Light diffusing barrier film

A light-diffusing barrier film with controlled surface roughness in the light-diffusing layer addresses the challenge of maintaining barrier properties and light diffusion during roll-to-roll processing, ensuring durability and efficiency in large-area production.

JP7580823B2Active Publication Date: 2024-11-12LG CHEM LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023039810
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-17
Filing Date
2023-03-14
Publication Date
2024-11-12
Estimated Expiration
2039-04-17

AI Technical Summary

Technical Problem

Existing barrier films for devices with light sources, such as OLEDs, face challenges in maintaining barrier properties against moisture and oxygen while also providing light diffusion, especially when manufactured using roll-to-roll processes, which can damage the barrier layer due to static electricity and unevenness.

Method used

A light-diffusing barrier film with a base layer, light-diffusing layer, and barrier layer is developed, where the light-diffusing layer has controlled surface roughness (Rt) to reduce static electricity and prevent damage during roll-to-roll processing, eliminating the need for separate adhesives and allowing for larger, thinner films to be produced.

Benefits of technology

The film maintains excellent barrier properties against moisture and oxygen, is resistant to damage during manufacturing, and can be produced efficiently over large areas, simplifying the manufacturing process and reducing thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580823000007
    Figure 0007580823000007
  • Figure 0007580823000008
    Figure 0007580823000008
  • Figure 0007580823000009
    Figure 0007580823000009
Patent Text Reader

Abstract

The present application provides a light-diffusing barrier film. The film is an integrated film including, in order, a barrier layer, a substrate layer, and a light diffusion layer. The film can prevent moisture penetration into devices such as organic light-emitting devices and provide light diffusion functionality to the devices. In particular, the film maintains excellent moisture barrier properties even after undergoing a roll-to-roll process.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Cross-reference to related applications This application claims the benefit of priority based on Korean Patent Application No. 10-2018-0044337 filed on April 17, 2018, and Korean Patent Application No. 10-2019-0044610 filed on April 17, 2019, and all contents disclosed in the documents of the relevant Korean patent applications are incorporated herein by reference.

[0002] The present application relates to a light diffusing barrier film and a manufacturing method thereof. In particular, the present application relates to an integrated film that simultaneously includes a barrier layer and a light diffusing layer, and a manufacturing method thereof using a roll-to-roll process. [Background technology]

[0003] Devices including organic light emitting materials and light sources such as backlight units have a problem of reduced durability when exposed to moisture or oxygen. Therefore, such devices may use a barrier film to protect the device from the external environment. Also, a light diffusion sheet is required to uniformly diffuse light projected from the light source. When both light diffusion function and barrier property are required, it may be considered to use a barrier film and a light diffusion sheet attached to each other using an adhesive.

[0004] The film or sheet may be manufactured using a dry coating or a wet coating. For example, when the barrier properties of the film are imparted mainly by inorganic materials such as metals, the barrier film may be manufactured using a dry coating method such as physical vapor deposition (PVD) or chemical vapor deposition (CVD). When the barrier properties of the film are imparted mainly by organic or organic / inorganic composite materials, the barrier film may be manufactured using a wet coating method.

[0005] Meanwhile, as displays become larger, barrier films for displays are also required to be manufactured in larger areas. When a barrier film is manufactured using a dry coating method such as vapor deposition, it has the advantage of being superior in thin film uniformity compared to wet coating, but it is expensive and difficult to manufacture in large areas. In addition, dry and wet coating can be performed during a roll-to-roll process, but during the roll-to-roll process, considerable pressure is applied during the process of winding or unwinding a transported film onto a roll, which can damage the barrier material, resulting in a deterioration of the barrier properties of the film.

[0006] Therefore, there is a need for a technology to provide a barrier film that does not lose its barrier properties during the manufacturing process, has light diffusibility, and can be mass-produced even in large areas. Summary of the Invention [Problem to be solved by the invention]

[0007] One object of the present application is to provide an integrated film having excellent blocking properties against the external environment (eg, moisture) and at the same time a light diffusing function, that is, a light diffusing barrier film.

[0008] Another object of the present application is to provide a large area light diffusive barrier film.

[0009] It is yet another object of the present application to provide an electronic or electrical device comprising said film.

[0010] It is yet another object of the present application to prevent damage to a barrier film during its manufacture using a roll-to-roll process.

[0011] It is still another object of the present invention to manufacture a light-diffusing barrier film according to a wet coating method without the need for a separate adhesive layer, thereby making the barrier film thinner and simplifying its manufacturing process.

[0012] The above and other objects of the present application may be alleviated by the present application as described in detail below. [Means for solving the problem]

[0013] In one embodiment of the present application, the present application relates to a light-diffusing barrier film, i.e., the present application relates to an integrated film that simultaneously has a barrier property as well as a light-diffusing function.

[0014] The light-diffusing barrier film includes a light-diffusing layer, a substrate layer, and a barrier layer. Specifically, the film may include a light-diffusing layer and a barrier layer on both opposing sides of the substrate layer. That is, the barrier film may include a light-diffusing layer, a substrate layer, and a barrier layer in this order, as shown in FIG. 1.

[0015] Unless otherwise defined, the terms "on" or "on top of" used in this application in connection with interlayer stacking positions may be used to mean not only when one structure is located directly on top of another structure, but also when a third structure is interposed between the structures.

[0016] The inventors of the present application have confirmed that when a barrier film is manufactured using wet coating during a roll-to-roll process, damage to the barrier material may occur. For example, when a barrier layer is formed on a substrate layer, a laminate including the barrier layer may undergo a process of being wound around a roll or roller or being unwound from the roll. In particular, when the wound film is unwound, a considerable amount of static electricity may be generated as the interface of the thin laminate film is separated, and the static electricity may induce damage to the barrier layer. In order to reduce the generation of static electricity, it is necessary that the interface between the barrier layer and the substrate layer is not completely adhered even in the wound state. However, this is not easy considering the tension applied to the film when it is wound around a roll. Meanwhile, in order to reduce the generation of static electricity, it is possible to consider forming irregularities on the surface of any layer so that the interface between the barrier layer and the substrate layer is not completely adhered. However, the irregularities of the barrier layer itself may cause defects in the thin film stability and barrier properties of the barrier layer. In addition, if the irregularities of a layer (e.g., a light diffusion layer) that contacts the barrier layer in the wound state are excessively large, the barrier layer may be damaged by the tension applied when it is wound.

[0017] In consideration of these points, the inventors of the present application have invented a light-diffusing barrier film that does not deteriorate the properties of the barrier layer and is suitable for the roll-to-roll process. The light-diffusing barrier film of the present application provides a light-diffusing layer with a predetermined unevenness to ensure the light-diffusing function, improve the roll-to-roll process, and prevent damage to the barrier layer at the same time.

[0018] In this regard, the light diffusing layer of the present application has a predetermined surface roughness (Rt) on one surface thereof.

[0019] In this specification, "surface roughness (Rt)" refers to the distance between the highest point (H1) and the lowest point (H2) when observed from the normal direction to the surface of the layer whose surface roughness is to be measured, i.e., the height difference (ΔH=H1-H2). As described below, the light diffusion layer may contain a resin matrix component and a particle component, and the highest point (H1) observed when measuring the surface roughness (Rt) may be a point formed by one particle or a cluster of multiple particles, and the lowest point (H2) may be a point formed by the resin or the particle component. Such surface roughness (Rt) may be measured using the equipment described in the examples.

[0020] Specifically, in the light-diffusing barrier film, the surface (S1) opposite to the substrate layer has irregularities with a surface roughness (Rt) of 6 μm or less. The surface (S1) of the light-diffusing layer having the irregularities comes into contact with the barrier layer when wound around a roller. Therefore, the irregularities reduce the degree of adhesion between the light-diffusing layer and the barrier layer, and prevent damage to the barrier layer due to static electricity.

[0021] In one example, the surface roughness (Rt) may be 0.01 μm or more, 0.02 μm or more, 0.03 μm or more, 0.04 μm or more, 0.05 μm or more, 0.06 μm or more, 0.07 μm or more, 0.08 μm or more, 0.09 μm or more, or 0.1 μm or more. Specifically, the surface roughness (Rt) may be 0.2 μm or more, 0.3 μm or more, 0.4 μm or more, 0.5 μm or more, 0.6 μm or more, 0.7 μm or more, 0.8 μm or more, 0.9 μm or more, or 1.0 μm or more, more specifically, 1 μm or more, 1.5 μm or more, 2.0 μm or more, 2.5 μm or more, 3.0 μm or more, 3.5 μm or more, 4.0 μm or more, 4.5 μm or more, or 5.0 μm or more.

[0022] If the surface roughness (Rt) exceeds 6 μm, one surface of the barrier layer in contact with the surface (S1) of the light diffusing layer may be damaged by unevenness.

[0023] Although not particularly limited, the lower limit of the surface roughness (Rt) may be 0.02 μm or more. If the lower limit of the surface roughness is smaller than the lower limit, there is a high possibility that static electricity will be generated when the film wound around the roller is unwound.

[0024] In one embodiment, the number of particles observed on the uneven surface is 0.8 to 3.0 particles / μm 2 For example, the surface area per unit area (μm 2 The number of particles observed per μm is 0.9 particles / μm 2 More than 1.0 pieces / μm 2 More than 1.1 pieces / μm 2 More than 1.2 pieces / μm 2 More than 1.3 pieces / μm 2 More than 1.4 pieces / μm 2 More than 1.5 pieces / μm 2 More than 1.6 pieces / μm 2 More than 1.7 pieces / μm 2 More than 1.8 pieces / μm 2 More than 1.9 pieces / μm 2 More than 2.0 pieces / μm 2 or more, and 2.9 particles / μm 2 Below, 2.8 pieces / μm 2 Below, 2.7 pieces / μm 2 Less than or 2.6 pieces / μm 2 The number of particles may be determined by obtaining an SEM image with a magnification of ×50,000 for a predetermined area (μm horizontal × μm vertical) of the layer and counting the number of particles observed from the surface. In one example, the number of particles may be counted several times, for example, three or five times, and the average value is taken as the number of particles.

[0025] In one example, the light diffusion layer, the substrate layer, and the barrier layer may further include another layer between the adjacent layers.

[0026] In another example, the light diffusion layer, the substrate layer, and the barrier layer may be in direct contact with the adjacent layers. Specifically, a separate adhesive may not be used between the adjacent layers. As a result, a thin film having excellent barrier properties may be provided.

[0027] In one example, the surface roughness (Rt) of the light diffusion layer may be in the range of 0.1 to 6 μm. When the range is satisfied, the possibility of static electricity being generated when the film is unwound is relatively low. Specifically, the light diffusing barrier film includes a light diffusion layer, a substrate layer, and a barrier layer in that order, and the surface (S1) opposite to the substrate layer of the light diffusion layer may have unevenness with a surface roughness (Rt) in the range of 0.1 to 6 μm.

[0028] In one example, when the surface roughness (Rt) of the light diffusion layer is less than 0.1 μm, for example, 0.01 to less than 0.1 μm, the sheet resistance of one surface (S1) of the light diffusion layer having the surface roughness is 10 10 Specifically, the light-diffusing barrier film includes a light-diffusing layer, a substrate layer, and a barrier layer in that order, and the surface (S1) of the light-diffusing layer opposite to the substrate layer has a surface roughness (Rt) of 0.02 μm or more and less than 0.1 μm, and the surface resistance of the surface (S1) of the light-diffusing layer having the surface roughness is 10 10 It may be Ω / sq or less.

[0029] In this regard, if one side (S1) of the light diffusion layer has unevenness, the possibility of static electricity being generated during peeling of the interface between the light diffusion layer and the barrier layer is lower than when there is no unevenness, but if the surface roughness is 0.02 to less than 0.1 μm, the surface resistance of one side (S1) of the light diffusion layer needs to be adjusted to a certain level, thereby preventing damage to the barrier layer due to static electricity that may be generated when the film is unwound, despite the relatively low surface unevenness.

[0030] In one example, the surface resistance of the surface (S1) of the light diffusing layer having a surface roughness (Rt) of less than 0.1 μm is 1.0×10 12Ω / sq or less, 1.0×10 11 Ω / sq or less 1.0×10 10 Ω / sq or less, 1.0×10 9 Ω / sq or less or 1.0×10 8 The surface resistance value is a value that defines a size that can prevent damage to the barrier layer due to static electricity in relation to the unevenness, and the lower limit is not particularly limited. For example, the lower limit may be 1.0×10 7 Ω / sq or more, 1.0×10 8 Ω / sq or more or 1.0×10 9 It may be Ω / sq or more.

[0031] The means for making the surface resistance of the light diffusion layer having a surface roughness (Rt) of less than 0.1 μm fall within the above range is not particularly limited. For example, the material for forming the light diffusion layer can be appropriately selected. In one example, the light diffusion layer having a surface roughness (Rt) of less than 0.1 μm can contain a predetermined amount of antistatic agent.

[0032] In one example, the light-diffusing barrier film may satisfy a change rate of moisture permeability of 30% or less, calculated by the following formula:

[0033] [Formula] Change in moisture permeability (%) = {(BA) / A} x 100

[0034] In the above formula, A is the moisture permeability of the light-diffusing barrier film (F1); B is the moisture permeability of the light-diffusing barrier film (F1) measured after applying a constant load to the surface of the barrier layer of the light-diffusing barrier film (F1) so that the uneven surfaces of the light-diffusing layer of the light-diffusing barrier film (F2) are in contact with each other (or are in contact with each other) and the two films (F1, F2) are stacked together, and the constant load is maintained for 24 hours; the light-diffusing barrier films (F1, F2) may have the same structure, and the moisture permeabilities (A, B) may be measured using AQUATRAN2 (MOCON) under conditions of 38°C and 100% relative humidity.

[0035] The light-diffusing barrier films (F1, F2) used in calculating the rate of change in moisture permeability are light-diffusing barrier films according to the present application, which include a light-diffusing layer, a substrate layer and a barrier layer in that order, and have the properties of each layer defined in the present application.

[0036] In one example, the constant load applied when calculating the rate of change in moisture permeability may be applied before the polysilazane layer of the film (F2) is cured. The polysilazane layer of the film (F2) may be cured after the constant load is applied. In one example, the moisture permeabilities A and B may be the moisture permeabilities of the films (F1, F2) measured before the polysilazane layer is cured. Or, the moisture permeabilities A and B may be the moisture permeabilities of the films (F1, F2) measured after the polysilazane layer is cured.

[0037] In one example, the rate of change may be 25% or less, 20% or less, 15% or less, 10% or less, or 5% or less.

[0038] For the above reasons, damage to the barrier layer may occur during the roll-to-roll process, and the barrier properties of the damaged film may be reduced. That is, the moisture permeability may be increased. Therefore, in relation to the above formula, a moisture permeability change rate (%) of 30% or less may mean that a moisture permeability increase rate (%) is 30% or less. That is, in this application, the moisture permeability change rate (%) may be used in the same sense as the moisture permeability increase rate (%). However, it is expressed as a change rate taking into account mechanical errors associated with the measurement of the moisture permeability change rate.

[0039] The moisture permeability change rate is a numerical change assuming that the film or a part thereof is unwound from and wound around a roller during the manufacturing process of the light diffusive barrier film using a roll-to-roll process. Specifically, the moisture permeability B is a value for confirming how much the moisture permeability of the barrier film has changed (decreased) when the film or a part thereof is wound around a roll (or roller) while tension is applied, and the wound state is maintained for a predetermined time, and then the film is unwound from the roll (or roller). As can be confirmed through the following experimental examples, the degree of decrease in moisture permeability (i.e., the degree of damage to the barrier film) can vary depending on, for example, the degree of unevenness or surface resistance of the light diffusive layer.

[0040] Although not particularly limited, the constant load or predetermined pressure applied to overlap the two films (F1, F2) when measuring the moisture permeability B may be a load of about 10 to 35 kg. Furthermore, when measuring the moisture permeability B, the two films (F1, F2) may be cut into sheets, and at this time, the size of the surface where the sheets contact each other may be 10 cm x 10 cm.

[0041] The type of the substrate layer is not particularly limited. For example, the substrate layer may include a glass substrate or a plastic (polymer) material.

[0042] In one example, the substrate layer may include, but is not limited to, a polyester film such as a polyethylene terephthalate (PET) film, a polycarbonate film, a polyethylene naphthalate film, or a polyarylate film, a polyether film such as a polyethersulfone film, a polyolefin film such as a cycloolefin polymer film, a polyethylene film, or a polypropylene film, a cellulose resin film such as a diacetyl cellulose film, a triacetyl cellulose film, or an acetyl cellulose butyrate film, a polyimide film, an acrylic film, or an epoxy resin film.

[0043] The substrate layer may include one or more of the films listed above, that is, the substrate layer may have a single layer or a multi-layer structure.

[0044] The thickness of the substrate layer is not particularly limited and may be selected, for example, from within the range of 2 to 200 μm, 5 to 190 μm, 10 to 180 μm, 20 to 180 μm, or 20 to 150 μm.

[0045] The thickness of the substrate layer may be measured by observing a cross-sectional image using, for example, a SEM (HR-SEM, S-4800, Hitachi) or a TEM (FE-TSEM, TITAN G2 ChemiSTEM 80-200, FEI). Alternatively, the thickness may be measured by analyzing the electron density difference between adjacent layers using an XRR (X'Petr Pro MRD XRD, PANalytical) to infer thickness oscillation. In this case, the thickness may be an average value of thickness values ​​measured at multiple points on the surface of the substrate layer whose thickness is to be measured, when observed from a normal direction to the surface.

[0046] In one example, the base layer may be transparent or translucent. In the present application, "transparent or translucent" may mean that a certain layer or film has a visible light transmittance in the wavelength range of 380 to 780 nm, specifically, a transmittance of 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, or 95% or more for light with a wavelength of 550 nm. The upper limit of the transmittance may be, for example, about 100%.

[0047] The substrate layer may contain one or more known additives selected from the group consisting of antistatic agents, light blocking agents, ultraviolet absorbing agents, plasticizers, lubricants, fillers, colorants, stabilizers, lubricants, crosslinking agents, and antioxidants.

[0048] As one example, one or both surfaces of the base layer may be subjected to a surface treatment such as primer treatment, corona discharge irradiation, plasma irradiation, ion irradiation, etc. For example, the base layer may be a layer having at least one surface subjected to a primer treatment in order to improve the adhesive strength or bonding strength with a light diffusion layer or a barrier layer.

[0049] In one embodiment, the barrier layer may include one or more sub-barrier layers. When two or more sub-barrier layers are laminated to form a barrier layer, the types of the sub-barrier layers may be the same or different. For example, as shown in FIG. 2, the light-diffusing barrier film may include a light-diffusing layer, a substrate layer, a second barrier layer, and a first barrier layer in this order.

[0050] In one example, the barrier layer or sub-barrier layer may be a polysilazane layer or a cured layer of polysilazane.

[0051] In the present application, the polysilazane layer may be in a pre-cured state, for example, a layer formed by coating one surface of a substrate layer with a polysilazane-containing composition (coating composition) described below and drying it. Also, the cured layer of polysilazane may refer to a layer formed by curing the polysilazane layer.

[0052] The polysilazane layer means a layer containing polysilazane as a main component (a coating layer in a pre-cured state formed on a substrate layer). The main component may mean, for example, that the proportion of polysilazane in the polysilazane layer or the polysilazane-containing composition is 55% or more, 60% or more, 65% or more, 70% or more, 75% or more, 80% or more, 85% or more, or 90% or more by weight. The weight proportion may be, for example, 100% or less, 99% or less, 98% or less, 97% or less, 96% or less, or 95% or less.

[0053] In this application, the term "polysilazane" refers to a polymer in which silicon atoms (Si) and nitrogen atoms (N) are repeated to form a basic backbone. Such polysilazanes can be modified through a certain treatment (e.g., plasma treatment described below) to form silicon oxide and / or silicon oxynitride having barrier properties. As a result, the cured product of the polysilazane layer, i.e., the cured layer, contains Si, N, and / or O and has barrier properties against the external environment.

[0054] In one example, the polysilazane used in the present application may include a unit represented by the following Formula 1:

[0055] [ka]

[0056] In formula 1, R 1 , R 2 and R 3 may each independently be a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, an aryl group, an alkylsilyl group, an alkylamide group, or an alkoxy group.

[0057] In the present application, the term "alkyl group" may mean an alkyl group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms, unless otherwise specified. The alkyl group may be linear, branched, or cyclic. The alkyl group may be optionally substituted with one or more substituents.

[0058] In this specification, unless otherwise specified, the term "alkenyl group" can mean an alkenyl group having 2 to 20 carbon atoms, 2 to 16 carbon atoms, 2 to 12 carbon atoms, 2 to 8 carbon atoms, or 2 to 4 carbon atoms. The alkenyl group may be linear, branched, or cyclic, and may be optionally substituted with one or more substituents.

[0059] In this specification, unless otherwise specified, the term "alkynyl group" can mean an alkynyl group having 2 to 20 carbon atoms, 2 to 16 carbon atoms, 2 to 12 carbon atoms, 2 to 8 carbon atoms, or 2 to 4 carbon atoms. The alkynyl group may be linear, branched, or cyclic, and may be optionally substituted with one or more substituents.

[0060] The term "aryl group" as used herein, unless otherwise specified, may refer to a monovalent residue derived from a compound or derivative thereof that includes a structure in which a benzene ring or two or more benzene rings are linked or condensed or bonded while sharing one or more carbon atoms. The scope of the aryl group as used herein may include not only functional groups that are generally called aryl groups, but also so-called aralkyl groups or arylalkyl groups. The aryl group may be, for example, an aryl group having 6 to 25 carbon atoms, 6 to 21 carbon atoms, 6 to 18 carbon atoms, or 6 to 12 carbon atoms. Examples of the aryl group include a phenyl group, a dichlorophenyl group, a chlorophenyl group, a phenylethyl group, a phenylpropyl group, a benzyl group, a tolyl group, a xylyl group, and a naphthyl group.

[0061] In the present application, unless otherwise specified, the term "alkoxy group" may mean an alkoxy group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. The alkoxy group may be linear, branched, or cyclic. In addition, the alkoxy group may be optionally substituted with one or more substituents.

[0062] As long as the polysilazane contains the unit represented by Chemical Formula 1, the specific type of polysilazane is not particularly limited.

[0063] In one example, taking into consideration the density of the modified polysilazane layer, the polysilazane of the present application is R 1 ~R 3 A polysilazane containing units of Formula 1 in which are all hydrogen atoms, such as perhydropolysilazane, can be used.

[0064] Although not particularly limited, the number average molecular weight (Mn) of the polysilazane compound may be, for example, 100 to 50,000.

[0065] In one example, the polysilazane layer may be formed by coating a composition (coating liquid containing polysilazane as a main component) prepared by dissolving polysilazane in a suitable organic solvent on a substrate layer. The type of solvent contained in the coating liquid is not particularly limited as long as it is a solvent that is not reactive with polysilazane and can dissolve it. For example, hydrocarbon solvents such as aliphatic hydrocarbons, alicyclic hydrocarbons, and aromatic hydrocarbons, halogenated hydrocarbon solvents, and ethers such as aliphatic ethers and alicyclic ethers may be used. Specifically, hydrocarbons such as pentane, hexane, cyclohexane, toluene, xylene, solvesso, and terben, halogenated hydrocarbons such as methylene chloride and trichloroethane, and ethers such as dibutyl ether, dioxane, and tetrahydrofuran may be used as the solvent.

[0066] In one example, a commercialized polysilazane or a composition containing the same may be used to form a barrier layer. For example, commercially available polysilazanes such as AQUAMICA (registered trademark) NN120-10, NN120-20, NAX120-10, NAX120-20, NN110, NN310, NN320, NL110A, NL120A, NL150A, NP110, NP140, or SP140 manufactured by AZ Electronic Materials Co., Ltd. may be used, but are not limited thereto.

[0067] The polysilazane layer may include a polysilazane modification-promoting catalyst, i.e., a compound that promotes the modification of the polysilazane compound by interacting with the polysilazane compound, such as, but not limited to, an organic amine compound, an organic acid, an inorganic acid, a metal carboxylate, an organometallic complex salt, and the like.

[0068] The composition for forming the barrier layer may contain other additives as necessary, such as, but not limited to, a viscosity modifier and a crosslinking promoter.

[0069] If the thickness of the polysilazane layer coated on the substrate layer, i.e., the sub-barrier layer, is too thin, the coating process is not performed smoothly, the barrier properties are not sufficiently secured, and the light diffusion layer is likely to be damaged by the unevenness. If the thickness is too thick, cracks (damage) may occur due to shrinkage of the polysilazane layer during the curing process. Although not particularly limited, the thickness of the coated polysilazane layer may have a lower limit of, for example, about 20 nm or more, 30 nm or more, 40 nm or more, 50 nm or more, 60 nm or more, 70 nm or more, 80 nm or more, 90 nm or more, or 100 nm or more, taking into consideration the above points. And the upper limit may be, for example, 400 nm or less, 350 nm or less, 300 nm or less, 250 nm or less, or 200 nm or less. In this case, the thickness of the barrier layer may mean the average thickness of the resin component (e.g., polysilazane) that forms the barrier layer coated or the thickness of the cured resin component.

[0070] The thickness of the barrier layer may be measured by a known method, for example, by observing a cross-sectional image using a SEM (HR-SEM, S-4800, Hitachi) or a TEM (FE-TSEM, TITAN G2 ChemiSTEM 80-200, FEI). Alternatively, the thickness may be measured by analyzing the electron density difference between adjacent layers using an XRR (X'Petr Pro MRD XRD, PANalytical) to infer thickness oscillation. In this case, the thickness may be an average value of thickness values ​​measured at multiple points on the surface formed by the resin component when observed from a normal direction to the surface of the layer whose thickness is to be measured.

[0071] In one example, the polysilazane layer may be applied onto one surface of a substrate layer, and then dried, so that the polysilazane layer may be present on the substrate layer in a pre-cured state.

[0072] In one example, the polysilazane layer can be cured on a substrate layer.

[0073] In one example, the thickness of the layer obtained by curing the polysilazane layer, i.e., the cured layer of polysilazane, can be determined by the thickness of the polysilazane layer described above. The thickness of the barrier layer including two or more sub-barrier layers can be appropriately adjusted by the number of the cured polysilazane layer or the polysilazane layer within a range of 1,500 nm or less.

[0074] In one example, the barrier layer may be a laminate of a first sub-barrier layer and a second sub-barrier layer. In this case, the thickness of each of the sub-barrier layers may be, for example, 40 nm or more, 50 nm or more, 60 nm or more, 70 nm or more, 80 nm or more, 90 nm or more, or 100 nm or more. The upper limit of the thickness of each of the sub-barrier layers may be, for example, 250 nm or less, 240 nm or less, 230 nm or less, 220 nm or less, 210 nm or less, or 200 nm or less.

[0075] When multiple sub-barrier layers are stacked, for example when a second sub-barrier layer is formed on a first sub-barrier layer, each sub-barrier layer can be distinguished by observing a cross section of the barrier layer with an SEM or TEM.

[0076] In one embodiment, the barrier layer may include only the polysilazane layer or the cured layer thereof, and may not include the metal component-containing layer formed by vapor deposition, for example.

[0077] In one embodiment, the barrier layer may include a particle component, which may be the same as that described for the light diffusion layer.

[0078] In one example, the barrier layer may be free of particulate components.

[0079] In one example, the barrier layer may be transparent or light-transmitting.

[0080] In one example, the barrier layer may be formed directly on one side of the substrate layer, i.e., there is no separate adhesive layer between them, thereby providing a thin film with excellent barrier properties.

[0081] In one example, the light diffusion layer having the surface roughness may include a matrix component forming a continuous phase in the light diffusion layer and a light diffusion agent as a dispersed phase present in the continuous phase. In this case, the matrix component may be a curable resin (or a cured product thereof), and the light diffusion agent may be (light diffusion) particles known to have a light diffusion function. The particles form surface irregularities to perform a unique light diffusion function.

[0082] In one example, the light diffusion layer having the surface roughness (Rt) may have a thickness of 20 μm or less. Specifically, the upper limit of the thickness of the light diffusion layer may be 19 μm or less, 18 μm or less, 17 μm or less, 16 μm or less, 15 μm or less, 14 μm or less, 13 μm or less, 12 μm or less, 11 μm or less, 10 μm or less, 9 μm or less, 8 μm or less, 7 μm or less, 6 μm or less, 5 μm or less, 4 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. In addition, the lower limit of the thickness may be, for example, 0.5 μm or more, 1 μm or more, 2 μm or more, 3 μm or more, 4 μm or more, 5 μm or more, 6 μm or more, 7 μm or more, 8 μm or more, 9 μm or more, or 10 μm or more. When the above range is satisfied, the light diffusion layer may be formed stably while having the above-mentioned surface roughness (Rt).

[0083] The thickness of the light diffusion layer is measured by observing a cross-sectional image using a known method, for example, a SEM (HR-SEM, S-4800, Hitachi) or a TEM (FE-TSEM, TITAN G2 ChemiSTEM 80-200, FEI), without considering the light diffusion particles, and only considering the matrix component, i.e., the resin component. Alternatively, the thickness can be measured by analyzing the electron density difference between adjacent layers using an XRR (X'Petr Pro MRD XRD, PANalytical) to infer thickness oscillation. In this case, the thickness may be an average value of thickness values ​​measured at many points on the surface formed by the resin component when observed from the normal direction to the surface of the layer whose thickness is to be measured.

[0084] In one example, the light diffusion layer may be formed of a coating composition containing 0.1 parts by weight or more of particles relative to 100 parts by weight of a curable resin (hereinafter referred to as "light diffusion layer coating composition"). Specifically, the lower limit of the content of the particles may be, for example, 0.2 parts by weight or more, 0.3 parts by weight or more, 0.4 parts by weight or more, or 0.5 parts by weight or more, specifically, 1 part by weight or more, 2 parts by weight or more, 3 parts by weight or more, 4 parts by weight or more, or 5 parts by weight or more, specifically, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 25 parts by weight or more, 30 parts by weight or more, 35 parts by weight or more, 40 parts by weight or more, 45 parts by weight or more, or 50 parts by weight or more. In addition, the upper limit of the content of the particles may be, for example, 100 parts by weight or less, 95 parts by weight or less, 90 parts by weight or less, 85 parts by weight or less, or 80 parts by weight or less.

[0085] In one example, in order to form a surface having irregularities, i.e., a surface of the light diffusion layer having a surface roughness (Rt) within a predetermined range, low density particles can be used when preparing the coating composition for the light diffusion layer. Specifically, when mixing a resin, a solvent, and particles to prepare the coating composition for the light diffusion layer, relatively low density particles can be used so that the particles can be protruded by buoyancy onto the surface of the coating composition for the light diffusion layer applied on the substrate layer.

[0086] In another example, a method of adjusting the particle diameter in consideration of the thickness of the light diffusion layer to be formed can be used. Specifically, particles having a diameter larger than the thickness (height) of the light diffusion layer formed after curing can be used in the coating composition for the light diffusion layer. When the above particle size is satisfied, the uneven structure can be formed more easily. For example, when the height of the light diffusion layer is about 20 μm, particles having a diameter of about 20 to 25 μm can be used. However, when the particle diameter is larger than the thickness of the layer, the interface between the particle and the light diffusion layer can act as a defect, so that the content of the particles should be appropriately adjusted so that the particles are not used in excess.

[0087] In another example, another method for forming surface roughness is to use components having different hydrophobic or hydrophilic properties when preparing the coating composition for the light diffusion layer. Specifically, when using particles having a diameter smaller than the thickness of the light diffusion layer, particles having a relatively higher hydrophobicity or a relatively higher hydrophilicity compared to the solvent or resin component used in the coating composition for the light diffusion layer can be used. As described above, when the hydrophobicity or hydrophilicity is different, the particles can exist in a floating state on the surface of the light diffusion layer (or the coating composition layer of the light diffusion layer applied on the substrate layer) formed after the resin is cured (or the curing can be performed while maintaining the above state). The hydrophobicity or hydrophilicity of the particles can be determined by the properties (e.g., components) of the particles themselves. Alternatively, the particles can be imparted with hydrophobicity or hydrophilicity through surface treatment with hydrophobic or hydrophilic functional groups. In this case, whether or not a particle is hydrophobic or hydrophilic is not uniformly determined, but may be determined in relation to other components (e.g., solvent or resin) in the composition used together, and may be relatively determined by comprehensively considering the polarity of the compound or functional group forming the surface of the particle, the length of the carbon chain in the compound, etc. For example, when the thickness of the light diffusion layer is on the order of 15 to 17 μm, the particle diameter can be adjusted to within the range of about 1 to 5 μm, and the surface properties of the particle can be adjusted so that the particle exists in a suspended state on the surface (S1) of the light diffusion layer.

[0088] The resin component used to form the light diffusing layer is not particularly limited, and may be a thermosetting resin or a photocurable resin.

[0089] In one example, the coating composition of the light diffusing layer may include an acrylic resin, a urethane resin, a melamine resin, an alkyd resin, an epoxy resin, a siloxane polymer, or a condensate of an organic silane compound described below.

[0090] Although there is no particular limitation, when weather resistance, scratch resistance, surface gloss characteristics, and heat resistance are taken into consideration, acrylic resins may be used.

[0091] Specifically, the acrylic resin can be obtained by copolymerizing a monomer mainly composed of acrylic acid and a methacrylic acid derivative. Examples of the monomer that can be used include, but are not limited to, (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, sec-butyl (meth)acrylate, pentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-ethylbutyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate, and tetradecyl (meth)acrylate.

[0092] In one embodiment, the light diffusion layer composition may include a polyfunctional (meth)acrylate as a resin component. Examples of the polyfunctional acrylate include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid, and the like. acid) neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentanyl di(meth)acrylate, ethylene oxide-modified di(meth)acrylate, di(meth)acryloxyethyl isocyanurate, allyl cyclohexyl di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, dimethylol dicyclopentane di(meth)acrylate, ethylene oxide-modified hexahydrophthalic acid di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, neopentyl glycol-modified trimethylpropane di(meth)acrylate, adamantane di(meth)acrylate or 9,9-bis[4- Bifunctional acrylates such as (2-acryloyloxyethoxy)phenyl]fluorine; trifunctional acrylates such as trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, propionic acid modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, trifunctional urethane (meth)acrylate or tris(meth)acryloxyethyl isocyanurate; tetrafunctional acrylates such as diglycerol tetra(meth)acrylate or pentaerythritol tetra(meth)acrylate; pentafunctional acrylates such as propionic acid modified dipentaerythritol penta(meth)acrylate;and hexafunctional acrylates such as dipentaerythritol hexa(meth)acrylate, caprolactone-modified dipentaerythritol hexa(meth)acrylate, or a reaction product of urethane(meth)acrylate (e.g., isocyanate monomer) and trimethylolpropane tri(meth)acrylate, but are not limited thereto;

[0093] As the epoxy resin that can be used to form the light diffusing layer, one or more types selected from the group consisting of alicyclic epoxy resins and aromatic epoxy resins can be used.

[0094] As the alicyclic epoxy resin, for example, one or more selected from the group consisting of alicyclic glycidyl ether type epoxy resins and alicyclic glycidyl ester type epoxy resins can be used. In addition, for example, 3,4-epoxycyclohexyl-methyl-3,4-epoxycyclohexane carboxylate (Celloxide 2021P (Daicel)) and its derivatives can be used, which are stable even at high temperatures, colorless and transparent, and have excellent toughness, adhesion, and adhesive strength for interleaf paper.

[0095] As the aromatic epoxy resin, for example, one or more aromatic epoxy resins selected from the group consisting of bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AD ​​type epoxy resins, fluorene-containing epoxy resins, and triglycidyl isocyanurate may be used.

[0096] The type of polymerization initiator that causes the resin to form the matrix of the light diffusion layer by polymerization is not particularly limited, and a publicly known photopolymerization initiator or thermal polymerization initiator may be used.

[0097] In addition, the coating composition for the light diffusion layer may further include a hardener, the type of which is not particularly limited.

[0098] The type of particles used to form the light diffusion layer is not particularly limited. As the particle component, organic particles, inorganic particles, organic-inorganic hybrid particles, or a mixture thereof may be used without limitation. The shape of the particles is also not particularly limited. For example, the particles may be spherical, elliptical, pyramidal, or amorphous.

[0099] In one example, when spherical particles are used in forming a light diffusing layer, the surface of the light diffusing layer having a predetermined surface roughness may have a shape in which hemispherical protrusions are irregularly protruded or an irregular embossing shape.

[0100] The type of inorganic particles that can be used in the light diffusion layer is not particularly limited. In one example, inorganic particles selected from clay, talc, alumina, calcium carbonate, zirconia, silica, barium sulfate, titanium dioxide, aluminum hydroxide, glass, talc, mica, white carbon, magnesium oxide, zinc oxide, indium oxide, and tin oxide particles can be used. Compared with the organic particle component described below, the inorganic particle component has better barrier properties against moisture, etc., so using inorganic particles is advantageous in improving the barrier properties of the film against the external environment.

[0101] The type of organic particles that can be used in the light diffusion layer is not particularly limited. The organic particles contain a polymer component, and examples of the organic particles include, but are not limited to, acrylic particles, siloxane particles, polycarbonate particles, and styrene particles.

[0102] In one example, the particles used in the light diffusion layer may be amphiphilic particles. The amphiphilic particles may be determined depending on the relative hydrophilicity and hydrophobicity of the solvent and resin used together. The amphiphilicity may be realized through a surface treatment, etc.

[0103] In one example, the size of the particles included in the light diffusion layer may be 50 nm or more or 100 nm or more. Specifically, the size of the particles may be 150 nm or more, 200 nm or more, 250 nm or more, 300 nm or more, 350 nm or more, 400 nm or more, 450 nm or more, or 500 nm or more. In addition, when considering the thickness and surface roughness of the light diffusion layer, for example, the upper limit of the size of the particles may be, for example, 25 μm or less, 20 μm or less, 15 μm or less, 10 μm or less, 5 μm or less, or 1 μm or less. In this regard, the "size of the particle" may be used in the same sense as the "particle size" and means the length of the largest dimension of the shape of the particle. The particle size may be analyzed using a known particle size analyzer, for example, a DLS (dynamic light scattering) device.

[0104] When the particle size is large compared to the thickness of the light diffusion layer, the unevenness of the light diffusion layer may be formed by the particle size of the particles, or when the particle size is small compared to the thickness of the light diffusion layer, the unevenness of the light diffusion layer may be formed by particles or agglomerates of particles suspended on the surface of the light diffusion layer.

[0105] In one embodiment, the particle size may include particles having two or more particle sizes. In this case, the particle size may refer to an average value, for example, an average particle size (D50). D50 refers to a particle size that corresponds to 50% of the weight percentage in a particle size distribution curve.

[0106] The coating composition of the light diffusion layer may include a solvent, such as, but not limited to, toluene, xylene, propylene glycol monoethyl ether, cyclopentanone, dimethylformamide (DMF), dimethyl sulfoxide (DMSO), dibutyl ether, anisole, or 1,2,4-trichlorobenzene.

[0107] The coating composition of the light diffusion layer may further include additives such as antistatic agents, antibacterial agents, heat stabilizers, antioxidants, release agents, light stabilizers, surfactants, coupling agents, plasticizers, compatibilizers, colorants, stabilizers, lubricants, coloring agents, flame retardants, weather resistance agents, UV absorbers, UV blocking agents, or combinations thereof. The content of these additives is not particularly limited, but may be in the range of 0.01 to 10 parts by weight based on 100 parts by weight of the resin component.

[0108] In one example, the light diffusion layer may be formed directly on one side of the substrate layer, i.e., there is no separate adhesive layer between the substrate layer and the light diffusion layer, thereby providing a thin film with excellent barrier properties.

[0109] In one example, the light diffusing layer may be transparent or translucent.

[0110] In one embodiment, the light-diffusing barrier film may further include a hard coating layer. The hard coating layer is a layer that provides hardness or strength to the film. Specifically, as shown in FIG. 3, the light-diffusing barrier film may include a light-diffusing layer, a substrate layer, a hard coating layer, and a barrier layer in that order.

[0111] In one embodiment, the hard coating layer may be in direct contact with the substrate layer and the barrier layer, respectively, which may improve the scratch resistance and solvent resistance of the substrate layer.

[0112] The specific composition of the hard coating layer-forming composition is not particularly limited.

[0113] In one example, the composition for forming the hard coating layer may include a curable resin. In this case, the composition for forming the hard coating layer may further include a polymerization initiator, etc. The type of the polymerization initiator is not particularly limited, and a known thermal polymerization initiator or photopolymerization initiator may be used.

[0114] In one example, the curable resin included in the composition of the hard coating layer may be a photocurable resin, such as, but not limited to, a urethane acrylate oligomer, a polyester acrylate, or the like.

[0115] As one example, (meth)acrylates having a hydroxyl group in addition to the resin component, such as pentaerythritol acrylate and dipentaerythritol hexaacrylate, may be used to form the hard coating layer.

[0116] In one embodiment, the composition for forming the hard coating layer may further include particles. The specific type of particles is not particularly limited, but for example, one or more organic or inorganic particles that can be used in a light diffusion layer may be used.

[0117] In one embodiment, the composition for forming the hard coating layer may further include a solvent. Any known solvent may be used without limitation, for example, the solvents described above.

[0118] In addition, the composition for forming the hard coating layer may further include a curing agent, the type of which is not particularly limited.

[0119] In one example, the hard coating layer may have the same composition as that described above for the light diffusion layer. For example, the composition of the hard coating layer may include the same resin component as the composition of the light diffusion layer. In this case, the composition for forming the hard coating layer may not include particles.

[0120] In one example, the hard coating layer may be transparent or translucent.

[0121] In one example, the light diffusion barrier film of the above configuration has a thickness of 5.0×10 -3 g / m 2 For example, the moisture permeability may be 4.5×10-3 g / m 2 day or less, 4.0×10 -3 g / m 2 day or less, 3.5×10 -3 g / m 2 day or less, 3.0×10 -3 g / m 2 day or less, 2.5×10 -3 g / m 2 day or less, 2.0×10 -3 g / m 2 day or less, 1.5×10 -3 g / m 2 days or less or 1.0×10 -3 g / m 2 The lower limit of the moisture permeability may be, for example, 0.001×10 -3 g / m 2 day or more, 0.01×10 -3 g / m 2 day or more or 0.1×10 -3 g / m 2 It may be more than one day.

[0122] In one example, the light diffusion barrier film having the above-mentioned configuration may have light transmissivity or transparency.

[0123] In one example, the haze of the light diffusion barrier film having the above configuration may be 60% or more, 80% or more, 85% or more, or 88% or more. The haze may be a percentage of the transmittance of diffused light relative to the transmittance of the total transmitted light passing through the measurement target.

[0124] The light-diffusing barrier film of the present application can be used as a barrier film or a sealing film in various applications, such as various packaging materials, displays such as LCDs (Liquid Crystal Displays), solar cell members, and substrates for electronic paper and OLEDs (Organic Light Emitting Diodes).

[0125] In another embodiment, the present application relates to an electric or electronic device, which may be, for example, an optical device, such as various display devices or lighting devices.

[0126] When used in the above applications, the light diffusing barrier film can be positioned such that the barrier layer is adjacent to the object to be protected, i.e., the structure vulnerable to moisture. For example, when the barrier film is attached to an OLED device, the stacking order can be a light diffusing layer, a substrate layer, a barrier layer, and an OLED device.

[0127] In yet another embodiment of the present application, the present application relates to a method for producing a light diffusive barrier film.

[0128] The barrier film may be manufactured using a roll-to-roll process, where the film or laminate is repeatedly wound and / or unwound from a roll (or roller) of a roll-to-roll machine.

[0129] The method can be carried out by forming a laminate of a substrate layer and a light diffusion layer first, and then forming a barrier layer, because the substrate layer does not have the unevenness and / or surface resistance of the light diffusion layer, and the barrier layer is damaged during the roll-to-roll process.

[0130] The properties of the light diffusion layer, the substrate layer and the barrier layer, and the materials constituting these layers are as described above.

[0131] In one embodiment, the method includes a first step of preparing a laminate including a substrate layer and a light diffusion layer, the surface roughness (Rt) of the surface (S1) of the substrate layer opposite to the surface of the light diffusion layer being within a range of 0.1 to 6 μm; and a second step of applying a coating composition for a barrier layer onto the surface of the substrate layer opposite to the surface of the light diffusion layer and drying the coating composition to form a barrier layer. In this case, the barrier layer may be a polysilazane layer.

[0132] In one embodiment, the method includes a substrate layer and a light diffusing layer, the surface roughness (Rt) of a surface (S1) of the light diffusing layer facing the substrate layer is 0.02 to 0.1 μm, and the surface resistance of the surface (S1) of the light diffusing layer having the surface roughness is 10 10 and a second step of forming a barrier layer by applying a coating composition for a barrier layer on the surface opposite to the surface of the substrate layer on which the light diffusion layer is formed, and then drying the coating composition. In this case, the barrier layer may be a polysilazane layer.

[0133] In one example, the light diffusion layer may be formed on one surface of the substrate layer by wet coating, i.e., by applying the coating composition of the light diffusion layer described above on one surface of the substrate layer and then drying and / or curing the coating composition.

[0134] The method of applying the coating composition for the light diffusion layer is not particularly limited, and may be, for example, a gravure coating method, a kiss coating method, a die coating method, a lip coating method, a comma coating method, a blade coating method, a roll-to-roll coating method, a knife coating method, a spray coating method, a bar coating method, a spin coating method, or a dip coating method, but is not limited thereto.

[0135] The drying method for the coating composition of the light diffusion layer is not particularly limited, and may be, for example, hot air drying, infrared drying, microwave drying, or the like.

[0136] The temperature during the drying may be adjusted in consideration of the boiling point of the liquid (e.g., solvent) component contained in the composition and the durability of the base layer, etc. In one example, the temperature at which the drying is performed may be 50° C. or higher, 60° C. or higher, or 70° C. or higher, more specifically, 80° C. or higher, 85° C. or higher, 90° C. or higher, 95° C. or higher, or 100° C. or higher. The upper limit may be, for example, 150° C. or lower, 140° C. or lower, 130° C. or lower, 120° C. or lower, 110° C. or lower, or 100° C. or lower.

[0137] The drying time is not particularly limited and may be within a range of several seconds to several tens of minutes, or within a range of several minutes. Although not particularly limited, drying may be performed for, for example, 1 minute or more to 10 minutes or less, 5 minutes or less, or 3 minutes or less.

[0138] The method of curing the coating composition of the light diffusion layer is not particularly limited. For example, ultraviolet (UV) irradiation can be used. The wavelength and energy of the UV light can be appropriately selected by those skilled in the art in consideration of the materials to be used, and are not particularly limited.

[0139] When a laminate having a light diffusion layer formed on one side of a substrate layer is prepared in the above manner, a roll-to-roll process can be used. The roll-to-roll process is a continuous process in which a process object is transferred using a plurality of rolls and subjected to bonding, coating, etc. In this process, the process object may have a thin sheet shape and may be wound around or unwound from a roll (or roller).

[0140] Hereinafter, the symbols R1, R2, R3, etc. used to describe winding and unwinding are for convenience of description, and these may be the same or different rolls.

[0141] In one example, the method may further include a step of winding the laminate prepared in the first step onto a roll (R1) before performing the second step. Since the wound laminate includes the light diffusion layer having the unevenness, static electricity may be suppressed when the interface between the substrate layer and the light diffusion layer is peeled off even when the wound laminate is unwound. In addition, damage to the substrate layer may be minimized even in a winding state where tension is applied due to the surface roughness in the above range.

[0142] In one example, the laminate prepared in the first step may be maintained in a wound state on a roll (roll: R1) for a predetermined time. In the case of a roll-to-roll process designed to enable mass production, the laminate may be maintained in a wound state for several minutes, several tens of minutes, several hours, or several days due to the need to continuously mass-produce the laminate. The time for which the wound state is maintained is not particularly limited, and may be, for example, 5 minutes or more, 10 minutes or more, 30 minutes or more, or 1 hour or more, specifically, 5 hours or more, 10 hours or more, 20 hours or more, 24 hours or more, or 48 hours or more.

[0143] In one embodiment, the method may perform the second step by unwinding the wound laminate from the roll (roll: R1), i.e., while transporting the unwound laminate, a process of coating a coating composition for a barrier layer on a surface of the laminate opposite to a surface of the substrate layer on which a light diffusion layer is formed, and then drying the coating composition may be performed.

[0144] The drying of the coating composition for the barrier layer is the same as that described above for the formation of the light diffusing layer.

[0145] In one example, the method may further include a step of winding the light-diffusing barrier film prepared in the second step onto a roll (roll: R2) and maintaining the wound state for a predetermined time. In the case of a roll-to-roll process designed to enable mass production, the wound state may be maintained for several minutes, several tens of minutes, several hours, or several days due to the need to continuously mass-produce the barrier film and its components. The time for which the wound state is maintained is not particularly limited, and may be, for example, 5 minutes or more, 10 minutes or more, 30 minutes or more, or 1 hour or more, and specifically, 5 hours or more, 10 hours or more, 20 hours or more, 24 hours or more, or 48 hours or more. After winding, a process for curing the dried barrier layer (coating composition) is performed.

[0146] In one embodiment, the method may further include unwinding the wound light diffusive barrier film from the roll (R2) and curing the polysilazane layer. The curing may ensure the denseness of the barrier layer and may provide better barrier properties.

[0147] The barrier layer may be cured by irradiation with light (e.g., irradiation with UV light) or plasma treatment, etc. UV irradiation may be performed in the same manner as described above.

[0148] In one example, the barrier layer, i.e., the polysilazane layer, can be cured by plasma treatment.

[0149] The plasma treatment is performed by generating plasma in an atmosphere containing a plasma generating gas such as Ar, and injecting cations into the plasma into the polysilazane layer, the plasma being generated by, for example, an external electric field, a negative high voltage pulse, etc. Such plasma treatment can be performed using a known device.

[0150] The plasma treatment for forming the hardened layer may be performed while injecting a discharge gas (Ar) and oxygen into a predetermined treatment space. More specifically, the plasma treatment may be performed under the following conditions.

[0151] In one embodiment, the plasma treatment may be performed under a predetermined power density. Specifically, the power density per unit area of ​​the electrode during the plasma treatment may be about 0.05 W / cm. 2 or 0.10 W / cm 2 In another embodiment, the power density is about 0.2 W / cm or more. 2 More than about 0.3W / cm 2 Above, about 0.4W / cm 2 More than about 0.5W / cm 2 More than about 0.6W / cm 2 More than about 0.7W / cm 2 Above, approximately 0.8W / cm 2 More than or equal to 0.9 W / cm 2Within the range of the power density, in the case of the positive electrode, the higher the power density, the higher the degree of plasma treatment in a short time and the higher the degree of modification of polysilazane due to the application of high voltage. In the case of the negative electrode, an excessively high power density may cause damage to the base layer due to the high voltage, so taking this into consideration, the upper limit of the power density is about 2 W / cm. 2 Below, 1.5W / cm 2 Less than or equal to 1.0 W / cm 2 It may be the following.

[0152] In one example, when the power density is as described above, the processing energy during plasma processing, which is determined by the product of the power density and the processing time, is 50 J / cm. 2 Specifically, the energy may be 45 J / cm or less. 2 Below, 40J / cm 2 Below, 35J / cm 2 Below, 30J / cm 2 Below, 25J / cm 2 Less than or equal to 20 J / cm 2 or less, with the lower limit being 5 J / cm 2 More than 10J / cm 2 or more than 15 J / cm 2 It may be more than that.

[0153] In one example, the plasma treatment may be performed under a predetermined process pressure. Specifically, the process pressure during the plasma treatment may be 350 mTorr or less. In the case of a positive electrode, the lower the process pressure, the easier it is to ensure a mean free path, so that the plasma treatment may be performed without energy loss due to collision with gas molecules. For example, the process pressure may be 340 mTorr or less, 330 mTorr or less, 320 mTorr or less, 310 mTorr or less, 300 mTorr or less, 290 mTorr or less, 280 mTorr or less, 270 mTorr or less, 260 mTorr or less, 250 mTorr or less, 240 mTorr or less, 230 mTorr or less, 220 mTorr or less, 210 mTorr or less, or 200 mTorr or less. Meanwhile, in the case of a negative electrode, the lower the process pressure, the fewer the gas molecules, so a high voltage and power are required to generate plasma, but high voltage and high power can damage the substrate layer, so for example, the lower limit of the process pressure may be 50 mTorr or more, 60 mTorr or more, 70 mTorr or more, 80 mTorr or more, 90 mTorr or more, 100 mTorr or more, 110 mTorr or more, 120 mTorr or more, 130 mTorr or more, 140 mTorr or more, 150 mTorr or more, 160 mTorr or more, 170 mTorr or more, 180 mTorr or more, or 190 mTorr or more. The pressure may be the pressure at the start of the process, or may be maintained within the range during the process.

[0154] When discharge gas (Ar) and oxygen are used as process gases, the vapor pressure of oxygen in the processing space may be in the range of 20 to 80%. The oxygen vapor pressure means the percentage of the injection flow rate of oxygen to the total flow rate of gas injected into the processing space. For example, when the plasma processing is performed while injecting Ar and O2 at flow rates of A sccm and B sccm, respectively, the vapor pressure of oxygen can be calculated as 100×B / (A+B).

[0155] The plasma treatment time may be appropriately adjusted to a level that does not impair the barrier properties of the film, for example, the plasma treatment may be performed for about 10 seconds to 10 minutes.

[0156] In addition, as described above, the light-diffusing barrier film may further include a hard coating layer. The application, drying and / or drying of the coating composition for the light-diffusing layer may be the same as that for forming the hard coating layer.

[0157] In one embodiment, the hard coating layer may be applied simultaneously or at a different time to the coating for the light diffusing layer.

[0158] In another example, the method may further include, before performing the second step, a step of winding the laminate prepared in the first step onto a roll (R1'); and a step of forming a hard coating layer while unwinding the laminate from the roll (R1') to prepare a second laminate. Thereafter, the method may be performed in a manner that includes a step of winding the second laminate having the hard coating layer formed thereon onto a roll (R1"), and performing the second step while unwinding the laminate from the roll (R1").

[0159] Also, as described above, the light-diffusing barrier film may include a plurality of sub-barrier layers. For example, the light-diffusing barrier film may have a structure in which a first sub-barrier layer and a second sub-barrier layer are laminated in order. In this case, the first sub-barrier layer is located closer to the substrate layer than the second sub-barrier layer (see FIG. 2 or FIG. 4). In this case, as described above, a step of applying a coating composition for the second sub-barrier layer to the outer surface of the first sub-barrier layer of the light-diffusing barrier film (F') obtained after curing the first sub-barrier layer, drying the coating composition, and curing the coating composition may be additionally performed. The formation of the second sub-barrier layer may be performed by a roll-to-roll method. As described above, the barrier film (F') may include a light-diffusing layer, a substrate layer, and a first sub-barrier layer in order, or may include a light-diffusing layer, a substrate layer, a hard coating layer, and a first sub-barrier layer in order.

[0160] In one example, the barrier film (F') may be wound on a roll (roll: R3) before the coating composition for the second sub-barrier layer is applied. Then, the coating composition for the second sub-barrier layer may be applied, dried and cured on the barrier film (F') unwound from the roll (roll: R3). As a result, a light-diffusing barrier film (F") may be manufactured which includes at least a light-diffusing layer, a substrate layer, a first sub-barrier layer and a second sub-barrier layer in that order. As described above, the barrier film (F") may further include a hard coating layer between the substrate layer and the first sub-barrier layer, and the related processes are as described above. Effect of the Invention

[0161] According to one example of the present application, since damage to the barrier film during the roll-to-roll process can be prevented, a light-diffusing barrier film having excellent barrier properties against gas and moisture can be provided. In addition, according to one example of the present application, the film manufacturing process is simplified, and the film can be easily made thin and large in area. [Brief description of the drawings]

[0162] [Figure 1] FIG. 2 is a schematic diagram showing the structure of a light-diffusing barrier film according to a specific example of the present application. [Diagram 2] FIG. 2 is a schematic diagram showing the structure of a light-diffusing barrier film according to a specific example of the present application. [Diagram 3] FIG. 2 is a schematic diagram showing the structure of a light-diffusing barrier film according to a specific example of the present application. [Figure 4] FIG. 2 is a schematic diagram showing the structure of a light-diffusing barrier film according to a specific example of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0163] The present application will be described in detail with reference to the following examples, but the scope of protection of the present application is not limited to the following examples.

[0164] <Measurement method> The physical properties of the films of the following Examples and Comparative Examples were measured as follows.

[0165] How to measure surface roughness The surface roughness of the surface of the light diffusing layer was measured by a non-contact (vibrating) method using an AFM (atomic force microscope) instrument, for example, an XE7 instrument manufactured by Park Science.

[0166] How to measure surface resistance The manufactured light-diffusing barrier film was cut into a specimen with a width of 10 cm and a length of 10 cm. Then, using a sheet resistance meter (Hiresta-UP MCP-HT450, Mitsubishi Chemical Co., Ltd.), the electrodes of the meter were pressed with a pressure of 2 kgf, and the sheet resistance was measured with an applied voltage of 500 V. Measurements were taken for 10 seconds at three points in the width direction of each specimen, and the average value was calculated.

[0167] How to measure moisture permeability (1) Moisture permeability (10 -3 g / m 2 day) The moisture permeability of the light-diffusing barrier films finally manufactured in the Examples and Comparative Examples was measured using AQUATRAN 2 (MOCON) at 38° C. and 100% relative humidity.

[0168] (2) Change in moisture permeability (%) It was calculated by the following formula.

[0169] [Formula] Change in moisture permeability (%) = {(BA) / A} x 100

[0170] In the above formula, A is the moisture permeability of the light-diffusing barrier film finally manufactured in each Example and Comparative Example without the blocking process (see item 4 in Example 1 below) (moisture permeability without blocking in Tables 1 and 2), and B is the moisture permeability of the light-diffusing barrier film finally manufactured in each Example and Comparative Example (moisture permeability with blocking in Tables 1 and 2). Each moisture permeability (A, B) was measured using AQUATRAN 2 (MOCON) under conditions of 38°C and 100% relative humidity.

[0171] Haze and light transmittance measurement method The haze and light transmittance of the produced light-diffusing barrier films were measured using a haze meter (hm-150, Murakami Color Research Laboratory).

[0172] <Examples and Comparative Examples> Example 1 1) Forming a light diffusing layer on the substrate layer A coating composition for the light diffusion layer was prepared by mixing 20 parts by weight of a photocurable resin with respect to a solvent. Specifically, 80 parts by weight of pentaerythritol triacrylate (PETA) and 20 parts by weight of dipentaerythritol hexaacrylate (DPHA) were dissolved in a solvent (propylene glycol monomethyl ether). 4 parts by weight of a polymerization initiator (Irgacure 127, Ciba), 5 parts by weight of an antistatic agent (ELEC ME-2, Kao), and 10 parts by weight of particles with an average particle size of 0.8 μm (MX80, Soken) were added to the solution to prepare a composition for the light diffusion layer.

[0173] One side of a 50 μm-thick polyethylene terephthalate (PET) film (T600E50, Mitsubishi) was coated with the bar coat method (using #5 bar).The resulting coating was then dried by heating at 100°C for 2 minutes, and then irradiated with vacuum UV light using a UV light irradiation line to form a light diffusion layer having the surface roughness (Rt) shown in the table below.

[0174] 2) Formation of a hard coating layer On the opposite side of the substrate film on which the light diffusion layer was formed, 80 parts by weight of pentaerythritol triacrylate (PETA) and 20 parts by weight of dipentaerythritol hexaacrylate (DPHA) were dissolved in a solvent (propylene glycol monomethyl ether). A polymerization initiator (Irgacure 127, Ciba) was added in an amount of 4 parts by weight to the solution to prepare a hard coating composition. A coating film was formed on the side of the substrate film on which the light diffusion layer was not formed using a bar coating method, and then the coating was dried at 100°C for 2 minutes and irradiated with UV light to form a hard coating layer with a thickness of 1 μm.

[0175] 3) Formation of a barrier layer Polysilazane (product name NL120) was dissolved in dibutyl ether, and the solution was applied by bar coating to the surface of the hard coating layer on which the base film was not formed. The resulting coating was dried by heating at 70°C for 1 minute and at 130°C for 2 minutes to form a barrier layer with a thickness of 150 nm (formation of uncured barrier layer).

[0176] 4) Blocking Execution The film having a laminated structure of "light diffusion layer / base layer / hard coating layer / barrier layer" formed through the above-mentioned processes 1) to 3) is referred to as the first film (F1). In addition, the second film (F2) was additionally manufactured through the same process as the manufacturing of the first film (F1). The first and second films (F1, F2) were stacked under a load of 18 kg so that the uneven surface of the light diffusion layer of the second barrier film (F2) was in contact with the surface of the barrier layer of the first film (F1), and the load was maintained for 24 hours. At this time, the first and second films (F1, F2) were in the form of sheets, and the size of the contact area was 10 cm x 10 cm. This process was the same as the process when the light diffusion barrier film was wound up in a roll-to-roll process.

[0177] 5) Hardening of the barrier layer (first barrier layer) The first film (F1) was subjected to a plasma treatment to harden the barrier layer. The plasma treatment was carried out at a flow rate of about Ar:O2=1:1 (based on sccm), a pressure of about 138 mTorr, and a pressure of about 0.27 W / cm. 2 of power and about 20J / cm 2 The light-diffusing barrier film of Example 1 was produced by finally curing the barrier layer under the energy conditions of 1000 nm to 1000 nm.

[0178] Example 2 A light-diffusing barrier film of Example 2 was produced in the same manner as in Example 1, except that a different coating bar (#4 bar) was used when coating the composition for the light-diffusing layer. The surface roughness (Rt) value of the light-diffusing layer is as shown in the table below.

[0179] Example 3 The light-diffusing barrier film of Example 3 was produced in the same manner as in Example 1, except that no antistatic agent was used and a different coating bar (#3 bar) was used when coating the composition for the light-diffusing layer. The surface roughness (Rt) value of the light-diffusing layer is as shown in the table below.

[0180] Example 4 The light-diffusing barrier film of Example 4 was manufactured in the same manner as in Example 1, except that no antistatic agent was used in the composition of the light-diffusing layer and particles with an average particle size of 5 μm (GB05S, Aica Kogyo) were used instead of the particles used in Example 1 (coating with #5 bar). The surface roughness (Rt) value of the light-diffusing layer is as shown in the table below.

[0181] Example 5 The light-diffusing barrier film of Example 5 was produced in the same manner as in Example 4, except that a different coating bar was used (#4 bar was used) when coating the composition for the light-diffusing layer. The surface roughness (Rt) value of the light-diffusing layer is as shown in the table below.

[0182] Example 6 The light-diffusing barrier film of Example 6 was prepared in the same manner as in Example 4, except that a different coating bar was used when coating the composition for the light-diffusing layer (coating with a #3 bar). The surface roughness (Rt) value of the light-diffusing layer is as shown in the table below.

[0183] Example 7 A light-diffusing barrier film of Example 7 was prepared in the same manner as in Example 6, except that the thickness of the barrier layer heated and dried in step 3 was 80 nm instead of 150 nm. The surface roughness (Rt) value of the light-diffusing layer is as shown in the table below.

[0184] Example 8 A polysilazane composition was coated and dried on the cured barrier layer (first barrier layer) of the light-diffusing barrier film prepared in Example 3 in the same manner as in step 3) described in Example 1. Then, a light-diffusing barrier film of Example 8 including a first barrier layer (cured) and a cured second barrier layer (cured) (thickness 150 nm) was prepared through steps 4) and 5) described in Example 1. The surface roughness (Rt) value of the light-diffusing layer is as shown in the table below.

[0185] Comparative Example 1 The light-diffusing barrier film of Comparative Example 1 was manufactured in the same manner as in Example 1, except that particles with an average particle size of 20 μm (MX-2000, Soken) were used instead of the particles used in Example 1, a coating composition for the light-diffusing layer containing 50 parts by weight of a photocurable resin relative to the solvent was used, no antistatic agent was used, and knife coating was used when coating the composition for the light-diffusing layer. The surface roughness (Rt) value of the light-diffusing layer is as shown in the table below.

[0186] Comparative Example 2 A light-diffusing barrier film of Comparative Example 2 was prepared in the same manner as in Example 1, except that no antistatic agent was used in the coating composition of the light-diffusing layer. The surface roughness (Rt) value of the light-diffusing layer is shown in the table below.

[0187] Comparative Example 3 A light-diffusing barrier film of Comparative Example 3 was prepared in the same manner as in Example 2, except that no antistatic agent was used in the coating composition of the light-diffusing layer. The surface roughness (Rt) value of the light-diffusing layer is as shown in the table below.

[0188] Comparative Example 4 3) A light-diffusing barrier film of Comparative Example 4 was prepared in the same manner as in Comparative Example 1, except that the thickness of the barrier layer dried by heating in the process was 80 nm instead of 150 nm.

[0189] [Table 1]

[0190] Looking at Examples 3 to 6, it can be seen that the surface resistance is large because no antistatic agent is used when forming the light diffusion layer. However, looking at the rate of change in moisture permeability, it can be seen that the barrier layer is less damaged in these Examples. This is because the surface roughness of the light diffusion layer is sufficient, so damage due to static electricity generated during interfacial peeling is avoided. In Comparative Example 1, the surface unevenness is excessively large, so the barrier layer is damaged by the unevenness and the rate of change in moisture permeability is large.

[0191] On the other hand, when comparing Examples 1 and 2 with Comparative Examples 2 and 3, it can be seen that when the surface roughness of the light diffusion layer is 0.1 μm or less, there is a limit to how much the surface unevenness can reduce the degree of interfacial adhesion between the light diffusion layer and the barrier layer, and therefore it is necessary to adjust the surface resistance of the light diffusion layer within a certain range.

[0192] [Table 2]

[0193] From Table 2, it can be seen that Comparative Example 4 has high "moisture permeability (when blocking is performed)" and "change rate of moisture permeability (%)". In particular, the change rate of moisture permeability is much higher than that of the Examples. This means that if the surface roughness (Rt) of the light diffusion layer is excessively large, the barrier layer will be damaged by the unevenness of the light diffusion layer in the wound state. In other words, the results of Example 7 and Comparative Example 4 suggest that even when the thickness of the barrier layer, which has the greatest effect on the moisture permeability of the film, is the same, it is important to prevent damage to the barrier layer during the roll-to-roll process.

[0194] [Table 3]

[0195] Table 3 shows that the moisture permeability decreases as more barrier layers are included (i.e., two or more sub-barrier layers are included), regardless of whether blocking is performed or not. Specifically, it can be seen that even if a second barrier layer is additionally formed on the first barrier layer after blocking is performed, excellent moisture blocking properties (low moisture permeability) are ensured in the examples of the present application. [Explanation of symbols]

[0196] 10: Barrier layer 11: Second sub-barrier layer 12: First sub-barrier layer 20: Base material layer 30: Light diffusion layer 40: Hard coating layer

Claims

1. The optical film includes a light diffusing layer, a substrate layer, and a barrier layer in that order, The light diffusion layer includes a curable resin, light diffusion particles that form surface irregularities, and an antistatic agent, The light diffusion layer contains 10 parts by weight or more of the light diffusion particles relative to 100 parts by weight of the curable resin, The surface (S 1 ) has a surface roughness (Rt) of 0.02 μm or more and less than 0.1 μm, and the surface (S 1 ) has a surface resistance of 10 10 Ω / sq or less, The change in moisture permeability calculated by the following formula is 30% or less. [Formula] Change in moisture permeability (%) = {(B - A) / A} x 100 In the above formula, A is the light-diffusing barrier film (F 1 ) is the moisture permeability of the light-diffusing barrier film (F 1 ) on the surface of the barrier layer of the light-diffusing barrier film (F 2 A constant load was applied so that the uneven surfaces of the light diffusion layers of the two light diffusion barrier films (F 1 , F 2 ) was placed on the substrate, and the constant load was maintained for 24 hours. Then, the light diffusion barrier film (F 1 ) is the moisture permeability of the light-diffusing barrier film (F 1 , F 2 ) are manufactured through the same process and have the same composition, and the moisture permeability (A, B) is measured using AQUATRAN 2 (MOCON) under conditions of 38° C. and 100% relative humidity.

2. The light-diffusing barrier film of claim 1 , wherein the barrier layer comprises one or more sub-barrier layers.

3. 3. The light-diffusing barrier film according to claim 2, wherein the sub-barrier layer has a thickness in the range of 20 to 400 nm.

4. 4. The light-diffusing barrier film according to claim 2, wherein the barrier layer or the sub-barrier layer is a polysilazane layer or a cured layer of a polysilazane layer.

5. The polysilazane has a unit of the following formula 1: 【Chemistry 1】 In Chemical Formula 1, R 1 , R 2 and R 3 The light-diffusing barrier film according to claim 4, wherein each of the groups independently represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, an aryl group, an alkylsilyl group, an alkylamide group, or an alkoxy group.

6. 6. The light-diffusing barrier film according to claim 1, wherein the light-diffusing layer has a thickness of 20 μm or less.

7. 7. The light-diffusing barrier film according to claim 1, wherein the light-diffusing layer is made of a coating composition containing 10 parts by weight or more of the light-diffusing particles per 100 parts by weight of the curable resin.

8. 8. The light-diffusing barrier film according to claim 1, wherein the light-diffusing layer, the substrate layer and the barrier layer are in direct contact with each other.

9. 9. An electric or electronic device comprising a light-diffusing barrier film according to any one of claims 1 to 8.

10. The light diffusing layer includes a base layer and a light diffusing layer, the light diffusing layer including a curable resin, light diffusing particles that form a surface unevenness, and an antistatic agent, the light diffusing layer including 10 parts by weight or more of the light diffusing particles with respect to 100 parts by weight of the curable resin, and an opposite surface (S 1 ) has a surface roughness (Rt) of 0.02 or more and less than 0.1 μm, and one surface (S 1 ) surface resistance is 10 10 A first step of providing a laminate having a resistivity of less than Ω / sq; A second step of applying a coating composition for a barrier layer on the surface opposite to the surface of the substrate layer on which the light diffusion layer is formed, and then drying the coating composition to form a polysilazane layer; The change in moisture permeability calculated by the following formula is 30% or less. [Formula] Change in moisture permeability (%) = {(B - A) / A} x 100 In the above formula, A is the light-diffusing barrier film (F 1 ) is the moisture permeability of the light-diffusing barrier film (F 1 ) on the surface of the barrier layer of the light-diffusing barrier film (F 2 A constant load was applied so that the uneven surfaces of the light diffusion layers of the two light diffusion barrier films (F 1 , F 2 ) was placed on the substrate, and the constant load was maintained for 24 hours. Then, the light diffusion barrier film (F 1 ) is the moisture permeability of the light-diffusing barrier film (F 1 , F 2 ) are manufactured through the same process and have the same configuration, and the moisture permeabilities (A, B) are measured using AQUATRAN 2 (MOCON Corporation) under conditions of 38° C. and 100% relative humidity.

11. 11. The method for producing a light-diffusing barrier film according to claim 10, wherein a coating composition for a light-diffusing layer, the coating composition including 10 parts by weight or more of the light-diffusing particles per 100 parts by weight of the curable resin, is applied onto one surface of a substrate layer and then cured to form a light-diffusing layer.

12. The coating composition of the barrier layer contains polysilazane represented by the following formula 2: 【Chemistry 2】 In Chemical Formula 2, R 1 , R 2 and R 3 The method for producing a light-diffusing barrier film according to claim 10 or 11, characterized in that each of them independently represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, an aryl group, an alkylsilyl group, an alkylamide group or an alkoxy group.

13. Using a roll-to-roll process, 13. The method for producing a light-diffusing barrier film according to claim 10, further comprising a step of winding up the laminate prepared in the first step onto a roll (R1) before carrying out the second step.

14. The method for producing a light-diffusing barrier film according to claim 13, characterized in that the second step is carried out by unwinding the wound laminate from the roll (R1).

15. The method for producing a light-diffusing barrier film according to claim 14, further comprising the step of winding the light-diffusing barrier film prepared in the second step onto a roll (R2) and maintaining the rolled state for one hour or more.

16. The method for producing a light-diffusing barrier film according to claim 15, further comprising the step of unwinding the wound light-diffusing barrier film from the roll (R2) and curing the polysilazane layer.

17. 17. The method for producing a light-diffusing barrier film according to claim 16, wherein the polysilazane layer is cured by a plasma treatment or UV light irradiation.

Citation Information

Patent Citations

  • Gas barrier laminated film, manufacturing method of it and image displaying element using the film

    JP2005289052A

  • Gas barrier film

    JP2016147967A

  • Optical sheet and method for producing optical sheet

    JP2017040834A

  • Elongated gas barrier laminate and method for producing same

    WO2015152077A1