Electrode group for secondary battery
By curving electrodes in a controlled negative direction and maintaining a specific curvature range, the design addresses distortion issues, enhancing the production efficiency and yield of electrode groups.
Patent Information
- Application Number
- JP2021043266
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-03-17
AI Technical Summary
The production of electrodes for secondary batteries is hindered by distortion and warpage due to residual stress at the boundary between coated and uncoated areas of the current collector, leading to misalignment and reduced yield in electrode groups.
The electrodes are designed with a specific curvature range (-1 mm to 0 mm) by adjusting the active material-containing layer and current collector structure, ensuring the uncoated area is stretched in the opposite direction to the pressing-induced curvature, maintaining a negative curvature.
This design stabilizes the electrodes over time, reducing misalignment and increasing the yield of electrode group production.
Smart Images

Figure 0007581094000008 
Figure 0007581094000009 
Figure 0007581094000010
Abstract
Description
[Technical field]
[0001] SUMMARY OF THE DISCLOSURE An embodiment of the present invention relates to an electrode. [Background technology]
[0002] In addition to conventional applications in small electronic devices, secondary batteries are now being used as power sources for vehicles such as hybrid electric vehicles, and so there is a demand for secondary batteries that combine high capacity, long cycle life, rapid charging, etc. In order to pack as much active material as possible into the limited battery space, electrodes have also become more densely compressed.
[0003] In the manufacture of electrodes, an electrode composite material containing an active material is applied to a substrate made of a strip-shaped current collector such as a metal foil, the coating is dried to form a composite layer, and then the composite layer is compressed using a roll press device or the like. The compressed coated area of the current collector also stretches due to plastic deformation, but the non-coated area of the current collector where the electrode composite material is not applied is not subjected to press pressure, so the exposed part of the current collector does not stretch. As a result, residual stress acts on the boundary between the coated area and the non-coated area due to the difference in the elongation of the current collector, causing distortion and warping of the electrode. When an electrode group is produced using an electrode, for example, when a laminate including a positive electrode and a negative electrode is wound to produce an electrode group having a wound structure, problems such as electrode misalignment occur due to the distortion and warping of the electrode. Even in the case of an electrode group that does not have a wound structure, for example, an electrode group having a laminated structure (so-called stack-type electrode group), there is a problem that the positions of the composite layers are likely to be inconsistent between the facing positive and negative electrodes. Therefore, if the electrodes are distorted, there is a problem that the production efficiency and yield during the manufacture of the electrode group are reduced.
[0004] As a manufacturing method aimed at improving the yield of electrode assembly production, for example, a method is known in which tension is applied to an uncoated portion of an electrode after pressing to stretch it and reduce the amount of curvature of the electrode. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-76711 A [Patent Document 2] JP 2012-174434 A [Patent Document 3] JP 2013-73690 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide an electrode that increases the production yield of an electrode group. [Means for solving the problem]
[0007] According to the embodiment, a positive electrode and a negative electrode , separator and An electrode group for a secondary battery is provided, comprising: The positive electrode comprises a positive electrode active material-containing layer and a positive electrode current collector. The positive electrode active material-containing layer includes a positive electrode first end having an arc shape and a positive electrode second end opposite to the positive electrode first end, and contains a positive electrode active material. The positive electrode current collector includes a positive electrode active material-supporting portion supporting the positive electrode active material-containing layer, and a positive electrode active material-free portion adjacent to the positive electrode active material-supporting portion and the positive electrode second end and not provided with the positive electrode active material-containing layer. The amount of positive electrode curvature, which is expressed as the maximum distance from the positive electrode first end to a reference line connecting two points on the positive electrode first end that are 1000 mm apart in a straight line, is in the range of -1 mm or more and less than 0 mm. The negative electrode comprises a negative electrode active material-containing layer and a negative electrode current collector. The negative electrode active material-containing layer includes a negative electrode first end and a negative electrode second end opposite to the negative electrode first end, and contains a negative electrode active material. The negative electrode current collector includes a negative electrode active material-supporting portion supporting the negative electrode active material-containing layer, and a negative electrode active material-free portion adjacent to the negative electrode active material-supporting portion and the negative electrode second end and not provided with the negative electrode active material-containing layer. The negative electrode curvature amount, which is expressed as the maximum distance from the negative electrode first end to a reference line connecting two points on the negative electrode first end that are 1000 mm apart in a straight line, is in the range of -1 mm or more and less than 0 mm, and the negative electrode first end has an arc shape, or the negative electrode curvature amount is 0 mm. The electrode group is a wound electrode group in which a positive electrode and a negative electrode are wound in a spiral shape with a separator interposed between them, or a stacked electrode group in which a positive electrode and a negative electrode are stacked with a separator interposed between them. According to another embodiment, a positive electrode and a negative electrode , separator and An electrode group for a secondary battery is provided, comprising: The negative electrode includes a negative electrode active material-containing layer and a negative electrode current collector. The negative electrode active material-containing layer includes a negative electrode first end having an arc shape and a negative electrode second end opposite to the negative electrode first end, and contains a negative electrode active material. The negative electrode current collector includes a negative electrode active material-supporting portion supporting the negative electrode active material-containing layer, and a negative electrode active material-free portion adjacent to the negative electrode active material-supporting portion and the negative electrode second end and not provided with the negative electrode active material-containing layer. The amount of negative electrode curvature, which is expressed as the maximum distance from the negative electrode first end to a reference line connecting two points on the negative electrode first end that are 1000 mm apart in a straight line, is within a range of -1 mm or more and less than 0 mm. The positive electrode comprises a positive electrode active material-containing layer and a positive electrode current collector. The positive electrode active material-containing layer includes a positive electrode first end and a positive electrode second end opposite to the positive electrode first end, and contains a positive electrode active material. The positive electrode current collector includes a positive electrode active material-supporting portion that supports the positive electrode active material-containing layer, and a positive electrode active material-free portion that is adjacent to the positive electrode active material-supporting portion and the positive electrode second end and does not have the positive electrode active material-containing layer. The positive electrode curvature amount, which is expressed as the maximum distance from the positive electrode first end to a reference line connecting two points on the positive electrode first end that are 1000 mm apart in a straight line, is in the range of -1 mm or more and less than 0 mm, and the positive electrode first end has an arc shape, or the positive electrode curvature amount is 0 mm. The electrode group is a wound electrode group in which a positive electrode and a negative electrode are wound in a spiral shape with a separator interposed between them, or a stacked electrode group in which a positive electrode and a negative electrode are stacked with a separator interposed between them. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a plan view illustrating an example of an electrode according to the embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 1 is a plan view illustrating an example of a conventional electrode. [Figure 4] FIG. 4 is a perspective view illustrating an electrode group. [Diagram 5] FIG. 2 is an explanatory diagram illustrating a schematic diagram of a drawing device used in manufacturing an electrode according to an embodiment. [Figure 6] 6 is an explanatory diagram showing the positional relationship between guide rollers and electrodes in the stretching device shown in FIG. 5. [Figure 7] FIG. 7 is a schematic cross-sectional view taken along line VII-VII in FIG. [Figure 8] FIG. 8 is a schematic cross-sectional view taken along line VIII-VIII in FIG. 6 . [Figure 9] FIG. 11 is a cross-sectional view illustrating a guide roller according to a modified example. [Figure 10] FIG. 11 is a cross-sectional view showing a guide roller according to another modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present inventors have found through extensive research that even if correction is performed to reduce the curvature caused by roll pressing, such as a tension application process, during electrode production, the amount of curvature increases again over time. Even if the degree of curvature of an electrode is kept small immediately after correction, after a certain period of time the amount of curvature of the electrode may increase to a level that causes problems such as misalignment during winding during the production of an electrode group. In other words, even if a curved electrode is corrected to a sufficiently small amount of curvature, the amount of curvature increases over time, resulting in a problem that the yield during the production of an electrode group may decrease.
[0010] Hereinafter, the embodiments will be described with reference to the drawings as appropriate. Note that the same reference numerals are used to designate common components throughout the embodiments, and duplicated descriptions will be omitted. Also, each figure is a schematic diagram for explaining the embodiments and for facilitating understanding thereof, and the shapes, dimensions, ratios, etc. may differ from those of the actual device, but these can be appropriately modified in design by taking into consideration the following explanation and known techniques.
[0011] <Electrode configuration> The electrode according to the embodiment includes an active material-containing layer that contains an electrode active material, and a current collector. The active material-containing layer includes a first end and a second end that have an arc shape. The second end is on the opposite side of the active material-containing layer to the first end. The current collector includes an active material-supporting portion and an active material-non-supporting portion. The active material-supporting portion supports the active material-containing layer. The active material-non-supporting portion is adjacent to the active material-supporting portion and the second end. The active material-non-supporting portion is not provided with the active material-containing layer. When the amount of curvature of the electrode is defined as a positive value in the direction from the first end to the second end, and is expressed as the maximum distance from the first end to a reference line that connects two points on the first end that are 1000 mm apart in a straight line, the amount of curvature is within a range of -1 mm or more and less than 0 mm.
[0012] During the press process in the manufacture of the electrode, the active material-supporting portion (coated region) of the current collector on which the active material-containing layer (composite layer) is provided extends due to plastic deformation, but the active material-unsupporting portion (uncoated region) does not extend, so the electrode deforms so that the side on which the active material-unsupporting portion is located is on the inside of the curve. In other words, in the deformation caused by the press process, the electrode warps toward the active material-unsupporting portion. Here, such a curve is considered to be a curve in the positive direction.
[0013] The electrode according to the embodiment is warped in the opposite direction from the active material non-supporting portion side so that the side of the current collector where the active material non-supporting portion is located is the outer side of the curvature. Here, such curvature is considered to be a negative curvature. In other words, such an electrode is curved in the opposite direction to the curvature caused by the press treatment. Since the amount of curvature in such an electrode is a negative value, even if the amount of curvature increases, the amount of curvature after the change with time is small, and the electrode group can be manufactured with a high yield using the electrode.
[0014] The electrode will be described with reference to the drawings, in which Fig. 1 is a plan view showing an example of an electrode according to an embodiment, and Fig. 2 is a schematic cross-sectional view taken along line II-II in Fig. 1.
[0015] The electrode 1 includes an active material-containing layer 2 and a current collector 3. The electrode 1 as a whole has a shape in which the current collector is in the shape of a band having a pair of long sides and the active material-containing layer provided on the current collector is curved within a plane parallel to the band shape.
[0016] The active material-containing layer 2 includes a first end 2a having an arc shape that is along the inner edge of the curved electrode 1, and a second end 2b that is located on the opposite side of the active material-containing layer 2 to the first end 2a. The second end 2b may correspond to the outer edge of the active material-containing layer 2 having an arc shape.
[0017] The active material-containing layer 2 is supported on a main surface of a current collector 3 having a belt-like shape describing an arc. In the illustrated example, the active material-containing layer 2 is provided on both the front and back main surfaces of the current collector 3, but the active material-containing layer 2 may be provided on only one main surface of the current collector 3. Alternatively, the active material-containing layer 2 may be provided on both sides of a portion of the current collector 3 extending in the long side direction, and the active material-containing layer 2 may be provided on only one side of the other portion.
[0018] The current collector 3 includes an active material-supporting portion 3a supporting the active material-containing layer 2, and an active material-non-supporting portion 3b on which no active material-containing layer is provided. When the current collector 3 is divided in a plane parallel to its main surface, the portion corresponding to the region on which the active material-containing layer 2 is provided on one or both of the main surfaces corresponds to the active material-supporting portion 3a, and the portion corresponding to the region on which the active material-containing layer 2 is not provided on either of the main surfaces corresponds to the active material-non-supporting portion 3b. In other words, in an electrode or part of an electrode in which the active material-containing layer 2 is provided only on one main surface of the current collector 3, the active material-containing layer is not supported over the entirety of the other main surface, but the region on the back side on which the active material-containing layer 2 is supported is regarded as the active material-supporting portion 3a.
[0019] The active material non-supporting portion 3b of the current collector 3 is adjacent to the active material supporting portion 3a and the second end portion 2b. The active material non-supporting portion 3b is along the outer long side of the arc of the current collector 3. The active material non-supporting portion 3b can function as an electrode current collecting tab. The active material non-supporting portion 3b of the current collector 3 may be referred to as a tab portion. The active material non-supporting portion 3b may be simply called a non-supporting portion. The end of the active material non-supporting portion 3b, that is, the end of the outer edge side of the current collector 3 on the opposite side of the active material non-supporting portion 3b with respect to the active material supporting portion 3a, may be conveniently called the third end portion 3c. The active material supporting portion 3a may also be simply called a supporting portion.
[0020] In the electrode 1 of the illustrated example, the edge (inner edge) of the active material-containing layer 2 and the edge (inner edge) of the current collector 3 are aligned at the first end 2a side of the active material-containing layer 2, but the positions of these edges may be slightly shifted. Even at the first end 2a side, both main surfaces of the current collector 3 may not support the active material-containing layer. In such a case, the widths in the first direction 101 along the shortest distance connecting the ends of both sides of each portion that does not support the active material-containing layer on both sides of the current collector 3 at both ends across the main surface of the current collector 3 are compared, and the wider portion is determined to be the active material-free portion 3b that can function as a current collecting tab. The end of the active material-containing layer 2 adjacent thereto is determined to be the second end 2b. In this way, the positional relationship between the first end 2a, the second end 2b, and the third end 3c can be grasped. These ends are arranged in the order of first end 2a, second end 2b, and third end 3c along a first direction 101 from the opposite side of electrode 1 relative to active material non-supporting portion 3b at any position along the longitudinal direction of electrode 1.
[0021] The amount of curvature of the electrode 1 can be confirmed as follows. Based on the arrangement of the active material non-supporting portion 3b of the current collector 3 and the active material-containing layer 2 (and the active material supporting portion 3a thereunder), the first end 2a and the second end 2b of the active material-containing layer 2 are specified as described above. The straight line connecting the points P1 and P2 on the first end 2a is set as the reference line L. The points P1 and P2 are set so that the distance D of the straight line connecting these points is constant. For example, the straight line distance D between the points P1 and P2 is set to 1000 mm. The amount of curvature is represented by the maximum distance M from the first end 2a to the reference line L between the points P1 and P2. Here, the direction from the first end 2a to the second end 2b is taken as a positive value. In other words, the amount of curvature is taken as a positive value in the direction toward the active material non-supporting portion 3b of the current collector 3 along the short side direction of the electrode 1. Alternatively, the position of the first end 2a is set to zero, and the direction from there along the short side width of the electrode main surface into the electrode plane is the positive direction, and the direction protruding from the electrode plane is the negative direction.
[0022] In this electrode, when the linear distance D is set to 1000 mm, the amount of curvature is a negative value within a range of -1 mm or more and less than 0 mm. In other words, the position of the reference line L connecting the points P1 and P2 is outside the first end 2a. Therefore, the electrode 1 is curved such that the first end 2a forms the inner edge of the arc shape and the third end 3c forms the outer edge of the arc shape.
[0023] The electrode according to the embodiment is curved in the opposite direction to the curvature of a conventional electrode, as will be described in comparison with an example of a conventional electrode shown in FIG.
[0024] Fig. 3 is a plan view showing a schematic example of a conventional electrode. The electrode 1 shown in the figure includes an active material-containing layer 2 and a current collector 3. The electrode 1 as a whole has a shape in which the current collector in a band shape having a pair of long sides and the active material-containing layer provided on the current collector are curved in a plane parallel to the band shape. However, the electrode 1 in Fig. 3 is curved in the opposite direction to that in Fig. 1.
[0025] For example, the active material-containing layer 2 is subjected to a rolling process in order to adjust the density of the active material-containing layer 2. In the rolling process by roll press using a general cylindrical roller having a constant diameter along its length, the roller does not come into contact with the non-active material-supporting portion 3b of the current collector 3 that does not support the active material-containing layer 2. Therefore, although the support portion of the current collector 3 is rolled, the non-active material-supporting portion 3b is not rolled. Although the support portion of the current collector 3 is widely stretched by rolling, the non-active material-supporting portion 3b is hardly deformed. As a result, the electrode 1 is curved in an arc shape so that the third end 3c side along which the non-active material-supporting portion 3b is aligned becomes the inner edge and the first end 2a side of the active material-containing layer 2 becomes the outer edge.
[0026] As shown in the figure, in the conventional electrode 1, a reference line L connecting points P1 and P2 on the first end 2a is located inside the first end 2a of the electrode 1. Therefore, the above-mentioned curvature amount has a positive value. The conventional electrode (FIG. 3) is curved in the positive direction, whereas the electrode according to the embodiment (FIG. 1) is curved in the negative direction.
[0027] The production of an electrode group using an electrode curved in the positive direction as shown in Fig. 3 results in low production efficiency and low yield. The present inventors have newly discovered that even if the amount of curvature of an electrode is reduced to zero or nearly zero by straightening the electrode, the electrode may be curved in the positive direction again over time. In other words, an electrode that has been straightened to eliminate distortion and warping may return to a state curved in the positive direction as shown in Fig. 3 as a result of changes over time.
[0028] The electrodes according to the embodiment are in a state of being pre-curved in the negative direction, and even if the electrodes undergo a change over time toward a positive direction, the amount of curvature remains small. Therefore, the manufacturing yield of an electrode group using such electrodes can be increased.
[0029] The width of the active material-containing layer can be, for example, 60 mm or more and 250 mm or less. The width of the active material-containing layer here corresponds to the distance between the first end and the second end. The width of the active material-containing layer corresponds to the width of the active material-supporting portion of the current collector.
[0030] The width of the current collector occupied by the non-active material carrying portion can be, for example, 5 mm to 25 mm, inclusive. The width of the non-active material carrying portion referred to here is the width in the direction intersecting with the second end portion of the active material-containing layer.
[0031] The mass per unit area of the active material-containing layer provided on the active material-supporting portion of the current collector is, for example, 100 g / m2 on each side of the current collector. 2 More than 300g / m 2 It can be the following:
[0032] Such an electrode may be a battery electrode. The battery electrode may be, for example, a positive electrode or a negative electrode for a secondary battery. The secondary battery referred to here includes, for example, a lithium ion secondary battery and a non-aqueous electrolyte battery.
[0033] The active material-containing layer has a density of, for example, 1.8 g / cm 3 More than 3.7g / cm 3 In the case of a positive electrode, the active material-containing layer (positive electrode active material-containing layer) may have a density of 2.7 g / cm 3may have a density of 3.7 g / cm or less. In the case of the negative electrode, the active material-containing layer (negative electrode active material-containing layer) may have a density of 1.8 g / cm or more and 2.9 g / cm or less. This density is the density of only the active material-containing layer excluding the current collector. 3 The electrode active material contained in the active material-containing layer includes a positive electrode active material or a negative electrode active material. Typically, the active material-containing layer (positive electrode active material-containing layer) of the electrode as the positive electrode includes a positive electrode active material as the electrode active material, and the active material-containing layer (negative electrode active material-containing layer) of the electrode as the negative electrode includes a negative electrode active material as the electrode active material. 3 The positive electrode may contain, as the positive electrode active material, one type of compound alone or a combination of two or more types of compounds. Similarly, the negative electrode may contain, as the negative electrode active material, one type of compound alone or a combination of two or more types of compounds. 3 As the positive electrode active material, for example, an oxide or a sulfide can be used. Examples of the oxide and the sulfide include compounds into which Li or Li ions can be inserted and desorbed.
[0034] Such compounds include, for example, manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (e.g., Li
[0035] Mn2O4 or Li
[0036] MnO2; 0 < x ≤ 1), lithium nickel composite oxide (e.g., Li
[0037] NiO2; 0 < x ≤ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≤ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni x Co x O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese cobalt composite oxide (e.g., Li x Mn 1-y Co y Mn x Co y O2; 0 < x ≤ 1, 0 < y < 1), etc. 1-yO2; 0 < x ≤ 1, 0 < y < 1), a lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), a lithium phosphate having an olivine structure (e.g., Li x FePO4; 0 < x ≤ 1, Li x Fe 1-y Mn y PO4; 0 < x ≤ 1, 0 < y ≤ 1, Li x CoPO4; 0 < x ≤ 1), iron sulfate (Fe2(SO4)3), vanadium oxide (e.g., V2O5), and a lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included.
[0038] Among the above, examples of more preferable compounds as the positive electrode active material include a lithium manganese composite oxide having a spinel structure (e.g., Li x Mn2O4; 0 < x ≤ 1), a lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≤ 1), a lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≤ 1), a lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≤ 1, 0 < y < 1), a lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), a lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≤ 1, 0 < y < 1), lithium iron phosphate (e.g., Li x FePO4; 0 < x ≤ 1), and a lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn zO2; where 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, and y + z < 1 is included. When these compounds are used as the positive electrode active material, the positive electrode potential can be increased.
[0039] When a room temperature molten salt is used as the electrolyte of the battery, it is preferable to use a positive electrode active material containing lithium iron phosphate, Li x VPO4F (0 ≤ x ≤ 1), a lithium manganese composite oxide, a lithium nickel composite oxide, a lithium nickel cobalt composite oxide, or a mixture thereof. Since these compounds have low reactivity with the room temperature molten salt, the cycle life can be improved.
[0040] A room temperature molten salt (ionic melt) refers to a compound that can exist as a liquid at room temperature (15°C or higher and 25°C or lower) among organic salts composed of a combination of an organic cation and an anion. Room temperature molten salts include those that exist as a liquid alone, those that become liquid when mixed with an electrolyte salt, those that become liquid when dissolved in an organic solvent, or mixtures thereof. Generally, the melting point of the room temperature molten salt used in a secondary battery is 25°C or lower. Also, the organic cation generally has a quaternary ammonium skeleton.
[0041] Examples of the negative electrode active material include lithium titanate having a ramsdellite structure (e.g., Li 2+x Ti3O7, 0 ≤ x ≤ 3), lithium titanate having a spinel structure (e.g., Li 4+x Ti5O 12 , 0 ≤ x ≤ 3), monoclinic titanium dioxide (TiO2), anatase-type titanium dioxide, rutile-type titanium dioxide, hollandite-type titanium composite oxide, orthorhombic titanium composite oxide, and monoclinic niobium titanium composite oxide.
[0042] Examples of the above orthorhombic titanium-containing composite oxide include Li 2+a M1 2-b Ti 6-c M2 d O 14+σHere, M1 is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb, and K. M2 is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na2Ti6O 14 (0≦a≦6).
[0043] As an example of the monoclinic niobium titanium composite oxide, Li x Ti 1-y M3 y Nb 2-z M4 z O 7+δ Here, M3 is at least one selected from the group consisting of Zr, Si, and Sn. M4 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium composite oxides include Li x Examples include Nb2TiO7 (0≦x≦5).
[0044] Another example of monoclinic niobium titanium composite oxide is Li x Ti 1-y M5 y+z Nb 2-z O 7-δ Here, M5 is at least one selected from the group consisting of Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦x<5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3.
[0045] The active material-containing layer may optionally contain a conductive agent and a binder in addition to the electrode active material.
[0046] The conductive agent is blended to improve the current collecting performance and to suppress the contact resistance between the electrode active material and the current collector. Examples of the conductive agent include carbonaceous materials such as vapor grown carbon fiber (VGCF), carbon black such as acetylene black, graphite, carbon nanotubes and carbon nanofibers. One of these may be used as the conductive agent, or two or more may be used in combination as the conductive agent. The conductive agent may be omitted. Alternatively, instead of using the conductive agent, a carbon coat or an electronically conductive inorganic material coat may be applied to the surface of the active material particles. The current collecting performance of the active material-containing layer may be improved by using the conductive agent and coating the active material surface with carbon or a conductive material.
[0047] The binder is blended to fill the gaps between the dispersed active materials and to bind the electrode active material and the current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene butadiene rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0048] The blending ratio of the electrode active material, conductive agent and binder in the active material-containing layer can be appropriately changed depending on the application of the electrode.
[0049] For example, when the electrode is used as a positive electrode of a secondary battery, the active material (positive electrode active material) and the binder are preferably mixed in proportions of 80% by mass or more and 99% by mass or less and 1% by mass or more and 20% by mass or less, respectively. By making the amount of the binder 1% by mass or more, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, by making the amount of the binder 20% by mass or less, the amount of the insulator contained in the electrode is reduced, and the internal resistance can be reduced.
[0050] When a conductive agent is added, the active material (positive electrode active material), the binder, and the conductive agent are preferably mixed in proportions of 77% by mass or more and 97% by mass or less, 1% by mass or more and 20% by mass or less, and 2% by mass or more and 15% by mass or less, respectively. By making the amount of the conductive agent 2% by mass or more, the above-mentioned effects can be achieved. Furthermore, by making the amount of the conductive agent 15% by mass or less, the proportion of the conductive agent in contact with the electrolyte can be reduced. If this proportion is low, the decomposition of the electrolyte can be reduced during high-temperature storage.
[0051] For example, when the electrode is used as the negative electrode of a secondary battery, it is preferable to mix the active material (negative electrode active material), conductive agent, and binder in proportions of 68% by mass or more and 97% by mass or less, 2% by mass or more and 30% by mass or less, and 1% by mass or more and 30% by mass or less, respectively. By making the amount of conductive agent 2% by mass or more, the current collection performance of the active material-containing layer can be improved. Also, by making the amount of binder 2% by mass or more, the binding between the active material-containing layer and the current collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, it is preferable to make the conductive agent and binder 30% by mass or less each in order to increase capacity.
[0052] When the surface of the active material is coated with carbon or a conductive material, the amount of the coating material can be considered to be included in the amount of conductive material. The amount of carbon or conductive material coated is preferably 0.5% by mass or more and 5% by mass or less. If the amount of coating is within this range, the current collection performance and electrode density can be improved.
[0053] For the current collector, a material that is electrochemically stable at a potential at which lithium (Li) is inserted into and extracted from the electrode active material is used.
[0054] For example, in the case of an electrode used as a positive electrode, the current collector (positive electrode current collector) is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from the group consisting of Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu and Si. The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99% by mass or more. The content of transition metals such as iron, copper, nickel and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1% by mass or less.
[0055] For example, in the case of an electrode used as a negative electrode, the current collector (negative electrode current collector) is preferably made of copper, nickel, stainless steel, aluminum, or an aluminum alloy containing one or more elements selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.
[0056] In both the positive and negative electrode embodiments, it is desirable for the current collector to comprise aluminum.
[0057] When the electrode is mounted in a battery, it constitutes, for example, a wound-type electrode group. That is, the electrode can be an electrode for a wound-type electrode group. Alternatively, the electrode can be included in, for example, a stacked-type electrode group and mounted in a battery. That is, the electrode can also be an electrode for a stacked-type electrode group.
[0058] An electrode group may be configured using an electrode according to the embodiment as a positive electrode and another electrode as a negative electrode. Alternatively, an electrode group may be configured using an electrode according to the embodiment as a negative electrode and another electrode as a positive electrode. Alternatively, an electrode group may be configured using an electrode according to the embodiment as a positive electrode and an electrode as a negative electrode.
[0059] In the electrode group, when another electrode is used as a counter electrode for the electrode according to the embodiment curved with the above-mentioned negative curvature amount, it is preferable that the other electrode has been straightened. More preferably, the other electrode has been straightened. In other words, in the electrode group, it is preferable to combine the positive electrode and the negative electrode of the electrode according to the above-mentioned embodiment, or to combine the electrode according to the above-mentioned embodiment with an electrode that is almost not curved as a counter electrode.
[0060] The electrode group may further include a separator disposed between the positive and negative electrodes in addition to the positive and negative electrodes. The separator is typically formed from a material having electrical insulation properties. The separator is formed from, for example, a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric.
[0061] An example of an electrode group is shown in Fig. 4. The electrode group 50 shown in Fig. 4 is a flat wound-type electrode group. The flat wound-type electrode group 50 includes a positive electrode 20, a negative electrode 30, and a separator 40. The separator 40 is interposed between the positive electrode 20 and the negative electrode 30. At least one of the positive electrode 20 and the negative electrode 30 is an electrode according to the embodiment.
[0062] The positive electrode 20 includes a positive electrode current collector 23 and a positive electrode active material-containing layer 22 formed on the surface of the positive electrode current collector 23. The positive electrode current collector 23 includes a positive electrode current collector tab 23b that corresponds to a portion of the surface of the positive electrode current collector 23 where the positive electrode active material-containing layer 22 is not provided. The positive electrode current collector tab 23b corresponds to an active material non-supporting portion of the positive electrode 20.
[0063] The negative electrode 30 includes a negative electrode current collector 33 and a negative electrode active material-containing layer 32 formed on the surface of the negative electrode current collector 33. The negative electrode current collector 33 includes a negative electrode current collector tab 33b that corresponds to a portion of the surface of the negative electrode where the negative electrode active material-containing layer 32 is not provided. The negative electrode current collector tab 33b corresponds to an active material non-supporting portion of the negative electrode 30.
[0064] Although no example is shown, the laminated electrode group may include, for example, a plurality of positive electrodes including a rectangular-shaped positive electrode active material-containing layer and a plurality of negative electrodes including a rectangular-shaped negative electrode active material-containing layer. The electrode group may further include, for example, one or more separators. According to a specific example, the laminated electrode group may have a structure in which a positive electrode, a separator, and a negative electrode are laminated in the order of "-positive electrode-separator-negative electrode-separator-positive electrode-separator-negative electrode-separator-". For example, a plurality of separators may be interposed between the positive electrode and the negative electrode, or a single separator may be folded zigzag and interposed at each position between the positive and negative electrodes.
[0065] <Electrode manufacturing method> Such an electrode can be manufactured, for example, as follows.
[0066] First, an electrode active material, a binder, and optionally a conductive agent are suspended in a solvent to prepare a slurry. This slurry is applied to one or both main surfaces of a current collector. The applied slurry is then dried to obtain an electrode sheet, which is a laminate of an active material-containing layer and a current collector. The electrode sheet is pressed to adjust the density of the active material-containing layer, and then the electrode sheet is stretched.
[0067] Here, the current collector may have, for example, a band shape. An example of the current collector may have a rectangular shape. When preparing the electrode sheet, for example, the end portion along one long side of the short side direction of the current collector is not coated with the slurry, so that the slurry-uncoated portion on the current collector is the active material-containing layer non-supporting portion. In addition, prior to the pressing or stretching of the electrode sheet, it is desirable to cut the electrode sheet so that the active material non-supporting portion is along only one of the long sides of the current collector.
[0068] The electrode sheet is produced, for example, by continuously applying a slurry onto a current collector and drying the slurry, and then winding the current collector into a hoop shape to obtain a roll. The electrode sheet can be unwound from the roll and continuously subjected to a pressing process and a stretching process. The electrode sheet can also be subjected to a pressing process and then wound into a hoop shape. Even after the electrode sheet is wound into a roll, the electrode sheet can be cut, for example, by slitting.
[0069] An example of the pressing process and the stretching process will be described with reference to Figs. 5 to 8. In each figure, arrows X, Y, and Z indicate three directions perpendicular to each other. In addition, in each figure, the configuration is enlarged, reduced, or omitted as appropriate for the purpose of explanation.
[0070] A stretching device used in the manufacture of such an electrode is shown diagrammatically in Fig. 5. The illustrated stretching device 70 is configured to include, in order from upstream to downstream along the feeding direction of the electrode sheet 10, a press unit 71 that compresses the electrode sheet 10 to improve the electrode density, a stretch unit 72 that stretches the electrode sheet 10, which curves in the positive direction when compressed, to curve it in the negative direction by stretching it, and a winding unit 73 that winds up the electrode sheet 10 after it has been pressed and stretched.
[0071] The press unit 71 has a pair of press rolls, 71a and 71b. The press rolls 71a and 71b are rotated by a drive unit about an axis along the Y axis, thereby compression-molding the electrode sheet 10 inserted between the press rolls 71a and 71b.
[0072] The winding unit 73 is configured to rotate the rotary shaft 73a about an axis along the Y axis by a drive unit, thereby winding up the electrode sheet 10 in a hoop shape to form a roll R1.
[0073] The stretching unit 72 has a plurality of metallic guide rollers 74-78 (driven rollers) and guides the electrode sheet 10 from the press unit 71 to the winding unit 73. Tension (winding tension) is applied in the longitudinal direction to the electrode sheet 10 transported from the press rolls 71a and 71b to the winding unit 73. The guide rollers 74-77 are arranged alternately on the upper and lower surfaces of the electrode sheet 10 so that the tension applied to the electrode sheet 10 is within a desired range suitable for winding. The guide roller 78 functions as a stretching member.
[0074] As shown in Figs. 6 to 8, the guide roller 78 has a small diameter portion 81 and a large diameter portion 82 aligned along the axial direction. Each of the small diameter portion 81 and the large diameter portion 82 has a cylindrical shape. The small diameter portion 81 and the large diameter portion 82 are connected on the same axis of each cylindrical shape. The small diameter portion 81 has a retracted surface 81a that corresponds to the side surface of the cylinder. The large diameter portion 82 has a protruding surface 82a that corresponds to the side surface of the cylinder. As shown in the figures, the guide roller 78 may have a relief portion 84 at a portion spaced a predetermined distance from the boundary position between the small diameter portion 81 and the large diameter portion 82 toward the large diameter portion 82. The relief portion 84 shown in the figures is formed continuously from the large diameter portion 82, has a gradually decreasing diameter, and is formed in a round shape with a curved cross section. The relief portion 84 may be omitted.
[0075] The outer peripheral surface of the small diameter portion 81 forms a retreat surface 81a, the outer peripheral surface of the large diameter portion 82 forms a protruding surface 82a, and the outer peripheral surface of the relief portion 84 forms a relief surface 84a. That is, on the outer peripheral surface of the guide roller 78, the retreat surface 81a facing the main surface of the active material containing layer 2 of the electrode sheet 10, the protruding surface 82a facing the active material non-supporting portion 3b of the current collector 3, and the relief surface 84a facing the end region along the third end portion 3c of the electrode sheet 10 are continuously formed.
[0076] The diameter r1 of the small-diameter portion 81, the diameter r2 of the large-diameter portion 82, and the diameter r3 of the relief portion 84 satisfy the relationship r1 < r3 < r2. The diameter r1 of the small-diameter portion 81 corresponds to the distance from the central axis of the cylindrical shape to the retreat surface 81a. The diameter r2 of the large-diameter portion 82 corresponds to the distance from the central axis of the cylindrical shape to the protruding surface 82a. The large-diameter portion 82 protrudes in the radial direction with respect to the small-diameter portion 81, and the protruding surface 82a is located outside compared to the retreat surface 81a. The diameter r3 of the relief portion 84 corresponds to the radius of the circular end face of the relief portion 84.
[0077] The protruding surface 82a protrudes with respect to the conveyance surface 90 shown by the broken line in the figure, and the retreat surface 81a is separated from the conveyance surface 90. The relief surface 84a is curved in an arcuate shape so as to gradually separate from the conveyance surface 90.
[0078] Regarding the positional relationship between the guide roller 78 and the electrode sheet 10, the active material-containing layer 2 faces the small-diameter portion 81, and the large-diameter portion 82 is set so as not to ride on the main surface of the active material-containing layer 2. That is, the axial direction (Y direction) arrangement of the electrode sheet 10 and the guide roller 78 is set so that the second end portion 2b of the active material-containing layer 2, which corresponds to the boundary between the active material-containing layer 2 and the active material non-supporting portion 3b, contacts the wall surface 83a of the step portion 83.
[0079] In a state where the electrode sheet 10 is wound around the guide roller 78, the retreat surface 81a, which is the outer peripheral surface of the small-diameter portion 81, is set not to contact the current collector 3 and the active material-containing layer 2 of the electrode sheet 10, and a gap 90a is formed therebetween. That is, the step H determined by the difference r2 - r1 between the radius r2 of the large-diameter portion 82 and the radius r1 of the small-diameter portion 81 is set to be larger than the thickness t1 of the active material-containing layer 2, satisfying H > t1.
[0080] It is desirable that the step H (%) is within the range of 150% ≤ H ≤ 600% with the thickness t1 of the active material-containing layer 2 as 100%.
[0081] By making the step H 150% or more of the thickness t1, it is possible to sufficiently concentrate stress on the non-active material supporting portion 3b and stretch it. Furthermore, by making the step H 600% or less of the thickness t1, it is possible to prevent wrinkles and cracks from occurring near the boundary between the non-active material supporting portion 3b and the active material-containing layer 2 (i.e., near the second end portion 2b). To enhance the effect of preventing wrinkles and cracks, a range of 200%≦H≦400% is more preferable.
[0082] The flank 84a faces a portion of the current collector 3 along the third end 3c. That is, the third end 3c of the current collector 3 is positioned outside the starting end 84b of the flank 84a in the axial direction (Y direction).
[0083] As shown in FIG. 8, the wrap angle θ at which electrode sheet 10 is wrapped around the outer periphery of guide roller 78 is preferably 60 degrees or more.
[0084] Furthermore, guide roller 78 may be provided with heater 78a as a heating device. By performing a heat treatment with a heater in the stretching process, electrode sheet 10 can be stretched and put into a state where it is easily deformed.
[0085] When the electrode sheet 10 is wound around the guide roller 78 configured as described above and wound up by the winding unit 73, the active material non-supporting portion 3b in contact with the contact surface is pulled and stretched in the length direction (feed direction) by tension. When a certain level of tension is applied to the active material non-supporting portion 3b, the curvature of the electrode sheet 10 caused by the difference in the amount of stretching during pressing is corrected. By applying a larger tension, the electrode sheet 10 can be curved in the direction opposite to the curvature during pressing. In other words, by stretching the active material non-supporting portion 3b with a tension larger than the tension for correcting the curvature of the electrode sheet 10, the electrode 1 according to the embodiment having the curved state shown in FIG. 1 can be obtained from the conventional curved state of the electrode 1 shown in FIG. 3.
[0086] By setting conditions such that the tension in the longitudinal direction (transport direction) applied to the electrode sheet 10 before and after the guide rollers 78 in the stretch unit 72 is between 10 N and 100 N, it is possible to obtain an electrode according to the embodiment that is curved in the direction opposite to the curvature caused by pressing. The tension at the midpoint described above can be controlled by, for example, appropriately adjusting the positions of the guide rollers 74 to 78, the unwinding speed of the electrode sheet 10, and the winding speed of the electrode sheet 10.
[0087] In the press treatment, for example, the electrode sheet 10 wound in a roll shape is inserted between rotating press rolls 71a and 71b while being unwound, and compression molding is performed. The insertion direction of the electrode sheet 10 is parallel to the longitudinal direction of the electrode sheet 10, and the press pressure is mainly applied to the active material-containing layer 2, which is compression molded to increase its density. At this time, almost no press pressure is applied to the active material non-supporting portion 3b, so that the elongation of the current collector 3 is smaller in the active material non-supporting portion 3b than in the active material supporting portion 3a. As a result, the electrode sheet 10 is distorted or warped.
[0088] The electrode sheet 10 that has passed between the press rolls 71a and 71b is sent downstream and transported to the winding unit 73 via guide rollers 74 to 78. At this time, in the guide roller 78 that also serves as a stretching member, the active material carrying portion 3a and the active material containing layer 2 correspond to the small diameter portion 81, and the large diameter portion 82 and the active material non-supporting portion 3b are arranged opposite to each other, as shown in Figures 6 to 8. That is, the active material non-supporting portion 3b of the current collector 3 contacts the protruding surface 82a that is the outer circumferential surface of the large diameter portion 82, and a gap 90a is formed between the retreating surface 81a that is the outer circumferential surface of the small diameter portion 81 and the active material containing layer 2.
[0089] In this state, the electrode sheet 10 is wound up by the winding unit 73 as a stretching process. In the stretching process, the tensile stress F in a cross section parallel to the short side direction (width direction) of the electrode sheet 10 is set to 1 N / mm 2 ≦F≦100N / mm 2 It is preferable to set the tensile stress F to within the range of 1N / mm 2By setting the tensile stress F to 100 N / mm or more, it is possible to sufficiently stretch the active material non-supporting portion 3b (current collector exposed portion) of the current collector 3 while satisfying the stress required for winding the electrode with high precision. 2 By setting the tensile stress F to 1 N / mm or less, the active material non-supporting portion 3b can be sufficiently stretched without causing the problems of electrode breakage and reduced winding accuracy. 2 ≦F≦100N / mm 2 By setting the range to 20 N / mm, the electrode can be wound up accurately without breaking and the active material non-supporting portion 3b can be sufficiently stretched. Although it depends on the height of the step and the shape of the corner portion, in order to enhance the effect of preventing the electrode from breaking and the deterioration of the winding accuracy, it is preferable to set the range to 20 N / mm 2 ≦F≦40N / mm 2 The range is more preferable.
[0090] The stretching treatment is desirably performed while applying a heat treatment at a temperature of 60° C. or more and 150° C. or less using heater 78a, for example. By setting the heat treatment temperature T to 60° C. or more, the effect of reducing the stress required for plastic deformation can be enhanced. Although the effect of reducing the stress can be enhanced as the heat treatment temperature T is higher, it is desirably set to the range of 60° C. or more and 150° C. or less in order to prevent deterioration of active material-containing layer 2 due to heat.
[0091] In the electrode sheet 10 after compression molding, the active material carrying portion 3a of the current collector 3 is stretched and slack, so that the winding tension (stress) from the guide roller 78 is hardly applied to the active material carrying portion 3a, and the winding tension is concentrated on the active material non-carrying portion 3b that has not been stretched after compression.
[0092] The electrode sheet 10 that has passed through the guide roller 78 passes through guide rollers 76 and 78 and is wound up by a winding unit 73. The hoop-shaped electrode sheet 10 is then cut to a desired size as necessary to obtain an electrode. The electrode sheet 10 can also be used as an electrode as it is.
[0093] In the illustrated example, the guide roller 78 is used to arrange the end region of the current collector 3 along the third end 3c and the relief surface 84a to face each other, and this arrangement is preferable because it can reduce stress concentration at the third end 3c. In detail, the large stress applied to the non-active material carrying portion 3b of the current collector 3 during the stretching process can be dispersed over the width of the non-active material carrying portion 3b in the short side direction (Y direction) without being concentrated only in the vicinity of the third end 3c. As a result, even if fine cracks are formed on the end face of the third end 3c of the current collector 3, for example, cracks and breakage can be prevented by reducing the stress concentration. That is, for example, when stress is concentrated on scratches or cracks on the end face, cracks or breaks are likely to occur from the scratches or cracks, but by concentrating stress on the active material non-supporting portion 3b near the second end 2b of the active material-containing layer 2 where distortion is particularly large and stretching is performed, while avoiding stress concentration at the third end 3c spaced a certain distance from the second end 2b, it is possible to suppress cracks and breaks while ensuring the stretching effect. In this preferred embodiment, stress concentration can be avoided by a simple configuration in which the diameter of the portion of the guide roller 78 facing the vicinity of the third end 3c of the current collector 3 is gradually reduced to form a relief surface 84a that retreats from the conveying surface 90 in the direction toward the axis (downward in FIG. 7).
[0094] The above-mentioned embodiment is an example of the pressing and stretching of the electrode sheet, and the manufacturing method of the electrode according to the embodiment can be modified as appropriate. For example, the recess 84 and the recess surface 84a may be omitted from the guide roller 78.
[0095] In the above example, the shape of the relief portion 84 of the guide roller 78 is a round shape that is formed continuously from the large diameter portion 82, the diameter gradually decreases, and the cross section is curved, but the shape is not limited to this. For example, the guide roller 178 according to the modified example shown in FIG. 9 has a relief portion 184 that is formed in a tapered shape with a decreasing diameter and an inclined cross section at a portion beyond the starting end portion 184b axially separated from the step portion 83. The outer surface of this relief portion 184 forms the relief surface 184a. Even when the diameter is changed so that such a cross-sectional shape becomes a straight line, it is possible to alleviate stress concentration at the third end portion 3c of the current collector 3.
[0096] In the above example, the press unit 71 including the press roll 71a and the press roll 71b was used, but any other material capable of densifying the active material-containing layer 2 can be used instead of the press roll. For example, a flat plate press can be used instead of the press roll. The pressing process may be performed by changing the pressing pressure in multiple stages.
[0097] In the above example, one of the multiple guide rollers, guide roller 78, is used as a stretching member, but the number of guide rollers is not limited to the above, and the number and positions of guide rollers used as stretching members are not limited to the above.
[0098] Although the outer peripheral surface of the large diameter portion 82 protruding from the circumferential surface at one end in the rotation axis direction of the guide roller 78 is used as the protruding surface, the present invention is not limited to this and may be any surface that can achieve the effect of stretching the active material non-supporting portion 3b. For example, the positions and numbers of the steps, large diameter portion, and small diameter portion can be changed as appropriate.
[0099] Furthermore, although the step 83 provided on the guide roller 78 is a right angle or a nearly right angle as shown in FIG. 6, the present invention is not limited to this and may be tapered. For example, a guide roller 278 according to another modified example shown in FIG. 10 has a curved corner portion of the step 283. The smaller the radius of curvature of the corner portion, the greater the effect of stretching the non-active material carrying portion 3b of the current collector 3, but the more likely the electrode breaks when the electrode sheet 10 meanders. For this reason, it is more preferable that the radius of curvature R (mm) of the corner portion is in the range of, for example, 0.5 mm≦R≦7 mm.
[0100] Although an example in which the active material-containing layer 2 is provided on both sides of the current collector 3 is illustrated, the active material-containing layer 2 may be provided on only one side of the current collector 3 .
[0101] The electrode produced as described above can be laminated with a counter electrode via a separator, and the resulting laminate can be spirally wound to produce a wound electrode group. For example, a secondary battery can be obtained by sequentially carrying out various procedures, such as housing the electrode group in an exterior member for a battery, introducing an electrolyte as necessary, and sealing the exterior member.
[0102] <How to measure the amount of curvature> The amount of curvature of the electrode can be measured as follows.
[0103] First, in the electrode, the position of the active material non-supporting portion of the current collector where the active material-containing layer is not provided is confirmed. For example, along one side of the planar electrode, a portion where the active material-containing layer is not provided on either of the front and back main surfaces and the current collector is exposed may be included. As a more specific example, along one long side of a planar electrode having a pair of arc-shaped long sides, a portion where the current collector is exposed may be included. In that case, the exposed portion of the current collector is determined to be the active material non-supporting portion. Alternatively, for example, a portion where the current collector is exposed along both of the pair of long sides may be included. In that case, as described above, the portion of the exposed current collector having a wider short side width is determined to be the active material non-supporting portion that can function as a current collecting tab.
[0104] An end along a long side of the non-active material-supporting portion is defined as a third end. An end of the active material-containing layer located at the boundary between the non-active material-supporting portion and the active material-containing layer is defined as a second end. An end of the active material-containing layer located on the opposite side of the second end to the third end in the electrode is defined as a first end.
[0105] Points P1 and P2 are set on a first end of the active material-containing layer. Points P1 and P2 are set so that the distance D of a straight line (reference line L) connecting these points is 1000 mm. The straight line connecting points P1 and P2 is defined as the reference line L. The maximum distance M from the first end to this reference line L is measured. The maximum distance M, when the direction from the first end to the second end is defined as a positive value, is defined as the amount of curvature.
[0106] The amount of curvature is measured at multiple points along the first end of the active material-containing layer, and evaluated as the range of the measured values. The measurement points can be, for example, 5 points at 0.5 m intervals per 2 m along the first end. When the electrode is in a strip shape, the measurement is performed from a point at least 0.5 m away from the end of the strip. However, the present invention is not limited to this.
[0107] The electrode according to the embodiment includes an active material-containing layer and a current collector. The active material-containing layer includes a first end having an arc shape and a second end opposite to the first end. The active material-containing layer contains an electrode active material. The current collector includes an active material-supporting portion that supports the active material-containing layer and an active material-non-supporting portion that does not have the active material-containing layer. The active material-non-supporting portion is adjacent to the active material-supporting portion and the second end. The electrode has a curved shape with a curvature amount within a range of -1 mm or more and less than 0 mm. Here, the curvature amount is expressed as the maximum distance from the first end to a reference line connecting two points on the first end that are 1000 mm apart in a straight line, with the direction from the first end to the second end being a positive value. An electrode group using this electrode can be manufactured with a high yield.
[0108] [Example] The above-mentioned embodiment will be described in more detail below based on examples, but the present invention is not limited to the examples listed below.
[0109] (Example P1) The electrode active material is LiNi 0.8 Co 0.1 Mn 0.1 A powder of lithium nickel cobalt manganese composite oxide having a composition represented by O2 was prepared.
[0110] The lithium nickel cobalt manganese composite oxide powder, acetylene black as a conductive agent, and polyvinylidene fluoride (PVdF) as a binder were mixed in a mixing ratio of 95 parts by weight: 3 parts by weight: 2 parts by weight in N-methylpyrrolidone (NMP) as a solvent, and then the mixture thus obtained was dispersed to prepare a slurry.
[0111] Next, the prepared slurry was applied to the surface of a current collector made of aluminum foil with a thickness of 15 μm. Next, the coating film was dried. The slurry was similarly applied to the back side of the aluminum foil, and the coating film was dried. The aluminum foil was cut into a strip shape with a slurry coating width of 100 mm and a slurry uncoated width of 10 mm. Next, the obtained electrode sheet was pressed and stretched in succession using a device similar to the stretching device shown in Figures 5 to 8. The stretching process was performed with a tension of 25 N at the midpoint near the guide roller as the stretching member.
[0112] The electrode sheet is pressed and stretched in succession until the mass per unit area on one side of the current collector is 160 g / m 2 and the density is 3.3 g / cm 3 The amount of curvature referred to here is a range of values obtained by measuring the maximum distance M from the first end of the active material-containing layer to the reference line L at five points at 0.5 m intervals along the first end when the linear distance D between points P1 and P2 is set to 1000 mm using the method described above.
[0113] An electrode was prepared according to the above procedure.
[0114] (Examples P2 to P13, Comparative Examples P1 to P3) As shown in Tables 1 and 2 below, the composition of the electrode active material, the mass of the active material-containing layer per unit area per side of the current collector, the density of the active material-containing layer, the width of the slurry coating and the width of the uncoated portion, and the tension on the electrode sheet at the midpoint during the stretching process were changed, but the electrodes were produced in the same manner as in Example P1. The mass of the active material-containing layer per side of the current collector was adjusted by the amount of slurry applied to the current collector per side. Table 2 also shows the amount of curvature measured for each electrode. The amount of curvature "almost zero" for Comparative Example P1 means that the absolute value of the amount of curvature was small and accurate measurement was not possible, and therefore curvature was not actually confirmed.
[0115] [Table 1]
[0116] [Table 2]
[0117] (Example N1) Niobium titanium composite oxide having a composition represented by TiNb2O7 was prepared as an electrode active material. Acetylene black (AB) was prepared as a conductive agent, and carboxymethyl cellulose (CMC) and styrene butadiene rubber (SBR) were prepared as binders. TiNb2O7, AB, CMC, and SBR were mixed in a mixing ratio of 95 parts by weight: 2 parts by weight: 1.5 parts by weight: 1.5 parts by weight into pure water as a solvent and mixed. The mixture was then dispersed to obtain a slurry.
[0118] Next, the coating was dried. The back side of the aluminum foil was similarly coated with the slurry, and the coating was dried. The aluminum foil was cut into a strip having a width of 100 mm for the coating of the slurry and a width of 10 mm for the non-coated portion of the slurry. Next, the obtained electrode sheet was subjected to a press and stretching process in succession in the same manner as in Example P1. The stretching process was performed with a tension of 30 N at the midpoint near the guide roller as the stretching member.
[0119] The electrode sheet is pressed and stretched in succession until the mass per unit area on one side of the current collector is 140 g / m 2 and the density is 2.7 g / cm 3 An electrode having an active material-containing layer having the above structure and having a curvature of -0.4 mm to -0.2 mm was produced.
[0120] An electrode was prepared according to the above procedure.
[0121] (Examples N2 to N11, Comparative Examples N1 to N3) As shown in Tables 3 and 4 below, the composition of the electrode active material, the mass of the active material-containing layer per unit area per side of the current collector, the density of the active material-containing layer, the width of the slurry coating and the width of the uncoated portion, and the tension at the winding point during the stretching process were changed, but the electrodes were produced in the same manner as in Example N1. The mass of the active material-containing layer per side of the current collector was adjusted by the amount of slurry applied to the current collector per side. Table 4 also shows the amount of curvature measured for each electrode. The amount of curvature "almost zero" for Comparative Example N1 means that, like Comparative Example P1, no curvature was actually observed.
[0122] (Example N12) As an electrode active material, Li4Ti5O 12 A composite oxide having the composition represented by the formula Li4Ti5O was prepared. Acetylene black (AB) was used as a conductive agent, and polyvinylidene fluoride (PVdF) was used as a binder. 12An electrode was produced in the same manner as in Example N1, except that AB and PVdF were mixed in a mixing ratio of 95 parts by weight:3 parts by weight:2 parts by weight in NMP as a solvent, and the density of the active material-containing layer and the tension at the midpoint during the stretching treatment were changed as shown in Tables 3 and 4. The mass of the active material-containing layer per side of the current collector was adjusted by the amount of slurry applied per side of the current collector.
[0123] [Table 3]
[0124] [Table 4]
[0125] (Example G1) The electrode prepared in Example P1 was prepared as the positive electrode. The electrode prepared in Example N1 was prepared as the negative electrode. For both the positive electrode and the negative electrode, electrodes that had been stored for a certain period of time after production were prepared. A separator made of a polyethylene porous film having a thickness of 15 μm was prepared. Next, the positive electrode and the negative electrode were spirally wound with the separator therebetween, and then a flat electrode group was produced by applying a hot press. A total of 100 flat electrode groups were produced in the same manner.
[0126] (Examples G2 to G26, Comparative Examples G1 to G9) Except for changing the combination of electrodes to those shown in Tables 5 to 7 below, 100 electrode groups were produced in the same manner as in Example G1.
[0127] [Table 5]
[0128] [Table 6]
[0129] [Table 7]
[0130] <Evaluation> Among the 100 electrode groups produced for each of Examples G1 to G26 and Comparative Examples G1 to G9, the number of "defective" electrode groups in which misalignment occurred during winding of the laminate including the positive electrode, negative electrode, and separator was recorded. The results are shown in Tables 5 to 7 above.
[0131] As the above results show, in the electrode groups (Examples G1 to G26) in which the electrodes according to Examples P1 to P13, in which the amount of curvature was adjusted to within the range of -1 mm or more and less than 0 mm by stretching treatment, were used as the positive electrode, and / or the electrodes according to Examples N1 to N12, in which the amount of curvature was similarly adjusted, were used as the negative electrode, the number of occurrences of defects due to misalignment of winding was low. In the electrode groups in which the electrodes in Comparative Examples G1 to G9, in which the amount of curvature was adjusted to the above range, were not used as either the positive electrode or the negative electrode, defects due to misalignment of winding occurred frequently.
[0132] According to one or more of the embodiments and examples described above, an electrode is provided that includes an active material-containing layer and a current collector. The active material-containing layer includes a first end having an arc shape and a second end opposite to the first end, and contains an electrode active material. The current collector includes an active material-supporting portion that supports the active material-containing layer, and an active material-free portion that is adjacent to the active material-supporting portion and the second end and does not have the active material-containing layer. The amount of curvature of the electrode, which is expressed as the maximum distance from the first end to a reference line that connects two points on the first end that are 1000 mm apart in a straight line, is in the range of -1 mm or more and less than 0 mm. The amount of curvature is defined as a positive value in the direction from the first end to the second end. By using the electrode, the yield of the production of the electrode group can be increased.
[0133] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. The invention as described in the claims of the present application as originally filed is set forth below. [1] An active material-containing layer including a first end portion having an arc shape and a second end portion opposite the first end portion, and containing an electrode active material; a current collector including an active material-supported portion supporting the active material-containing layer, and an active material-free portion adjacent to the active material-supported portion and the second end portion and not provided with the active material-containing layer, An electrode, wherein a direction from the first end to the second end is defined as a positive value, and an amount of curvature represented by the maximum distance from the first end to a reference line connecting two points on the first end that are 1000 mm apart in a straight line is within a range of -1 mm or more and less than 0 mm. [2] The electrode according to [1], wherein the current collector contains aluminum. [3] The electrode described in [1] or [2], wherein a width of the active material-containing layer between the first end and the second end is 60 mm or more and 250 mm or less, and a width of the active material-free portion in a direction intersecting with the second end is 5 mm or more and 25 mm or less. [4] The mass per unit area of the active material-containing layer on the active material support portion is 100 g / m on each side of the current collector. 2 More than 300g / m 2 The electrode according to any one of [1] to [3], which is: [Explanation of symbols]
[0134] 1...electrode, 2...active material-containing layer, 2a...first end, 2b...second end, 3...current collector, 3a...active material-supporting portion, 3b...active material-non-supporting portion, 3c...third end, 10...electrode sheet, 20...positive electrode, 22...positive electrode active material-containing layer, 23...positive electrode current collector, 23b...positive electrode current collector tab, 30...negative electrode, 32...negative electrode active material-containing layer, 33...negative electrode current collector, 33b...negative electrode current collector tab, 40...separator, 50...electrode group, 70...stretching device, 71...press unit, 71a, 71b...press roll, 72...stretch unit , 73...winding unit, 73a...rotating shaft, 73...winding unit, 74, 75, 76, 77...guide rollers, 78...guide roller (stretch member), 78a...heater, 81...small diameter portion, 81a...retraction surface, 82...large diameter portion, 82a...protruding surface, 83...step portion, 84...relief portion, 84a...relief surface, 90...conveying surface, 90a...gap, 178...guide roller, 184...relief portion, 184a...relief surface, 184b...starting end, 278...guide roller, 283...step portion, H...step.
Claims
1. An electrode group including a positive electrode, a negative electrode, and a separator, The positive electrode includes a positive electrode first end having an arc shape and a positive electrode second end opposite to the positive electrode first end, and a positive electrode active material-containing layer containing a positive electrode active material; a positive electrode current collector including a positive electrode active material-supporting portion supporting the positive electrode active material-containing layer, and a positive electrode active material-non-supporting portion adjacent to the positive electrode active material-supporting portion and the positive electrode second end portion and not provided with the positive electrode active material-containing layer, a positive electrode curvature amount represented by a maximum distance from the positive electrode first end to a reference line connecting two points on the positive electrode first end that are separated by a linear distance of 1000 mm is within a range of -1 mm or more and less than 0 mm, the negative electrode includes a negative electrode first end and a negative electrode second end opposite the negative electrode first end, and a negative electrode active material-containing layer containing a negative electrode active material; a negative electrode current collector including a negative electrode active material-supporting portion supporting the negative electrode active material-containing layer, and a negative electrode active material-free portion adjacent to the negative electrode active material-supporting portion and the negative electrode second end portion and not provided with the negative electrode active material-containing layer, a negative electrode curvature amount, which is expressed by a maximum distance from the negative electrode first end to a reference line connecting two points on the negative electrode first end that are 1000 mm apart in a straight line, is within a range of -1 mm or more and less than 0 mm, and the negative electrode first end has an arc shape, or the negative electrode curvature amount is 0 mm, The electrode group is a wound electrode group in which the positive electrode and the negative electrode are wound in a spiral shape with the separator interposed therebetween, or An electrode group for a secondary battery, which is a stacked electrode group in which the positive electrode and the negative electrode are stacked with the separator interposed therebetween.
2. the positive electrode current collector comprises aluminum, or 2. The electrode group according to claim 1, wherein the negative electrode curvature amount is within a range of −1 mm or more and less than 0 mm, the negative electrode first end has an arc shape, and the negative electrode current collector contains aluminum.
3. the width of the positive electrode active material-containing layer between the positive electrode first end and the positive electrode second end is 60 mm or more and 250 mm or less, and the width of the positive electrode active material-free portion in a direction intersecting with the positive electrode second end is 5 mm or more and 25 mm or less, or 3. The electrode group according to claim 1, wherein the negative electrode curvature amount is within a range of −1 mm or more and less than 0 mm, the negative electrode first end has an arc shape, the width of the negative electrode active material-containing layer between the negative electrode first end and the negative electrode second end is 60 mm or more and 250 mm or less, and the width of the negative electrode active material-free portion in a direction intersecting with the negative electrode second end is 5 mm or more and 25 mm or less.
4. The mass per unit area of the positive electrode active material-containing layer on the positive electrode active material support portion is 100 g / m on each side of the positive electrode current collector. 2 More than 300g / m 2 is less than or equal to The negative electrode curvature amount is within a range of −1 mm or more and less than 0 mm, the negative electrode first end portion has an arc shape, and the mass per unit area of the negative electrode active material-containing layer on the negative electrode active material support portion is 100 g / m2 on each side of the negative electrode current collector. 2 More than 300g / m 2 The electrode group according to claim 1 , wherein:
5. An electrode group including a positive electrode, a negative electrode, and a separator, The negative electrode includes a negative electrode first end having an arc shape and a negative electrode second end opposite to the negative electrode first end, and a negative electrode active material-containing layer containing a negative electrode active material; a negative electrode current collector including a negative electrode active material-supporting portion supporting the negative electrode active material-containing layer, and a negative electrode active material-free portion adjacent to the negative electrode active material-supporting portion and the negative electrode second end portion and not provided with the negative electrode active material-containing layer, a negative electrode curvature amount represented by a maximum distance from the negative electrode first end to a reference line connecting two points on the negative electrode first end that are 1000 mm apart in a straight line, is within a range of -1 mm or more and less than 0 mm, the negative electrode curvature amount being represented by a maximum distance from the negative electrode first end to a reference line connecting two points on the negative electrode first end that are 1000 mm apart in a straight line, the positive electrode includes a positive electrode first end and a positive electrode second end opposite the positive electrode first end, and a positive electrode active material-containing layer containing a positive electrode active material; a positive electrode current collector including a positive electrode active material-supporting portion supporting the positive electrode active material-containing layer, and a positive electrode active material-non-supporting portion adjacent to the positive electrode active material-supporting portion and the positive electrode second end portion and not provided with the positive electrode active material-containing layer, a positive electrode curvature amount represented by a maximum distance from the positive electrode first end to a reference line connecting two points on the positive electrode first end that are separated by a linear distance of 1000 mm is 0 mm, The electrode group is a wound electrode group in which the positive electrode and the negative electrode are wound in a spiral shape with the separator interposed therebetween, or An electrode group for a secondary battery, which is a stacked electrode group in which the positive electrode and the negative electrode are stacked with the separator interposed therebetween.
6. The electrode group according to claim 5 , wherein the negative electrode current collector comprises aluminum.
7. 7. The electrode group according to claim 5, wherein a width of the negative electrode active material-containing layer between the negative electrode first end and the negative electrode second end is 60 mm or more and 250 mm or less, and a width of the negative electrode active material-free portion in a direction intersecting with the negative electrode second end is 5 mm or more and 25 mm or less.
8. The mass per unit area of the negative electrode active material-containing layer on the negative electrode active material support portion is 100 g / m for each side of the negative electrode current collector. 2 More than 300g / m 2 The electrode group according to claim 5 , wherein:
Citation Information
Patent Citations
Manufacture of sheet electrode
JP2001076711A
Manufacturing method of electrode
JP2007273390A
Nonaqueous electrolyte battery
JP2008226555A
Method for manufacturing battery
JP2012174434A
Press device of electrode, manufacturing apparatus of electrode and manufacturing method of electrode
JP2013073690A