Semiconductor nanoparticles made of AgAuSe-based multicomponent compounds
AgAuSe-based semiconductor nanoparticles address the limitations of conventional nanoparticles by enhancing photoresponsiveness in near-infrared and short-wave infrared regions, providing improved optical properties and biocompatibility for various applications.
Patent Information
- Application Number
- JP2023010539
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-01-26
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2043-01-26
AI Technical Summary
Conventional semiconductor nanoparticles, particularly those containing Pb and Cd, are not suitable for near-infrared and short-wave infrared applications due to environmental and biocompatibility concerns, and lack optimal optical properties for these regions.
Development of AgAuSe-based semiconductor nanoparticles with a specific composition including Ag, Au, Se, and a metal M, such as In, to enhance photoresponsiveness in the near-infrared and short-wave infrared regions, utilizing a chalcogenide compound with a high chalcogen element content and optimized metal ratios.
The AgAuSe-based nanoparticles exhibit improved light absorption and emission characteristics in the long wavelength regions, offering biocompatibility and high quantum efficiency, suitable for applications in light-emitting devices, optical sensors, and photoelectric conversion elements.
Smart Images

Figure 0007580090000010 
Figure 0007580090000011 
Figure 0007580090000012
Abstract
Description
[Technical field]
[0001] The present invention relates to semiconductor nanoparticles made of a AgAuSe-based multi-component compound, and more particularly to semiconductor nanoparticles which are novel AgAuSe-based multi-component compounds composed of Ag, Au, Se and a metal M and have excellent optical semiconductor properties. [Background technology]
[0002] When semiconductors are made into nano-scale particles, they exhibit a quantum confinement effect and exhibit a band gap according to the particle size. Therefore, by controlling the composition and particle size of the semiconductor nanoparticles to adjust the band gap, it becomes possible to arbitrarily set the emission wavelength and absorption wavelength. Semiconductor nanoparticles utilizing this characteristic are also called quantum dots (QDs), and are expected to be used in various technical fields. Examples of applications of semiconductor nanoparticles include light-emitting elements and fluorescent substances used in display devices and marker substances for detecting biological substances. This is because semiconductor nanoparticles can control the emission wavelength by adjusting the particle size as described above, and also have a sufficiently narrow and stable emission peak width compared to organic dyes.
[0003] In addition, semiconductor nanoparticles have the characteristics of being able to control the absorption wavelength, having high quantum efficiency and a high absorption coefficient. As a result, semiconductor nanoparticles are being considered for use in photoelectric conversion elements and light receiving elements mounted on solar cells and various optical sensors. In particular, semiconductor nanoparticles are expected to be applied as light receiving elements of optical sensors corresponding to the near infrared region (NIR) and shortwave infrared region (SWIR). Optical sensors corresponding to these long wavelength regions are mounted on LIDAR (Light Detection and Ranging) and SWIR image sensors. LIDAR is a remote sensing system for automatic driving of automobiles, drones, ships, etc., and has become an important device in the recent development of automatic driving technology. In addition, SWIR image sensors are devices whose demand is expected to increase in the future in fields such as food inspection, agriculture, and drones. In the past, there have been many examples of Si thin films being applied to the light receiving elements of optical sensors. However, sensors using Si thin films have a significant decrease in sensitivity in the wavelength range of 900 nm or more, so they are not suitable for the above applications. For this reason, the development of light receiving elements using semiconductor nanoparticles is expected.
[0004] Specific examples of semiconductor nanoparticles that have been investigated so far include semiconductor nanoparticles made of binary compound semiconductors such as Group 11-Group 16 compound semiconductors, such as CdS, CdSe, CdTe, PbS, PbSe, and Ag2S, and ternary compound semiconductors such as Group 11-Group 13-Group 16 compound semiconductors, such as AgInTe2 (Patent Documents 1 to 4). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2004-243507 A [Patent Document 2] JP 2004-352594 A [Patent Document 3] JP 2017-014476 A [Patent Document 4] International Publication No. WO2020 / 054764 Summary of the Invention [Problem to be solved by the invention]
[0006] As mentioned above, semiconductor nanoparticles with various compositions are known, but semiconductor nanoparticles are still in the research stage, and the optimum ones have not yet been found with practical use in mind. In particular, there are few semiconductor nanoparticles that have suitable response characteristics corresponding to the above-mentioned near infrared region (NIR) and shortwave infrared region (SWIR).
[0007] Regarding the conventional semiconductor nanoparticles mentioned above, PbS nanoparticles are compatible with the near infrared region (NIR) and shortwave infrared region (SWIR). However, Pb is prohibited from use under the European RoHS Directive (Restriction of the use of certain Hazardous Substances, It is included in the list of specified hazardous substances whose use in electrical and electronic equipment is restricted by regulations, and from the perspective of environmental impact, it is difficult to say that this metal element should be used extensively in the future.
[0008] Furthermore, even when considering applications other than light-receiving elements such as optical sensors, some conventional semiconductor nanoparticles contain Cd in addition to Pb, and few can be used due to requirements such as biocompatibility (low toxicity composition).
[0009] Therefore, the present invention proposes semiconductor nanoparticles of a novel configuration not found in any reported examples so far, which have suitable optical semiconductor properties and also take into consideration practicality such as biocompatibility, etc. In particular, the present invention presents semiconductor nanoparticles that are compatible with the near infrared region (NIR) and shortwave infrared region (SWIR) and can exhibit suitable optical absorption and emission properties in these wavelength regions. [Means for solving the problem]
[0010] The present inventors have focused on semiconductor nanoparticles made of chalcogenide compounds containing two kinds of metals (noble metals), Ag and Au, as new semiconductor nanoparticles. As shown in the above-mentioned prior art, nanoparticles of Ag chalcogenide compounds (Ag2S) are known to exhibit optical semiconductor properties. Au also has the same potential. And, both the noble metals Ag and Au are relatively chemically stable metals, and have long been known as metals with biocompatibility. Therefore, it should be considered that a specific study of semiconductor nanoparticles of ternary chalcogenide compounds containing both Ag and Au has technical significance.
[0011] Furthermore, the present inventors have also investigated the optimization of chalcogen elements that constitute the compound together with Ag and Au, and have confirmed that semiconductor nanoparticles made of AgAuSe-based compounds, which are made of chalcogen elements essentially containing Ag, Au, and Se (selenium), have properties that can contribute to solving the problems of the present invention.
[0012] According to the study by the present inventors, from the viewpoint of only exhibiting optical semiconductor properties, suitable semiconductor nanoparticles can be constructed by using an AgAuS ternary compound in which S (sulfur) is used as a chalcogen element. However, the present inventors have confirmed that nanoparticles of the AgAuS ternary compound are insufficient with respect to the photoresponsiveness in the infrared region (NIR) and shortwave infrared region (SWIR), which is another object of the present invention. The present inventors have also confirmed that photoresponsiveness in the long wavelength region can be exhibited by using Se as an essential chalcogen element.
[0013] Therefore, the present inventors have investigated the properties of semiconductor nanoparticles made of AgAuSe-based compounds and have attempted to find an optimal structure based on the properties of the semiconductor nanoparticles. As a result, they have found nanoparticles made of AgAuSe-based multi-compounds in which a specific metal element (M) is added to the AgAuSe-based compound.
[0014] That is, the present invention, which solves the above-mentioned problems, is a semiconductor nanoparticle composed of a compound containing chalcogen elements, essential components of which are Ag, Au, and Se, and a metal M, wherein the metal M is at least one of Al, Ga, In, Tl, Zn, Cd, Hg, and Cu, and the compound is a semiconductor nanoparticle in which the total content of the chalcogen elements, essential components of which are Ag, Au, and Se, and the metal M is 95 mass% or more.
[0015] The structure of semiconductor nanoparticles made of AgAuSe-based multi-component compound semiconductors according to the present invention and the manufacturing method thereof will be described below. For convenience, in this specification, chalcogenide compounds composed of chalcogen elements including Ag, Au, and Se are referred to as "AgAuSe-based compounds". And, the multi-component chalcogenide compounds of quaternary or higher elements obtained by adding at least one metal M to the AgAuSe-based compounds, which are the subject of the present invention, will be referred to as "AgAuSe-based multi-component compounds".
[0016] A. Structure of the semiconductor nanoparticles according to the present invention A-1. Chemical composition of semiconductor nanoparticles As described above, the semiconductor nanoparticles according to the present invention are composed of an AgAuSe multi-element compound obtained by adding a metal M to an AgAuSe compound. In the present invention, Ag and Au are essential metals as metal elements (transition metal elements) constituting the AgAuSe compound, which is the basic compound of the present invention. The AgAuSe multi-element compound of the present invention changes its characteristics depending on the abundance ratio of Ag and Au in the compound. In the present invention, the ratio (x / (x+y)) of the number of Ag atoms to the total number of Ag atoms (x) and the number of Au atoms (y) in the compound constituting the nanoparticles is preferably 0.20 or more and 0.95 or less. The ratio of the number of Ag atoms is more preferably 0.40 or more, even more preferably 0.5 or more, and particularly preferably 0.6 or more. The ratio of the number of Ag atoms is more preferably 0.90 or less, even more preferably 0.88 or less. In these composition ranges, the effect of increasing the luminescence quantum efficiency and the like becomes clear.
[0017] Se is also an essential component element of the AgAuSe-based multi-element compound of the present invention. In the present invention, Se is selected as the chalcogen element in order to impart effective photoresponse characteristics to the semiconductor nanoparticles in both the near infrared region (NIR) and the shortwave infrared region (SWIR). The AgAuS ternary compound in which S is used as the chalcogen element exhibits effective photoresponse characteristics and emission peaks in the wavelength region near 800 nm, but tends to attenuate in the wavelength region of 900 nm or more. In the present invention, by using Se as the essential chalcogen element, it is possible to exhibit suitable photoresponse characteristics and emission peaks even in the wavelength region of 900 nm or more. It is presumed that this effect is caused by the orbital energy difference between each metal in the compound and the chalcogen element being reduced by using Se, which has a larger mass than S.
[0018] The chalcogen element having Se as an essential element is contained in the AgAuSe multi-component compound so that charge compensation is performed for Ag, Au, and metal M. Therefore, the content of the chalcogen element having Se as an essential element varies depending on the respective contents and valences of Ag, Au, and metal M. The content of the chalcogen element having Se as an essential element in the AgAuSe multi-component compound is preferably 25 atomic % or more and 60 atomic % or less. The content of the chalcogen element having Se as an essential element is more preferably 30 atomic % or more and 45 atomic % or less.
[0019] In the present invention, the metal M added to improve the properties of the AgAuSe compound is at least one of Al, Ga, In, Tl, Zn, Cd, Hg, and Cu, which are elements belonging to Groups 11 to 13. These metal elements cause property changes such as an improvement in the luminescence quantum efficiency of the AgAuSe compound and a shift in the absorption wavelength. More preferred examples of the metal M include In, Cu, Zn, and Ga.
[0020] The AgAuSe multi-element compound constituting the semiconductor nanoparticles according to the present invention changes its structure and properties depending on the type and content of metal M. The content of metal M in the compound is preferably 1 atomic % or more and 50 atomic % or less. If the content of metal M is less than 1 atomic %, there is essentially no difference from an AgAuSe compound. If the content of metal M exceeds 50 atomic %, the effect of improving properties such as quantum efficiency is greatly reduced. If metal M is an element belonging to Group 13 elements such as Al, Ga, or In, the content of metal M is more preferably 1 atomic % or more and 15 atomic % or less.
[0021] The semiconductor nanoparticles according to the present invention are composed of an AgAuSe-based multi-component compound having Ag, Au, and Se as essential chalcogen elements and metal M as essential constituent elements. In this AgAuSe-based multi-component compound, the total content of the chalcogen elements Ag, Au, and Se as essential chalcogen elements and metal M is 95% by mass or more relative to the entire compound. Elements that may be contained other than the essential constituent elements Ag, Au, Se, and metal M include Ge, Si, Sn, Pb, O, etc., and these elements are acceptable if they are less than 5% by mass. However, the compound preferably has a total content of the chalcogen elements Ag, Au, and Se as essential chalcogen elements and metal M of 99% by mass or more, more preferably 99.9% by mass or more. The composition value of the compound here is the value of the AgAuSe-based multi-component compound constituting the semiconductor nanoparticles, and does not include the components of the protective agent described below.
[0022] In addition, the AgAuSe-based multi-component compound constituting the semiconductor nanoparticles according to the present invention contains Se as an essential chalcogen element, so it may contain chalcogen elements other than Se, such as S. For example, in the manufacturing process of semiconductor nanoparticles described later, when a chalcogen element other than Se is used during doping of metal M, semiconductor nanoparticles containing Se and S may be formed. However, from the viewpoint of photoresponse and luminescence quantum efficiency in the long wavelength region, a particularly preferred embodiment is a semiconductor nanoparticle of an AgAuSe-based multi-component compound in which only Se is the chalcogen element. In this case, the preferred range of the Se content is the same as the preferred range of the content of the chalcogen element described above.
[0023] A-2. Structure of the semiconductor nanoparticles according to the present invention Regarding the structure of the semiconductor nanoparticles made of the AgAuSe multi-component compound of the present invention, there is no particular limitation on the distribution state of each atom of the constituent elements Ag, Au, Se, and metal M. The structure of the compound constituting the semiconductor nanoparticles includes a compound in which an AgAuSe compound containing Ag, Au, or Se is doped with metal M. In this case, doping refers to a state in which metal M atoms are substituted and / or interstitially inserted into the crystal lattice of the semiconductor compound crystal made of the AgAuSe compound.
[0024] In addition, the compound constituting the semiconductor nanoparticles of the present invention may be composed of a single phase, but may also be composed of multiple phases. Particles composed of multiple phases may have a so-called core-shell structure. In the core-shell structure, an AgAuSe-based compound containing Ag, Au, and Se becomes a core compound (core compound), and a metal M or a compound essentially containing metal M and containing at least one of Ag, Au, and Se becomes a shell (shell compound), and the shell may have a structure that covers at least a part of the surface of the core compound. With respect to semiconductor nanoparticles of a core-shell structure, it is considered that the metal M in the shell modifies the surface defects of the AgAuSe-based compound that becomes the core, leading to improved properties of the AgAuSe-based compound. In this case, the shell compound may be composed of only metal M, or may be composed of a compound of metal M and at least one of Ag, Au, and Se (for example, AgMSe2, etc.), or may be a mixture of them. In any of these structures, the element distribution in the AgAuSe-based multi-element compound that becomes the semiconductor nanoparticles may be regular or irregular.
[0025] In addition, a scanning transmission electron microscope (Scanning TEM) can be suitably used in the analysis of the composition and structure of the semiconductor nanoparticles according to the present invention. In particular, a high angle annular dark field scanning transmission microscope (HAADF-STEM) can provide a scattering image reflecting the composition information of the nanoparticles, and by combining it with an energy dispersive X-ray spectrometer (EDX) or the like, the distribution state of Ag, Au, Se, and metal M and the composition of the entire nanoparticles can be grasped.
[0026] The semiconductor nanoparticles according to the present invention preferably have an average particle size of 2 nm or more and 20 nm or less. The particle size of the semiconductor nanoparticles is related to the band gap adjustment action due to the quantum confinement effect. In order to exhibit suitable light emission and light absorption properties by adjusting the band gap, it is preferable to set the average particle size as described above. The average particle size of the semiconductor nanoparticles can be obtained by observing a plurality of particles (preferably 100 or more) using an electron microscope such as a TEM, measuring the particle size of each particle, and calculating the particle number average.
[0027] A-3. Optical semiconductor properties of the semiconductor nanoparticles according to the present invention As described above, the band gap of the semiconductor nanoparticles is adjusted by the quantum confinement effect according to the particle size, and the light absorption characteristics change. In the semiconductor nanoparticles according to the present invention, the absorption edge wavelength on the long wavelength side of the absorption spectrum is preferably 800 nm or more. This allows the semiconductor nanoparticles to have absorptivity and responsiveness to light in the visible light region to the near infrared region. In a more preferred embodiment, the present invention can provide semiconductor nanoparticles having an absorption edge wavelength on the long wavelength side of the absorption spectrum of 850 nm or more. In addition, in the semiconductor nanoparticles according to the present invention, the peak wavelength of the emission spectrum is preferably in a wavelength region longer than 900 nm, more preferably in a wavelength region longer than 1000 nm, in the measurement of the emission spectrum.
[0028] A-4. Use of the semiconductor nanoparticles according to the present invention The semiconductor nanoparticles according to the present invention can be applied to the above-mentioned various uses such as light-emitting devices by coating and supporting them on an appropriate substrate or carrier. There are no particular limitations on the configuration, shape, and dimensions of the substrate or carrier. Examples of the substrate in the form of a plate or foil or film include glass, quartz, silicon, ceramics, and metals. Examples of the granular or powdered carrier include inorganic oxides such as ZnO, TiO2, WO3, SnO2, In2O3, and Al2O3. The semiconductor nanoparticles may be supported on the inorganic oxide carrier and then fixed to the substrate.
[0029] In addition, when semiconductor nanoparticles are applied to and supported on a substrate or carrier, as described above, a solution, slurry, or ink in which semiconductor nanoparticles are dispersed in an appropriate dispersion medium is often used. As the dispersion medium for this solution, chloroform, toluene, cyclohexane, hexane, etc. can be used. As a method for applying the solution of semiconductor nanoparticles, dipping or spin coating can be used, and as a method for supporting, various methods such as a dropping method, an impregnation method, or an adsorption method can be used.
[0030] In addition, the semiconductor nanoparticles according to the present invention preferably contain a protective agent to suppress aggregation during the synthesis process or when dispersed in a dispersion medium as described above. As the protective agent, at least one of alkylamines having 4 to 20 carbon atoms in the alkyl chain, alkenylamines having 4 to 20 carbon atoms in the alkenyl chain, alkylcarboxylic acids having 3 to 20 carbon atoms in the alkyl chain, alkenylcarboxylic acids having 3 to 20 carbon atoms in the alkenyl chain, alkanethiols having 4 to 20 carbon atoms in the alkyl chain, trialkylphosphines having 4 to 20 carbon atoms in the alkyl chain, trialkylphosphine oxides having 4 to 20 carbon atoms in the alkyl chain, triphenylphosphine, and triphenylphosphine oxide is preferable. These protective agents are bonded to the surface of the semiconductor nanoparticles to cover at least a part of them, and the dispersion liquid suppresses the aggregation of the semiconductor nanoparticles to form a uniform solution. In addition, by adding a protective agent to the reaction system together with the raw materials in the synthesis process of the semiconductor nanoparticles, nanoparticles having a suitable average particle size are synthesized. The protecting agent may be any of the above-mentioned alkylamines, alkenylamines, alkylcarboxylic acids, alkenylcarboxylic acids, alkanethiols, trialkylphosphines, trialkylphosphine oxides, triphenylphosphine, and triphenylphosphine oxides, used alone or in combination.
[0031] B. Method for producing semiconductor nanoparticles according to the present invention Next, a method for producing semiconductor nanoparticles according to the present invention will be described. The semiconductor nanoparticles according to the present invention are made of an AgAuSe multi-element compound in which an AgAuSe compound is doped with metal M. The method for producing nanoparticles of this AgAuSe multi-element compound includes, first, a method for synthesizing an AgAuSe multi-element compound by simultaneously reacting precursors containing Ag, Au, Se, and metal M (Ag precursor, Au precursor, Se precursor, metal M precursor) (this synthesis method is sometimes called direct synthesis). As a second production method, there is a method for synthesizing nanoparticles of an AgAuSe compound, and adding / doping metal M to the nanoparticles to synthesize an AgAuSe multi-element compound (this synthesis method is sometimes called two-step synthesis). Hereinafter, a method for producing semiconductor nanoparticles using each synthesis method will be described.
[0032] B-1. Method for producing semiconductor nanoparticles by direct synthesis When nanoparticles of AgAuSe-based multi-component compounds are produced by direct synthesis, Ag precursors, Au precursors, Se precursors, and metal M precursors are mixed in a reaction solvent, and the reaction system consisting of these is heated at a temperature of 30°C or higher and 200°C or lower.
[0033] The Ag precursor and Au precursor are Ag salt or Ag complex and Au salt or Au complex, respectively. The Ag precursor and Au precursor are preferably salts or complexes containing monovalent Ag and monovalent Au. However, the Au precursor may be a precursor containing trivalent Au. This is because, in the synthesis process of semiconductor nanoparticles, trivalent Au is reduced to monovalent Au by the solvent or coexisting Se precursor.
[0034] Suitable Ag precursors include silver acetate (Ag(OAc)), silver nitrate, silver carbonate, silver oxide, silver oxalate, silver chloride, silver iodide, silver(I) cyanide, and silver diethyldithiocarbamate. Suitable Au precursors include chloro(dimethylsulfide)gold(I) ((CH3)2SAuCl), Au resinate (C 10 H 18 Au2S2: CAS68990-27-2), gold iodide(I), gold sulfite(I) salt, chloroauric acid(III), gold acetate(III), gold cyanide(I) salt, gold cyanide(III) salt, 1,10-phenanthroline gold(III), etc.
[0035] As the Se compound serving as the Se precursor, in addition to powdered selenium, Selenourea (Se=C(NH2)2), selenocysteine, trioctylphosphine selenide, triphenylphosphine selenide, diphenyl diselenide, dibenzyl diselenide, and other Se compounds can be used.
[0036] Compounds that can be metal M precursors include chlorides, sulfides, nitrates, acetates, sulfates, sulfamates, stearates, and the like of metal M. Examples include indium chloride, indium acetate, indium diethyldithiocarbamate, copper chloride, copper acetate, zinc stearate, zinc acetate, and the like.
[0037] The composition of the AgAuSe multi-element compound to be synthesized can be adjusted by the ratio of the amount of Ag precursor and the amount of Au precursor charged. The amount of Ag precursor and the amount of Au precursor charged to obtain a suitable AgAuSe multi-element compound is preferably set so that the ratio of the number of Ag atoms to the total number of Ag atoms (a / (a+b): hereinafter sometimes referred to as Ag charge ratio) is 0.20 or more and 0.95 or less, when the number of Ag atoms in the Ag precursor is a and the number of Au atoms in the Au precursor is b. It is more preferable that the Ag charge ratio is 0.4 or more.
[0038] The amount of the Se precursor in the reaction system can be set in a relatively wide range relative to the amounts of Ag, Au, and metal M. This is because the Se precursor has little effect on the composition of the AgAuSe multi-element compound even if there is excess Se in the reaction system.
[0039] In addition, as described above, the semiconductor nanoparticles of the present invention preferably have a protective agent bonded to the AgAuSe multi-element compound. Therefore, it is preferable to add a protective agent to the above-mentioned reaction system together with the Ag precursor, the Au precursor, etc. As the protective agent, it is preferable to add at least one of alkylamines having an alkyl chain carbon number of 4 to 20, alkenylamines having an alkenyl chain carbon number of 4 to 20, alkylcarboxylic acids having an alkyl chain carbon number of 3 to 20, alkenylcarboxylic acids having an alkenyl chain carbon number of 3 to 20, alkanethiols having an alkyl chain carbon number of 4 to 20, trialkylphosphines having an alkyl chain carbon number of 4 to 20, trialkylphosphine oxides having an alkyl chain carbon number of 4 to 20, triphenylphosphine, and triphenylphosphine oxide.
[0040] Although the reaction system for synthesizing semiconductor nanoparticles can produce nanoparticles without a solvent, it is preferable to use a solvent. When a solvent is used, octadecene, tetradecane, oleic acid, oleylamine, dodecanethiol, or a mixture thereof can be used.
[0041] Then, AgAuSe multi-element compound nanoparticles are synthesized by heating the reaction system consisting of the Ag precursor, Au precursor, Se precursor, metal M precursor, and protective agent. The heating temperature (reaction temperature) at this time is 30°C or more and 200°C or less. If the temperature is less than 30°C, the synthesis of the AgAuSe multi-element compound is difficult to proceed. On the other hand, if the temperature exceeds 200°C, there is a problem that Au alone forms nanoparticles and a compound with the desired composition may not be produced. The average particle size of the semiconductor nanoparticles increases with an increase in the reaction temperature, but it rarely exceeds the preferred average particle size within the above temperature range. A more preferred reaction temperature is 40°C or more and 120°C or less.
[0042] The reaction time (heating time) can be adjusted depending on the amount of raw materials charged, but is preferably 5 minutes or more and 120 minutes or less. The reaction time is more preferably 10 minutes or more, and even more preferably 15 minutes or more. It is preferable to stir the reaction system during the synthesis reaction of the semiconductor nanoparticles.
[0043] After the synthesis reaction of the semiconductor nanoparticles is completed, the reaction system is cooled as necessary, and the semiconductor nanoparticles are recovered. At this time, the nanoparticles are precipitated by adding a non-solvent alcohol (ethanol, methanol, etc.), or the semiconductor nanoparticles are precipitated and recovered by centrifugation or the like, and the particles are further washed with alcohol (ethanol, methanol, etc.) or the like, and then uniformly dispersed in a good solvent such as chloroform.
[0044] B-2. Method for producing semiconductor nanoparticles by two-step synthesis The semiconductor nanoparticles of the AgAuSe-based multi-component compound according to the present invention can also be produced by doping nanoparticles of the AgAuSe-based compound with a metal M. In this case, the AgAuSe-based compound is synthesized, and then reacted with a metal M precursor to synthesize the AgAuSe-based multi-component compound.
[0045] Nanoparticles of AgAuSe-based compounds can be synthesized by mixing an Ag precursor, an Au precursor, and an Se precursor in a reaction solvent and heating the reaction system formed from these at a temperature of 30°C or higher and 200°C or lower.
[0046] The Ag precursor, Au precursor, and Se precursor, which are the raw materials of the AgAuSe compound, can be the same metal salts and metal complexes as those used in the direct synthesis of the AgAuSe multi-component compound described above. The amounts of the Ag precursor, Au precursor, and Se precursor used in the synthesis of the AgAuSe compound can also be the same as those used in the direct synthesis of the AgAuSe multi-component compound. Furthermore, the use of solvents and protective agents for forming a reaction system is set in the same manner as in the direct synthesis of the AgAuSe multi-component compound.
[0047] The heating temperature (reaction temperature) of the reaction system consisting of the Ag precursor, Au precursor, Se precursor and protective agent is 30°C or higher and 200°C or lower. If the temperature is lower than 30°C, the synthesis of the AgAuSe compound does not proceed easily. A more suitable reaction temperature is 40°C or higher and 120°C or lower. The heating time (reaction time) is preferably 1 minute or higher and 120 minutes or lower. After the synthesis reaction of the semiconductor nanoparticles of the AgAuSe compound is completed, they can be recovered in the same manner as described above, and then used for doping with the metal M.
[0048] The nanoparticles of AgAuSe-based compounds synthesized as described above are compounds represented by the composition formulas Ag1Au7Se4, AgAu3Se2, Ag3Au5Se4, AgAuSe, Ag5Au3Se4, Ag3AuSe2, and Ag7AuSe4, or compounds that approximate the composition formulas. However, in addition to the compounds of stoichiometric composition as described above, compounds of compositions not in the stoichiometric composition as described above can be mentioned. These may be stoichiometric compositions, may not be stoichiometric compositions, or may be mixed phases thereof.
[0049] Although the doping of the metal M into the AgAuSe compound can be performed without a solvent, it is preferable to do so in a solvent. The same solvent as that used in the reaction system of the AgAuSe compound described above can be used. The reaction system containing the nanoparticles of the AgAuSe compound produced above may be used as is, or the nanoparticles may be recovered by the above separation means and then redispersed in a solvent to form a reaction system.
[0050] In the process of adding metal M to AgAuSe-based compound nanoparticles, a compound of metal M is added as a metal M precursor to the reaction system, mixed, and heated. The metal M precursor can be the same metal salt or metal complex as in the direct synthesis of AgAuSe-based multi-element compounds. The preferred range of the amount of metal M precursor added to the reaction system is the same as in the direct synthesis.
[0051] In addition, when doping metal M in two-step synthesis, a chalcogen element may be added to the reaction system together with the metal M precursor for charge compensation to make the AgAuSe compound into an AgAuSe multi-element compound. The chalcogen element at this time is not limited to Se, and S may be added. For example, in addition to elemental sulfur, compounds such as thiourea, alkylthiourea, thioacetamide, and alkanethiol, β-dithiones, dithiols, xanthates, and diethyldithiocarbamate may be added. However, the addition of a chalcogen element is not essential when doping metal M into AgAuSe compound nanoparticles.
[0052] The doping of metal M proceeds by heating a reaction system containing an AgAuSe compound, a metal M precursor, and an optionally added chalcogen element. The heating temperature is preferably 30°C or more and 200°C or less. If the temperature is less than 30°C, the doping of metal M does not proceed easily. On the other hand, if the temperature exceeds 200°C, the AgAuSe compound may decompose. A more suitable reaction temperature is 100°C or more and 150°C or less. The heating time (reaction time) can be adjusted depending on the amount of each component in the reaction system, and is preferably 5 minutes or more and 60 minutes or less. It is preferable to stir the reaction system.
[0053] Semiconductor nanoparticles made of AgAuSe-based multi-compounds can be synthesized by the reaction step of adding the metal M. Thereafter, the semiconductor nanoparticles can be collected in the same manner as in the direct synthesis manufacturing method. Effect of the Invention
[0054] As described above, the present invention relates to semiconductor nanoparticles made of AgAuSe-based multi-component compounds obtained by adding metal M to AgAuSe-based compounds. AgAuSe-based compounds exhibit optical semiconductor properties when made into nanoparticles, and further suitable properties are exhibited by adding metal M such as In to the AgAuSe-based compounds.
[0055] The semiconductor nanoparticles made of the AgAuSe-based multi-compound according to the present invention are expected to be applied to markers for use in the body in addition to general semiconductor devices such as light-emitting elements, since their main constituent elements are low-toxicity elements with biocompatibility.
[0056] Furthermore, the semiconductor nanoparticles according to the present invention have improved light emission and light absorption properties in the near-infrared region. In recent years, photoelectric conversion elements for which responsiveness in the near-infrared region is important include light receiving elements applied to LIDAR and SWIR image sensors. The semiconductor nanoparticles according to the present invention are expected to be used in such photoelectric conversion elements operating in the near-infrared region. [Brief description of the drawings]
[0057] [Figure 1] TEM images of semiconductor nanoparticles of Example 1 and Example 2 (AgAuSeIn), Reference Example 1 (AgAuSe), and Reference Example 2 (AgAuS) of the first embodiment. [Diagram 2] 4 shows absorption spectra of semiconductor nanoparticles of Example 1 and Example 2 (AgAuSeIn) of the first embodiment. [Diagram 3] 4 shows absorption spectra of semiconductor nanoparticles of Reference Example 1 (AgAuSe) and Reference Example 2 (AgAuS) of the first embodiment. [Figure 4] 1 shows emission spectra of semiconductor nanoparticles of Example 1 and Example 2 (AgAuSeIn) of the first embodiment. [Diagram 5] 4 shows emission spectra of Reference Example 1 (AgAuSe) and Reference Example 2 (AgAuS) of the first embodiment. [Figure 6] TEM image of AgAuSeIn nanoparticles synthesized by adjusting the amount of In added in the second embodiment. [Figure 7] 13 shows the results of measuring the absorption spectrum of AgAuSeIn nanoparticles synthesized by adjusting the amount of In added in the second embodiment. [Figure 8] 13 is an emission spectrum of AgAuSeIn nanoparticles synthesized by adjusting the amount of In added in the second embodiment. [Figure 9a] TEM image of AgAuSeIn nanoparticles synthesized in a reaction time of 20 minutes by adjusting the Ag charging ratio in the third embodiment. [Figure 9b] TEM image of AgAuSeIn nanoparticles synthesized in a reaction time of 10 minutes by adjusting the Ag charging ratio in the third embodiment. [Figure 10a] 13 shows an absorption spectrum of AgAuSeIn nanoparticles synthesized in a reaction time of 20 minutes by adjusting the Ag charging ratio in the third embodiment. [Figure 10b] 13 shows an absorption spectrum of AgAuSeIn nanoparticles synthesized in a reaction time of 10 minutes by adjusting the Ag charging ratio in the third embodiment. [Figure 11a] 13 shows an emission spectrum of AgAuSeIn nanoparticles synthesized in the third embodiment with the Ag charging ratio adjusted and the reaction time set to 20 minutes. [Figure 11b]13 shows an emission spectrum of AgAuSeIn nanoparticles synthesized in the third embodiment with a reaction time of 10 minutes by adjusting the Ag charging ratio. [Figure 12] 13 shows XRD diffraction patterns of AgAuSeIn nanoparticles (reaction times 20 minutes and 10 minutes) synthesized in the third embodiment with Ag loading ratios of 0.5 and 0.75. [Figure 13] 13 is a TEM image of AgAuSeIn nanoparticles synthesized by adjusting the reaction time in the fourth embodiment. [Figure 14] 13 shows an absorption spectrum of AgAuSeIn nanoparticles synthesized by adjusting the reaction time in the fourth embodiment. [Figure 15] 13 shows an emission spectrum of AgAuSeIn nanoparticles synthesized by adjusting the reaction time in the fourth embodiment. [Figure 16] 13 shows XRD diffraction patterns of AgAuSeIn nanoparticles synthesized in the fourth embodiment with reaction times of 0.5 and 0.75. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0058] First embodiment Hereinafter, an embodiment of the present invention will be described. In this embodiment, semiconductor nanoparticles made of AgAuSe-based multi-component compound (AgAuSeIn) containing In as metal M were synthesized by the above-mentioned two synthesis methods. Then, their composition analysis was performed and their photoresponse characteristics were evaluated.
[0059] Example 1 In this example, AgAuSeIn nanoparticles were synthesized by direct synthesis. 0.075 mmol of silver acetate (Ag(OAc)) as the Ag precursor, 0.025 mmol of chloro(dimethylsulfide)gold(I) as the Au precursor, 0.10 mmol of indium acetate (In(OAc)3) as the In precursor, which is the metal M, and 0.20 mmol of selenourea as the Se precursor were placed in a test tube. 2.9 mL of oleylamine (OLA) as a solvent and 0.1 mL of 1-dodecanethiol (DDT) as a protective agent were added to the tube.
[0060] A stirrer was placed in the test tube containing the above raw materials and solvent, and the mixture was replaced with nitrogen three times, after which the reaction temperature was set to 50°C and the mixture was heated and stirred for 10 minutes using a hot stirrer. After the reaction was completed, the mixture was left to cool for 20 minutes, then transferred to a small test tube and centrifuged at 4000 rpm for 5 minutes to separate the supernatant and precipitate.
[0061] Then, add 4 cm of methanol as a poor solvent to the supernatant. 3 The mixture was added to the flask to cause precipitation, which was then centrifuged at 4,000 rpm for 5 minutes to collect the precipitate. 3 After adding and dispersing, centrifugation was performed under the same conditions to remove by-products and solvent, and the nanoparticles of the AgAuSeIn compound were purified.
[0062] The nanoparticles of AgAuSeIn compound obtained by the above procedure were dissolved in 3 cm of chloroform. 3 This dispersion was transferred to a sample bottle and purged with nitrogen, after which it was stored in a refrigerator in a dark place.
[0063] Example 2 In this example, AgAuSeIn nanoparticles were synthesized by a two-step synthesis. In this example, first, AgAuSe nanoparticles, which is an AgAuSe-based compound, were synthesized, and then In was doped to synthesize AgAuSeIn nanoparticles.
[0064] To synthesize AgAuSe nanoparticles, 0.3 mmol of silver acetate as the Ag precursor, 0.1 mmol of chloro(dimethylsulfide)gold(I) as the Au precursor, and 0.20 mmol of selenourea as the Se precursor were placed in a test tube, along with 2.9 mL of oleylamine as a solvent and 0.1 mL of 1-dodecanethiol as a protective agent.
[0065] After replacing the inside of the test tube with nitrogen, the reaction temperature was set to 50°C and the mixture was stirred with heating for 10 minutes using a hot stirrer. After the reaction was completed, the mixture was left to cool for 20 minutes, then transferred to a small test tube and centrifuged at 4000 rpm for 5 minutes to separate the supernatant and precipitate. After that, the mixture was recovered and purified in the same manner as in Example 1 to obtain AgAuSe nanoparticles.
[0066] The AgAuSe nanoparticles obtained above were then 1.0 × 10 -5 mmol and 4.13 × 10 In precursor indium chloride (InCl3). -6 6.19 x 10 mol of the S compound thioacetamide -6 mol was mixed with 3.0 mL of dehydrated oleylamine as a solvent, and heated to dope In into the AgAuSe nanoparticles. The heating temperature was 110°C and the mixture was heated for 15 minutes. After the reaction was completed, the mixture was allowed to cool for 20 minutes, then transferred to a small test tube and centrifuged at 4000 rpm for 5 minutes to separate the supernatant and precipitate. After that, the mixture was purified in the same manner as above, and the AgAuSe(S)In nanoparticles were collected and made into a dispersion in the same manner as in Example 1.
[0067] Reference example 1 In order to confirm the effect of doping an AgAuSe compound with In (metal M), the nanoparticles of the AgAuSe compound synthesized in Example 2 above were evaluated without doping with In.
[0068] Reference example 2 Nanoparticles of the AgAuS ternary compound, in which S is used as a chalcogen element that forms a compound with Ag and Au, were synthesized as follows.
[0069] 0.3 mmol of silver acetate as the Ag precursor, 0.1 mmol of chloro(dimethylsulfide)gold(I) as the Au precursor, and 0.2 mmol of thiourea as the S precursor were placed in a test tube, and 2.9 mL of oleylamine as a solvent and 0.1 mL of 1-dodecanethiol as a protective agent were added.
[0070] Then, after replacing the atmosphere with nitrogen in the same manner as above, the mixture was stirred with heating for 10 minutes at a reaction temperature of 150° C. using a hot stirrer. After the reaction was completed, the mixture was left to cool for 30 minutes, transferred to a small test tube, and centrifuged at 4000 rpm for 5 minutes to separate the supernatant and precipitate.
[0071] Thereafter, in the same manner as in Example 1, centrifugal separation and purification were carried out to obtain a dispersion of nanoparticles of an AgAuS ternary compound.
[0072] [TEM observation and average particle size measurement] TEM observation was performed on each of the nanoparticles of Example 1 and Example 2 (AgAuSeIn), Reference Example 1 (AgAuSe), and Reference Example 2 (AgAuS). FIG. 1 shows a TEM image of each of the semiconductor nanoparticles produced (for the magnification, see the scale bar of each photograph). From each TEM image, it was confirmed that approximately spherical nanoparticles were synthesized. Then, based on the TEM image, the average particle size of the nanoparticles of each composition was measured and calculated. In the particle size measurement, the particle size was obtained for all measurable nanoparticles included in the TEM image, and the average particle size was calculated.
[0073] [Nanoparticle composition analysis] In addition to the above TEM observation, EDX analysis was performed to analyze the composition of the nanoparticles. Table 1 shows the results of measuring the composition of each semiconductor nanoparticle. In this embodiment and each of the following embodiments, the results of the composition analysis are shown in atomic % relative to the total nanoparticles. Table 1 also shows the ratio (x / (x+y)) of the number of Ag atoms to the total number of Ag atoms (x) and Au atoms (y) calculated based on the results of the composition analysis.
[0074] [Table 1]
[0075] [Measurement of absorption and emission spectra] Next, the absorption spectrum was measured for each of the semiconductor nanoparticles of Examples 1 and 2 and Reference Examples 1 and 2. The absorption spectrum was measured using an ultraviolet-visible spectrophotometer (Agilent 8453, manufactured by Agilent Technologies Inc.) in the wavelength range of 400 nm to 1100 nm.
[0076] Furthermore, the emission spectrum and emission quantum efficiency of each nanoparticle were measured. The emission spectrum was measured using a diode array spectrophotometer (PMA-12, C10027-02) manufactured by Hamamatsu Photonics K.K. The sample was dissolved in chloroform (n=1.4429) and adjusted so that the absorbance at 365 nm was 0.1, and the measurement was performed.
[0077] The emission quantum yield in the wavelength region of 900 nm or less was measured using an absolute PL quantum yield measurement device (C9920-03, manufactured by Hamamatsu Photonics KK). When emission was observed at wavelengths longer than 1000 nm, the emission spectrum was measured using a multichannel spectrophotometer (Hamamatsu Photonics, PMA-12 (model number: C10027-02 (wavelength range 350-1100 nm) and 10028-01 (wavelength range 900-1650 nm)). At this time, the sample was adjusted to a chloroform solution (n = 1.4429) so that the absorbance at 700 nm was 0.1, and the measurement was performed. The excitation light wavelength was 700 nm. The emission quantum yield in the near-infrared region was calculated by measuring the emission spectrum measured by the fluorescence spectrophotometer and measuring the emission spectrum of an ethanol solution (n = 1.3618) of indocyanine green (ICG: Φ = 13.2%), a near-infrared emitting organic fluorescent dye, as a standard sample, and calculating the emission quantum yield of each sample by the relative method using the following formula.
[0078]
number
[0079] The measurement results of the absorption spectrum of each semiconductor nanoparticle produced in this embodiment are shown in Figures 2 and 3. The measurement results of the emission spectrum are shown in Figures 4 and 5. Table 2 summarizes the relationship between the emission wavelength and the emission quantum yield of each semiconductor nanoparticle.
[0080] [Table 2]
[0081] Referring to FIG. 3, Example 1 (AgAuSeIn) and Example 2 (AgAuSe(S)In) containing Se as an essential chalcogen element In the case of Reference Example 1 (AgAuSe), the absorption edge wavelength is 900 nm or more. only The absorption edge wavelength is longer than that of Reference Example 2 (AgAuS) in 2. It can be seen that the photoresponse in the long wavelength region is improved by using Se as the chalcogen element.
[0082] 4, the AgAuSeIn nanoparticles of Examples 1 and 2, in which AgAuSe is doped with In, exhibit an emission peak at approximately the same position (about 980 to 1000 nm) as the nanoparticles (AgAuSe, FIG. 5) of Reference Example 1, and further exhibit an emission peak position on the longer wavelength side than the emission peak (about 780 nm) of Reference Example 2 (AgAuS, FIG. 5). This result confirms that by using Se as an essential chalcogen element, it is possible to address photoresponse characteristics in the long wavelength region.
[0083] In addition, by comparing Examples 1 and 2 with Reference Example 1, it is confirmed that the effect of doping In (metal M) into the AgAuS-based compound is an increase in luminescence quantum efficiency. In particular, the AgAuSeIn nanoparticles of Example 1 synthesized by direct synthesis showed extremely good quantum efficiency. From the results of this embodiment, it was confirmed that in order to form suitable semiconductor nanoparticles, it is preferable to dope In (metal M) based on an AgAuSe-based compound that requires Se as a chalcogen element, and this allows for compatibility with the long wavelength region as well as excellent luminescence characteristics.
[0084] Second embodiment In response to the favorable results of the AgAuSeIn nanoparticles of the first embodiment, in this embodiment, the change in characteristics depending on the amount of In doped in the AgAuSeIn nanoparticles was investigated.
[0085] The synthesis of AgAuSeIn nanoparticles in this embodiment was basically in accordance with Example 1 (direct synthesis) of the first embodiment. That is, indium acetate and selenourea, which are In precursors, were placed in a test tube together with 0.075 mmol of silver acetate and 0.025 mmol of chloro(dimethylsulfide)gold(I), and 2.9 mL of a solvent (oleylamine) and 0.1 mL of a protective agent (1-dodecanethiol) were added to synthesize AgAuSeIn nanoparticles. The reaction conditions were a heating temperature of 50°C and a reaction time of 10 minutes, and the treatments before and after the reaction were the same as those in Example 1.
[0086] In this embodiment, the amount of In added in Example 1 (0.1 mmol) was taken as "1x" as the standard, and 0.5x, 0.75x, 0.88x, 1.25x, 1.5x, 2x, and 4x the amount of In added to the reaction system. In addition, taking into consideration the positive charges of Ag, Au, and In from the amount of In added in each sample, the amount of Se (selenourea) added was adjusted so that the negative charge was equal to this.
[0087] The AgAuSeIn nanoparticles synthesized with each In doping amount were subjected to TEM observation and composition analysis in the same manner as in the first embodiment. Figure 6 shows TEM images of AgAuSeIn nanoparticles with various In doping amounts (feed amount: 0.5 times, 0.75 times, 0.88 times, 1 time, 1.25 times, 1.5 times, 2 times, 4 times). The results of the composition analysis of these semiconductor nanoparticles are shown in Table 3.
[0088] [Table 3]
[0089] From Table 3, it can be seen that there is no significant difference in the In content of the AgAuSeIn nanoparticles when the amount of In added is changed between 0.5 and 1.25 times. The In content increases significantly when the amount of In added is 1.5 times or more.
[0090] The absorption spectrum, emission spectrum, and luminescence quantum efficiency of the AgAuSeIn synthesized in this embodiment were measured in the same manner as in the nanoparticle embodiment 1. The measurement results of the absorption spectrum and the measurement results of the emission spectrum of the semiconductor nanoparticles (In loading amount: 0.5 times, 0.75 times, 0.88 times, 1 time, 1.25 times, 1.5 times, 2 times, 4 times) produced in this embodiment are shown in Figure 7 and Figure 8, respectively. The peak wavelengths of the emission spectra and the luminescence quantum efficiency are summarized in Table 4.
[0091] [Table 4]
[0092] Referring to the absorption spectrum curves in Figure 7, AgAuSeIn nanoparticles with 0.5 and 0.75 times the amount of In shown similar curves, showing a small peak thought to be an exciton peak near 850 nm and having an absorption edge near 1040 nm. AgAuSeIn nanoparticles with 0.88 and 1 times the amount of In shown curves almost overlap, showing a small peak thought to be an exciton peak near 780 nm, and having absorption edges near 850 nm and 1000 nm. And AgAuSeIn nanoparticles with 1.25 times or more the amount of In shown no small peak thought to be an exciton peak is seen, and the absorption edge is near 1040 nm.
[0093] Next, the measurement results of the emission spectrum in Fig. 8 and Table 4 will be referred to. Compared with the AgAuSeIn nanoparticles of Reference Example 2 of the first embodiment, the AgAuSeIn nanoparticles produced in this embodiment have an emission peak in the long wavelength region and show a high quantum yield. In particular, the AgAuSeIn nanoparticles with an In loading amount of 0.88 to 1.5 times show a high quantum yield of 40% or more.
[0094] The peak wavelength of the emission spectrum is classified according to the amount of In added. AgAuSeIn nanoparticles with 0.5 and 0.75 times the amount of In added showed a low intensity emission peak wavelength near 985 nm. When the amount of In added was 0.88 and 1, the emission intensity became very high, and the peak wavelength was observed near 960 to 980 nm. When the amount of In added was 1.25 times or more, the emission peak wavelength shifted to a long wavelength near 1000 nm. This is similar to the classification of the absorption spectrum shape according to the amount of In added.
[0095] Third embodiment In this embodiment, the ratio of the amounts of Ag precursor and Au precursor charged when synthesizing AgAuSeIn nanoparticles was adjusted to synthesize AgAuSeIn nanoparticles of various compositions, and their properties were investigated.
[0096] The synthesis method of AgAuSeIn nanoparticles in this embodiment was basically the same as that in Example 1 (direct synthesis) of the first embodiment. A total of 0.1 mmol of silver acetate and chloro(dimethylsulfide)gold(I), 0.1 mmol of indium acetate, and 0.2 mmol of selenourea were placed in a test tube, and 2.9 mL of a solvent (oleylamine) and 0.1 mL of a protective agent (1-dodecanethiol) were added and heated to synthesize AgAuSeIn nanoparticles.
[0097] In this embodiment, AgAuSeIn nanoparticles were synthesized by setting the ratio (a / (a+b)) of the amount of Ag precursor (silver acetate) and the amount of Au precursor (chloro(dimethylsulfide)gold(I)) to the sum of the number of Ag atoms in the Ag precursor (a) and the number of Au atoms in the Au precursor (b) to be 0, 0.25, 0.5, 0.75, 0.82, 0.88, 0.94, and 1.0. For the reaction systems with these ratios of the amounts of Ag, AgAuSeIn nanoparticles were synthesized at a heating temperature of 50° C. and a reaction time of 20 minutes. In addition to the above, for the reaction systems with the ratios of the amount of Ag charged of 0.25, 0.5, 0.75, and 0.88, AgAuSeIn nanoparticles were also synthesized at a heating temperature of 50° C. and a reaction time of 10 minutes.
[0098] The AgAuSeIn nanoparticles synthesized in this embodiment by adjusting the Ag content ratio were subjected to TEM observation and composition analysis in the same manner as in the first embodiment. Fig. 9a is a TEM photograph of AgAuSeIn nanoparticles synthesized with Ag content ratios of 0, 0.25, 0.5, 0.75, 0.82, 0.88, 0.94, and 1.0 and a heating time of 20 minutes. Fig. 9b is a TEM photograph of AgAuSeIn nanoparticles synthesized with Ag content ratios of 0.25, 0.5, 0.75, and 0.88 and a heating time of 10 minutes. The results of the composition analysis of these semiconductor nanoparticles are shown in Table 5.
[0099] [Table 5]
[0100] It is confirmed from Table 5 that the Ag content of AgAuSeIn nanoparticles changes by adjusting the Ag charge ratio. In other words, the ratio (x / (x+y)) of the number of Ag atoms to the sum of the number of Ag atoms (x) and the number of Au atoms (y) in the AgAuSeIn compound constituting the AgAuSeIn nanoparticles increases with an increase in the Ag charge ratio.
[0101] Then, the absorption spectrum, emission spectrum, and emission quantum efficiency were measured for each AgAuSeIn nanoparticle. The measurement method and conditions were basically the same as those of the first embodiment, but for the measurement of the emission spectrum, the sample with an Ag loading ratio of 0.25 has an absorption edge at about 700 nm and cannot be excited with excitation light of 700 nm wavelength, so only this sample was measured with an excitation wavelength of 365 nm. The measurement results of the absorption spectrum of the semiconductor nanoparticles produced in this embodiment are shown in Figures 10a and 10b, and the measurement results of the emission spectrum are shown in Figures 11a and 11b. Table 6 summarizes the measured values of the peak wavelength of the emission spectrum and the emission quantum efficiency.
[0102] [Table 6]
[0103] Referring to the absorption spectrum curves in Figures 10a and 10b, the absorption edge wavelength tends to become longer as the Ag content ratio increases. However, referring to Figure 10b, for AgAuSeIn nanoparticles with a reaction time of 10 minutes, the AgAuSeIn nanoparticles with an Ag content ratio of 0.75 have the longest absorption edge wavelength, but when the Ag content ratio is 0.88, the absorption edge wavelength becomes slightly shorter. In contrast, referring to Figure 10a, by setting the reaction time to 20 minutes, the absorption edge wavelength of the AgAuSeIn nanoparticles with an Ag content ratio of 0.88 becomes longer than that of the AgAuSeIn nanoparticles with an Ag content ratio of 0.75.
[0104] Next, referring to the emission spectrum measurement results and measured values in Figures 11a and 11b and Table 6, it can be seen that the emission peak tends to shift to the longer wavelength side with an increase in the Ag loading ratio. The AgAuSeIn nanoparticles with Ag loading ratios of 0.5 and 0.75 had particularly high emission quantum yields and narrow peak widths. No emission was observed for nanoparticles with Ag loading ratios of 0 and 1.0. Regarding the reaction time, the AgAuSeIn nanoparticles synthesized by heating for 20 minutes generally have emission peaks on the longer wavelength side.
[0105] FIG. 12 shows the results of XRD analysis of AgAuSeIn nanoparticles with Ag loading ratios of 0.5 and 0.75 (reaction times of 20 and 10 minutes). The XRD analyzer was a Smart-Lab-3K manufactured by Rigaku Corporation, with characteristic X-rays being CuKα radiation, and analysis conditions being 1° / min. From FIG. 12, a diffraction peak corresponding to Ag3AuSe2 is observed for AgAuSeIn nanoparticles synthesized with any Ag loading ratio and reaction time. However, the AgAuSeIn nanoparticles with an Ag loading ratio of 0.75 have higher crystallinity than those with an Ag loading ratio of 0.5. In addition, the AgAuSeIn nanoparticles with an Ag loading ratio of 0.75 have a sharper peak and higher crystallinity when the reaction time is set to 20 minutes.
[0106] Fourth embodimentIn this embodiment, AgAuSeIn nanoparticles were synthesized at multiple reaction times in order to study the reaction time in more detail. In this embodiment, the reaction system was configured under the same conditions as in Example 1 of the first embodiment (Ag charge ratio: 0.75, In charge amount 1 time), and AgAuSeIn nanoparticles were synthesized at a reaction temperature of 50°C for reaction times of 5 minutes, 10 minutes, 15 minutes, 20 minutes, 40 minutes, and 80 minutes.
[0107] TEM observation and composition analysis were performed on the AgAuSeIn nanoparticles synthesized by adjusting the reaction time in this embodiment. Figure 13 shows TEM images of various AgAuSeIn nanoparticles (reaction times: 5 minutes, 10 minutes, 15 minutes, 20 minutes, 40 minutes, and 80 minutes). Table 7 shows the results of the composition analysis of these semiconductor nanoparticles.
[0108] [Table 7]
[0109] Referring to Table 7, it can be seen that the Ag content tends to decrease and the Se content tends to increase with increasing reaction time. However, these changes are small and not dramatic. It is considered that the increase in reaction time does not have a significant effect on the composition of AgAuSeIn nanoparticles.
[0110] Therefore, the absorption spectrum, emission spectrum, and luminescence quantum efficiency were measured for each AgAuSeIn nanoparticle. The measurement method and conditions were basically the same as those in the first embodiment. The measurement results of the absorption spectrum and the emission spectrum of the semiconductor nanoparticles (reaction time: 5 minutes, 10 minutes, 15 minutes, 20 minutes, 40 minutes, 80 minutes) produced in this embodiment are shown in FIG. 14 and FIG. 15, respectively. In addition, the peak wavelengths of the emission spectra and the luminescence quantum efficiency are summarized in Table 8.
[0111] [Table 8]
[0112] Referring to the absorption spectrum curve in Figure 14, it can be seen that the absorption edge tends to shift to the longer wavelength side as the reaction time increases. Looking at the enlarged image in Figure 14, the absorption spectra for reaction times of 5 and 10 minutes are slightly shifted, but the shapes are similar and two absorption edges can be confirmed. The shape of the absorption spectrum changes significantly when the reaction time exceeds 15 minutes, and thereafter remains almost the same shape.
[0113] 15 and Table 8, the AgAuSeIn nanoparticles synthesized in this embodiment while adjusting the reaction time all show a high luminescence quantum yield of 40% or more. However, looking at the emission peak wavelength, it can be said that they are grouped into two groups: those with a reaction time of 10 minutes or less that have a peak below 1000 nm, and those with a reaction time of 15 minutes or more that have a peak above 1000 nm.
[0114] FIG. 16 shows the results of XRD analysis of AgAuSeIn nanoparticles synthesized with reaction times of 10, 20, and 80 minutes. As described in the results of the study in the third embodiment, by setting the reaction time to 20 minutes, the diffraction peak becomes sharp and the crystallinity is improved. However, the crystallinity due to the increase in reaction time does not change much even if the reaction time is excessively long. This is because the diffraction peak at a reaction time of 80 minutes is almost the same as that at a reaction time of 20 minutes. Considering the grouping based on the measurement results of the emission peak wavelength in Table 8, it is predicted that some structural change occurs in the AgAuSeIn nanoparticles at the stage of reaction times of 10 to 15 minutes. This structural change is not limited to simple crystallization, and it is assumed that the nanoparticles will have a core-shell structure, or other changes including element distribution in the particles, but the details are unclear. [Industrial Applicability]
[0115] As described above, the novel semiconductor nanoparticles made of the AgAuSe multi-element compound according to the present invention can exhibit excellent optical semiconductor properties. In addition, the AgAuSe multi-element compound is a low-toxicity compound having biocompatibility. For these reasons, the semiconductor nanoparticles according to the present invention are expected to be applied to light-emitting elements and fluorescent materials used in display devices and marker materials for detecting biological substances, as well as photoelectric conversion elements and light-receiving elements mounted on solar cells, optical sensors, etc.
[0116] The semiconductor nanoparticles according to the present invention have improved light emission and light absorption properties in the long wavelength region of the near infrared region (NIR) and shortwave infrared region (SWIR). Therefore, the present invention is particularly useful for light receiving elements applied to LIDAR and SWIR image sensors, among the above-mentioned optical elements, in which responsiveness in the near infrared region is important.
Claims
1. A semiconductor nanoparticle made of a compound containing a chalcogen element having Ag, Au, and Se as essential constituent elements, and a metal M, The metal M is at least one of Al, Ga, In, Tl, Zn, Cd, Hg, and Cu; The compound has a total content of chalcogen elements, essentially consisting of Ag, Au, and Se, and a metal M of 95 mass % or more; The content of metal M in the compound is 1 atomic % or more and 50 atomic % or less, a ratio of the number of Ag atoms to the sum of the number of Ag atoms x and the number of Au atoms y in the compound (x / (x+y)) is 0.20 or more and 0.95 or less; The compound has a chalcogen element content of 25 atomic % or more and 60 atomic % or less.
2. 2. The semiconductor nanoparticles according to claim 1, wherein the content of chalcogen elements, of which Se is an essential element, in said compound is 25 atomic % or more and 60 atomic % or less.
3. 3. The semiconductor nanoparticles according to claim 1, wherein the compound is a compound containing chalcogen elements essentially consisting of Ag, Au and Se, doped with a metal M.
4. 3. The semiconductor nanoparticles according to claim 1, having an average particle size of 2 nm or more and 20 nm or less.
5. A semiconductor nanoparticle having a protective agent bonded to the surface of the semiconductor nanoparticle according to claim 1 or claim 2, The protective agent is at least one of an alkylamine having an alkyl chain carbon number of 4 to 20, an alkenylamine having an alkenyl chain carbon number of 4 to 20, an alkylcarboxylic acid having an alkyl chain carbon number of 3 to 20, an alkenylcarboxylic acid having an alkenyl chain carbon number of 3 to 20, an alkanethiol having an alkyl chain carbon number of 4 to 20, a trialkylphosphine having an alkyl chain carbon number of 4 to 20, a trialkylphosphine oxide having an alkyl chain carbon number of 4 to 20, triphenylphosphine, and triphenylphosphine oxide.
6. 3. The semiconductor nanoparticles according to claim 1, wherein the long-wavelength absorption edge wavelength of the absorption spectrum is 800 nm or more.
Citation Information
Patent Citations
Fluorescent quantum dots and preparation method therefor and use thereof
EP4092095A1
Semiconductor nanoparticles and method of manufacture
JP2004243507A
Nanoparticle production method, and nanoparticle produced by the method
JP2004352594A
Method for preparing chalcopyrite-type compounds and other inorganic compounds
JP2008540304A
Tellurium compound nanoparticle and production method thereof
JP2015189636A
Cited By
Semiconductor nanoparticles mainly composed of AgAuTeS compounds
JP7913715B1