) with lithium styrene-sulfonyl(trifluoromethylsulfonyl)imide monomer (STFSILi).
[0069] Step i) comprises in particular the following sub-steps: ia) polycondensing an alkylene oxide oligomer as defined herein with at least one compound containing a crosslinkable alkene or alkyne functional group as defined herein; and ib) functionalizing the crosslinkable poly(alkylene oxide) obtained in sub-step ia) with a substituent M as defined above.
[0070] According to a particularly preferred embodiment of the present invention, substep ia) comprises reacting 3-chloro-2-chlorophenyl with 1,2-dichlorophenyl ether to form a crosslinkable poly(alkylene oxide) of the formula Methyl 3-Chloro-2-chloro-1-propene and oligomers of the formula H-[O-(CH2)x]y'-OH as defined in the present invention. Methyl -1-Propene is deficient relative to the oligomers.
[0071] [ka]
[0072] In the formula, y and p are as defined in the present invention.
[0073] The polycondensation is usually carried out in the presence of a strong base such as potassium hydroxide in a solvent such as THF.
[0074] Substep ib) may comprise replacing the terminal hydroxyl functions with acrylate functions in the presence of an excess of triethylamine chloride and acryloyl, in particular in a solvent such as THF; followed by radical addition of an alkoxyamine of the following formula MAMA-SG1, in particular in a solvent such as ethanol.
[0075] [ka]
[0076] Substep ib) may thus enable the formation of a crosslinkable poly(alkylene oxide) of formula (II-b) as defined in the present invention.
[0077] Step ii) of the copolymerization can be carried out by mediated radical polymerization, in particular NMP (nitroxide mediated radical polymerization).
[0078] Step ii) is preferably carried out in a polar solvent such as N,N-dimethylformamide (DMF), dimethylsulfoxide (DMSO) or water, in particular at a temperature in the range of 90-120° C., in particular for a period of 2-20 hours.
[0079] A second subject of the present invention is the use of at least one crosslinked copolymer as defined in the first subject of the present invention for the preparation of a solid polymer electrolyte, in particular in lithium batteries, and in particular in lithium metal batteries.
[0080] The use of the crosslinked copolymers according to the invention for preparing solid polymer electrolytes, especially in lithium metal batteries, is particularly advantageous in that they have a lithium ion transport number of the order of 1 and an ionic conductivity at 60° C. of 10 -5 S.cm -1 This results in an energy storage device with excellent low-temperature performance (about 60° C.) or higher.
[0081] A high transport number makes it possible to limit the formation of concentration gradients in the electrolyte during discharge (or charging), improving the power performance (or charging rate). The use of this cross-linked copolymer also makes it possible to limit the dendritic growth of lithium, thus envisaging a fast and reliable recharge. In fact, a problem with lithium metal battery technology is the formation of non-uniform electrodeposits of lithium (including dendrites) during recharge, which reduces the cycling capacity and can cause short circuits.
[0082] In addition, the crosslinked copolymer according to the present invention has good mechanical strength, high thermal stability (ensuring the safety of the energy storage device containing it), and improved voltage stability (e.g., up to 4.5 V vs Li + / Li stability).
[0083] A third subject of the invention is a solid polymer electrolyte, characterized in that it comprises at least one crosslinked copolymer as defined in the first subject and at least one plasticizer.
[0084] The solid polymer electrolyte of the present invention has optimized mechanical strength, which makes it particularly easy to use and handle, and furthermore has a cationic transport number equal to 1 and good ionic conductivity, which results in good resistance to dendritic growth.
[0085] The plasticizer may be selected from one of linear and cyclic carbonates such as propylene carbonate, ethylene carbonate or dimethyl carbonate; fluorinated carbonates such as fluoroethylene carbonate; nitriles such as succinonitrile; lactones such as gamma-butyrolactone; liquid linear or cyclic polyethers; fluorinated polyethers; and mixtures thereof.
[0086] In fact, the crosslinked copolymers of the present invention can absorb plasticizers while retaining good mechanical strength and remaining solid. Furthermore, the presence of plasticizers results in improved ionic conductivity (e.g., at least 1x10 at 60°C). -5This makes it possible to obtain a solid polymer electrolyte having a conductivity of 0.1 S / cm.
[0087] The liquid linear or cyclic polyether preferably has a molecular weight of about 10,000 g·mol -1 Less than or equal to 2000 g mol, preferably about 2000 g mol -1 Less than or equal to 600 g mol -1 It has the following molar mass:
[0088] The liquid linear or cyclic polyethers may be chosen from: * Formula H-[O-CH2-CH2] q -OH, where q is 1 to 13; *Formula R 7 -[O-CH2-CH2] q’ -OR 7’ (wherein q' is 1 to 13; R 7 and R 7’ are the same or different and are linear, branched or cyclic alkyl groups which may contain 1 to 10 carbon atoms;
[0089] *Formula R 8 -[CH2-O] q’’ -R 8’ (wherein q″ is 1 to 13; R 8 and R 8’ are the same or different and are linear, branched or cyclic alkyl groups having 1 to 10 carbon atoms and optionally containing heteroatoms; * cyclic ethers, which may contain from 2 to 20 carbon atoms, cyclic polyethers, which may contain from 3 to 40 carbon atoms; and *One of those mixtures.
[0090] The polyethers used in the electrolyte of the present invention are particularly stable with respect to lithium.
[0091] In a preferred embodiment, the plasticizer is a liquid linear or cyclic polyether and has the formula CH3O-(CH2-CH2)4-OCH3 (i.e., R 7 ,R7’ =CH3 and q'=4) or tetraethylene glycol (TEG) of formula H-(O-CH2-CH2)4-OH (i.e. q=4).
[0092] The solid polymer electrolyte according to the invention can be provided in any suitable form, for example in the form of a sheet, film or membrane. The solid polymer electrolyte according to the invention can be prepared by any technique known to the person skilled in the art, for example by coating or extrusion.
[0093] The solid polymer electrolyte according to the present invention can contain about 60 to 90% by weight of the crosslinked copolymer, and preferably about 75 to 85% by weight of the crosslinked copolymer, based on the total weight of the solid polymer electrolyte.
[0094] The solid polymer electrolyte according to the present invention can contain about 10-40 wt.% plasticizer, preferably about 15-25 wt.% plasticizer, based on the total weight of the solid polymer electrolyte, to ensure operation of LMP batteries utilizing such electrolytes with optimal ionic conductivity.
[0095] Finally, a fourth subject of the invention is a battery, in particular an LMP battery, comprising: - a negative electrode containing metallic lithium or an alloy of metallic lithium; - a positive electrode, optionally supported by a current collector; and - a solid polymer electrolyte placed between the positive and negative electrodes; The solid polymer electrolyte is characterised in that it is as defined in the third subject of the invention.
[0096] The composite positive electrode may include: - at least one positive electrode active material; - at least one polymeric binder; - optionally at least one electronically conductive agent; and Optionally, at least one plasticizer.
[0097] The composite positive electrode can contain at least about 50% by weight of the positive electrode active material, and preferably about 55 to 85% by weight of the positive electrode active material, based on the total weight of the composite positive electrode.
[0098] The positive electrode active material may be selected from lithium phosphates, particularly LiFePO4, Li3V2(PO4)3, LiCoPO4, LiMnPO4, LiNiPO4; lithium oxides, such as LiNiO2, LiCoO2, and LiMn2O4, and mixtures thereof.
[0099] Among these positive electrode active materials, LiFePO4 is particularly preferred.
[0100] According to certain embodiments, the composite positive electrode comprises about 10-40 wt % polymer binder, and preferably about 13-20 wt % polymer binder, based on the total weight of the composite positive electrode.
[0101] The polymer binder may be a triblock copolymer of the BAB type as defined in the present invention (i.e., without crosslinking) or a material selected from the following: ethylene homopolymers and copolymers; propylene homopolymers and copolymers; ethylene oxide homopolymers and copolymers (e.g., PEO, PEO copolymers), methylene oxide, propylene oxide, epichlorohydrin, allyl glycidyl ether, and mixtures thereof; vinyl chloride homopolymers and copolymers, vinylidene fluoride (PVdF), vinylidene chloride, tetrafluoroethylene, or chlorotrifluoroethylene, vinylidene fluoride. and halogenated polymers such as hexafluoropropylene copolymers (PVdF-co-HFP) or mixtures thereof; non-electronically conductive polymers of anionic type such as poly(styrenesulfonic acid), poly(acrylic acid), poly(glutamic acid), alginates, pectins, gelatins or mixtures thereof; polymers of cationic type such as polyethylenimine (PEI), polyaniline in emeraldine salt (ES) form, quaternized poly(N-vinylimidazole), poly(acrylamide-co-diallyldimethylammonium chloride) (AMAC) or mixtures thereof; polyacrylates; and mixtures thereof.
[0102] According to a particularly preferred embodiment of the present invention, the polymer binder is a triblock copolymer of the BAB type defined in the present invention (i.e. without crosslinking). The presence of the triblock copolymer of the BAB type defined in the present invention in the composite positive electrode can reduce or even eliminate the formation of concentration gradients in the thickness of the positive electrode during cycling, thus improving the power performance of the battery or providing the possibility of increasing the basis weight of the positive electrode.
[0103] The composite positive electrode can contain about 0.05 to 10% by weight of the electronic conductivity generator, and preferably about 0.2 to 5% by weight of the electronic conductivity generator, based on the total weight of the composite positive electrode.
[0104] The electronic conductivity generator suitable for the present invention is preferably selected from one of carbon black, carbon sp, acetylene black, carbon fibers and nanofibers, carbon nanotubes, graphene, graphite, metal particles and fibers, and mixtures thereof.
[0105] The electronic conductivity generator is preferably carbon black.
[0106] Preferably, the electronic conductivity generator is in the form of spherical particles (i.e., bead-shaped) to promote electrical conductivity, especially in a direction perpendicular to the composite positive electrode (i.e., through its thickness), thereby promoting the electrochemical processes within the electrode. Indeed, the spherical particles of the electronic conductivity generator tend to form a three-dimensional conductive matrix.
[0107] Examples of carbon black include those sold under the following references: Ketjenblack 600JD™, Ketjenblack 700JD™, and Timcal Ensaco 350G™.
[0108] The composite positive electrode may also comprise at least one plasticizer, said plasticizer being as defined in the present invention. The plasticizer of the positive electrode is preferably a liquid linear or cyclic polyether as defined in the present invention, or a linear, cyclic or fluorinated carbonate as defined in the present invention.
[0109] The composite positive electrode may include about 2-10% by weight of plasticizer, and preferably about 3-5% by weight of plasticizer, based on the total weight of the composite positive electrode.
[0110] It should be noted that the total weight of the composite positive electrode includes the weight of the active material, the weight of the polymer binder, if present, the weight of the optional electronic conductivity generator, and the weight of the optional plasticizer.
[0111] According to a preferred embodiment of the present invention, the basis weight of the positive electrode (i.e., the amount of positive electrode active material / cm 2 / surface) is 1~3mAh / cm 2 The range is.
[0112] A composite positive electrode can be prepared as follows: a) mixing a positive electrode active material with a polymer binder, optionally an electronic conductivity generator, optionally a plasticizer, and optionally at least one solvent for the polymer binder to obtain an electrode paste; b) applying said electrode paste to at least one substrate; c) drying the electrode paste to obtain a composite positive electrode in the form of a supported film.
[0113] Step a) can be carried out by extrusion or by grinding.
[0114] Extrusion is very advantageous since it allows to easily obtain electrodes with low porosity with little use of solvents. It also makes it possible to avoid the step of pressing the dry electrode, which may cause deformations in the structure of the electrode and impair the effective coating of the particles of the electronic conductivity generator, thereby causing structural failure of the electrode during cycling. Finally, the pressing step has the drawback of increasing the number of steps to obtain the electrode, thereby increasing its manufacturing costs.
[0115] The solvent of the polymeric binder of step a) makes it possible to solubilize said polymeric binder.
[0116] When present, the solvent preferably comprises less than about 50% by weight of the total weight of the mixture of the positive electrode active material, polymeric binder, optional electronic conductivity generator, and optional plasticizer.
[0117] The use of small amounts of solvent for the polymer binder during the preparation of the composite positive electrode makes it possible to obtain a positive electrode with low porosity (i.e., ≦about 10% by volume). This low porosity makes it possible to control and optimize the amount of active material present in the composite positive electrode, thereby achieving optimal volumetric energy density.
[0118] The solvent in step a) may be selected from the following: water, N-methylpyrrolidone; carbonates such as ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, or methyl and ethyl carbonate; acetone; alcohols such as methanol, ethanol, or propanol; and one of their mixtures.
[0119] Step b) can be carried out by calendering or coating.
[0120] The support may be a current collector and / or a support film.
[0121] An example of a current collector is one made from aluminum covered with a base layer (anti-corrosive layer) of carbon.
[0122] An example of a support film is a silicone-treated polyethylene terephthalate (PET) type plastic film.
[0123] The positive electrode support film obtained at the end of step c) may have a thickness in the range of about 2 to 100 μm, preferably about 10 to 60 μm.
[0124] Step c) can be carried out at a temperature sufficient to remove the solvent of step a).
[0125] The operating temperature of the battery is approximately 60 to 100°C.
[0126] By using the crosslinked copolymer according to the present invention at least in the solid polymer electrolyte, the operating temperature of the battery can be reduced.
[0127] The performance of the battery of the present invention at 60° C. is better in the high regime (e.g., (>C / 2)) and similar in the low regime (e.g., (C / 10)) than that of commercially available batteries with an operating temperature of 80° C., i.e., a saving of 20° C. with comparable or better performance.
[0128] The present invention is illustrated by the following embodiments, which are not limiting.
[0129] The accompanying drawings illustrate the invention. [Brief description of the drawings]
[0130] [Figure 1] FIG. 1 shows the Young's modulus (MPa) as a function of the weight percentage of PSTFSILi for materials according to the invention and not according to the invention. [Diagram 2] Figure 2 shows the variation of ionic conductivity (S / cm) as a function of the ratio 1000 / T, where T is the temperature in Kelvin for materials according to the invention and not according to the invention. [Diagram 3] FIG. 3 shows the glass transition temperature (° C.) as a function of weight percent of PSTFSILi for materials according to the invention and not according to the invention. [Figure 4] FIG. 4 shows the melting temperature (° C.) as a function of weight percent of PSTFSILi for materials according to the invention and not according to the invention. [Diagram 5] 5 shows the voltage (volts) of a composite positive electrode according to the invention as a function of the discharge capacity (mAh) in various regimes (D / 9.4 to D / 0.9) at 60° C. The load is always C / 9.4. [Figure 6] Figure 6 shows the curves of discharge capacity (mAh) and coulombic efficiency (%) as a function of cycle number for different discharge regimes (D / 9.4 to D / 0.9) at 60 °C. The load is always C / 9.4. [Figure 7] FIG. 7 illustrates the power performance of two LMP batteries, one according to the invention and one not according to the invention. EXAMPLES
[0131] The materials used in the examples are as follows: - Carbon black, Ketjenblack EC600JD, AkzoNobel; - LiFePO4, Pulea; - PVDF-co-HFP, Solvay; - Homo-PEO, Sumitomo Seika; - LiTFSI, Solvay; - Armor, an aluminum current collector covered with a layer of carbon; - Lithium metal sheets, Blue Solutions; - PEO Oligomer, PEG2000, Sigma-Aldrich; - 3-Chloro-2-chloro Methyl -1-propene; -TEGDME, Sigma-Aldrich; - Potassium hydroxide (KOH); - Tetrahydrofuran (THF); - diethyl ether; - acetonitrile; - water; - acryloyl chloride; - Triethylamine; - dimethylformamide (DMF); - 2-Hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone: photoinitiator Irgacure 2959; - nitroxides SG1 and alkoxyamines MAMA-SG1 of the following formula:
[0132] [ka]
[0133] Unless otherwise stated, all materials were used as received from the manufacturer.
[0134] Example 1: Preparation of a crosslinked copolymer according to the first subject of the invention Preparation of crosslinkable poly(ethylene oxide) precursors of the A block. Preparation of crosslinkable poly(ethylene oxide): Substep ia) as defined herein
[0135] [ka]
[0136] Dissolve 127.6 g of 1.5 kDa PEO oligomer and 9.5 g of KOH in 200 ml of tetrahydrofuran (THF) at 40 °C. When the solution becomes homogeneous, add 10 g of 3-chloro-2-chloropropanediol dissolved in 20 ml of THF. Methyl 3-Chloro-2-chloro-1-propene was added to the previously prepared solution of PEO oligomer. The polycondensation reaction was carried out at 40° C. for 3 days. Methyl Due to the deficiency of -1-propene, the resulting crosslinkable poly(ethylene oxide) is terminated with hydroxyl functional groups.
[0137] The reaction medium is then cooled and centrifuged, and the supernatant is then precipitated in diethyl ether. Purification is completed by ultrafiltration to remove low molecular weight polymers and salts that were not removed in the centrifugation step. Water is removed by rotary evaporation to dryness, and the product is dried under vacuum.
[0138] Preparation of crosslinkable poly(ethylene oxide): Substep ib) as defined herein
[0139] [ka]
[0140] 26.5 g of previously prepared crosslinkable poly(ethylene oxide) was reacted with 7.4 g of acryloyl chloride in the presence of 8 g of triethylamine in 200 ml of tetrahydrofuran at ambient temperature for 15 hours, whereby the terminal hydroxyl functions were functionalized with acrylate functions. The resulting residue was precipitated in diethyl ether, filtered, and then dried under vacuum.
[0141] Then, under an inert atmosphere, 2 g of alkoxyamine of formula MAMA-SG1 was added to the previously obtained diacrylate in 50 ml of ethanol at 80° C. After 4 hours of reaction, the product obtained was precipitated in diethyl ether, filtered and then dried under vacuum.
[0142] Copolymerization of crosslinkable poly(ethylene oxide) and lithium styrene-sulfonyl(trifluoromethylsulfonyl)imide (STFSILi), the precursor of the A block, to form the BAB triblock copolymer: step ii) defined in the present invention
[0143] [ka]
[0144] 5 g of crosslinkable poly(ethylene oxide) with pre-prepared initiator in 30 ml of DMF was reacted with 1 g of lithium styrene-sulfonyl(trifluoromethylsulfonyl)imide (STFSILi) and 7 mg of nitroxide SG1 under an inert atmosphere at 120° C. At the end of the 16-h reaction, approximately 80% of the monomer STFSILi had reacted.
[0145] Lithium styrene-sulfonyl(trifluoromethylsulfonyl)imide (STFSILi) can be prepared as described in International Patent Application WO 2013 / 034848 A1.
[0146] The resulting copolymer was precipitated in diethyl ether and then dialyzed in water (3 kg.mol -1 The product was purified by a 50% purity standard (cut-off value) and then dried by lyophilization.
[0147] A BAB triblock copolymer CP-1 according to the invention was obtained containing 13.1% by weight of PSTFSILi relative to the total weight of the copolymer, the EO / Li ratio of this copolymer being 48.4.
[0148] Crosslinking and molding of copolymers 100 mg of the copolymer previously prepared was placed in a solution of 5 ml of acetonitrile / water mixture (5 / 1 by volume). 0.9 mg of UV photoinitiator (2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone) was placed in the solution. The resulting solution was then poured into a polypropylene Petri dish (6 cm diameter) placed on a flat surface. Most of the solvent was evaporated in an oven at 40°C for 24 hours and then at 60°C for 12 hours. The resulting polymer film was then photoinduced by irradiation with 15 mW / cm under a mercury UV lamp sold by Fusion UV System Inc under the trade name P300 MT Power supply. 2 The resulting film was dried in a glove box to give the crosslinked copolymer CP 1 according to the invention, which contains 13.1% by weight of PSTFSILi relative to the total weight of the copolymer and has an EO / Li ratio of 48.4. r -1 was formed.
[0149] Other copolymers available By changing the amount of STFSILi monomer, another copolymer, cross-linked CP r -2 and CP r -3; and non-crosslinked CP-2 and CP-3.
[0150] The compositions of the resulting copolymers are shown in Table 1 below:
[0151] [Table 1]
[0152] Example 2: Preparation of a solid polymer electrolyte according to the third subject of the invention Crosslinked polymer CP in film form r -1, CP r -2 and CP rAfter quenching in TEGDME as a plasticizer for 1 h in a drying room (dew point: -45°C), the resulting films were collected and the excess plasticizer was removed with Kimtech tissue paper. The weight of the films was measured before and after absorption of the plasticizer so that the percentage of plasticizer in the films could be estimated. The average thickness of the films ranges from 30 to 60 μm.
[0153] Table 2 below shows the composition of the resulting solid polymer electrolyte:
[0154] [Table 2]
[0155] Example 3: Physicochemical properties Young's Modulus The Young's modulus (elastic modulus) was calculated based on tensile stress-elongation curves obtained at 50°C in a dry air stream using a dynamic mechanical analyzer sold by TA Instruments under the name Dynamic Mechanical Analyzer DMA Q800.
[0156] FIG. 1 of the accompanying drawings shows the cross-linked copolymer CP r -1, CP r -2 and CP r -3), as a function of the weight percentage (%) of PSTFSILi in the non-crosslinked copolymers (black circle curves: copolymers CP-1, CP-2, and CP-3), and as a function of the weight percentage (%) of PSTFSILi for mixtures of crosslinked copolymers and TEGDME plasticizer (black square curves: electrolytes E-1b, E-2b, and E-3b).
[0157] First, FIG. 1 shows that the crosslinking of the A blocks of the BAB triblock copolymer has a significant effect on the Young's modulus, since a 3-5-fold increase is obtained with exactly the same weight percentage of PSTFSILi (for example, from 0.46 MPa to 1.7 MPa for a copolymer containing 28.4 wt.% PSTFSILi). Moreover, this crosslinking makes it possible to obtain sufficient mechanical strength that allows the crosslinked copolymer according to the invention to be combined with plasticizers. In particular, the plasticization improves the ionic conductivity and ensures a perfectly acceptable Young's modulus.
[0158] Thus, for the solid polymer electrolytes E-1b, E-2b, and E-3b, a good ionic conductivity / mechanical strength compromise is obtained at 50° C. Finally, it is possible to tune the mechanical strength of the copolymer as a function of the weight percentage of PSTFSILi in the crosslinked copolymer.
[0159] Ionic Conductivity The ionic conductivity was calculated according to the following formula:
[0160]
number
[0161] In the formula, S and l are the surface area and thickness of the solid polymer electrolyte or copolymer, respectively. el is the resistance of the solid polymer electrolyte or copolymer measured at high frequency by impedance spectroscopy (VMP300, Bio-Logic) in a Li / solid polymer electrolyte or copolymer / Li symmetric cell. The temperature is set between 10 and 80 °C by the climatic enclosure.
[0162] The attached Figure 2 shows the non-crosslinked copolymers CP-2 (black circle curve) and CP-3 (black triangle curve), and the crosslinked copolymer CP r -2 (white circle curve) and CP r4 shows the variation of ionic conductivity (S / cm) as a function of the 1000 / T ratio for E-3 (curve with open triangles), and for the solid polymer electrolytes E-2c (curve with closed squares) and E-3c (curve with open squares), where T is the temperature in Kelvin.
[0163] Figure 2 shows that the conductivity of the copolymer without plasticizer is 4~8*10 at 60℃. -6 S / cm. This is especially true in the high regime when the cathode basis weight is high (e.g., >0.8 mAh / cm 2 ), which is too low for use in batteries. By plasticizing with a small amount of plasticizer, the crosslinked copolymer can be made 1,3*10 without compromising its mechanical stability. -5 Conductivities of 100 S / cm can be achieved.
[0164] 3 and 4 show the cross-linked copolymer (white circle curve; copolymer CP r -1, CP r -2 and CP r The glass transition temperatures (°C) (FIG. 3) and melting temperatures (°C) (FIG. 4) of the crosslinked copolymers (curves with filled circles; copolymers CP-1, CP-2, and CP-3), non-crosslinked copolymers (curves with filled squares; electrolytes E-1a, E-2a, and E-3a), and solid polymer electrolytes (curves with filled squares; electrolytes E-1a, E-2a, and E-3a), respectively, are shown as a function of the weight percentage of PSTFSILi.
[0165] The glass transition and melting temperatures were obtained by measuring the thermodynamic properties by DSC using an instrument sold by Mettler-Toledo under the trade name DSC3. The measurements were carried out with the following parameters: between -110°C and 130°C at 10°C / min.
[0166] Figures 3 and 4 show that the glass transition temperature and melting temperature of the solid polymer electrolyte are significantly lowered compared to those of the crosslinked and non-crosslinked copolymers, respectively, which is suitable for obtaining an electrolyte with good ionic conductivity at low temperatures (low polymer crystallinity) and can be implemented in batteries at lower temperatures.
[0167] Example 4: Electrochemical characterization 4.1 Preparation of composite positive electrode A composite cathode in the form of a film was prepared as follows: a mixture of 46.3 g of LiFePO4, 1.2 g of carbon black, 17.5 g of copolymer CP-3 and 6.5 g of deionized water was introduced into a Brabender Plastograph. Mixing was carried out at 60° C. and 80 rpm.
[0168] The paste thus obtained was then calendered onto a current collector made of carbon-coated aluminum at 60° C. The film obtained was dried at 100° C. for 10 minutes before use.
[0169] The resulting composite cathode contains 71.2 wt.% LFP active material, 26.9 wt.% copolymer CP-3, and 1.9 wt.% carbon black. It has a thickness of about 45 μm. The resulting basis weight is 1.37 mAh / cm. 2 It is.
[0170] The LMP accumulator was fabricated in a controlled atmosphere (dew point -50°C) with the following assembly: - a prefabricated film of solid polymer electrolyte E-3d with a thickness of 58.8 μm; - a sheet of metallic lithium having a thickness of about 50 μm; and - A prefabricated positive electrode.
[0171] For this purpose, a sheet of lithium and a solid polymer electrolyte film are calendered at 70 °C and 5 bar to ensure good Li / electrolyte contact, then finally a composite cathode is calendered onto the lithium / electrolyte assembly to form the accumulator. The electrolyte film is placed between the metallic lithium film and the composite cathode film. A conductor is connected to the lithium and another conductor is connected to the current collector of the composite cathode.
[0172] The resulting sandwich-type structured accumulator is sealed in a pouch (known as a "coffee bag") under vacuum and tested in an uncontrolled atmosphere.
[0173] Pressure 1 bar, surface area 2.8 cm 2 An accumulator of is obtained.
[0174] During operation of the accumulator, the TEGDME contained in the solid polymer electrolyte migrates at least partially to the composite positive electrode (in particular until an equilibrium is reached between the amounts of TEGDME in the composite positive electrode on the one hand and in the solid polymer electrolyte on the other hand).
[0175] Figure 5 shows the voltage in volts of the composite positive electrode as a function of the discharge capacity (mAh) in various regimes (D / 9.4 to D / 0.9) at 60 °C. The load is always C / 9.4. D represents the nominal capacity in mAh and D / n is the discharge current corresponding to obtain a capacity D in n hours. The polarization is proportional to the applied current density, which is typical for single-ion polymers where the transport of ions is ensured only by migration. The obtained capacity value therefore depends strongly on the low voltage cut-off terminal.
[0176] Figure 6 shows the curves of discharge capacity (mAh) and coulombic efficiency (%) as a function of cycle number for different discharge regimes (D / 9.4 to D / 0.9) at 60 °C. The charge is always C / 9.4. Very good cycle strength is obtained over 60 cycles, with a faradic yield of 98.4%.
[0177] Figure 7 shows a comparison of the power performance of the two LMP batteries: A first LMP cell (open diamond curve) operating at 60°C containing the solid polymer electrolyte E-3d and a composite cathode as defined above; and
[0178] A solid polymer electrolyte containing 48 wt% homo-PEO, 12 wt% LiTFSi lithium salt, and 40 wt% PVdF-co-HFP, and a cathode containing 68 wt% LFP active material, 24 wt% homo-PEO, 6 wt% LiTFSi lithium salt, and 2 wt% carbon black, has a thickness of approximately 60 μm and a nominal capacity of 1.5 mAh / cm. 2 and the second LMP battery currently used in industry (black circle curve), which operates at 80°C.
[0179] FIG. 7 shows the discharge capacity normalized to the nominal capacity (D / D0) as a function of the discharge regime (D / n) of the cell.
[0180] For the initially unplasticized composite cathode, the thickness of the solid polymer electrolyte (58.8 μm), the very high electrode basis weight (1.37 mAh / cm 2 ), the obtained results are remarkable. They show that the solid polymer electrolyte of the present invention has a better performance than the commercial electrolyte in the high cycle regime and is comparable in the low cycle regime.
Claims
1. A crosslinked copolymer comprising at least a repeating unit of lithium polystyrene-sulfonyl(trifluoromethylsulfonyl)imide (PSTFSILi) and a repeating unit of a poly(alkylene oxide) selected from the group consisting of poly(ethylene oxide) units, poly(propylene oxide) units, poly(ethylene and propylene) oxide units, and mixtures thereof, Crosslinked copolymers obtained by crosslinking BAB type triblock copolymers: - the A block is a crosslinkable poly(alkylene oxide) containing functional polymer obtained by reacting: * at least one monomer selected from ethylene glycol, propylene glycol and mixtures thereof, or at least one poly(alkylene oxide) oligomer selected from one of poly(ethylene oxide), poly(propylene oxide), poly(ethylene and propylene) oxides and mixtures thereof, having a molar mass in the range of less than or equal to 5000 g / mol; and, * at least one compound containing at least one crosslinkable alkene or alkyne functional group selected from the compounds of formula (IV) below: [Formula 1] In the formula, R' 1 is an alkylene group containing at least one alkene or alkyne functional group, said alkylene group containing from 4 to 10 carbon atoms; X and X′ are the same or different and are independently selected from halogen, carboxylic acid, acyl chloride, ester and aldehyde functional groups; Each B block is an anionic polystyrene substituted with an anion of lithium sulfonyl(trifluoromethylsulfonyl)imide (TFSILi) and corresponds to the following formula (I): [chemical 2] (wherein n represents the number of lithium styrene-sulfonyl(trifluoromethylsulfonyl)imides in each B block).
2. 2. The cross-linked copolymer according to claim 1, comprising 10 to 50% by weight of PSTFSILi, based on the total weight of the cross-linked copolymer.
3. 3. The crosslinked copolymer according to claim 1, wherein the A block has a number average molecular weight of 10 kDa or more and 50 kDa or less.
4. The crosslinked copolymer of claim 1, wherein the functional polymer has a structure of formula (II): [C3] In the formula, R 1 is a substituent containing at least one crosslinkable alkene or alkyne functional group; CoA is a poly(alkylene oxide) chain selected from one of a poly(ethylene oxide) chain, a poly(propylene oxide) chain, a poly(ethylene and propylene) oxide chain, and mixtures thereof; and p is 10-50.
5. In the formula (IV), X and X' are halogens, 5. Crosslinked copolymer according to claim 4, characterized in that the functional polymer of formula (II) corresponds to the following formula (II-a): [C4] In the formula, y is 11 to 91, and p is 10 to 50.
6. The crosslinked copolymer according to any one of claims 1 to 5, characterized in that the ratio of the number of moles of alkylene oxide to the number of moles of STFSILi (AO / Li) is in the range of 7 to 65.
7. 7. The crosslinked copolymer according to claim 1, wherein the compound containing a crosslinkable alkene or alkyne functional group is 3-chloro-2-chloromethyl-1-propene.
8. 8. Crosslinked copolymer according to any one of the preceding claims, characterized in that the poly(alkylene oxide) oligomer has a molar mass in the range of 700 to 4000 g / mol.
9. Use of at least one crosslinked copolymer as defined in any one of claims 1 to 8 for the preparation of a solid polymer electrolyte.
10. A solid polymer electrolyte comprising at least one crosslinked copolymer as defined in any one of claims 1 to 8 and at least one plasticizer.
11. 11. The solid polymer electrolyte of claim 10, wherein the plasticizer is selected from one of: linear or cyclic carbonates; fluorinated carbonates; nitriles; lactones; liquid linear or cyclic polyethers; fluorinated polyethers; and mixtures thereof.
12. The plasticizer has a molar mass of 10,000 g / mol. -1 12. A solid polymer electrolyte according to claim 10 or 11, characterized in that it is a liquid linear or cyclic polyether selected from: *Formula H-[O-CH 2 -CH 2 ] q -OH, where q is 1 to 13; *Formula R 7 -[O-CH 2 -CH 2 ] q’ -O-R 7’ (wherein q′ is 1 to 13; R 7 and R 7’ are the same or different and are linear, branched or cyclic alkyl groups; *Formula R 8 - [CH 2 -O] q’’ -R 8’ (wherein q″ is 1 to 13; R 8 and R 8’ are the same or different and are linear, branched or cyclic alkyl groups; * Cyclic ethers; cyclic polyethers; and *One of those mixtures.
13. 13. The solid polymer electrolyte according to claim 10, further comprising 10 to 40% by weight of a plasticizer based on the total weight of the solid polymer electrolyte.
14. a negative electrode comprising metallic lithium or an alloy of metallic lithium; a positive electrode, optionally supported by a current collector; and - a solid polymer electrolyte disposed between the positive and negative electrodes; Including, A battery, characterized in that the solid polymer electrolyte is as defined in any one of claims 10 to 13.
15. The positive electrode is - at least one positive electrode active material; at least one polymeric binder; optionally at least one electronically conductive agent; and optionally at least one plasticizer; A composite positive electrode comprising:
15. The battery of claim 14, wherein the polymer binder is a BAB triblock copolymer as defined in claim 1.
Citation Information
Patent Citations
Copolymer, its preparation and its use for production of material having ionic conductivity
JP1994256673A
Triblock copolymers, particularly solid polymer electrolytes based on polystyrene-poly(oxyethylene)polystyrene.
JP2009531820A
A block copolymer containing polyanions based on TFSI-Li anion monomers is used as the battery electrolyte.
JP2014529863A
Block copolymer including a polyanion based on a tfsili anion monomer as a battery electrolyte
WO2013034848A1