Neutral stripping composition
A neutral release agent composition efficiently separates layers of multilayer resin molded bodies, addressing the issues of decomposition and corrosion in existing agents, allowing for the recovery of materials like aluminum and polyester.
Patent Information
- Application Number
- JP2023575647
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-07-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-07-11
AI Technical Summary
Existing cleaning agents for multilayer resin molded bodies are either too alkaline, causing decomposition, corrosion, and dissolution of materials, or insufficient for effectively separating layers, making recycling difficult and manual cleaning inefficient.
A neutral release agent composition comprising specific polar solvents, amphiphilic glycols, fatty acid salts, paraffinic hydrocarbons, and alkanolamide surfactants, which allows for the separation of multilayer resin molded articles without damaging the base materials.
The neutral release agent effectively separates layers of multilayer resin molded bodies, preventing decomposition and corrosion, enabling the recovery of materials like aluminum and polyester, and facilitating the recycling of resin and absorbent articles.
Smart Images

Figure 0007580856000001 
Figure 0007580856000002 
Figure 0007580856000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a neutral stripper composition. [Background technology]
[0002] Many multi-layer resin molded products that combine different materials to meet the performance requirements of packaging materials are on the market. However, because multi-layer resin molded products are made of laminated films and metal foils with different properties, these materials are difficult to separate, which makes material recycling difficult. In addition, in reaction equipment such as a reaction vessel used in producing a monomer or resin, or a mold used in resin molding, gelled materials and resins adhere to the inside after use, and therefore it is necessary to periodically clean and remove them. Conventionally, when cleaning a reaction vessel, a person may have to enter the vessel and scrape off and remove unnecessary materials using a spatula or the like, which is a manual procedure that is cumbersome and dangerous. In addition, manual cleaning may not be sufficient, or a lot of time may be required for cleaning, and cleaning efficiency may not be high.
[0003] Conventionally, as a stripping agent, for example, a water-soluble paint stripping agent characterized by containing an alkali hydroxide, an aromatic alcohol, an alkanolamine, a glycol, and water has been proposed (Patent Document 1). However, such stripping agents are strongly alkaline and may cause decomposition, corrosion, dissolution, etc., depending on the material used, so their applications are limited.
[0004] On the other hand, for example, Patent Document 2 discloses a non-flammable cleaning agent composition for removing oily substances necessary for metal processing, electronic component processing, optical component processing, or the like, or oily substances adhered during such processing, which is characterized by comprising 10 to 84% by weight of 3-methoxy-3-methylbutanol as a first component and 90 to 16% by weight of water as a second component.
[0005] Furthermore, Patent Document 3 discloses a stripping agent for matting agents such as floor polish, which is adjusted to be neutral to alkaline and contains fatty acids, amines, solvents, and α-hydroxy acids as main components.
[0006] Patent Document 4 discloses a release agent composition for a resin wax coating layer, which comprises 85% to 98% by weight of at least one volatile solvent selected from propylene glycol monomethyl ether, propylene glycol monoethyl ether, and ethyl alcohol, 1% to 10% by weight of benzyl alcohol, and 1% to 5% by weight of amylcinnamic aldehyde.
[0007] Specifically, Patent Document 5 discloses an industrial cleaning agent composition for safely and effectively removing various different solid contaminants adhering to members having hard surfaces such as metals and glass materials, which is characterized by comprising (A) benzyl alcohol, (B) a specific water-soluble glycol ether, (C) a nonionic surfactant having an HLB value of 12 to 18, and (D) water, the total of which accounts for 100% by weight.
[0008] However, the above-mentioned prior art documents do not disclose the use of the above-mentioned cleaning agents, release agents, etc. for peeling the multilayer resin molded body into its individual layers. Furthermore, there is room for further improvement in peeling the multilayer resin molded body. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2002-275394 A [Patent Document 2] Japanese Patent Application Publication No. 6-346094 [Patent Document 3] JP 2005-28515 A [Patent Document 4] JP 2006-282976 A [Patent Document 5] JP 2020-8080 A Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention aims to provide a neutral release agent composition having excellent release performance for multilayer resin molded bodies, etc. Another object of the present invention is to provide a neutral release agent composition capable of preventing decomposition, corrosion, and dissolution of a substrate constituting a multilayer resin molded body, etc. [Means for solving the problem]
[0011] The present invention is a neutral release agent composition containing the following (A) to (F): (A) A polar solvent with an SP value of 9 to 12.4 (excluding those falling under (B) below). and at least one selected from the group consisting of benzyl alcohol, phenyl glycol, and phenethyl alcohol. (B) Amphiphilic glycol and / or glycol ether solvents (C) Salts of fatty acids having 12 to 18 carbon atoms (D) Paraffinic hydrocarbons (E) Alkanolamide type nonionic surfactants (F)Water
[0013] The amphiphilic glycol and / or glycol ether solvent (B) is preferably at least one selected from the group consisting of propylene glycol, ethylene glycol, diethylene glycol, propylene glycol monomethyl ether, and dipropylene glycol monomethyl ether.
[0014] The fatty acid salt (C) is preferably at least one selected from the group consisting of sodium laurate, sodium oleate, and sodium stearate. The paraffinic hydrocarbon (D) has a kinetic viscosity of 130 mm 2 It is preferable that the liquid paraffin used is one having a viscosity of 1 / s or less.
[0015] The present invention is also a method for recovering aluminum and / or polyester from a multilayer resin molded body having an aluminum layer and / or a polyester layer, which comprises the steps of applying the above-mentioned neutral release agent composition to a multilayer resin molded body having an aluminum layer and / or a polyester layer, and peeling and separating each layer.
[0016] The present invention is a method for treating used or unused absorbent articles that have, as at least constituent components, an absorbent body, a nonwoven fabric, and a film containing pulp and a superabsorbent polymer, and the method for treating used or unused absorbent articles includes a step of separating each constituent component using the above-mentioned neutral release agent composition and recovering the polyester material.
[0017] The present invention also relates to a method for cleaning a reaction vessel or a mold made of aluminum, in which the above-mentioned neutral release agent composition is used to remove a resin adhering to the reaction vessel or the mold. Effect of the Invention
[0018] The neutral release agent composition of the present invention has a neutral pH and has the same release performance as an alkaline agent. In addition, because it is neutral, it can prevent decomposition, corrosion, and dissolution of the substrate constituting the multilayer resin molded body or the like. By using the neutral release agent composition of the present invention, it becomes possible to recover base materials such as aluminum and polyethylene terephthalate (PET) when separating multilayer resin molded bodies or absorbent articles. In addition, it becomes possible to use the neutral release agent composition of the present invention on aluminum materials in reaction equipment such as reaction kettles and metal molds used in resin molding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The neutral release agent composition of the present invention contains the following (A) to (F): (A) Polar solvents with SP values between 9 and 13 (B) Amphiphilic glycol and / or glycol ether solvents (C) Salts of fatty acids having 12 to 18 carbon atoms (D) Paraffinic hydrocarbons (E) Alkanolamide type nonionic surfactants (F)Water In the present invention, "neutral" means that the stripping agent composition has a pH of 6.0 to 8.0 (hereinafter, sometimes referred to as neutral range).
[0020] Until now, strongly alkaline stripping agents have been used to peel off multilayer resin molded bodies having various resin layers, aluminum layers, adhesive layers, printed layers, etc., because adhesives and the like cannot be sufficiently peeled off with neutral or slightly alkaline agents. However, in the present invention, a release agent composition has been discovered that enables peeling of each layer of a multilayer resin molding in the neutral range by preparing an aqueous composition that contains a polar solvent (A) having a specific SP value, an amphiphilic glycol-based and / or glycol ether-based solvent (B), as well as a specific fatty acid salt (C), a paraffinic hydrocarbon (D), and an alkanolamide-type nonionic surfactant (E).
[0021] In particular, by blending a specific fatty acid salt (C) and a paraffinic hydrocarbon (D), it becomes possible to peel off each layer of the multilayer resin molded body in the neutral range. In the present invention, by using the fatty acid salt (C) and the paraffinic hydrocarbon (D) in combination, it is possible to sufficiently dissolve or remove the adhesive layer, the printed layer, and the like in the multilayer resin molded body.
[0022] Furthermore, in the present invention, by enabling peeling in the neutral range, when separating multilayer resin moldings, absorbent articles, etc., aluminum or resins such as polyethylene terephthalate (PET) and polycarbonate, which are vulnerable to alkali, are not decomposed, corroded, or dissolved, making it possible to recover these substrates. Furthermore, it will become possible to use the compound in aluminum materials in reaction equipment such as reaction vessels and in molds used for resin molding.
[0023] The polar solvent (A) used in the present invention must have an SP value of 9-13. The SP value (solubility parameter (δ)) is a value defined by the regular solution theory introduced by Hildebrand, and is 3 The square root of the heat of vaporization required to evaporate a liquid (cal / cm 3 ) 1 / 2 It is calculated from
[0024] In the present invention, by using a polar solvent having an SP value in this range, the adhesive layer and the printed layer can be removed without attacking the substrate such as a multilayer resin molded product. The SP value of the polar solvent used in the present invention is preferably 10 or more. On the other hand, the SP value is preferably 13 or less.
[0025] Specific examples of polar solvents (A) having the above SP value include benzyl alcohol (SP value: 10.8), phenyl glycol (SP value: 12.4), N-methyl-2-pyrrolidone (NMP) (SP value: 11.2), isopropanol (SP value: 11.5), dimethylformamide (DMF) (SP value: 11.9), dimethyl sulfoxide (DMSO) (SP value: 12.0), phenethyl alcohol (SP value: 11.2), etc. These may be used alone or in combination of two or more. Of these, benzyl alcohol, phenyl glycol, dimethyl sulfoxide (DMSO), phenethyl alcohol, and dimethylformamide (DMF) are preferred, and benzyl alcohol is particularly preferred.
[0026] The amphiphilic glycol and / or glycol ether solvent (B) used in the present invention functions as a compatibilizer between the polar solvent (A), fatty acid salt (C), and paraffinic hydrocarbon (D) and water (F). Therefore, it is necessary for the amphiphilic glycol and / or glycol ether solvent to have both a portion with high affinity for water (hydrophilic group) and a portion with low affinity for water (hydrophobic group).
[0027] Specific examples of the amphiphilic glycol and / or glycol ether solvent (B) used in the present invention include propylene glycol, diethylene glycol, ethylene glycol, polyethylene glycol, polypropylene glycol, 3-methoxy-3-methylbutanol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, etc. These may be used alone or in combination of two or more. Of these, propylene glycol, diethylene glycol, polyethylene glycol, propylene glycol monomethyl ether, and dipropylene glycol monomethyl ether are preferred.
[0028] Specific examples of the fatty acid salt (C) having 12 to 18 carbon atoms used in the present invention include sodium oleate, sodium stearate, sodium laurate, sodium myristate, sodium palmitate, sodium linoleate, sodium linolenate, potassium laurate, potassium myristate, potassium palmitate, potassium linoleate, potassium linolenate, potassium oleate, potassium stearate, etc. These may be used alone or in combination of two or more. Of these, sodium laurate, potassium laurate, sodium oleate, potassium oleate, sodium stearate, and potassium stearate are preferred.
[0029] The paraffinic hydrocarbon (D) used in the present invention is preferably a hydrocarbon represented by the general formula CnH2n+2 (n is an integer of 15 or more). Specifically, for example, liquid paraffin can be mentioned. By using a paraffin-based hydrocarbon (D) that is an oily liquid such as the above-mentioned liquid paraffin, a homogeneous state can be maintained when mixed as a solution. The liquid paraffin has a kinetic viscosity of 130 mm 2 It is preferable that the ratio is 1 / s or less. The above kinematic viscosity is a value measured at 40° C. using a glass capillary viscometer in accordance with JIS K2231-1993 and JIS K2283.
[0030] In the present invention, the incorporation of the alkanolamide type nonionic surfactant (E) improves the dispersibility of the components in the stripping composition, thereby contributing to the stripping performance. In particular, it is possible to provide dilution stability, uniformly disperse the components when diluted, and exhibit sufficient stripping performance.
[0031] The alkanolamide type nonionic surfactant (E) used in the present invention preferably has an HLB value of 5.0 to 16.0. In the present invention, HLB is a value defined by the following calculation formula according to the Griffin method. HLB value = 20 x [sum of chemical formula weights of hydrophilic parts] / molecular weight
[0032] Specific examples of the alkanolamide type nonionic surfactant (E) include coconut oil fatty acid monoethanolamide, coconut oil fatty acid diethanolamide, lauric acid monoethanolamide, lauric acid diethanolamide, lauric acid myristic acid monoethanolamide, lauric acid myristic acid diethanolamide, myristic acid monoethanolamide, myristic acid diethanolamide, palm kernel oil fatty acid monoethanolamide, palm kernel oil fatty acid diethanolamide, stearic acid monoethanolamide, stearic acid diethanolamide, isostearic acid monoethanolamide, isostearic acid diethanolamide, oleic acid monoethanolamide, oleic acid diethanolamide, polyoxyethylene (EO 2 to 5 moles) coconut oil fatty acid monoethanolamide, etc. These may be used alone or in combination of two or more. Among these, coconut oil fatty acid monoethanolamide (HLB 10.1), coconut oil fatty acid diethanolamide (HLB 15.5), lauric acid monoethanolamide (HLB 10.7), lauric acid diethanolamide (HLB 12.5), stearic acid monoethanolamide (HLB 7.5), stearic acid diethanolamide (HLB 9.1), oleic acid monoethanolamide (HLB 7.5), and oleic acid diethanolamide (HLB 9.1) are preferred.
[0033] The polar solvent (A) is preferably contained in the neutral release agent composition in an amount of 10 to 80% by mass. The lower limit of the content is more preferably 20% by mass, and even more preferably 30% by mass. On the other hand, the upper limit of the content is more preferably 70% by mass, and even more preferably 60% by mass. If the polar solvent (A) is within the above range, a homogeneous state can be maintained when mixed as a solution, and good peelability can be exhibited.
[0034] The neutral release agent composition preferably contains the component (B) in an amount of 1 to 50% by mass. The lower limit of the content is more preferably 3% by mass. On the other hand, the upper limit of the content is more preferably 40% by mass, and even more preferably 30% by mass. When the content of component (B) is within the above range, a homogeneous state can be maintained when components (A), (C), (D) and (F) are mixed as a solution.
[0035] The neutral release agent composition preferably contains the component (C) in an amount of 1 to 40% by mass. The lower limit of the content is more preferably 5% by mass. On the other hand, the upper limit of the content is more preferably 30% by mass, and even more preferably 20% by mass. If the amount of component (C) is within the above range, a homogeneous state can be maintained when mixed as a solution, and good peelability can be exhibited.
[0036] The neutral release agent composition preferably contains the component (D) in an amount of 1 to 30% by mass. The lower limit of the content is more preferably 1% by mass. On the other hand, the upper limit of the content is more preferably 20% by mass, and even more preferably 10% by mass. If the component (D) is within the above range, a homogeneous state can be maintained when mixed as a solution, and good peelability can be exhibited.
[0037] The content of the component (E) in the neutral release agent composition is preferably 5 to 30% by mass. When the component (E) is within the above range, the components (A), (C) and (D) can be solubilized, and the stripping composition can maintain its dilution stability with water.
[0038] The neutral stripper composition of the present invention is an aqueous solution. The content of water (F) in the neutral release agent composition is preferably 10% by mass or more, and more preferably 15% by mass or more. On the other hand, the upper limit is preferably 40% by mass, and more preferably 30% by mass. If the content of water (F) is within the above range, a homogeneous state can be maintained when mixed into a solution, and good peelability can be exhibited.
[0039] The neutral release agent composition of the present invention may be prepared by appropriately mixing and stirring the above-mentioned raw materials in a conventional manner.
[0040] The multilayer resin molding to which the neutral release agent composition of the present invention is applied is not particularly limited, and examples thereof include commonly used materials such as packaging materials such as packaging films and sheets, packaging containers, fuel tanks for gasoline, etc., hoses for transporting refrigerants, and optical materials. In particular, it can be suitably used for a multi-layer resin formed body having an aluminum layer and a polyester layer such as polyethylene terephthalate.
[0041] Examples of these multi-layered resin molded bodies include laminates formed by combining two or more types of resin layers, an aluminum layer, a pulp layer, and the like.
[0042] Examples of resin layers of the multilayer resin molding include unstretched polyethylene (PE) resin film, unstretched polypropylene (CPP) resin film, cyclic polyolefin (COP or COC) resin film, olefin-based films consisting of co-extruded films of unstretched polyethylene and unstretched polypropylene (PE / CPP), polyethylene terephthalate (PET) resin film, polyamide (PA) resin film, polyethylene naphthalate (PEN) resin film, polyacrylonitrile (PAN) resin film, polycarbonate (PC) resin film, polyimide (PI) resin film, polyvinyl chloride (PVC) resin film, etc. Any of these may be used in the present invention.
[0043] The multilayer resin molded product may be one in which each layer is bonded using an adhesive. Examples of the adhesive include commonly used polyurethane adhesive compositions, polyolefin adhesive compositions, etc. The adhesive layer formed by these adhesives is dissolved or removed by the release agent composition of the present invention, so that the multilayer resin molded product can be peeled off without any problems.
[0044] The multilayer resin molded product may have a printed layer. The printed layer is also dissolved or removed by the neutral release agent composition of the present invention, so that the multilayer resin molded product can be peeled off without any problems.
[0045] The printed layer is formed from printing ink, and suitable examples of the printing ink include screen ink, gravure ink, flexographic ink, inkjet ink, offset ink and other printing inks. Among these, the use of gravure ink, flexo ink, and inkjet ink is preferred, and the use of gravure ink and / or flexo ink is even more preferred.
[0046] The binder resin contained in the printing layer can be preferably exemplified by polyurethane resin, cellulose resin, polyamide resin, vinyl chloride resin such as vinyl chloride-vinyl acetate copolymer resin, vinyl chloride-acrylic copolymer resin, chlorinated polyolefin, ethylene-vinyl acetate copolymer, chlorinated ethylene-vinyl acetate copolymer, rosin resin, ethylene-vinyl acetate copolymer resin, vinyl acetate resin, acrylic resin, styrene resin, dammar resin, styrene-maleic acid copolymer resin, polyester resin, alkyd resin, terpene resin, phenol-modified terpene resin, ketone resin, cyclized rubber, chlorinated rubber, butyral, polyacetal resin, petroleum resin, and modified resins thereof. These resins can be used alone or in a mixture of two or more.
[0047] Among the above, it is preferable to contain at least one binder resin selected from the group consisting of polyurethane resin, vinyl chloride-vinyl acetate copolymer resin, polyamide resin, acrylic resin, polyester resin, rosin resin and cellulose resin.Moreover, it is preferable that the binder resin contains two types of resins consisting of a combination of polyurethane resin and vinyl chloride-vinyl acetate copolymer resin, polyamide resin and cellulose resin, or acrylic resin and cellulose resin, etc., in an amount of 50 mass% or more in the total mass of the binder resin, and it is even more preferable that the mass ratio of the former:latter is 95:5 to 30:70.
[0048] The printing layer preferably contains a colorant. The colorant is preferably a pigment, and examples of organic pigments include, but are not limited to, soluble azo, insoluble azo, azo, phthalocyanine, halogenated phthalocyanine, anthraquinone, anthanthrone, dianthraquinonyl, anthrapyrimidine, perylene, perinone, quinacridone, thioindigo, dioxazine, isoindolinone, quinophthalone, azomethine azo, flavanthrone, diketopyrrolopyrrole, isoindoline, indanthrone, and carbon black pigments. Other suitable examples include carmine 6B, lake red C, permanent red 2B, disazo yellow, pyrazolone orange, carmine FB, chromophthalic yellow, chromophthalic red, phthalocyanine blue, phthalocyanine green, dioxazine violet, quinacridone magenta, quinacridone red, indanthrone blue, pyrimidine yellow, thioindigo bordeaux, thioindigo magenta, perylene red, perinone orange, isoindolinone yellow, aniline black, diketopyrrolopyrrole red, daylight fluorescent pigments, etc. CI pigments listed in the Color Index can be used as appropriate.
[0049] The method for separating the multilayer resin molded article into each layer using the neutral release agent composition of the present invention may be carried out by a conventionally known method. For example, a method in which the multilayer resin molded article is immersed in the release agent composition for a desired period of time is suitable. The neutral stripping composition of the present invention may be further diluted with water before use.
[0050] The form of the multilayer resin molded article to be immersed may be set as desired, and the molded article may be used as is, or may be crushed or pulverized into small pieces or granules before being immersed.
[0051] The temperature of the solution during the peeling step may be room temperature, but is preferably 60 to 90° C. An autoclave or the like may also be used. During the peeling step, it is preferable to agitate or vibrate the solution in which the multilayer resin molded body is immersed.
[0052] The present invention is also a method for recovering aluminum and / or polyester from a multilayer resin molded body having an aluminum layer and / or a polyester layer, which comprises the steps of applying the above-mentioned neutral release agent composition to a multilayer resin molded body having an aluminum layer and / or a polyester layer, and peeling and separating each layer.
[0053] By using the neutral release agent composition of the present invention, the multilayer resin molding can be easily peeled and separated into each layer. In addition, since the decomposition, corrosion and dissolution of the aluminum layer and the polyester layer such as the polyethylene terephthalate layer can be prevented, these substrates can be recovered and reused.
[0054] Each of the separated layers may be recovered and dried using a dryer or the like.
[0055] The neutral release agent composition of the present invention can also be used in a method for treating used or unused absorbent articles that include, as at least one component, an absorbent body, nonwoven fabric, or film containing pulp and a highly absorbent polymer.
[0056] Examples of the absorbent article include paper diapers, urine pads, sanitary napkins, bed sheets, and pet sheets. A used absorbent article is an absorbent article that has been used by a user, and is usually an absorbent article that has absorbed liquid excrement from the user. However, in this embodiment, a used absorbent article includes an absorbent article that has been used but has not absorbed excrement. An unused absorbent article includes an absorbent article that has become defective during the manufacturing process at a factory.
[0057] The pulp contained in the absorbent body may be, for example, a cellulosic fiber, such as wood pulp, crosslinked pulp, non-wood pulp, regenerated cellulose, or semi-synthetic cellulose. In addition, examples of the superabsorbent polymer (SAP) contained in the absorbent body include water-absorbing polymers such as polyacrylates, polysulfonates, maleic anhydrides, etc. The superabsorbent polymer is usually in the form of particles dispersed in the pulp.
[0058] Examples of materials for the nonwoven fabric or film include olefin resins such as polyethylene and polypropylene, polyamide resins such as 6-nylon and 6,6-nylon, and polyester resins such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT).
[0059] As the nonwoven fabric and film, a liquid-permeable nonwoven fabric, a synthetic resin film having liquid-permeable holes, a composite sheet of these, or a liquid-impermeable nonwoven fabric, a liquid-impermeable synthetic resin film, a composite sheet of these nonwoven fabrics and synthetic resin films, etc. are used depending on the purpose.
[0060] An example of the configuration of the absorbent article is one that includes a top sheet, a back sheet, and an absorbent disposed between the top sheet and the back sheet. The top sheet and the back sheet are made of the nonwoven fabric or film.
[0061] In the above configuration example, for example, one side and the other side of the absorbent are respectively bonded to the top sheet and the back sheet via an adhesive. In a plan view, the portion (peripheral portion) of the top sheet that extends outside the absorbent so as to surround the absorbent is bonded to the portion (peripheral portion) of the back sheet that extends outside the absorbent so as to surround the absorbent. Therefore, the absorbent is enclosed inside the bonded body of the top sheet and the back sheet.
[0062] Examples of the adhesive include hot melt adhesives, etc. Examples of the hot melt adhesive include pressure-sensitive adhesives or heat-sensitive adhesives mainly made of rubber such as styrene-ethylene-butadiene-styrene, styrene-butadiene-styrene, and styrene-isoprene-styrene, or mainly made of olefin such as polyethylene.
[0063] In the present invention, the above-mentioned neutral release agent composition can be used to disassemble the above-mentioned used absorbent article into each component part. The neutral release agent composition dissolves or releases adhesives and the like used in the absorbent article. In addition, when polyester materials such as polyethylene terephthalate (PET) are used, these can be easily recovered.
[0064] In other words, the present invention is a method for treating used or unused absorbent articles that have, as at least constituent components, an absorbent body, a nonwoven fabric, and a film containing pulp and a superabsorbent polymer, and is also a method for treating used or unused absorbent articles that includes a step of separating each decomposed constituent component using the above-mentioned neutral release agent composition and recovering the polyester material.
[0065] The method for treating a used or unused absorbent article of the present invention includes, for example, a step (1) of applying the neutral release agent composition to the absorbent article and disassembling the absorbent article into each of the constituent members; Step (2) of separating and recovering each component part disassembled in step (1). The method includes the following steps:
[0066] In the above step (1), the method of applying the neutral release agent composition to the absorbent article is not particularly limited and may be appropriately performed. For example, the absorbent article is immersed in the neutral release agent composition by placing the absorbent article in a container or tank containing the neutral release agent composition. In this case, the immersion temperature is preferably 70 to 80° C. Within this temperature range, the adhesive can be removed without any problems. The immersion time is preferably 30 to 60 minutes. If necessary, the mixture may be stirred by rotating a propeller or the like.
[0067] In the above step (1), the adhesive bonding the components together is dissolved or removed by the neutral release agent composition, and the components are decomposed into components such as an absorbent, a nonwoven fabric, and a film. In this method, the adhesive at the bonding portion between the nonwoven fabric or film and other components (film, nonwoven fabric, absorbent, etc.) is removed by the neutral release agent composition, so the nonwoven fabric or film and other components can be decomposed into each other while maintaining their original shape without breaking or the like. Therefore, the components of the absorbent article, such as the nonwoven fabric and film, can be efficiently recovered. In addition, since the adhesive can be separated without leaving any adhesive on the film or nonwoven fabric, the nonwoven fabric or film can be reused as a high-purity resin, and the adverse effect of the adhesive when the nonwoven fabric or film is reused can be suppressed.
[0068] Next, in step (2), the decomposed components are separated and collected. The method of separation is not particularly limited. For example, each component is separated and collected from the mixed liquid obtained in step (1) by utilizing the buoyancy difference of the components, or by filtering using a nonwoven fabric, a sieve, or the like. In the treatment method of the present invention, the pulp and the superabsorbent polymer are not separated, but are separated and recovered as an integrated absorbent body. In step (2), washing with water may be carried out before or during the separation, or after recovery.
[0069] The nonwoven fabrics, films, etc. thus recovered may be dehydrated as necessary and dried by heating, that is, appropriately dried in an atmosphere or with hot air at a temperature higher than room temperature.
[0070] When carrying out the method of the present invention, a step of washing a used or unused absorbent article with water containing a detergent or the like may be carried out in advance, or the present method may also serve as a washing step.
[0071] The nonwoven fabric and film recovered in the above manner are suitable for recycling because they are free of adhesive.
[0072] The pulp and the superabsorbent polymer in the recovered absorbent body may be separated and recovered by any known method. The recovered pulp and the superabsorbent polymer may be reused.
[0073] The neutral stripping composition of the present invention is also effective for cleaning reaction equipment, molds, and the like. The reaction equipment to be washed includes equipment components such as reaction vessels made of metal, baffle plates, stirring blades, conduits, connecting jigs, etc. Furthermore, examples of the mold include metal molds used for molding resins and the like. In particular, in the case of a reaction apparatus or a mold made of aluminum, this is preferable since aluminum will not corrode or dissolve.
[0074] That is, the present invention also relates to a method for cleaning a reaction vessel or a mold made of aluminum, in which the above-mentioned neutral release agent composition is used to remove a resin adhering to the reaction vessel or the mold.
[0075] In the present invention, the unwanted materials such as resins to be cleaned are not particularly limited, and examples thereof include gelled materials generated during the production of monomers such as acrylic acid, isocyanate-based compounds, and epoxy-based compounds, residual resins such as acrylic resins, urethane-based resins, epoxy-based resins, and silicone resins, gelled materials derived from these resins, and silica.
[0076] Examples of substances that adhere to the inside of a reaction vessel include residual resins such as acrylic resins, urethane resins, and epoxy resins, gels derived from these resins, gels generated during the production of monomers such as acrylic acid, isocyanate compounds, and epoxy compounds, and silica. Examples of substances that adhere to or accumulate on equipment components include dirt derived from epoxy resins, dirt derived from isocyanate compounds, and dirt derived from silicone resins. Examples of substances that adhere to a mold include silicone resins and various rubbers.
[0077] In the present invention, it is possible to satisfactorily clean gelled substances such as carboxylic acids (or their origin) which have been difficult to remove using conventional aqueous or solvent-based cleaners. The present invention is particularly effective for cleaning acrylic resins, urethane resins, and the like.
[0078] The method for cleaning a reaction tool or a mold of the present invention may be carried out by a known method as appropriate. For example, the method includes the steps of: (1) applying the aqueous cleaner to unnecessary matters adhering to a reaction tool or a mold using the neutral stripping composition to swell and strip the unnecessary matters; Step (2) of removing the unnecessary material peeled off in step (1) The method includes the following steps:
[0079] The temperature of the neutral stripping composition during cleaning is preferably 60 to 100° C., more preferably 70 to 90° C. Depending on the state of adhesion of unwanted matter, room temperature may also be used.
[0080] The immersion time may be appropriately set depending on the type of unwanted matter and the degree of adhesion, and is preferably about 1 minute to 2 hours, and more preferably 30 minutes to 1 hour. During immersion, if a reaction vessel is used, it is preferable to generate a water current by rotating a propeller or the like to stir the inside of the vessel. This allows for faster cleaning.
[0081] As described above, by immersing the waste material in the neutral release agent composition of the present invention, the neutral release agent composition penetrates the waste material, causing the waste material to gradually swell and be peeled off from the reaction equipment or mold. EXAMPLES
[0082] The present invention will be specifically described below based on examples. Note that the present invention is not limited to the following examples. In the examples, "parts" and "%" refer to "parts by mass" and "% by mass" unless otherwise specified.
[0083] Example 1 Benzyl alcohol 35% by mass, propylene glycol 5% by mass, sodium oleate 10% by mass, liquid paraffin (dynamic viscosity 1.8 to 2.6 mm 2 A stripping agent composition containing 5 mass % of glycerin (HEXA-100 / s), 20 mass % of coconut oil fatty acid ethanolamide (HLB 15.5) and 25 mass % of water was prepared. The resulting stripping composition had a pH of 6.8. The peelability and solubilization properties were evaluated by the following methods.
[0084] (Multi-layer resin molding) In the peelability test, a multilayer resin molding having the following structure was used. Object to be peeled: Sake pack (Kuro Kirishima, Kirishima Shuzo Co., Ltd.) Composition: Polyethylene / adhesive layer / polyethylene terephthalate / adhesive layer / aluminum foil / adhesive layer / polyethylene / pulp / polyethylene / printed layer
[0085] (Peeling test) 1. The above multi-layer resin molding was cut into a size of approximately 20 x 20 mm. 2. The multilayer resin molded body was immersed in the release agent under normal pressure and heated to 80° C., and the release property and solubilization property were visually confirmed and evaluated according to the following criteria. The results are shown in Table 1. (peelability) ◯: All layers peeled off within 5 hours. △: All layers peeled off within 20 hours. ×: Partial peeling was observed after 48 hours, but was insufficient.
[0086] (Solubilization) ◯: The stripping composition was transparent. Δ: The stripping agent composition was cloudy and separated within 72 hours. ×: The stripping composition was cloudy and quickly separated.
[0087] [Examples 2 to 6] Each test was carried out in the same manner as in Example 1, except that the composition of the stripping agent composition was as shown in Table 1. The results are also shown in Table 1.
[0088] [Comparative Examples 1 to 8] Each test was carried out in the same manner as in Example 1, except that the composition of the stripping agent composition was as shown in Table 2. The results are also shown in Table 2.
[0089] [Table 1]
[0090] [Table 2]
[0091] From the results in Tables 1 and 2, the release agent compositions of the Examples were excellent in releasing the multilayer resin molded article, whereas the compositions of the Comparative Examples did not provide satisfactory results. In the examples, the adhesive layers of the multilayer resin molded body dissolved and each of the base layers laminated with the adhesive layer peeled off. In addition, the ink of the printed layer was also detached from the polyethylene film. In the laminated portion of the polyethylene film and the pulp, the polyethylene film that had been adhered in a state where it was partially embedded in the pulp was separated from the pulp by the action of the moisture and oil of the release agent composition, and both were completely peeled off. Furthermore, the polyethylene terephthalate and the aluminum foil in the multi-layered resin molding could be recovered without decomposition, corrosion, dissolution, or the like.
[0092] <Hot melt adhesive removal test> A commercially available paper diaper (Relief (registered trademark) manufactured by Kao) was cut to a size of 5 cm x 5 cm and immersed in 50 g of release agent at a temperature of 80°C for 30 minutes, and then the following evaluations were carried out. ◯: The hot melt adhesive was completely removed within 30 minutes, and there was no stickiness on the surface of the component. Δ: The hot melt adhesive was completely removed within 1 hour, and there was no stickiness on the surface of the component. ×: The disposable diaper was decomposed into its constituent parts within 1 hour, but the surfaces of the constituent parts were very sticky, or the disposable diaper was not decomposed.
[0093] [Examples 7 to 12] The release agent compositions were prepared in the same manner as in Example 1, except that the compositions of the release agent compositions were as shown in Table 3, and the above-mentioned hot melt adhesive removal test was carried out. The results are also shown in Table 3.
[0094] [Comparative Examples 9 to 16] The release agent compositions were prepared in the same manner as in Example 1, except that the compositions of the release agent compositions were as shown in Table 4, and the above-mentioned hot melt adhesive removal test was carried out. The results are also shown in Table 4.
[0095] [Table 3]
[0096] [Table 4]
[0097] From the results in Tables 3 and 4, the release agent compositions of the Examples were excellent in hot melt adhesive removal properties, whereas the compositions of the Comparative Examples did not provide satisfactory results.
[0098] <Mold cleaning test> (Peel test) 0.1 g of acrylic resin was applied to a 1.30 x 50 mm stainless steel plate (JISG4305 SUS304) and baked at 800°C for 20 minutes to prepare a test piece. 2. After heating 120 g of the stripping cleaner to 80°C, the test piece (1) was immersed in it and the state of peeling was confirmed. 〇: 100% peeling within 2 hours △: 100% peeled off within 5 hours ×: No peeling even after 5 hours
[0099] [Examples 13 to 18] The release agent compositions were prepared in the same manner as in Example 1, except that the compositions of the release agent compositions were as shown in Table 5, and the above-mentioned release test was carried out. The results are also shown in Table 5.
[0100] [Comparative Examples 17 to 24] The release agent compositions were prepared in the same manner as in Example 1, except that the compositions of the release agent compositions were as shown in Table 6, and the above-mentioned release test was carried out. The results are also shown in Table 6.
[0101] [Table 5]
[0102] [Table 6]
[0103] From the results in Tables 5 and 6, the release agent compositions of the Examples were excellent in the release properties for acrylic resins, whereas the compositions of the Comparative Examples did not provide satisfactory results. [Industrial Applicability]
[0104] The present invention enables a multi-layered resin molded product, etc. to be peeled into each layer. It also enables all resin layers and aluminum layers to be recovered, which is useful for protecting the global environment.
Claims
1. A neutral release agent composition comprising the following (A) to (F): (A) A polar solvent having an SP value of 9 to 12.4 (excluding those falling under (B) below), which is at least one selected from the group consisting of benzyl alcohol, phenyl glycol, and phenethyl alcohol. (B) Amphiphilic glycol and / or glycol ether solvents (C) Salt of fatty acid having 12 to 18 carbon atoms (D) Paraffinic hydrocarbons (E) Alkanolamide type nonionic surfactant (F) Water
2. 2. The neutral stripping agent composition according to claim 1, wherein the amphiphilic glycol and / or glycol ether solvent (B) is at least one selected from the group consisting of propylene glycol, ethylene glycol, diethylene glycol, propylene glycol monomethyl ether, and dipropylene glycol monomethyl ether.
3. 3. The neutral stripping agent composition according to claim 1, wherein the fatty acid salt (C) is at least one selected from the group consisting of sodium laurate, sodium oleate and sodium stearate.
4. The paraffinic hydrocarbon (D) has a kinetic viscosity of 130 mm 2 The neutral stripping composition according to any one of claims 1 to 3, which is liquid paraffin having a viscosity of 1 / s or less.
5. A method for recovering aluminum and / or polyester from a multilayer resin molded article having an aluminum layer and / or a polyester layer, comprising the steps of applying the neutral release agent composition according to any one of claims 1 to 4 to a multilayer resin molded article having an aluminum layer and / or a polyester layer, and peeling and separating each layer.
6. A method for treating a used or unused absorbent article comprising, as at least components, an absorbent body, a nonwoven fabric, and a film, each of which contains pulp and a highly absorbent polymer, the method comprising the steps of separating the components and recovering a polyester material using the neutral stripping agent composition according to any one of claims 1 to 4.
7. A method for cleaning a reaction vessel or a mold, comprising removing a resin adhering to an aluminum reaction vessel or a mold by using the neutral release agent composition according to any one of claims 1 to 4.
Citation Information
Patent Citations
Non-flammable cleanser composition
JP1994346094A
Coating film releasing agent composition
JP1999021482A
Aqueous coating-removing agent
JP2002275394A
Jig board
JP2005028515A
Releaser composition for resin wax film layer and method for releasing the same
JP2006282976A