Method for producing high-rate lithium iron phosphate cathode material
The novel high-temperature solid phase process for lithium iron phosphate cathode materials addresses the issue of large primary particles by producing spherical particles with 100 nm size and uniform distribution, achieving high discharge capacity and cycle stability.
Patent Information
- Application Number
- JP2022577335
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-09
- Filing Date
- 2022-07-08
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-07-08
Smart Images

Figure 0007581611000001 
Figure 0007581611000002 
Figure 0007581611000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of lithium batteries, and more particularly to the preparation of positive electrode materials for lithium ion batteries, and more particularly to the preparation of high-rate lithium iron phosphate positive electrode materials.
[0002] <Cross reference> This application claims priority to a Chinese patent application filed with the China Patent Office on October 9, 2021, with application number 202111175470.8 and titled "Method for manufacturing high-rate lithium iron phosphate positive electrode material," the entire contents of which are incorporated herein by reference. [Background technology]
[0003] Traditional lead-acid batteries have mature technology and low cost, but their mass and volume energy density is low, cycle life is short, and there is a risk of lead pollution in the industrial chain. On the other hand, the positive electrode material for lithium-ion batteries, such as polyanion lithium iron phosphate, represented by lithium iron phosphate, has the advantages of high theoretical capacity, good thermal stability, good cycle performance, stable structure, and environmental friendliness, and has attracted great attention, especially in the fields of power batteries and idling stop power supplies. As the technology of lithium iron phosphate becomes more and more mature, lithium iron phosphate will be increasingly widely used in the field of start-stop power supplies to replace lead-acid batteries.
[0004] The synthesis methods of lithium iron phosphate positive electrode materials can be divided into five types: high temperature solid-state method, carbothermal reduction method, microwave synthesis method, sol-gel method and hydrothermal / solvothermal method. The hydrothermal / solvothermal method and high temperature solid-state method are the main methods used to synthesize lithium iron phosphate. The lithium iron phosphate material produced by the hydrothermal / solvothermal method has the advantages of complete crystal structure, no impurity peak, uniform particle size, and uniform carbon coating layer on the particle surface, but the production process is complicated, the lithium source consumption is relatively large, the cost is high, and the reaction temperature during the production of lithium iron phosphate by the hydrothermal / solvothermal method is low, which makes it easy to generate antisite defects in the material crystal lattice.
[0005] The high-temperature solid-state method is a method in which a lithium source, an iron source, a phosphorus source, a carbon source and pure water are mixed in a certain ratio and thoroughly polished, then pyrolyzed by high-temperature spraying to obtain a pale yellow precursor powder, which is then reacted at high temperature for a certain period of time under a protective atmosphere to obtain lithium iron phosphate with good crystallinity. This method has the advantages of low cost, simple process route, good product stability, uniform carbon coating, and easy large-scale industrial production, but it also has the disadvantages of large primary particles, non-uniform particle size, long lithium ion diffusion distance, low diffusion coefficient, and significant limitations in the application to high-power start-stop power sources. Therefore, investigating and solving the above problems has become the direction of further research into the high-temperature solid-state method. Summary of the Invention [Problem to be solved by the invention]
[0006] In order to solve the problem that the primary particles of the lithium iron phosphate positive electrode material produced by the above-mentioned high-temperature solid-phase method are large and tend to be non-uniform, the present invention proposes a new high-rate lithium iron phosphate positive electrode material and a method for producing the same. [Means for solving the problem]
[0007] The present invention is realized in the following manner. The high-rate lithium iron phosphate material has a substantially spherical shape, with the primary particle size being 100 nm.
[0008] The anhydrous iron phosphate used in the high-rate lithium iron phosphate positive electrode material has a honeycomb structure and its BET is 9 to 11 m. 2 / g.
[0009] In the above-mentioned high-rate lithium iron phosphate positive electrode material, the precursor powder and a lithium source are thoroughly mixed, the molar ratio of the iron source to the lithium source is 1:1 to 1:1.05, and the mass of the carbon source is 5 to 15% of the total mass of the iron source and the lithium source.
[0010] In the method for preparing the lithium iron phosphate cathode material, the carbon source is one or more of glucose, PEG2000, PEG6000, white sugar, and citric acid.
[0011] In the method for producing the lithium iron phosphate positive electrode material, the final particle size D50 of the slurry after sand milling is controlled to be 100 to 200 nm.
[0012] In the method for producing the lithium iron phosphate positive electrode material, the precursor is sintered at a high temperature of 650 to 700° C. under the protection of a nitrogen atmosphere. In the following preferred embodiment of the present invention, the conditions such as the excess coefficient of the lithium source, the type of the carbon source, the particle size D50 of the sand mill, and the temperature of the high-temperature sintering are limited.
[0013] In the method for producing the lithium iron phosphate positive electrode material, A step of weighing out a predetermined amount of iron phosphate and lithium carbonate in a molar ratio of 1:1 to 1:1.05, collecting a carbon source compound in an amount of 10% based on the total mass of the phosphorus source and lithium source materials, and preparing a slurry with a solid content of 40%; ball milling the slurry for 2 hours to uniformly mix the slurry; A step of finely pulverizing the ball-milled slurry in a sand mill so as to control the final particle size D50 after sand milling to 100 to 200 nm; a step of spray-drying the slurry after the sand milling is completed at a spray air temperature of 240 to 280°C and a spray exhaust temperature of 80 to 95°C to obtain a pale yellow precursor powder; The precursor powder is placed in a graphite sagger, sintered at a high temperature of 650-700° C. for 18-20 hours under the protection of a nitrogen atmosphere, and then naturally cooled.
[0014] The sintered material is pulverized in a jet mill so that the pulverized particle size D50 is controlled to 0.4 to 1.5 μm, and then sieved to remove iron using an electric current, to obtain a high-rate lithium iron phosphate positive electrode material. Effect of the Invention
[0015] The beneficial effects of the present invention are as follows: According to the high-temperature solid-phase method of the present invention, a lithium iron phosphate precursor having a substantially spherical shape and a primary particle diameter of 100 nm is produced. When the characteristics of the XRD spectrum of the produced lithium iron phosphate material were examined, a characteristic peak of lithium iron phosphate appeared, and no impurity peak was observed. A CR2032 button-type half cell was assembled using the produced material. When the electrical characteristics of the CR2032 button-type half cell were measured, the produced substantially spherical lithium iron phosphate positive electrode material reached an initial discharge specific capacity of 161 mAh / g at room temperature under a current of 0.1 C and an initial discharge specific capacity of 140 mAh / g at a current of 10 C, and the capacity retention rate after 17,878 operating cycles at 25° C. was 95% or more. As shown in FIG. 8, the material of Example 1 has a capacity retention rate of 90% or more after 11,922 operating cycles at 45° C., and has good rate capability and cycle stability.
[0016] The material produced by the present invention has a perfect crystal structure, is free of impurity peaks, and has good discharge capacity and cycle performance. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is an XRD pattern of the lithium iron phosphate positive electrode material of Example 1 of the present invention. [Diagram 2] FIG. 2 is a SEM image of the lithium iron phosphate positive electrode material of Example 1 of the present invention. [Diagram 3] FIG. 3 is a diagram showing the initial charge / discharge curve at 0.1 C of the lithium iron phosphate positive electrode material of Example 1 of the present invention. [Figure 4] FIG. 4 is a particle size distribution curve diagram of the lithium iron phosphate positive electrode material of Example 1 of the present invention in the cases of 0.5C charge, 0.5C discharge, 0.5C charge, 1C discharge / 0.5C charge, 0.5C discharge / 2C charge, 0.5C discharge / 5C charge, and 10C discharge. [Diagram 5]FIG. 5 is a particle size distribution curve diagram of the lithium iron phosphate positive electrode material of Example 2 of the present invention in the cases of 0.5C charge, 0.5C discharge, 0.5C charge, 1C discharge / 0.5C charge, 0.5C discharge / 2C charge, 0.5C discharge / 5C charge, and 10C discharge. [Figure 6] FIG. 6 is a particle size distribution curve diagram of the lithium iron phosphate positive electrode material of Example 3 of the present invention in the cases of 0.5C charge, 0.5C discharge, 0.5C charge, 1C discharge / 0.5C charge, 0.5C discharge / 2C charge, 0.5C discharge / 5C charge, and 10C discharge. [Figure 7] FIG. 7 is a diagram showing the operation cycle curve of the lithium iron phosphate positive electrode material of Example 1 in the present invention at 25° C. [Figure 8] FIG. 8 is a diagram showing the operation cycle curve of the lithium iron phosphate positive electrode material of Example 1 in the present invention at 45° C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The technical solution of the present invention will be described clearly and completely below with reference to the embodiments of the present invention, but it is clear that the described embodiments are only some of the embodiments of the present invention, not all of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative efforts belong to the protection scope of the present invention.
[0019] The high-rate lithium iron phosphate positive electrode material according to the present invention has a substantially spherical shape with a primary particle diameter of 100 nm, and was specifically produced by the following method.
[0020] First, iron phosphate and lithium carbonate materials were weighed out in a molar ratio of 1:1 to 1:1.05, then 5 to 15% of the carbon source relative to the total mass of the iron source and lithium source materials, and 0 to 1% of the metal ion dopant relative to the total mass of the iron source and lithium source materials were weighed out, and pure water was added to them to prepare a slurry with a solid content of 40%. This slurry was ball milled and sand milled so that the D50 particle size was controlled to 100 to 200 nm, so that the raw materials such as the iron source, lithium source, phosphorus source, and carbon source were thoroughly mixed. Furthermore, the obtained slurry was dried by centrifugal spraying to obtain a pale yellow precursor powder. The precursor was placed in a graphite sagger and sintered at a high temperature for 18 to 20 hours under the protection of a nitrogen atmosphere at a temperature of 650 to 700 ° C. After natural cooling, it was pulverized with a jet mill to remove iron, and a high-rate lithium iron phosphate positive electrode material was obtained.
[0021] However, the iron source and phosphorus source have a honeycomb structure and a BET value of 9 to 11 m. 2 Anhydrous iron phosphate having a molecular weight of 1.001 mg / g was used. Battery grade lithium carbonate with a main content of ≥99.7% was used as the lithium source. As the carbon source, one or more of glucose, PEG2000, PEG6000, white sugar, and citric acid were used. As the metal ion dopant, one or more of nano titanium dioxide and zirconium dioxide were used.
[0022] In the present invention, a spherical lithium iron phosphate precursor was prepared by a high-temperature solid-state method, and the precursor was sintered to obtain a roughly spherical lithium iron phosphate cathode material with a primary particle size of 100 nm. The prepared material has a perfect crystal structure, no impurity peaks, and good discharge capacity and cycle performance. EXAMPLES
[0023] <Example 1> First, 25g of anhydrous iron phosphate, 6.3g of lithium carbonate, 2.64g of glucose, 0.32g of PEG2000, and 0.25g of titanium dioxide were weighed, and the above raw materials were dispersed in 5.3g of deionized water, and then ball milled for 2 hours. After that, the raw materials such as iron source, lithium source, carbon source, and metal ion dopant were sand milled to control the particle size D50 to 100-200nm, and the raw materials were thoroughly and uniformly mixed, and further dried by centrifugal spraying to obtain a pale yellow precursor powder. The precursor was placed in a graphite sagger and sintered at a high temperature for 18-20 hours under the protection of a nitrogen atmosphere at a temperature of 650-700 ° C. After natural cooling, it was pulverized with a jet mill to remove iron, and a high-rate lithium iron phosphate positive electrode material was obtained.
[0024] <Example 2> First, 25g of anhydrous iron phosphate, 6.3g of lithium carbonate, 3.8g of sucrose, 0.78g of PEG2000, and 0.25g of titanium dioxide were weighed, and the above raw materials were dispersed in 5.3g of deionized water, and ball milled for 2 hours, and then sand milled in a sand mill so that the particle size D50 was controlled to 100-200nm. The raw materials such as iron source, lithium source, carbon source, and metal ion dopant were thoroughly and uniformly mixed, and further dried by centrifugal spraying to obtain a pale yellow precursor powder. The precursor was placed in a graphite sagger and sintered at a high temperature for 18-20 hours under the protection of a nitrogen atmosphere at a temperature of 650-700 ° C. After natural cooling, it was pulverized in a jet mill to remove iron, and a high-rate lithium iron phosphate positive electrode material was obtained.
[0025] <Example 3> First, 25g of anhydrous iron phosphate, 6.3g of lithium carbonate, 5.68g of citric acid, and 0.13g of titanium dioxide were weighed, and the above raw materials were dispersed in 5.3g of deionized water, and then ball milled for 2 hours. After that, the raw materials were sand milled in a sand mill so that the particle size D50 was controlled to 100-200nm. The raw materials such as the iron source, lithium source, carbon source, and metal ion dopant were thoroughly and uniformly mixed, and further dried by centrifugal spraying to obtain a pale yellow precursor powder. The precursor was placed in a graphite sagger and sintered at a high temperature for 18-20 hours under the protection of a nitrogen atmosphere at a temperature of 650-700°C. After natural cooling, it was pulverized in a jet mill to remove iron, and a high-rate lithium iron phosphate positive electrode material was obtained.
[0026] <Example 4> First, 25g of anhydrous iron phosphate, 6.3g of lithium carbonate, 5.68g of glucose, 0.32g of PEG2000, and 0.31g of zirconium dioxide were weighed, and the above raw materials were dispersed in 5.3g of deionized water, and ball milled for 2 hours, and then sand milled in a sand mill so that the particle size D50 was controlled to 100-200nm. The raw materials such as iron source, lithium source, carbon source, and metal ion dopant were thoroughly and uniformly mixed, and further dried by centrifugal spraying to obtain a pale yellow precursor powder. The precursor was placed in a graphite sagger and sintered at a high temperature for 18-20 hours under the protection of a nitrogen atmosphere at a temperature of 650-700 ° C. After natural cooling, it was pulverized in a jet mill to remove iron, and a high-rate lithium iron phosphate positive electrode material was obtained.
[0027] The lithium iron phosphate material produced in Example 1 was characterized using a Nippon Rigaku type X-ray powder diffractometer (XRD), and as a result, the XRD spectrum showed peaks characteristic of lithium iron phosphate, but no impurity peaks, as shown in Figure 1. The lithium iron phosphate material produced in Example 1 was characterized using a Zeiss Sigma500 field emission scanning electron microscope (SEM), and as a result, the lithium iron phosphate material produced in Example 1 was in the form of nearly spherical particles, with the primary particle size being 100 nm, as shown in Figure 2.
[0028] The lithium iron phosphate positive electrode material prepared in Example 1, conductive carbon powder and PVDF binder were mixed in a mass ratio of 90:5:5, homogenized, coated on an aluminum foil sheet, dried at 100°C, rolled with a pair of rollers, and then punched to obtain an electrode sheet with a diameter of 14 mm. The electrode sheet was then weighed and the mass of the aluminum foil was subtracted to obtain the mass of the active material. After drying, a CR2032 button half cell was assembled in a German Braun UNlab type inert gas glove box in the order of anode shell, lithium sheet, electrolyte, separator, electrolyte, piece, gasket, connector, and cathode shell. The electrochemical performance of the CR2032 button half cell was measured using a Wuhan LAND Electronics Co., Ltd. CT2001A battery test system with a voltage range of 2.0 to 3.9 V, and the results are shown in Figures 3 and 4. As shown in FIG. 3, the lithium iron phosphate positive electrode material produced in Example 1 reached an initial discharge capacity of 161 mAh / g at room temperature under a current of 0.1 C. As shown in FIG. 4, the lithium iron phosphate positive electrode material produced in Example 1 reached a discharge capacity of 140 mAh / g at 10 C under a charge current of 0.5 C at room temperature. As shown in FIG. 5, the lithium iron phosphate positive electrode material produced in Example 2 reached a discharge capacity of 135 mAh / g at 10 C under a charge current of 0.5 C at room temperature. As shown in FIG. 6, the lithium iron phosphate positive electrode material produced in Example 3 reached a discharge capacity of 124 mAh / g at 10 C under a charge current of 0.5 C at room temperature. As shown in FIG. 7, the material of Example 1 had a capacity retention rate of 95% or more after 17,878 operating cycles at 25° C. As shown in FIG. 8, the material of Example 1 had a capacity retention rate of 90% or more after 11,922 operating cycles at 45° C., and had excellent rate performance and cycle performance.
[0029] It should be noted that the above is only a preferred embodiment of the present invention, and a person skilled in the art may make some improvements and modifications without departing from the principles of the present invention, and these improvements and modifications are also included in the protection scope of the present invention.
Claims
1. A method for producing a high-rate lithium iron phosphate cathode material, comprising: The lithium iron phosphate positive electrode material has a micro-morphology of approximately spherical particles, and the primary particle diameter of the lithium iron phosphate positive electrode material is 100 nm; The method for producing the lithium iron phosphate positive electrode material is a high-temperature solid-state method, A step A of adding pure water to an iron source and a lithium source weighed out in a predetermined molar ratio, a carbon source and a metal ion dopant weighed out in a predetermined amount, and ball milling the mixture to prepare a slurry having a predetermined solid content; A step B of sand milling the slurry after ball milling in a sand mill so as to control the particle diameter within a predetermined range; Step C of spraying the slurry after sand milling to obtain a pale yellow precursor powder; A step D of sintering the precursor powder at high temperature in a sintering furnace under nitrogen protection and obtaining a sintered material after cooling; and a step E of crushing the sintered material, sieving it to remove iron, and then obtaining lithium iron phosphate; The iron source selected in the step A is anhydrous iron phosphate, has a honeycomb structure, and has a BET value of 9 to 11 m. 2 / g, In the step B, the D50 of the slurry after sand milling is controlled to 100 to 200 nm; In the step D, the precursor powder is sintered at a high temperature of 650 to 700° C. for 18 to 20 hours under nitrogen protection.
2. 2. The method for producing a lithium iron phosphate positive electrode material according to claim 1, wherein the molar ratio of the iron source to the lithium source in step A is 1:1 to 1:1.
05.
3. 2. The method for producing a lithium iron phosphate positive electrode material according to claim 1, wherein the carbon source in step A is one or more selected from the group consisting of glucose, PEG 2000, PEG 6000, white sugar, and citric acid.
4. 2. The method for producing a lithium iron phosphate positive electrode material as claimed in claim 1, wherein the metal ion dopant in step A is one of titanium dioxide, zirconium dioxide.
5. 2. The method for producing a lithium iron phosphate positive electrode material according to claim 1, wherein in the step C, the blowing temperature of the spray is 240 to 280° C., and the exhaust temperature of the spray is 80 to 95° C.
6. 2. The method for producing a lithium iron phosphate positive electrode material according to claim 1, wherein in the step E, the D50 of the sintered material after pulverization is controlled to 0.4 to 1.5 μm.
Citation Information
Patent Citations
Preparation method and application of lithium iron phosphate positive electrode material
CN107814372A
Preparation method of high-capacity lithium-ion battery cathode material lithium iron phosphate
CN111313010A
Manufacturing method of iron lithium phosphate powder for electrode
JP2009070666A
Positive electrode active material substance for lithium secondary battery, method for manufacturing the same, and lithium secondary battery using the same
JP2012195156A
Production method of olivine-type lithium transition metal complex oxide