Optical element, laminate, display device, and method for manufacturing optical element

An optical element with an optically anisotropic and isotropic layer formed using liquid crystal compounds and specific convex structures addresses the issue of insufficient blackness in display devices, enhancing black density and reducing unwanted color tints.

JP7579753B2Active Publication Date: 2024-11-08FUJIFILM CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021090278
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-28
Publication Date
2024-11-08
Estimated Expiration
2041-05-28

AI Technical Summary

Technical Problem

Existing display devices, such as organic EL display devices, suffer from insufficient blackness during black display due to observed reflected light when viewed from the front, necessitating improvements in optical elements used in combination with polarizers.

Method used

The use of an optical element comprising an optically anisotropic layer and an optically isotropic member with a refractive index difference of 0.08 or less, where the isotropic member has convex portions projecting opposite to the anisotropic layer, formed using liquid crystal compounds, and arranged periodically with specific dimensions and shapes to minimize interfacial reflection.

Benefits of technology

The solution provides enhanced black density and reduces bluish tint when viewed from the front in black display, while suppressing bluish tint from oblique views in white display.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579753000016
    Figure 0007579753000016
  • Figure 0007579753000017
    Figure 0007579753000017
  • Figure 0007579753000018
    Figure 0007579753000018
Patent Text Reader

Abstract

To provide an optical element, in which when a polarizing plate obtained by combining with a polarizer is applied to a display element, well-defined black at visual recognition time from a front direction in a black display is given, a laminate, a display device, and a manufacturing method of the optical element.SOLUTION: An optical element comprises: an optical anisotropy layer; and an optical isotropic member. In the optical element, the optical anisotropy layer and the optical isotropic member contact to each other, an absolute value of a difference between an average refractive index of the optical anisotropy layer and a refractive index of the optical isotropic member is less than or equal to 0.08, and the optical isotropic member has a protrusion part that protrudes to an opposite side of an optical anisotropy layer side.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical element, a laminate, a display device, and a method for manufacturing an optical element. [Background technology]

[0002] 2. Description of the Related Art Known examples of display devices that display images include organic electroluminescence (organic EL) display devices that display images by causing a light-emitting layer to emit light. Display devices such as organic EL display devices may include various optical elements. For example, in Patent Document 1, a circular polarizing plate having a polarizing member and a phase difference member, and an optical sheet having a plurality of first portions arranged in a first direction and each extending in a second direction intersecting the first direction, and second portions arranged alternately with the first portions along the first direction, are included in the display device. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-187261 A Summary of the Invention [Problem to be solved by the invention]

[0004] On the other hand, the inventors have investigated the characteristics of the display device described in Patent Document 1 and found that when the display is set to black and viewed from the front, reflected light is observed, the blackness is not necessarily sufficient, and further improvement is required.

[0005] An object of the present invention is to provide an optical element which, when a polarizing plate obtained in combination with a polarizer is used in a display element, exhibits good black clarity when viewed from the front in black display. Another object of the present invention is to provide a method for producing a laminate, a display device, and an optical element. [Means for solving the problem]

[0006] As a result of extensive investigation into the problems of the conventional techniques, the present inventors have found that the above-mentioned problems can be solved by the following configuration.

[0007] (1) an optically anisotropic layer; an optically isotropic member; The optically anisotropic layer is in contact with the optically isotropic member, the absolute value of the difference between the average refractive index of the optically anisotropic layer and the refractive index of the optically isotropic member is within 0.08; The optically isotropic member is an optical element having a convex portion protruding on the side opposite to the optically anisotropic layer. (2) The optical element according to (1), wherein the optically anisotropic layer and the optically isotropic member are both formed using a liquid crystal compound. (3) The optical element according to (1) or (2), wherein the optically anisotropic layer and the optically isotropic member are both formed using the same liquid crystal compound. (4) The optical element according to any one of (1) to (3), wherein the optically anisotropic layer is a λ / 4 plate. (5) The optical element according to any one of (1) to (4), wherein a plurality of convex portions are periodically arranged. (6) The optical element according to any one of (1) to (5), wherein the intervals between the multiple convex portions are 0.2 to 20 μm. (7) The optical element according to any one of (1) to (6), wherein the convex portions are arranged in a dot pattern or a stripe pattern. (8) The optical element according to any one of (1) to (7), wherein the width of the convex portions gradually increases from the side opposite the optically anisotropic layer side to the optically anisotropic layer side of the convex portions. (9) A laminate comprising the optical element according to any one of (1) to (8) and an adhesive layer disposed on the optical isotropic member side of the optical element. (10) An optical display comprising a polarizer, the optical element according to any one of (1) to (8), and a display element, in this order; A display device, in which an optically anisotropic layer in an optical element is disposed on the polarizer side. (11) Step 1 of forming a composition layer containing a liquid crystal compound having a polymerizable group on a substrate; Step 2 of subjecting the composition layer to a heat treatment to align the liquid crystal compound in the composition layer; After the step 2, a step 3 of irradiating the composition layer with light under conditions of an oxygen concentration of 1% by volume or more; Step 4 of pressing a mold having a concave-convex structure on its surface against the surface of the composition layer opposite the substrate side to transfer the concave-convex structure of the mold to the composition layer; and step 5 of subjecting the composition layer to a curing treatment to form an optical element having an optically isotropic member having an optically anisotropic layer and a convex portion protruding from the substrate side to the side opposite to the optically anisotropic layer side, A method for producing an optical element, which satisfies any one of requirements 1 to 4 described below. Effect of the Invention

[0008] According to the present invention, it is possible to provide an optical element which, when a polarizing plate obtained in combination with a polarizer is used in a display element, exhibits good black crispness when viewed from the front in black display. The present invention also provides methods for producing a laminate, a display device, and an optical element. [Brief description of the drawings]

[0009] [Figure 1] 1 shows a schematic cross-sectional view of one embodiment of an optical element of the present invention. [Diagram 2] 2 shows a plan view of a portion of the optical element shown in FIG. [Diagram 3] FIG. 2 shows a plan view of another embodiment of the optical element of the present invention. [Figure 4] 2 shows a schematic cross-sectional view of another embodiment of the optical element of the present invention. [Diagram 5] 5 shows a plan view of a portion of the optical element shown in FIG. [Figure 6] FIG. 11 is a cross-sectional view of a composition layer for explaining step 2. [Figure 7] FIG. 11 is a cross-sectional view of a composition layer for explaining step 3. [Figure 8] FIG. 4 is a cross-sectional view of a composition layer for explaining step 4. [Figure 9]FIG. 4 is a cross-sectional view of a composition layer for explaining step 4. [Figure 10] FIG. 2 is a cross-sectional view illustrating an optical element. [Figure 11] FIG. 11 is a cross-sectional view of a composition layer for explaining step 2. [Figure 12] FIG. 11 is a cross-sectional view of a composition layer for explaining step 3. [Figure 13] FIG. 2 is a cross-sectional view of a composition layer for illustrating a heat treatment. [Figure 14] FIG. 2 is a schematic diagram of a graph plotting the relationship between the helical twisting power (HTP) (μm−1)×concentration (mass%) and the light irradiation dose (mJ / cm2) for each of chiral agent A and chiral agent B. [Figure 15] FIG. 1 is a schematic diagram of a graph plotting the relationship between the weighted average helical twisting power (μm−1) and the light irradiation dose (mJ / cm2) in a system in which chiral agent A and chiral agent B are used in combination. [Figure 16] FIG. 11 is a cross-sectional view of a composition layer for explaining step 3. [Figure 17] FIG. 2 is a cross-sectional view illustrating an optical element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. In this specification, a numerical range expressed using "to" means a range including the numerical values ​​before and after "to" as the lower and upper limits. First, the terms used in this specification will be described.

[0011] The slow axis is defined at a wavelength of 550 nm unless otherwise specified.

[0012] In the present invention, Re(λ) and Rth(λ) respectively represent the in-plane retardation and the retardation in the thickness direction at a wavelength λ, which is set to 550 nm unless otherwise specified. In the present invention, Re(λ) and Rth(λ) are values ​​measured at a wavelength λ using an AxoScan (manufactured by Axometrics). By inputting the average refractive index ((nx+ny+nz) / 3) and the film thickness (d(μm)) into AxoScan, Slow axis direction (°) Re(λ)=R0(λ) Rth(λ)=((nx+ny) / 2-nz)×d is calculated. Note that R0(λ) is displayed as a numerical value calculated by AxoScan, but it means Re(λ).

[0013] In this specification, the refractive indices nx, ny, and nz are measured using an Abbe refractometer (NAR-4T, manufactured by Atago Co., Ltd.) and a sodium lamp (λ=589 nm) as a light source. In addition, when measuring wavelength dependency, it can be measured using a multi-wavelength Abbe refractometer DR-M2 (manufactured by Atago Co., Ltd.) in combination with an interference filter. In addition, values ​​from the Polymer Handbook (JOHN WILEY & SONS, INC.) and catalogs of various optical films can be used. The average refractive index values ​​of major optical films are shown below as examples: cellulose acylate (1.48), cycloolefin polymer (1.52), polycarbonate (1.59), polymethyl methacrylate (1.49), and polystyrene (1.59).

[0014] In this specification, the term "light" refers to actinic rays or radiation, such as the bright line spectrum of a mercury lamp, far ultraviolet rays represented by an excimer laser, extreme ultraviolet rays (EUV light: extreme ultraviolet), X-rays, ultraviolet rays, and electron beams (EB), etc. Among these, ultraviolet rays are preferred.

[0015] In this specification, "visible light" refers to light having a wavelength of 380 to 780 nm. In addition, in this specification, unless otherwise specified, the measurement wavelength is 550 nm.

[0016] In the optical element of the present invention, an optically anisotropic layer and an optically isotropic member are arranged in contact with each other, and since the refractive index difference between the two is small, interfacial reflection between the two is suppressed, resulting in the effects of the present invention. In addition, when a polarizing plate obtained by combining the optical element and polarizer of the present invention is applied to a display element, the blackness when viewed from the front in black display is superior, which will hereinafter be simply referred to as "the effect of the present invention is superior." As described below, when the convex portions have a predetermined structure and arrangement (for example, when the convex portions have a predetermined size or when the interval between the convex portions is within a predetermined range), when a polarizing plate obtained by combining the light-emitting element of the present invention with a polarizer is applied to a display element, the occurrence of a bluish tint when viewed from an oblique direction in white display is suppressed. Hereinafter, the fact that the occurrence of a bluish tint when viewed from an oblique direction in white display as described above is further suppressed is also simply referred to as "the occurrence of a bluish tint is further suppressed."

[0017] <Optical elements> An embodiment of the optical element of the present invention will be described below with reference to the drawings. Fig. 1 shows a schematic cross-sectional view of one embodiment of the optical element of the present invention. Fig. 2 shows a plan view of a part of the optical element shown in Fig. 1. The plan view is a view of a part of the optical element in Fig. 1 seen from above. Fig. 1 is also a cross-sectional view taken along line AA in Fig. 2. For the sake of explanation, the left-right direction in Fig. 2 is taken as the X-axis direction, and the up-down direction is taken as the Y-axis direction. The optical element 10A has an optically anisotropic layer 12 and an optically isotropic member 14A. The optically anisotropic layer 12 and the optically isotropic member 14A are in direct contact with each other. In addition, an uneven structure is formed on the surface of the optically isotropic member 14A opposite to the optically anisotropic layer 12 side, and a plurality of dot-shaped convex portions 16A protruding toward the opposite side to the optically anisotropic layer 12 side are formed. More specifically, the optically isotropic member 14A has a base portion 18A and dot-shaped convex portions 16A arranged on the base portion 18A. The convex portions 16A are in the shape of a truncated cone, and the convex portions 16A are in the shape of a circle in a plan view. There are a plurality of convex portions 16A, and the plurality of convex portions 16A are arranged in a hexagonal close-packed manner. That is, the plurality of convex portions 16A are arranged periodically. The base portion 18A is continuously connected along the surface direction and is in contact with the optically anisotropic layer 12.

[0018] Although only eight convex portions 16A are shown in FIG. 2, FIG. 2 is a plan view of a portion of the optical element, and eight or more convex portions 16A are formed on the optical element. In Fig. 1, the convex portion 16A is in the shape of a truncated cone, but the present invention is not limited to this, and may be in the shape of a hemisphere, a cone, an inverted truncated cone, or a pyramid. Note that the inverted truncated cone shape corresponds to a shape in which the width of the upper base is larger than the width of the lower base, unlike the shape in Fig. 1. In addition, in FIG. 1, the convex portion 16A has a circular shape in a plan view, but the present invention is not limited to this embodiment, and may have, for example, any of a polygonal shape, an elliptical shape, and an irregular shape. In Fig. 1, the convex portion 16A is a trapezoid whose upper base is smaller than its lower base in a cross-sectional view. That is, the width of the convex portion 16A gradually increases from the side opposite to the optically anisotropic layer 12 side of the convex portion 16A toward the optically anisotropic layer 12 side (toward the direction of the white arrow in the figure). More specifically, as shown in Fig. 2, the width WA1 (diameter of the upper base) of the upper base of the convex portion 16A is smaller than the width WA2 (diameter of the lower base) of the lower base of the convex portion 16A, and the width of the convex portion 16A gradually increases from the upper base toward the lower base. The cross-sectional shape of the protrusion 16A may be a trapezoid whose legs are not necessarily straight but may be curved. When the protrusions 16A have the above structure, the occurrence of blue tinge is further suppressed.

[0019] The width WA1 of the upper base of the truncated cone-shaped protrusion 16A shown in FIG. 2 is not particularly limited, and is preferably 0.1 to 20.0 μm in terms of providing better effects of the present invention, and is more preferably 0.2 to 20.0 μm in terms of further suppressing the occurrence of blue tinge, and is even more preferably 0.2 to 5.0 μm. The width WA2 of the lower base of the truncated convex portion 16A is not particularly limited, and is preferably 0.1 to 20.0 μm in order to obtain a better effect of the present invention, and is more preferably 0.2 to 20.0 μm in order to further suppress the occurrence of blue tinge, and is even more preferably 0.2 to 5.0 μm. As described above, it is preferable that the width WA1 of the upper base of the protrusion 16A is smaller than the width WA2 of the lower base, and it is preferable that the width of the protrusion 16A gradually increases from the upper base to the lower base.

[0020] The height HA1 of the protrusions 16A is not particularly limited, and is preferably 0.1 to 20.0 μm in terms of providing better effects of the present invention, and is more preferably 0.2 to 20.0 μm, and even more preferably 0.2 to 5.0 μm in terms of further suppressing the occurrence of blue tinge. The thickness HA2 of the base portion 18A (the total thickness of the optically isotropic member 14A minus the height of the convex portion 16A) is not particularly limited, and is preferably 0.1 to 20.0 μm in order to provide a better effect of the present invention, and is more preferably 0.2 to 20.0 μm in order to further suppress the occurrence of blue tinge, and is even more preferably 0.2 to 5.0 μm. The period PA of the convex portions 16A (the distance between adjacent convex portions) is not particularly limited, and is preferably 0.1 to 20.0 μm in order to obtain a better effect of the present invention, and is more preferably 0.2 to 5.0 μm in order to further suppress the occurrence of blue tinge, and is even more preferably 0.2 to 5.0 μm. The ratio of the height HA1 of the protrusions 16A to the period PA of the protrusions 16A is not particularly limited, and is preferably 0.005 to 200, more preferably 0.01 to 100, and even more preferably 0.1 to 10, in terms of better effects of the present invention.

[0021] In FIG. 1, the truncated cone-shaped protrusions 16A are arranged in a hexagonal close-packed pattern, but the present invention is not limited to this embodiment. For example, as shown in FIG. 3, the truncated cone-shaped protrusions 16A may be arranged in a square lattice pattern or randomly.

[0022] 1, the embodiment of the convex portion 16A having a truncated cone shape has been described, but the present invention is not limited to this embodiment, and the convex portions may be arranged in a stripe pattern. This embodiment will be described in detail below. Fig. 4 shows a schematic cross-sectional view of another example of the optical element of the present invention. Fig. 5 shows a plan view of a part of the optical element shown in Fig. 4. The plan view is a view of a part of the optical element in Fig. 4 seen from above. Fig. 4 is also a cross-sectional view taken along line BB in Fig. 5. For the sake of explanation, the left-right direction in Fig. 5 is taken as the X-axis direction, and the up-down direction is taken as the Y-axis direction.

[0023] The optical element 10B has an optically anisotropic layer 12 and an optically isotropic member 14B. The optically anisotropic layer 12 and the optically isotropic member 14B are in direct contact with each other. In addition, an uneven structure is formed on the surface of the optically isotropic member 14B opposite to the optically anisotropic layer 12 side, and the convex portions 16B are arranged in a stripe pattern. More specifically, the optically isotropic member 14B has a base portion 18B and convex portions 16B arranged in a stripe pattern on the base portion 18B. The convex portions 16B extend in the Y direction and are periodically arranged in a direction (X direction) perpendicular to the extending direction. The base portion 18B is continuously connected along the surface direction and is in contact with the optically anisotropic layer 12.

[0024] Although only three convex portions 16B are shown in FIG. 5, FIG. 5 is a plan view of a portion of the optical element, and three or more convex portions 16B are formed on the optical element. As shown in FIG. 4, the shape of the protrusion 16B in a cross section perpendicular to the extending direction is trapezoidal, but the present invention is not limited to this form, and the shape may be semicircular. In Fig. 4, the convex portion 16B is a trapezoid whose upper base is smaller than its lower base in a cross-sectional view. That is, the width of the convex portion 16B gradually increases from the side opposite to the optically anisotropic layer 12 side of the convex portion 16B toward the optically anisotropic layer 12 side (toward the direction of the white arrow in the figure). More specifically, as shown in Fig. 5, the width WB1 (diameter of the upper base) of the upper base of the convex portion 16B is smaller than the width WB2 (diameter of the lower base) of the lower base of the convex portion 16B, and the width of the convex portion 16B gradually increases from the upper base toward the lower base. The cross-sectional shape of the protrusion 16B may be a trapezoid whose legs are not necessarily straight but may be curved. When the protrusions 16B have the above-described structure, the occurrence of blue tinge is further suppressed.

[0025] The width WB1 of the upper base of the protrusion 16B having a trapezoidal cross section as shown in FIG. 5 is not particularly limited, and is preferably in the same range as the width WA1 described above. The width WB2 of the lower base of the truncated cone-shaped protrusion 16B is not particularly limited, and is preferably in the same range as the width WB2 described above. As described above, it is preferable that the width WB1 of the upper base of the protrusion 16B is smaller than the width WB2 of the lower base, and it is preferable that the width of the protrusion 16B gradually increases from the upper base to the lower base. The height HB1 of the protrusion 16B is not particularly limited, and is preferably in the same range as the height HA1 described above. The thickness HB2 of the base portion 18B (the total thickness of the optically isotropic member 14B minus the height of the convex portion 16B) is not particularly limited, and is preferably in the same range as the above-mentioned height HA2. The period PB of the protrusions 16B is not particularly limited, and is preferably in the same range as the period PB described above. The ratio of the height HB1 of the protrusions 16A to the period PB of the protrusions 16A is not particularly limited, and is preferably in the same range as the ratio of the height HA1 to the period PA described above.

[0026] 1 and 4, a configuration in which base portion 18A and base portion 18B are provided has been described, but the present invention is not limited to this configuration, and the optically isotropic member may be composed of only a plurality of convex portions.

[0027] In the optical element of the present invention, the optically anisotropic layer and the optically isotropic member are in contact with each other. In particular, it is preferable that the optically anisotropic layer and the optically isotropic member are in contact with each other along the thickness direction of the optical element, and more specifically, it is preferable that one of the two main surfaces of the optically isotropic member is in contact with the main surface on which the concave-convex structure is not arranged, as shown in Figs. 1 and 4.

[0028] In the optical element of the present invention, the absolute value of the difference between the average refractive index of the optically anisotropic layer and the refractive index of the optically isotropic member is 0.08 or less, and in terms of the effect of the present invention being more excellent, it is preferably 0.06 or less, and more preferably 0.04 or less. The lower limit is not particularly limited, but may be 0. The average refractive index of an optically anisotropic layer is the arithmetic average of the refractive index in the in-plane direction in which the refractive index of the optically anisotropic layer is maximum and the refractive index in the direction perpendicular to the in-plane direction in which the refractive index of the optically anisotropic layer is maximum. A method for measuring the average refractive index of the optically anisotropic layer includes, for example, removing the optically isotropic member of the optical element by etching to expose the optically anisotropic layer, and then using an Abbe refractometer with a polarizer, measuring the refractive index in the direction in which the in-plane refractive index of the optically anisotropic layer is maximized and the refractive index in the direction perpendicular to the direction in which the in-plane refractive index is maximized, and calculating the arithmetic average of the obtained values ​​to determine the average refractive index of the optically anisotropic layer. Furthermore, the refractive index of an optically isotropic member can be measured by scraping off a portion of the optically isotropic member to produce a powder, and then immersing the powder in a solvent with a refractive index different from that of the powder to observe the Becke lines (the so-called Becke line method) to determine the refractive index. The above average refractive index and refractive index are measured at a temperature of 23° C. and a wavelength of 589 nm. As described below, when the optically anisotropic layer has multiple regions along the thickness direction in which the liquid crystal compound has different orientation states, the average refractive index of the region in contact with the optically isotropic member is measured and used as the average refractive index of the optically anisotropic layer.

[0029] The method for adjusting the range of the absolute value of the difference between the average refractive index of the optically anisotropic layer and the refractive index of the optically isotropic member is not particularly limited, and examples thereof include a method of adjusting the type of material constituting the optically anisotropic layer and the type of material constituting the optically isotropic member, and a method of forming the optically anisotropic layer and the optically isotropic member using the same material. As described later, both the optically anisotropic layer and the optically isotropic member may be formed using a liquid crystal compound. Therefore, in order to set the absolute value of the difference between the average refractive index of the optically anisotropic layer and the refractive index of the optically isotropic member within the above-mentioned range, it is preferable that both the optically anisotropic layer and the optically isotropic member are layers formed using the same liquid crystal compound.

[0030] The optically anisotropic layer and the optically isotropic member will be described in more detail below.

[0031] <Optical anisotropic layer> An optically anisotropic layer is a layer that exhibits optical anisotropy. Examples of optically anisotropic layers include layers in which at least two of nx, ny, and nz are different. Here, nx represents the refractive index in a direction perpendicular to the thickness direction of the optically anisotropic layer (in-plane direction) and giving the maximum refractive index. ny represents the refractive index in an in-plane direction of the optically anisotropic layer and perpendicular to the direction of nx. nz represents the refractive index in the thickness direction of the optically anisotropic layer. Examples of optically anisotropic layers include a λ / 4 plate, a λ / 2 plate, a layer having a fixed cholesteric liquid crystal phase, and a layer having a fixed hybrid alignment phase. A λ / 4 plate is preferred in that it provides better effects for the present invention.

[0032] A λ / 4 plate is a plate that has the function of converting linearly polarized light of a certain wavelength into circularly polarized light (or circularly polarized light into linearly polarized light). More specifically, it is a plate that exhibits an in-plane retardation Re of λ / 4 (or an odd multiple thereof) at a certain wavelength λ nm. The in-plane retardation (Re(550)) of the λ / 4 plate at a wavelength of 550 nm may have an error of about 25 nm around the ideal value (137.5 nm), and is preferably 110 to 160 nm, and more preferably 120 to 150 nm, for example. Moreover, a λ / 2 plate refers to an optically anisotropic film in which the in-plane retardation Re(λ) at a specific wavelength λ nm satisfies Re(λ)≒λ / 2. This formula may be achieved at any wavelength in the visible light range (e.g., 550 nm). In particular, it is preferable that the in-plane retardation Re(550) at a wavelength of 550 nm satisfies the following relationship: 210nm≦Re(550)≦300nm

[0033] The material constituting the optically anisotropic layer is not particularly limited, and includes liquid crystal compounds and polymers, and liquid crystal compounds are preferred in terms of the superior effect of the present invention. In particular, the optically anisotropic layer is preferably a layer formed using a liquid crystal compound, and more preferably a layer formed using a liquid crystal compound having a polymerizable group.

[0034] The type of liquid crystal compound is not particularly limited. In general, liquid crystal compounds can be classified into rod-shaped type (rod-shaped liquid crystal compounds) and disk-shaped type (discotic liquid crystal compounds) based on their shape. Furthermore, liquid crystal compounds can be classified into low molecular type and polymer type. Polymer generally refers to a compound with a degree of polymerization of 100 or more (Polymer Physics, Phase Transition Dynamics, Masao Doi, page 2, Iwanami Shoten, 1992). In the present invention, any liquid crystal compound can be used, but it is preferable to use rod-shaped liquid crystal compounds or discotic liquid crystal compounds, and it is more preferable to use rod-shaped liquid crystal compounds. Two or more rod-shaped liquid crystal compounds, two or more discotic liquid crystal compounds, or a mixture of rod-shaped liquid crystal compounds and discotic liquid crystal compounds may be used. Examples of the rod-like liquid crystal compound include the liquid crystal compounds described in claim 1 of JP-A-11-513019 and in paragraphs 0026 to 0098 of JP-A-2005-289980. Examples of discotic liquid crystal compounds include those described in paragraphs 0020 to 0067 of JP-A No. 2007-108732 and paragraphs 0013 to 0108 of JP-A No. 2010-244038.

[0035] The liquid crystal compound preferably has a polymerizable group. That is, the liquid crystal compound is preferably a polymerizable liquid crystal compound. When the liquid crystal compound has a polymerizable group, the alignment state of the liquid crystal compound can be easily fixed by a curing treatment described later. The type of polymerizable group possessed by the liquid crystal compound is not particularly limited, and is preferably a functional group capable of an addition polymerization reaction, more preferably a polymerizable ethylenically unsaturated group or a ring-polymerizable group, and further preferably a (meth)acryloyl group, a vinyl group, a styryl group, or an allyl group. The number of polymerizable groups that the liquid crystal compound has is not particularly limited, but is preferably at least 2. The upper limit is not particularly limited, but is often 10 or less.

[0036] The liquid crystal compound may be a liquid crystal compound exhibiting either forward wavelength dispersion or reverse wavelength dispersion, and a liquid crystal compound exhibiting reverse wavelength dispersion is preferred, and a liquid crystal compound having two or more polymerizable groups and exhibiting reverse wavelength dispersion is more preferred. In this specification, the term "liquid crystal compound exhibiting reverse wavelength dispersion" refers to a compound that satisfies the relationship between the following formulas (A) and (B) when the in-plane retardation (Re) value at a specific wavelength (visible light range) of an optically anisotropic film prepared using this compound is measured. Formula (A) Re(450) / Re(550)<1.00 Formula (B) Re(650) / Re(550)≧1.00 Re(450) represents the in-plane retardation of the optically anisotropic film at a wavelength of 450 nm, Re(550) represents the in-plane retardation of the optically anisotropic film at a wavelength of 550 nm, and Re(650) represents the in-plane retardation of the optically anisotropic film at a wavelength of 650 nm. In this specification, the term "liquid crystal compound exhibiting normal wavelength dispersion" refers to a compound that satisfies the relationship between the following formulas (C) and (D) when the in-plane retardation (Re) value at a specific wavelength (visible light range) of an optically anisotropic film prepared using this compound is measured. Formula (C) Re(450) / Re(550)≧1.00 Formula (D) Re(650) / Re(550)<1.00

[0037] As described above, the optically anisotropic layer is preferably a layer formed using a liquid crystal compound having a polymerizable group, and more preferably a layer in which the orientation state of a liquid crystal compound having a polymerizable group is fixed. The orientation state that the liquid crystal compound having a polymerizable group can take is not particularly limited, and examples thereof include homogeneous orientation, homeotropic orientation, twisted orientation, cholesteric orientation, hybrid orientation (orientation in which the tilt angle of the liquid crystal compound changes continuously from one surface to the other surface), and tilted orientation (orientation in which the tilt angle of the liquid crystal compound is constant from one surface to the other surface). The twisted orientation refers to an orientation state in which the liquid crystal compound is twisted with the thickness direction as the axis of rotation, and when the liquid crystal compound is twisted and has a predetermined tilt angle (tilt angle is greater than 0°), it corresponds to a twisted hybrid orientation. In this specification, the twisted orientation corresponds to an embodiment in which the twist angle of the liquid crystal compound is less than 360°, and the cholesteric orientation corresponds to an embodiment in which the twist angle of the liquid crystal compound is 360° or more. The "fixed" state is the most typical and preferred state in which the alignment of the liquid crystal compound is maintained, but is not limited thereto. Specifically, it is more preferred that the layer has no fluidity and the alignment is not changed by an external field or force in a temperature range of usually 0 to 50°C, or in a more severe condition of -30 to 70°C, and that the fixed alignment can be stably maintained.

[0038] The optically anisotropic layer may have a plurality of regions in which the liquid crystal compound has a different alignment state along the thickness direction. In particular, it is preferable that the optically anisotropic layer has a plurality of regions in which the liquid crystal compound has a different alignment state along the thickness direction, and the liquid crystal compound in each region is fixed. For example, the optically anisotropic layer may have, along the thickness direction, a region in which the liquid crystal compound is fixed in a homogeneous alignment state and a region in which the liquid crystal compound is fixed in a twisted alignment state.

[0039] The thickness of the optically anisotropic layer is not particularly limited, but is preferably from 0.1 to 10.0 μm, and more preferably from 0.5 to 5.0 μm.

[0040] The method for producing the optically anisotropic layer will be described in detail later.

[0041] <Optical isotropic material> The optically isotropic member is a layer that exhibits optical isotropy. The method for identifying an optically isotropic member is as follows. First, the optically isotropic member, which is the object of measurement, is cut along one in-plane direction (hereinafter also referred to as "direction D1") of the optically isotropic member to cut out a thin-film-shaped (approximately 2 μm thick) slice sample 1. If the direction D1 is the x-direction, the in-plane direction perpendicular to the direction D1 is the y-direction, and the thickness direction of the object of measurement is the z-direction, the main surface of the slice sample 1 corresponds to the xz-plane of the object of measurement. Furthermore, the object of measurement is cut along the in-plane direction perpendicular to the direction D1 to cut out a thin-film-shaped (approximately 2 μm thick) slice sample 2. The main surface of the slice sample 2 corresponds to the yz-plane of the object of measurement. Furthermore, the object of measurement is cut along the in-plane direction (hereinafter also referred to as "direction D2") that is 45 degrees to the direction D1 to cut out a thin-film-shaped (approximately 2 μm thick) slice sample 3. Furthermore, the measurement object is cut along a direction within a plane perpendicular to the direction D2 to cut out a thin-film-like slice sample 4 (having a thickness of about 2 μm). Next, one of the two principal surfaces of each of the obtained section samples (section samples 1 to 4) was placed facing a cover glass and fixed with an adhesive. Each section sample was observed under crossed Nicols conditions using a polarizing microscope, and the retardation per 1 μm of thickness was measured by the Senarmont method using light with a wavelength of 546 nm. If the retardation per 1 μm of thickness in any of the section samples was 10 nm or less, the object to be measured was determined to be optically isotropic, in other words, the object to be measured was determined to be an optically isotropic member. The specific measurement method of the Senarmont method is to first set a GIF filter (wavelength 546 nm) with the polarizer and analyzer of the polarizing microscope at 0° (crossed Nicols), and rotate the cover glass on which the section sample is fixed so that the part of the section sample to be observed is the brightest. Then, set the Senarmont compensator, rotate the analyzer, and read the rotation angle θ of the analyzer at which the part of the section sample to be observed is the darkest. Retardation (Re) is calculated using the formula Re = (546 nm x θ) / 180.

[0042] The material constituting the optically isotropic member is not particularly limited, and examples thereof include liquid crystal compounds and polymers, and liquid crystal compounds are preferred in that the effects of the present invention are more excellent. In particular, the optically isotropic member is preferably a layer formed using a liquid crystal compound, and more preferably a layer formed using a liquid crystal compound having a polymerizable group. The type of liquid crystal compound used to form the optically isotropic member is the same as the type of liquid crystal compound used to form the optically anisotropic layer. As a method for forming an optically isotropic member using a liquid crystal compound, a method in which a liquid crystal compound in an isotropic phase state is fixed, as will be described later, can be mentioned.

[0043] As described above, the optically isotropic member is preferably a member formed using a liquid crystal compound having a polymerizable group, and more preferably a member formed by fixing a liquid crystal compound having a polymerizable group in an isotropic phase state.

[0044] The thickness of the optically isotropic member (the distance from the surface of the optically isotropic member where there are no convex portions to the tip of the convex portion) is not particularly limited, but is preferably 0.1 to 40 μm, and more preferably 0.4 to 10 μm.

[0045] The method for producing the optically isotropic member will be described in detail later.

[0046] <Method of manufacturing optical elements> The method for producing the optical element of the present invention is not particularly limited, and the element can be produced by combining known methods. Among these, a production method including the following steps 1 to 5 and satisfying any one of requirements 1 to 4 is preferred from the viewpoint of efficient production of the optical element of the present invention. Step 1: Forming a composition layer containing a liquid crystal compound having a polymerizable group on a substrate Step 2: A step of subjecting the composition layer to a heat treatment to align the liquid crystal compound in the composition layer. Step 3: After step 2, a step of irradiating the composition layer with light under conditions of an oxygen concentration of 1% by volume or more. Step 4: A step of pressing a mold having a concave-convex structure on its surface against the surface of the composition layer opposite the substrate side to transfer the concave-convex structure of the mold to the composition layer. Step 5: A step of subjecting the composition layer to a heat treatment to harden the liquid crystal compound, and forming an optical element having an optically isotropic member having an optically anisotropic layer and a convex portion protruding from the substrate side to the side opposite to the optically anisotropic layer side. Requirement 1: Step 4 is carried out under heating conditions equal to or higher than the phase transition temperature from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer. Requirement 2: Step 5 is carried out under heating conditions at or above the phase transition temperature from a liquid crystal phase to an isotropic phase of the composition constituting the composition layer. Requirement 3: Between steps 3 and 4, there is further included a step 6 of heating the composition layer to a temperature equal to or higher than the phase transition temperature from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer. Requirement 4: Between steps 4 and 5, a step 7 of heating the composition layer to a temperature equal to or higher than the phase transition temperature from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer is further included. Steps 1 to 5 will be described in detail below. In the following explanation, an embodiment that satisfies requirement 1 will first be described.

[0047] (Process 1) Step 1 is a step of forming a composition layer containing a liquid crystal compound having a polymerizable group on a substrate. By carrying out this step, a composition layer to be subjected to a light irradiation treatment described later is formed. In the following, first, the materials used in this process will be described in detail, and then the process procedure will be described in detail.

[0048] [Liquid crystal compounds having polymerizable groups] The composition layer contains a liquid crystal compound having a polymerizable group. The liquid crystal compound having a polymerizable group is as described above.

[0049] The content of the liquid crystal compound in the composition layer is not particularly limited, but is preferably 60% by mass or more, more preferably 70% by mass or more, based on the total mass of the composition layer, in terms of ease of controlling the alignment state of the liquid crystal compound. The upper limit is not particularly limited, but is preferably 99% by mass or less, more preferably 97% by mass or less.

[0050] [Other ingredients] The composition layer may contain other components in addition to the liquid crystal compound having a polymerizable group.

[0051] The composition layer may contain, for example, a photosensitive chiral agent whose helical twisting power changes upon irradiation with light. By containing the photosensitive chiral agent in the composition layer, as described below, it is possible to form a region in which liquid crystal compounds in a twisted or cholesteric orientation are fixed. The helical twisting power (HTP) of a chiral agent is a factor indicating the helical orientation ability represented by the following formula (A). Formula (A) HTP = 1 / (helix pitch length (unit: μm) × concentration of chiral agent relative to liquid crystal compound (mass%)) [μm -1 ] The helical pitch length refers to the length of the pitch P (=helical period) of the helical structure of a cholesteric liquid crystal phase, and can be measured by the method described on page 196 of Liquid Crystal Handbook (published by Maruzen Co., Ltd.).

[0052] The photosensitive chiral agent (hereinafter, simply referred to as "chiral agent A") whose helical twisting power changes upon irradiation with light may be liquid crystalline or non-liquid crystalline. Generally, chiral agent A often contains an asymmetric carbon atom. Note that chiral agent A may be an axially asymmetric compound or a planar asymmetric compound that does not contain an asymmetric carbon atom.

[0053] The chiral agent A may be a chiral agent whose helical twisting power increases or decreases upon irradiation with light, and is preferably a chiral agent whose helical twisting power decreases upon irradiation with light. In this specification, "increase and decrease in helical twisting power" refers to an increase or decrease when the initial helical direction (before light irradiation) of the chiral agent A is taken as "positive." Therefore, even when the helical twisting power continues to decrease upon light irradiation and exceeds 0, causing the helical direction to become "negative" (i.e., when a helical direction opposite to the initial helical direction (before light irradiation) is induced), this also corresponds to "a chiral agent whose helical twisting power decreases."

[0054] An example of the chiral agent A is a so-called photoreactive chiral agent. The photoreactive chiral agent has a chiral moiety and a photoreactive moiety that undergoes a structural change upon irradiation with light, and is a compound that, for example, significantly changes the twisting power of a liquid crystal compound depending on the amount of irradiation. Examples of photoreactive sites that undergo a structural change upon irradiation with light include photochromic compounds (Kingo Uchida, Masahiro Irie, Chemical Industry, vol. 64, p. 640, 1999; Kingo Uchida, Masahiro Irie, Fine Chemical, vol. 28(9), p. 15, 1999). The structural change refers to decomposition, addition reaction, isomerization, racemization, [2+2] photocyclization, dimerization, and the like that occur upon irradiation of the photoreactive site with light, and the structural change may be irreversible. Examples of chiral sites include the asymmetric carbons described in Hiroyuki Nodaira's Chemical Review, No. 22, Chemistry of Liquid Crystals, p. 73: 1994.

[0055] Examples of the chiral agent A include photoreactive chiral agents described in paragraphs 0044 to 0047 of JP-A-2001-159709, optically active compounds described in paragraphs 0019 to 0043 of JP-A-2002-179669, optically active compounds described in paragraphs 0020 to 0044 of JP-A-2002-179633, optically active compounds described in paragraphs 0016 to 0040 of JP-A-2002-179670, optically active compounds described in paragraphs 0017 to 0050 of JP-A-2002-179668, optically active compounds described in paragraphs 0018 to 0020 of JP-A-2002-180051, and 44, the optically active isosorbide derivatives described in paragraphs 0016 to 0055 of JP-A-2002-338575, the photoreactive optically active compounds described in paragraphs 0023 to 0032 of JP-A-2002-080478, the photoreactive chiral agents described in paragraphs 0019 to 0029 of JP-A-2002-080851, the optically active compounds described in paragraphs 0022 to 0049 of JP-A-2002-179681, the optically active compounds described in paragraphs 0015 to 0044 of JP-A-2002-302487, the optically active compounds described in paragraphs 0015 to 0044 of JP-A-2002-338668 the optically active polyesters described in paragraphs 0015 to 0050 of JP-A-2003-055315, the binaphthol derivatives described in paragraphs 0019 to 0041 of JP-A-2003-073381, the optically active fulgide compounds described in paragraphs 0008 to 0043 of JP-A-2003-073381, the optically active isosorbide derivatives described in paragraphs 0015 to 0057 of JP-A-2003-306490, the optically active isosorbide derivatives described in paragraphs 0015 to 0041 of JP-A-2003-306491, the optically active isosorbide derivatives described in paragraphs 0015 to 0049 of JP-A-2003-313187, Examples of the optically active isosorbide derivatives include the optically active isomannide derivatives described in paragraphs 0015 to 0057 of JP-A-2003-313188, the optically active isosorbide derivatives described in paragraphs 0015 to 0049 of JP-A-2003-313189, the optically active polyester / amides described in paragraphs 0015 to 0052 of JP-A-2003-313292, the optically active compounds described in paragraphs 0012 to 0053 of WO2018 / 194157, and the optically active compounds described in paragraphs 0020 to 0049 of JP-A-2002-179682.

[0056] As the chiral agent A, a compound having at least a photoisomerization site is preferable, and the photoisomerization site is more preferably a compound having a photoisomerizable double bond. As the photoisomerization site having the photoisomerizable double bond, a cinnamoyl site, a chalcone site, an azobenzene site, or a stilbene site is preferable because photoisomerization is easily caused and the difference in helical induction power before and after light irradiation is large, and a cinnamoyl site, a chalcone site, or a stilbene site is more preferable because the absorption of visible light is small. The photoisomerization site corresponds to the photoreactive site whose structure changes by light irradiation described above.

[0057] It is preferable that the chiral agent A has any partial structure selected from a binaphthyl partial structure, an isosorbide partial structure (a partial structure derived from isosorbide), and an isomannide partial structure (a partial structure derived from isomannide). The binaphthyl partial structure, the isosorbide partial structure, and the isomannide partial structure each refer to the following structures. In the binaphthyl moiety, the solid and dashed lines are parallel to each other, and each represents a single or double bond. In the structures shown below, * represents the bond position.

[0058] [ka]

[0059] The chiral agent A may have a polymerizable group. The type of the polymerizable group is not particularly limited, and is preferably a functional group capable of an addition polymerization reaction, more preferably a polymerizable ethylenically unsaturated group or a ring-polymerizable group, and further preferably a (meth)acryloyl group, a vinyl group, a styryl group, or an allyl group.

[0060] The chiral agent A is preferably a compound represented by formula (C). Formula (C) RLR Each R independently represents a group having at least one moiety selected from the group consisting of a cinnamoyl moiety, a chalcone moiety, an azobenzene moiety, and a stilbene moiety. L represents a divalent linking group formed by removing two hydrogen atoms from the structure represented by formula (D) (a divalent linking group formed by removing two hydrogen atoms from the binaphthyl partial structure), a divalent linking group represented by formula (E) (a divalent linking group consisting of the isosorbide partial structure), or a divalent linking group represented by formula (F) (a divalent linking group consisting of the isomannide partial structure). In formula (E) and formula (F), * represents a bonding position.

[0061] [ka]

[0062] Step 1 may be an embodiment in which two or more types of chiral agent A are used, or an embodiment in which at least one type of chiral agent A and at least one type of chiral agent whose helical twisting power does not change upon irradiation with light (hereinafter, also simply referred to as "chiral agent B") are used. The chiral agent B may be liquid crystal or non-liquid crystal. The chiral agent B generally contains an asymmetric carbon atom. The chiral agent B may be an axially asymmetric compound or a planar asymmetric compound that does not contain an asymmetric carbon atom. The chiral agent B may have a polymerizable group. Examples of the type of the polymerizable group include the polymerizable groups that the chiral agent A may have. As the chiral agent B, a known chiral agent can be used. Chiral agent B is preferably a chiral agent that induces a helical twist in the opposite direction to that of the above-mentioned chiral agent A. That is, for example, when the helical twist induced by chiral agent A is right-handed, the helical twist induced by chiral agent B is left-handed.

[0063] The molar absorption coefficients of the chiral agent A and the chiral agent B are not particularly limited, but the molar absorption coefficient at the wavelength (e.g., 365 nm) of the light irradiated in step 3 described below is preferably 100 to 100,000 L / (mol cm), and more preferably 500 to 50,000 L / (mol cm).

[0064] The contents of the chiral dopant A and the chiral dopant B in the composition layer can be appropriately set according to the properties (e.g., retardation and wavelength dispersion) of the optically anisotropic layer to be formed. Since the twist angle of the liquid crystal compound in the optically anisotropic layer is largely dependent on the types and concentrations of the chiral dopant A and B, the alignment state of the liquid crystal compound can be controlled by adjusting these.

[0065] The total content of the chiral agent in the composition layer (total content of all chiral agents) is not particularly limited, but in terms of ease of controlling the alignment state of the liquid crystal compound, it is preferably 5.0 mass% or less, more preferably 4.0 mass% or less, and even more preferably 2.0 mass% or less, based on the total mass of the liquid crystal compound. The lower limit is not particularly limited, but is preferably 0.01 mass% or more, more preferably 0.02 mass% or more, and even more preferably 0.05 mass% or more.

[0066] The content of chiral agent A in the chiral agent is not particularly limited, but is preferably 5 to 95 mass %, more preferably 10 to 90 mass %, based on the total mass of the chiral agent, in terms of ease of controlling the alignment state of the liquid crystal compound.

[0067] The composition layer may contain a polymerization initiator, in which case the polymerization of the liquid crystal compound having a polymerizable group proceeds more efficiently. The polymerization initiator may be a known polymerization initiator, such as a photopolymerization initiator or a thermal polymerization initiator, and is preferably a photopolymerization initiator. In particular, a polymerization initiator that is sensitive to the light irradiated in step 5 described below is preferable.

[0068] The polymerization initiator preferably has a maximum molar absorption coefficient of the light irradiated in step 3 that is 0.1 times or less than the maximum molar absorption coefficient of the light irradiated in step 5. The molar absorption coefficient of the polymerization initiator at the wavelength of light irradiation in step 3 is preferably 5000 L / (mol cm) or less, more preferably 4000 L / (mol cm) or less, and even more preferably 3000 L / (mol cm) or less. There is no particular lower limit, and 0 L / (mol cm) is preferable, but it is often 30 L / (mol cm) or more. The content of the polymerization initiator in the composition layer is not particularly limited, but is preferably from 0.01 to 20% by mass, and more preferably from 0.5 to 10% by mass, based on the total mass of the composition layer.

[0069] The composition layer may include a photosensitizer. The type of photosensitizer is not particularly limited, and examples include known photosensitizers. The molar absorption coefficient of the photosensitizer at the wavelength of light irradiation in step 3 is preferably 5000 L / (mol cm) or less, more preferably 4800 L / (mol cm) or less, and even more preferably 4500 L / (mol cm) or less. There is no particular lower limit, and 0 L / (mol cm) is preferable, but it is often 30 L / (mol cm) or more. The content of the photosensitizer in the composition layer is not particularly limited, but is preferably from 0.01 to 20% by mass, and more preferably from 0.5 to 10% by mass, based on the total mass of the composition layer.

[0070] The composition layer may contain a polymerizable monomer different from the liquid crystal compound having a polymerizable group. The polymerizable monomer may be a radical polymerizable compound or a cationic polymerizable compound, and a polyfunctional radical polymerizable monomer is preferable. The polymerizable monomer may be, for example, the polymerizable monomer described in paragraphs 0018 to 0020 of JP-A-2002-296423. The content of the polymerizable monomer in the composition layer is not particularly limited, but is preferably from 1 to 50% by mass, and more preferably from 5 to 30% by mass, based on the total mass of the liquid crystal compound.

[0071] The composition layer may contain a surfactant. Examples of the surfactant include conventionally known compounds, but fluorine-based compounds are preferred. Specific examples of the surfactant include the compounds described in paragraphs 0028 to 0056 of JP-A No. 2001-330725 and the compounds described in paragraphs 0069 to 0126 of JP-A No. 2003-295212.

[0072] The composition layer may contain a polymer. Examples of the polymer include cellulose esters. Examples of the cellulose esters include those described in paragraph 0178 of JP-A-2000-155216. The content of the polymer in the composition layer is not particularly limited, but is preferably from 0.1 to 10% by mass, and more preferably from 0.1 to 8% by mass, based on the total mass of the liquid crystal compound.

[0073] In addition to the above, the composition layer may contain an additive (alignment control agent) that promotes horizontal or vertical alignment in order to bring the liquid crystal compound into a horizontal or vertical alignment state.

[0074] [substrate] As described below, when forming a composition layer, it is preferable to form the composition layer on a substrate. The substrate is a plate that supports the composition layer. The substrate is preferably a transparent substrate. Note that the transparent substrate refers to a substrate having a visible light transmittance of 60% or more, preferably 80% or more, and more preferably 90% or more.

[0075] The retardation value (Rth(550)) in the thickness direction of the substrate at a wavelength of 550 nm is not particularly limited, but is preferably −110 to 110 nm, more preferably −80 to 80 nm. The in-plane retardation value (Re(550)) of the substrate at a wavelength of 550 nm is not particularly limited, but is preferably 0 to 50 nm, more preferably 0 to 30 nm, and further preferably 0 to 10 nm.

[0076] The material for forming the substrate is preferably a polymer having excellent optical properties such as transparency, mechanical strength, thermal stability, moisture barrier properties, and isotropy. Examples of polymer films that can be used as the substrate include cellulose acylate films (e.g., cellulose triacetate film (refractive index 1.48), cellulose diacetate film, cellulose acetate butyrate film, and cellulose acetate propionate film), polyolefin films such as polyethylene and polypropylene, polyester films such as polyethylene terephthalate and polyethylene naphthalate, polyethersulfone films, polyacrylic films such as polymethyl methacrylate, polyurethane films, polycarbonate films, polysulfone films, polyether films, polymethylpentene films, polyether ketone films, (meth)acrylonitrile films, and films of polymers having an alicyclic structure (norbornene-based resins (Arton: product name, manufactured by JSR Corporation, and amorphous polyolefins (Zeonex: product name, manufactured by Zeon Corporation)). Among these, the material for the polymer film is preferably triacetyl cellulose, polyethylene terephthalate, or a polymer having an alicyclic structure, and more preferably triacetyl cellulose.

[0077] The substrate may contain various additives (for example, an optical anisotropy adjusting agent, a wavelength dispersion adjusting agent, fine particles, a plasticizer, an ultraviolet protection agent, a deterioration inhibitor, a release agent, etc.).

[0078] The thickness of the substrate is not particularly limited, but is preferably 10 to 200 μm, more preferably 10 to 100 μm, and even more preferably 20 to 90 μm. The substrate may be made of a laminate of multiple sheets. In order to improve adhesion with a layer provided thereon, the surface of the substrate may be subjected to a surface treatment (e.g., glow discharge treatment, corona discharge treatment, ultraviolet (UV) treatment, flame treatment). In addition, an adhesive layer (undercoat layer) may be provided on the substrate. In addition, in order to impart slipperiness to the substrate during the transport process and to prevent sticking between the front and back surfaces after winding, a polymer layer containing inorganic particles having an average particle size of about 10 to 100 nm at a solid content ratio of 5 to 40 mass % may be placed on one side of the substrate.

[0079] The substrate may be a so-called temporary support, that is, the substrate may be peeled off from the optically anisotropic layer after carrying out the production method of the present invention.

[0080] In addition, the surface of the substrate may be directly subjected to rubbing treatment. In other words, a substrate that has been subjected to rubbing treatment may be used. The direction of the rubbing treatment is not particularly limited, and an optimal direction is appropriately selected depending on the direction in which the liquid crystal compound is desired to be aligned. The rubbing treatment can be a treatment method that is widely used as a liquid crystal alignment treatment process for LCDs (liquid crystal displays), in which the surface of the substrate is rubbed in a certain direction with paper, gauze, felt, rubber, nylon fiber, polyester fiber, or the like to obtain alignment.

[0081] An alignment film may be disposed on the substrate. The alignment layer can be formed by such means as rubbing an organic compound (preferably a polymer), oblique deposition of an inorganic compound, formation of a layer with microgrooves, or deposition of an organic compound (e.g., ω-tricosanoic acid, dioctadecylmethylammonium chloride, methyl stearate) by the Langmuir-Blodgett technique (LB film). Furthermore, an alignment film is also known that exhibits an alignment function when an electric field is applied, a magnetic field is applied, or light (preferably polarized light) is irradiated. The alignment film is preferably formed by a rubbing treatment of a polymer.

[0082] Examples of the polymer contained in the alignment film include methacrylate copolymers, styrene copolymers, polyolefins, polyvinyl alcohol and modified polyvinyl alcohol, poly(N-methylol acrylamide), polyesters, polyimides, vinyl acetate copolymers, carboxymethyl cellulose, and polycarbonates, as described in paragraph 0022 of JP-A-8-338913. A silane coupling agent can also be used as the polymer. Among these, water-soluble polymers (e.g., poly(N-methylol acrylamide), carboxymethyl cellulose, gelatin, polyvinyl alcohol, and modified polyvinyl alcohol) are preferred, gelatin, polyvinyl alcohol, or modified polyvinyl alcohol are more preferred, and polyvinyl alcohol or modified polyvinyl alcohol are even more preferred.

[0083] As described above, the alignment film can be formed by applying a solution containing the above-mentioned polymer, which is an alignment film forming material, and any additives (e.g., a crosslinking agent) onto a substrate, followed by heating and drying (crosslinking) and rubbing treatment.

[0084] [Step 1 Procedure] In step 1, a composition layer containing the above-mentioned components is formed, but the procedure is not particularly limited. For example, a method of applying a composition containing the above-mentioned liquid crystal compound having a polymerizable group onto a substrate and performing a drying treatment as necessary (hereinafter, also simply referred to as a "coating method"), and a method of forming a composition layer separately and transferring it onto a substrate are included. Among them, the coating method is preferable from the viewpoint of productivity. The coating method will be described in detail below.

[0085] The composition used in the coating method contains the above-mentioned liquid crystal compound having a polymerizable group, and other components (e.g., a chiral agent, a polymerization initiator, a polymerizable monomer, a surfactant, and a polymer) that are used as necessary. The content of each component in the composition is preferably adjusted to the content of each component in the composition layer described above.

[0086] The coating method is not particularly limited, and examples thereof include wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, and die coating. If necessary, after coating the composition, a treatment for drying the composition layer coated on the substrate may be carried out. By carrying out the drying treatment, the solvent can be removed from the composition layer.

[0087] The thickness of the composition layer is not particularly limited, but is preferably from 0.1 to 20 μm, more preferably from 0.2 to 15 μm, and even more preferably from 0.5 to 10 μm.

[0088] (Process 2) In step 2, the composition layer is subjected to a heat treatment to align the liquid crystal compound in the composition layer. By carrying out this step, the liquid crystal compound in the composition layer is brought into a predetermined alignment state. For example, as shown in FIG. 6, a composition layer 22 in which the liquid crystal compound LC is homogeneously aligned is formed on a substrate 20.

[0089] The heat treatment conditions are selected optimally depending on the liquid crystal compound used, and the heat treatment is preferably performed at a temperature equal to or higher than the phase transition temperature from a solid to a liquid crystal phase of the liquid crystal compound. Among these, the heating temperature is often 25 to 250°C, more often 40 to 150°C, and even more often 50 to 130°C. The heating time is often 0.1 to 60 minutes, and more often 0.2 to 5 minutes.

[0090] (Step 3) Step 3 is a step of irradiating the composition layer with light under conditions where the oxygen concentration is 1% by volume or more after step 2. 7, in the above-mentioned step 3, light irradiation is performed from the direction opposite to the composition layer 22 side of the substrate 20 (the direction of the white arrow in FIG. 7) under the condition of an oxygen concentration of 1% by volume or more. Note that, although light irradiation is performed from the substrate 20 side in FIG. 7, it may be performed from the composition layer 22 side. In this case, when comparing the lower region 22A on the substrate 20 side of the composition layer 22 with the upper region 22B on the opposite side to the substrate 20 side, the oxygen concentration in the upper region 22B is higher and the oxygen concentration in the lower region 22A is lower because the surface of the upper region 22B is closer to the air. Therefore, when the composition layer 22 is irradiated with light, polymerization of the liquid crystal compound is likely to proceed in the lower region 22A, and the alignment state of the liquid crystal compound is fixed. Furthermore, since the oxygen concentration is high in the upper region 22B, even if light is irradiated, the polymerization of the liquid crystal compound is inhibited by oxygen, and the polymerization does not progress easily. That is, by carrying out step 3, fixation of the alignment state of the liquid crystal compound is likely to proceed in the region of the composition layer on the substrate side (lower region). On the other hand, fixation of the alignment state of the liquid crystal compound is unlikely to proceed in the region of the composition layer on the opposite side to the substrate side (upper region), and the liquid crystal compound can form an isotropic phase by carrying out any of the requirements 1 to 4 described below.

[0091] Step 3 is carried out under conditions of an oxygen concentration of 1% by volume or more. In particular, the oxygen concentration is preferably 2% by volume or more, and more preferably 5% by volume or more, in terms of ease of production of the optical element of the present invention. There is no particular upper limit, but an example of the upper limit is 100% by volume.

[0092] The amount of light irradiation in step 3 is not particularly limited, but is preferably 300 mJ / cm because it is easy to form a desired optically anisotropic layer. 2 Less than 200 mJ / cm is preferable. 2 Less than 100 J / cm is more preferable. 2 The lower limit is preferably 10 mJ / cm because it is easy to form a desired optically anisotropic layer. 2 More than 30 mJ / cm is preferable. 2 The above is more preferable. The light irradiation in step 3 is preferably carried out at a temperature of 15 to 70°C (preferably 15 to 50°C).

[0093] The light used for the light irradiation is not particularly limited as long as it is light that promotes the fixation of the alignment state of the liquid crystal compound in the region (lower region) on the substrate side of the composition layer. For example, the bright line spectrum of a mercury lamp, far ultraviolet light represented by an excimer laser, extreme ultraviolet light, X-rays, ultraviolet light, and electron beams can be mentioned. Among them, ultraviolet light is preferable.

[0094] (Step 4) Step 4 is a step of pressing a mold having a concave-convex structure on its surface against the surface of the composition layer opposite to the substrate side to transfer the concave-convex structure of the mold to the composition layer. In this step, as shown in Fig. 8, a mold 24 having a concave-convex structure on its surface, in which a plurality of convex portions 28 are arranged on a support 26, is prepared, and the mold 24 is pressed against the composition layer 22 as shown in Fig. 9 to transfer the concave-convex structure of the mold to the composition layer 22. In this embodiment, since Requirement 1 is satisfied as described above, Step 4 is performed under heating conditions equal to or higher than the phase transition temperature from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer. By performing the heat treatment, the orientation state of the liquid crystal compound (not shown) in the upper region 22B of the composition layer 22 is not fixed, so the orientation state is disturbed and changes to an isotropic phase. On the other hand, in the lower region 22A of the composition layer 22, the orientation state of the liquid crystal compound LC is fixed by Step 3 as described above, so that the orientation state of the liquid crystal compound LC does not change even when the heat treatment is performed.

[0095] The mold used in this step is one having an appropriate shape that is optimal for the shape of the convex portion of the optically isotropic member that is to be formed.

[0096] The heating conditions when carrying out the above-mentioned requirement 1 (step 4 is carried out under heating conditions equal to or higher than the phase transition temperature from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer) may be equal to or higher than the phase transition temperature from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer, and are preferably 5° C. or higher than the above phase transition temperature. There is no particular upper limit, but it is preferably equal to or lower than a temperature 100° C. higher than the above phase transition temperature.

[0097] After the concave-convex structure of the mold is transferred to the composition layer, the mold may be peeled off as appropriate.The mold may also be peeled off after carrying out step 5 described below.

[0098] (Step 5) Step 5 is a step of performing a curing treatment on the composition layer to form an optical element having an optically anisotropic layer and an optically isotropic member having a convex portion protruding from the substrate side to the side opposite to the optically anisotropic layer side. By carrying out this step, an optical element 10C is formed having an optically anisotropic layer 12 and an optically isotropic member 14C having a convex portion 16C as shown in Fig. 10. In the embodiment of Fig. 10, the optically anisotropic layer 12 is a layer formed by fixing a homogeneously aligned liquid crystal compound.

[0099] The method of the curing treatment is not particularly limited, and examples thereof include photocuring treatment and heat curing treatment. The temperature conditions for the heat curing treatment are not particularly limited as long as the polymerization reaction of the liquid crystal compound having a polymerizable group can be carried out, and the temperature is preferably 20 to 200°C, and more preferably 50 to 180°C. The heating time for the heat curing treatment is not particularly limited, but is preferably from 30 to 600 seconds, and more preferably from 60 to 300 seconds. The photocuring treatment is preferably an ultraviolet ray irradiation treatment. For ultraviolet irradiation, a light source such as an ultraviolet lamp is used. The amount of light (e.g., ultraviolet light) applied is not particularly limited, but is generally 100 to 1000 mJ / cm 2 About 300 mJ / cm is preferable. 2 Super 1000mJ / cm 2 The following is more preferred: When performing photocuring treatment, it is preferable to perform it under conditions of an oxygen concentration of less than 1% by volume (preferably an oxygen concentration of 0.1% by volume or less). The lower limit of the oxygen concentration is not particularly limited, but may be 0% by volume.

[0100] Although the embodiment satisfying requirement 1 has been described above, the present invention may satisfy any one of requirements 2 to 4 instead of requirement 1. For example, in requirement 2, step 5 is performed under heating conditions equal to or higher than the phase transition temperature from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer. More specifically, requirement 2 can be satisfied by adopting, as the curing treatment in step 5, a heat curing treatment performed under heating conditions equal to or higher than the phase transition temperature from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer. When requirement 2 is satisfied, the alignment state of the liquid crystal compound in the upper region of the composition layer is disturbed and changes to an isotropic phase, as in the case where requirement 1 described above is satisfied, and as a result, a desired optical element can be formed. When requirement 2 is satisfied, the temperature of the heat curing treatment in step 5 is preferably 5° C. or more higher than the phase transition temperature from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer. There is no particular upper limit, but it is preferably a temperature not higher than 100° C. higher than the phase transition temperature.

[0101] Moreover, requirement 3 further includes, between steps 3 and 4, step 6 of heating the composition layer to a temperature equal to or higher than the phase transition temperature from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer. Furthermore, requirement 4 further includes, between step 4 and step 5, step 7 of heating the composition layer to a temperature equal to or higher than the phase transition temperature from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer. By carrying out the above steps 6 or 7, the alignment state of the liquid crystal compound in the upper region of the composition layer is disturbed and changes to an isotropic phase, as in requirements 1 and 2, and as a result, the desired optical element can be formed. The temperature of the heat curing treatment in steps 6 and 7 is preferably 5° C. or more higher than the phase transition temperature from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer. There is no particular upper limit, but it is preferably a temperature not higher than 100° C. higher than the phase transition temperature.

[0102] The above describes an embodiment in which the optically anisotropic layer is a layer in which the orientation state of a single liquid crystal compound is fixed. However, the above manufacturing method can also form an optically anisotropic layer having multiple regions in which the orientation state of the liquid crystal compound differs along the thickness direction. For example, the following describes an embodiment in which an optically anisotropic layer is formed having, along the thickness direction, a first region in which the orientation state of liquid crystal compounds that are twisted and aligned along a helical axis extending along the thickness direction is fixed, and a second region in which the orientation state of liquid crystal compounds that are homogeneously aligned is fixed.

[0103] When forming the optically anisotropic layer as described above, there is a method of using a composition layer further containing chiral dopant A and chiral dopant B. In this method, the absolute value of the weighted average helical twisting power of the chiral dopant in the composition layer obtained in step 1 is 0.0 to 1.9 μm -1 It is preferable that the thickness is 0.0 to 1.5 μm. -1 More preferably, the thickness is 0.0 to 1.0 μm. -1 More preferably, the thickness is 0.0 to 0.5 μm. -1 It is particularly preferable that the thickness is 0.0 to 0.02 μm. -1 is more particularly preferred, with 0 being most preferred.

[0104] The weighted average helical twisting power of the chiral agent means, when two or more chiral agents are contained in the composition, the sum of the product of the helical twisting power of each chiral agent contained in the composition layer and the concentration (mass%) of each chiral agent in the composition layer divided by the total concentration (mass%) of the chiral agents in the composition layer. For example, when two types of chiral agents (chiral agent X and chiral agent Y) are used in combination, it is represented by the following formula (Y). Equation (Y) Weighted average helical induced force (μm -1 )=(helix-inducing power of chiral agent X (μm -1 ) × concentration of chiral dopant X in the composition layer (% by mass) + helical twisting power of chiral dopant Y (μm -1 ) × concentration of chiral agent Y in the composition layer (mass%) / (concentration of chiral agent X in the composition layer (mass%) + concentration of chiral agent Y in the composition layer (mass%)) However, in the above formula (Y), when the helical direction of the chiral agent is right-handed, the helical twisting power is a positive value. On the other hand, when the helical direction of the chiral agent is left-handed, the helical twisting power is a negative value. That is, for example, when the helical twisting power is 10 μm -1In the case of the chiral agent, when the helical direction of the helix induced by the chiral agent is right-handed, the helical induction force is 10 μm -1 On the other hand, when the helical direction of the helix induced by the chiral agent is left-handed, the helical induction force is expressed as -10 μm -1 It is expressed as:

[0105] When the absolute value of the weighted average helical twisting power of the chiral agent in the composition layer formed in step 1 is 0, a composition layer 32 in which liquid crystal compound LC is homogeneously aligned is formed on substrate 30 by carrying out step 2, as shown in Fig. 11. Note that chiral agent A and chiral agent B are present in the composition layer 32 shown in Fig. 11 at the same concentration, and the helical direction induced by chiral agent A is left-handed, and the helical direction induced by chiral agent B is right-handed. Also, the absolute value of the helical twisting power of chiral agent A and the absolute value of the helical twisting power of chiral agent B are the same.

[0106] Next, when the above-mentioned step 3 is carried out, as in the above-mentioned embodiment, as shown in FIG. 12, when comparing the lower region 32A on the substrate 30 side of the composition layer 32 with the upper region 32B on the opposite side to the substrate 30 side, the oxygen concentration in the upper region 32B is higher and the oxygen concentration in the lower region 32A is lower because the surface of the upper region 32B is closer to the air. Therefore, when the composition layer 32 is irradiated with light, polymerization of the liquid crystal compound is likely to proceed in the lower region 32A, and the alignment state of the liquid crystal compound is fixed. Note that the chiral agent A is also present in the lower region 32A, and the chiral agent A is also photosensitive, and the helical twisting force changes. However, since the alignment state of the liquid crystal compound is fixed in the lower region 32A, even if any of the requirements 1 to 4 is carried out, the alignment state of the liquid crystal compound is not changed. Furthermore, since the oxygen concentration is high in the upper region 32B, even if light is irradiated, the polymerization of the liquid crystal compound is inhibited by oxygen, and the polymerization does not proceed easily. Since the chiral agent A is also present in the upper region 32B, the chiral agent A is exposed to light, and the helical twisting force changes. Therefore, when step 8 described later is performed, the alignment state of the liquid crystal compound changes according to the changed helical twisting force. That is, by carrying out step 3, fixation of the alignment state of the liquid crystal compound is facilitated in the region of the composition layer on the substrate side (lower region), whereas fixation of the alignment state of the liquid crystal compound is difficult in the region of the composition layer on the opposite side to the substrate side (upper region), resulting in a state in which the helical twisting power changes depending on the photoexposed chiral dopant A.

[0107] Next, the obtained composition layer is heated in step 8. By carrying out step 8, in the upper region 32B of the composition layer 32, the liquid crystal compound LC is formed in a twisted alignment state in response to a change in the helical twisting power of the chiral dopant A. The heating temperature in step 8 is not particularly limited, and an optimal temperature is appropriately selected depending on the type of liquid crystal compound, but a temperature lower than the temperature at which the composition constituting the composition layer undergoes a phase transition from a liquid crystal phase to an isotropic phase is preferable. The lower limit of the heating temperature in step 8 is not particularly limited, and a temperature equal to or higher than the phase transition temperature from a solid state to a liquid crystal phase is preferable. The reason why the above-mentioned change in the alignment state occurs will be described in detail below.

[0108] As described above, when step 3 is performed on the composition layer 32 shown in FIG. 11, the orientation state of the liquid crystal compound is fixed in the lower region 32A, whereas the polymerization of the liquid crystal compound is difficult to proceed in the upper region 32B, and the orientation state of the liquid crystal compound is not fixed. Furthermore, the helical twisting power of the chiral agent A changes in the upper region 32B. When such a change in the helical twisting power of the chiral agent A occurs, the force twisting the liquid crystal compound changes in the upper region 32B compared to the state before light irradiation. This point will be explained in more detail. As described above, chiral agent A and chiral agent B are present in the composition layer 32 shown in Fig. 11 at the same concentration, the helical direction induced by chiral agent A is left-handed, and the helical direction induced by chiral agent B is right-handed. Furthermore, the absolute value of the helical twisting power of chiral agent A is the same as the absolute value of the helical twisting power of chiral agent B. Therefore, the weighted average helical twisting power of the chiral agents in the composition layer before light irradiation is 0. The above embodiment is shown in Figure 14. In Figure 14, the vertical axis indicates the helical twisting power of the chiral agent (μm -1The helical twisting power of chiral agent A is calculated by multiplying the concentration of chiral agent (mass%) by the concentration of chiral agent (mass%). The further this value is from zero, the stronger the helical twisting power. First, the relationship between chiral agent A and chiral agent B in the composition layer before light irradiation corresponds to the point where the amount of light irradiation is 0, and the helical twisting power of chiral agent A (μm -1 ) × concentration of chiral agent A (mass%) and the helical twisting power of chiral agent B (μm -1 This corresponds to a state in which the absolute value of "the helical twist induction potential (mass%) × the concentration (mass%) of chiral dopant B" is equal to that of chiral dopant A. In other words, the helical twist induction potential of chiral dopant A, which induces left-handedness, and that of chiral dopant B, which induces right-handedness, are offset. When light is irradiated to upper region 32B in this state, and the helical twisting power of chiral agent A decreases depending on the amount of light irradiation as shown in Fig. 14, the weighted average helical twisting power of the chiral agent in upper region 12B increases and the right-handed helical twisting power becomes stronger as shown in Fig. 15. In other words, the helical twisting power of the liquid crystal compound increases in the direction (+) of the helical twist induced by chiral agent B as the amount of irradiation increases. Therefore, when the composition layer 32 after step 3, in which such a change in the weighted average helical twisting force has occurred, is subjected to a heat treatment to promote reorientation of the liquid crystal compound, as shown in Figure 13, in the upper region 32B, the liquid crystal compound LC is twisted and aligned along the helical axis extending along the thickness direction of the composition layer 32. On the other hand, as described above, in the lower region 32A of the composition layer 32, the polymerization of the liquid crystal compound has progressed during step 3, and the orientation state of the liquid crystal compound has been fixed, so that reorientation of the liquid crystal compound does not proceed.

[0109] 14 and 15, the embodiment in which a chiral agent whose helical twisting power decreases upon light irradiation is used as the chiral agent A is described, but the present invention is not limited to this embodiment. For example, a chiral agent whose helical twisting power increases upon light irradiation may be used as the chiral agent A. In this case, the helical twisting power induced by the chiral agent A increases upon light irradiation, and the liquid crystal compound is twisted in the direction of the rotation induced by the chiral agent A. 14 and 15, the embodiment in which the chiral agent A and the chiral agent B are used in combination is described, but the present invention is not limited to this embodiment. For example, the embodiment may be an embodiment in which two types of chiral agents A are used. Specifically, the embodiment may be an embodiment in which a chiral agent A1 that induces left-handedness and a chiral agent A2 that induces right-handedness are used in combination. The chiral agents A1 and A2 may each independently be a chiral agent whose helical induction power increases, or a chiral agent whose helical induction power decreases. For example, a chiral agent that induces left-handedness and whose helical induction power increases upon light irradiation and a chiral agent that induces right-handedness and whose helical induction power decreases upon light irradiation may be used in combination.

[0110] Next, when step 3 is performed again on the composition layer obtained above, when composition layer 32 is irradiated with light as shown in Fig. 16, polymerization of the liquid crystal compound is likely to proceed in region 32C, which is the region on the substrate 30 side in the upper region, and the alignment state of the liquid crystal compound is fixed. On the other hand, fixation of the alignment state of the liquid crystal compound is difficult to proceed in region 32D, which is the region on the opposite side to substrate 30 in the upper region. Therefore, when the above-mentioned steps 4 and 5 are carried out on the obtained composition layer 32, and further a process that satisfies any one of the requirements 1 to 4 is carried out, an optical element 10D is formed, which includes an optically anisotropic layer 12A having, along the thickness direction, a first region in which the alignment state of the liquid crystal compound that is twisted along a helical axis extending along the thickness direction is fixed, and a second region in which the alignment state of the liquid crystal compound that is homogeneously aligned is fixed, as shown in Fig. 17. Note that, as shown in Fig. 17, the optically isotropic member 14D is composed of a convex portion 16D and a base portion 18D.

[0111] <Laminate> The optical element of the present invention may be combined with other members. For example, the optical element of the present invention may be combined with an adhesive layer to form a laminate. In particular, the laminate of the present invention preferably has the optical element described above and an adhesive layer disposed on the optical isotropic member side of the optical element. As the adhesive layer, a known adhesive layer is used.

[0112] The optical element of the present invention may be combined with a polarizer. That is, the present invention also relates to a laminate (polarizing plate) having the optical element of the present invention and a polarizer. The polarizer may be any member capable of converting natural light into a specific linearly polarized light, and an example of the polarizer is an absorptive polarizer. The type of polarizer is not particularly limited, and any commonly used polarizer can be used, such as an iodine-based polarizer, a dye-based polarizer using a dichroic dye, and a polyene-based polarizer. Iodine-based polarizers and dye-based polarizers are generally produced by adsorbing iodine or a dichroic dye to polyvinyl alcohol and stretching it. A protective film may be disposed on one or both sides of the polarizer. An adhesive layer or bonding layer may be disposed between the optical element of the present invention and the polarizer. When the optically anisotropic layer in the optical element of the present invention is a λ / 4 plate, a laminate including the optical element of the present invention and a polarizer can be suitably used as a circular polarizing plate.

[0113] <Application> The optical element of the present invention can be applied to various applications. For example, the optical element of the present invention can be used for anti-reflection applications in display devices. More specifically, the present invention also relates to a display device having a polarizer, the optical element of the present invention, and a display element in this order. Examples of the display element include known display elements such as an organic EL display element and a liquid crystal display element. In particular, the optical element of the present invention is preferably applied to an organic EL display element, and in particular, by applying the optical element of the present invention to an organic EL display element having a microcavity structure, the occurrence of a bluish color can be further suppressed. EXAMPLES

[0114] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts, ratios, processing contents, and processing procedures shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.

[0115] <Example 1> The following composition was put into a mixing tank, stirred, and heated at 90°C for 10 minutes. The obtained composition was then filtered through a filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm to prepare a dope. The solid content concentration of the dope was 23.5% by mass, the amount of the plasticizer added was the ratio relative to the cellulose acylate, and the solvent of the dope was methylene chloride / methanol / butanol = 81 / 18 / 1 (mass ratio). ---------------------------------------------------------------------------------- Cellulose Acylate Dope ---------------------------------------------------------------------------------- Cellulose acylate (acetyl substitution degree 2.86, viscosity average polymerization degree 310) 100 parts by mass Sugar ester compound 1 (shown in chemical formula (S4)) 6.0 parts by mass Sugar ester compound 2 (shown in chemical formula (S5)) 2.0 parts by mass Silica particle dispersion (AEROSIL R972, Nippon Aerosil Co., Ltd.) 0.1 part by mass Solvent (methylene chloride / methanol / butanol) ----------------------------------------------------------------------------------

[0116] [ka]

[0117] [ka]

[0118] The dope prepared above was cast using a drum film-forming machine. The dope was cast from a die onto a metal support cooled to 0° C., and then the obtained web (film) was peeled off. The drum was made of SUS. The web (film) obtained by casting was peeled off from the drum, and then dried for 20 minutes in a tenter apparatus, which clips both ends of the web with clips and transports the web at 30 to 40°C during film transport. The web was then post-dried by zone heating while being transported by rolls. The obtained web was knurled and then wound up. The obtained cellulose acylate film had a thickness of 40 μm, an in-plane retardation Re(550) at a wavelength of 550 nm of 1 nm, and a retardation in the thickness direction Rth(550) at a wavelength of 550 nm of 26 nm.

[0119] The cellulose acylate film thus produced was subjected to continuous rubbing treatment. At this time, the longitudinal direction of the long film was parallel to the transport direction, and the angle between the longitudinal direction of the film (transport direction) and the rotation axis of the rubbing roller was 80°. The longitudinal direction of the film (transport direction) was set to 90°, and when observed from the film side, the film width direction was taken as the reference (0°) and the clockwise direction was expressed as a positive value, so the rotation axis of the rubbing roller was at 10°. In other words, the position of the rotation axis of the rubbing roller was rotated 80° counterclockwise with the longitudinal direction of the film as the reference. The above-mentioned rubbed cellulose acylate film was used as a substrate, and a composition (1) containing a rod-shaped liquid crystal compound having the following composition was applied thereon by using a Giesser coater to form a composition layer. Next, the obtained composition layer was heated for 60 seconds at 80° C. By this heating, the rod-like liquid crystal compound in the composition layer was aligned in a predetermined direction. Thereafter, the composition layer was irradiated with ultraviolet light (irradiation dose: 15 mJ / cm ) using a 365 nm LED lamp (manufactured by Acroedge Co., Ltd.) at 30° C. in oxygen-containing air (oxygen concentration: approximately 20% by volume). 2 ). The resulting composition layer was then heated at 80° C. for 10 seconds. Thereafter, the composition layer was irradiated with ultraviolet light (irradiation dose: 20 mJ / cm ) using a 365 nm LED lamp (manufactured by Acroedge Co., Ltd.) at 30° C. in air containing oxygen (oxygen concentration: approximately 20% by volume). 2 ). Thereafter, the obtained film was heated to 130°C (corresponding to a temperature higher than the phase transition temperature (117°C) from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer), and in a state in which the shaping-treated film was pressed against the surface of the uncured composition layer, nitrogen purging was performed to set the oxygen concentration to 100 ppm by volume, and the composition layer was irradiated with ultraviolet light from a metal halide lamp (manufactured by Eye Graphics Co., Ltd.) to fix the alignment state of the liquid crystal compound (irradiation dose: 500 mJ / cm 2 ). Thereafter, the shaping-treated film was peeled off from the composition layer to form an optically isotropic member having convex portions on the outermost surface.

[0120] The obtained optical member (F-1) was an optical element having an optically anisotropic layer having, along the thickness direction, a first region in which the alignment state of the liquid crystal compound twisted along a helical axis extending along the thickness direction is fixed, and a second region in which the alignment state of the liquid crystal compound homogeneously aligned is fixed, as described in FIG. 17, and an optically isotropic member arranged in contact with the optically anisotropic layer. As shown in FIG. 1 and FIG. 2, the convex portions of the optically isotropic member were in the shape of a truncated cone and arranged in a hexagonal close-packed manner. The period PA (the interval between adjacent convex portions) of the multiple convex portions was 2.0 μm, the height HA1 of the convex portions was 1.6 μm, the width WA1 of the upper base of the convex portions (the diameter of the upper base) was 1.0 μm, and the width WA2 of the lower base of the convex portions (the diameter of the lower base) was 1.6 μm. The thickness of the base portion of the optically isotropic member (the thickness of the base portion 18D in FIG. 17) was 0.4 μm. The optically anisotropic layer had a thickness of 1.4 μm in the first region and a thickness of 1.3 μm in the second region. The optical characteristics of the optical element (F-1) were determined using Axometrics' AxoScan and its analysis software (Multi-Layer Analysis). The product (Δn2d2) of Δn2 and thickness d2 at a wavelength of 550 nm in the second region was 173 nm, the twist angle of the liquid crystal compound was 0°, and the alignment axis angle of the liquid crystal compound with respect to the long length direction was -10° on the side in contact with the substrate and -10° on the side in contact with the first region. The product (Δn1d1) of Δn1 and thickness d1 at a wavelength of 550 nm in the first region was 184 nm, the twist angle of the liquid crystal compound was 75°, and the alignment axis angle of the liquid crystal compound with respect to the long length direction was -10° on the side in contact with the second region and -85° on the air side.

[0121] ---------------------------------------------------------------------------------- Composition (1) ---------------------------------------------------------------------------------- 80 parts by weight of the following rod-shaped liquid crystal compound (A) 10 parts by weight of the following rod-shaped liquid crystal compound (B) 10 parts by mass of the following polymerizable compound (C) Ethylene oxide modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 4 parts by mass Photopolymerization initiator (Irgacure 819, manufactured by BASF) 3 parts by weight 0.43 parts by mass of the following left-twisted chiral agent (L1) 0.38 parts by mass of the right-twisted chiral agent (R1) shown below 0.08 parts by weight of the following polymer (A) 0.50 parts by weight of the following polymer (E) Methyl isobutyl ketone 116 parts by mass Ethyl propionate 40 parts by mass ----------------------------------------------------------------------------------

[0122] Rod-shaped liquid crystal compound (A) (hereinafter, a mixture of compounds)

[0123] [ka]

[0124] Rod-shaped liquid crystal compound (B) (see structural formula below)

[0125] [ka]

[0126] Polymerizable compound (C) (see structural formula below)

[0127] [ka]

[0128] Left-twisted chiral agent (L1) (see structural formula below)

[0129] [ka]

[0130] Right-twisted chiral agent (R1) (see structural formula below)

[0131] [ka]

[0132] Polymer (A) (see structural formula below. In the formula, the numerical value for each repeating unit indicates the content (mass%) of each repeating unit relative to the total repeating units.)

[0133] [ka]

[0134] Polymer (E) (see structural formula below. In the formula, the numerical value for each repeating unit indicates the content (mass%) of each repeating unit relative to the total repeating units.)

[0135] [ka]

[0136] <Example 2> The cellulose acylate film produced in Example 1 was passed through a dielectric heating roll at a temperature of 60° C. to raise the film surface temperature to 40° C., and then an alkaline solution having the composition shown below was applied to the band surface of the film using a bar coater in an amount of 14 ml / m. 2 The plate was then conveyed for 10 seconds under a steam-type far-infrared heater manufactured by Noritake Co., Ltd., which had been heated to 110°C. Next, pure water was applied at a rate of 3 ml / m using the same bar coater. 2 Next, the film was washed with water using a fountain coater and then dried with an air knife three times, and then conveyed to a drying zone at 70° C. for 10 seconds to prepare an alkali saponified cellulose acylate film. ---------------------------------------------------------------------------------- Alkaline solution ---------------------------------------------------------------------------------- Potassium hydroxide 4.7 parts by mass Water 15.8 parts by mass Isopropanol 63.7 parts by weight Surfactant: C 14 H 29 O(CH2CH2O) 20 H 1.0 parts by mass Propylene glycol 14.8 parts by weight ----------------------------------------------------------------------------------

[0137] An alignment layer coating solution having the following composition was continuously coated on the alkaline saponified surface of the cellulose acylate film using a wire bar #14, and then dried with hot air at 60° C. for 60 seconds and then with hot air at 100° C. for 120 seconds.

[0138] ---------------------------------------------------------------------------------- Alignment film coating solution ---------------------------------------------------------------------------------- 28 parts by weight of modified polyvinyl alcohol shown below Citric acid ester (AS3, Sankyo Chemical Co., Ltd.) 1.2 parts by mass Photopolymerization initiator (Irgacure 2959, manufactured by BASF) 0.84 parts by mass Glutaraldehyde 2.8 parts by mass Water 699 parts by mass Methanol 226 parts by weight ----------------------------------------------------------------------------------

[0139] Modified polyvinyl alcohol (see structural formula below)

[0140] [ka]

[0141] The alignment film prepared above was continuously subjected to rubbing treatment. At this time, the longitudinal direction of the long film was parallel to the transport direction, and the angle between the longitudinal direction of the film (transport direction) and the rotation axis of the rubbing roller was 45°. The longitudinal direction of the film (transport direction) was set to 90°, and when observed from the film side, the film width direction was taken as the reference (0°) and the clockwise direction was expressed as a positive value, so the rotation axis of the rubbing roller was at 135°. In other words, the position of the rotation axis of the rubbing roller was rotated 45° counterclockwise with the longitudinal direction of the film as the reference.

[0142] The above-mentioned rubbed cellulose acylate film with the alignment layer was used as a substrate, and a composition (2) containing a rod-shaped liquid crystal compound having the following composition was applied thereon by using a Giesser coater to form a composition layer. Next, the obtained composition layer was heated for 80 seconds at 120° C. By this heating, the rod-like liquid crystal compound in the composition layer was aligned in a predetermined direction. Thereafter, the composition layer was irradiated with ultraviolet light for 5 seconds (irradiation dose: 50 mJ / cm ) using a 365 nm LED lamp (manufactured by Acroedge Co., Ltd.) at 40° C. in oxygen-containing air (oxygen concentration: approximately 20% by volume). 2 ). Next, the obtained film was pressed against the uncured composition layer surface with the shaping-treated film under conditions of 195°C (corresponding to a temperature higher than the phase transition temperature (190°C) from the liquid crystal phase to the isotropic phase of the composition constituting the composition layer), and nitrogen purging was performed in a state in which the oxygen concentration was set to 100 ppm by volume. The composition layer was then irradiated with ultraviolet light using a metal halide lamp (manufactured by Eye Graphics Co., Ltd.) to fix the alignment state of the liquid crystal compound (irradiation dose: 500 mJ / cm). 2 Thereafter, the shaping-treated film was peeled off from the composition layer to form an optically isotropic member having convex portions on the outermost surface. The obtained optical member (F-2) was an optical element having an optically anisotropic layer, which is a layer formed by fixing the alignment state of homogeneously aligned liquid crystal compounds, and an optically isotropic member arranged in contact with the optically anisotropic layer, as described in Figs. 1 and 2. The shape and arrangement of the convex portion of the optically isotropic member were the same as those in Example 1. The thickness of the base portion of the optically isotropic member (thickness of the base portion 18A in Fig. 1) was 0.4 µm. The thickness of the optically anisotropic layer was 3.0 µm. The optical characteristics of the optical element (F-2) were determined using AxoScan from Axometrics and its analysis software (Multi-Layer Analysis). The in-plane retardation of the optically anisotropic layer at a wavelength of 550 nm was 140 nm, and the angle of the in-plane slow axis with respect to the longitudinal direction of the film was -45°.

[0143] ---------------------------------------------------------------------------------- Composition (2) ---------------------------------------------------------------------------------- The above rod-shaped liquid crystal compound (A) 20 parts by mass 40 parts by weight of the following rod-shaped liquid crystal compound (D) 40 parts by weight of the following rod-shaped liquid crystal compound (E) Ethylene oxide modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 4 parts by mass Photopolymerization initiator (Irgacure 819, manufactured by BASF) 3 parts by weight 0.08 parts by weight of the above polymer (A) Methyl ethyl ketone 156 parts by mass ----------------------------------------------------------------------------------

[0144] Rod-shaped liquid crystal compound (D) (see structural formula below)

[0145] [ka]

[0146] Rod-shaped liquid crystal compound (E) (see structural formula below)

[0147] [ka]

[0148] <Example 3> An optical element (F-3) was obtained following the same procedure as in Example 2, except that the film subjected to the shaping treatment was changed so as to obtain convex portions arranged in a stripe pattern as shown in Figures 4 and 5. The obtained optical member (F-3) was an optical element having an optically anisotropic layer, which is a layer formed by fixing the alignment state of homogeneously aligned liquid crystal compounds, and an optically isotropic member arranged in contact with the optically anisotropic layer, as described in Figs. 4 and 5. The convex parts of the optically isotropic member had a trapezoidal cross-sectional shape and were arranged in a stripe pattern, as shown in Figs. 4 and 5. The period PB (the distance between adjacent convex parts) of the multiple convex parts was 2.0 μm, the height HB1 of the convex parts was 1.6 μm, the width WB1 of the upper base of the convex parts was 1.0 μm, and the width WA2 of the lower base of the convex parts was 1.6 μm. The thickness of the base part of the optically isotropic member was 0.4 μm. The thickness of the optically anisotropic layer was 3.0 μm. The optical characteristics of the optical element (F-3) were determined using AxoScan from Axometrics and its analysis software (Multi-Layer Analysis). The in-plane retardation of the optically anisotropic layer at a wavelength of 550 nm was 140 nm, and the angle of the in-plane slow axis with respect to the longitudinal direction of the film was -45°.

[0149] <Example 4> An optical element (F-4) was obtained in the same manner as in Example 2, except that the film subjected to the shaping treatment was changed so as to obtain a moth-eye structure in which the convex portions were randomly arranged. The obtained optical member (F-4) was an optical element having an optically anisotropic layer, which is a layer in which the alignment state of homogeneously aligned liquid crystal compounds is fixed, and an optically isotropic member arranged in contact with the optically anisotropic layer. The optically isotropic member had convex portions protruding on the side opposite to the optically anisotropic layer side, and the convex portions were arranged randomly. The convex portions of the optically isotropic member were in the shape of a truncated cone that gradually increased from the optically anisotropic layer side to the side opposite to the optically anisotropic layer side of the convex portions. The height HA1 of the convex portions was 0.4 μm, the width WA1 of the upper base of the convex portions (diameter of the upper base) was 0.18 μm, and the width WA2 of the lower base of the convex portions (diameter of the lower base) was 0.05 μm. The thickness of the base portion of the optically isotropic member was 1.6 μm. The average interval between the convex portions was 0.18 μm, and the thickness of the optically anisotropic layer was 3.0 μm. The optical characteristics of the optical element (F-3) were determined using AxoScan from Axometrics and its analysis software (Multi-Layer Analysis). The in-plane retardation of the optically anisotropic layer at a wavelength of 550 nm was 140 nm, and the angle of the in-plane slow axis with respect to the longitudinal direction of the film was -45°.

[0150] <Example 5> The rubbing-treated cellulose acylate film with the alignment layer prepared in Example 2 was used as a substrate, and the composition (2) containing a rod-like liquid crystal compound was applied thereon by using a Giesser coater to form a composition layer. Next, the obtained composition layer was heated for 80 seconds at 120° C. By this heating, the rod-like liquid crystal compound in the composition layer was aligned in a predetermined direction. Thereafter, nitrogen purging was performed, the oxygen concentration was adjusted to 100 ppm by volume, and the composition layer was irradiated with ultraviolet light (irradiation dose: 50 mJ / cm) using a metal halide lamp (manufactured by Eye Graphics Co., Ltd.). 2 ) to fix the alignment state of the liquid crystal compound, thereby obtaining an optically anisotropic layer. Then, the uneven structure forming composition (1) containing zirconia nanoparticles was applied onto the optically anisotropic layer to form a composition layer. Next, a film subjected to a shaping treatment was pressed against the surface of the uncured composition layer, and nitrogen purging was performed, and the composition layer was irradiated with ultraviolet light using a metal halide lamp (manufactured by Eye Graphics Co., Ltd.) at an oxygen concentration of 100 volume ppm, thereby curing the composition containing zirconia nanoparticles, and an optical member (F-5) was obtained.

[0151] ---------------------------------------------------------------------------------- Composition for forming uneven structure (1) ---------------------------------------------------------------------------------- Mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate (DPHA, manufactured by Nippon Kayaku Co., Ltd.) 90.0 parts by mass Zirconia nanoparticle dispersion 10.0 parts by mass Photopolymerization initiator (Irgacure 907, manufactured by BASF) 1.3 parts by mass Photosensitizer (Kayacure DETX, manufactured by Nippon Kayaku Co., Ltd.) 0.4 parts by mass RS-90 (leveling agent, manufactured by DIC Corporation) 0.1 parts by weight Methyl isobutyl ketone 120 parts by mass ----------------------------------------------------------------------------------

[0152] The obtained optical member (F-5) was an optical element having an optically anisotropic layer, which is a layer formed by fixing the alignment state of homogeneously aligned liquid crystal compounds, and an optically isotropic member arranged in contact with the optically anisotropic layer. The shape and arrangement of the convex portion of the optically isotropic member were the same as those in Example 1. The thickness of the base portion of the optically isotropic member (thickness of the base portion 18A in FIG. 1) was 0.4 μm. The thickness of the optically anisotropic layer was 3.0 μm. The optical characteristics of the optical element (F-5) were determined using AxoScan from Axometrics and its analysis software (Multi-Layer Analysis). The in-plane retardation of the optically anisotropic layer at a wavelength of 550 nm was 140 nm, and the angle of the in-plane slow axis with respect to the longitudinal direction of the film was -45°.

[0153] <Comparative Example 1> An optical member (F-6) was produced in the same manner as in Example 5, except that the concave-convex structure-forming composition (1) was changed to the concave-convex structure-forming composition (2).

[0154] ---------------------------------------------------------------------------------- Composition for forming uneven structure (2) ---------------------------------------------------------------------------------- Aromatic Urethane Acrylate (EBECRYL 220, manufactured by Daicel Allnex Co., Ltd.) 100 parts by weight Photopolymerization initiator (Irgacure 819, manufactured by BASF) 2 parts by mass 0.08 parts by weight of the above polymer (A) Methyl isobutyl ketone 120 parts by mass

[0155] The obtained optical member (F-6) was an optical element having an optically anisotropic layer, which is a layer formed by fixing the alignment state of homogeneously aligned liquid crystal compounds, and an optically isotropic member arranged in contact with the optically anisotropic layer. The shape and arrangement of the convex portion of the optically isotropic member were the same as those in Example 1. The thickness of the base portion of the optically isotropic member (thickness of the base portion 18A in FIG. 1) was 0.4 μm. The thickness of the optically anisotropic layer was 3.0 μm. The optical characteristics of the optical element (F-6) were determined using AxoScan from Axometrics and its analysis software (Multi-Layer Analysis). The in-plane retardation of the optically anisotropic layer at a wavelength of 550 nm was 140 nm, and the angle of the in-plane slow axis with respect to the longitudinal direction of the film was -45°.

[0156] <Comparative Example 2> Following the same procedure as in Example 2, the above-mentioned composition (2) was applied to the above-mentioned rubbed cellulose acylate film with an alignment film as a substrate using a Giesser coater to form a composition layer. Next, the obtained composition layer was heated for 80 seconds at 120° C. By this heating, the rod-like liquid crystal compound in the composition layer was aligned in a predetermined direction. Thereafter, nitrogen purging was performed to set the oxygen concentration to 100 ppm by volume, and the composition layer was irradiated with ultraviolet light using a metal halide lamp (manufactured by Eye Graphics Co., Ltd.) to fix the alignment state of the liquid crystal compound (irradiation dose: 500 mJ / cm 2 ) and an optical film including a λ / 4 plate was prepared. The optical properties of the optical film including the λ / 4 plate were determined using Axometrics' AxoScan and its analysis software (Multi-Layer Analysis). The in-plane retardation of the optically anisotropic layer at a wavelength of 550 nm was 140 nm, and the angle of the in-plane slow axis with respect to the longitudinal direction of the film was -45°.

[0157] Next, the uneven structure-forming composition (1) used in Example 5 was applied to the cellulose acylate film (substrate) prepared in Example 1 using a Giesser coater to form a composition layer. Next, while a film that had been subjected to a shaping treatment was pressed against the surface of the uncured composition layer, nitrogen purging was performed, and the composition layer was irradiated with ultraviolet light using a metal halide lamp (manufactured by Eye Graphics Co., Ltd.) at an oxygen concentration of 100 ppm by volume to cure the aromatic urethane acrylate (irradiation dose: 500 mJ / cm2). 2 The shaping-treated film was then peeled off from the composition layer to produce two concave-convex structure films (S) having convex portions on the outermost surface. The shape of the concave-convex portions was the same stripe shape as in Example 3.

[0158] <Preparation of polarizer> A polyvinyl alcohol (PVA) film with a thickness of 80 μm was dyed by immersing it in an aqueous iodine solution with an iodine concentration of 0.05% by mass for 60 seconds at 30° C. Next, the obtained film was longitudinally stretched to 5 times its original length while being immersed in an aqueous boric acid solution with a boric acid concentration of 4% by mass for 60 seconds, and then dried at 50° C. for 4 minutes to obtain a polarizer with a thickness of 20 μm.

[0159] <Preparation of Polarizer Protective Film> A commercially available cellulose acylate film, Fujitac TG40UL (manufactured by Fujifilm Corporation), was prepared and immersed in a 1.5 mol / L aqueous solution of sodium hydroxide at 55°C, and then the sodium hydroxide was thoroughly washed off with water. The obtained film was then immersed in a 0.005 mol / L aqueous solution of dilute sulfuric acid at 35°C for 1 minute, and then immersed in water to thoroughly wash off the dilute sulfuric acid. Finally, the obtained film was thoroughly dried at 120°C to produce a polarizer protective film with a saponified surface.

[0160] <Preparation of circular polarizing plate> In the same manner as in the preparation of the polarizer protective film, the optical elements (F-1) to (F-6) prepared above were saponified, and the polarizer and the polarizer protective film were continuously bonded to the substrate surface included in the optical elements using a polyvinyl alcohol adhesive to prepare long circular polarizing plates (P-1) to (P-6). That is, the circular polarizing plates (P-1) to (P-6) had a polarizer protective film, a polarizer, a substrate, an optically anisotropic layer, and an optically isotropic member in this order. The above-mentioned polarizer and the above-mentioned polarizer protective film were continuously bonded to the substrate surface of the optical film produced in Comparative Example 2 using a polyvinyl alcohol-based adhesive. Furthermore, the λ / 4 plate side of the obtained laminate and the concave-convex structure side of the concave-convex structure film (S) produced in Comparative Example 2 were bonded to each other using an optically transparent adhesive (OCA tape #8146 manufactured by 3M). Furthermore, the substrate side of the concave-convex structure film (S) of the obtained laminate and the concave-convex structure side of another concave-convex structure film (S) were bonded to each other using an optically transparent adhesive (OCA tape #8146 manufactured by 3M) to produce a circular polarizing plate (P-7). The two concave-convex structure films were bonded to each other so that the directions in which the convex portions extend were orthogonal to each other. In this circular polarizing plate (P-7), an optically anisotropic layer and an optically isotropic member having convex portions were laminated via an adhesive. This circular polarizing plate (P-7) corresponds to the embodiment of Patent Document 1.

[0161] <Fabrication of organic EL display devices and evaluation of display performance> (Mounting to a display device) A Samsung GALAXY S4 equipped with an organic EL panel was disassembled, the circular polarizing plate was peeled off, and the circular polarizing plates (P-1) to (P-7) prepared in the above examples were attached to the display device with an adhesive so that the polarizer protective film was placed on the outside. (Display performance evaluation) (Front / Black display) The organic EL display device thus produced was made to display black, and was observed from the front in environments with different brightness levels. The reflected light was evaluated for blackness according to the following criteria. The results are shown in Table 1. 1: No reflected light is visible even in a 1000 lux environment. 2: Reflected light is visible in a 1000 lux environment, but not in a 100 lux environment. 3: Reflected light is visible in a 100 lux environment, but not in a 10 lux environment. 4: Reflected light is visible even in a 10 lux environment.

[0162] (Diagonal / White display) The organic EL display device thus fabricated was set to display white, and the color of the display device was observed from all directions at a polar angle of 45°. The azimuth angle dependency of the color change was evaluated according to the following criteria. The results are shown in Table 1. 1: The image appears white in all directions. 2: The image appears bluish only in certain directions. 3: The image appears bluish in all directions.

[0163] It should be noted that the optically isotropic members produced in Examples 1 to 5 were confirmed to be optically isotropic by measuring the retardation of slice samples by the Senarmont method described above. The average refractive index of the optically anisotropic layer and the refractive index of the optically isotropic member were measured by the method described above.

[0164] In Table 1, the "Liquid Crystal Type" column indicates the type of liquid crystal compound used to prepare the optically anisotropic layer and the optically isotropic member, and "normal wavelength dispersion" means a liquid crystal compound that exhibits normal wavelength dispersion, and "reverse wavelength dispersion" means a liquid crystal compound that exhibits reverse wavelength dispersion. In Table 1, the "optically anisotropic layer" column indicates the orientation state of the liquid crystal compound fixed in the optically anisotropic layer, with "homogeneous orientation / twisted orientation" meaning that the optically anisotropic layer contains regions in which homogeneously oriented liquid crystal compounds are fixed and regions in which twistedly oriented liquid crystal compounds are fixed, and "homogeneous orientation" meaning that the optically anisotropic layer is a layer in which homogeneously oriented liquid crystal compounds are fixed. In Table 1, the column "Convex portion" indicates the shape of the convex portion of the optically isotropic member. In Table 1, the column "Refractive index difference" indicates the absolute value of the difference between the average refractive index of the optically anisotropic layer and the refractive index of the optically isotropic member. In Table 1, the "Contact" column indicates "A" when the optically anisotropic layer and the optically isotropic member are in contact with each other in each Example and Comparative Example, and "B" when they are not in contact with each other.

[0165] [Table 1]

[0166] As shown in Table 1 above, it was confirmed that the optical element of the present invention exhibits the desired effects. In the display devices of Examples 1 and 2, the image was viewed as white in all directions in the oblique / white display, and the display performance was good. In the display performance of Example 3, the image was viewed as white when observed from a direction perpendicular to the direction in which the convex portion extends in the oblique / white display, but the image was observed as bluish when observed from a direction parallel to the direction in which the convex portion extends. In order to view the image of the display device of Example 3 as white in all directions, a method is available in which an optical element having an optically isotropic member having a stripe-shaped convex portion is separately prepared, and the separately prepared optical element is further laminated on the display device of Example 3 so that the direction in which the convex portion of the optically isotropic member in this optical element extends is perpendicular to the direction in which the convex portion of the optically isotropic member in the optical element included in the display device of Example 3 extends. In the display device of Example 4, the reflection at the interface between the optically anisotropic layer and the adhesive was suppressed by the convex portions (structural portions), so that reflected light was not visible in the front / black display, and the display performance was good. [Explanation of symbols]

[0167] 10A, 10B, 10C, 10D Optical elements 12, 12A Optically anisotropic layer 14A, 14B, 14C, 14D Optically isotropic members 16A, 16B, 16C, 16D Convex part 18A, 18B, 18C, 18D Base part 20,30 Board 22,32 Composition layer 24 Mold 26 Support 28 Convex 32A lower area 32B Upper area 32C,32D area

Claims

1. An optically anisotropic layer; an optically isotropic member; the optically anisotropic layer is in contact with the optically isotropic member, an absolute value of a difference between an average refractive index of the optically anisotropic layer and a refractive index of the optically isotropic member is within 0.08; the optically isotropic member is an optical element having a convex portion protruding on a side opposite to the optically anisotropic layer, The optical element, wherein the optically anisotropic layer and the optically isotropic member are both formed using a liquid crystal compound.

2. The optical element according to claim 1 , wherein the optically anisotropic layer and the optically isotropic member are both formed using the same liquid crystal compound.

3. The optical element according to claim 1 , wherein the optically anisotropic layer is a λ / 4 plate.

4. 4. The optical element according to claim 1, wherein the plurality of convex portions are periodically arranged.

5. 5. The optical element according to claim 4, wherein the intervals between the plurality of convex portions are 0.2 to 20 μm.

6. 6. The optical element according to claim 1, wherein the convex portions are arranged in a dot pattern or a stripe pattern.

7. 7. The optical element according to claim 1, wherein the width of the convex portion gradually increases from the side opposite to the optically anisotropic layer side of the convex portion toward the optically anisotropic layer side.

8. 8. A laminate comprising the optical element according to claim 1 and an adhesive layer disposed on the optical isotropic member side of the optical element.

9. A polarizer, the optical element according to any one of claims 1 to 7, and a display element, in this order; A display device, wherein the optically anisotropic layer in the optical element is disposed on the polarizer side.

10. Step 1 of forming a composition layer containing a liquid crystal compound having a polymerizable group on a substrate; A step 2 of subjecting the composition layer to a heat treatment to align the liquid crystal compound in the composition layer; a step 3 of irradiating the composition layer with light under a condition of an oxygen concentration of 1% by volume or more after the step 2; A step 4 of pressing a mold having a concave-convex structure on its surface against the surface of the composition layer opposite to the substrate to transfer the concave-convex structure of the mold to the composition layer; and step 5 of subjecting the composition layer to a curing treatment to form an optical element having an optically isotropic member having an optically anisotropic layer and a convex portion protruding from the substrate side to a side opposite to the optically anisotropic layer side, A method for producing an optical element that satisfies any one of the following requirements 1 to 4: Requirement 1: The step 4 is carried out under a heating condition equal to or higher than the phase transition temperature from a liquid crystal phase to an isotropic phase of the composition constituting the composition layer. Requirement 2: The step 5 is carried out under a heating condition equal to or higher than the phase transition temperature from a liquid crystal phase to an isotropic phase of the composition constituting the composition layer. Requirement 3: Between the steps 3 and 4, a step 6 of heating the composition layer to a temperature equal to or higher than the phase transition temperature from a liquid crystal phase to an isotropic phase of the composition constituting the composition layer is further included. Requirement 4: Between the step 4 and the step 5, a step 7 of heating the composition layer to a temperature equal to or higher than the phase transition temperature from a liquid crystal phase to an isotropic phase of the composition constituting the composition layer is further included.

Citation Information

Patent Citations

  • Polarizing plate protection film, polarizing plate and liquid crystal display apparatus using same

    JP2009014886A

  • Retardation substrate and method for manufacturing the same, and liquid crystal display device

    JP2010044283A

  • Diffraction grating integrated polarization conversion element

    JP2012003278A

  • Liquid crystal display module and liquid crystal display comprising the same