Metal-air cell with extremely small air access

JP7579256B2Active Publication Date: 2024-11-07ENERGIZER BRANDS LLC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021537727
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-27
Filing Date
2019-12-24
Publication Date
2024-11-07
Estimated Expiration
2039-12-24

Smart Images

  • Figure 0007579256000008
    Figure 0007579256000008
  • Figure 0007579256000009
    Figure 0007579256000009
  • Figure 0007579256000010
    Figure 0007579256000010
Patent Text Reader

Abstract

The present technology provides a battery including an air cathode, an anode, an aqueous electrolyte including an amphoteric surfactant, and a housing including one or more air ports defining a total area of ​​void space (the "vent area"), wherein: (1) The battery is a size 13 metal-air battery, and the total vent area defined by all of the air ports is approximately 0.050 mm 2 ~about 0.115mm 2 is; or (2) The battery is a size 312 metal-air battery, and the total vent area defined by all of the air ports is approximately 0.03 mm 2 ~approx. 0.08mm 2 is.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Application No. 62 / 785,619, filed December 27, 2018, the entire contents of which are incorporated herein by reference for all purposes. The present technology relates generally to the field of metal-air batteries and their uses. Summary of the Invention

[0002] In one embodiment, a battery is provided that includes an air cathode, an anode, an aqueous electrolyte, and a housing, the housing including one or more air ports defining a vent area, the aqueous electrolyte including an amphoteric fluorosurfactant and, optionally, lithium hydroxide. If the battery is a size 13 metal-air battery, the total vent area defined by all of the air ports is less than 0.05 mm 2 ~0.115mm 2 If the battery is a size 312 metal-air battery, the total vent area defined by all of the air ports is 0.03 mm 2 ~0.08mm 2 It is. [Brief description of the drawings]

[0003] [Figure 1] FIG. 1 is a cross-sectional schematic diagram illustrating an exemplary electrochemical cell. [Diagram 2] 1 is a box plot comparing size 13 cells of the present technology with comparative "standard" cells discharged at 10 / 2 mA at 80% RH (relative humidity) according to ANSI / IEC testing, according to an embodiment. [Diagram 3] 13 is a box plot comparing size 312 cells of the present technology to comparative "standard" cells discharged at 10 / 2 mA at 80% RH (relative humidity) according to ANSI / IEC testing, according to an embodiment. [Figure 4] 1 is a box plot comparing size 312 cells of the present technology to comparative "standard" cells discharged at 10 / 2 mA at 20% RH (relative humidity) according to ANSI / IEC testing, according to an embodiment. [Diagram 5] FIG. 13 is a plot of potential versus a pure zinc reference for a current draw of 1 mA / cm2 and 5 mA / cm2 applied to the positive electrode of a metal-air cell using three different electrolytes, according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0004] Various embodiments are described below. It should be noted that the specific embodiments are not intended to be exhaustive or to be limiting to the broader aspects described herein. An aspect described in connection with a particular embodiment is not necessarily limited to that embodiment and can be practiced with any other embodiment(s). As used herein, "about" is understood by those of ordinary skill in the art and varies to some extent depending on the context in which it is used. If there is a use of a term that is not clear to those of ordinary skill in the art, given the context in which it is used, "about" will be understood to mean up to plus or minus 10% of that particular term, for example, "about 10% by weight" means "9% to 11% by weight". When "about" precedes a term, the term is interpreted as "approximately" representing that term as well as the term not modified by "about", for example, "about 10% by weight" represents not only "9% to 11% by weight". The use of the terms "a" and "an" and "the" and similar referents in the context of describing elements (particularly in the context of the claims that follow) are intended to encompass both the singular and the plural, unless otherwise indicated herein or clearly contradicted by context. The recitation of ranges of values ​​herein is merely intended to serve as a shorthand method of referring individually to each individual value falling within the range, unless otherwise indicated herein, and each individual value is incorporated herein as if it were individually recited herein. All methods described herein can be performed in any suitable order, unless otherwise indicated herein or otherwise clearly contradicted by context. The use of any and all examples, or exemplary language (e.g., "e.g., "etc.") provided herein is intended merely to better clarify the embodiments and does not pose a limitation on the scope of the claims, unless otherwise indicated. No language in this specification should be construed as indicating any non-claimed element as essential.

[0005] In general, "substituted" refers to an alkyl, alkenyl, alkynyl, aryl, or ether group, as defined below (e.g., an alkyl group), in which one or more bonds to a hydrogen atom contained therein are replaced with a bond to a non-hydrogen or non-carbon atom. Substituted groups also include groups in which one or more bonds to a carbon(s) or hydrogen(s) atom are replaced with one or more bonds, including double or triple bonds, to a heteroatom. Thus, a substituent is substituted with one or more substituents, unless otherwise specified. In some embodiments, a substituent is substituted with 1, 2, 3, 4, 5, or 6 substituents. Examples of substituents include halogens (i.e., F, Cl, Br, and I); hydroxyl; alkoxy, alkenoxy, alkynoxy, aryloxy, aralkyloxy, heterocyclyloxy, and heterocyclylalkoxy groups; carbonyl (oxo); carboxyl; ester; urethane; oxime; hydroxylamine, alkoxyamine; aralkoxyamine; thiol; sulfide; sulfoxide; sulfone; sulfonyl; sulfonamide; amine; N-oxide; hydrazine; hydrazide; hydrazone; azide; amide; urea; amidine; guanidine; enamine; imide; isocyanate; isothiocyanate; cyanate; thiocyanate; imine; nitro group; nitrile (i.e., CN), and the like.

[0006] As used herein, "alkyl" groups include straight-chain and branched alkyl groups having 1 to about 20 carbon atoms, typically 1 to 12 carbons, or in some embodiments, 1 to 8 carbon atoms. The alkyl groups may be substituted or unsubstituted. Examples of straight-chain alkyl groups include methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, and n-octyl groups. Examples of branched alkyl groups include, but are not limited to, isopropyl, sec-butyl, t-butyl, neopentyl, and isopentyl groups. Representative substituted alkyl groups may be substituted one or more times, for example, with amino groups, thio groups, hydroxy groups, cyano groups, alkoxy groups, and / or halo groups (e.g., F, Cl, Br, and I groups, etc.). As used herein, the term haloalkyl is an alkyl group having one or more halo groups. In some embodiments, haloalkyl refers to a perhaloalkyl group. Cycloalkyl groups are cyclic alkyl groups such as, but not limited to, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, and cyclooctyl groups. In some embodiments, cycloalkyl groups have 3 to 8 ring members, while in other embodiments, the number of ring carbon atoms ranges from 3 to 5, 6, or 7. Cycloalkyl groups can be substituted or unsubstituted. Cycloalkyl groups further include polycyclic cycloalkyl groups such as, but not limited to, norbornyl, adamantyl, bornyl, camphenyl, isocamphenyl, and carenyl groups, and fused rings such as, but not limited to, decalinyl. Cycloalkyl groups also include rings substituted with straight or branched chain alkyl groups as defined above. Representative substituted cycloalkyl groups may be mono- or di-substituted, such as, but not limited to, 2,2-, 2,3-, 2,4-, 2,5-, or 2,6-disubstituted cyclohexyl groups or mono-, di-, or tri-substituted norbornyl or cycloheptyl groups, which may be substituted, for example, with alkyl, alkoxy, amino, thio, hydroxy, cyano, and / or halo groups. Alkenyl groups are straight-chain, branched, or cyclic alkyl groups having 2 to about 20 carbon atoms and further comprising at least one double bond. In some embodiments, alkenyl groups have 1 to 12 carbons, or typically 1 to 8 carbon atoms. Alkenyl groups can be substituted or unsubstituted. Examples of alkenyl groups include vinyl, propenyl, 2-butenyl, 3-butenyl, isobutenyl, cyclohexenyl, cyclopentenyl, cyclohexadienyl, butadienyl, pentadienyl, and hexadienyl groups, among others. Alkenyl groups can also be substituted with alkyl groups. Divalent alkenyl groups, i.e., alkenyl groups having two points of attachment, include, but are not limited to, CH-CH=CH2, C=CH2, or C=CHCH3.

[0007] The term "alkoxy" refers to a hydroxy group (OH) where H is substituted with an alkyl group containing 1 to 12 carbon atoms, as defined herein. In some embodiments, the alkoxy group contains 1 to 7 or 1 to 4 carbon atoms. The alkoxy group can be, for example, a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a n-butoxy group, a sec-butoxy group, a tert-butoxy group, a pentoxy group, a isopentoxy group, a 3-methylbutoxy group, a 2,2-dimethylpropoxy group, a n-hexoxy group, a 2-methylpentoxy group, a 2,2-dimethylbutoxy group, a 2,3-dimethylbutoxy group, a n-heptoxy group, a 2-methylhexoxy group, a 2,2-dimethylpentoxy group, a 2,3-dimethylpentoxy group, a cyclopropoxy group, a cyclobutoxy group, a cyclopentyloxy group, a cyclohexyloxy group, a cycloheptyloxy group, a 1-methylcyclopropyloxy group, and the like. In some embodiments, the alkoxy group comprises an O-C1-C6-alkyl group, while in other embodiments, the alkoxy group comprises an O-C1-C4-alkyl group.

[0008] The term "amine" (or "amino"), as used herein, refers to -NR 100 R 101 R 100 and R 101are independently hydrogen or a substituted or unsubstituted alkyl, alkenyl, alkynyl, cycloalkyl, aryl, aralkyl, heterocyclylalkyl, or heterocyclyl group as defined herein. In some embodiments, the amine is an alkylamino, dialkylamino, arylamino, or alkylarylamino. In other embodiments, the amine is NH2, methylamino, dimethylamino, ethylamino, diethylamino, propylamino, isopropylamino, phenylamino, or benzylamino.

[0009] As used herein, the term "halogen" or "halo" refers to bromine, chlorine, fluorine, or iodine. In some embodiments, the halogen is fluorine. In other embodiments, the halogen is chlorine or bromine. As used herein, the term "hydroxyl" may refer to either --OH or its ionized form, --O--. The term "nitrile" or "cyano" as used herein refers to the group --CN. As used herein, the term "thio" refers to an -S- group or an ether where the oxygen has been replaced with a sulfur. As used herein, an "amphoteric fluorosurfactant" is at least one cationic group and / or group that can be protonated to form a cationic group, such as a primary, secondary, tertiary, and / or quaternary amine group; at least one anionic group and / or a group that can be deprotonated to form an anionic group, such as a carboxy group, a sulfonate group, a phosphate group, a phosphonate group, and any one or more salts thereof; This refers to fluorosurfactants including: As used herein, the term "betaine-functional" refers to a neutral compound having a positively charged cationic functional group and a negatively charged functional group. In some embodiments, the cationic functional group may be a quaternary ammonium or phosphonium cation that does not have a hydrogen atom. In some embodiments, the negatively charged functional group may be a carboxylate group. As used herein, the term "short chain perfluoro substituent" refers to a C1-C7 perfluoro substituent. As used herein, the term "zinc anode" refers to anodes that include zinc as the anode active material. As used herein, the term "ppm" means parts per million by mass, unless expressly expressed otherwise.

[0010] It has now been observed that oxygen utilization in metal-air electrochemical cells can be unexpectedly improved by combining an electrolyte with a fluorinated amphoteric surfactant and lithium hydroxide in a cell housing with limited air access. The electrolyte formulation was found to increase the closed cell voltage and allow for a reduction in the concentration of oxygen required by the cell for a given current draw while maintaining a desired closed circuit voltage. This greater oxygen utilization efficiency and higher cell voltage allows for a smaller vent area to the outside of the cell, reducing exposure to the deleterious effects of moisture and CO2. This improves performance in low and high humidity conditions as well as environments with high CO2 concentrations.

[0011] Described herein is the combination of a high voltage negative electrode formulation containing an amphoteric fluorosurfactant and a cell designed to reduce the cell limit current to the lowest possible level while still meeting drain rate usage requirements. The technology provides a battery including an air positive electrode, a negative electrode, an aqueous electrolyte containing an amphoteric surfactant, and a housing including one or more air ports that define the total area of ​​the void (the "vent area"), where: (1) The battery is a size 13 metal-air battery and the total vent area defined by all of the air ports is approximately 0.050 mm 2 ~about 0.115mm 2 is; or (2) The battery is a size 312 metal-air battery, and the total vent area defined by all of the air ports is approximately 0.03 mm 2 ~ approx. 0.08 mm 2 It is. In any of the embodiments herein, the electrolyte may include lithium hydroxide (LiOH), which is discussed in more detail herein.

[0012] In accordance with the surprising observations described herein, it has been found that when amphoteric fluorosurfactants are used in the electrolyte of the batteries of the present technology, the minimum required total vent area defined by the air ports is surprisingly low. By way of example, in the improved batteries of the present technology, the total vent area of ​​a size 312 cell is 0.0498 mm 2 (Standard / conventional dimensions: 0.1329 mm 2 As another example, in the improved battery of the present technology, the total vent area of ​​a size 13 cell is 0.0845 mm 2 (Standard / conventional dimensions: 0.1537 mm 2 Without being bound by theory, it is proposed that the reduction in vent area is possible due to the high voltage and a more efficient electrolyte formulation (i.e., including an amphoteric fluorosurfactant and optionally LiOH), where the amphoteric fluorosurfactant can help suppress voltage while maintaining reliable gassing, and the combination of components in the negative electrode can result in a greatly enhanced improvement in cell voltage and cell performance.

[0013] In any embodiment herein, the amphoteric fluorosurfactant may contain a short-chain perfluoro substituent, which cannot decompose to perfluorooctanoic acid. In any embodiment herein, the amphoteric fluorosurfactant may contain a betaine functionality. For example, the amphoteric fluorosurfactant may be represented as a compound of formula (I): [ka] In the formula, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 are each independently a hydrogen atom, an alkyl group, an alkenyl group, or a cycloalkyl group; 1 are -C(O)-, -SO2-, and -C(O)NR a -,-SO2NR a-, -CO2-, or -SO2O-; R a is H or an alkyl group; m and p are each independently 0, 1, 2, 3, 4, 5, or 6; and n and r are each independently 1, 2, 3, 4, or 5. In some embodiments, R 1 ~R 6 is H and R 7 and R 8 is a C1-C4 alkyl group, n and p are 2, m is 4, 5, or 6, and X 1 is SO2; r is 1. In any embodiment herein, the amphoteric fluorosurfactant may be present in the electrolyte at about 200 ppm to about 20,000 ppm. Thus, in any embodiment herein, the electrolyte may contain the amphoteric fluorosurfactant at about 500 ppm, about 600 ppm, about 700 ppm, about 800 ppm, about 900 ppm, about 1,000 ppm, about 2,000 ppm, about 3,000 ppm, about 4,000 ppm, about 5,000 ppm, about 6,000 ppm, about 7,000 ppm, about 8,000 ppm, about 9,000 ppm, or about 10,000 ppm. The amphoteric fluorosurfactant may be present in the electrolyte in an amount of about 2000 ppm to about 15000 ppm, about 3000 ppm to about 12000 ppm, about 1000 ppm, about 11000 ppm, about 12000 ppm, about 13000 ppm, about 14000 ppm, about 15000 ppm, about 16000 ppm, about 17000 ppm, about 18000 ppm, about 19000 ppm, about 20000 ppm, or a range between any two of these values ​​(including the endpoints). For example, in any embodiment herein, the amphoteric fluorosurfactant may be present in the electrolyte in an amount of about 2000 ppm to about 15000 ppm or about 3000 ppm to about 12000 ppm. As another example, in any embodiment herein, the amphoteric fluorosurfactant concentration in the electrolyte may be about 4000 ppm.

[0014] The battery may be constructed according to or consistent with metal-air battery cell designs such as zinc / silver oxide, zinc / manganese dioxide, etc. For example, the battery may be designed to specifications suitable for metal-air button size batteries. Additionally, the shape of the battery may be such that the negative electrode is held in a somewhat flat or dished position.

[0015] The disclosure will be described hereinafter with reference to FIG. 1 for understanding, but this is not intended to mandate inclusion of the features described in the metal-air battery of the present technology. However, in any embodiment of the present disclosure, the battery of the present disclosure may be as illustrated in FIG. 1. FIG. 1 shows that in a battery cell 10, the negative electrode includes a negative electrode can assembly 22, a negative electrode can 24 including an electrochemically reactive negative electrode 26 housed therein, and an insulating gasket 60. The negative electrode can 24 has a bottom wall 28 and a circumferentially downwardly depending side wall 30. The side wall 30 terminates at a circumferential can foot 36. The bottom wall and the side wall 30 generally define a negative electrode cavity 38 within the negative electrode can 24, which contains the negative electrode 26. Anode can 24 may comprise an alloy of copper, which includes copper and a metal such as aluminum, silicon, cobalt, tin, chromium, zinc, and mixtures of any two or more thereof. For example, in any of the embodiments disclosed herein, the entire anode can 24 may comprise an alloy of copper. The cathode 42 includes the area below the separator 74 to the cathode can 44. This cathode 42 area includes a porous diffusion layer 57, a cellulose air diffusion layer, and a cathode active layer 72. The cathode can 44 has a bottom 46 and a circumferentially upstanding sidewall 47. The bottom 46 has a generally planar inner surface 48, a generally planar outer surface 50, and an outer perimeter 52 defined on the planar outer surface 50. A plurality of air ports 54 extend through the bottom 46 of the cathode can 44 and provide a path for oxygen to traverse through the bottom 46 to the adjacent cathode can assembly 40. An air reservoir 55 spaces the cathode can assembly 40 from the bottom 46 and the corresponding air port 54. The porous diffusion layer 57 and the cellulose air diffusion layer 32 fill the air reservoir 55. The cathode can sidewall 47 has an inner surface 56 and an outer surface 58.

[0016] As noted above, the air ports 54 define a vent area through which oxygen can enter the cell and form a voltaic cell with the zinc to generate an electric current. In accordance with the surprising observations described herein, it has been discovered that when an amphoteric fluorosurfactant is used in the electrolyte of the batteries of the present technology, the minimum required total vent area defined by the air ports 54 is surprisingly low. As previously noted, when the metal-air battery is a size 13 cell, the total vent area defined by all of the air ports in the housing is approximately 0.05 mm 2 ~about 0.115mm 2 Thus, in any embodiment of a size 13 cell disclosed herein, the total vent area defined by all of the air openings is about 0.05 mm 2 ~about 0.10mm 2 , about 0.06 mm 2 ~about 0.095mm 2 , about 0.06 mm 2 ~about 0.085mm 2 , about 0.07 mm 2 ~ approx. 0.09mm 2 , or about 0.08 mm 2 ~about 0.085mm 2 As also previously described in this disclosure, if the metal-air battery is a size 312 cell, the total vent area defined by all of the air openings in the housing can be about 0.03 mm 2 ~ approx. 0.08 mm 2 Thus, in any embodiment of a size 312 cell disclosed herein, the total vent area defined by all of the air openings is about 0.04 mm 2 ~ approx. 0.07mm 2 , about 0.04 mm 2 ~ approx. 0.06mm 2 , or about 0.04 mm 2 ~about 0.05mm 2 It could be. The anode can assembly 22 is electrically insulated from the cathode can assembly 40 by an insulating gasket 60. The insulating gasket 60 includes a circumferential sidewall 62 disposed between the upstanding sidewall 47 of the cathode can and the downwardly depending sidewall 30 of the anode can. An insulating gasket foot 64 is disposed generally between the can foot 36 of the anode can and the cathode can assembly 40. An insulating gasket top 66 is positioned where the sidewall 62 of the insulating gasket 60 extends from between the sidewall 30 adjacent the top of the cell and the sidewall 47. Thus, exterior surface 68 of cell 10 is defined by the exterior surface of the top of anode can 24 , exterior surface 58 of sidewall 47 of cathode can 44 , exterior surface 50 of the bottom of cathode can 44 , and a portion of top 66 of insulating gasket 60 .

[0017] The insulating gasket serves at least two primary functions. First, the insulating gasket 60 serves as a seal for the cell 10, preventing the anode 26 and / or electrolyte from leaking out of the cell between the exterior surface of the sidewall of the anode can 30 and the interior surface 56 of the sidewall of the cathode can 47. Thus, the insulating gasket 60 must have suitable liquid sealing properties to prevent such leakage. Typically, such properties can be obtained with a variety of elastically deformable thermoplastic polymeric materials. Second, the insulating gasket 60 provides electrical insulation to prevent any effective direct electrical contact between the anode can 24 and cathode can 44. Thus, the sidewall 62 of the insulating gasket 60 should generally surround and provide insulating properties around the entire periphery of the cell between the exterior and interior surfaces 56, from the top of sidewall 47 to the bottom of sidewall 30. Similarly, the foot 64 of the insulating gasket 60 should surround and provide electrical insulation properties around the entire periphery of the cell between the foot 36 of sidewall 30, the bottom of sidewall 47, and the outer periphery of the cathode can assembly 40. The combination of good liquid sealing properties and good electrical insulation properties is typically achieved by constructing known battery grade nylon polymeric materials in the desired configuration. To meet electrical insulation requirements, the insulating gasket 60 may have good dielectric insulating properties, may have a minimal thickness for the sidewall 62, and may be free of pinholes or other defects that may allow current transfer between the sidewalls 30 and 47. Thicknesses of the insulating gasket sidewall 62 of about 200 to about 250 microns are typical for conventional electrochemical cells. Thicknesses as thin as 100 microns are acceptable for the cells of the present disclosure, using the same elastically deformable thermoplastic nylon material as the thicker insulating gaskets of the prior art. Depending on the construction of the battery to which the insulating gasket is applied, intermediate thicknesses such as 150 microns, 140 microns, 127 microns, etc. may be selected for some cells. However, where cell volumetric efficiency is an operational consideration, preferred thicknesses are, for example, less than 120 or 110 microns, down to as low as 100 microns. Thus, the preferred range of insulating gasket 60 thicknesses for use in cells 10 of the present disclosure has a lower end of about 100 microns.

[0018] In any embodiment disclosed herein, the porous diffusion layer 57 is a microporous hydrophobic polymeric material, such as a polytetrafluoroethylene (PTFE) membrane, about 25 to about 100 microns thick, that allows the passage of air and is generally impermeable to the battery electrolyte. For example, the porous diffusion layer 57 is Teflon™. In any embodiment disclosed herein, the porous diffusion layer 57 may be used in combination with the air port 54 to efficiently transport oxygen to the active reactive surface area of ​​the positive electrode assembly. The cellulose air diffusion layer 32 may be positioned below the porous diffusion layer 57 and may act as a protective lateral air diffusion layer. Specifically, when the cell is activated, the anode can assembly 22 presses down on the separator 74 and the cellulose air diffusion layer 32 helps protect the air vents 54 from being completely covered. The active layer 72 may further include a connection base layer, i.e., a conductive woven nickel wire layer (not shown), that may interface with the positive electrode can as a current collector. In any embodiment disclosed herein, carbon may form a matrix surrounding the conductive layer of nickel wire. Nickel may be used for the conductive layer because it exhibits little or no corrosion in the zinc-air cell environment and because nickel is an excellent electrical conductor. In any embodiment disclosed herein, the thickness of the positive electrode assembly between the separator 74 and the porous diffusion layer 57 is as small as possible.

[0019] The aqueous electrolyte for the metal-air battery of the present technology may include a base such as sodium hydroxide (NaOH), potassium hydroxide (KOH), or a combination thereof. The electrolyte of any embodiment disclosed herein may include a surfactant system, a corrosion inhibitor (e.g., one or more of indium hydroxide, polyaniline, polyethylene glycol, or polypropylene glycol, and lithium hydroxide), a gelling agent (e.g., a polyacrylate polymer), a gas suppressing additive (e.g., one or more of zinc oxide, aluminum hydroxide, LiOH, and calcium bromide), potassium hydroxide, sodium hydroxide, cesium hydroxide, boric acid, sodium borate, potassium borate, sodium stannate, potassium stannate, or a combination of any two or more thereof.

[0020] The surfactant system may include at least one amphoteric fluorosurfactant. For example, the surfactant system may include at least two amphoteric fluorosurfactants. In any embodiment herein, the surfactant system may include one or more amphoteric fluorosurfactants and one or more of corrosion inhibitors (e.g., one or more of indium hydroxide, polyaniline, polyethylene glycol or polypropylene glycol, and lithium hydroxide), gelling agents (e.g., polyacrylate polymers), gas suppression additives (e.g., one or more of zinc oxide, aluminum hydroxide, LiOH, and calcium bromide), potassium hydroxide, sodium hydroxide, cesium hydroxide, boric acid, sodium borate, potassium borate, sodium stannate, and potassium stannate. In any embodiment herein, the surfactant system may be CHEMGUARD® S-111, CHEMGUARD® S-500, CAPSTONE® FS-50, CAPSTONE® FS-51, APFS-14, DYNAX DX3001, ZONYL® FSK, ZONYL® FS-500, or a combination of any two or more thereof.

[0021] The electrolyte and / or surfactant system of any embodiment herein may include additional surfactants, such as hexyldiphenyloxide disulfonic acid, diethylenetriamine, octylphenoxypolyethoxyethanol, a compound of formula (III), or a combination of any two or more thereof. Compounds of formula (III) include: [ka] In the formula, R 13 , R 14 , R 15 , R 16 , R 17 , R 18 , R 19 , R 20 , and R 21 are each independently a hydrogen atom, an alkyl group, an alkenyl group, or a cycloalkyl group; 2 is O or S; X 3is OH or SH; and w is 5 to 50. In any embodiment disclosed herein, R 13 , R 14 , R 15 , R 16 , R 17 , R 18 , R 19 , R 20 , and R 21 Each of X may be hydrogen. In any embodiment disclosed herein, X 2 may be O. In any embodiment disclosed herein, X 3 may be OH. In any embodiment disclosed herein, w may be 5 to 15. In any embodiment disclosed herein, w may be 5 to 10. In any embodiment disclosed herein, R 13 is C1~C 12 R is an alkyl group; 14 , R 15 , R 16 , R 17 , R 18 , R 19 , R 20 , and R 21 are hydrogen; X 2 is O;X 3 is OH; and w can be 5 to 15. In any embodiment disclosed herein, R 13 may be octyl and w may be 5 to 10. In another embodiment, R 13 is 1,1,3,3-tetramethylbutyl, and w is 5 to 10.

[0022] The electrolyte of any embodiment herein may further include hexyldiphenyloxide disulfonic acid as part of a hexyldiphenyloxide disulfonic acid surfactant system. The hexyldiphenyloxide disulfonic acid surfactant system may reduce voltage suppression. The hexyldiphenyloxide disulfonic acid surfactant system of any embodiment disclosed herein has a surfactant concentration of about 1.08 g / cm. 3 ~Approx. 1.20g / cm 3(about 9.0 to about 10.0 pounds per gallon), e.g., about 1.17 g / cm 3 (about 9.8 pounds per gallon). The hexyl diphenyl oxide disulfonic acid surfactant system of any embodiment disclosed herein may have a pH of less than about 2.0. The hexyl diphenyl oxide disulfonic acid may have a solubility of about 50% in water. The hexyl diphenyl oxide disulfonic acid surfactant system of any embodiment disclosed herein may comprise about 70% to about 75% by weight of the sulfonated benzene, 1,1'-oxybis-sec-hexyl derivative. In any embodiment disclosed herein, the hexyl diphenyl oxide disulfonic acid surfactant system may comprise about 0% to about 5% or about 2% to about 4% by weight of sulfuric acid. The hexyl diphenyl oxide disulfonic acid surfactant of any embodiment disclosed herein may comprise about 20% to about 30% or about 22% to about 28% by weight of water. In an exemplary embodiment, the hexyl diphenyl oxide disulfonic acid surfactant is Calfax® 6LA-70 available from Pilot Chemical Company, 2744 East Kemper Road, Cincinnati, Ohio, 45241, which may also act as a coupling agent and / or HLB adjuster in other embodiments of the present disclosure. Thus, the term "surfactant" should not be considered in a limiting sense as exemplified by Calfax® 6LA-70, but rather describes one of the functions that, for example, hexyl diphenyl oxide disulfonic acid and / or hexyl diphenyl oxide disulfonic acid surfactant systems may provide. In any embodiment herein, the hexyl diphenyl oxide disulfonic acid may be present in an amount of about 500 ppm to about 5,000 ppm, for example, about 1,000 ppm to about 4,000 ppm or about 2,000 ppm to about 3,000 ppm. Thus, the hexyl diphenyl oxide disulfonic acid may be present in an amount of about 1,000 ppm, about 2,000 ppm, about 3,000 ppm, about 4,000 ppm, or about 5,000 ppm, or a range between any two of these values ​​(including the endpoints). For example, the hexyl diphenyl oxide disulfonic acid may be present in an amount of about 3000 ppm; in another embodiment, the hexyl diphenyl oxide disulfonic acid may be present in an amount of about 4,500 ppm.

[0023] The electrolyte of any embodiment disclosed herein may further include a corrosion inhibitor. The corrosion inhibitor may be used to assist in maintaining a clean zinc surface, which in turn increases cell voltage and efficiency. Both the corrosion inhibitor and the amphoteric fluorosurfactant may result in improved cell voltage and cell performance. The corrosion inhibitor may enhance electrical conductivity. The corrosion inhibitor may be present in the electrolyte at about 100 ppm to about 15,000 ppm, for example, about 200 ppm to about 300 ppm. In any embodiment herein, the corrosion inhibitor may be present in an amount of about 150 ppm, about 200 ppm, about 250 ppm, about 300 ppm, about 350 ppm, or a range between any two of these values, including the endpoints. In any embodiment herein, the corrosion inhibitor may be present at about 250 ppm. For corrosion inhibitors only, the ppm amounts are based on the total weight of the electrolyte if the corrosion inhibitor is a liquid at room temperature, or based on the weight of zinc in the negative electrode if the corrosion inhibitor is a solid at room temperature.

[0024] The corrosion inhibitor of any embodiment of the present technology may be an aromatic amine polymer, indium hydroxide, polyaniline, polyethylene glycol, polypropylene glycol, lithium hydroxide, or a combination of any two or more thereof. For example, the corrosion inhibitor may include a compound of formula (II): [ka] In the formula, R 9 , R 10 , R 11 , and R 12 are each independently hydrogen, a substituted or unsubstituted alkyl, a substituted or unsubstituted alkenyl, or a substituted or unsubstituted cycloalkyl group; and t is 100 to 500. In any embodiment disclosed herein, R 9 , R 10 , R 11 , and R 12 may each be hydrogen. In any embodiment disclosed herein, t may be from 100 to 200. In any embodiment disclosed herein, R 9 , R 10 , R 11 , and R 12 may each be hydrogen, and m may be 100 to 200. As mentioned above, the corrosion inhibitor may include polyaniline. For example, the polyaniline may be emeraldine polyaniline. The emeraldine type polyaniline may be neutral and have high stability at room temperature. The polyaniline of any embodiment disclosed herein may be a non-acid doped type polyaniline and is not a conductive type polyaniline. The polyaniline of any embodiment disclosed herein may act as a corrosion inhibitor and / or provide other benefits that are not limited to polyaniline acting only as a corrosion inhibitor. Thus, referring to polyaniline as a "corrosion inhibitor" does not limit polyaniline to only that particular function. For example, polyaniline may enhance electrical conductivity. As noted above, the corrosion inhibitor may include indium hydroxide. In any embodiment disclosed herein, the indium hydroxide may be present in an amount of about 2000 ppm to about 4000 ppm, for example, about 2,500 ppm to about 3,500 ppm, or about 2,750 ppm to about 3,250 ppm, based on the total mass of zinc in the negative electrode. Thus, the indium hydroxide may be present in an amount of about 2,000 ppm, about 2,500 ppm, about 3,000 ppm, about 3,500 ppm, about 4,000 ppm, or a range between any two of these values ​​(including the endpoints). For example, the indium hydroxide may be present in an amount of about 3000 ppm, based on the total mass of zinc in the negative electrode, in any embodiment disclosed herein.

[0025] The electrolyte may include a gelling agent. Any suitable gelling agent in the art may be used as long as it does not deviate from the scope of the present disclosure. The gelling agent may be present in an amount of about 500 ppm to about 1,500 ppm, about 750 ppm to about 1,250, or about 900 ppm to about 1,100 ppm based on the total weight of the electrolyte. Thus, the gelling agent may be present in an amount of about 500 ppm, about 600 ppm, about 700 ppm, about 800 ppm, about 900 ppm, about 1,000 ppm, about 1,100 ppm, about 1,200 ppm, about 1,300 ppm, about 1,400 ppm, or about 1,500 ppm, or a range between any two of these values ​​(including the endpoints). For example, the gelling agent may be present in an amount of about 1,000 ppm in any embodiment disclosed herein. In any of the embodiments disclosed herein, the gelling agent may be a polyacrylic acid polymer, such as a cross-linked polyacrylic acid polymer.

[0026] The electrolyte may include a polyacrylate polymer. The polyacrylate polymer may be present in an amount of about 1,000 ppm to about 5,000 ppm. This may include about 2,000 ppm to about 4,000 ppm, or about 2,500 ppm to about 3,500 ppm. Thus, the polyacrylate polymer may be present in any embodiment disclosed herein in an amount of about 2,000 ppm, about 2,500 ppm, about 3,000 ppm, about 3,500 ppm, about 4,000 ppm, or a range between any two of these values ​​(including the endpoints). For example, the polyacrylate polymer may be present in an amount of about 2,000 ppm. By way of example, a suitable polyacrylate polymer is a crosslinked polyacrylate polymer. Zinc oxide may be present in an amount of about 1% to about 10% by weight of the electrolyte. This may include about 1% to about 8%, 1% to about 5%, about 1.5% to about 5%, or about 2% to about 5% by weight of the electrolyte. Thus, zinc oxide may be present in any embodiment disclosed herein in an amount of about 1%, about 1.5%, about 2%, about 2.5%, about 3%, about 3.5%, or about 4% by weight of the electrolyte, or a range between any two of these values ​​(including the endpoints). For example, zinc oxide may be present in an amount of about 2% by weight of the electrolyte. Zinc oxide is not limited to acting solely as a gas suppressing additive, as it may provide other benefits. Thus, referring to zinc oxide as a "gas suppressing additive" does not limit zinc oxide to only that particular function. For example, zinc oxide in any embodiment disclosed herein may modulate zinc surface passivation. The electrolyte may include potassium hydroxide. The potassium hydroxide may be present in an amount of about 20% to about 45%, e.g., about 25% to about 40% or about 30% to about 35%, based on the weight of the electrolyte. In any embodiment disclosed herein, the potassium hydroxide may be present in an amount of about 45%, about 30%, about 25%, or about 20%, based on the weight of the electrolyte, or a range between any two of these values ​​(including the endpoints). For example, the potassium hydroxide may be present in an amount of about 33% based on the weight of the electrolyte. The electrolyte may include sodium hydroxide. The sodium hydroxide may be present in an amount of about 20% to about 45%, for example, about 25% to about 40% or about 30% to about 35%, based on the electrolyte mass. The sodium hydroxide may be present in an amount of about 45%, about 30%, about 25%, or about 20%, based on the electrolyte mass, or a range between any two of these values ​​(including the endpoints), in any embodiment disclosed herein. For example, the sodium hydroxide may be present in an amount of about 33% based on the electrolyte mass.

[0027] In any embodiment disclosed herein, the electrolyte of the metal-air battery may include a surfactant system and a corrosion inhibitor, the surfactant system including an amphoteric fluorosurfactant. The surfactant system may further include a gas-suppressing additive. In any embodiment disclosed herein, the surfactant system may further include hexyldiphenyloxide disulfonic acid, diethylenetriamine, or octylphenoxypolyethoxyethanol, a compound of formula (III), or a combination of any two or more thereof. The gas-suppressing additive may include a material such as LiOH or ZnO. In any embodiment disclosed herein, the electrolyte may include about 500 ppm to about 20,000 ppm of the gas-suppressing additive. Thus, the electrolyte may contain the gas suppressing additive at about 500 ppm, about 600 ppm, about 700 ppm, about 800 ppm, about 900 ppm, about 1,000 ppm, about 2,000 ppm, about 3,000 ppm, about 4,000 ppm, about 5,000 ppm, about 6,000 ppm, about 7,000 ppm, about 8,000 ppm, about 9,000 ppm, about 10 The composition may include an amount of about 1,000 ppm, about 11,000 ppm, about 12,000 ppm, about 13,000 ppm, about 14,000 ppm, about 15,000 ppm, about 16,000 ppm, about 17,000 ppm, about 18,000 ppm, about 19,000 ppm, about 20,000 ppm, or a range between any two of these values ​​(inclusive of the endpoints). The electrolyte of any embodiment disclosed herein may contain LiOH at about 500 ppm, about 600 ppm, about 700 ppm, about 800 ppm, about 900 ppm, about 1,000 ppm, about 2,000 ppm, about 3,000 ppm, about 4,000 ppm, about 5,000 ppm, about 6,000 ppm, about 7,000 ppm, about 8,000 ppm, about 9,000 ppm, or about 10,000 ppm. pm, about 10,000 ppm, about 11,000 ppm, about 12,000 ppm, about 13,000 ppm, about 14,000 ppm, about 15,000 ppm, about 16,000 ppm, about 17,000 ppm, about 18,000 ppm, about 19,000 ppm, about 20,000 ppm, or a range between any two of these values ​​(inclusive of the endpoints).

[0028] The metal-air battery of any embodiment disclosed herein may include a carbon dioxide scrubbing agent to improve cell performance and lifespan. When air enters the cell, the carbon dioxide reacts with the carbon dioxide scrubber to prevent or at least minimize the reaction of the carbon dioxide with alkaline components in the electrolyte or on the surface of the air diffusion membrane. The scrubber allows the electrolyte conductivity and positive electrode porosity to be maintained over time. The electrolyte of any embodiment disclosed herein may be doped with a material that reacts preferentially with dissolved carbon dioxide before reacting with the alkali hydroxide present in the electrolyte. Illustrative carbon dioxide absorbents include, but are not limited to, lithium hydroxide, calcium hydroxide, lithium peroxide, lithium oxide, amines, olivine, or other basic hydroxides. In any embodiment disclosed herein, the carbon dioxide absorbent can be used to coat the inside of the cathode can in the space where incoming air may encounter the absorbent before contacting the anode active material (i.e., zinc). For example, as illustrated in FIG. 1, the air reservoir 55 is the void space within the battery cell. The cell is configured such that air enters the cell through the air port 54 before contacting the diffusion layer 32. Thus, the carbon dioxide absorbent may be applied to the interior surface of the cell within the air reservoir 55 to remove or at least reduce the carbon dioxide as it enters the cell through the air port 54. The absorbent may be embedded in or deposited on either the cellulose air diffusion layer 32, the cathode 42, or the porous diffusion layer 57. The absorbent may be applied as a powder, as a film by painting with a solvent that is subsequently removed, or by other practical means. In any of the embodiments disclosed herein, a carbon dioxide absorbent may be added to the alkaline electrolyte. In such embodiments, the absorbent is selected such that the material will first react with the carbon dioxide while retaining any NaOH or KOH present in the electrolyte. Without wishing to be bound by theory, it is believed that when CO2 enters the zinc-air cell, it may dissolve in the aqueous electrolyte, thereby generating carbonic acid. The carbonic acid then reacts with the absorbent before reacting with the NaOH or KOH present in the electrolyte, thereby maintaining the desired alkalinity of the electrolyte. In any embodiment disclosed herein, a carbon dioxide absorbent may be included in the packaging housing the hearing aid cell (according to the present technology) to minimize storage damage from carbon dioxide exposure prior to cell use. For example, the package may contain a chamber intended to hold a zinc-air cell, such as a hearing aid battery, for storage or sale. The package may include the carbon dioxide absorbent as a powder, as a coating on the package, or embedded within the plastic or paper of the packaging and chamber forming material.

[0029] The negative electrode includes an active negative electrode material, and the negative electrode can assembly surrounds the active negative electrode material. In any embodiment disclosed herein, the active negative electrode material may include zinc, and the negative electrode is referred to as a "zinc negative electrode." In this regard, it is noted that as used herein, the negative electrode "active material" may refer to a single chemical compound that is part of the discharge reaction at the negative electrode of the cell and contributes to the cell discharge capacity, including impurities and small amounts of other moieties that may be present therein. The negative electrode "active material" does not include current collectors, electrode leads, etc., that may contain or support the zinc active material. Physical modifications to the negative electrode, alone or in combination with the chemical modifications described above, can also improve the life of the cell. For example, by reducing the diffusion resistance for hydroxide ions, the cell can be efficiently discharged with a lower concentration of hydroxide ions in the electrolyte than can be used in conventional cells. This can be achieved, for example, by adjusting the zinc particle size distribution to provide a narrow distribution of similar zinc particle sizes in the negative electrode, thereby enhancing the porosity (diffusion paths) for hydroxide ions. In addition to improving the diffusion properties, the particle size distribution of the present disclosure also provides porous sites for ZnO deposition, thereby delaying negative electrode passivation. This approach is effective for use in the negative electrode of zinc-air battery cells and can be used in combination with other improvements disclosed herein.

[0030] A suitable zinc particle size distribution may be one in which at least 70% of the particles have a standard mesh sieve size within the 100 micron size range, and the mode of the distribution is between about 100 and about 300 microns. Suitable zinc particle size distributions include particle size distributions that meet the above test and have a mode of about 100 microns, about 150 microns, or about 200 microns. In any embodiment disclosed herein, about 70% of the particles are distributed in a particle size distribution range narrower than about 100 microns, such as about 50 microns, or about 40 microns or less.

[0031] The anode may include a cathode can assembly 40 including a cathode can 44 and a cathode 42. An exemplary embodiment of the cathode 42 is best seen in FIG. 1. An active layer 72 of the cathode 42 is disposed between a separator 74 and a porous diffusion layer 57. The active layer 72 is preferably in the range of about 50 microns to about 1,250 microns in thickness and promotes the reaction between hydroxyl ions in the electrolyte and the cathode oxygen of the air. The separator 74 may include or consist of one or both of a microporous plastic membrane and a microporous cellulose paper. The microporous plastic membrane is about 25 μm thick and is typically constructed of polypropylene. The paper material is 70 to 90 microns in thickness and has a basis weight of 20 to 25 g / m. 2 and is typically composed of polyvinyl alcohol and cellulose materials. The separator has the primary function of preventing the zinc particles of the anode from physical contact with the residual elements of the cathode 42. However, the separator 74 does allow hydroxyl ions and water to pass through the separator to the cathode assembly. Here, the cathode is an air cathode and the cathode active layer comprises carbon. The sidewall 47 of the cathode can 44 is joined to the bottom 46 of the can by an intermediate element 80. The outer surface of the intermediate element 80 extends from its lower end at the outer periphery 52 of the outer surface 50 of the bottom 46 to its upper end where it joins the outer surface 58 of the sidewall 47 in a generally vertical orientation. The inner surface of the intermediate element 80, if present, is represented at the junction of the inner surface 48 of the bottom 46 and the inner surface 56 of the sidewall 47. The inner surfaces 48 and 56 come together at a sharp corner such that the inner surface of the intermediate element is of nominal dimensions. The corner may be work hardened to the extent that the corner material is worked during corner formation, thereby strengthening the corner structure relative to the bottom 46 and sidewall 47 as it is formed in the intermediate element 80.

[0032] In any embodiment disclosed herein, the can / housing may be formed entirely of a metal or alloy having a hydrogen overvoltage close to that of the positive electrode (as opposed to a plating or cladding of the can), so long as sufficient strength and ductility is available from the material selected. In addition to nickel, materials having such hydrogen overvoltage characteristics include, for example, but are not limited to, cobalt and gold. In some embodiments, such materials may be coated onto a core layer as one or more coating layers, for example, by plating, cladding, or other application process. Materials that provide sufficient strength and ductility may be used as a single layer material instead of a composite structure. A single layer material includes CRS or other suitable material as a core layer. In any of the embodiments disclosed herein, nickel and nickel alloy plated steel strip may be used due to cost considerations and also due to the commercially available pre-plated steel strip that generally does not require post plating processes. The metal in the can / housing is preferably both ductile enough to withstand the drawing process and strong and rigid enough to withstand the cell crimping and sealing process and otherwise provide the primary overall structural strength to the cell / battery. In any of the embodiments disclosed herein, the housing may include nickel-clad stainless steel; nickel-plated cold rolled steel; INCONEL® (a non-magnetic alloy of nickel); pure nickel with minor alloying elements (e.g., Nickel 200 and related series of Nickel 200 alloys, such as Nickel 201) (all available from Huntington Alloys), or DURANICKEL® 301 available from Special Metals. For example, the housing may be made of nickel-plated stainless steel. Some precious metals may also be used as plating, cladding, or other coatings for the can / housing metals, examples of which are nickel-plated steel strip and the covering of mild steel strip that is plated with nickel after the can is manufactured. When multiple layers (e.g., CRS) coated on both sides with nickel are used, the present disclosure contemplates optional additional (e.g., fourth, fifth, etc.) layers, either between the nickel and the CRS or with a nickel layer between the CRS and the additional layer(s). For example, gold, cobalt, or other good electrical conductors may be deposited on some or all of the exterior surface of the cathode can (outside the nickel layer) after drawing or drawing and ironing the cathode can. Alternatively, such a fourth layer, etc., may be, for example, a bond-enhancing layer between the CRS and the nickel. When the can / housing is manufactured using the typical raw material structure nickel / stainless steel (SST) / nickel / NI / SST / NI as the sheet structure, such sheet structure may be about 0.002 inches to about 0.012 inches. This may include about 0.003 inches to about 0.010 inches or about 0.004 inches to about 0.006 inches, and thus the thickness may be about 0.002 inches, about 0.08 mm, about 0.003 inches, about 0.004 inches, about 0.005 inches, or about 0.006 inches, or a range between any two of these values ​​(including the endpoints). For example, the thickness may be about 0.005 inches (0.13 mm). In any embodiment disclosed herein, each of the nickel layers may represent about 1% to about 10% of the total thickness of the metal sheet in such a three-layer structure. This may include about 1.5% to about 9%, about 2% to about 8%, about 2.5% to about 7%, or about 3% to about 6.5% of the total thickness of the metal sheet in such a three-layer structure. For example, each of the nickel layers may represent about 2% to about 4% of the total thickness of the metal sheet in such a three-layer structure. In any embodiment disclosed herein, each of the nickel layers may represent about 2% of the total thickness of the metal sheet in such a three-layer structure.

[0033] The invention thus generally described will be more readily understood by reference to the following examples, which are provided by way of illustration and are not intended to limit the invention. EXAMPLES

[0034] Example 1. Total ventilation area is 0.0498 mm 2 Size 312 cells of the present technology, which are 0.001 to 0.001 mm in diameter, were prepared using a zinc anode and an aqueous electrolyte containing (by electrolyte weight) 31.5% potassium hydroxide, 10,000 ppm amphoteric fluorosurfactant, 1.5% lithium hydroxide, 2% zinc oxide, and 1,000 ppm polyacrylic acid. A comparative "standard" cell was prepared, the standard cell containing no amphoteric fluorosurfactant and having a total vent area of ​​0.1329 mm 2 The cells were discharged at 10 / 2mA at 80% RH (relative humidity) as per ANSI / IEC testing, and the technology cells showed approximately 15% capacity improvement over the comparative "standard" cells. Example 2. Total ventilation area is 0.0998 mm 2 Size 13 cells of the present technology, having a total vent area of ​​0.1295 mm, were prepared using a zinc negative electrode and an aqueous electrolyte containing potassium hydroxide, the amphoteric fluorosurfactant of Example 1, lithium hydroxide, and the polyacrylic acid of Example 1 in the same amounts as the electrolyte of Example 1. A comparative "standard" cell was prepared, the standard cell containing no amphoteric fluorosurfactant, and having a total vent area of ​​0.1295 mm 2 The cells were discharged at 12 / 3 mA at 80% RH (relative humidity) as per ANSI / IEC testing, and the cells with this technology showed approximately 7% capacity improvement compared to the comparative "standard" cells (Figure 2). Example 3. Total ventilation area is 0.0660 mm 2 Size 312 cells of the present technology, 0.001 to 0.001 mm2 in diameter, were prepared using a zinc negative electrode and an aqueous electrolyte containing potassium hydroxide, the amphoteric fluorosurfactant of Example 1, lithium hydroxide, and the polyacrylic acid of Example 1 in the same amounts as the electrolyte of Example 1. A comparative "standard" cell was prepared, the standard cell containing no amphoteric fluorosurfactant, and having a total vent area of ​​0.0869 mm2. 2The cells were discharged at 10 / 2mA at 80% RH (relative humidity) as per ANSI / IEC testing, and the cells showed approximately 13% capacity improvement over the comparative "standard" cells (Figure 3). Example 4. Total ventilation area is 0.0660 mm 2 Size 312 cells of the present technology, 0.001 to 0.001 mm2 in diameter, were prepared using a zinc negative electrode and an aqueous electrolyte containing potassium hydroxide, the amphoteric fluorosurfactant of Example 1, lithium hydroxide, and the polyacrylic acid of Example 1 in the same amounts as the electrolyte of Example 1. A comparative "standard" cell was prepared, the standard cell containing no amphoteric fluorosurfactant, and having a total vent area of ​​0.0869 mm2. 2 The cells were discharged at 20% RH (relative humidity) per ANSI / IEC test 10 / 2mA, and the technology cells showed approximately 4% capacity improvement over the comparative "standard" cells (Figure 4). Example 5. To further illustrate the contribution of the electrolyte itself to the performance of the batteries of the present technology, three aqueous electrolytes were prepared and evaluated as follows. The three electrolytes were: (1) an aqueous electrolyte containing 33% potassium hydroxide (by weight of electrolyte) and 2% zinc oxide (by weight of electrolyte); (2) an aqueous electrolyte comprising 33% potassium hydroxide (by weight of electrolyte), 2% zinc oxide (by weight of electrolyte), and 7,500 ppm of a carboxylated amine surfactant; and (3) An aqueous electrolyte of the present technology comprising 33% potassium hydroxide (based on the electrolyte mass), 2% zinc oxide (based on the electrolyte mass), and 10,000 ppm amphoteric fluorosurfactant. It was. The positive electrode performance resulting from the use of the electrolyte was tested independently of the negative electrode by placing a pure zinc reference electrode in the solution close to the positive electrode (Note: the same distance from the positive electrode was used for all tests). The positive electrode had unrestricted air access on one side and was exposed to the electrolyte on the other side. A current of 1 mA / cm was then applied to the positive electrode. 2 and 5mA / cm 2A current draw of 0.01 V was applied and the potential against a pure zinc reference was recorded for each of the above electrolytes. As illustrated in Figure 5, the aqueous electrolyte (3) of the present technology showed improved behavior with less voltage drop at the same current draw compared to the aqueous electrolytes (1) and (2).

[0035] While certain embodiments have been illustrated and described, it will be understood that changes and modifications may be made thereto, in accordance with ordinary skill in the art, without departing from the technology in its broader aspects as defined in the following claims. The embodiments illustratively described herein may suitably be practiced in the absence of any element or elements, limitation or limitations not specifically disclosed herein. Thus, for example, the terms "comprise", "include", "contain", etc. shall be read expansively and without limitation. Furthermore, the terms and expressions used herein are used as terms of description, not terms of limitation, and in the use of such terms and expressions, there is no intention to exclude any equivalents of the illustrated and described features or portions thereof, and it is recognized that various modifications are possible within the scope of the claimed technology. Furthermore, the phrase "consisting essentially of" is understood to include the specifically recited elements and additional elements that do not materially affect the basic and novel characteristics of the claimed technology. The phrase "consisting of" excludes elements not specified. The present disclosure is not limited with respect to the specific embodiments described in this application. Many modifications and variations can be made without departing from the spirit and scope thereof, as will be apparent to those skilled in the art. Functionally equivalent methods and compositions within the scope of the present disclosure, in addition to those recited herein, will be apparent to those skilled in the art from the foregoing description. Such modifications and variations are intended to fall within the scope of the appended claims. The present disclosure is limited only by the terms of the appended claims, along with the full scope of equivalents to which such claims are entitled. It is to be understood that the present disclosure is not limited to particular methods, reagents, compound compositions, or biological systems, which can, of course, vary. It is also to be understood that the terminology used herein is for the purpose of describing particular embodiments only, and is not intended to be limiting. Additionally, when features or aspects of the disclosure are described in terms of Markush groups, those skilled in the art will recognize that the disclosure is also thereby described in terms of any individual components or subgroups of components of the Markush group. As will be understood by those skilled in the art, for any and all purposes, particularly in terms of providing a written description, all ranges disclosed herein also encompass any and all possible subranges and combinations of those subranges. Any recited range can be readily recognized as fully descriptive and allowing the same range to be broken down into at least two, three, four, five, ten, etc. As a non-limiting example, each range described herein can be readily broken down into a lower third, a middle third, and an upper third, etc. As will be understood by those skilled in the art, all phrases, such as "up to," "at least," "greater than," "less than," etc., refer to ranges that include the recited numbers and can subsequently be broken down into subranges as described above. Finally, as will be understood by those skilled in the art, a range includes its individual components. All publications, patent applications, issued patents, and other documents mentioned herein are incorporated by reference herein as if each individual publication, patent application, issued patent, or other document was specifically and individually indicated to be incorporated by reference in its entirety. Definitions contained in text incorporated by reference are excluded to the extent that they negate definitions in this disclosure.

[0036] The present technology may include, but is not limited to, the features and combinations of features set forth in the lettered paragraphs below, and the following paragraphs should not be construed as limiting the scope of the claims appended hereto or as mandating that all such features must be included in such claims. A. A battery comprising an air cathode, an anode, an aqueous electrolyte, and a housing, The battery is a size 13 metal-air battery; the housing includes one or more air vents defining a vent area; The total vent area defined by all of the air openings is approximately 0.050 mm 2 ~about 0.115mm 2 and The aqueous electrolyte comprises an amphoteric fluorosurfactant. battery. B. The total vent area defined by all of the air openings is approximately 0.05 mm 2 ~about 0.10mm 2 The battery of paragraph A, C. The total vent area defined by all of the air openings is approximately 0.060 mm 2 ~about 0.950mm 2 The battery of paragraph A or B, D. The total vent area defined by all of the air openings is approximately 0.060 mm 2 ~about 0.085mm 2 The battery of any one of paragraphs A to C, E. The total vent area defined by all of the air openings is approximately 0.07 mm 2 ~ approx. 0.09mm 2The battery of any one of paragraphs A to C, F. The total vent area defined by all of the air openings is approximately 0.08 mm 2 ~about 0.085mm 2 The battery of any one of paragraphs A through E, G. The battery of any one of paragraphs A-F, wherein the negative electrode comprises zinc. H. The battery of any one of paragraphs A through G, further comprising a carbon dioxide absorbent. I. The battery of paragraph H, wherein the carbon dioxide absorbent comprises lithium hydroxide, calcium hydroxide, lithium peroxide, an amine, or olivine. J. The battery of paragraph H or paragraph I, further comprising an air diffusion pad, the air diffusion pad comprising a carbon dioxide absorbent. K. The battery of any one of paragraphs H-J, further comprising an interior surface of the housing having a coating of a carbon dioxide absorbent. L. The battery of any one of paragraphs H-K, further comprising an air reservoir defined by the housing and an air diffusion layer within the battery, the carbon dioxide absorbent being deposited on a surface of the air reservoir as a powder or a film. M. The battery of any one of paragraphs A-L, wherein the amphoteric fluorosurfactant contains a short chain perfluoro substituent that cannot decompose to perfluorooctanoic acid. N. The battery of any one of paragraphs A through M, wherein the amphoteric fluorosurfactant comprises a betaine functionality. O. Amphoteric fluorosurfactants include compounds of formula (I): [ka] During the ceremony, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 are each independently a hydrogen, an alkyl, an alkenyl, or a cycloalkyl group; X 1 are -C(O)-, -SO2-, and -C(O)NRa -,-SO2NR a -, -CO2-, or -SO2O-; R a is H or an alkyl group; m and p are each independently 0, 1, 2, 3, 4, 5, or 6; n and r are each independently 1, 2, 3, 4, or 5; The battery of any one of paragraphs A through N. PR 1 , R 2 , R 3 , R 4 , R 5 , and R 6 are H, respectively; R 7 and R 8 are each independently C1-C4 alkyl; X 1 is SO2 or -SO2NR a and; R a is H; n is 2 or 3; p is 2, 3, 4, or 5; m is 3, 4, 5, or 6; r is 1, A battery as described in paragraph O. QR 1 , R 2 , R 3 , R 4 , R 5 , and R 6 are H, respectively; R 7 and R 8 are each independently C1-C4 alkyl; X 1 is SO2; n and p are 2; m is 4, 5, or 6; r is 1, A battery described in paragraph O or paragraph P. R. The battery of any one of paragraphs A-Q, wherein the aqueous electrolyte includes a surfactant system. S. The battery of paragraph R, wherein the surfactant system comprises an amphoteric fluorosurfactant. T. The battery of paragraph R or S, wherein the surfactant system includes CHEMGUARD® S-111, CHEMGUARD® S-500, CAPSTONE® FS-50, CAPSTONE® FS-51, APFS-14, DYNAX DX3001, ZONYL® FSK, ZONYL® FS-500, or a combination of any two or more thereof. U. The battery of any one of paragraphs A-T, wherein the aqueous electrolyte further comprises lithium hydroxide. V. The battery of any one of paragraphs A through U, wherein the aqueous electrolyte comprises from about 500 ppm to about 20,000 ppm of lithium hydroxide. W. A battery comprising an air cathode, an anode, an aqueous electrolyte, and a housing, The battery is a size 312 metal-air battery; the housing includes one or more air vents defining a vent area; The total ventilation area defined by all of the air openings is approximately 0.03 mm 2 ~ approx. 0.08 mm 2 and; The aqueous electrolyte comprises an amphoteric fluorosurfactant. battery. X. The total ventilation area defined by all of the air openings is approximately 0.04 mm 2 ~ approx. 0.07mm 2 The battery of paragraph W, Y. The total ventilation area defined by all of the air openings is approximately 0.04 mm 2 ~ approx. 0.06mm 2 The battery of paragraph W or paragraph X, Z. The total vent area defined by all of the air openings is approximately 0.04 mm 2 ~about 0.05mm 2 The battery of any one of paragraphs WY. AA. The battery of any one of paragraphs W-Z, wherein the negative electrode comprises zinc. AB. The battery of any one of paragraphs W through AA, further comprising a carbon dioxide absorbent. AC. The battery of paragraph AB, wherein the carbon dioxide absorbent comprises lithium hydroxide, calcium hydroxide, lithium peroxide, an amine, or olivine. AD. The battery of paragraph AB or paragraph AC, further comprising an air diffusion pad, the air diffusion pad comprising a carbon dioxide absorbent. AE. The battery of any one of paragraphs AB-AD, further comprising an interior surface of the housing having a coating of a carbon dioxide absorbent. AF. The battery of any one of paragraphs AB-AE, further comprising an air reservoir defined by the housing and an air diffusion layer within the battery, the carbon dioxide absorbent being deposited on a surface of the air reservoir as a powder or film. AG. The battery of any one of paragraphs W through AF, wherein the amphoteric fluorosurfactant contains short chain perfluoro substituents that cannot decompose to perfluorooctanoic acid. AH. The battery of any one of paragraphs W-AG, wherein the amphoteric fluorosurfactant includes betaine functionality. AI. The amphoteric fluorosurfactant comprises a compound of formula (I): [ka] During the ceremony, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 are each independently a hydrogen, an alkyl, an alkenyl, or a cycloalkyl group; X 1 are -C(O)-, -SO2-, and -C(O)NR a -,-SO2NR a -, -CO2-, or -SO2O-; R a is H or an alkyl group; m and p are each independently 0, 1, 2, 3, 4, 5, or 6; n and r are each independently 1, 2, 3, 4, or 5; A battery as described in any one of paragraphs W through AH. A.J.R. 1 , R 2 , R 3 , R 4 , R 5 , and R 6 are H, respectively; R 7 and R 8 are each independently C1-C4 alkyl; X 1 is SO2 or -SO2NR a and; R a is H; n is 2 or 3; p is 2, 3, 4, or 5; m is 3, 4, 5, or 6; r is 1, A battery as described in paragraph AI. A.K.R. 1 , R 2 , R 3 , R 4 , R 5 , and R 6 are H, respectively; R 7 and R 8 are each independently C1-C4 alkyl; X 1 is SO2; n and p are 2; m is 4, 5, or 6; r is 1, A battery described in paragraph AI or paragraph AJ. AL. The battery of any one of paragraphs W-AK, wherein the aqueous electrolyte includes a surfactant system. AM. The battery of paragraph AL, wherein the surfactant system includes an amphoteric fluorosurfactant. AN. The battery of paragraph AL or AM, wherein the surfactant system includes CHEMGUARD® S-111, CHEMGUARD® S-500, CAPSTONE® FS-50, CAPSTONE® FS-51, APFS-14, DYNAX DX3001, ZONYL® FSK, ZONYL® FS-500, or a combination of any two or more thereof. AO. The battery of any one of paragraphs W-AN, wherein the aqueous electrolyte further comprises lithium hydroxide. AP. The battery of any one of paragraphs W through AO, wherein the aqueous electrolyte comprises from about 500 ppm to about 20,000 ppm of lithium hydroxide.

[0037] Other embodiments are within the scope of the following claims.

Claims

1. A battery comprising an air cathode, an anode, an aqueous electrolyte, and a housing, the battery is a size 13 metal-air battery; the housing includes one or more air vents defining a ventilation area; The total vent area defined by all of said air openings is about 0.050 mm 2 ~Approx. 0.115mm 2 and The aqueous electrolyte comprises an amphoteric fluorosurfactant. battery.

2. The total vent area defined by all of said air openings is about 0.05 mm 2 ~Approx. 0.10mm 2 2 , or from about 0.060 mm 2 to about 0.950 mm 2 , or from about 0.060 mm 2 to about 0.085 mm 2 , or from about 0.07 mm 2 to about 0.09 mm 2 , or from about 0.08 mm 2 to about 0.085 mm 2 .

3. 10. The battery of claim 1 , wherein the negative electrode comprises zinc.

4. 10. The battery of claim 1, further comprising a carbon dioxide absorbent, the carbon dioxide absorbent comprising lithium hydroxide, calcium hydroxide, lithium peroxide, an amine, or olivine.

5. further comprising an air diffusion pad, said air diffusion pad comprising said carbon dioxide absorbent; or or further comprising an interior surface of the housing having a coating of the carbon dioxide absorbent; 5. The battery of claim 4, further comprising an air reservoir defined by the housing and an air diffusion layer within the battery, and wherein the carbon dioxide absorbent is deposited on a surface of the air reservoir as a powder or a film.

6. The amphoteric fluorosurfactant comprises a compound of formula (I): 【Chemistry 1】 During the ceremony, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 are each independently a hydrogen, an alkyl, an alkenyl, or a cycloalkyl group; X 1 is -C(O)-, -SO 2 --, --C(O)NR a -, -SO 2 N.R. a --, --CO 2 - or -SO 2 is O-; R a is H or an alkyl group; m and p are each independently 0, 1, 2, 3, 4, 5, or 6; n and r are each independently 1, 2, 3, 4, or 5; 10. The battery of claim 1.

7. R 1 , R 2 , R 3 , R 4 , R 5 , and R 6 are each H; R 7 and R 8 are each independently 1 ~C 4 is alkyl; X 1 , SO 2 and n and p are 2; m is 4, 5, or 6; r is 1; 7. The battery of claim 6.

8. A battery comprising an air cathode, an anode, an aqueous electrolyte, and a housing, the battery is a size 312 metal-air battery; the housing includes one or more air vents defining a ventilation area; The total vent area defined by all of the air openings is about 0.03 mm 2 ~ approx. 0.08 mm 2 and The aqueous electrolyte comprises an amphoteric fluorosurfactant. battery.

9. The total vent area defined by all of said air openings is about 0.04 mm 2 ~ approx. 0.07 mm 2 9. The battery of claim 8, wherein the cell diameter is about 0.04 mm 2 to about 0.06 mm 2 , or about 0.04 mm 2 to about 0.05 mm 2 .

10. 10. The battery of claim 8, wherein the negative electrode comprises zinc.

11. 10. The battery of claim 8, further comprising a carbon dioxide absorbent, the carbon dioxide absorbent comprising lithium hydroxide, calcium hydroxide, lithium peroxide, an amine, or olivine.

12. further comprising an air diffusion pad, said air diffusion pad comprising a carbon dioxide absorbent; or or further comprising an interior surface of the housing having a coating of the carbon dioxide absorbent; 12. The battery of claim 11, further comprising an air reservoir defined by the housing and an air diffusion layer within the battery, and wherein the carbon dioxide absorbent is deposited on a surface of the air reservoir as a powder or a film.

13. The amphoteric fluorosurfactant comprises a compound of formula (I): 【Chemistry 2】 During the ceremony, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 are each independently a hydrogen, an alkyl, an alkenyl, or a cycloalkyl group; X 1 is -C(O)-, -SO 2 --, --C(O)NR a -, -SO 2 N.R. a --, --CO 2 - or -SO 2 is O-; R a is H or an alkyl group; m and p are each independently 0, 1, 2, 3, 4, 5, or 6; n and r are each independently 1, 2, 3, 4, or 5; 9. The battery of claim 8.

14. R 1 , R 2 , R 3 , R 4 , R 5 , and R 6 are each H; R 7 and R 8 are each independently 1 ~C 4 is alkyl; X 1 , SO 2 and n and p are 2; m is 4, 5, or 6; r is 1; 14. The battery of claim 13.

15. 15. The battery of claim 8, wherein the aqueous electrolyte further comprises about 500 ppm to about 20,000 ppm of lithium hydroxide.

Citation Information

Patent Citations

  • Tabs for zinc / air batteries

    JP2004518243A

  • Air battery

    JP2007141745A

  • Lithium air battery

    JP2011108388A

  • Flat battery

    JP2017174795A

  • Surfactants for zinc-air batteries

    JP2017531295A