Evaporation mask, method of manufacturing an evaporation mask, method of manufacturing an organic semiconductor element, method of manufacturing an organic EL display device, and evaporation method

The method of manufacturing a vapor deposition mask using a resin layer and reinforcing film on a support without a metal layer addresses the challenge of forming high-definition through-holes, ensuring precise and wrinkle-free patterns.

JP7579510B2Active Publication Date: 2024-11-08DAI NIPPON PRINTING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020066799
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-02
Publication Date
2024-11-08
Estimated Expiration
2040-04-02

AI Technical Summary

Technical Problem

Current metal processing technology struggles to accurately form high-definition through-holes in large metal plates used for vapor deposition masks, leading to issues like wrinkles in resin layers when forming finer through-holes in laminated mask sheets.

Method used

A method for manufacturing a vapor deposition mask involves forming a resin layer on a substrate, attaching a reinforcing film, removing the substrate, and fixing the resin layer to a support, using a self-supporting thin film configuration without a metal layer to suppress wrinkles, and forming openings with precise control.

Benefits of technology

This approach enables the formation of fine vapor deposition patterns while preventing wrinkles in the resin layer, allowing for high-definition patterns and improved handling properties during the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579510000001
    Figure 0007579510000001
  • Figure 0007579510000002
    Figure 0007579510000002
  • Figure 0007579510000003
    Figure 0007579510000003
Patent Text Reader

Abstract

To provide techniques that make it possible to form a fine vapor deposition pattern, for example, a vapor deposition mask capable of suppressing a resin layer from wrinkling, a method of manufacturing the vapor deposition mask, a method of manufacturing an organic EL display device, and a vapor deposition method.SOLUTION: There is provided a method of manufacturing a vapor deposition mask that comprises the processes of: preparing a substrate; forming a resin layer on the substrate; removing the substrate from the resin layer; fixing the resin layer to a support body 40; and forming a plurality of opening parts 31, corresponding to a pattern to be manufactured by vapor deposition, in the resin layer, wherein the support body 40 is provided on one surface (Z-directionally minus-side surface) of a resin mask 30 and also joined to the resin mask 30 with an adhesion layer 35, and the resin mask 30 located inside the support body 40 is a membrane (independent thin film) which is not supported by a metal layer etc., but independent. Further, there are provided a method of manufacturing an organic EL display device and a vapor deposition method that uses the vapor deposition mask.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present embodiment relates to a deposition mask, a method for manufacturing a deposition mask, a method for manufacturing an organic semiconductor element, a method for manufacturing an organic EL display device, and a deposition method. [Background technology]

[0002] As products using organic EL elements or substrate sizes become larger, there is an increasing demand for larger deposition masks. Metal plates used to manufacture deposition masks made of metal are also becoming larger. However, with current metal processing technology, it is difficult to form through holes in large metal plates with high accuracy, and it is not possible to meet the demand for high-definition through holes.

[0003] Under these circumstances, Patent Document 1 proposes a mask sheet comprising a film layer having a plurality of opening patterns and a metal layer having a plurality of through holes each containing at least one of the opening patterns. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-179591 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, there has been a demand for forming finer through-holes in deposition masks. In order to form finer through-holes, it is necessary to make the resin layer in which the through-holes are formed thinner. However, when the resin layer such as polyimide is thinned in a mask sheet in which a resin layer and a metal layer are laminated, there is a problem that wrinkles are easily generated in the resin layer, especially at the boundary between the resin layer and the metal layer.

[0006] The present disclosure provides a technique that enables the formation of a fine deposition pattern, and provides, for example, a deposition mask that can suppress the occurrence of wrinkles in a resin layer, a manufacturing method for a deposition mask, a manufacturing method for an organic EL display device, and a deposition method. [Means for solving the problem]

[0007] The method for manufacturing a deposition mask according to the present embodiment includes the steps of preparing a substrate, forming a resin layer on the substrate, removing the substrate from the resin layer, fixing the resin layer to a support, and forming a plurality of openings in the resin layer corresponding to a pattern to be prepared by deposition.

[0008] The method for manufacturing a deposition mask according to the present embodiment may further include removing a portion of the resin layer that is positioned more outer than the support.

[0009] In the method for manufacturing a deposition mask according to this embodiment, the method may further include a step of attaching a reinforcing film onto the resin layer, and in the step of removing the substrate, the substrate may be removed from the resin layer to which the reinforcing film is attached.

[0010] In the method for manufacturing a deposition mask according to the present embodiment, the reinforcing film may include an outer periphery portion in a region that is gripped when the resin layer is fixed to the support.

[0011] In the method for manufacturing a deposition mask according to the present embodiment, the reinforcing film may include a central portion located more inward than the outer circumferential portion, and the central portion and the outer circumferential portion may be spaced apart from each other.

[0012] In the method for manufacturing a deposition mask according to the present embodiment, an inwardly facing portion of the outer circumferential portion may be formed in a comb-teeth shape in a plan view.

[0013] In the method for manufacturing a deposition mask according to the present embodiment, the resin layer may have a thickness of 1 μm or more and 5 μm or less.

[0014] The deposition mask according to the present embodiment includes a resin mask provided with a plurality of openings corresponding to a pattern to be formed by deposition, and a support joined to the resin mask.

[0015] In the deposition mask according to the present embodiment, the support may be joined to the resin mask without a metal material therebetween.

[0016] In the deposition mask according to this embodiment, the resin mask has an effective area in which a plurality of the openings are arranged in a regular array, and a surrounding area surrounding the effective area, and only the resin mask may be present within the effective area.

[0017] In the deposition mask according to the present embodiment, the support may be frame-shaped, the multiple openings of the resin mask may be located inside the support in a planar view, and the resin mask inside the support may be a free-standing thin film.

[0018] The manufacturing method of an organic EL display device according to the present embodiment is a manufacturing method of an organic EL display device, and includes a step of forming a deposition pattern on a deposition target using the deposition mask according to the present embodiment.

[0019] The deposition method according to the present embodiment includes the steps of preparing a deposition mask according to the present embodiment, preparing a deposition object, placing the deposition object on the deposition mask, and depositing a deposition material onto the deposition object placed on the deposition mask.

[0020] The manufacturing method for an organic EL display device according to the present embodiment includes a step of forming a deposition pattern on a deposition target using the deposition mask manufactured by the deposition mask manufacturing method according to the present embodiment.

[0021] The deposition method according to the present embodiment includes the steps of preparing a deposition mask manufactured by the deposition mask manufacturing method according to the present embodiment, preparing a deposition object, placing the deposition object on the deposition mask, and depositing a deposition material on the deposition object placed on the deposition mask.

[0022] The method for manufacturing an organic semiconductor device according to the present embodiment includes a step of forming a deposition pattern on a deposition target using the deposition mask according to the present embodiment.

[0023] The manufacturing method of an organic semiconductor element according to the present embodiment includes a step of forming a deposition pattern on a deposition target using the deposition mask manufactured by the manufacturing method of a deposition mask according to the present embodiment.

[0024] The method for manufacturing a deposition mask according to this embodiment includes the steps of preparing a resin layer having a reinforcing film disposed thereon, fixing the resin layer having the reinforcing film disposed thereon to a support, and producing a resin mask by forming a plurality of openings in the resin layer corresponding to a pattern to be produced by deposition.

[0025] In the method for manufacturing a deposition mask according to this embodiment, the resin mask has an effective area in which a plurality of the openings are arranged in a regular array, and a surrounding area surrounding the effective area, and only the resin mask may be present within the effective area.

[0026] In the method for manufacturing a deposition mask according to this embodiment, the support may be frame-shaped, the multiple openings of the resin mask may be located inside the support in a planar view, and the resin mask inside the support may be a free-standing thin film. Effect of the Invention

[0027] According to this embodiment, it is possible to suppress the occurrence of wrinkles in the resin layer. [Brief description of the drawings]

[0028] [Figure 1] FIG. 1 is a plan view showing a deposition mask according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view (cross-sectional view taken along line II-II in FIG. 1) showing the deposition mask according to the embodiment. [Diagram 3] 3(a) and (b) are cross-sectional views showing a part of a method for manufacturing a deposition mask according to one embodiment. [Figure 4] 4(a) and 4(b) are a cross-sectional view and a plan view showing a part of a method for manufacturing a deposition mask according to one embodiment. [Diagram 5] 5(a) and (b) are plan views showing modified examples of the reinforcing film. [Figure 6] 6(a) and (b) are cross-sectional views showing a part of a method for manufacturing a deposition mask according to one embodiment. [Figure 7] 7(a) and (b) are a cross-sectional view and a plan view showing a part of a method for manufacturing a deposition mask according to one embodiment. [Figure 8] 8(a) and (b) are cross-sectional views showing a part of a method for manufacturing a deposition mask according to one embodiment. [Figure 9] 9(a) to 9(c) are cross-sectional views showing the positional relationship between the resin layer and the adhesive layer. [Figure 10] 10(a) and 10(b) are a cross-sectional view and a plan view showing a part of a method for manufacturing a deposition mask according to one embodiment. [Figure 11] 11(a) and (b) are plan views showing the order in which a plurality of openings are formed. [Figure 12] FIG. 12 is a schematic diagram showing a deposition apparatus. [Figure 13] FIG. 13 is a schematic diagram showing an organic EL display device produced using a deposition mask. [Figure 14] 14(a) to 14(c) are schematic diagrams showing a method for manufacturing an organic EL display device using a deposition mask. [Figure 15] 15(a) and (b) are plan views showing modified examples of the reinforcing film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] Each embodiment will be described below with reference to the drawings. Each of the figures shown below is a schematic illustration. Therefore, the size and shape of each part are appropriately exaggerated to facilitate understanding. In addition, it is possible to carry out appropriate modifications within the scope of the technical idea. In each of the figures shown below, the same parts are given the same reference numerals, and some detailed explanations may be omitted. In addition, the numerical values ​​such as dimensions of each member and the material names described in this specification are examples of embodiments, and are not limited to these, and can be appropriately selected and used. In this specification, terms that specify shapes and geometric conditions, such as parallel, orthogonal, and vertical, are intended to include substantially the same state in addition to their strict meanings.

[0030] In this specification, the X direction and the Y direction are two directions parallel to each side of the deposition mask 10, and the X direction and the Y direction are perpendicular to each other. The Z direction is a direction perpendicular to both the X direction and the Y direction. Moreover, the terms "inner" and "inside" refer to the side facing the center of the deposition mask 10, and the terms "outer" and "outside" refer to the side away from the center of the deposition mask 10.

[0031] First, one embodiment will be described with reference to Figures 1 to 14. Figures 1 to 14 are diagrams showing this embodiment.

[0032] (Configuration of deposition mask) The configuration of the deposition mask according to the present embodiment will be described with reference to FIGS.

[0033] As shown in Figures 1 and 2, the deposition mask 10 according to this embodiment includes a resin mask 30 having a plurality of openings 31 corresponding to a pattern to be formed by deposition, and a support 40 joined to the resin mask 30.

[0034] The deposition mask 10 is used to simultaneously form deposition patterns for multiple screens, and one deposition mask 10 can simultaneously form deposition patterns corresponding to multiple products. Here, the "opening" means a pattern to be produced using the deposition mask 10. For example, when the deposition mask is used to form an organic layer in an organic EL display, the shape of the opening 31 is the shape of the organic layer. In addition, "one screen" is composed of a collection of openings 31 corresponding to one product, and when the one product is an organic EL display, a collection of organic layers necessary to form one organic EL display, that is, a collection of openings 31 that become an organic layer, becomes "one screen". The area that becomes one screen is also called "effective part". In addition, in the deposition mask 10, in order to simultaneously form deposition patterns for multiple screens, the above-mentioned "one screen" is arranged in the resin mask 30 at a predetermined interval for multiple screens. In other words, the resin mask 30 is provided with openings 31 necessary to form multiple screens.

[0035] The resin mask 30 is provided on one surface (the surface on the positive side in the Z direction) of the support 40. The resin mask 30 has a rectangular shape with each side extending in the X direction and the Y direction. The resin mask 30 has a first surface 30a and a second surface 30b located on the opposite side to the first surface 30a. The first surface 30a is a surface facing the opposite side of the support 40 (the positive side in the Z direction), and the second surface 30b is a surface facing the support 40 side (the negative side in the Z direction).

[0036] The resin mask 30 is provided with openings 31 used to form multiple screens. Each opening 31 has a quadrilateral shape, specifically, a rectangular shape with each side extending in the X direction and the Y direction. The corners of the quadrilateral forming the opening 31 may be rounded.

[0037] The resin mask 30 includes an effective area 32 in which openings 31 are formed in a regular arrangement, and a peripheral area 33 surrounding the effective area 32. The peripheral area 33 is an area for supporting the effective area 32, and is not an area through which a deposition material 92 (see FIG. 12) intended to be deposited on a deposition target substrate 91 passes. On the other hand, in a deposition mask 10 used for deposition of an organic light-emitting material, the effective area 32 is an area in the deposition mask 10 facing an area that becomes a display area of ​​the deposition target substrate 91 where the organic light-emitting material is deposited to form pixels. However, for various purposes, through holes or recesses may be formed in the peripheral area 33. Only the resin mask 30 exists in the effective area 32. That is, no metal layer that supports the resin mask 30 exists in the effective area 32. In the example shown in FIG. 1, each effective area 32 may have a contour that is substantially quadrangular in plan view, or more precisely, substantially rectangular in plan view. Although not shown, each effective area 32 may have a contour of various shapes depending on the shape of the display area of ​​the deposition substrate 91. For example, each effective area 32 may have a circular contour.

[0038] 1, the multiple effective areas 32 of the deposition mask 10 are arranged at predetermined intervals along two directions perpendicular to each other. In the illustrated example, one effective area 32 corresponds to one organic EL display device. That is, the deposition mask 10 according to the present embodiment enables multi-face deposition. Furthermore, the multiple openings 31 formed in each effective area 32 may be arranged at a predetermined pitch along the X direction and the Y direction perpendicular to each other in the effective area 32.

[0039] The multiple openings 31 are aligned in the X and Y directions and may have the same shape. The length L1 of one side of each opening 31 (length in the X and Y directions) may be, for example, 5 μm or more and 120 μm or less. Specifically, the length L1 may be, for example, 100 μm or more and 120 μm or less in the case of low resolution (200 ppi), and may be, for example, 5 μm or more and 20 μm or less in the case of high resolution (1000 ppi or more and 3000 ppi or less). The pitch P1 of each opening 31 (center-to-center distance of the openings 31 in the X and Y directions) may be, for example, 6 μm or more and 400 μm or less. Specifically, the pitch P1 may be, for example, 110 μm or more and 400 μm or less in the case of low resolution (200 ppi), and may be, for example, 6 μm or more and 100 μm or less in the case of high resolution (1000 ppi or more and 3000 ppi).

[0040] In plan view, the minimum distance between the support 40 and the opening 31 may be 1 mm or more. This allows a wide region for forming the deposition pattern while leaving a margin in the manufacturing process of the deposition mask 10.

[0041] As shown in FIG. 2, the periphery of each opening 31 may be tapered. In this case, each opening 31 has a shape in which the opening area gradually increases from the first surface 30a side (positive side in the Z direction) toward the second surface 30b side (negative side in the Z direction). The periphery of each opening 31 is inclined with respect to the normal direction (Z direction) of the resin mask 30 in a cross-sectional view. The periphery of each opening 31 may be inclined linearly or curvedly inclined in a cross-sectional view. The length L1 of one side of each opening 31 and the pitch P1 of each opening 31 described above refer to the length measured on the side where the area of ​​each opening 31 is narrower (the second surface 30b side).

[0042] The resin mask 30 can be made of a conventionally known resin material, and the material is not particularly limited. The resin mask 30 is preferably made of a material that allows high-definition openings 31 to be formed by laser processing or the like, has a small dimensional change rate and moisture absorption rate due to heat or over time, and is lightweight. Examples of such materials include polyimide resin, polyamide resin, polyamideimide resin, polyester resin, polyethylene resin, polyvinyl alcohol resin, polypropylene resin, polycarbonate resin, polystyrene resin, polyethylene terephthalate resin, polyacrylonitrile resin, ethylene vinyl acetate copolymer resin, ethylene-vinyl alcohol copolymer resin, ethylene-methacrylic acid copolymer resin, polyvinyl chloride resin, polyvinylidene chloride resin, cellophane, and ionomer resin. Among the materials exemplified above, a resin material whose thermal expansion coefficient is 16 ppm / °C or less is preferable, a resin material whose moisture absorption rate is 1.0% or less is preferable, and a resin material that satisfies both of these conditions is particularly preferable. By using this resin material to make a resin mask, the dimensional accuracy of the opening 31 can be improved, and the dimensional change rate and moisture absorption rate due to heat and time can be reduced. In addition, it is preferable to use a resin material whose difference in thermal expansion coefficient with the material constituting the support 40 is 15 ppm / °C or less, and the difference may be 10 ppm / °C or less. This makes it possible to prevent wrinkles from occurring in the resin mask 30 due to the difference in thermal expansion coefficient with the support 40. The resin mask 30 may contain a filler other than the resin material. The filler may include pigments, particles of inorganic materials, etc.

[0043] The thickness T1 of the resin mask 30 is not particularly limited, but may be 1 μm or more and 25 μm or less, preferably 1 μm or more and 5 μm or less, and more preferably 1 μm or more and 3 μm or less. By setting the thickness T1 of the resin mask 30 within this range, the risk of defects such as pinholes and deformations can be reduced, and the occurrence of shadows can be effectively prevented. In particular, by setting the thickness T1 of the resin mask 30 to 1 μm or more and 5 μm or less, a high-definition pattern exceeding 1000 ppi can be formed.

[0044] The resin mask 30 is suppressed from wrinkling on the surface. In particular, the occurrence of wrinkles at the boundary between the resin mask 30 and the support 40 when viewed in a plan view is reduced. That is, the first surface 30a of the resin mask 30 is flattened in-plane (particularly within the effective area 32). The flatness of the resin mask 30 may be 1 μm or more and 5 μm or less. As shown in FIG. 2, on the second surface 30b side of the resin mask 30, the area (inter-aperture area) 31a between the openings 31 is located on approximately the same plane. In the description of this embodiment, the "wrinkles" may include a mode showing thin lines formed on the surface of the resin layer, a mode in which the resin layer itself is bent, and the like.

[0045] The support 40 is provided on one surface (surface on the negative side in the Z direction) of the resin mask 30. In this embodiment, the support 40 is bonded to the resin mask 30 by an adhesive layer 35. The adhesive layer 35 exists in the area where the support 40 and the resin mask 30 overlap in a plan view. From another perspective, the resin mask 30 located inside the support 40 exists as a free-standing membrane (free-standing thin film) without being supported by a metal layer or the like. In the illustrated example, the support 40 is bonded to the resin mask 30 without the intervention of a metal layer that supports the resin mask 30. For the adhesive layer 35, for example, a thermosetting, photosetting, thermoplastic, or other adhesive can be used. In addition to the above-mentioned adhesion method using the adhesive layer 35, the method of bonding the support 40 and the resin mask 30 can include, for example, a welding method, a melting method, a pressure-sensitive adhesive, a bonding method using a thermoplastic resin, and a method using a polyimide precursor instead of an adhesive. As a result, even if the resin mask 30 is thinned to, for example, about 1 μm or more and 5 μm or less, by configuring the resin mask 30 itself as a self-supporting membrane, it is possible to suppress the occurrence of wrinkles in the resin mask 30 that occur when there is a metal layer supporting the resin mask. In this specification, the fact that the support 40 and the resin mask 30 are bonded includes not only the case where they are directly bonded without any member being interposed between the support 40 and the resin mask 30, but also the case where the support 40 and the resin mask 30 are bonded only with a member (which may be a member containing a metal material or may be a member not containing a metal material) such as an adhesive that is exclusively used for bonding the support 40 and the resin mask 30 being interposed.

[0046] The support 40 may be a frame that supports the resin mask 30. The support 40 supports the resin mask 30 in a state where the resin mask 30 is pulled in the direction of its surface so that the resin mask 30 does not bend. The support 40 is a frame member having a substantially rectangular shape, and has a through hole 41 for exposing the openings 31 provided in the resin mask 30 to the deposition source side. That is, the multiple openings 31 are located inside the through hole 41 in a plan view. The outer periphery of the support 40 is larger than the outer periphery of the resin mask 30. However, without being limited thereto, the outer periphery of the support 40 may have a shape smaller than the outer periphery of the resin mask 30, and the outer periphery of the resin mask 30 and the outer periphery of the support 40 may have the same shape. There is no particular limitation on the material of the support 40, but a metal material with high rigidity, for example, SUS, Invar material, ceramic material, resin material, semiconductor material such as silicon, etc. can be used.

[0047] The thickness T2 of the support 40 is not particularly limited, but is preferably about 10 mm or more and 30 mm or less in terms of rigidity, etc. The width W1 between the outer peripheral end face of the through hole 41 of the support 40 and the outer peripheral end face of the support 40 is not particularly limited as long as the width is sufficient to fix the support 40 and the resin mask 30, and can be, for example, about 10 mm or more and 250 mm or less.

[0048] Incidentally, whether or not the support 40 is provided is optional, and the support 40 does not necessarily have to be provided. In the present embodiment, the deposition mask 10 may include the support 40 (also called a deposition mask device) or may not include the support 40.

[0049] (Method of manufacturing deposition mask) Next, a method for manufacturing a deposition mask according to the present embodiment will be described with reference to Fig. 3 to Fig. 10. Fig. 3 to Fig. 10 are process diagrams for explaining the method for manufacturing a deposition mask according to the present embodiment.

[0050] First, as shown in FIG. 3(a), a substrate 51 is prepared. The substrate 51 is for supporting the resin layer 30A described below. The surface of the substrate 51, particularly the surface on which the resin layer 30A described below is formed, preferably has a small surface roughness. For example, the roughness of the surface of the substrate 51 may be set to an arithmetic mean height Sa of 1 μm or less. The "arithmetic mean height (Sa)" is a parameter obtained by extending the arithmetic mean height (Ra) of a line to a surface, and is a value calculated by averaging the absolute values ​​of the heights of each point with respect to the average surface of the surface to be measured. The arithmetic mean height (Sa) can be calculated, for example, by measuring the surface of the substrate 51 using a shape analysis laser microscope and calculating by a method conforming to ISO 25178. Examples of materials for the substrate 51 include glass, resin, silicon, and metals such as SUS. In particular, it is desirable to use transparent glass, taking into consideration the flatness of the surface and peeling by a laser lift-off method described below. For example, the transparent glass may have a transmittance of 80% or more for light with a wavelength of 308 nm. The thickness of the substrate 51 may be, for example, not less than 0.1 mm and not more than 10 mm.

[0051] Next, as shown in FIG. 3(b), a resin layer 30A is formed on one surface of the substrate 51. This resin layer 30A is for producing the resin mask 30 of the deposition mask 10 described above. Specifically, a resin solution such as a polyamic acid solution, which is a precursor of polyimide, is applied to the substantially entire surface of the substrate 51, and the resin layer 30A is obtained by heat-treating the applied solution. Alternatively, the resin layer 30A may be obtained by applying a resin solution such as a polyimide varnish, heating it, and drying it. Examples of a method for applying the resin solution include a spin coat method, a die coat method, a slit coat method, a dip coat method, and a spray coat method. The thickness of the applied resin solution may be, for example, 1 μm or more and 25 μm or less, preferably 1 μm or more and 5 μm or less, and more preferably 1 μm or more and 3 μm or less. The material of the resin layer 30A is not limited to polyimide, and a material with a small thermal expansion coefficient can be suitably used. The resin layer 30A may be formed by attaching a film-like material to the surface of the substrate 51. The resin layer 30A may have a single-layer structure, or may have a multi-layer structure in which a plurality of layers are laminated.

[0052] 4(a)(b), the reinforcing film 60 is attached onto the resin layer 30A. The reinforcing film 60 reinforces the thin resin layer 30A. By providing the reinforcing film 60 on the resin layer 30A, the handleability of the resin layer 30A can be improved in the manufacturing process of the deposition mask 10. For example, a removable film, a slightly adhesive film, a heat peeling film, or the like can be used as the reinforcing film 60. For the material of the reinforcing film 60, a resin such as polyethylene terephthalate (PET), polyethylene (PE), or polypropylene (PP) can be used. It is preferable that the reinforcing film 60 is thicker than the resin layer 30A. Specifically, the thickness of the reinforcing film 60 may be 50 μm or more and 500 μm or less. The reinforcing film 60 may be formed by patterning a photosensitive resin or the like on the resin layer 30A.

[0053] The reinforcing film 60 may be composed of only one portion. For example, the reinforcing film 60 may have only an outer peripheral portion 61 without having a central portion 62 described later (see FIG. 5(a)). The outer peripheral portion 61 is provided in an area that is gripped by a grip 55 when the resin layer 30A is fixed to the support 40 as described later. In this case, the reinforcing film 60 may be composed of a single frame-shaped (square ring-shaped) outer peripheral portion 61.

[0054] The reinforcing film 60 may be composed of a plurality of parts. Specifically, the reinforcing film 60 may have an outer peripheral part 61 and a central part 62 located on the inside of the outer peripheral part (see FIG. 5(b)). In this case, the reinforcing film 60 has the central part 62 and one outer peripheral part 61, and the outer peripheral part 61 may be formed in a frame shape (square ring shape).

[0055] As shown in FIG. 4(b), the reinforcing film 60 has a plurality of (four in this case) outer peripheral portions 61 and a (one in this case) central portion 62 located inside the outer peripheral portions. Each outer peripheral portion 61 extends in a strip shape in a plan view. Each outer peripheral portion 61 is arranged along the four sides of the rectangle constituting the resin layer 30A. The width of the outer peripheral portion 61 (the length in a direction perpendicular to the longitudinal direction of the outer peripheral portion 61) is preferably larger than the area gripped by the grip 55, and may be, for example, 10 mm or more and 50 mm or less. The area occupied by the outer peripheral portion 61 may be 10% or more and 50% or less, or may be 10% or more and 30% or less, of the entire area of ​​the resin layer 30A. This allows the effective area 32 to be provided widely while ensuring the strength required for the reinforcing film 60.

[0056] The central portion 62 has a rectangular shape in a plan view and is arranged so as to be surrounded by the four outer peripheral portions 61. The central portion 62 is provided in the region where the opening 31 is formed and the region where the support 40 is bonded, and plays a role in protecting these regions. Specifically, the central portion 62 can suppress scratches and dirt on the resin layer 30A in the manufacturing process of the deposition mask. The central portion 62 and each outer peripheral portion 61 are spaced apart from each other, and a gap is formed between the central portion 62 and each outer peripheral portion 61. In this way, the outer peripheral portions 61 and the central portion 62, which have different functions, are arranged apart from each other, so that they can be peeled off and removed from the resin layer 30A at different times. There is no limit to the size of the gap, but it may be, for example, 1 mm or more and 250 mm or less, or further 10 mm or more and 50 mm or less. In the bonding with the support 40 described later, when the resin layer 30A and the support 40 are bonded with the central portion 62 left, the support 40 may be in contact with the resin layer 30A through the gap. In addition, the outer peripheral portions 61 are also spaced apart from each other, and a gap is formed between the outer peripheral portions 61. There is no limit to the size of the gap, but it may be, for example, 1 mm or more and 20 mm or less. This makes it possible to prevent the outer peripheral portions 61 that are spaced apart from each other from overlapping each other, while ensuring a margin for the attachment position in the attachment step of the reinforcing film 60.

[0057] The outer peripheral portion 61 and the central portion 62 of the reinforcing film 60 may be made of the same material or different materials. For example, the outer peripheral portion 61 may be made thicker than the central portion 62 to increase its physical strength. For example, the outer peripheral portion 61 may be made of a reinforcing film having a higher adhesive strength than the central portion 62 to increase the adhesive strength with the resin layer 30A. For example, the central portion 62 may be made of a reinforcing film having a lower adhesive strength than the outer peripheral portion 61 to reduce the burden on the resin layer 30A when peeling and removing the reinforcing film. The reinforcing film 60 may be composed of only a plurality of outer peripheral portions 61 without having the central portion 62.

[0058] Next, as shown in FIG. 6(a), the substrate 51 is removed from the resin layer 30A to which the reinforcing film 60 is attached. As a result, an intermediate body (also called a deposition mask preparation body) having the resin layer 30A and the reinforcing film 60 on the resin layer 30A is obtained. The method for removing the substrate 51 from the resin layer 30A can be a laser lift-off method, a peeling method, a water immersion method, or the like. When using the peeling method, the resin layer 30A may be formed larger than the substrate 51 to provide a portion that serves as a trigger for peeling, or a physical notch may be provided at the end of the substrate 51 to provide a portion that serves as a trigger for peeling. In addition, in order to improve the handleability of the resin layer 30A, a re-peelable film for reinforcement (not shown) may be attached to the surface of the resin layer 30A after the substrate 51 is removed. In addition, a release agent may be applied to the substrate 51 in advance to make it easier to remove the substrate 51 from the resin layer 30A.

[0059] After removing the substrate 51, the resin layer 30A may be provided with another reinforcing film 67 (imaginary line) in the region where the central portion 62 was present on the side of the resin layer 30A that faced the substrate 51. In this case, the effective region 32 can be protected by the reinforcing film 67.

[0060] Next, as shown in FIG. 6(b), the central portion 62 of the reinforcing film 60 is peeled off and removed from the resin layer 30A. At this time, the outer peripheral portion 61 of the reinforcing film 60 remains on the resin layer 30A. By removing the central portion 62 of the reinforcing film 60 from the resin layer 30A in advance in this manner, when the resin layer 30A is pulled by the grip 55 as described below, the central portion of the resin layer 30A can stretch along the pulling direction of the grip 55. As a result, wrinkles in the central portion of the resin layer 30A are smoothed out and flattened.

[0061] In the case where the reinforcing film 67 is provided on the resin layer 30A, the reinforcing film 67 is also removed in the same manner as the reinforcing film 62.

[0062] Next, as shown in FIG. 7(a)(b), the support 40 is prepared, and the resin layer 30A is fixed to the support 40. Specifically, the resin layer 30A may be joined to the resin mask 30 by the adhesive layer 35 in a stretched state. At this time, the resin layer 30A is gripped by a plurality of grips 55 via the outer peripheral portion 61, and is in a state of being pulled in the surface direction. In this state, the resin layer 30A is joined to the support 40 by the adhesive layer 35. At this time, a pressing member 56 may be disposed at a position on the opposite side of the support 40 with respect to the resin layer 30A, and the support 40 may be pressed against the pressing member 56. This makes it easier to join the resin layer 30A to the support 40. In addition, the outer peripheral portion 61 of the reinforcing film 60 is interposed between the grip 55 and the resin layer 30A. Therefore, unlike the case where the thin resin layer 30A is pulled alone, the resin layer 30A is stretched while the strength of the thin resin layer 30A is supplemented by the outer peripheral portion 61. Therefore, the occurrence of wrinkles in the resin layer 30A due to pulling by the grip 55 is suppressed. In contrast, if the thin resin layer 30A is pulled by itself, the strength of the film may be insufficient and it may break. In this embodiment, the resin layer 30A is reinforced by the outer peripheral portion 61, so that the possibility of such breaking can be reduced. The resin layer 30A and the support 40 may be fixed over the entire surface where they contact, or over a part of the surface where they contact. Also, the resin layer 30A may be fixed to the support 40 without being pulled.

[0063] Methods for joining the support 40 and the resin layer 30A include, in addition to the adhesion method using the adhesive layer 35 described above, for example, a welding method in which the resin layer 30A is melted by heat, a welding method using a heat-sealing film, an adhesion method using an adhesive, a thermocompression method in which the support 40 and the resin layer 30A are thermocompressed by temperature and heat, a bonding method using a thermoplastic resin, and a method in which a polyimide precursor is used instead of an adhesive.

[0064] In the present embodiment, the support 40 is fixed to the surface (second surface 30b) of the resin layer 30A on which the reinforcing film 60 is provided. The surface (first surface 30a) of the resin layer 30A on which the reinforcing film 60 is not provided is the surface that was in contact with the substrate 51, and has a higher flatness than the second surface 30b. Therefore, by fixing the support 40 to the second surface 30b side of the resin layer 30A, the surface with a higher flatness (first surface 30a) can be opposed to the deposition substrate 91. However, the present invention is not limited to this, and the support 40 may be fixed to the first surface 30a of the resin layer 30A.

[0065] In order to increase the adhesive strength between the support 40 and the resin layer 30A, at least one of the support 40 and the resin layer 30A may be subjected to a surface treatment or a surface activation treatment. Examples of the surface treatment include a roughening treatment or the like that forms irregularities on the surface of the support 40 or the resin layer 30A. Specifically, the surface roughness of the support 40 or the resin layer 30A may be set to an arithmetic mean height Sa of 0.001 μm or more and 1 μm or less. Examples of the surface activation treatment include a treatment that makes the surface of the support 40 or the resin layer 30A hydrophobic or hydrophilic.

[0066] 8(a), an intermediate body (also called a deposition mask device preparation body) having the resin layer 30A, the outer peripheral portion 61 of the reinforcing film 60 formed on the resin layer 30A, and the support 40 fixed to the resin layer 30A is obtained. At this time, the support 40 is located inside the outer peripheral portion 61.

[0067] Next, as shown in FIG. 8(b), a portion 30c of the resin layer 30A located on the outer periphery of the support 40 is removed. At this time, the outer peripheral portion 61 of the reinforcing film 60 is also removed together with the portion 30c. In this case, the resin layer 30A may be cut by, for example, a blade or laser light. The cutting position of the resin layer 30A is a position that corresponds to the inner side of the outer periphery 40b of the support 40 and the outer side of the inner periphery 40a of the support 40. However, the present invention is not limited to this, and the cutting position of the resin layer 30A may be a position that corresponds to the outer periphery 40b of the support 40 or a position that corresponds to the outer periphery 40b of the support 40.

[0068] As shown in FIG. 9(a), the outer periphery 30d of the resin layer 30A after cutting and the outer periphery 35a of the adhesive layer 35 may overlap in a plan view. As shown in FIG. 9(b), the outer periphery 35a of the adhesive layer 35 may be located inside the outer periphery 30d of the resin layer 30A after cutting, and the amount δ of the outer periphery 35a of the adhesive layer 35 recessed from the outer periphery 30d of the resin layer 30A after cutting may be 0.1 mm or less. As shown in FIG. 9(c), the boundary between the resin layer 30A and the adhesive layer 35 may be free of a recess, and the two may be connected by a substantially flat or curved surface. That is, the outer periphery 35a of the adhesive layer 35 may extend from the outer periphery 30d of the resin layer 30A after cutting to be gently curved toward the outer periphery 40b of the support 40. This can suppress the residue of the cleaning liquid when cleaning the deposition mask 10.

[0069] Next, as shown in FIG. 10(a)(b), the resin layer 30A is irradiated with laser light (see the arrow in FIG. 10(a)) from the support 40 side to form the openings 31 in the resin layer 30A corresponding to the pattern to be formed by deposition. For example, a KrF excimer laser with a wavelength of 248 nm or a YAG laser with a wavelength of 355 nm can be used as the laser. At this time, a protective film 57 may be attached to the surface of the resin layer 30A opposite to the support 40, and in this state, the openings 31 may be formed by irradiating the laser light from the support 40 side. In this case, a laser mask (not shown) corresponding to the pattern to be formed by deposition may be used, and a condenser lens may be placed between the laser mask and the resin layer 30A, to form the openings 31 by a laser processing method using a so-called reduced projection optical system. As described above, the deposition mask 10 in this embodiment is configured as a membrane in which the effective area 32 of the resin mask 30 is not supported by a metal layer and is independent. As a result, the tension of the grip 55 is easily transmitted to the resin mask 30, so that the occurrence of wrinkles in the resin mask 30 is suppressed.

[0070] In addition, when forming a plurality of openings 31 for each of a plurality of effective regions 32, the plurality of openings 31 may be formed sequentially for adjacent effective regions 32 as shown by the arrows in FIG. 11(a). That is, after forming a plurality of openings 31 in one effective region 32, the plurality of openings 31 may be formed in an effective region 32 adjacent to the effective region 32 in the X direction or Y direction, and by repeating this, a plurality of openings 31 may be formed in all effective regions 32. Alternatively, as shown by the arrows in FIG. 11(b), the plurality of openings 31 may be formed sequentially for non-adjacent effective regions 32. That is, after forming a plurality of openings 31 in one effective region 32, the plurality of openings 31 may be formed in an effective region 32 not adjacent to the effective region 32 in the X direction or Y direction, and by repeating this, a plurality of openings 31 may be formed in all effective regions 32. After forming a plurality of openings 31 in a certain effective region 32, it is preferable to select the effective region 32 to be processed next while observing the state of the resin layer 30A. For example, in Fig. 11(a), after processing the effective area 32 in the upper right column, the resin layer 30A is observed to check whether wrinkles or the like have occurred, and the effective area 32 in the middle right column is processed. Thereafter, similar processing is performed sequentially. For example, in Fig. 11(b), after processing the effective area 32 in the upper right column, the resin layer 30A is observed to check whether wrinkles or the like have occurred, and the effective area 32 in the lower left column (the effective area corresponding to the diagonal position) is processed to adjust the in-plane balance. Thereafter, similar processing is performed sequentially.

[0071] In this manner, a deposition mask 10 (see FIGS. 1 and 2) is obtained, which includes a resin mask 30 having a plurality of openings 31 corresponding to the pattern to be formed by deposition, and a support 40 joined to the resin mask 30.

[0072] The manufacturing method according to the present embodiment includes, but is not limited to, a step of forming the resin layer 30A on the substrate 51. For example, the resin layer 30A on which the reinforcing film 60 is previously arranged may be prepared, and the resin layer 30A may be bonded to the support 40.

[0073] (Configuration of deposition device) Next, a deposition apparatus for depositing a deposition material onto a deposition target using the above-described deposition mask 10 will be described with reference to FIG.

[0074] As shown in FIG. 12, the deposition apparatus 80 has a deposition source (e.g., a crucible 81), a heater 82, and a deposition mask 10 arranged therein. The deposition apparatus 80 further has an exhaust means (not shown) for creating a vacuum atmosphere inside the deposition apparatus 80. The crucible 81 contains a deposition material 92 such as an organic light-emitting material. The heater 82 heats the crucible 81 to evaporate the deposition material 92 under a vacuum atmosphere. The deposition mask 10 is arranged to face the crucible 81. That is, the deposition mask 10 is arranged in the deposition apparatus 80 so that the resin mask 30 faces a deposition target substrate (e.g., an organic EL substrate) 91, which is a deposition target to which the deposition material 92 is to be attached.

[0075] Fig. 13 is a cross-sectional view showing an organic EL display device 90 manufactured using the deposition apparatus 80 shown in Fig. 12. As shown in Fig. 13, the organic EL display device 90 includes a deposition target substrate (e.g., an organic EL substrate) 91 and pixels including a deposition material 92 provided in a pattern on the deposition target substrate 91.

[0076] When a color display using a plurality of colors is desired, deposition devices 80 each equipped with a deposition mask 10 corresponding to each color are prepared, and the deposition substrate 91 is sequentially placed in each deposition device 80. In this way, for example, a red organic light-emitting material, a green organic light-emitting material, and a blue organic light-emitting material can be deposited on the deposition substrate 91 in that order.

[0077] (Manufacturing method for organic EL display device) Next, a method for manufacturing an organic EL display device according to the present embodiment will be described with reference to Fig. 14(a)-(c). In the method for manufacturing an organic EL display device according to the present embodiment, a deposition material 92 is deposited on a deposition target substrate 91, which is a deposition object, by a deposition method using the deposition mask 10 described above, to form a deposition pattern.

[0078] First, as shown in FIG. 14(a), a deposition apparatus 80 including the deposition mask 10 shown in FIGS. 1 and 2, a crucible 81 containing a deposition material 92, and a heater 82 is prepared.

[0079] 14(b), the substrate 91 to be deposited is placed on the resin mask 30 of the deposition mask 10. At this time, for example, an alignment mark (not shown) of the substrate 91 to be deposited and an alignment mark (not shown) of the deposition mask 10 may be directly observed, and the substrate 91 to be deposited may be placed on the deposition mask 10 while positioning the substrate 91 so that the alignment marks overlap each other.

[0080] Next, the deposition material 92 is deposited on the deposition substrate 91 placed on the resin mask 30 of the deposition mask 10. At this time, for example, as shown in FIG. 14(c), the surface of the deposition substrate 91 opposite to the deposition mask 10 is brought into close contact with the resin mask 30. Next, the heater 82 heats the crucible 81 to evaporate the deposition material 92. Then, the deposition material 92 that has evaporated from the crucible 81 and reached the deposition mask 10 passes through the openings 31 of the resin mask 30 and adheres to the deposition substrate 91.

[0081] In this manner, the deposition material 92 is deposited on the deposition substrate 91 in a desired pattern corresponding to the positions of the openings 31 in the resin mask 30. That is, the deposition material 92 is formed in a shape corresponding to the multiple openings 31 in the resin mask 30. In this manner, an organic EL display device 90 is obtained that includes a deposition substrate (e.g., an organic EL substrate) 91 and pixels including the deposition material 92 provided in a pattern (see FIG. 13).

[0082] (Method of manufacturing an organic semiconductor device) Next, a method for manufacturing an organic semiconductor device according to the present embodiment will be described. The method for manufacturing an organic semiconductor device according to the present embodiment includes a step of forming a deposition pattern on a deposition target using the deposition mask 10 described above, or a step of forming a deposition pattern on a deposition target using the deposition mask 10 manufactured by the method for manufacturing the deposition mask 10 described above. The step of forming a deposition pattern on a deposition target is not limited in any way, and examples of the method include physical vapor deposition methods such as reactive sputtering, vacuum deposition, ion plating, and electron beam deposition, and chemical vapor deposition methods such as thermal CVD, plasma CVD, and photo CVD.

[0083] The manufacturing method of an organic semiconductor device according to an embodiment having a step of forming a deposition pattern on a deposition target includes an electrode forming step of forming an electrode on a substrate, an organic layer forming step, a counter electrode forming step, a sealing layer forming step, and the like, and in each optional step, a deposition pattern may be formed on the substrate by a deposition method using a deposition mask 10. For example, when a deposition method using a deposition mask 10 is applied to each of the steps of forming the R, G, and B light-emitting layers of an organic EL device, a deposition pattern of each color light-emitting layer is formed on the substrate. The manufacturing method of an organic semiconductor device according to this embodiment is not limited to these steps, and can be applied to any of the steps of a conventionally known organic semiconductor device using a deposition method.

[0084] The deposition mask 10 may be the deposition mask 10 according to the present embodiment described above, and detailed description thereof will be omitted here. The deposition mask 10 according to the present embodiment described above allows an organic semiconductor element having a highly precise pattern to be formed. Examples of the organic semiconductor element manufactured by the manufacturing method according to the present embodiment include an organic layer, a light-emitting layer, and a cathode electrode of an organic EL element. In particular, the manufacturing method for an organic semiconductor element according to the present embodiment can be suitably used for manufacturing the R, G, and B light-emitting layers of an organic EL element, which require highly precise pattern accuracy.

[0085] As described above, according to the present embodiment, when manufacturing the deposition mask 10, a step of attaching the reinforcing film 60 onto the resin layer 30A is provided. This makes it possible to improve the handleability of the resin layer 30A in the manufacturing process of the deposition mask 10. Furthermore, by attaching the reinforcing film 60 onto the resin layer 30A, it is possible to suppress the generation of wrinkles in the deposition mask 10.

[0086] According to the present embodiment, a step of attaching a reinforcing film 60 onto the resin layer 30A is provided. This makes it possible to suppress the occurrence of wrinkles on the outer periphery of the resin layer 30A (for example, a position near the grip 55) or the breakage of the resin layer 30A when the resin layer 30A is pulled in the step of fixing the resin layer 30A to the support 40 (FIGS. 7(a) and 7(b)). As a result, the resin mask 30 of the deposition mask 10 can be flattened, and the distance between the resin mask 30 and the deposition substrate 91 during deposition can be made uniform. This makes it possible to form pixels of the organic EL display device 90 with high quality.

[0087] Furthermore, according to the present embodiment, a step of removing a portion of the resin layer 30A located on the outer periphery of the support 40 is provided (FIG. 8(b)). This makes it possible to remove the unnecessary portion 30c of the resin layer 30A located around the support 40. Moreover, since the outer periphery portion 61 of the reinforcing film 60 is also removed together with the portion 30c of the resin layer 30A, there is no need to provide a separate step of removing the outer periphery portion 61.

[0088] Furthermore, according to this embodiment, the reinforcing film 60 includes an outer peripheral portion 61 in an area that is gripped when the resin layer 30A is fixed to the support 40. This allows the resin layer 30A to be pulled while maintaining the flatness of the resin layer 30A by the outer peripheral portion 61 in the step of fixing the resin layer 30A to the support 40 (FIGS. 7(a) and 7(b)). This makes it possible to prevent wrinkles from occurring in the resin layer 30A due to being pulled by the grip 55.

[0089] According to this embodiment, the reinforcing film 60 includes a central portion 62 located more centrally than the peripheral portion 61, and the central portion 62 and the peripheral portion 61 are spaced apart from each other. This central portion 62 can protect the area where the opening 31 is formed and the area where the support 40 is bonded. In addition, since the central portion 62 and the peripheral portion 61 are not integrated, the central portion 62 can be removed before the peripheral portion 61. Therefore, in the step of fixing the resin layer 30A to the support 40 (FIGS. 7(a)(b)), the area of ​​the resin layer 30A where the central portion 62 was provided is pulled, and it is possible to prevent wrinkles from occurring in this area. In addition, the support 40 can be bonded to the area of ​​the resin layer 30A where the central portion 62 was provided.

[0090] According to the present embodiment, the deposition mask 10 includes the resin mask 30 and the support 40 bonded to the resin mask 30. By configuring the resin mask 30 itself as a self-supporting membrane, it is possible to suppress the occurrence of wrinkles in the resin mask 30, which would occur if there was a metal layer supporting the resin mask 30.

[0091] (Modification) Next, various modifications of this embodiment will be described.

[0092] (Modification of Reinforcement Film) 15(a) and 15(b) are plan views showing a state in which a reinforcing film 60A according to this modification is attached onto a resin layer 30A. As shown in FIG. 15(a) and 15(b), the reinforcing film 60A according to this modification has a frame-shaped outer peripheral portion 61A. This outer peripheral portion 61A is arranged along the inside of the four sides of the rectangle constituting the resin layer 30A. In the part of the outer peripheral portion 61A facing inward, a notch portion 65 (FIG. 15(a)) or a slit 66 (FIG. 15(b)) is formed in a plan view, and specifically, the notch portion 65 or the slit 66 is formed in a comb-tooth shape. That is, the outer peripheral portion 61A has a peripheral edge portion 63 and a plurality of protruding portions 64 protruding inward in the planar direction from the peripheral edge portion 63. The plurality of protruding portions 64 are arranged at intervals from each other (FIG. 15(a)), or are arranged via gaps that have substantially no width (FIG. 15(b)).

[0093] In this way, the inwardly facing portion of the outer peripheral portion 61A is formed in a comb-tooth shape in a plan view, and thus, in the process of fixing the resin layer 30A to the support 40 (FIGS. 7(a)(b)), it is possible to suppress the occurrence of wrinkles in the resin layer 30A. That is, since the outer peripheral portion 61A is formed in a comb-tooth shape, when the resin layer 30A is pulled, it is possible to suppress the occurrence of wrinkles in the resin layer 30A. When the reinforcing film 60A has long sides (sides extending in the vertical direction in FIG. 15(a)(b)) and short sides (sides extending in the horizontal direction in FIG. 15(a)(b)), the number of protrusions 64 present on the long sides may be greater than the number of protrusions 64 present on the short sides. The intervals between the multiple protrusions 64 may be constant, or the intervals may be locally increased or decreased.

[0094] In this modification, the reinforcing film 60A may have a plurality of outer peripheral portions 61A. For example, as in the embodiment shown in Fig. 4(b), the outer peripheral portion 61A may extend in a band shape in a plan view and be formed in a comb-like shape. In this modification, the central portion 62 may be provided inside the outer peripheral portion 61A.

[0095] (Modification of the deposition mask manufacturing method) Next, each of the modified examples of the method for manufacturing the deposition mask will be described.

[0096] In the above embodiment, an example has been described in which the steps of (i) removing the substrate 51 from the resin layer 30A (FIG. 6(a)), (ii) fixing the resin layer 30A to the support 40 (FIGS. 7(a)(b)), (iii) removing a portion of the resin layer 30A that is located on the outer periphery of the support 40 (FIG. 8(b)), and (iv) forming a plurality of openings 31 in the resin layer 30A (FIGS. 10(a)(b)) are performed in this order, but the present invention is not limited to this.

[0097] For example, (iv) a step of forming a plurality of openings 31 in the resin layer 30A, (i) a step of removing the substrate 51 from the resin layer 30A, (ii) a step of fixing the resin layer 30A to the support 40, and (iii) a step of removing a portion of the resin layer 30A located on the outer periphery of the support 40 may be performed in this order. As a result, the openings 31 can be formed in a state in which the resin layer 30A is fixed to the support 40, so that the waviness of the resin layer 30A is suppressed by the support 40, and the step of forming the openings 31 can be stably performed. In this case, the step of attaching the reinforcing film 60 to the resin layer 30A may be performed between the step of forming the openings 31 and the step of removing the substrate from the resin layer 30A.

[0098] Alternatively, (iv) a step of forming a plurality of openings 31 in the resin layer 30A, (ii) a step of fixing the resin layer 30A to the support 40, (i) a step of removing the substrate 51 from the resin layer 30A, and (iii) a step of removing a portion of the resin layer 30A located on the outer periphery of the support 40 may be performed in this order. This allows the flat surface of the resin layer 30A (the surface in contact with the substrate 51) to be protected by the substrate 51 throughout the manufacturing process of the deposition mask 10. In this case, it is not necessary to provide a step of attaching a reinforcing film 60 to the resin layer 30A.

[0099] Also, (ii) a step of fixing the resin layer 30A to the support 40, (i) a step of removing the substrate 51 from the resin layer 30A, (iii) a step of removing a portion of the resin layer 30A located on the outer periphery of the support 40, and (iv) a step of forming a plurality of openings 31 in the resin layer 30A may be performed in this order. This makes it possible to easily perform the fixing operation since waviness of the resin layer 30A is suppressed in the step of fixing the resin layer 30A to the support 40. In this case, it is not necessary to provide a step of attaching the reinforcing film 60 to the resin layer 30A.

[0100] Also, (ii) a step of fixing the resin layer 30A to the support 40, (iv) a step of forming a plurality of openings 31 in the resin layer 30A, (i) a step of removing the substrate 51 from the resin layer 30A, and (iii) a step of removing a portion of the resin layer 30A located on the outer periphery of the support 40 may be performed in this order. This makes it easier to perform the step of fixing the resin layer 30A to the support 40, and also makes it possible to stably perform the step of forming the openings 31. In this case, it is not necessary to provide a step of attaching a reinforcing film 60 to the resin layer 30A.

[0101] It is also possible to combine the multiple components disclosed in the above embodiment and modified examples as necessary. Alternatively, some components may be deleted from all the components shown in the above embodiment and modified examples. [Explanation of symbols]

[0102] 10 Deposition mask 30 Resin Mask 30A resin layer 31 Opening 32 Effective Area 33 Surrounding Area 35 Adhesive layer 40 Support 51 Substrate 60 Reinforcement film 61 Outer area 62 Central part

Claims

1. providing a substrate; forming a resin layer on the substrate; removing the substrate from the resin layer; fixing the resin layer to a support; forming a plurality of openings in the resin layer corresponding to a pattern to be formed by vapor deposition; removing a portion of the resin layer located on an outer periphery of the support.

2. providing a substrate; forming a resin layer on the substrate; removing the substrate from the resin layer; fixing the resin layer to a support; forming a plurality of openings in the resin layer corresponding to a pattern to be formed by vapor deposition; and attaching a reinforcing film onto the resin layer. In the step of removing the substrate, the substrate is removed from the resin layer to which the reinforcing film is attached, The reinforcing film includes an outer peripheral portion in a region that is gripped when the resin layer is fixed to the support.

3. The method for manufacturing a deposition mask according to claim 2 , wherein the reinforcing film includes a central portion located more inward than the outer circumferential portion, and the central portion and the outer circumferential portion are spaced apart from each other.

4. The method for manufacturing a deposition mask according to claim 2 , wherein an inwardly facing portion of the outer circumferential portion is formed in a comb-like shape in a plan view.

5. The method for manufacturing a deposition mask according to claim 1 , wherein the resin layer has a thickness of 1 μm or more and 5 μm or less.

6. A method for manufacturing an organic electroluminescence display device, comprising the steps of: A method for manufacturing an organic electroluminescence display device, comprising: forming a deposition pattern on a deposition target by using the deposition mask manufactured by the method for manufacturing a deposition mask according to claim 1 .

7. preparing a deposition mask manufactured by the method for manufacturing a deposition mask according to claim 1 ; preparing a deposition object; placing the deposition object on the deposition mask; and depositing a deposition material onto the deposition target placed on the deposition mask.

8. A method for manufacturing an organic semiconductor device, comprising the steps of: A method for manufacturing an organic semiconductor element, comprising: forming a deposition pattern on a deposition target using the deposition mask manufactured by the method for manufacturing a deposition mask according to claim 1 .

Citation Information

Patent Citations

  • Manufacturing method of mask and manufacturing device of mask

    JP2013108143A

  • Method for manufacturing vapor deposition mask, vapor deposition mask preparation body, method for manufacturing organic semiconductor element and vapor deposition mask

    JP2017014620A

  • Film deposition mask, manufacturing method of the mask and repair method of film deposition mask

    JP2017179591A

  • Mask frame assembly and method of manufacturing the same

    US20150368785A1

  • Method for producing resin film having fine pattern, method for producing organic el display device, base film for forming fine pattern, and resin film provided with support member