Anode piece and electrochemical device including same

A multilayered negative electrode skeleton structure addresses lithium metal-related issues in electrochemical devices by stabilizing lithium deposition and reducing dendrite formation, enhancing the safety and stability of electrochemical devices.

JP7581360B2Active Publication Date: 2024-11-12NINGDE AMPEREX TECHNOLOGY LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022552979
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-30
Publication Date
2024-11-12
Estimated Expiration
2040-03-30

AI Technical Summary

Technical Problem

Lithium metal-based negative electrodes in electrochemical devices face issues such as high reactivity with electrolytes, formation of lithium dendrites, severe volume changes, and reduced cycle coulomb efficiency, leading to safety concerns and instability.

Method used

A negative electrode piece with a multilayer skeleton structure, featuring a first layer with higher porosity near the current collector and a second layer with lower porosity, providing stable lithium deposition and suppressing dendrite growth, while reducing volume changes and enhancing ion and electron transport.

Benefits of technology

The multilayer structure improves lithium deposition uniformity, suppresses dendrite formation, and enhances the stability and safety of electrochemical devices by minimizing volume changes and side reactions, thereby increasing cycle stability and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581360000009
    Figure 0007581360000009
  • Figure 0007581360000010
    Figure 0007581360000010
  • Figure 0007581360000011
    Figure 0007581360000011
Patent Text Reader

Abstract

The present invention relates to an anode piece and an electrochemical device including the same. Specifically, the anode piece includes a current collector (101) and an anode skeleton located on the current collector (101). The anode skeleton includes at least a first anode skeleton layer (102) and a second anode skeleton layer (103). The first anode skeleton layer (102) is located between the current collector (101) and the second anode skeleton layer (103). The porosity of the first anode skeleton layer (102) is greater than that of the second anode skeleton layer (103). This design reduces side reactions between lithium metal and the electrolyte, inhibits the formation of lithium dendrites, and significantly reduces or even eliminates the rapid volumetric expansion and contraction of the anode piece due to the absorption and desorption of lithium ions, thereby improving the safety and stability of the electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of energy storage technology, and more particularly to negative electrode pieces and electrochemical devices containing the same. [Background technology]

[0002] With the continuous progress of science and technology and the continuous increase of the demand for environmental protection, electrochemical devices play an increasingly important role in our daily life. Here, lithium-ion batteries have the advantages of large specific energy, high working voltage, low self-discharge rate, small volume, light weight, etc., and are therefore widely used in the consumer electronics field. However, with the rapid development of electric vehicles and mobile electronic devices, the requirements for the energy density, safety, cycle characteristics, etc. of electrochemical devices are increasingly higher. Among them, volumetric energy density and mass energy density are important parameters for evaluating the characteristics of electrochemical devices.

[0003] Lithium metal has the smallest relative atomic mass (6.94) and the lowest standard electrode potential (-3.045V) of all metallic elements, and its theoretical gram capacity can reach 3860mAh / g. Therefore, by using lithium metal as the negative electrode of an electrochemical device and compounding it with some high-energy-density positive electrode materials, the energy density of the electrochemical device and its operating voltage can be greatly increased. However, in practical commercial applications, using lithium metal as the negative electrode piece of an electrochemical device may cause various problems during the charge-discharge cycle, which hinders the commercialization of lithium metal as a negative electrode active material. Summary of the Invention

[0004] The present invention has found that when lithium metal is used as the negative electrode active material of an electrochemical device, the following problems occur during the charge and discharge process of the electrochemical device.

[0005] (1) Lithium metal is highly active and is prone to side reactions with the electrolyte in the electrochemical device. As a result, lithium metal and the electrolyte are consumed simultaneously, resulting in a significantly lower cycle coulombic efficiency than electrochemical devices that use conventional graphite as the negative electrode active material.

[0006] (2) During the charging and discharging process of the electrochemical device, lithium metal is deposited on the surface of the negative electrode. Due to the current density and the non-uniformity of the lithium ion concentration in the electrolyte, the deposition speed is too fast in some places, and sharp lithium dendrite structures are formed. The formation of lithium dendrites may reduce the energy density of the electrochemical device, and even pierce the separator in the electrochemical device, causing a short circuit and causing safety problems.

[0007] (3) In the charging and discharging process of the electrochemical device, the negative electrode piece undergoes severe expansion and contraction. According to the general design of the current commercial lithium ion battery, in the process of the electrochemical device going from a fully charged state to a fully discharged state, the thickness of the negative electrode coated with lithium metal on one side changes within a range of 8 μm to 100 μm. This causes the interface between the lithium metal negative electrode active layer and the adjacent structure (e.g., current collector) to peel off, which greatly increases the impedance of the electrochemical device and reduces the stability of the electrochemical device.

[0008] In view of the above problems, the present invention provides a negative electrode piece and an electrochemical device including the same to solve, at least in part, at least one of the above problems.

[0009] In some embodiments, the present invention provides a negative electrode piece including a current collector and a negative electrode skeleton located on the current collector, the negative electrode skeleton including at least a first negative electrode skeleton layer and a second negative electrode skeleton layer, the first negative electrode skeleton layer being located between the current collector and the second negative electrode skeleton layer, and the porosity of the first negative electrode skeleton layer being greater than the porosity of the second negative electrode skeleton layer.

[0010] In some embodiments, the present invention provides an electrochemical device including the negative electrode piece of any of the above embodiments.

[0011] In some embodiments, the present invention provides an electronic device that includes the electrochemical device of any of the above embodiments.

[0012] The present invention provides a special negative electrode skeleton for use in a lithium metal negative electrode, the negative electrode skeleton being located on a current collector and including at least two skeleton layers with different porosities, i.e., a first negative electrode skeleton layer (e.g., located near the current collector and also referred to as an "inner layer") and a second negative electrode skeleton layer (e.g., located farther from the current collector than the first negative electrode skeleton layer and also referred to as an "outer layer"), where the first negative electrode skeleton layer according to the present invention has a larger porosity and plays the following role:

[0013] (1) The first negative electrode skeleton layer has a larger porosity, so that it can provide sufficient space for lithium metal deposition during charging. During discharging, a stable structural support is formed in the process of lithium metal in the negative electrode decreasing continuously, so that the negative electrode piece does not undergo a large volume change, or even a large volume change, during the charging and discharging process of the electrochemical device. Therefore, the large volume change that occurs in the lithium metal negative electrode during the charging and discharging process of the electrochemical device can be alleviated or even eliminated.

[0014] (2) The first negative electrode skeleton layer has a larger porosity, which can provide a good transport path for ions and electrons, and has a larger specific surface area, which can effectively distribute the current during the charge and discharge process, reduce the current density, and form a more uniform electric field, thereby improving the uniformity of lithium deposition and suppressing the growth of lithium dendrites.

[0015] (3) The first negative electrode framework layer has a larger porosity, which can provide a large number of nucleation sites and reduce the current density, thereby effectively improving the compactness of the deposited lithium.

[0016] Here, the second negative electrode framework layer according to the present invention has a smaller porosity and plays the following role.

[0017] (1) Similar to the first negative electrode framework layer, it provides space for lithium metal deposition during charging and discharging, and can greatly reduce or eliminate the large volume change, reduce the current density, inhibit the growth of lithium dendrites, and increase the lithium deposition density.

[0018] (2) The second negative electrode skeletal layer has a denser skeletal structure than the first negative electrode skeletal layer, which contributes to the formation of a dense electrode surface, reduces side reactions between lithium metal and the electrolyte, and improves the cycle stability of the electrode. In addition, a negative electrode protective layer can be further formed on the dense electrode surface of the second negative electrode skeletal layer to further reduce side reactions between lithium metal and the electrolyte and improve the cycle stability of the electrode. [Brief description of the drawings]

[0019] In the following, in order to explain the embodiments of the present invention, necessary drawings for explaining the embodiments of the present invention or the prior art will be briefly described. The drawings described below are only a part of the embodiments of the present invention. [Figure 1] FIG. 1 is a schematic plan view of a stamped negative electrode current collector according to some embodiments of the present invention. [Diagram 2] FIG. 2 is a schematic plan view of a first negative electrode framework layer constructed on the negative electrode current collector shown in FIG. 1 according to some embodiments of the present invention. [Diagram 3] FIG. 3 is a schematic plan view of a second negative electrode skeleton layer constructed on the first negative electrode skeleton layer shown in FIG. 2 according to some embodiments of the present invention. [Figure 4] FIG. 4 is a schematic cross-sectional view of a negative electrode piece taken along line AA' shown in FIG. 3, according to some embodiments of the present invention. [Diagram 5] FIG. 5 is a cross-sectional schematic diagram of a negative electrode piece having a negative electrode skeleton disposed on either side of a current collector according to some embodiments of the present invention. [Figure 6] FIG. 6 is a cross-sectional schematic diagram of an anode piece including more anode skeleton layers according to some embodiments of the present invention. [Figure 7] FIG. 7 is a schematic cross-sectional view of an anode piece having an anode protective layer disposed on a surface of an anode skeleton according to some embodiments of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] In order to make the objectives, technical solutions and advantages of the present invention clearer, the following will refer to the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention, but obviously, the described embodiments are only some of the embodiments of the present invention, and not all of the embodiments. Based on the technical solutions and embodiments provided by the present invention, all other embodiments obtained by those skilled in the art without creative labor also belong to the scope of the protection claims of the present invention.

[0021] In this specification, unless otherwise indicated, terms expressing relative positions, such as "center," "vertical," "horizontal," "front," "rear," "right," "left," "inside," "outside," "relatively low," "relatively high," "horizontal," "vertical," "larger," "smaller," "higher," "lower," "upper," "lower," "top," "bottom," and terms derived therefrom (e.g., "horizontally," "down," "upward," etc.), should be construed as referring to the orientation depicted in the description or drawings in the discussion. These terms expressing relative positions are merely for convenience of explanation and do not require the invention to be constructed or operated in a particular orientation.

[0022] Furthermore, for convenience of description, the terms "first", "second", "third", etc. are used herein to distinguish between different parts of a figure or sequence of figures. The terms "first", "second", "third", etc. are not intended to describe corresponding parts.

[0023] In the detailed description and claims of the present invention, the terms "approximately," "generally," "substantially," and "about" are used to describe and account for small variations. When used in conjunction with an event or circumstance, the term refers to an instance in which the event or circumstance occurs exactly and an instance in which the event or circumstance occurs very similarly. For example, when used in conjunction with a numerical value, the term can refer to a variation range of ±10% or less of the numerical value, such as ±5% or less, ±4% or less, ±3% or less, ±2% or less, ±1% or less, ±0.5% or less, ±0.1% or less, or ±0.05% or less. In the present invention, quantities, ratios, and other numerical values ​​may be expressed in the form of a range. It is to be understood that such range formats are used for convenience and brevity, and are intended to be flexible in their interpretation, including not only the numerical values ​​limited to the ranges explicitly stated, but also all individual numerical values ​​or subranges within said ranges, as if each numerical value and subrange were explicitly stated.

[0024] In the detailed description and claims, a list of items followed by the term "at least one of," "at least one of," or other similar terminology can mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means A only, B only, or A and B. In another embodiment, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means A only, B only, C only, A and B (excluding C), A and C (excluding B), B and C (excluding A), or all of A, B, and C. Item A may include one component or multiple components. Item B may include one component or multiple components. Item C may include one component or multiple components.

[0025] In electrochemical devices (e.g., lithium ion batteries), the use of lithium metal as the negative electrode piece of the electrochemical device can increase the energy density of the battery and the operating voltage of the battery. However, during the charge-discharge cycle of the electrochemical device, the use of lithium metal as the negative electrode piece can cause various problems, such as side reactions between the lithium metal and the electrolyte, the formation of lithium dendrites, and the rapid expansion and contraction of the volume of the negative electrode piece. Here, the rapid expansion and contraction of the volume of the negative electrode piece easily causes the peeling of the interface between the negative electrode piece and the adjacent structure, resulting in a large increase in impedance and a significant decrease in the safety and stability of the electrochemical device.

[0026] The present invention provides a negative electrode skeleton with a multi-layer structure, which has two or more layers, in which different porosity designs are adopted for each layer, such that the negative electrode skeleton layer closer to the current collector has a larger porosity, and the negative electrode skeleton layer further away from the current collector has a smaller porosity.

[0027] The structure of the negative electrode piece and its beneficial effects in the embodiment of the present invention will be described below with reference to FIGS.

[0028] The negative electrode piece of the present invention may have a single-sided structure or a double-sided structure. Here, the single-sided structure refers to a negative electrode skeleton described in the present invention being installed on only one side of a current collector, and the double-sided structure refers to a negative electrode skeleton described in the present invention being installed on both sides of a current collector. Figures 1 to 4 are plan views and cross-sectional views of a negative electrode piece having a single-sided structure according to some embodiments of the present invention.

[0029] 1 to 3 are schematic diagrams showing a preparation process of a negative electrode piece of the present invention. First, FIG. 1 shows a plan view of a punched negative electrode current collector 101. According to an embodiment of the present invention, the current collector 101 may be a common negative electrode current collector in the art, including but not limited to nickel foil, tin foil, copper foil, lithium foil, and lithium-coated copper foil.

[0030] As shown in FIG. 2, a first negative electrode skeleton layer 102 having a larger porosity is placed on the surface of a current collector 101 .

[0031] As shown in Fig. 3, the second negative electrode skeleton layer 103, which has a smaller porosity, is disposed on the surface of the first negative electrode skeleton layer 102. Here, in order to clearly show the layered structure of the negative electrode skeleton (i.e., to clearly show the first negative electrode skeleton layer 102 coated on the second negative electrode skeleton layer 103), Fig. 3 shows only a portion of the second negative electrode skeleton layer 103. In one or more embodiments of the present invention, the second negative electrode skeleton layer 103 should completely cover the surface of the first negative electrode skeleton layer 102.

[0032] Fig. 4 is a cross-sectional view of the negative electrode piece cut along the line AA' in Fig. 3. As shown in Fig. 4, the negative electrode piece of the present invention includes a current collector 101 and a negative electrode skeleton located on the current collector 101, and the negative electrode skeleton includes at least a first negative electrode skeleton layer 102 and a second negative electrode skeleton layer 103, the first negative electrode skeleton layer 102 is located between the current collector 101 and the second negative electrode skeleton layer 103, and the porosity of the first negative electrode skeleton layer 102 is greater than the porosity of the second negative electrode skeleton layer 103. According to the direction indicated by the arrow from inside to outside in Fig. 4, the first negative electrode skeleton layer 102 may be referred to as an inner layer, and the second negative electrode skeleton layer 103 may be referred to as an outer layer.

[0033] The pores in the first negative electrode skeleton layer 102 and the second negative electrode skeleton layer 103 are spaces prepared for the deposition of lithium metal. During the charge and discharge process of the electrochemical device, lithium metal, which is a negative electrode active material, is absorbed or released in the negative electrode skeleton constructed in the present invention, so that the violent volume change caused by the absorption and release of lithium ions can be mitigated and even eliminated, thereby effectively avoiding the peeling of the interface and improving the safety and stability of the electrochemical device.

[0034] In addition, the first negative electrode skeleton layer 102 has a larger porosity, which can provide a good conductive path for the transport of ions and electrons, and can improve the rate characteristics of the electrochemical device. In addition, the first negative electrode skeleton layer 102 has a higher specific surface area, which can effectively distribute the current during the charge and discharge process, reduce the current density, improve the uniformity of lithium deposition, and suppress the formation of lithium dendrites.

[0035] The second negative electrode skeleton layer 103 has a denser skeleton structure than the first negative electrode skeleton layer 102. The dense structure of the second negative electrode skeleton layer 103 provides at least the following advantages: (1) Like the first negative electrode skeleton layer 102, it provides space for lithium metal deposition during charging and discharging, and can greatly reduce or eliminate the severe volume change, reduce the current density, inhibit the growth of lithium dendrites, and increase the lithium deposition density. (2) It contributes to further forming a dense negative electrode protective layer on the surface of the second negative electrode skeleton layer, reduces the difficulty of forming the negative electrode protective layer, reduces the side reaction between the lithium metal and the electrolyte, further improves the strength and stability of the lithium metal negative electrode, and can improve the Coulombic efficiency and cycle life of the electrochemical device.

[0036] In some embodiments, the porosity of the first negative electrode skeleton layer is about 55% to about 90%.

[0037] In some embodiments, the porosity of the second negative electrode skeletal layer is about 10% to about 50%. In some embodiments, the porosity of the second negative electrode skeletal layer is about 20% to about 50%. In some embodiments, the porosity of the second negative electrode skeletal layer is about 20% to about 40%.

[0038] The porosity of the first negative electrode skeleton layer may be a nearly constant percentage or may be a percentage that varies within the above range. In some embodiments, when the porosity of the first negative electrode skeleton layer varies, it is preferable that the porosity decreases as the relative distance from the current collector increases. The porosity of the second negative electrode skeleton layer may be a nearly constant percentage or may be a percentage that varies within the above range. In some embodiments, when the porosity of the second negative electrode skeleton layer varies, it is preferable that the porosity decreases as the relative distance from the current collector increases.

[0039] In some embodiments, the total thickness of the negative electrode skeleton is about 5 μm to about 100 μm. In some embodiments, the thickness of the first negative electrode skeleton layer is about 1 μm to about 95 μm. In some embodiments, the thickness of the second negative electrode skeleton layer is about 0.1 μm to about 50 μm.

[0040] In some embodiments, the thickness of the negative electrode skeleton and the porosity of the negative electrode skeleton satisfy the following relationship: [Formula 1] JPEG0007581360000001.jpg1997[Formula 2] JPEG0007581360000002.jpg2180[Formula 3] JPEG0007581360000003.jpg1899[Formula 4] JPEG0007581360000004.jpg1684

[0041] Here, t is the total thickness of the negative electrode skeleton / μm, x is the distance (integral element) / μm from any plane of the negative electrode skeleton parallel to the current collector surface to the current collector surface, and p is the porosity of the negative electrode skeleton.

[0042] Here, the above formula 1 indicates that the cumulative thickness of the pores provided in the negative electrode skeleton is 5 μm to 50 μm. The above formula 1 may be understood to mean that the cumulative thickness of the lithium metal that can be deposited on the negative electrode skeleton is 5 μm to 50 μm. With reference to the arrows from the inside to the outside in FIG. 4, the above formula 2 indicates that the porosity of the negative electrode skeleton decreases from the inside to the outside. The above formula 3 indicates that the porosity of the negative electrode skeleton is 20% to 90%. The above formula 4 indicates that the thickness of the negative electrode skeleton is 5 μm to 100 μm. It should be noted that the porosity described in the present invention is calculated based on the material of the negative electrode skeleton itself, and does not include the lithium metal previously filled in the negative electrode skeleton before the first charge and discharge.

[0043] In some embodiments, the present invention provides a negative electrode skeleton having a porosity that gradually decreases from the inside to the outside, i.e., the thickness and porosity of the negative electrode skeleton satisfy the relationship described in the above formula (2). In some embodiments, the negative electrode skeleton described in the present invention further satisfies at least one of the above formulas (1), (3), and (4).

[0044] In some embodiments, the negative electrode piece further comprises lithium metal pre-occluded (i.e., pre-loaded) within the negative electrode skeleton as a negative electrode active material for an electrochemical device, wherein the amount of pre-occluded lithium metal is about 0.001 mg / cm 2 ~about 6mg / cm 2 "Pre-occluded" refers to lithium metal that is pre-occluded in the negative electrode skeleton before the negative electrode piece is first charged and discharged. In some embodiments, the amount of pre-occluded lithium metal is about 0.005 mg / cm. 2 ~about 3mg / cm 2 For example, the amount of pre-occluded lithium metal is about 0.005 mg / cm 2 , about 0.01mg / cm 2 , about 0.1mg / cm 2 , about 0.5mg / cm 2 , about 1mg / cm 2 , about 1.5mg / cm 2 , about 2mg / cm 2 , about 2.5mg / cm 2, and about 3 mg / cm 2 may be also possible.

[0045] FIG. 5 is a cross-sectional view of an anode piece having an anode skeleton according to the present invention disposed on either side of a current collector, according to some embodiments of the present invention.

[0046] 5, a first negative electrode skeleton layer 102 and a second negative electrode skeleton layer 103 are disposed on both surfaces of the current collector 101, and the first negative electrode skeleton layer 102 is located between the current collector 101 and the second negative electrode skeleton layer 103. In some embodiments, the negative electrode skeletons disposed on both sides of the current collector 101 may be two different negative electrode skeletons.

[0047] FIG. 6 is a cross-sectional view of an anode piece including more anode skeleton layers according to some embodiments of the present invention.

[0048] In some embodiments, the negative electrode piece of the present invention further includes at least one third negative electrode skeleton layer 104. The third negative electrode skeleton layer 104 is located on the surface of the second negative electrode skeleton layer 103, as shown in FIG.

[0049] It should be understood that Fig. 6 is a schematic embodiment in which the negative electrode skeleton of the present invention has a structure of more than two layers. Although Fig. 6 only shows a negative electrode skeleton having a three-layer structure, those skilled in the art can adjust the number of layers of the negative electrode skeleton layers in the negative electrode piece according to specific needs based on the teaching of the present invention, and are not limited to the number of layers of the negative electrode skeleton shown in the drawings of the present invention.

[0050] According to an embodiment of the present invention, the first negative electrode skeleton layer, the second negative electrode skeleton layer, and the third negative electrode skeleton layer each independently include at least one material selected from the group consisting of a polymer material, a carbon material, a metal material, and an inorganic material.

[0051] In some embodiments, the polymer material includes at least one of polyethylene oxide, polyimide, polyacrylic acid, polyethylene, polypropylene, polyacrylonitrile, polystyrene, polyvinyl fluoride, polyether ether ketone, polyester, polyvinylidene fluoride, polytetrafluoroethylene, polyethylene terephthalate, and one or more derivatives of the above polymer materials.

[0052] In some embodiments, the carbon material includes at least one of porous carbon, carbon nanotubes, carbon fibers, graphene and its derivatives, and hollow carbon spheres.

[0053] In some embodiments, the metal material includes at least one of copper, nickel, chromium, titanium, tungsten, zirconium, and an alloy composed of two or more of the above materials.

[0054] In some embodiments, the inorganic material is lithium phosphate (Li3PO4); LiPON; Li2O; LiF; LiOH; Li2CO3; LiAlO2; Li4SiO4; Li2O - Al2O3 - SiO2 - P2O5 - TiO2 - GeO2 ceramic; lithium titanium phosphate (Li x Ti y (PO4)3, where 0 < x < 2 and 0 < y < 3); lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, where 0 < x < 2, 0 < y < 1, and 0 < z < 3); Li 1+x+y (Al,Ga) x (Ti,Ge) 2-x Si y P 3-y O 12 , where 0 ≤ x ≤ 1 and 0 ≤ y ≤ 1; lithium lanthanum titanate (Li x La y TiO3, where 0 < x < 2 and 0 < y < 3); lithium germanium thiophosphate (Li x Ge y P z Sw , where 0 < x < 4, 0 < y < 1, 0 < z < 1, and 0 < w < 5); lithium nitride (Li x N y , where 0 < x < 4 and 0 < y < 2); SiS2 glass (Li x Si y S z , where 0 ≤ x < 3, 0 < y < 2, and 0 < z < 4); P2S5 glass (Li x P y S z , where 0 ≤ x < 3, 0 < y < 3, and 0 < z < 7); and garnet ceramic (Li 3+x La3M2O 12 , where 0 ≤ x ≤ 5, and M is at least one of Te, Nb, and Zr) includes at least one of them.

[0055] In some embodiments, the first negative electrode skeleton layer, the second negative electrode skeleton layer, and the third negative electrode skeleton layer are each independently made of a composite material, where the composite material is any combination of two or more of a polymer material, a carbon material, a metal material, and an inorganic material. For example, the negative electrode skeleton may include a basic skeleton prepared from a polymer material or a carbon material and an inorganic material further deposited on the basic skeleton. In some embodiments, the inorganic material coats the inner and outer surfaces of the porous structure of the material in the form of particles or a coating. In some embodiments, the inorganic material includes at least one of HfO2, SrTiO3, SnO2, CeO2, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, CuO, and AgO. In at least one aspect, the inorganic material serves as a deposition site to indicate that lithium is deposited inside the porous structure.

[0056] In some embodiments, the method for preparing the composite material may be a common preparation method in the art, including but not limited to atomic layer deposition technology (ALD) and electrochemical deposition methods.

[0057] In some embodiments, the negative electrode tab further includes one or more negative electrode protective layers located on the surface of the negative electrode skeleton. As shown in FIG. 7, one or more negative electrode protective layers 105 may be further formed on the surface of the second negative electrode skeleton layer 103. Literally, the negative electrode protective layer plays a role in protecting the negative electrode. For example, the negative electrode protective layer 105 can block the contact between the electrolyte and the lithium metal which is the negative electrode active material, greatly reduce the side reaction between the electrolyte and the lithium metal, and improve the cycle stability of the electrochemical device. Also, it should be noted that since the skeleton of the second negative electrode skeleton layer is denser than the porous structure of the first negative electrode skeleton layer, the difficulty of forming the negative electrode protective layer is reduced, which is advantageous for further forming a dense negative electrode protective layer on the surface of the negative electrode skeleton.

[0058] In some embodiments, the porosity of the negative electrode protective layer is from about 0% to about 10%.

[0059] In some embodiments, the material used for the negative electrode protective layer includes at least one of inorganic substances, silicon, metals, and organic substances.

[0060] In some embodiments, the inorganic substances include lithium phosphate (Li3PO4); LiPON; Li2O; LiF; LiOH; Li2CO3; LiAlO2; Li4SiO4; Li2O - Al2O3 - SiO2 - P2O5 - TiO2 - GeO2 ceramic; lithium titanium phosphate (Li x Ti y (PO4)3, where 0 < x < 2 and 0 < y < 3); lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, where 0 < x < 2, 0 < y < 1, and 0 < z < 3); Li 1+x+y (Al,Ga) x (Ti,Ge) 2-x Si y P 3-y O 12 , where 0 ≤ x ≤ 1 and 0 ≤ y ≤ 1; lithium lanthanum titanate (Li x La yTiO3, where 0 < x < 2 and 0 < y < 3); Lithium germanium thiophosphate (Li x Ge y P z S w , where 0 < x < 4, 0 < y < 1, 0 < z < 1, and 0 < w < 5); Lithium nitride (Li x N y , where 0 < x < 4 and 0 < y < 2); SiS2 glass (Li x Si y S z , where 0 ≤ x < 3, 0 < y < 2, and 0 < z < 4); P2S5 glass (Li x P y S z , where 0 ≤ x < 3, 0 < y < 3, and 0 < z < 7); and garnet ceramic (Li 3+x La3M2O 12 , where 0 ≤ x ≤ 5, and M is at least one of Te, Nb, and Zr)) includes at least one of them.

[0061] In some embodiments, the metal includes at least one of Au, Pt, Ag, Al, In, Sn, and an alloy composed of two or more of the above materials.

[0062] In some embodiments, the organic substance includes at least one of polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), polymethyl methacrylate (PMMA), polypropylene carbonate (PPC), polyethylene carbonate (PEC), polycaprolactone (PCL), tetraethylene glycol diacrylate (TEGDA), perfluorosulfonic acid resin (Nafion), polyacrylonitrile (PAN), polydimethylsiloxane (PDMS), and derivatives of the above organic substances.

[0063] Some embodiments of the present invention provide an electrochemical device comprising the negative electrode piece of the above embodiment. The electrochemical device further comprises a positive electrode piece and a separator located between the positive electrode piece and the negative electrode piece, and the positive electrode piece and the separator are not particularly limited and may be a positive electrode piece and a separator common in the art. In some embodiments, the electrochemical device is a lithium ion battery.

[0064] According to some embodiments of the present invention, the positive electrode piece includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, where the positive electrode active material layer includes a positive electrode active material, a conductive material, and a binder. In some embodiments, the positive electrode current collector includes, but is not limited to, aluminum foil or nickel foil.

[0065] In some embodiments, specific examples of the positive electrode active material include, but are not limited to, at least one of lithium cobalt oxide, lithium iron phosphate, lithium manganese iron phosphate, sodium iron phosphate, lithium vanadium phosphate, sodium vanadium phosphate, lithium vanadyl phosphate, sodium vanadyl phosphate, lithium vanadate, lithium manganate, lithium nickel oxide, lithium nickel cobalt manganate, lithium excess manganese-based materials, lithium nickel cobalt aluminate, and lithium titanate.

[0066] In the above positive electrode active material, the chemical formula of lithium cobalt oxide is Li a Co b M 1c O 2-dwhere M1 includes at least one of nickel (Ni), manganese (Mn), magnesium (Mg), aluminum (Al), boron (B), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zinc (Zn), molybdenum (Mo), tin (Sn), calcium (Ca), strontium (Sr), tungsten (W), yttrium (Y), lanthanum (La), zirconium (Zr), and silicon (Si), and the values ​​of a, b, c, and d are 0.8≦a≦1.2, 0.8≦b≦1, 0≦c≦0.2, and −0.1≦d≦0.2, respectively.

[0067] In the above positive electrode active material, the chemical formula of lithium nickel oxide is Li e Ni f M 2g O 2-h where M2 comprises at least one of cobalt (Co), manganese (Mn), magnesium (Mg), aluminum (Al), boron (B), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zinc (Zn), molybdenum (Mo), tin (Sn), calcium (Ca), strontium (Sr), tungsten (W), zirconium (Zr), and silicon (Si), and the values ​​of e, f, g, and h are 0.8≦e≦1.2, 0.3≦f≦0.98, 0.02≦g≦0.7, and −0.1≦h≦0.2, respectively.

[0068] In the above positive electrode active material, the chemical formula of lithium manganese oxide is Li i Mn 2-j M 3j O 4-k where M3 includes at least one of cobalt (Co), nickel (Ni), magnesium (Mg), aluminum (Al), boron (B), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zinc (Zn), molybdenum (Mo), tin (Sn), calcium (Ca), strontium (Sr), and tungsten (W), and the values ​​of i, j, and k are 0.8≦i≦1.2, 0≦j<1.0, and −0.2≦k≦0.2, respectively.

[0069] In the above positive electrode active material, the chemical formula of lithium nickel cobalt manganate is LiNi l Co m Mn n O2, where the values of l, m, and n are 0 < l < 1.0, 0 < m < 1.0, and 0 < n < 1.0, respectively, and l + m + n = 1.

[0070] In some embodiments, the conductive material includes at least one of conductive carbon black, carbon fiber, acetylene black, ketjen black, graphene, and carbon nanotube. It should be understood by those skilled in the art that various positive electrode plates widely used in lithium ion batteries can be applied to the present invention without limitation.

[0071] According to some embodiments of the present invention, the separator includes at least one of polyethylene, polypropylene, polyethylene terephthalate, polyimide, and aramid, but is not limited thereto. For example, polyethylene includes at least one of high density polyethylene, low density polyethylene, and ultra-high molecular weight polyethylene. In particular, polyethylene and polypropylene have excellent effects in preventing short circuits and can improve the stability of the battery by the shutdown effect. It should be understood by those skilled in the art that various separators widely used in lithium ion batteries can be applied to the present invention.

[0072] According to some embodiments of the present invention, the above lithium ion battery further includes an electrolyte, and the electrolyte may be in a gel state or a liquid state, and the electrolyte includes a lithium salt and a non-aqueous solvent.

[0073] In some embodiments, the lithium salt comprises at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, LiBOB, and lithium difluoroborate. For example, LiPF6 is selected as the lithium salt because it can provide high ionic conductivity and improve cycleability.

[0074] In some embodiments, the non-aqueous solvent may be a carbonate compound, a carboxylate compound, an ether compound, another organic solvent, or a combination thereof.

[0075] In some embodiments, the carbonate ester compound may be a linear carbonate ester compound, a cyclic carbonate ester compound, a fluorocarbonate ester compound, or a combination thereof.

[0076] In some embodiments, specific examples of the linear carbonate ester compound are diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, methylethyl carbonate, or a combination thereof.Specific examples of the cyclic carbonate ester compound are ethylene carbonate, propylene carbonate, butylene carbonate, vinylethylene carbonate, propyl propionate, or a combination thereof. Specific examples of the fluorocarbonate compound include fluoroethylene carbonate, 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate, and combinations thereof.

[0077] In some embodiments, examples of carboxylic acid ester compounds include methyl acetate, ethyl acetate, n-propyl acetate, t-butyl acetate, methyl propionate, ethyl propionate, gamma-butyrolactone, decanolactone, valerolactone, mevalonolactone, caprolactone, methyl formate, or combinations thereof.

[0078] In some embodiments, examples of ether compounds include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, or combinations thereof.

[0079] In some embodiments, examples of other organic solvents include dimethylsulfoxide, 1,2-dioxolane, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate, or combinations thereof.

[0080] Some embodiments of the present invention provide a method for preparing a lithium ion battery, including sequentially winding or stacking the above-mentioned positive electrode piece, separator and the negative electrode piece of the present invention into a cell, and then inserting the cell into, for example, an aluminum plastic film, injecting an electrolyte, forming and packaging the cell to obtain a lithium ion battery.

[0081] It should be understood by those skilled in the art that the cell structure and the preparation method of the lithium ion battery described above are merely exemplary examples, and other methods common in the art may be adopted to prepare the lithium ion battery or other electrochemical device without departing from the teachings of the present invention.

[0082] It should be understood by those skilled in the art that although the above description is based on the lithium ion battery, the electrochemical device of the present invention may further include any other suitable electrochemical device. Without departing from the scope of the present disclosure, the electrochemical device in the embodiments of the present invention may include any device in which an electrochemical reaction occurs, and examples thereof include any type of primary battery, secondary battery, solar cell, or capacitor. In particular, the electrochemical device is a lithium secondary battery, including a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.

[0083] The application of the electrochemical device of the present invention is not particularly limited, and can be used for any application known in the prior art. According to some embodiments of the present invention, the electronic device including the electrochemical device of the present invention includes, but is not limited to, notebook computers, pen-input computers, mobile computers, electronic book players, mobile phones, portable facsimiles, portable copy machines, portable printers, stereo headsets, video recorders, liquid crystal televisions, portable cleaners, portable CD players, mini discs, transceivers, electronic notebooks, calculators, memory cards, portable tape recorders, radios, backup power sources, motors, automobiles, motorcycles, auxiliary bicycles, bicycles, lighting equipment, toys, game machines, watches, power tools, flashlights, cameras, large household storage batteries, and lithium ion capacitors.

[0084] The technical solution of the present invention will be further described below with reference to comparative examples and specific examples, but is not limited thereto.Those skilled in the art should understand that the preparation methods described in the present invention are merely illustrative examples, and any modification or equivalent replacement of the technical solution of the present invention without departing from the scope of the technical solution of the present invention is also included in the protection scope of the present invention.

[0085] Specific Examples Preparation of positive electrode pieces The positive electrode active materials, lithium iron phosphate (LiFePO4), conductive carbon black (SuperP), and polyvinylidene fluoride (PVDF), were mixed in a weight ratio of 97.5:1.0:1.5, and N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 55% and stirred until uniform. The slurry was uniformly applied to an aluminum foil positive electrode current collector and dried at 90°C to obtain a positive electrode piece. The load of the positive electrode was 1 mAh / cm. 2 After the coating was completed, the pole piece was cut to a size of (38mm x 58mm) and kept as a spare.

[0086] Preparation of electrolyte First, dioxolane (DOL) and dimethyl ether (DME) were mixed in a volume ratio of 1:1 in a dry argon gas atmosphere, and then lithium bistrifluoromethanesulfonylimide (LiTFSI) was dissolved in an organic solvent as a lithium salt and mixed uniformly to obtain an electrolyte with a lithium salt concentration of 1M.

[0087] Preparation of Li-ion batteries Using a 15 μm thick polyethylene separator, the two-layer coated negative electrode pieces, separator, and one-layer coated positive electrode pieces in the examples and comparative examples were stacked in order. After stacking, the four corners of the stacked structure were fixed with tape, placed on an aluminum plastic film, top-side sealed, filled, and packaged to obtain the lithium metal stacked batteries of the following examples and comparative examples.

[0088] Materials and Lithium-ion Battery Testing Methods (1) Porosity measurement The framework to be measured was placed in an automatic mercury porosimeter (model number is AutoPoreV9610) and measured to obtain the porosity of the sample, where the pressure was 0.5-30,000 psia.

[0089] (2) Measurement of the thickness of the negative electrode skeleton layer The pole piece to be measured was cut to a size of approximately 10 mm x 5 mm, placed in an ion-exchange grinding and polishing machine to polish the cross section of the pole piece, and the obtained pole piece was transferred to a scanning electron microscope (SEM) to observe the polished cross section at an appropriate magnification and measure the thickness of the negative electrode skeleton layer.

[0090] (3) Measurement of the amount of lithium metal pre-deposition The pole piece to be measured was punched out into a wafer with a diameter of 14 mm to serve as the positive electrode. Copper foil was punched out into a wafer with a diameter of 18 mm to serve as the negative electrode. Polyethylene with a thickness of 15 μm and a diameter of 20 mm was used as a separator, and 60 μL of the above-mentioned electrolyte was poured into it to assemble it into a button battery. 0.1 mA / cm 2 The button battery was charged at a current density of 0 V and the charging voltage was 0 to 1 V. The amount of pre-deposited lithium metal per unit area was calculated from the measured charging capacity and the gram capacity of lithium of 3860 mAh / g.

[0091] (4) Measurement of cycle characteristics of lithium-ion batteries In order to perform formation on the stacked battery, the stacked battery was charged and discharged once at 60°C and a rate of 0.1C, and then the battery was subjected to a charge-discharge cycle at room temperature. Here, the battery was first charged at a constant current of 1C until the cutoff voltage was 3.8V, then the battery was charged at a constant voltage until the cutoff current was 0.05C, and then the battery was discharged at a constant current of 1C until the cutoff voltage was 2.7V. In the above manner, the number of cycles of the lithium ion batteries in the comparative example and the example was measured when the discharge capacity was 80% of the initial discharge capacity.

[0092] Preparation of negative electrode pieces Example 1 By electrospinning technology, polyacrylonitrile was used as a precursor to prepare two layers of polyacrylonitrile fiber layers, in which the porosity of the first negative electrode skeleton layer (i.e., the inner layer) was 70%, the thickness was 45 μm, and the porosity of the second negative electrode skeleton layer (i.e., the outer layer) was 30%, the thickness was 5 μm. The above two layers of polyacrylonitrile fiber layers were heated at a temperature of 210°C in an air environment for 1 hour, and then heated at a temperature of 900°C in an argon gas atmosphere for 3 hours to obtain a carbon membrane. The nickel foil, which is a current collector, the first negative electrode skeleton layer, and the second negative electrode skeleton layer were aligned in the manner shown in FIG. 5 of the present invention, and lithium foil was placed on the two outer surfaces of the negative electrode skeleton and heated to 300°C, and lithium was melted and inserted into the inside of the skeleton, and lithium was pre-absorbed. Finally, the pole pieces were cut into a size of (40 mm x 60 mm) and used as spares.

[0093] Example 2 The preparation method and raw materials in Example 2 were the same as those in Example 1, except that the porosity of the first negative electrode framework layer (ie, the inner layer) in Example 2 was 55%.

[0094] Example 3 The preparation method and raw materials in Example 3 were the same as those in Example 1, except that the porosity of the first negative electrode framework layer (ie, the inner layer) in Example 3 was 80%.

[0095] Example 4 The preparation method and raw materials in Example 4 were the same as those in Example 1, except that the porosity of the first negative electrode framework layer (ie, the inner layer) in Example 4 was 90%.

[0096] Example 5 The preparation method and raw materials in Example 5 were the same as those in Example 1, except that the porosity of the first negative electrode framework layer (ie, the inner layer) in Example 5 was 95%.

[0097] Example 6 The preparation method and raw materials in Example 6 were the same as those in Example 1, except that the porosity of the second negative electrode framework layer (ie, the outer layer) in Example 6 was 20%.

[0098] Example 7 The preparation method and raw materials in Example 7 were the same as those in Example 1, except that the porosity of the second negative electrode framework layer (ie, the outer layer) in Example 7 was 40%.

[0099] Example 8 The preparation method and raw materials in Example 8 were the same as those in Example 1, except that the porosity of the second negative electrode framework layer (ie, the outer layer) in Example 8 was 10%.

[0100] Comparative Example 1 The difference between Comparative Example 1 and Examples 1 to 8 is that the negative electrode skeleton was not provided, and the lithium metal was simply placed on the current collector, and the two were tightly bonded by roll pressing. The thickness of the pre-absorbed lithium metal was 10 μm.

[0101] Comparative Example 2 Comparative Example 2 was similar to the preparation method and raw materials of Example 1, except that only a negative electrode skeleton layer with a porosity of 30% and a thickness of 50 μm was provided on both surfaces of the current collector.

[0102] Comparative Example 3 Comparative Example 3 was similar to the preparation method and raw materials of Example 1, except that only a negative electrode skeleton layer with a porosity of 70% and a thickness of 50 μm was provided on both surfaces of the current collector.

[0103] The test parameters and measurement results for the above-mentioned Examples 1 to 8 and Comparative Examples 1 to 3 are shown in Table 1 below.

[0104] [Table 1]

[0105] When lithium is pre-absorbed in the negative electrode skeleton, the amount of pre-absorbed lithium is related to the porosity of the negative electrode skeleton. Usually, when the porosity of the negative electrode skeleton is low, the space for depositing lithium is small, so the amount of pre-absorbed lithium is correspondingly reduced. As shown in Table 1, the electrochemical devices prepared by using the negative electrode pieces of Examples 1 to 8 of the present invention have better cycle stability than the electrochemical devices prepared by using the negative electrode pieces of Comparative Examples 1 to 3. In Comparative Example 1, no framework was constructed for lithium metal, so the cycle stability of the obtained electrochemical device was the worst. In Comparative Examples 2 and 3, a single-layer framework was constructed for lithium metal (which may be understood as a framework of two layers with the same porosity), so the cycle stability of the obtained electrochemical device was improved to a certain extent compared to Comparative Example 1. However, in Examples 1 to 8 of the present invention, the framework of two layers with different porosities, in which the porosity of the inner layer is greater than that of the outer layer, was constructed, so that the cycle stability of the obtained electrochemical device was further improved compared to Comparative Examples 2 and 3.

[0106] In addition, it can be seen from the comparison between Example 5 and other Examples that the cycle stability of the electrochemical device obtained in Example 5 is relatively poor, mainly because the inner layer porosity of Example 5 is too large to provide strong support for the deposition of lithium metal. However, the cycle stability of the electrochemical device obtained in Example 5 is still superior to that of Comparative Examples 1 to 3.

[0107] Example 9 The first negative electrode skeleton layer (i.e., inner layer) was made of foamed copper with a porosity of 70%, and had a thickness of 45 μm. The second negative electrode skeleton layer (i.e., outer layer) was made of foamed copper with a porosity of 30%, and had a thickness of 5 μm. In the manner described in FIG. 5 of the present invention, the nickel foil as a current collector, the first negative electrode skeleton layer, and the second negative electrode skeleton layer were arranged, and lithium foil was placed on the two outer surfaces of the negative electrode skeleton, and heated to 300 degrees to melt the lithium and insert it into the skeleton, thereby performing pre-occlusion of lithium. Finally, the pole piece was cut into a size of (40 mm x 60 mm) and used as a spare.

[0108] Example 10 The preparation method and raw materials in Example 10 were the same as those in Example 9, except that the porosity of the first negative electrode framework layer (ie, the inner layer) in Example 10 was 80%.

[0109] Example 11 By electrospinning technology, two layers of polyimide fiber were prepared using polyimide as a precursor, the first negative electrode skeleton layer (i.e., inner layer) had a porosity of 70% and a thickness of 45 μm, and the second negative electrode skeleton layer (i.e., outer layer) had a porosity of 30% and a thickness of 5 μm. In the manner shown in FIG. 5 of the present invention, nickel foil as a current collector, the first negative electrode skeleton layer, and the second negative electrode skeleton layer were aligned, and lithium foil was placed on the two outer surfaces of the negative electrode skeleton and heated to 300 degrees, and lithium was melted and inserted into the skeleton, and pre-occlusion of lithium was performed. Finally, the pole piece was cut into a size of (40 mm x 60 mm) and used as a spare.

[0110] Example 12 The preparation method and raw materials in Example 12 were the same as those in Example 11, except that the porosity of the first negative electrode framework layer (ie, the inner layer) in Example 12 was 80%.

[0111] Example 13 A copper foam with a porosity of 70% was used as the first negative electrode skeleton layer (i.e., inner layer) with a thickness of 45 μm. A fiber layer with a porosity of 30% was prepared by electrospinning technology using polyacrylonitrile as a precursor to obtain a second negative electrode skeleton layer (i.e., outer layer) with a thickness of 5 μm. The polyacrylonitrile fiber layer was heated at a temperature of 210°C for 1 hour in an air environment, and then heated at a temperature of 900°C for 3 hours in an argon gas atmosphere to obtain a carbon film with a thickness of 5 μm. In the manner shown in FIG. 5 of the present invention, a nickel foil as a current collector, a first negative electrode skeleton layer, and a second negative electrode skeleton layer were aligned, and a lithium foil was placed on the two outer surfaces of the negative electrode skeleton and heated to 300°C to melt the lithium and insert it into the skeleton, thereby performing pre-occlusion of lithium. Finally, the pole piece was cut into a size of (40 mm x 60 mm) and used as a spare.

[0112] Example 14 The preparation method and raw materials in Example 14 were the same as those in Example 13, except that the porosity of the first negative electrode framework layer (ie, the inner layer) in Example 14 was 80%. The test parameters and measurement results for Examples 9 to 14 above are shown in Table 2 below.

[0113] [Table 2] The inner and outer layers of the negative electrode skeleton in Examples 1 to 8 are all prepared by adopting carbon materials. Unlike them, in Examples 9 to 14, the negative electrode skeleton is prepared by adopting a metal material (e.g., Cu) and a polymer material (e.g., polyimide). Compared with Comparative Example 1, the cycle characteristics of the electrochemical devices obtained in Examples 9 to 14 are all improved, because the negative electrode skeleton prepared from the metal material and the polymer material can provide a framework and support for the deposition of lithium metal, similar to the carbon material. However, when the negative electrode skeleton is prepared by adopting metallic Cu, the cycle stability of the obtained electrochemical device is slightly inferior to that of the electrochemical device adopting the negative electrode skeleton layer prepared from the carbon material and / or the polymer material. This is mainly because the wettability of Cu to lithium is poor, and lithium tends to be deposited on the surface of the pole piece during the electrochemical charge-discharge cycle, and the role of the negative electrode skeleton cannot be fully exerted. Adding a wetting / protection layer, such as an oxide layer, to the surface of Cu significantly improves the cycling stability of the electrochemical device (see, for example, the electrochemical data in Examples 16 and 18 below).

[0114] Example 15 Example 15 was an improvement on Example 1 based on Example 1. The specific improvement was that after the two polyacrylonitrile fiber layers were heated to obtain a carbon membrane, a zinc oxide coating having a thickness of 20 nm was applied to the inner and outer surfaces of the pore structure of the carbon membrane by atomic layer deposition technology.

[0115] Example 16 Example 16 was an improvement on Example 9 based on Example 9. The specific improvement was that the inner and outer surfaces of the pore structures of the two types of foamed copper materials were coated with a layer of aluminum oxide coating having a thickness of 20 nm by atomic layer deposition technology.

[0116] Example 17 Example 17 was an improvement on Example 11. The specific improvement was that a single layer of copper oxide coating having a thickness of 20 nm was applied to the inner and outer surfaces of the pore structure of the polyimide fiber layer by atomic layer deposition technology.

[0117] Example 18 Example 18 was an improvement over Example 13. The specific improvement was that a single layer of titanium dioxide coating having a thickness of 20 nm was applied to the inner and outer surfaces of the carbon film and the pore structure of the foamed copper by atomic layer deposition technology. The test parameters and measurement results for Examples 15 to 18 above are shown in Table 3 below.

[0118] [Table 3] In Examples 15 to 18, the inner and outer surfaces of the pore structure of the skeleton formed in Examples 1, 9, 11, and 13 are coated with an additional layer of inorganic material (e.g., ZnO, Al2O3, CuO, and TiO2). That is, the structure of the negative electrode skeleton in Examples 15 to 18 may be explained as a structure in which a basic negative electrode skeleton is formed by first adopting a carbon material / metal material / polymer material, and an inorganic material is further formed on the inner and outer surfaces of the pore structure of the basic negative electrode skeleton formed. That is, the negative electrode skeleton in Examples 15 to 18 is made of a composite material. And, when the electrochemical data of Examples 15 to 18 and Examples 1, 9, 11, and 13 are compared, it can be seen that the cycle stability of the electrochemical device can be further improved by further coating or depositing an inorganic material on the inner and outer surfaces of the pore structure of the skeleton.

[0119] Example 19 Example 19 was an improvement of Example 1 based on Example 1. Specifically, after pre-absorbing lithium, a LiF negative electrode protective layer having a thickness of 1 μm was deposited on the surface of the second negative electrode skeleton layer by magnetron sputtering. See FIG. 7 for a schematic diagram of the specific structure.

[0120] Example 20 Example 20 was an improvement on Example 19. Specifically, the improvement was achieved by applying a single layer of ZnO coating having a thickness of 20 nm to the inner and outer surfaces of the pore structure of the negative electrode skeleton by atomic layer deposition technology.

[0121] Examples 21 and 22 The difference between Examples 21 and 22 and Example 20 was that the materials of the negative electrode protective layer were changed to metal In and organic PEO, respectively.

[0122] Example 23 Example 23 was an improvement of Example 9 based on Example 9. Specifically, after lithium was pre-absorbed, a LiF negative electrode protective layer having a thickness of 1 μm was deposited on the surface of the second negative electrode skeleton layer by magnetron sputtering.

[0123] Example 24 Example 24 was an improvement of Example 23 based on Example 23. Specifically, the improvement was that a single layer of ZnO coating having a thickness of 20 nm was applied to the inner and outer surfaces of the pore structure of the negative electrode skeleton by atomic layer deposition technology.

[0124] Examples 25 and 26 The difference between Examples 25 and 26 and Example 24 was that the materials of the negative electrode protective layer were changed to metal In and organic PEO, respectively.

[0125] Example 27 Example 27 was an improvement of Example 11 based on Example 11. Specifically, after lithium was pre-absorbed, a LiF negative electrode protective layer having a thickness of 1 μm was deposited on the surface of the second negative electrode skeleton layer by magnetron sputtering.

[0126] Example 28 Example 28 was an improvement of Example 27 based on Example 27. Specifically, the improvement was that a single layer of ZnO coating having a thickness of 20 nm was applied to the inner and outer surfaces of the pore structure of the negative electrode skeleton by atomic layer deposition technology.

[0127] Examples 29 and 30 The difference between Examples 29 and 30 and Example 28 was that the materials of the negative electrode protective layer were changed to metal In and organic PEO, respectively.

[0128] Example 31 Example 31 was an improvement of Example 13 based on Example 13. Specifically, after lithium was pre-absorbed, a LiF negative electrode protective layer having a thickness of 1 μm was deposited on the surface of the second negative electrode skeleton layer by magnetron sputtering.

[0129] Example 32 Example 32 was an improvement on Example 31. Specifically, the improvement was achieved by applying a single layer of ZnO coating having a thickness of 20 nm to the inner and outer surfaces of the pore structure of the negative electrode skeleton by atomic layer deposition technology.

[0130] Examples 33 and 34 The difference between Examples 33 and 34 and Example 32 was that the materials of the negative electrode protective layer were changed to metal In and organic PEO, respectively. The test parameters and measurement results for the above Examples 19 to 34 are shown in Table 4 below.

[0131] [Table 4]

[0132] In Examples 19, 23, 27 and 31, a negative electrode protective layer was deposited on the surface of the negative electrode skeleton in Examples 1, 9, 11 and 13, respectively. Compared with Examples 1, 9, 11 and 13, the cycle stability of Examples 19, 23, 27 and 31 is further improved because the negative electrode protective layer can better protect the negative electrode skeleton and the negative electrode active material, reduce and even block the contact between the lithium metal and the electrolyte, greatly reduce the side reaction between the lithium metal and the electrolyte, and improve the cycle stability of the electrode and the electrochemical device.

[0133] Comparing Examples 20, 24, 28 and 32 with Examples 19, 23, 27 and 31, respectively, the improvement of the negative electrode pieces of Examples 20, 24, 28 and 32 is that a ZnO coating is further coated on the basic negative electrode skeleton. Also, comparing the electrochemical data, it can be seen that further depositing an inorganic material on the basic negative electrode skeleton is advantageous for further improving the cycle stability of the electrochemical device. Examples 21 and 22, Examples 25 and 26, Examples 29 and 30, and Examples 33 and 34 use metal materials and polymer materials as the negative electrode protective layer, respectively. From the electrochemical data of these examples, it can be seen that the use of metal materials and polymer materials can protect the negative electrode skeleton and the negative electrode active material as well as the use of inorganic materials.

[0134] As can be seen from the description of the examples and comparative examples described in the present invention, the present invention provides a new anode piece, and an electrochemical device and an electronic device including the same. Specifically, the present invention provides a two or more layers of anode skeleton layer for a lithium metal anode, in which the anode skeleton layer close to the current collector has a high porosity, and the anode skeleton layer away from the current collector has a low porosity. By adopting such a design, it is possible to reduce the side reaction between the lithium metal and the electrolyte, inhibit the formation of lithium dendrites, and greatly reduce or even eliminate the severe expansion and contraction of the volume of the anode piece due to the absorption and release of lithium ions, thereby improving the safety and stability of the electrochemical device.

[0135] In the present specification, references to "an embodiment," "some embodiments," "one embodiment," "another embodiment," "an example," "embodiment," or "some examples" mean that at least one embodiment or example of the embodiments of the invention includes a particular feature, structure, material, or characteristic described in that embodiment or example. Thus, the appearances of, for example, "in some embodiments," "in an embodiment," "in one embodiment," "in another embodiment," "an example," "in a particular example," or "an example" in various places throughout the specification do not necessarily refer to the same embodiment or example of the embodiments of the invention. Furthermore, particular features, structures, materials, or characteristics of the invention may be combined in any suitable manner in one or more embodiments or examples.

[0136] The above description of several embodiments can allow those skilled in the art to fully understand various aspects of the present invention, and those skilled in the art can easily design or modify the contents based on the present invention to achieve the same objectives and / or advantages as those of the embodiments of the present invention.

[0137] Although illustrative embodiments have been disclosed and described, those skilled in the art should understand that the above embodiments should not be construed as limiting the present invention, and that the embodiments can be modified, substituted, and altered without departing from the spirit, principle, and scope of the present invention.

Claims

1. A negative electrode piece, A current collector; a negative electrode skeleton located on the current collector, The negative electrode skeleton includes at least a first negative electrode skeleton layer and a second negative electrode skeleton layer, the first negative electrode skeleton layer is located between the current collector and the second negative electrode skeleton layer, and the porosity of the first negative electrode skeleton layer is greater than the porosity of the second negative electrode skeleton layer, The negative electrode piece further includes one or more negative electrode protective layers positioned on the negative electrode skeleton, The porosity of the negative electrode protective layer is 0% to 10%. Negative pole piece.

2. The negative electrode piece according to claim 1 , wherein the porosity of the first negative electrode skeleton layer is 55% to 90%.

3. The negative electrode piece according to claim 1 , wherein the porosity of the second negative electrode skeleton layer is 10% to 50%.

4. The negative electrode further includes lithium metal occluded in the skeleton, the amount of the lithium metal being 0.001 to 6 mg / cm 2 The negative electrode piece of claim 1 .

5. The negative electrode piece according to claim 1 , wherein the first negative electrode skeleton layer and the second negative electrode skeleton layer each independently include at least one material selected from the group consisting of a polymer material, a carbon material, a metal material, and an inorganic material.

6. the polymeric material comprises at least one of polyethylene oxide, polyimide, polyacrylic acid, polyethylene, polypropylene, polyacrylonitrile, polystyrene, polyvinyl fluoride, polyether ether ketone, polyester, polyvinylidene fluoride, polytetrafluoroethylene, polyethylene terephthalate, and derivatives of one or more of the above materials; The carbon material includes at least one of porous carbon, carbon nanotubes, carbon fibers, graphene and its derivatives, and hollow carbon spheres; The metal material includes at least one of copper, nickel, chromium, titanium, tungsten, zirconium, and an alloy of two or more of the above materials; The inorganic material is Li 3 PO 4 ; LiPON; Li 2 O; LiF; LiOH; Li 2 CO 3 ; LiA-O 2 ; Li 4 SiO 4 , Li 2 O-Al 2 O 3 -SiO 2 -P 2 O 5 -TiO 2 -GeO 2 ceramic; Li x Ti y (P.O. 4 ) 3 , where 0<x<2 and 0<y<3; Li x A y Ti z (P.O. 4 ) 3 , where 0<x<2, 0<y<1, and 0<z<3; Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x S y P 3-y O 12 , where 0≦x≦1 and 0≦y≦1; Li x La y TiO 3 , where 0<x<2 and 0<y<3; Li x Ge y P z S w , where 0<x<4, 0<y<1, 0<z<1, and 0<w<5; Li x N y , where 0<x<4 and 0<y<2; Li x S y S z , where 0≦x<3, 0<y<2, and 0<z<4; Li x P y S z , where 0≦x<3, 0<y<3, and 0<z<7; and Li 3+x La 3 M 2 O 12 where 0≦x≦5 and M is at least one of Te, Nb, and Zr; The negative electrode piece of claim 5 , comprising at least one of:

7. 10. The negative electrode piece of claim 1, wherein the negative electrode skeleton further comprises an inorganic material deposited on the negative electrode skeleton.

8. The inorganic material is HfO 2 , SrTiO 3 , SnO 2 , CeO 2 , MgO, NiO, CaO, BaO, ZnO, ZrO 2 , Y 2 O 3 , Al 2 O 3 , TiO 2 , SiO 2 8. The anode pole piece of claim 7, comprising at least one of the following: MnO, CuO, and AgO.

9. The anode piece according to claim 1 , wherein the material used for the anode protection layer includes at least one of inorganic, silicon, metal, and organic materials.

10. The inorganic substance is Li 3 PO 4 ; LiPON; Li 2 O; LiF; LiOH; Li 2 CO 3 ; LiA-O 2 ; Li 4 SiO 4 , Li 2 O-Al 2 O 3 -SiO 2 -P 2 O 5 -TiO 2 -GeO 2 ceramic; Li x Ti y (P.O. 4 ) 3 , where 0<x<2 and 0<y<3; Li x A y Ti z (P.O. 4 ) 3 , where 0<x<2, 0<y<1, and 0<z<3; Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x S y P 3-y O 12 , where 0≦x≦1 and 0≦y≦1; Li x La y TiO 3 , where 0<x<2 and 0<y<3; Li x Ge y P z S w , where 0<x<4, 0<y<1, 0<z<1, and 0<w<5; Li x N y , where 0<x<4 and 0<y<2; Li x S y S z , where 0≦x<3, 0<y<2, and 0<z<4; Li x P y S z , where 0≦x<3, 0<y<3, and 0<z<7; and Li 3+x La 3 M 2 O 12 where 0≦x≦5 and M is at least one of Te, Nb, and Zr; At least one of the following is included: The metal includes at least one of Au, Pt, Ag, Al, In, Sn, and an alloy of two or more of the above materials; 10. The anode piece of claim 9, wherein the organic material comprises at least one of PEO, PVDF, PMMA, PPC, PEC, PCL, TEGDA, Nafion, PAN, PDMS, and derivatives of the above organic materials.

11. An electrochemical device comprising a negative electrode piece according to any one of claims 1-10.

12. An electronic device comprising the electrochemical device of claim 11.

Citation Information

Patent Citations

  • Lithium secondary battery and its manufacturing method

    JP2003077542A

  • Anode for lithium-ion secondary battery and lithium-ion secondary battery

    JP2010160984A

  • Nonaqueous electrolyte secondary battery and secondary battery module

    JP2021150062A