Insulating composition for electrodes having excellent wet adhesion and method for producing same
The insulating composition for electrodes, using a non-aqueous solvent and inorganic particles, addresses the issue of poor wet adhesion in conventional coating layers, improving lithium ion containment and battery stability.
Patent Information
- Application Number
- JP2023509437
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-07-22
- Filing Date
- 2022-07-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-07-29
AI Technical Summary
Conventional insulating coating layers for electrodes in secondary batteries suffer from poor wet adhesion when impregnated with electrolyte, leading to lithium ion migration and capacity loss, which can cause safety issues.
An insulating composition for electrodes comprising an aqueous binder substituted with a non-aqueous organic solvent and inorganic particles, with a weight ratio of inorganic particles to aqueous binder ranging from 1:99 to 95:5, is applied to form an insulating coating layer.
The insulating composition achieves excellent wet adhesion in electrolytic solutions, preventing lithium ion movement and suppressing capacity development, thereby enhancing the stability and safety of secondary batteries.
Smart Images

Figure 0007580843000006 
Figure 0007580843000007 
Figure 0007580843000008
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0100879 filed on July 30, 2021 and Korean Patent Application No. 10-2022-0090835 filed on July 22, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to an insulating composition for electrodes having excellent wet adhesion and a method for producing the same. [Background technology]
[0003] 2. Description of the Related Art With technological developments and increasing demand for mobile devices, the demand for secondary batteries as an energy source is growing rapidly, and as a result, much research is being conducted into batteries that can meet various needs.
[0004] Typically, from the viewpoint of battery shape, there is a high demand for prismatic batteries and pouch-type batteries that are thin and applicable to products such as mobile phones, and from the viewpoint of materials, there is a high demand for lithium secondary batteries such as lithium cobalt polymer batteries that have excellent energy density, discharge voltage, and safety.
[0005] One of the main research topics for such secondary batteries is to improve their safety. The main cause of safety-related accidents in batteries is the abnormally high temperature caused by a short circuit between the positive and negative electrodes. In other words, under normal circumstances, a separator is located between the positive and negative electrodes and maintains electrical insulation. However, under abnormal circumstances such as when the battery is overcharged or overdischarged, when an internal short circuit occurs due to dendritic growth of the electrode material or a foreign object, when a sharp object such as a nail or screw penetrates the battery, or when the battery is deformed excessively by an external force, the conventional separator alone shows its limitations.
[0006] Generally, a microporous membrane made of polyolefin resin is used as a separator, but its heat resistance is insufficient, being only about 120°C to 160°C. Therefore, when an internal short circuit occurs, the separator shrinks due to the short circuit reaction heat, expanding the short circuit area and causing a thermal runaway state in which more reaction heat is generated. This phenomenon occurs mainly at the edge of the electrode active material coating of the electrode current collector coated with the electrode active material when the electrodes are stacked, and various methods have been attempted to reduce the possibility of short circuiting of the electrodes under external impact or high temperature.
[0007] Specifically, in order to solve the internal short circuit of the battery, methods have been proposed, such as attaching insulating tape to the uncoated portion of the electrode and a part of the active material layer, or coating with an insulating liquid to form an insulating coating layer. For example, there are methods of applying a binder for insulating purposes to the uncoated portion of the positive electrode and a part of the active material layer, or coating with an insulating liquid in which a mixture of the binder and inorganic particles is dispersed in a solvent to form an insulating coating layer.
[0008] Meanwhile, in actual secondary batteries, electrodes exist in a state of being immersed in an electrolyte, and the adhesive strength of the conventional insulating coating layer when immersed in the electrolyte (hereinafter referred to as wet adhesive strength) is reduced, and the layer is unable to prevent lithium ions from migrating to the overlay region of the electrode, resulting in the problem of capacity development (see Figure 1). In particular, lithium ions may precipitate in the overlay region of the electrode when capacity is developed, which may cause a decrease in the safety of the battery cell.
[0009] Therefore, there is a need to develop an insulating composition that has excellent wet adhesion. Summary of the Invention [Problem to be solved by the invention]
[0010] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide an insulating composition for electrodes having excellent wet adhesion, and a method for producing the same. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention provides an insulating composition for an electrode, comprising an aqueous binder substituted with a non-aqueous organic solvent, and inorganic particles, wherein the weight ratio of the inorganic particles to the aqueous binder is within a range of 1:99 to 95:5.
[0012] In a specific embodiment, the weight ratio of the inorganic particles to the aqueous binder is in the range of 45:55 to 90:10.
[0013] In a specific example, the non-aqueous organic solvent is at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAC), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol.
[0014] In another example, the inorganic particles are one or more selected from the group consisting of AlOOH, Al2O3, γ-AlOOH, Al(OH)3, Mg(OH)2, Ti(OH)4, MgO, CaO, Cr2O3, MnO2, Fe2O3, Co3O4, NiO, ZrO2, BaTiO3, SnO2, CeO2, Y2O3, SiO2, silicon carbide (SiC), and boron nitride (BN).
[0015] In another example, the water-based binder is at least one selected from the group consisting of styrene-butadiene rubber, acrylate styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, acrylic rubber, butyl rubber, fluororubber, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene copolymer, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, hydroxypropyl methylcellulose, hydroxypropyl cellulose, and diacetyl cellulose.
[0016] For example, in the electrode insulating composition according to the present invention, the non-aqueous organic solvent is N-methyl-pyrrolidone (NMP) and the aqueous binder is styrene-butadiene rubber.
[0017] In one embodiment, the inorganic particles have an average particle size in the range of 0.01 μm to 100 μm.
[0018] In a more specific embodiment, the insulating composition according to the present invention comprises first and second inorganic particles having a particle size balance different from each other and has a bimodal particle size distribution.
[0019] For example, the insulating composition has a viscosity at 25°C in the range of 50 cP to 50,000 cP.
[0020] In one embodiment, the insulating composition according to the present invention is applied to the positive electrode of a secondary battery.
[0021] The present invention also provides a method for producing the insulating composition for an electrode described above. In one embodiment, the method for producing the insulating composition for an electrode according to the present invention includes mixing an aqueous binder dispersed in water with a non-aqueous organic solvent, and performing a solvent replacement while removing the contained water through a heat treatment.
[0022] In one embodiment, the method further comprises, after the solvent replacing step, including a step of including inorganic particles.
[0023] In a specific embodiment, the weight ratio of the inorganic particles to the aqueous binder is in the range of 1:99 to 95:5.
[0024] In another embodiment, the heat treatment in the solvent replacement step is carried out at a temperature in the range of 80 to 150°C. Effect of the Invention
[0025] The present invention provides an insulating composition for electrodes having excellent wet adhesion and a method for manufacturing the same. The insulating composition has an advantage that it has excellent wet adhesion in an electrolyte and can inhibit the migration of lithium ions in the overlay region of an electrode, thereby suppressing capacity expression, etc. [Brief description of the drawings]
[0026] [Figure 1] FIG. 2 is a schematic diagram showing the movement of lithium ions in an overlay region of an electrode. [Diagram 2] FIG. 4 is a diagram showing the results of measuring the wet adhesion strength of coating layers formed of insulating compositions in Examples and Comparative Examples. [Diagram 3] 1 is a graph showing the results of measuring the discharge capacity to evaluate the capacity development of the battery cells of Examples 5 to 7 (room temperature discharge characteristics). [Figure 4] 1 is a graph showing the results of measuring the discharge capacity to evaluate the capacity development of the battery cells of Examples 5 to 7 (high temperature discharge characteristics). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] While the present invention may be modified in various ways and may have a variety of embodiments, specific examples will be described in detail in the detailed description.
[0028] It should be understood, however, that this is not intended to limit the invention to the particular embodiment, but rather to include all modifications, equivalents, or alternatives falling within the spirit and scope of the invention.
[0029] In the present invention, the terms "comprise" or "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0030] In addition, in the present invention, when a layer, film, region, plate, or other portion is described as being "on" another portion, this includes not only the case where it is "directly on" the other portion, but also the case where there is another portion in between. Conversely, when a layer, film, region, plate, or other portion is described as being "under" the other portion, this includes not only the case where it is "directly under" the other portion, but also the case where there is another portion in between. In addition, in the present application, being "located on" may include not only the case where it is located at the top, but also the case where it is located at the bottom.
[0031] In the present invention, the term "insulating coating layer" refers to an insulating member formed by applying and drying from at least a portion of an uncoated portion of an electrode current collector to at least a portion of an electrode active material layer.
[0032] In the present invention, the term "wet adhesion" refers to the adhesion of an insulating coating layer measured in a state where the insulating coating layer is immersed in an electrolyte. More specifically, the wet adhesion can be measured by immersing a metal test piece having an insulating coating layer formed thereon in an electrolyte, applying ultrasonic waves, and then checking whether or not the insulating coating layer is swelled or detached.
[0033] In the present invention, the term "metal test piece" refers to a space in which an insulating coating layer is formed, and refers to a metal current collector used in the manufacture of an electrode, and may be a metal current collector punched to have a predetermined width and length. For example, the metal test piece may be aluminum, copper, or an aluminum alloy.
[0034] In the present invention, the term "overlay region" refers to a region of an electrode where an insulating coating layer is formed. More specifically, the insulating coating layer covers from at least a portion of a non-coated portion of an electrode on which an active material layer is formed to at least a portion of the active material layer, and the region of the active material layer on which the insulating coating layer is formed can be referred to as the overlay region.
[0035] The present invention will now be described in more detail.
[0036] <Insulating composition> In one embodiment, the present invention includes an aqueous binder substituted with a non-aqueous organic solvent, and inorganic particles, and the weight ratio of the inorganic particles to the aqueous binder is within the range of 1:99 to 95:5.
[0037] The insulating composition for an electrode according to the present invention has an advantage that it has excellent wet adhesion in an electrolyte and can inhibit the migration of lithium ions in the overlay region of an electrode, thereby suppressing the expression of capacity.
[0038] Generally, electrodes in secondary batteries exist in a state of being impregnated with an electrolyte, but the wet adhesion strength of conventional insulating coating layers decreases when the electrodes are impregnated with an electrolyte, and the layers are unable to prevent lithium ions from migrating to the overlay region of the electrodes, resulting in the problem of capacity development. In particular, lithium ions may precipitate in the overlay region of the electrodes when capacity development occurs, which may cause a decrease in the stability of the battery cell.
[0039] In the present invention, an insulating composition for an electrode is provided, which includes an aqueous binder substituted with a non-aqueous organic solvent used as a solvent for an electrode slurry, and inorganic particles dispersed therein, thereby improving wet adhesion in an electrolyte. That is, the insulating composition improves wet adhesion when applied to an electrode, and can suppress the migration of lithium ions in an overlay region of the electrode, thereby preventing the precipitation of lithium ions. As a result, the insulating composition can improve the stability of a secondary battery when applied to an electrode of the secondary battery.
[0040] In a specific example, the insulating composition for electrodes according to the present invention has a composition in which inorganic particles and a water-based binder are mixed in a range of 1:99 to 95:5. The insulating coating layer formed from the insulating composition for electrodes has excellent wet adhesion.
[0041] Meanwhile, the wet adhesion strength of the insulating coating layer can be measured by immersing a metal test piece having an insulating coating layer formed thereon in an electrolyte, applying ultrasonic waves to the metal test piece, and then checking whether or not the insulating coating layer formed on the metal test piece is swelled or detached.
[0042] The electrolyte used in measuring the wet adhesion strength may contain an organic solvent and an electrolyte salt, and the electrolyte salt may be a lithium salt. The lithium salt may be any of those commonly used in non-aqueous electrolytes for lithium secondary batteries without any restrictions. For example, the anion of the lithium salt may be F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 -, CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - The composition may contain any one or two or more selected from the group consisting of:
[0043] The organic solvent contained in the electrolyte may be any organic solvent commonly used in electrolytes for lithium secondary batteries, and may be any organic solvent such as ether, ester, amide, linear carbonate, or cyclic carbonate, which may be used alone or in combination of two or more. Among these, the electrolyte may typically contain a carbonate compound that is a cyclic carbonate, a linear carbonate, or a mixture thereof.
[0044] Furthermore, the insulating composition for an electrode according to the present invention is applied to a positive electrode, and the non-aqueous organic solvent may be at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAC), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol.
[0045] In a specific example, the non-aqueous organic solvent may be one or more selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAC) and dimethylsulfoxide (DMSO), or may be one or more selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF) and dimethylacetamide (DMAC).
[0046] For example, the non-aqueous organic solvent may be an amide-based organic solvent, and the same solvent as that used in preparing the positive electrode slurry may be used, and the non-aqueous organic solvent may be N-methyl-pyrrolidone (NMP).
[0047] In a specific example, when the insulating composition according to the present invention is applied to an insulating coating layer of a positive electrode, it can be introduced into a process of simultaneously coating and drying the coating of the positive electrode active material layer. In this case, when the solvent of the insulating composition is the same as the solvent of the positive electrode slurry, it is possible to reduce the difference in drying speed, etc., and prevent cracks from occurring at the boundary between the insulating coating layer and the positive electrode active material layer. In particular, the NMP solvent is used as a replacement solvent, and the aqueous binder can be present as a binder replaced with NMP.
[0048] The aqueous binder may be one or more selected from the group consisting of styrene-butadiene rubber, acrylate styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, acrylic rubber, butyl rubber, fluororubber, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene copolymer, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenol resin, epoxy resin, polyvinyl alcohol, hydroxypropyl methylcellulose, hydroxypropyl cellulose, and diacetyl cellulose. In a specific example, the aqueous binder may be one or more selected from the group consisting of styrene-butadiene rubber, acrylate styrene-butadiene rubber, acrylonitrile-butadiene rubber, and acrylonitrile-butadiene-styrene rubber. For example, the aqueous binder may be styrene-butadiene rubber.
[0049] Conventionally, polyvinylidene fluoride (hereinafter referred to as PVDF) has been used as a binder for the insulating coating layer of the positive electrode, but this has a problem of decreasing wet adhesion when immersed in an electrolyte. Therefore, in the present invention, SBR can be used as the binder polymer. Meanwhile, when SBR is used as the polymer binder, water can be used as the solvent. In this case, gelation of PVDF, an organic binder used as a binder for the positive electrode, may occur between the insulating composition and the positive electrode slurry when the insulating composition is simultaneously coated with the positive electrode slurry. As a result, cracks may occur at the boundary between the insulating composition for the electrode and the positive electrode slurry.
[0050] Furthermore, the insulating composition contains inorganic particles, which can improve the safety of the battery and can also improve the strength of the insulating coating layer. The content of the inorganic particles can be appropriately adjusted in consideration of the viscosity, heat resistance, insulating properties, filling effect, dispersibility, or stability of the insulating composition. In general, the larger the size of the inorganic particles, the higher the viscosity of the composition containing them, and the higher the possibility of settling in the insulating composition. In addition, the smaller the size, the higher the heat resistance tends to be. Therefore, considering the above points, inorganic particles of appropriate type and size can be selected, and two or more types of inorganic particles can be used together as necessary.
[0051] In a specific example, the inorganic particles may be one or more selected from the group consisting of AlOOH, Al2O3, γ-AlOOH, Al(OH)3, Mg(OH)2, Ti(OH)4, MgO, CaO, Cr2O3, MnO2, Fe2O3, Co3O4, NiO, ZrO2, BaTiO3, SnO2, CeO2, Y2O3, SiO2, silicon carbide (SiC) and boron nitride (BN), or one or more selected from the group consisting of AlOOH, Al2O3, γ-AlOOH and Al(OH)3. For example, the inorganic particles may be AlOOH.
[0052] The weight ratio of the inorganic particles to the aqueous binder may be within the range of 1:99 to 95:5, specifically within the range of 45:55 to 90:10, or within the range of 50:50 to 90:10. For example, the weight ratio of the inorganic particles to the aqueous binder in the insulating composition may be 50:50. On the other hand, if the content of the aqueous binder is too low, it is difficult to exhibit the insulating effect aimed at in the present invention, and the adhesive strength with the electrode may be weakened. Furthermore, if the content of the aqueous binder is too high, the insulating composition may flow into the overlay region when coating the electrode, causing a decrease in the safety of the battery cell.
[0053] The inorganic particles may have an average particle size of 0.1 μm to 100 μm, 0.5 μm to 80 μm, 1 μm to 50 μm, 2 μm to 30 μm, 3 μm to 20 μm, or 5 μm to 10 μm. If the size of the inorganic particles is within the above range, the electrodes cannot be uniformly coated with the inorganic particles, and the resistance of lithium ions can be minimized to ensure the performance of the lithium secondary battery.
[0054] In another example, the insulating composition may include first and second inorganic particles having different particle size balances and have a bimodal particle size distribution. This means that the inorganic particles are a mixture of small and large particles, and an appropriate amount of inorganic particles may be dispersed so that the empty spaces between the large first inorganic particles can be filled with the small second inorganic particles. However, the present invention is not limited to this.
[0055] Meanwhile, in the insulating composition for electrodes according to the present invention, the inorganic particles and SBR may be contained in an amount of 1 to 50 parts by weight, or 5 to 40 parts by weight, or 10 to 40 parts by weight, based on 100 parts by weight of the NMP solvent.
[0056] The insulating composition may have a viscosity at 25°C of 50 cP to 50,000 cP, 100 cP to 45,000 cP, 1,000 cP to 40,000 cP, 2,000 cP to 35,000 cP, 3,000 cP to 30,000 cP, 4,000 cP to 20,000 cP, or 5,000 cP to 10,000 cP. When the viscosity is within the above range, the adhesive strength with the electrode active material layer can be improved, and coating properties, processability, and the like can be improved.
[0057] In one example, the insulating composition for an electrode according to the present invention can be prepared by mixing an aqueous binder dispersed in water with a non-aqueous organic solvent, and then performing a solvent replacement by removing the contained water through a heat treatment. In the present invention, by forming an aqueous binder replaced with a non-aqueous organic solvent, an insulating coating layer containing the aqueous binder can be applied to a positive electrode that is vulnerable to moisture.
[0058] In another example, the method further includes a step of adding inorganic particles after the step of replacing the solvent. Specifically, the weight ratio of the inorganic particles to the aqueous binder is in the range of 1:99 to 95:5. The mixing ratio of the inorganic particles to the aqueous binder is as described above.
[0059] In one example, in the solvent replacement step, the heat treatment is performed within a range of 80 to 150°C. The heat treatment is intended to evaporate and remove the water component contained in the water-based binder. The heat treatment process can be performed under atmospheric pressure (1 atm), and can also be performed under vacuum or reduced pressure conditions (0.1 atm or more and less than 1 atm) for rapid water evaporation. The heat treatment is intended to effectively evaporate water, and can be performed within a range of 80 to 150°C or within a range of 100 to 130°C.
[0060] <Electrode for secondary batteries> In one embodiment, the present invention comprises: A metal current collector; an active material layer located on the metal current collector; the metal current collector includes a non-coated portion where the active material layer is not located, an insulating coating layer is formed covering at least a portion of the non-coated portion to at least a portion of the active material layer, The insulating coating layer includes inorganic particles and an aqueous binder substituted with a non-aqueous organic solvent.
[0061] The secondary battery electrode according to the present invention has an advantage in that it includes an insulating coating layer having excellent wet adhesion and can inhibit the migration of lithium ions in the overlay region of the electrode, thereby suppressing the capacity development.
[0062] In a specific example, the inorganic particles of the insulating coating layer may be one or more selected from the group consisting of AlOOH, Al2O3, γ-AlOOH, Al(OH)3, Mg(OH)2, Ti(OH)4, MgO, CaO, Cr2O3, MnO2, Fe2O3, Co3O4, NiO, ZrO2, BaTiO3, SnO2, CeO2, Y2O3, SiO2, silicon carbide (SiC) and boron nitride (BN), or one or more selected from the group consisting of AlOOH, Al2O3, γ-AlOOH and Al(OH)3. For example, the inorganic particles may be AlOOH.
[0063] Furthermore, the water-based binder may be one or more selected from the group consisting of styrene-butadiene rubber, acrylate styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, acrylic rubber, butyl rubber, fluororubber, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene copolymer, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenol resin, epoxy resin, polyvinyl alcohol, hydroxypropyl methylcellulose, hydroxypropyl cellulose and diacetyl cellulose. In a specific example, the water-based binder may be one or more selected from the group consisting of styrene-butadiene rubber, acrylate styrene-butadiene rubber, acrylonitrile-butadiene rubber and acrylonitrile-butadiene-styrene rubber. For example, the water-based binder may be styrene-butadiene rubber.
[0064] In a specific example, the aqueous binder may be an aqueous binder substituted with a non-aqueous organic solvent, or may be styrene-butadiene rubber substituted with an amide-based solvent, for example, styrene-butadiene rubber substituted with an NMP solvent. More specifically, the insulating coating layer may be formed by applying the insulating composition for a secondary battery electrode described above to cover at least a portion of the non-coated portion to at least a portion of the active material layer, and then drying at a temperature of about 50 to 300° C. In this case, the insulating coating layer may be present as styrene-butadiene rubber in which the solvent is removed during the drying process and the styrene-butadiene rubber dispersed in the solvent is substituted with the NMP.
[0065] In one example, the thickness of the insulating coating layer is set within a range of 0.2 μm to 100 μm, and may be specifically 1 μm to 50 μm, and more specifically 1 μm to 30 μm, 2 μm to 30 μm, 3 μm to 20 μm, or 5 μm to 15 μm. If the thickness of the coating portion is too thin, it is difficult to expect the effect of improving safety by applying the insulating coating layer.
[0066] Furthermore, the secondary battery electrode may be a positive electrode.
[0067] Furthermore, the active material layer may include a positive electrode active material. In a specific example, the positive electrode active material may be any commonly used positive electrode active material, such as, but not limited to, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or a lithium composite oxide that is a combination of these.
[0068] The content of the positive electrode active material may be 85 to 95 parts by weight, specifically 88 to 95 parts by weight, 90 to 95 parts by weight, 86 to 90 parts by weight, or 92 to 95 parts by weight, per 100 parts by weight of the active material layer.
[0069] In this case, the conductive material can be used to improve the performance of the positive electrode, such as the electrical conductivity, and can be one or more selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber. For example, the conductive material may include acetylene black.
[0070] The conductive material may be contained in an amount of 1 to 10 parts by weight, specifically 2 to 8 parts by weight, or 2 to 6 parts by weight, relative to 100 parts by weight of the active material layer.
[0071] Furthermore, the binder may include one or more resins selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, and copolymers thereof. As an example, the binder may include polyvinylidene fluoride.
[0072] The binder may be contained in an amount of 1 to 10 parts by weight, specifically 2 to 8 parts by weight, or 2 to 6 parts by weight, relative to 100 parts by weight of the entire active material layer.
[0073] Furthermore, the average thickness of the active material layer is not particularly limited, but may be specifically 0.1 μm to 20 μm, and more specifically 0.1 μm to 15 μm, 0.1 μm to 10 μm, 2 μm to 10 μm, 4 μm to 10 μm, or 5 μm to 9 μm.
[0074] Meanwhile, the positive electrode for a lithium secondary battery according to the present invention can use a current collector having high conductivity without inducing chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. can be used, and in the case of aluminum or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the current collector can be formed with fine irregularities on the surface to increase the adhesive force of the positive electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. Furthermore, the average thickness of the current collector can be appropriately applied to 3 to 500 μm in consideration of the conductivity and total thickness of the positive electrode to be manufactured.
[0075] <Lithium secondary battery> In one embodiment, the present invention provides a lithium secondary battery including the above-described secondary battery electrode according to the present invention.
[0076] As explained above, the secondary battery electrode according to the present invention can be used as a positive electrode in a lithium secondary battery.
[0077] A lithium secondary battery according to the present invention may include the above-described positive electrode of the present invention, a negative electrode, and a separator located between the positive electrode and the negative electrode.
[0078] In particular, the lithium secondary battery according to the present invention has an advantage that the insulating coating layer has excellent wet adhesion in an electrolyte and can prevent the migration of lithium ions in the overlay region of the electrode, thereby suppressing capacity development, etc. As a result, the lithium secondary battery according to the present invention can have improved stability.
[0079] Here, the negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector and containing a negative electrode active material. Specifically, the negative electrode is manufactured by applying a negative electrode active material onto the negative electrode current collector, drying and pressing the negative electrode active material, and may further include the conductive material, organic binder polymer, filler, etc. as necessary.
[0080] In addition, the negative electrode active material may be, for example, graphite having a perfect layered crystal structure such as natural graphite, soft carbon having a low crystalline layered crystal structure (graphene structure; a structure in which hexagonal honeycomb-shaped carbon planes are arranged in layers), hard carbon in which such a structure is mixed with a non-crystalline portion, carbon and graphite materials such as artificial graphite, expanded graphite, carbon fiber, non-graphitizable carbon, carbon black, carbon nanotubes, fullerene, and activated carbon; x Fe2O3(0≦x≦1), Li x WO2(0≦x≦1), Sn x Me 1-x Me' y O z(Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, Group 1, 2, 3 elements of the periodic table, halogen; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8), etc. metal composite oxides; lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4 and Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials; titanium oxides; lithium titanium oxides, etc. can be used.
[0081] As an example, the negative electrode active material may contain both graphite and silicon (Si)-containing particles. As the graphite, it may contain any one or more of natural graphite having a layered crystal structure and artificial graphite having an isometric structure. As the silicon (Si)-containing particles, they are particles mainly containing silicon (Si) as a metal component, and may include silicon (Si) particles, silicon oxide (SiO2) particles, or a mixture of the silicon (Si) particles and silicon oxide (SiO2) particles.
[0082] In this case, the negative electrode active material may contain 80 to 95 parts by weight of graphite and 1 to 20 parts by weight of silicon (Si)-containing particles with respect to 100 parts by weight in total. The present invention can reduce the lithium consumption amount and irreversible capacity loss during the initial charge and discharge of the battery and improve the charge capacity per unit mass by adjusting the content of graphite and silicon (Si)-containing particles contained in the negative electrode active material within the above range.
[0083] Also, the negative electrode active material layer may have an average thickness of 100 μm to 200 μm. Specifically, it may have an average thickness of 100 μm to 180 μm, 100 μm to 150 μm, 120 μm to 200 μm, 140 μm to 200 μm, or 140 μm to 160 μm.
[0084] Furthermore, the negative electrode current collector is not particularly limited as long as it has high conductivity without inducing a chemical change in the battery. For example, copper, stainless steel, nickel, titanium, baked carbon, etc. can be used. In the case of copper or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. can also be used.
[0085] In addition, the negative electrode current collector may have fine irregularities on its surface to strengthen the bonding force with the negative electrode active material, similar to the positive electrode current collector, and may be in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a nonwoven fabric, etc. Furthermore, the average thickness of the negative electrode current collector may be appropriately set to 3 to 500 μm, taking into consideration the conductivity and total thickness of the negative electrode to be manufactured.
[0086] The separator is an insulating thin film having high ion permeability and mechanical strength, and is interposed between the positive and negative electrodes. The separator is not particularly limited as long as it is one commonly used in the industry. Specifically, a sheet or nonwoven fabric made of chemically resistant and hydrophobic polypropylene, glass fiber, or polyethylene can be used. In some cases, a composite separator made of a porous polymer substrate such as the sheet or nonwoven fabric coated with inorganic particles / organic particles by an organic binder polymer can be used. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte can also serve as the separator. The pore diameter of the separator may be an average of 0.01 to 10 μm, and the thickness may be an average of 5 to 300 μm.
[0087] Meanwhile, the positive electrode and the negative electrode may be wound in a jelly roll form and housed in a cylindrical battery, a square battery, or a pouch battery, or may be housed in a pouch battery in a folded or stack-and-folded form, but is not limited thereto.
[0088] The lithium salt-containing electrolyte according to the present invention may be composed of an electrolyte and a lithium salt. The electrolyte may be a non-aqueous organic solvent, an organic solid electrolyte, or an inorganic solid electrolyte.
[0089] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydroxyfuran (franc), 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0090] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymerizing agents containing an ionic dissociation group.
[0091] Examples of the inorganic solid electrolyte that can be used include nitrides, halides, and sulfates of Li, such as Li3N, LiI, Li5Ni2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, and Li3PO4-Li2S-SiS2.
[0092] The lithium salt is a substance that is easily dissolved in a non-aqueous electrolyte, and examples of the lithium salt include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylates, lithium 4-phenylboronate, imides, etc. can be used.
[0093] In addition, for the purpose of improving charge / discharge characteristics, flame retardancy, etc., the electrolyte may contain, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. In some cases, in order to impart non-flammability, a halogen-containing solvent such as carbon tetrachloride or trifluoroethylene may be further contained, and in order to improve high-temperature storage characteristics, carbon dioxide gas may be further contained, or FEC (Fluoro-Ethylene Carbonate), PRS (Propene sultone, propene sultone, etc. may be further contained.
[0094] Meanwhile, in one embodiment, the present invention provides a battery module including the above-mentioned secondary battery as a unit cell, and provides a battery pack including the battery module.
[0095] The battery pack can be used as a power source for medium- to large-sized devices that require high temperature stability, long cycle characteristics, and high rate characteristics. Specific examples of such medium- to large-sized devices include power tools that are driven by electric motors; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs); electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts; and power storage systems, and more specifically, examples thereof include hybrid electric vehicles (HEVs), but are not limited to these.
[0096] Furthermore, the positive and negative electrodes may be wound in a jelly roll form and housed in a cylindrical battery, a square battery, or a pouch battery, or may be folded or stacked and folded and housed in a pouch battery. For example, the lithium secondary battery according to the present invention may be a pouch battery.
[0097] As described above, the lithium secondary battery including the positive electrode active material according to the present invention can be used in a battery module or battery pack including a number of unit batteries. Specifically, the lithium secondary battery is useful in the fields of portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0098] The present invention will now be described in more detail with reference to examples and experimental examples.
[0099] However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.
[0100] <Example 1> 100g of styrene-butadiene rubber (hereinafter referred to as SBR) (ZEON, BM451B product) binder dispersed in water as a solvent at a ratio of 60:40 (parts by weight) was added to 500g of N-methyl-2-pyrrolidone (NMP) solvent and stirred. Next, the stirred mixture was heated at 100-120°C for 2 hours to completely evaporate the contained water, producing an NMP-substituted SBR binder. Next, the NMP-substituted SBR binder and inorganic particles were mixed and stirred in a weight ratio of 50:50 to produce an insulating composition. The viscosity of the produced insulating composition was 5,000 cP.
[0101] <Examples 2 to 4, Comparative Examples 1 to 2> An insulating coating solution was obtained in the same manner as in Example 1, except that the contents of inorganic particles and binder were changed when preparing the insulating composition.
[0102] The specific compositions of Examples 1 to 4 and Comparative Examples 1 and 2 are shown in Table 1 below.
[0103] [Table 1]
[0104] <Experimental Example 1. Measurement of wet adhesion strength of insulating coating layer> In order to evaluate the adhesive strength of the insulating coating layer according to the present invention, the following experiment was carried out.
[0105] (Metal test piece with insulating coating layer) The insulating compositions produced in Examples 1 to 4 and Comparative Examples 1 and 2 were coated on aluminum metal foil and dried to prepare metal test pieces having an insulating coating layer of about 10 μm in thickness. The metal test pieces having the insulating coating layer were punched out to a size of 2 cm × 2 cm using a punching machine for adhesive strength measurement.
[0106] (Ultrasonic application) 200 g of an electrolyte (EC / EMC=3 / 7 (vol.%)) was placed in a 250 ml beaker, and the metal test piece on which the insulating layer was formed was impregnated with the electrolyte. In order to control the movement of the metal test piece, the metal test piece was fixed with a jig.
[0107] In addition, ultrasonic waves were applied to the electrolyte in which the metal test pieces were impregnated, using an ultrasonic disperser (BANDELIN, 4200). The conditions for applying ultrasonic waves were as follows. - Frequency: 20kHz - Tip diameter: 13mm (TS-113) - Amplitude: 100% (Peak-to-peak interval 132μm when using a 13mm tip)
[0108] The results are shown in Table 2 below and in FIG.
[0109] [Table 2]
[0110] Figure 2 shows the results of measuring the wet adhesion strength of the insulating coating layer of Examples 1 and 4 and Comparative Examples 1 and 2. As can be seen from Table 2 and Figure 2, the insulating coating layer of the electrode specimen of Example 1 did not experience swelling or detachment. However, in the case of Example 1, the boiling point of EMC was 107.5°C due to the increase in temperature of the electrolyte caused by the application of ultrasound, and the measurement environment changed when the solvent evaporated and reached 109°C, and the measurement was stopped.
[0111] Furthermore, in the cases of Examples 2 and 3, although not shown in the photographs, no swelling or detachment occurred in the insulating coating layer of the electrode test piece, similar to Example 1. However, the boiling point of EMC is 107.5°C, and the measurement environment changed due to the evaporation of the solvent, and the measurement was stopped when it reached 109°C.
[0112] In the case of Example 4, no swelling or detachment occurred in the electrode specimen for 15 minutes after ultrasonic waves were applied to the electrolyte. However, although not shown in the figure, when the temperature of the electrolyte increased to 108°C due to the continued application of ultrasonic waves, swelling and detachment of the electrode specimen occurred.
[0113] Furthermore, in the case of Comparative Examples 1 and 2, swelling and detachment occurred in the electrode test pieces 5 minutes after ultrasonic waves were applied to the electrolyte.
[0114] Through this, it was confirmed that the insulating coating layer of the embodiment had superior wet adhesion strength compared to the insulating coating layers of Comparative Examples 1 and 2.
[0115] <Experimental Example 2. Evaluation of battery cell capacity development> In order to evaluate the performance of the positive electrode including the insulating coating layer according to the present invention, a half cell was prepared and then the capacity development was evaluated.
[0116] (Half-cell manufacturing) LiNi as the positive electrode active material 0.8 Co 0.1 Mn 0.1 96 parts by weight of O2, 2 parts by weight of PVDF as a binder, and 2 parts by weight of carbon black as a conductive material were weighed and mixed in N-methylpyrrolidone (NMP) solvent to prepare a slurry for a positive electrode active material. The above slurry for the active material layer was applied to an aluminum foil, dried, and then rolled to prepare a positive electrode having a positive electrode active material layer (average thickness: 130 μm).
[0117] In addition, the positive electrode was dip-coated with the insulating coating solution obtained in Examples 1 to 3, and then dried in a convection oven (130°C) to form an insulating coating layer with a thickness of 10 μm on the positive electrode. A coin-type half cell was manufactured using lithium foil as the negative electrode and an electrolyte containing 1M LiPF6 in a solvent of EC:DMC:DEC=1:2:1.
[0118] [Table 3]
[0119] (Measurement of discharge capacity) The discharge characteristics were evaluated under the following conditions for the batteries of Examples 5 to 7. The discharge characteristics were measured at room temperature (25° C.) and at a high temperature (45° C.). -Discharge: 0.1C, 0.33C, 0.5C, 1.0C, 2.5V cutoff
[0120] On the other hand, in order to compare the capacity development of each battery, a battery cell including an electrode on which an insulating coating layer was not formed was used as Comparative Example 3. The results are shown in Table 4 and FIG. 3, and Table 5 and FIG. 4.
[0121] [Table 4]
[0122] [Table 5]
[0123] Referring to Tables 4 and 5 and Figures 3 and 4 above, it was confirmed that in the case of Example 7, a portion of the capacity was expressed during 0.1C discharge at high temperature (45°C), but the batteries of Examples 5 and 6 hardly expressed any capacity during room temperature discharge (25°C).
[0124] These results suggest that the insulating coating layer has excellent wet adhesion in the electrolyte and prevents the movement of lithium ions in the overlay region of the electrode, thereby suppressing the development of capacity during discharge. As a result, the lithium secondary battery according to the present invention is expected to be able to improve safety while suppressing capacity degradation due to increased cycles.
[0125] Although the present invention has been described above with reference to preferred embodiments thereof, it will be understood that a person skilled in the art or having ordinary knowledge in the art can make various modifications and variations to the present invention without departing from the spirit and technical scope of the present invention as described in the claims below.
[0126] Therefore, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.
Claims
1. The binder includes an aqueous binder substituted with a non-aqueous organic solvent, and inorganic particles, the weight ratio of the inorganic particles to the aqueous binder is in the range of 1:99 to 95:5; The non-aqueous organic solvent is N-methyl-pyrrolidone (NMP); the water-based binder is styrene-butadiene rubber; The insulating composition for an electrode, wherein the inorganic particles are at least one type selected from the group consisting of AlOOH, Al(OH) 3 , Mg(OH) 2 , Ti(OH) 4 , silicon carbide (SiC) and boron nitride (BN).
2. 2. The insulating composition for electrodes according to claim 1, wherein a weight ratio of said inorganic particles to said aqueous binder is within a range of 45:55 to 90:
10.
3. 2. The insulating composition for electrodes according to claim 1, wherein the inorganic particles have an average particle size in the range of 0.01 μm to 100 μm.
4. The insulating composition for an electrode according to claim 3 , wherein the insulating composition for an electrode contains first inorganic particles and second inorganic particles having particle size balances different from each other, and has a bimodal particle size distribution.
5. 2. The electrode insulating composition according to claim 1, wherein the electrode insulating composition has a viscosity of 50 cP to 50,000 cP at 25°C.
6. The insulating composition for an electrode according to claim 1 , which is applied to a positive electrode of a secondary battery.
7. mixing an aqueous binder dispersed in water with a non-aqueous organic solvent; and performing a solvent exchange while removing the water contained therein through a heat treatment. The method for producing an insulating composition for electrodes, wherein the non-aqueous organic solvent is N-methyl-pyrrolidone (NMP), and the aqueous binder is styrene-butadiene rubber.
8. The method for producing an insulating composition for an electrode according to claim 7 , further comprising the step of adding inorganic particles after the step of replacing the solvent.
9. A step of mixing an aqueous binder dispersed in water with a non-aqueous organic solvent; removing water contained in the mixture by heat treatment and replacing the solvent; and incorporating inorganic particles, A method for producing an insulating composition for an electrode, wherein the weight ratio of the inorganic particles to the aqueous binder is within a range of 1:99 to 95:
5.
10. A method of producing a binder composition comprising the steps of: mixing an aqueous binder dispersed in water with a non-aqueous organic solvent; and performing a solvent exchange while removing the water contained therein through a heat treatment. In the solvent replacement step, the heat treatment is performed at a temperature in the range of 80 to 150° C.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery and manufacturing method of electrode
JP2009054455A
Non-aqueous secondary battery
JP2009134915A
Method for manufacturing slurry for lithium ion secondary battery heat-resistant layer and method for manufacturing electrode for lithium ion secondary battery
JP2014165096A
Secondary battery, battery pack, and vehicle
JP2018160444A
Electrode and nonaqueous electrolyte secondary battery
JP2020136117A