Improved method for forming thermoplastic powders for additive manufacturing.
The method of forming thermoplastic polymer foams with controlled properties addresses the challenges of residual stresses and angular irregularities in additive manufacturing, achieving defect-free and uniformly metered powders for improved additive manufacturing processes.
Patent Information
- Application Number
- JP2023561020
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-07-01
- Filing Date
- 2022-05-16
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2042-05-16
AI Technical Summary
Existing methods for producing thermoplastic powders for additive manufacturing, such as selective laser sintering (SLS), multi-jet fusion (MJF), and high-speed sintering (HSS), face challenges with residual stresses, angular irregularities, and the need for flow aids due to crystalline or semi-crystalline polymers, which limit the production of defect-free and uniformly metered powders.
A method involving the formation of thermoplastic polymer foams with controlled particle size, distribution, and morphology by cooling below the embrittlement temperature and milling to produce powders without the need for flow aids, utilizing foams with specific porosity and strut/cell wall thicknesses.
The method efficiently produces thermoplastic powders with improved flow characteristics and reduced defects, enabling high-quality layered manufacturing without the use of flow aids, enhancing the efficiency and quality of additive manufacturing processes.
Smart Images

Figure 0007579461000013 
Figure 0007579461000014 
Figure 0007579461000015
Abstract
Description
[Technical field]
[0001] The present disclosure relates to methods of forming thermoplastic powders useful in additive manufacturing. [Background technology]
[0002] Methods that utilize powder for additive manufacturing include: Selective laser sintering (SLS) is a 3D printing technique that uses a laser to fuse powdered material in successive layers (see, for example, U.S. Patent No. 5,339,933). Rapid sintering (HSS) and multi-jet fusion (MJF) 3D printing utilize multiple jets that similarly deposit successive layers of infrared absorbing (IR absorbing) ink onto a powdered material, which is then exposed to IR energy for selective melting. Electrophotographic 3D printing utilizes a rotating photoconductor that builds an object layer by layer from a base.
[0003] Selective laser sintering (SLS), multi-jet fusion (MJF), and high speed sintering (HSS) 3D printing methods use the same type of floating, unfixed powder bed, where each successive layer of powder is metered and a dry flow of powder is required to ensure good part integrity. They generally have the same material requirements to be compatible with the printing process, since the additively built object experiences similar stresses, only with different heating mechanisms to obtain the molten phase. Typically, a free body diagram of the 3D printed object can be used to determine the residual stresses predicted in the printed object. This is necessary to successfully build the object. If the residual stresses are too high or the powder does not flow properly, the object will deform or have unacceptable defects.
[0004] Residual stresses have typically been minimized for these powder-bed based 3D printers by using crystalline or semi-crystalline thermoplastic polymers that have a sufficiently large window between their melting and recrystallization temperatures. Unfortunately, this is limited to polymers (e.g., polyamides) that have been successfully used to print large or complex parts using SLS and MJF methods, thus limiting the use of these additive manufacturing methods. Similarly, the use of semi-crystalline polymers upon recrystallization after heating to produce additively manufactured articles can limit the properties of the article.
[0005] There are several examples of induced crystallization of polymers such as polycarbonates, such as those described in US Pat. Nos. 5,993, 6,149, 6,153, 6,166, 6,171, 6,182, 6,193, 7,146, 7,157, 7,163, 7,178, 7,189, 7,196, 8,197, 9,103, 9,104, 9,111, 9,112, 9,113, 9,121, 9,136, 9,147, 9,155, 9,166, 9,177, 9,189, 9,194, 9,195, 9,189, 9,196, 9,197, 9,198, 9,199, 10,106, 10,117, 10,122, 10,131, 10,142, 10,152, 10,163, 10,174, 10,185, 10,19 ...
[0006] Generally, freeze-fracturing and classification of polymers are required to melt and fuse the powder to allow successive layers to adhere to achieve the required particle size. Freeze-fracturing is unfortunately a laborious process that consumes a lot of energy. Similarly, the fracturing process tends to result in powders with angular irregularities due to brittle fracture of the polymer mass and can also form excessively fine particles that must be heated and reprocessed. Due to the angularity of the particles and the presence of fine particles resulting from milling, the particle flow and distribution can cause defects in the manufactured article. As a result, flow aids have often been required to enable dry metering of powders with the required uniformity to achieve defect-free and non-deformed additive manufacturing parts. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] U.S. Pat. No. 5,597,589 [Patent Document 2] U.S. Pat. No. 3,214,407 [Patent Document 3] U.S. Pat. No. 4,853,462 [Patent Document 4] US Patent Application Publication No. 2021 / 0277180 [Patent Document 5] International Publication No. 2017 / 033146 Summary of the Invention [Problem to be solved by the invention]
[0008] It would therefore be desirable to provide a method that avoids one or more of the problems for producing polymeric powders useful for additive manufacturing, such as SLS, HSS, MJF, etc. For example, it would be desirable to provide a more efficient method for achieving useful additive manufacturing powders that do not require flow aids. [Means for solving the problem]
[0009] The applicant has discovered a more efficient method than previous methods for producing thermoplastic polymer powders useful for additive manufacturing, with control over particle size, particle size distribution and particle morphology. The method includes forming a polymer foam (porous polymeric body) with specific microstructural characteristics that allow efficient milling and the realization of useful powder particle size, particle size distribution and microstructure. It has been discovered that foams (porous thermoplastic polymeric bodies) with minimum strut or cell wall thicknesses larger than the smallest desired particle can be milled more efficiently with fewer undesirable small particles. The foams may be made at ambient or elevated temperatures, and the pores or cells of the foam desirably have an average size smaller than the average strut or cell wall size. Typically, the foams have a porosity of about 2% to 50% to achieve the desired properties and efficient milling to form polymer powders.
[0010] The thermoplastic polymer powder for additive manufacturing can be made by a process that includes cooling a foam comprised of a thermoplastic foam below the brittle temperature of the thermoplastic polymer, the foam having an average column size of 10 to 500 micrometers, and grinding the cooled foam to form a thermoplastic polymer powder.
[0011] Thermoplastic polymer powders formed by the methods described below can be sintered or fused by the application of directed heat or electromagnetic energy to produce laminated manufactured articles. [Brief description of the drawings]
[0012] [Figure 1] Optical micrograph at 300x of the surface of a foam useful in the method of the present invention [Diagram 2] 100x optical microscope image of the surface of a foam useful in the method of the present invention [Diagram 3] 200x optical microscope photograph of the surface of a foam useful in the method of the present invention [Figure 4] 200x optical microscope photograph of a cross section of a foam useful in the method of the present invention DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Although the present disclosure has been described with reference to particular embodiments, it should be understood that the disclosure is not limited to the disclosed embodiments, but rather is intended to cover various modifications and equivalent arrangements included within the scope of the appended claims, which scope is to be accorded the broadest interpretation so as to encompass all such modifications and equivalent structures as permitted under law.
[0014] Surprisingly, the method may be carried out at a temperature (i.e., cooling temperature) significantly above the brittle temperature. For example, the temperature may be any temperature below the glass transition temperature of the particular polymer, and desirably above the brittle temperature. The glass transition temperature (Tg) may be determined by any known method, such as methods known in the art, such as differential scanning calorimetry (DSC), dynamic mechanical measurement (DMA), and thermomechanical analysis (TMA). By way of illustration, Tg may be determined by DSC from the deviation of a heating curve (heating rate of 20° C. / min) from a straight line using ASTM D3418 or ISO 11357-2, where Tg is further defined as "the temperature at which the polymer breaks down into a desired shape." Measurement of Tg by DSC ", PETech-09, Thermal Analysis, PerkinElmer, Inc., 2000. On the other hand, when dense polymers are used, milling almost always requires temperatures very close to the brittle temperature (within about 5% of the brittle temperature given in Kelvin) or below. Improved shape may result from the use of milling at temperatures above the brittle temperature up to the Tg, and improved morphology may be achieved with cooling temperatures closer to the Tg, such as within 25%, 20%, or 10% of the Tg given in Kelvin. However, lower cooling temperatures closer to the brittle temperature (e.g., within 20% or 10% of the brittle temperature) may improve the efficiency of milling. This method usually involves cooling to a temperature below the glass transition temperature up to the brittle temperature of the thermoplastic polymer. The brittle temperature is determined according to ASTM D746 or ISO 974. The temperature may be below the brittle temperature. Cooling may be accomplished by any suitable method, such as those known in the art of freeze milling. Illustratively, cooling may be by freezing or exposure to dry ice or liquid nitrogen. The freeze milling temperature may be any suitable temperature depending on the particular thermoplastic polymer and its glass transition temperature and brittle temperature. Typical temperatures may be anywhere from 40°C or less, 20°C or less, 0°C or less, -25°C or less, -50°C or less, to about -75°C, -100°C, -150°C, or -190°C.
[0015] The thermoplastic polymer may be any thermoplastic polymer that can be used to produce additive manufacturing articles by floating bed 3D printing methods such as selective laser sintering (SLS), for example, as described in US 6,136,948 and WO 96 / 06881. The thermoplastic polymer may also be useful for producing articles by SIB processes (selective inhibition of bonding of powder), as described in WO 01 / 38061, 3D printing, as described in EP 0 431 924, or microwave processes, as described in US 10,479,733.
[0016] Illustrative thermoplastic polymers include, but are not limited to, polyamides, polyesters, polycarbonates, polyketones, polysulfones, polyarylates, polyimides, polyolefins, polystyrenes, polyesters, copolymers of the above, and blends of the above. Thermoplastic polymers may be linear or branched. Thermoplastic polymers may be aliphatic or aromatic. It may be desirable for at least a portion of a thermoplastic polymer to consist of repeating aromatic units within the polymer backbone. Illustratively, a thermoplastic polymer may be 5 mol%, 10 mol%, 25 mol% or 50 mol% aromatic (e.g., aromatic groups make up 50% or more of the molar mass of the polymer).
[0017] The thermoplastic polymer generally comprises a semi-crystalline polymer, which when heated and cooled at rates normally experienced in forming or compounding such polymers (e.g., heating and cooling rates from an ambient temperature of about 25° C. to the melting temperature), exhibits at least about 5% crystallinity to substantially complete crystallinity. That is, the polymer exhibits crystallinity without forced crystallization methods, such as those known in the art (e.g., solvent-induced crystallization). Generally, the amount of crystallinity is at least about 5%, 10%, 15%, or 20% to about 95%, 75%, 50%, or 30%. The crystallinity may be determined by any suitable method, such as those known in the art. By way of illustration, percent crystallinity can be determined by X-ray diffraction, including wide angle X-ray diffraction (WAXD), such as using a Rigaku SmartLab X-ray diffractometer, or by differential scanning calorimetry (DSC), such as using a TA Instruments DSC250 differential scanning calorimeter utilizing ASTM D3418-15, where a heating or cooling rate of 20° C. / min is used when determining crystallinity by differential scanning calorimetry (DSC), unless otherwise specified. m and T c (melting and crystallization temperatures) are determined from the melting / crystallization peaks of the DSC as described in ASTM D3418 using the midpoint of the peak. m and T c The onset of the peak is similarly determined by ASTM D3418 or ISO 111357-2 (ie, the deviation of the scan from a straight line).
[0018] Semi-crystalline as used herein includes amorphous thermoplastic polymers that have induced crystallinity that reverts to amorphous when heated above the melting temperature, such as those described in co-pending U.S. Provisional Patent Application No. 63 / 289,465, which is incorporated herein by reference.
[0019] Examples of useful polycarbonates include those described in U.S. Patent Application Publication No. 2021 / 0277192, paragraphs 49 to 56, which are incorporated herein by reference.
[0020] Examples of useful polysulfones include:
[0021] [ka]
[0022] where n is any integer value that results in a PAES having a weight average molecular weight (Mw) anywhere from 1, 10, or 20 to 1000, 500, or 200 kDa; m typically ranges from 0 to 10; and R 1 each occurrence of represents an aromatic or fused ring of about 5 to 10 carbon atoms, such as, but not limited to, 1,2-, 1,3-, or 1,4-phenylene, or diphenylene, such as, but not limited to, 4,4'-diphenylene; R 2 Each occurrence of is independently C1~C 20 Alkyl, C5-C 18 Or C5~C 12 It is an aromatic ring or a condensed ring consisting of 5 to 10 carbon atoms, or a combination thereof. Fragment structure-R 1 -S(=O)2-R 1 - may also represent any of the fused heterocyclic structures shown in formulas 2 and 3, 1 At least 60% of the total number of groups are aromatic or each R 2 At least one C 6~30 Fragment structure -R 1 -S(=O)2-R 1 may also represent any of the fused heterocyclic structures shown in formulas 2 and 3:
[0023] [ka]
[0024] or
[0025] [ka]
[0026] In an embodiment, R 1 and R 2 may be the residue of an aryl or diaryl compound:
[0027] [ka]
[0028] In another embodiment, the PAES of formula (1) has m having an integer value of zero or more (typically, from 1 to 10, 6, 5, 4, 3, or 2); and each R 2 is the residue of a dihydroxy compound, such as an aromatic dihydroxy compound:
[0029] [ka]
[0030] [ka]
[0031] In formulas (3), (4), and (5), each R 3 , R 4 , and R 5 are independently selected from, for example and without limitation, halogen atoms (e.g., chlorine or bromine), C 3~20 Alkoxy, C 1~20 Hydrocarbyl groups (e.g., C 1~20 Alkyl, halogen substituted C 1~10 Alkyl, C 6~10 Aryl or halogen substituted C 6~10aryl), p, q, and r are each independently integers from 0 to 4, such that when p, q, or r is less than 4, the valence of each unsubstituted carbon of the ring is filled with hydrogen, and X represents a bridging group connecting two phenolic groups, where the bridging group and the hydroxyl substituents of each C6 arylene group are arranged ortho, meta, or para (preferably para) to each other on the C6 arylene group, and the X group can be, for example, a single bond, -O-, -S-, -S(=O)-, -S(=O)2- (e.g., bisphenol-S), -C(=O)-, or cyclic or acyclic, aromatic or non-aromatic, and can further include heteroatoms such as halogens, oxygen, nitrogen, sulfur, silicon, or phosphorus; 1~20 It consists of an organic group.
[0032] Particular dihydroxy compounds include, but are not limited to, resorcinol, 2,2-bis(4-hydroxyphenyl)propane ("bisphenol A" or "BPA" where each of the aryl rings is para-substituted and X is isopropylidene in formula (3), 3,3-bis(4-hydroxyphenyl)-phthalimidine, 2-phenyl-3,3-bis(4-hydroxyphenyl)phthalimidine ("N-phenylphenolphthalein bisphenol", "PPPBP", or 3,3-bis(4-hydroxyphenyl)-2-phenylisoindolin-1-one), 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane, 1,1-bis(4-hydroxy-3-methylphenyl)-3,3,5-trimethylcyclohexane (also known as "isophorone bisphenol").
[0033] Examples of suitable polyarylethersulfones are:
[0034] [ka]
[0035] [ka]
[0036] [ka]
[0037] [ka]
[0038] Examples of useful PAES polymers include polyethersulfone (PSU, catalog number 25667-42, formula 7), poly(1,4-phenylene-ether-ether-sulfone) (PES or PEES, catalog number 28212-68-2, formula 8), polyphenylene sulfone (PPSU, catalog number 25839-81-0, formula 9), and poly(bisphenol-A sulfone) (PSF, catalog number 25135-51-7, formula 10), such as those commercially available under the tradename RADEL from Curbel Plastics Inc., Arlington, Texas, those commercially available under the tradename PARYLS from UJU New Materials, Ltd., and those commercially available under the tradename UDEL from Solvay Specialty Polymers USA, LLC, Alpharetta, Georgia.
[0039] The crystallizable polymer may be a polyketone, including polyketones having ether repeat units, such as polyetherketones, polyetheretherketones, polyetherketoneketones, etc. Exemplary polyketones without ether repeat units may be formed by the reaction of carbon monoxide with an alkene monomer in the presence of a Group 8 to Group 10 transition metal catalyst. In particular, the method may be any one of those described in U.S. Pat. Nos. 4,835,250, 4,894,435, and 5,138,032, and U.S. Patent Publication No. 2008 / 0058494, each of which is incorporated herein by reference in its entirety. In particular, the method, reaction conditions, and monomers are those described in U.S. Pat. No. 5,138,032, column 2, line 52 to column 5, line 17, which are specifically incorporated herein by reference. Such polyketones are typically TIFF0007579461000011.tif18114
[0040] The polyketones are preferably made of repeating units represented by the formula: where A is the residue of an alkene monomer converted to a saturated hydrocarbon group, m is about 1 to 6, and n is at least about 2 up to any practical amount to achieve the desired number average molecular weight (Mn) useful in the present invention. The alkene monomer preferably comprises an olefin having from 2 to 12, 8, or 6 carbons. Illustratively, the alkene monomer is ethylene, or the alkene monomer comprises ethylene and at least one other olefin monomer, such as propylene. When the polyketone is a copolymer of ethylene and another olefin monomer (e.g., propylene), the amount of ethylene and another olefin is as described in U.S. Pat. No. 5,138,032, column 2, line 17 to column 3, line 14. The polyketone preferably is a terpolymer of carbon monoxide, ethylene, and another alkene monomer (e.g., an olefin of from 3 to 12, 8, or 6 carbons, especially propylene). Such polyketones may comprise random repeating units: TIFF0007579461000012.tif19114
[0041] where G is a saturated residue of an olefin of 3 to 12, 8 or 6 carbons polymerized with a double bond, and x / y is at least 2 to 100 or 50 or 20. Desirably, G is propylene. The polyketone may be terminated with any useful group, such as an alkyl group, hydroxyl, ester, carboxylic acid, ether, or combinations thereof. Particular end groups may be generated by using solvents such as low molecular weight alcohols, such as methanol, or water, or combinations thereof. Examples of commercially available polyketones include those available under the trade name POKETONE™ from Hyosung, Korea.
[0042] In general, the polyketone may be a polyaryletherketone (PAES) such as those known in the art. Illustratively, the PAES may be a polyetherketoneketone (PEKK) such as those known in the art, in particular amorphous PEKK, as described in U.S. Pat. No. 10,364,349, column 2, lines 13 to 55, which are incorporated herein by reference. PEKK may be produced by known methods, such as those described in U.S. Pat. Nos. 3,065,205, 3,441,538, 3,442,857, 3,516,966, 4,704,448, 4,816,556, and 6,177,518.
[0043] The polyamide may be any known in the art and is typically semi-crystalline as described in U.S. Patent No. 5,391,640, incorporated herein by reference, column 4, line 7 to column 5, line 22. Specifically, the polyamide may be amorphous as described in U.S. Patent No. 5,391,640, incorporated herein by reference, column 5, line 23 to column 8, line 12. Examples of conventional polyamides include polypyrrolidone (nylon 4), polycaprolactam (nylon 6), polyheptanolactam (nylon 7), polycapryllactam (nylon 8), polynonanolactam (nylon 9), polyundecanolactam (nylon 11), polydodecanolactam (nylon 12), poly(tetramethylenediamine-co-oxalic acid) (nylon 4,2), poly(tetramethylenediamine-co-adipic acid) (nylon 4,6), poly(tetramethylenediamine-co-isophthalic acid) (nylon 4,1), polyhexamethylene azelaamide (nylon 6,9), polyhexamethylene sebacamide (nylon 6,10), polyhexa-5 methylene isophthalamide (nylon 6,IP), and polymetaxylylene adipamide (nylon MXD6). , polyamides of n-dodecanedioic acid and hexamethylene diamine (nylon 6,12), polyamides of dodecanedioic acid and n-dodecanedioic acid (nylon 12,12), and copolymers thereof, examples of which include hexamethylene adipamide-caprolactam (nylon 6,6 / 6), hexamethylene adipamide / -hexamethylene-isophthalamide (nylon 6,6 / 6IP), hexamethylene adipamide / hexamethylene terephthalamide (nylon 6,6 / 6T), trimethylene adipamide-hexamethyl-15-ene-azelaicamide (nylon trimethyl 6,2 / 6,2), and hexamethylene adipamide-hexamethylene azelaicamide caprolactam (nylon 6,6 / 6,9 / 6), as well as those not specifically mentioned herein.
[0044] The polyimide may be any of those known in the art, and is preferably a known aromatic polyimide. Illustrative aromatic polyimides which may be suitable are described in U.S. Patent Nos. 3,179,631, 3,249,588, and 4,755,555, each of which is incorporated herein by reference.
[0045] The thermoplastic foam has an average strut or cell wall thickness ranging from 10 to 500 micrometers. The average strut or cell wall thickness may be determined using a photomicrograph of a cross-section of the foam using any suitable technique, such as optical or scanning electron microscopy of cut or fractured cross-sections, optionally filled with resin. The average strut or cell wall thickness is measured at about 2 mm of the cross-section of the foam. 2 The wall thickness may be determined by measuring the wall thickness of at least about 25 randomly selected walls in one or more photomicrographs of 100 times the area of the wall. Desirably, the average strut dimension is at least 20, 30 or 50 micrometers to 400, 300 or 250 micrometers.
[0046] It is desirable for the strut or cell wall thickness to have a distribution that achieves the desired flow without the use of flow aids, as described below. In general, it is desirable for the D10 strut size to be at least 1, 5 or 10 micrometers. The D10 strut size is such that at least 90% of the struts have a size greater than the D10 strut size as determined herein. Similarly, it is desirable for the D90 strut size to be up to about 1 mm, 750 micrometers or 500 micrometers.
[0047] It is desirable for the foam to achieve the desired strut dimensions while also having low porosity. This is believed to increase the efficiency of the crushing of the thermoplastic polymer to form a thermoplastic polymer powder useful for additive manufacturing, without limitation. Illustratively, the porosity may be at least 2%, 5%, 10% and up to 70%, 60% or 50%. The porosity may be determined by any suitable method, such as those known in the art, such as mercury, helium pycnometry or Archimedes method (for low porosity, method A of ISO 18754:2020), or by determining the mass and volume of the foam, which may be facilitated by coating the irregular foam to seal the open pores and determine the volume by liquid displacement. The porosity of the foam may be open or closed, but is desirably comprised of open porosity. Illustratively, at least 5%, 10%, 25%, 50%, 75%, 90% or substantially all of the porosity is open porosity.
[0048] The size of the pore cells may be any size so long as the strut dimensions are as described herein. However, it may be desirable for the cell pore size to be smaller than the strut dimensions. For example, the average cell size may be 10%, 20% or 50% smaller than the average strut dimensions. Pore size may be determined photomicrographically in a manner similar to that for determining strut dimensions, or using a mercury intrusion pycnometer.
[0049] The cross-sectional shape of the foam formed may be any that is useful and is not limited. For example, the foam may be globules, symmetric or asymmetric beads, fibers (monofilaments), pellets, platelets, cut sheets, cut rods, and tubes of any cross-sectional shape, etc. The foam may be of any size suitable for grinding. The size of the foam may be any suitable for grinding into the desired thermoplastic polymer powder. Illustratively, the foam has an average particle size of 0.5 mm to 50 mm equivalent spherical diameter. The foam may be initially larger and may be reduced in size before grinding by known methods, such as cutting the extruded foam with known cutters, such as wire cutters or wire saws. The foam may be spherical, symmetric or asymmetric, such as any one of the shapes described above. Typically, the foam to be ground has an equivalent spherical diameter of about 0.5 mm to 50, 25, or 10 mm. The foam before grinding may have an aspect ratio of 1 or more, 1.5, 2 to 50, 75, or 100. Aspect ratio may be measured from micrographs of the longest and shortest axes of randomly selected foam particles (approximately 100) using commercially available digital vision software or manually by known methods.
[0050] Thermoplastic polymer foams may be produced by any suitable method, such as those known in the art. The method may be either using a blowing agent or using mechanically induced foaming. The foaming is preferably achieved by fusion of polymer particles, such as when polymerized to form a polymer, precipitated from a solvent, or during introduction of a solution and precipitation in any suitable manner, such as those known in the art. These foams (porous bodies) have been found to be particularly suitable for the method of the present invention and provide the desired characteristics of dry particle flow without the use of flow aids. That is, the powder without the addition of any flow aid may have a flow rate (flow rate) of at least about 0.5 g / s, 1 g / s, or 2 g / s, as determined by ASTM D1895, Method A, to any practically achievable rate (e.g., 50 g / s) using a 15 mm nozzle.
[0051] A foam or porous body having the required properties may be demonstrated by polymerization of a polymer that precipitates from a reaction medium such as that described in U.S. Pat. No. 5,138,032, column 2, line 17 to column 3, line 14, herein incorporated by reference.
[0052] The foam may be formed by dissolving a thermoplastic polymer in a solvent and precipitating it from the solution while providing sufficient agitation or introducing a blowing agent (e.g., a chemical or physical blowing agent). Air or any gaseous component of air may be used.
[0053] Illustratively, foams may be made by dissolving a thermoplastic polymer in a solvent with heat. Typically, heating is above 50° C. and below the onset melting temperature of the thermoplastic polymer to form a solution of the melted thermoplastic polymer. Typically, the solvent is heated from above 100° C. to below the onset melting temperature of the particular thermoplastic polymer (determined by differential scanning calorimetry (DSC) as described herein). Illustratively, the solvent is heated to above 75° C. or 100° C. and 5%, 10%, or 20% below the onset melting temperature of the thermoplastic polymer, examples of which are up to about 200° C., 180° C., 170° C., or 160° C.
[0054] The time at the maximum heating temperature (melting temperature) is any time that achieves the desired dissolution of the thermoplastic polymer (typically 3 or 4 minutes to 3 or 4 hours). Multiple elevated temperatures may be used (held at) during this process. For example, a higher temperature (melting temperature) may be used to melt the thermoplastic polymer, and a lower temperature (precipitation temperature) may be used when precipitating the thermoplastic polymer. The precipitation temperature is the temperature at which the thermoplastic polymer begins to precipitate when cooled or at which precipitation is induced by the addition of a non-solvent. The precipitation temperature may be any useful temperature from ambient temperature or above, about 20°C, up to the melting temperature (if precipitated by the addition of a non-solvent) to a temperature below the melting temperature (e.g., 130°C, 125°C, 100°C, 75°C, or 50°C). It is desirable for the precipitation temperature to be lower than the temperature at which the non-solvent begins to boil (the boiling onset temperature as determined by DSC in the same manner in which the melting peak is determined). Agitation may be used during any part or the entire process, with shear varied depending on the desired foam properties at different stages of the process.
[0055] Agitation is generally understood to mean the stirring of ingredients in a liquid or suspension mixture under conditions that generate shear forces to create flow and turbulence patterns, typically using an impeller rotating within a stator. The agitation may be any useful to achieve a shear rate at which a foam or porous body is formed. Once the impeller has drawn the mixture in, it is subjected to a sudden change in direction and acceleration such that the mixture is either centrifugal contacted with the walls of the stator or forced through the pores of the stator under pressure and velocity with the final change in direction and acceleration (which may induce foaming and air entrapment).
[0056] Any suitable agitation method may be used to achieve the desired shear, such as those known in the art, including, for example, the use of impellers, magnetic stirring devices, homogenizers, colloid mills, ultrasonic agitation, cavitation, etc. Examples of useful agitation may be achieved with any commercially available mixer.
[0057] It is desirable that the atmosphere be one in which the solvent and other chemicals do not adversely react with it. Typically, dissolution is performed in a closed vessel at or near ambient pressure (e.g., ±10%, ±1%, or ±0.1% of atmospheric pressure) to minimize volatilization losses. High pressure may be used and may be desirable or necessary depending on the particular solvent used (e.g., using supercritical carbon dioxide). Exemplary atmospheres would include nitrogen or a noble gas (e.g., argon) or combinations thereof or air (e.g., dry air and any components in air, either individually or in combination), depending on the solvent.
[0058] The amount of thermoplastic polymer that is soluble in the solvent may be any useful amount that may then precipitate from solution upon cooling, introduction of a non-solvent, or a combination thereof. Illustratively, the amount of soluble thermoplastic polymer may be from 1%, 5%, 10% by weight, to any practical amount (without gelling), 50%, 40%, 30% or 25% by weight.
[0059] The solvent may be any useful solvent for dissolving the thermoplastic polymer, such as a polar aprotic solvent. Typically, the solvent has a volatility or low viscosity that allows for easy removal in subsequent processing steps, such as separating the precipitated thermoplastic polymer from the solvent. Typically, the solvent has a viscosity within an order of magnitude of that of water at ambient conditions (e.g., about 1 centipoise at about 20°C to 25°C and 1 atmosphere (about 101 kPa)) or a similar viscosity at the temperature and pressure of dilution (e.g., supercritical fluid). That is, the viscosity is typically less than 10 centipoise to 0.1 centipoise (cp) at the dissolution temperature. Similarly, the volatility measured at the boiling point (or boiling range) at 1 atmosphere (about 101 kPa) is typically from about 30°C, 50°C, or 75°C to 150°C, 200°C, or 250°C. The solvent typically has a molecular weight (weight average Mw) of up to about 500 g / mol, 200 g / mol, or even 150 g / mol, to at least about 30 g / mol. In some cases, the solvent may be a solid at ambient conditions, but is understood to have a useful viscosity (e.g., less than about 100 cp or less than 10 cp) at the boiling point and elevated temperatures at which dissolution occurs, as described above. Similarly, the solvent may be gaseous at ambient conditions and liquid at the dissolution temperature and pressure.
[0060] The solvent may be a mixture of solvents. Illustratively, the solvent may be a mixture of a solvent that is liquid at room temperature and another solvent that is solid at room temperature that dissolves in the liquid solvent, the dissolved solvent imparting one or more desired properties (e.g., improved solubility of a thermoplastic polymer or the formation of particles when a non-solvent is used to precipitate a polymer from solution).
[0061] Exemplary solvents include those described in paragraphs 26 to 34 of co-pending U.S. patent application entitled "Polyketone Powder for Laser Sintering" by T. Fry and J. Eue et al., filed on the same day as the present application, which is hereby incorporated by reference. The method may be carried out in a supercritical fluid such as carbon dioxide as described in co-pending U.S. Provisional Patent Application No. 63 / 289465, at a temperature, concentration and pressure to dissolve in the carbon dioxide or other solvents described above, and precipitation occurs by adding a non-solvent to the carbon dioxide or other solvent. Agitation may be varied during precipitation to promote particle formation and clustering in the desired foam. For example, shear may be high during the initial injection of non-solvent during nucleation of the precipitated particles, then lowered to promote clustering of the initial precipitated particles, and then increased again to achieve the desired foam porosity and structure.
[0062] The non-solvent used to induce precipitation at the precipitation temperature may be any suitable one based on the solvent and thermoplastic polymer used. Illustratively, the solvent may be NMP, DMPU, PGMEA or HMPA, and the non-solvent may be a protic solvent such as water, low molecular weight alcohols (e.g., C1 to C4 alcohols) or mixtures thereof when precipitating an aliphatic polyketone. The amount of non-solvent may be any amount necessary to cause precipitation at a given precipitation temperature, and the amount is any amount useful to achieve the desired precipitated thermoplastic polymer particle size, particle size distribution and morphology. Typically, the concentration of non-solvent added may be from 0.1%, 1%, 5% or 10% by volume of the solvent and non-solvent, typically 75%, 50% or 25% by volume.
[0063] The foam may be made by a phase inversion process to form a foam / porous body. Typically, the phase inversion method includes dissolving a thermoplastic polymer in a solvent to form a dope, contacting the dope with an anti-solvent in an amount sufficient to invert the solvent and anti-solvent, and removing the anti-solvent to form a foam. The dope may have the properties of a paste that allows for the continued formation of a foam, for example, by forming an extrudate of the dope and passing it through a non-solvent, such as those common in forming gas separation membranes, as described for making polyimide membranes (e.g., U.S. Patent Application Publication No. 2015 / 0011815). Phase inversion may be performed using liquid or supercritical carbon dioxide, as described in Tissue Engineering, Part B, Vol. 19, November 3, 2013.
[0064] The foam may be produced by extrusion of a polymer having a chemical or physical blowing agent therein that produces foam as it exits the die. The volatile liquid or gas may be carbon dioxide. Exemplary methods are described in U.S. Pat. Nos. 4,824,720, 6,284,810, and U.S. Patent Application Publication Nos. 2017 / 0282430 and 2005 / 0276967, each of which is incorporated herein by reference. In some cases, it has been found that the thermoplastic polymer powder has a morphology that improves flow without the use of flow aids. It is desirable for the polyketone to have sufficient sphericity to achieve the necessary unassisted flow. With regard to particle shape, particularly particle roundness, which aids flow and is derived from microscopic images of individual particles, the circularity feature, or circularity, may be expressed, where the circularity of an individual particle is determined by the following formula: 4πA / P 2where A is the area of the particle and P is the perimeter of the particle, both viewed from a random perspective. A related parameter, sphericity, is derived as the square root of the circularity. Circularity is a number greater than zero and less than or equal to 1. A perfectly circular particle is said to have a circularity of 1.00. Tables of population circularity data are presented in such a way that various levels of circularity (e.g., 0.65, 0.75, 0.85, 0.90, and 0.95) are accompanied by the percentage of the particle sample population that has a circularity greater than the tabulated value. Circularity is determined at a solidity filter level of 0.9 or 0.95. Solidity filters are filters used to remove overlapping particles in two-dimensional micrographs that are available in commercially available image analysis software. Solidity is essentially the area of the particle (particle area) that lies on the area of the region defined by the major and minor axes of the particle area in a two-dimensional micrograph. The size and shape of the particles can be measured by any suitable method known in the art for measuring particle size by diameter. In some embodiments, the size and shape of the particles are determined by laser diffraction as known in the art. For example, the particle size can be determined using a laser diffractometer such as a Microtrac S3500 equipped with a static image analysis accessory using PartAnSI software to analyze captured images of the particles. It is desirable that at least about 65%, 70%, 80%, 95% or 99% (by number) of the particles have a circularity of at least about 0.8, 0.85, 0.9 or 0.95 for the powder separated from the reactor and classified without further processing other than purification.
[0065] Similarly, the methods allow for the formation of useful powders without further classification or separation of undesirably small or large particles. By way of illustration, thermoplastic polymer powders generally have particle sizes and size distributions that are useful for producing additive manufacturing articles, typically having a mean or median particle size (D) of about 1 micrometer (μm), 10 μm, 20 μm, 30 μm, or 40 μm, to 150 μm, 125 μm, 110 μm, or 100 μm, by volume. 50Similarly, to allow for consistent heating and dissolution of the powder, the powder should have a D of up to 300 μm, 200 μm or 150 μm. 90 To aid in flowability, the thermoplastic polymer powder preferably has a D by volume of at least 0.1 μm, 0.5 μm or 1 μm. 10 It is desirable to have D 90 means the particle size (equivalent spherical diameter) in the particle size distribution in which 90% by volume of the particles are equal to or smaller than that size, and similarly, D 50 means the particle size (equivalent spherical diameter) in a particle size distribution below which at least 50% by volume of the particles are smaller, and D 10 means the particle size (equivalent spherical diameter) in a particle size distribution below which at least 10% by volume of the particles are. Particle size may be determined by any suitable method, such as those known in the art, including, for example, laser diffraction of a sufficient number of particles (about 100 to about 200 particles) or image analysis of photomicrographs. Exemplary laser diffractometers are those manufactured by Microtrac, such as the Microtrac S3500. EXAMPLES
[0066] Example 1: The polyketone powder is produced in the manner described in U.S. Patent No. 5,138,032, column 2, line 52 to column 5, line 17. The flakes have a theoretical density of about 90 to 99%. The polyketone has a glass transition temperature of about 27°C.
[0067] The thermoplastic foam is milled using a counter rotating pin mill operating at 75% of its maximum capacity. The foam is milled at 1700m 3The foam is gravity fed to the mill with a slight vacuum at the central discharge into the air classifier with an air flow rate of 1 / hr and a classification speed of 1100 rpm. The foam and equipment are cooled to -35°C and maintained at that temperature for the duration of the foam being milled. The average feed rate is 97.5 kg / hr. The average product output is 77 kg / hr with oversize recycled back to the mill. The product is 98.5% by weight particles less than 106 microns. The effective product throughput based on the upper limit of the less than 106 microns size is 75.89 kg / hr.
[0068] Comparative Example 1: Polyketone extrusion pellets produced in the same manner as described in Example 1 are ground in the same manner, with the following exceptions: The feed pellets are substantially dense, generally pellets about 2 mm in diameter and 2 mm in length. The pellets are cooled to -40°C. The feed rate is 28.5 kg / hr. The feed is reduced due to the large amount of oversized material produced being recycled. The average throughput is 22 kg / hr. The mass of the product is about 34.8% by mass below 106 micrometers. The effective product throughput based on the particle size of the product below 106 micrometers is 7.6 kg / hr. From this, it is easy to see that even at the lower feed rate, the powder produced is not as effectively milled to the desired size. That is, using the thermoplastic polymer foam of the present invention is more than 10 times more efficient in achieving the desired thermoplastic polymer powder useful for layered manufacturing.
[0069] Example 2: Polyetherketoneketone (PEKK) powder is milled in a counter rotating pin mill as in Example 1, but at temperatures ranging from 0°C to within 20% of the brittle temperature of PEKK. The foam is shown in Figures 1-4. Typical size of the foam is irregular flakes with thickness of about 100 micrometers to 3 mm. The average strut size is about 82 micrometers. It is readily apparent from the figures that there is significant porosity of at least 10% (i.e., less than about 90% theoretical density). The foam is milled in a manner similar to Example 1 with rapid milling, desired particle size, and high efficiency without significantly oversized material. Polyetherketoneketone has a Tg of about 160°C, a melting temperature of about 305°C, and a T:l ratio of about 60:40. Preferred embodiments of the present invention will be described below in detail. EMBODIMENT 1 (i) cooling a foam comprised of a thermoplastic polymer having a glass transition temperature to a cooling temperature below the glass transition temperature to form a cooled foam, the foam having an average column dimension of 10 to 500 micrometers; and (ii) pulverizing the cooled foam to form a thermoplastic polymer powder; The method comprising: EMBODIMENT 2 2. The method of claim 1, wherein the foam has a porosity of 10% to 50%. EMBODIMENT 3 3. The method of embodiment 2, wherein the foam has a porosity of up to 40%. EMBODIMENT 4 The method of any one of the preceding claims, wherein the average pillar size is between 20 and 300 micrometers. EMBODIMENT 5 4. The method of embodiment 3, wherein the average strut size is 25 to 250 micrometers. EMBODIMENT 6 The foam has a D 10 5. The method of any one of claims 1 to 4, having strut dimensions. EMBODIMENT 7 The foam has a D of up to 500 micrometers. 90 7. The method of any one of claims 1 to 6, having strut dimensions. EMBODIMENT 8 8. The method of any one of the preceding claims, wherein the foam has an average cell size less than the average strut size. EMBODIMENT 9 9. The method of embodiment 8, wherein the average cell dimension is at least 10% smaller than the average strut dimension. EMBODIMENT 10 The thermoplastic polymer powder has (i) a D 90 (ii) a particle size D of at least 10 μm10 and (iii) having an average particle size of about 20 μm to about 150 μm. EMBODIMENT 11 11. The method of embodiment 10, wherein at least 80% by number of the thermoplastic polymeric powders have a circularity of at least about 0.8. EMBODIMENT 12 12. The method of any one of the preceding claims, wherein the thermoplastic polymer powder has a flow rate of at least 0.5 g / sec using a 15 mm nozzle according to ASTM-D, Method A. EMBODIMENT 13 13. The method of embodiment 12, wherein the flow rate is at least 1 g / sec. EMBODIMENT 14 14. The method of any one of the preceding claims, wherein the foam has an average size of equivalent spherical diameter of 0.5 mm to 50 mm. EMBODIMENT 15 15. The method of embodiment 14, wherein the foam has an aspect ratio of at least 1.5 to 50. EMBODIMENT 16 16. The method of embodiment 15, wherein the foam comprises one or more of platelets, tubes, and fibers. EMBODIMENT 17 The foam is (i) incorporating a blowing agent into a thermoplastic polymer at a temperature and pressure such that the thermoplastic polymer melts; and (ii) reducing the pressure sufficiently so that the blowing agent becomes gaseous and forms a thermoplastic foam; 17. The method of any one of the preceding claims, wherein the polymer is formed by a process comprising: EMBODIMENT 18 8. The method of any one of claims 1 to 7, wherein the foam is formed by a process comprising dissolving the thermoplastic polymer in a solvent to form a dope, contacting the dope with an anti-solvent in an amount sufficient to cause phase inversion of the solvent and anti-solvent, and removing the anti-solvent to form the foam. EMBODIMENT 19 18. The method of embodiment 17, wherein the blowing agent comprises one or more of a chemical blowing agent and a physical blowing agent. EMBODIMENT 20 20. The method of embodiment 19, wherein the blowing agent comprises supercritical carbon dioxide. EMBODIMENT 21 21. The method of any one of the preceding claims, wherein the thermoplastic polymer is a semi-crystalline thermoplastic polymer. EMBODIMENT 22 22. The method of any one of the preceding claims, wherein the thermoplastic polymer has a brittle temperature, and the cooling temperature is below the glass transition temperature and above the brittle temperature of the thermoplastic polymer. EMBODIMENT 23 23. The method of embodiment 22, wherein the cooling temperature is within 20% of the glass transition temperature. EMBODIMENT 24 23. The method of claim 22, wherein the cooling temperature is within 20% of the brittle temperature. EMBODIMENT 25 The foam is (i) dissolving the thermoplastic polymer in a solvent to form a solution; (ii) precipitating the thermoplastic polymer by adding a non-solvent to form precipitated thermoplastic polymer particles; (iii) coalescing the precipitated thermoplastic polymer particles to form a particulate foam slurry; and (iv) removing the solvent and the non-solvent to form the foam; 25. The method of any one of the preceding claims, wherein the polymer is formed by a process comprising: EMBODIMENT 26 26. The method of embodiment 25, wherein the solution and the slurry are agitated during the precipitating and combining steps. EMBODIMENT 27 27. The method of embodiment 26, wherein a gas is introduced into one or more of the solution and the particulate foam slurry.
Claims
1. (i) cooling a foam comprised of a thermoplastic polymer having a glass transition temperature to a cooling temperature below the glass transition temperature to form a cooled foam, the foam having an average strut dimension of 10 to 500 micrometers and an average cell dimension less than the average strut dimension; and (ii) pulverizing the cooled foam to form a thermoplastic polymer powder; The method comprising:
2. The method of claim 1 , wherein the foam has a porosity of from 2% to 50%.
3. The method of claim 1 , wherein the average pillar size is from 20 to 300 micrometers.
4. The foam has a D of at least 10 micrometers. 10 The method of claim 1 , further comprising strut dimensions.
5. The foam has a D of up to 500 micrometers. 90 The method of claim 4 , further comprising strut dimensions.
6. The method of claim 1 , wherein said average cell size is at least 10% smaller than said average strut size.
7. The method of claim 6 , wherein said average cell size is at least 20% smaller than said average strut size.
8. (i) cooling a foam comprised of a thermoplastic polymer having a glass transition temperature to a cooling temperature below the glass transition temperature to form a cooled foam, the foam having an average column dimension of 10 to 500 micrometers; and (ii) pulverizing the cooled foam to form a thermoplastic polymer powder, the thermoplastic polymer powder having (i) a D 90 (ii) a particle size of at least 10 μm, 10 and (iii) having an average particle size of 20 μm to 150 μm, at least 80% by number of said thermoplastic polymer powder having a circularity of at least 0.8; The method comprising:
9. The method of claim 1 , wherein the foam has an average equivalent spherical diameter size of 0.5 mm to 50 mm.
10. (i) cooling a foam comprised of a thermoplastic polymer having a glass transition temperature to a cooling temperature below the glass transition temperature to form a cooled foam, the foam having an average column dimension of 10 to 500 micrometers; and (ii) pulverizing the cooled foam to form a thermoplastic polymer powder; In a method comprising: The foam is A first method comprising incorporating a blowing agent into a thermoplastic polymer at a temperature and pressure at which the thermoplastic polymer melts, and reducing the pressure sufficiently to cause the blowing agent to become gaseous and form a thermoplastic foam; a second method comprising dissolving the thermoplastic polymer in a solvent to form a dope, contacting the dope with an anti-solvent in an amount sufficient to cause phase inversion of the solvent and the anti-solvent, and removing the anti-solvent to form the foam; and a third method comprising dissolving the thermoplastic polymer in a solvent to form a solution, precipitating the thermoplastic polymer by adding a non-solvent to form precipitated thermoplastic polymer particles, coalescing the precipitated thermoplastic polymer particles to form a particulate foam slurry, and removing the solvent and the non-solvent to form the foam; The method is formed by a process including one of:
11. The method of claim 10 , wherein the foam is formed by polymerizing the thermoplastic polymer and precipitating it from a reaction medium.
12. The method of claim 11 , wherein the blowing agent comprises one or more of a chemical blowing agent and a physical blowing agent.
13. (i) cooling a foam comprised of a thermoplastic polymer having a glass transition temperature to a cooling temperature below the glass transition temperature to form a cooled foam, the foam having an average column size of 10 to 500 micrometers, the thermoplastic polymer having a brittle temperature, the cooling temperature being below the glass transition temperature and above the brittle temperature of the thermoplastic polymer; and (ii) pulverizing the cooled foam to form a thermoplastic polymer powder; The method comprising:
14. The method of claim 13, wherein the cooling temperature is within 20% of the embrittlement temperature.
15. The method of claim 13, wherein the cooling temperature is within 20% of the glass transition temperature.
Citation Information
Patent Citations
Absorbent extruded thermoplastic foam
JP2002511031A
Cellulose structures and viscoelastic polyurethane foam
JP2011528726A
Resin powder granule for 3D printer by powder bed melt bonding method and manufacturing method thereof, and manufacturing method of three-dimensional molded product using resin powder granule
JP2021053887A
Porous materials, methods of making and uses
US20120077010A1
Polymer Powder and Method of Using the Same
US20180200922A1