Rubber composition for studless tires
The rubber composition for studless tires addresses the limitations of existing technologies by incorporating specific resin particles and diene rubber components, resulting in enhanced on-ice performance and wear resistance through improved dispersibility and mechanical properties.
Patent Information
- Application Number
- JP2020191394
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-11-18
AI Technical Summary
Existing studless tires face limitations in improving both on-ice performance and wear resistance, with increased surface roughness enhancing wet performance but reducing ice contact area and potentially deteriorating wear resistance due to the use of foaming agents or thermally expandable microcapsules.
A rubber composition for studless tires comprising 30 parts by mass of a white filler, 0.5 to 0.5 parts by mass of resin particles with specific properties, and 100 parts by mass of diene rubber containing polybutadiene and natural rubber, along with other additives to enhance dispersibility and compatibility, improves on-ice performance and wear resistance.
The composition achieves improved dispersibility of resin particles, enhancing both on-ice performance and wear resistance beyond conventional levels by maintaining flexibility and mechanical properties while ensuring effective ice adhesion.
Smart Images

Figure 0007579680000001 
Figure 0007579680000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for studless tires which improves performance on ice and abrasion resistance. [Background technology]
[0002] It is known that the surface roughness (unevenness) of tread rubber can be increased to improve the performance of studless tires on ice. It is believed that increasing the surface roughness increases the contact area with the ice surface compared to tread rubber with a smooth surface, as the concave parts absorb the water film present on the ice and the convex parts come into contact with the ice surface. For this reason, a common method is to increase the roughness of the entire rubber by compounding a foaming agent or thermally expandable microcapsules into the tread rubber (see, for example, Patent Document 1).
[0003] However, although rubber with a large surface roughness improves wet performance by absorbing and expelling a water film, the surface area that can contact the ice surface is reduced, so the effect of improving ice performance due to surface roughness is limited. In addition, there is a problem that the wear resistance of the tread rubber decreases when a foaming agent or thermally expandable microcapsules are compounded. Furthermore, if the thermally expandable microcapsules are not well dispersed in the diene rubber, there is a concern that the wear resistance may worsen due to the decrease in breaking strength.
[0004] As described above, despite recent technological advances, there are still higher demands for improved performance on ice and wear resistance in studless tires, and further improvements have been required. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2018-123209 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a rubber composition for studless tires which has improved performance on ice and wear resistance. [Means for solving the problem]
[0007] The rubber composition for studless tires of the present invention, which achieves the above object, comprises 100 parts by mass of diene rubber containing 30% by mass or more of polybutadiene and natural rubber, 30 parts by mass or more of white filler, 0.5 to 30 parts by mass of resin particles, and 10 parts by mass or more of liquid rubber having a weight average molecular weight of 1,000 to 100,000. The resin particles are made of a polymer of a monomer mixture consisting of a non-crosslinkable monomer including a (meth)acrylic acid ester monomer and a crosslinkable monomer, the average particle size of the resin particles is 15 to 50 μm, and the glass transition temperature of the resin particles is −50 to −30° C. It is characterized by: Effect of the Invention
[0008] The rubber composition for studless tires of the present invention is formulated so that a liquid rubber having a weight-average molecular weight of 1,000 to 100,000 is blended together with the resin particles, thereby improving the dispersibility of the resin particles in the diene rubber and improving the performance on ice and abrasion resistance beyond conventional levels.
[0009] The rubber composition for studless tires preferably has a rubber hardness of 60 or less at 20°C according to JIS K6253, durometer type A, and / or a glass transition temperature of -30°C or less, and can contain carbon black to improve performance on ice.
[0010] before The mass ratio of the (meth)acrylic acid ester monomer in the non-crosslinkable monomer is 85 to 100 mass %, and the mass ratio of the crosslinkable monomer in the monomer mixture is 2 to 5 mass %. be By using such crosslinked acrylic resin particles, it is possible to improve the performance on ice and the abrasion resistance.
[0011] The diene rubber preferably contains a modified butadiene rubber, and the rubber composition for studless tires preferably contains an aromatic modified terpene resin, which improves the dispersibility of the resin particles and provides better abrasion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The diene rubber constituting the rubber composition for studless tires of the present invention necessarily contains polybutadiene and natural rubber. By containing polybutadiene, flexibility at low temperatures can be ensured. The polybutadiene is contained in an amount of 30 mass% or more, preferably 30 to 70 mass%, more preferably 35 to 65 mass%, in 100 mass% of the diene rubber. If the polybutadiene content is less than 30 mass%, flexibility at low temperatures cannot be ensured. The polybutadiene is at least one selected from unmodified polybutadiene and modified polybutadiene (modified butadiene rubber), and when both unmodified polybutadiene and modified butadiene rubber are included, the total of both may be 30 mass% or more.
[0013] The modified butadiene rubber is not particularly limited, and it is sufficient that it has affinity with resin particles, particularly crosslinked acrylic resin particles. Examples of the modified group of the modified butadiene rubber include a hydroxyl group, an amino group, a carboxyl group, an epoxy group, an alkoxy group, a silyl group, an amide group, and an organosiloxane group. Among them, the organosiloxane group and the carboxyl group are preferred.
[0014] The natural rubber is not particularly limited, and may contain any natural rubber that is normally used in rubber compositions for studless tires. The natural rubber is preferably contained in an amount of 30 to 70 mass%, more preferably 35 to 65 mass%, based on 100 mass% of the diene rubber. By containing 30 mass% or more of natural rubber, excellent abrasion resistance is achieved. Furthermore, by containing 70 mass% or less of natural rubber, excellent flexibility at low temperatures is achieved.
[0015] The diene rubber may contain other diene rubbers other than polybutadiene and natural rubber. Examples of other diene rubbers include isoprene rubber, styrene-butadiene rubber, styrene-isoprene rubber, styrene-isoprene-butadiene rubber, and acrylonitrile-butadiene rubber. Among these, styrene-butadiene rubber is preferred. These other diene rubbers may be unmodified, but may also be modified diene rubbers in which the terminals and / or side chains of the molecular chain are modified with epoxy groups, carboxy groups, amino groups, hydroxy groups, alkoxy groups, silyl groups, amide groups, or the like.
[0016] The rubber composition for studless tires contains a white filler. The amount of the white filler is 30 parts by mass or more, preferably 30 to 100 parts by mass, more preferably 40 to 90 parts by mass, and further preferably 45 to 80 parts by mass, per 100 parts by mass of the diene rubber. By making the amount of the white filler 30 parts by mass or more, the mechanical properties of the rubber composition can be improved and the abrasion resistance can be improved. Furthermore, by making the amount of the white filler 100 parts by mass or less, the flexibility of the rubber composition can be maintained and the performance on ice can be ensured. Furthermore, the weight increase can be suppressed when the tire is made.
[0017] Examples of white fillers include silica, calcium carbonate, magnesium carbonate, talc, clay, alumina, aluminum hydroxide, titanium oxide, and calcium sulfate. These may be used alone or in combination of two or more. Among these, silica is preferred, as it can provide better performance on ice.
[0018] Examples of silica include wet silica (hydrated silicic acid), dry silica (anhydrous silicic acid), calcium silicate, aluminum silicate, etc., which may be used alone or in combination of two or more. The CTAB adsorption specific surface area of silica is not particularly limited, but is preferably 80 to 260 m 2 / g, more preferably 140 to 200m 2 / g. The CTAB adsorption specific surface area of silica is 80m 2By making the CTAB adsorption specific surface area of the silica 200 m / g or more, the abrasion resistance of the rubber composition can be ensured. 2 By making the CTAB specific surface area of silica equal to or less than 1 / g, it is possible to improve wet performance and low rolling resistance. In this specification, the CTAB specific surface area of silica is a value measured according to ISO 5794.
[0019] In the present invention, it is preferable to compound a silane coupling agent together with silica, which improves the dispersibility of silica in diene rubber and improves the balance between abrasion resistance and performance on ice.
[0020] The type of silane coupling agent is not particularly limited as long as it can be used in a rubber composition containing silica. Examples of the silane coupling agent include sulfur-containing silane coupling agents such as bis-(3-triethoxysilylpropyl) tetrasulfide, bis(3-triethoxysilylpropyl) disulfide, 3-trimethoxysilylpropyl benzothiazole tetrasulfide, γ-mercaptopropyl triethoxysilane, and 3-octanoylthiopropyl triethoxysilane.
[0021] The amount of the silane coupling agent is preferably 3 to 15 mass % based on the weight of silica, and more preferably 5 to 10 mass %. If the amount of the silane coupling agent is less than 3 mass % of the amount of silica, the dispersion of the silica may not be sufficiently improved. If the amount of the silane coupling agent is more than 15 mass % of the amount of silica, the silane coupling agents condense with each other, and the desired hardness and strength of the rubber composition cannot be obtained.
[0022] The rubber composition for studless tires may optionally contain carbon black. When carbon black is contained, the total amount of the white filler and the carbon black is preferably more than 30 parts by mass and not more than 100 parts by mass, more preferably 40 to 90 parts by mass, and even more preferably 45 to 80 parts by mass, per 100 parts by mass of the diene rubber. Examples of carbon black include furnace carbon black such as SAF, ISAF, HAF, FEF, GPF, HMF, and SRF, which may be used alone or in combination of two or more kinds. The nitrogen adsorption specific surface area of the carbon black is not particularly limited, but is preferably 70 to 240 m 2 / g, more preferably 90 to 200m 2 / g. The nitrogen adsorption specific surface area of carbon black is preferably 70m 2 By making the carbon black have a specific surface area of 240 m / g or more, the mechanical properties and abrasion resistance of the rubber composition can be ensured. 2 / g or less, the performance on ice can be improved. In this specification, the nitrogen adsorption specific surface area of carbon black is measured in accordance with JIS K6217-2.
[0023] The rubber composition for studless tires improves the performance on ice and the wear resistance by blending resin particles. The resin particles can be prepared by polymerizing a monomer mixture consisting of a crosslinkable monomer having at least two ethylenically unsaturated groups in one molecule and a non-crosslinkable monomer having one ethylenically unsaturated group in one molecule by suspension polymerization, seed polymerization, or dispersion polymerization. In addition, it is preferable that the resin particles are resin particles that are incompatible with diene rubber. Here, "incompatible with diene rubber" does not mean incompatible with all types of rubber components contained in diene rubber, but only incompatible with the specific diene rubber contained in the rubber composition for studless tires. The specific resin particles that are incompatible with diene rubber form a phase separation structure with the diene rubber, thereby making the performance on ice excellent.
[0024] The resin particles are blended in an amount of 0.5 to 30 parts by mass, preferably 1 to 20 parts by mass, and more preferably 2 to 15 parts by mass, per 100 parts by mass of diene rubber. If the resin particles are less than 0.5 parts by mass, the performance on ice cannot be improved. If the resin particles are more than 30 parts by mass, the abrasion resistance decreases.
[0025] The resin particles preferably have an average particle size of 15 to 50 μm and a glass transition temperature of -50 to -30°C.
[0026] The average particle diameter of the resin particles is preferably 15 to 50 μm, more preferably 20 to 45 μm, and even more preferably 25 to 40 μm. If the average particle diameter of the resin particles is 15 μm or more, the surface of the tread rubber can be deformed to correspond to minute irregularities on the ice surface, improving performance on ice. However, if the average particle diameter of the resin particles exceeds 50 μm, the resin particles fall off the surface of the tread rubber, and the abrasion resistance deteriorates. In this specification, the average particle diameter of the resin particles is the average value of the particle diameters of at least 100 resin particles measured from a microscope observation image taken at 1000 to 5000 times. When the image of the resin particles is not circular, the circle-equivalent diameter calculated from the projected area can be used as the particle diameter.
[0027] The glass transition temperature of the resin particles is preferably -50°C to -30°C, more preferably -50°C to -35°C, and even more preferably -50°C to -38°C. By setting the glass transition temperature of the resin particles to -30°C or lower, the flexibility of the rubber compound at low temperatures is maintained and the adhesive strength to ice surfaces is increased, so that the resin particles can be suitably used in the tread portion of studless tires. Furthermore, by setting the glass transition temperature to -50°C or higher, rigidity can be ensured. The glass transition temperature is determined as the midpoint temperature of the transition region measured by differential scanning calorimetry (DSC) at a heating rate of 20°C / min.
[0028] The material for forming the resin particles is not particularly limited as long as it satisfies the characteristic of having a glass transition temperature of -50°C to -30°C, but it is preferable that the material is a polymer of a monomer mixture consisting of a non-crosslinkable monomer including a (meth)acrylic acid ester monomer and a crosslinkable monomer.
[0029] The (meth)acrylic acid ester monomer refers to a non-crosslinkable monofunctional (meth)acrylic acid ester having one ethylenically unsaturated group in one molecule. Examples of (meth)acrylic acid ester monomers include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate; (meth)acrylic acid esters of alicyclic alcohols such as cyclohexyl (meth)acrylate and isobornyl (meth)acrylate; (meth)acrylic acid aryl esters such as phenyl (meth)acrylate; and (meth)acrylic acid alkoxyalkyls such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate. These (meth)acrylic acid ester monomers may be used alone or in combination of two or more. Among these, (meth)acrylic acid alkyl esters are preferred, acrylic acid alkyl esters are more preferred, and n-butyl acrylate, isobutyl acrylate, and 2-ethylhexyl acrylate are particularly preferred. Incidentally, (meth)acrylic means acrylic and / or methacrylic.
[0030] The (meth)acrylic acid ester monomer in the non-crosslinkable monomer is preferably used in a proportion of 85 to 100 mass %. If the mass ratio of the (meth)acrylic acid ester monomer is less than 85 mass %, when resin particles are added to the rubber composition, it may not be possible to eliminate the sticky feel of the surface while maintaining a soft feel. The mass proportion of the (meth)acrylic acid ester monomer is more preferably from 90 to 100 mass %, more preferably from 92.5 to 100 mass %, and particularly preferably from 95 to 100 mass %.
[0031] As the non-crosslinking monomer, in addition to the above-mentioned (meth)acrylic acid ester monomer, other non-crosslinking monomers copolymerizable therewith (hereinafter referred to as other non-crosslinking monomers) may be included within a range in which the performance of the resin particles is not deteriorated. Examples of other non-crosslinkable monomers include styrene-based monomers, nitrile-based monomers, carboxyl group-containing monomers, vinyl-based monomers, vinylidene-based monomers, amide group-containing monomers, and maleimide-based monomers. Examples of styrene-based monomers include styrene, p-methylstyrene, α-methylstyrene, etc., examples of nitrile-based monomers include acrylonitrile, methacrylonitrile, etc., examples of carboxyl group-containing monomers include acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, etc., examples of vinyl-based monomers include vinyl acetate, vinyl chloride, vinyl methyl ether, etc., examples of vinylidene-based monomers include vinylidene chloride, etc., examples of amide group-containing monomers include acrylamide, methacrylamide, etc., examples of maleimide-based monomers include N-phenylmaleimide, N-laurylmaleimide, etc. Other monofunctional monomers may be used alone or in combination of two or more. The mass proportion of other non-crosslinkable monomers in the non-crosslinkable monomers is preferably 15 mass % or less, more preferably 10 mass % or less, further preferably 7.5 mass % or less, and particularly preferably 5 mass % or less.
[0032] The monomer mixture is composed of a non-crosslinkable monomer and a crosslinkable monomer, and the mass ratio of the crosslinkable monomer in the monomer mixture is preferably 2 to 5 mass %. Examples of crosslinkable monomers include aromatic divinyl monomers such as divinylbenzene and divinylnaphthalene; and bifunctional or higher (meth)acrylate monomers such as allyl methacrylate, triacrylformal, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, PEG#200 di(meth)acrylate, PEG#600 di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and 2-butyl-2-ethyl 1,3-propanediol di(meth)acrylate. These crosslinkable monomers may be used alone or in combination of two or more. Among these, trimethylolpropane trimethacrylate and ethylene glycol dimethacrylate are preferred, and ethylene glycol dimethacrylate is particularly preferred.
[0033] The crosslinkable monomer is preferably used in an amount of 2 to 5% by mass in the monomer mixture as described above. If the crosslinkable monomer is used in an amount of less than 2% by mass, the resin particles will be easily aggregated when dried due to a low degree of crosslinking, resulting in poor handling. On the other hand, if the crosslinkable monomer is used in an amount of more than 5% by mass, the resin particles will become hard and the soft feel will be lost when added to a rubber composition. The mass proportion of the crosslinkable monomer in the monomer mixture is more preferably from 2.3 to 4.7 mass %, further preferably from 2.6 to 4.4 mass %, and particularly preferably from 3.0 to 4.0 mass %.
[0034] The resin particles can be produced by a conventional method, for example, suspension polymerization, in which a monomer mixture is dispersed in an aqueous dispersion medium and polymerized to produce the resin particles easily. In the suspension polymerization, a polymerization initiator, an electrolyte, a dispersant, a surfactant, etc. are used as necessary.
[0035] The polymerization initiator is preferably an oil-soluble peroxide or azo compound, and specific examples thereof include oil-soluble peroxides such as diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, and dilauroyl peroxide, and oil-soluble azo compounds such as 2,2'-azobisisobutyronitrile and 2,2'-azobis(2,4-dimethylvaleronitrile). Examples of electrolytes include sodium chloride, magnesium chloride, and calcium chloride. Examples of dispersants include poorly water-soluble inorganic compounds such as colloidal silica, calcium phosphate, magnesium hydroxide, and magnesium pyrophosphate, and water-soluble polymers such as polyvinyl alcohol, methyl cellulose, and polyvinylpyrrolidone. Examples of the surfactant include anionic surfactants such as sodium lauryl sulfate and sodium dodecylbenzenesulfonate, nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, sorbitan fatty acid esters, polyoxyethylene alkylamines, and adipic acid-diethanolamine condensates, and amphoteric surfactants such as lauryl dimethylamine oxide and lauryl dimethylaminoacetate betaine. The above polymerization initiators, electrolytes, dispersants, and surfactants can each be used alone or in combination of two or more.
[0036] The polymerization reaction is carried out by dispersing the monomer mixture in an aqueous dispersion medium so as to prepare spherical oil droplets of a predetermined particle size, and then raising the temperature while stirring. Methods for dispersing the monomer mixture in an aqueous dispersion medium include, for example, a method of dispersing using an emulsifying disperser such as a homomixer or a static mixer, a method of dispersing using an ultrasonic disperser, and a method utilizing a membrane emulsification method. The polymerization temperature is preferably 40 to 100°C, and the polymerization time is preferably 1 to 20 hours.
[0037] The rubber composition for studless tires improves the dispersibility of the resin particles in the diene rubber and improves the wear resistance by blending a liquid rubber having a weight-average molecular weight of 1,000 to 100,000 together with the resin particles. The weight-average molecular weight of the liquid rubber is 1,000 to 100,000, preferably 2,000 to 90,000, and more preferably 3,000 to 80,000. If the weight-average molecular weight of the liquid rubber is less than 1,000, it is likely to migrate to other components. If the weight-average molecular weight of the liquid rubber exceeds 100,000, the dispersing effect of the resin decreases. The weight-average molecular weight of the liquid rubber is a standard polystyrene equivalent value obtained by gel permeation chromatography (GPC) measurement using a RI detector with tetrahydrofuran as a solvent.
[0038] The liquid rubber is not particularly limited, but examples thereof include liquid isoprene rubber, liquid butadiene rubber, liquid styrene butadiene rubber, liquid ethylene propylene rubber, liquid nitrile rubber, liquid chloroprene rubber, liquid acrylic rubber, liquid epichlorohydrin rubber, etc. Liquid isoprene rubber, liquid butadiene rubber, and liquid styrene butadiene rubber are preferable.
[0039] The liquid rubber is blended in an amount of 10 parts by mass or more, preferably 12 to 50 parts by mass, more preferably 14 to 40 parts by mass, per 100 parts by mass of diene rubber. If the amount of liquid rubber is less than 10 parts by mass, the dispersibility of the resin particles cannot be improved, and the abrasion resistance cannot be improved. In addition, the mass ratio of the amount of liquid rubber to the amount of resin particles (amount of liquid rubber blended / amount of resin particles blended) is preferably 1 to 100, more preferably 2 to 50. If the mass ratio (amount of liquid rubber blended / amount of resin particles blended) is less than 1, the dispersibility of the resin particles cannot be improved, and the abrasion resistance cannot be improved. In addition, if the mass ratio (amount of liquid rubber blended / amount of resin particles blended) exceeds 50, migration to other components is likely to occur.
[0040] The rubber composition for studless tires can improve the dispersibility of resin particles and improve the wear resistance by blending aromatic modified terpene resin. The aromatic modified terpene resin is blended in an amount of preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, per 100 parts by mass of diene rubber. If the aromatic modified terpene resin is less than 1 part by mass, the effect of improving the dispersibility of resin particles and improving the wear resistance cannot be sufficiently obtained. If the aromatic modified terpene resin is more than 20 parts by mass, the wear resistance deteriorates.
[0041] Aromatic modified terpene resin is obtained by polymerizing terpene and aromatic compound. Examples of terpene include α-pinene, β-pinene, dipentene, limonene, etc. Examples of aromatic compounds include styrene, α-methylstyrene, vinyltoluene, indene, etc. Among them, styrene modified terpene resin is preferred as aromatic modified terpene resin.
[0042] The rubber composition for studless tires may be blended with thermally expandable microcapsules. The thermally expandable microcapsules may be configured such that a thermally expandable substance is encapsulated in a shell material formed of a thermoplastic resin such as polyacrylonitrile. When the thermally expandable microcapsules are heated, the thermally expandable substance encapsulated in the shell material expands to increase the particle size of the shell material, forming a large number of resin-coated bubbles in the tread rubber. Examples of such thermally expandable microcapsules include those manufactured by Expancel AG of Sweden under the trade names "EXPANCEL 091DU-80" or "EXPANCEL 092DU-120" and those manufactured by Matsumoto Yushi Seiyaku Co., Ltd. under the trade names "Microsphere F-85" or "Microsphere F-100". The amount of the thermally expandable microcapsules is not particularly limited, but is preferably 2.5 parts by mass or more, more preferably 3.5 to 20 parts by mass, per 100 parts by mass of diene rubber. By compounding 2.5 parts by mass or more of the thermally expandable microcapsules, the surface of the rubber composition can be appropriately roughened to improve the performance on ice and on snow. If the amount of the thermally expandable microcapsules exceeds 20 parts by mass, there is a risk that the performance on ice, on snow, and on wet roads may be deteriorated.
[0043] The rubber composition for studless tires preferably has a rubber hardness of JIS K6253, durometer type A, at 20° C. of 60 or less, more preferably 40 to 57. By making the rubber hardness 60 or less, high frictional force on ice can be obtained.
[0044] The rubber composition for studless tires preferably has a glass transition temperature of -60°C or lower, more preferably -100 to -62°C. By making the glass transition temperature of the rubber composition for studless tires -60°C or lower, the flexibility of the rubber compound is maintained at low temperatures and the adhesive strength to ice surfaces is increased, making it suitable for use in the tread portion of studless tires. The glass transition temperature is determined by measuring a thermogram by differential scanning calorimetry (DSC) at a heating rate of 20°C / min, and is taken as the midpoint of the transition region.
[0045] The rubber composition for studless tires of the present invention may contain various additives that are generally used in rubber compositions for tires, such as vulcanizing or crosslinking agents, vulcanization accelerators, antioxidants, plasticizers, processing aids, and thermosetting resins, within the range that does not impair the object of the present invention. Furthermore, such additives can be kneaded in a general manner to form a rubber composition, which can then be used for vulcanization or crosslinking. The amount of these additives may be a conventional amount, as long as it does not violate the object of the present invention. The rubber composition for studless tires may be produced by mixing the above-mentioned components using a general rubber kneading machine, such as a Banbury mixer, kneader, roll, etc.
[0046] The rubber composition for studless tires of the present invention is suitable for forming the tread portion of a studless tire. A studless tire having a tread rubber made of the rubber composition for studless tires of the present invention can improve performance on ice and abrasion resistance to levels higher than those of conventional tires.
[0047] The present invention will be further described below with reference to examples, but the scope of the present invention is not limited to these examples. EXAMPLES
[0048] Preparation of resin particles (resin particles-A and B) Resin particles-A An aqueous dispersion medium was prepared by adding and mixing 50 parts by mass of sodium chloride, 0.5 parts by mass of adipic acid-diethanolamine condensate (concentration: 50% by mass) which is a low molecular weight nonionic surfactant, 20 parts by mass of colloidal silica containing 20% by mass of silica active ingredient, and 0.02 parts by mass of ethylenediaminetetraacetic acid tetrasodium salt to 200 parts by mass of ion-exchanged water, and adjusting the pH to 2.8 to 3.2. Separately from this, 97.5 parts by mass of n-butyl acrylate, 2.5 parts by mass of ethylene glycol dimethacrylate, and 3 parts by mass of di-2-ethylhexyl peroxydicarbonate containing 70% active ingredient were mixed and dissolved to prepare an oily mixture. The aqueous dispersion medium and oil mixture obtained above were stirred (8000 rpm x 1 minute) with a TK Homomixer 2.5 type (manufactured by Primix Corporation) to prepare a suspension. This suspension was transferred to a 1.5 liter pressure reactor and substituted with nitrogen, and then the initial reaction pressure was set to 0.2 MPa. Polymerization was carried out for 15 hours at a polymerization temperature of 65°C while stirring at 80 rpm to obtain an aqueous dispersion containing resin particles. The obtained aqueous dispersion containing resin particles was filtered and dried to obtain resin particles-A. The obtained resin particles-A were spherical particles having an average particle size of 25 μm and a glass transition temperature of -45°C.
[0049] Resin particles-B An aqueous dispersion medium was prepared by adding and mixing 50 parts by mass of sodium chloride, 0.5 parts by mass of adipic acid-diethanolamine condensate (concentration: 50% by mass) which is a low molecular weight nonionic surfactant, 30 parts by mass of colloidal silica containing 20% by mass of active silica ingredient, and 0.02 parts by mass of ethylenediaminetetraacetic acid tetrasodium salt to 200 parts by mass of ion-exchanged water, and adjusting the pH to 2.8 to 3.2. Separately from this, 92.5 parts by mass of n-butyl acrylate, 5 parts by mass of ethyl acrylate, 2.5 parts by mass of ethylene glycol dimethacrylate, and 3 parts by mass of di-2-ethylhexyl peroxydicarbonate containing 70% active ingredient were mixed and dissolved to prepare an oily mixture. The aqueous dispersion medium and oil mixture obtained above were stirred (7000 rpm x 1 minute) with a TK Homomixer 2.5 type (manufactured by Primix Corporation) to prepare a suspension. This suspension was transferred to a 1.5 liter pressure reactor and substituted with nitrogen, and then the initial reaction pressure was set to 0.2 MPa. Polymerization was carried out for 15 hours at a polymerization temperature of 65°C while stirring at 80 rpm to obtain an aqueous dispersion containing resin particles. The obtained aqueous dispersion containing resin particles was filtered and dried to obtain resin particles-B. The obtained resin particles-B were spherical particles having an average particle size of 35 μm and a glass transition temperature of -39°C.
[0050] Preparation and evaluation of rubber compositions for studless tires In preparing 14 types of rubber compositions for studless tires (Examples 1 to 9, Comparative Examples 1 to 5) having the common composition shown in Table 2 and compounded with the resin particles shown in Table 1, the components other than sulfur, vulcanization accelerator, and resin particles were kneaded in a 1.7 L Banbury mixer for 5 minutes, and when the temperature reached 145°C, the components were released to form a master batch. Sulfur, vulcanization accelerator, and resin particles were added to the obtained master batch, and the mixture was kneaded with an open roll at 70°C to obtain 14 types of rubber compositions for studless tires. The compounding amounts of the standard recipes shown in Table 2 are expressed as parts by mass relative to 100 parts by mass of the diene rubber shown in Table 1.
[0051] The obtained rubber composition for studless tires was vulcanized at 170°C for 10 minutes using a mold of a specified shape (inner dimensions: length 150 mm, width 150 mm, thickness 2 mm) to prepare a vulcanized rubber test piece. The obtained vulcanized rubber test piece was used to measure the tensile breaking strength and friction performance on ice by the test methods shown below.
[0052] Tensile Break Strength From the obtained vulcanized rubber test pieces, JIS No. 3 dumbbell-shaped test pieces were cut in accordance with JIS K6251. The tensile strength at break was measured in accordance with JIS K6251, and the results are shown in the "Breaking strength" column of Table 1 as an index, with the value of Comparative Example 1 being 100. A higher index value indicates better abrasion resistance.
[0053] Friction performance on ice The obtained vulcanized rubber test piece was attached to a flat cylindrical rubber base and tested using an inside drum type ice friction tester at a measurement temperature of -1.5°C and a load of 5.5kg / cm 2 The coefficient of friction on ice was measured under conditions of a drum rotation speed of 25 km / h. The obtained coefficient of friction on ice was indexed, with the value for Comparative Example 1 being set at 100, and is shown in the "Performance on ice" column. A higher index value indicates a higher coefficient of friction on ice and better performance on ice.
[0054] [Table 1]
[0055] The types of raw materials used in Table 1 are shown below. Natural rubber: RSS#3 Polybutadiene: Polybutadiene rubber Nipol BR1220 manufactured by Nippon Zeon Co., Ltd. Modified butadiene rubber: JSR BR54 Carbon black: Carbon black Seast 6 manufactured by Tokai Carbon Co., Ltd., with a nitrogen adsorption specific surface area of 115 m 2 / g Silica: Nipsil AQ manufactured by Nippon Silica Industry Co., Ltd. Coupling agent: Sulfur-containing silane coupling agent, Si69 by Dexa Resin particles-A and -B: Resin particles obtained by the above-mentioned preparation method Liquid rubber-1: Liquid butadiene rubber with a weight average molecular weight of 30,000, manufactured by Zeon Corporation Liquid rubber-2: Liquid butadiene rubber with a weight average molecular weight of 5000, Kuraray LBR302 Modified terpene resin: Aromatic modified terpene resin, TO-125 manufactured by Yasuhara Chemical Co., Ltd.
[0056] [Table 2]
[0057] The types of raw materials used in Table 2 are shown below. Zinc oxide: Three types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd. Stearic acid: NOF stearic acid beads Anti-aging agent: Flexis 6PPD Aroma oil: Aroma oil made by Fuji Kosan Co., Ltd. Wax: Sannock manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Sulfur: Kinka-in oil-filled fine sulfur manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator: Noccela CZ-G manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0058] As is clear from Table 1, it was confirmed that the rubber compositions for studless tires of Examples 1 to 9 improved the tensile breaking strength and performance on ice beyond conventional levels.
[0059] The rubber composition for studless tires of Comparative Example 2 does not contain resin particles, and therefore the performance on ice cannot be improved. The rubber composition for studless tires of Comparative Example 3 does not contain liquid rubber and is therefore inferior in tensile strength at break. The rubber composition for studless tires in Comparative Example 4 contains less than 10 parts by mass of liquid rubber, and therefore has poor tensile strength at break. The rubber composition for studless tires of Comparative Example 5 has a resin particle content of more than 30 parts by mass, and therefore has poor tensile strength at break.
Claims
1. A rubber composition for studless tires, comprising 100 parts by mass of diene rubber containing 30% by mass or more of polybutadiene and natural rubber, 30 parts by mass or more of a white filler, 0.5 to 30 parts by mass of resin particles, and 10 parts by mass or more of a liquid rubber having a weight average molecular weight of 1,000 to 100,000, wherein the resin particles are made of a polymer of a monomer mixture consisting of a non-crosslinkable monomer containing a (meth)acrylic acid ester monomer and a crosslinkable monomer, the average particle size of the resin particles being 15 to 50 μm, and the glass transition temperature of the resin particles being -50 to -30°C.
2. 2. The rubber composition for studless tires according to claim 1, characterized in that the rubber hardness at 20° C. according to JIS K6253, durometer type A, is 60 or less.
3. 3. The rubber composition for studless tires according to claim 1, wherein the glass transition temperature is −30° C. or lower.
4. A rubber composition for studless tires described in any one of claims 1 to 3, characterized in that the mass proportion of the (meth)acrylic acid ester monomer in the non-crosslinkable monomer is 85 to 100 mass%, and the mass proportion of the crosslinkable monomer in the monomer mixture is 2 to 5 mass%.
5. The rubber composition for studless tires according to any one of claims 1 to 4, characterized in that the diene rubber contains a modified butadiene rubber.
6. The rubber composition for studless tires according to any one of claims 1 to 5, further comprising an aromatic modified terpene resin.
Citation Information
Patent Citations
Studless tire rubber composition
JP2018123209A
Rubber composition for tires, and studless tire
JP2019156951A
Rubber composition and pneumatic tire
JP2020143289A
Rubber composition for tires, and pneumatic tire and studless tire using the same
JP2021091839A