Positive electrode for energy storage element and energy storage element
By optimizing the pore diameter distribution in the positive electrode active material layer, the increase in current collection resistance during charge/discharge cycles is mitigated, improving the performance and durability of power storage elements.
Patent Information
- Application Number
- JP2020174228
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-15
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-10-15
AI Technical Summary
Conventional positive electrodes in power storage elements experience an increase in current collection resistance due to charge/discharge cycles, primarily attributed to an increase in electronic resistance within the active material layer.
The positive electrode active material layer is designed with a specific pore diameter distribution, where the sum of the maximum differential pore volumes in the ranges of 0.04 μm to 0.1 μm and 0.1 μm to 1.0 μm is maintained at 0.60 cm³/g or more, ensuring good dispersibility and maintaining conductive paths between active materials.
This design effectively suppresses the increase in current collection resistance during charge/discharge cycles, enhancing the performance and longevity of the power storage element.
Smart Images

Figure 0007581762000002 
Figure 0007581762000003 
Figure 0007581762000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode for an energy storage element and an energy storage element. [Background technology]
[0002] Non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc., due to their high energy density. The non-aqueous electrolyte secondary batteries generally have a pair of electrodes electrically isolated by a separator and a non-aqueous electrolyte interposed between the electrodes, and are configured to charge and discharge by transferring ions between the electrodes. In addition, capacitors such as lithium ion capacitors and electric double layer capacitors are also widely used as storage elements other than non-aqueous electrolyte secondary batteries.
[0003] It is known that in the positive electrode of such a storage element, the output characteristics of the battery can be improved by setting the pore diameter of the positive electrode mixture layer or the pore volume per unit weight of the positive electrode active material in the positive electrode mixture layer within a predetermined range (see Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. WO2006 / 129756 Summary of the Invention [Problem to be solved by the invention]
[0005] On the other hand, it is desirable that the internal resistance of an electric storage element does not increase even when the charge / discharge cycle is repeated. However, in an electric storage element using a positive electrode having a conventional positive electrode active material layer, the current collection resistance may increase with the charge / discharge cycle, and further improvement is required with respect to suppressing the increase in the current collection resistance, one of the causes of which is an increase in electronic resistance in the positive electrode active material layer.
[0006] The present invention has been made in view of the above circumstances, and has an object to provide a positive electrode for an electricity storage element that can suppress an increase in current collection resistance that accompanies charge / discharge cycles of the electricity storage element. [Means for solving the problem]
[0007] A positive electrode for an electric storage element according to one aspect of the present invention includes a positive electrode active material layer containing a positive electrode active material and a conductive agent, and in a Log differential pore volume distribution of the positive electrode active material layer, when a maximum value of the differential pore volume in a pore diameter range of 0.04 μm or more and 0.1 μm or less is defined as A and a maximum value of the differential pore volume in a pore diameter range of more than 0.1 μm and 1.0 μm or less is defined as B, the sum of A and B is 0.60 cm 3 / g or more. Effect of the Invention
[0008] A positive electrode for an energy storage device according to one aspect of the present invention can suppress an increase in current collection resistance that occurs with charge / discharge cycles of the energy storage device. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a perspective view showing an embodiment of an energy storage element. [Diagram 2] FIG. 2 is a schematic diagram showing an embodiment of an electricity storage device configured by assembling a plurality of electricity storage elements. [Diagram 3] FIG. 3 is a graph showing the relationship between the total maximum differential pore volume and the rate of increase in AC resistance after charge-discharge cycling. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] First, an overview of the positive electrode for an energy storage device and the energy storage device disclosed in this specification will be described.
[0011] A positive electrode for an electric storage element according to one aspect of the present invention includes a positive electrode active material layer containing a positive electrode active material and a conductive agent, and in a Log differential pore volume distribution of the positive electrode active material layer, when a maximum value of the differential pore volume in a pore diameter range of 0.04 μm or more and 0.1 μm or less is defined as A and a maximum value of the differential pore volume in a pore diameter range of more than 0.1 μm and 1.0 μm or less is defined as B, the sum of A and B is 0.60 cm 3 / g or more.
[0012] In the positive electrode for an energy storage element, in the Log differential pore volume distribution of the positive electrode active material layer, the sum of the maximum value A of the differential pore volume in the pore diameter range of 0.04 μm or more and 0.1 μm or less (hereinafter also referred to as the first range) and the maximum value B of the differential pore volume in the pore diameter range of more than 0.1 μm and 1.0 μm or less (hereinafter also referred to as the second range) is 0.60 cm 3 / g or more, an increase in the current collection resistance accompanying the charge / discharge cycle of the energy storage element can be suppressed. Although the reason for this is unclear, the following reason is presumed. In the Log differential pore volume distribution, the differential pore volume in the first range of 0.04 μm or more and 0.1 μm or less is considered to be based on the pores of the conductive agent, and the differential pore volume in the second range of pore diameters of more than 0.1 μm and 1.0 μm or less is considered to be based on the pores of the positive electrode active material. In the Log differential pore volume distribution of the positive electrode active material layer, the sum of the maximum value A of the differential pore volume in the first range and the maximum value B of the differential pore volume in the second range is 0.60 cm 3 / g or more, the dispersibility of the positive electrode active material and the conductive agent is good. As a result, even if the positive electrode active material layer expands with charge / discharge cycles, the conductive path between the active materials is maintained, and therefore the positive electrode for an energy storage element can suppress an increase in current collection resistance with charge / discharge cycles of the energy storage element. Here, "Log differential pore volume (dV / d(logD))" indicates the relationship between the size of the pores in the measured object and their volume, and refers to the value obtained by dividing the differential pore volume dV, which is the increase in pore volume between the measurement points of the pore diameter, by the logarithmic difference value d(logD) of the pore diameter. The log differential pore volume distribution refers to the plot of the log differential pore volume against the average pore diameter of each section. The "current collection resistance" can be evaluated by 1 kHz alternating current resistance (ACR).
[0013] The above A is 0.23 cm 3 / g or more, and the above B is 0.33 cm 3 / g or more. When the maximum value A of the differential pore volume in the first range and the maximum value B of the differential pore volume in the second range in the Log differential pore volume distribution of the positive electrode active material layer are equal to or greater than the lower limit, the positive electrode for an energy storage element can further improve the effect of suppressing an increase in current collection resistance accompanying charge / discharge cycles of the energy storage element.
[0014] The conductive agent is preferably carbon black, which improves the electronic conductivity of the conductive agent and the coatability of the positive electrode mixture paste.
[0015] The electric storage element according to one aspect of the present invention includes the positive electrode. By including the positive electrode, the electric storage element can suppress an increase in current collection resistance that occurs with charge and discharge cycles.
[0016] The configuration of a positive electrode for an energy storage element, the configuration of an energy storage device, a method for manufacturing a positive electrode for an energy storage element, a method for manufacturing an energy storage element, and other embodiments according to one embodiment of the present invention will be described in detail. Note that the names of the components (components) used in each embodiment may differ from the names of the components (components) used in the background art.
[0017] <Positive electrodes for energy storage elements> The positive electrode has a positive electrode substrate and a positive electrode active material layer disposed on the positive electrode substrate directly or via an intermediate layer.
[0018] (Positive electrode substrate) The positive electrode substrate has electrical conductivity. Whether or not it has "electrical conductivity" is judged by using a volume resistivity of 107 Ω·cm measured in accordance with JIS-H-0505 (1975) as a threshold value. Metals such as aluminum, titanium, tantalum, stainless steel, etc., or alloys thereof are used as the material of the positive electrode substrate. Among these, aluminum or aluminum alloys are preferred from the viewpoints of potential resistance, high electrical conductivity, and cost. Examples of the positive electrode substrate include foil, vapor deposition film, mesh, and porous material, and foil is preferred from the viewpoint of cost. Therefore, aluminum foil or aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or aluminum alloys include A1085, A3003, A1N30, etc., as specified in JIS-H-4000 (2014) or JIS-H4160 (2006).
[0019] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode active material layer. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode active material layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a binder and a conductive agent.
[0020] (Cathode active material layer) The positive electrode active material layer contains a positive electrode active material and a conductive agent, and may further contain optional components such as a binder, a thickener, and a filler, as necessary.
[0021] The positive electrode active material can be appropriately selected from known positive electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the positive electrode active material for a lithium ion secondary battery. Examples of the positive electrode active material include lithium transition metal composite oxides having an α-NaFeO2 type crystal structure, lithium transition metal composite oxides having a spinel type crystal structure, polyanion compounds, chalcogen compounds, and sulfur. Examples of the lithium transition metal composite oxides having an α-NaFeO2 type crystal structure include Li[Li x Ni (1-x) ]O2(0≦x<0.5), Li[Lix Ni γ Co (1-x-γ) ]O2(0≦x<0.5, 0<γ<1), Li[Li x Co (1-x) ]O2(0≦x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O2(0≦x<0.5, 0<γ<1), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O2(0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1), etc. Lithium transition metal composite oxides with spinel crystal structure include Li x Mn2O4, Li x Ni γ Mn (2-γ) O4, etc. Examples of polyanion compounds include LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc. Examples of chalcogen compounds include titanium disulfide, molybdenum disulfide, molybdenum dioxide, etc. Atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. The surfaces of these materials may be coated with other materials. In the positive electrode active material layer, one of these materials may be used alone, or two or more may be mixed and used.
[0022] The positive electrode active material is usually a particle (powder). The average particle size of the positive electrode active material is preferably, for example, 0.1 μm or more and 20 μm or less. By setting the average particle size of the positive electrode active material to the above lower limit or more, the positive electrode active material can be easily manufactured or handled. By setting the average particle size of the positive electrode active material to the above upper limit or less, the electronic conductivity of the positive electrode active material layer is improved. In addition, when a composite of the positive electrode active material and another material is used, the average particle size of the composite is taken as the average particle size of the positive electrode active material. The "average particle size" means a value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by a laser diffraction / scattering method for a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013).
[0023] In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, etc. are used. Examples of the pulverization method include a method using a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow type jet mill, or a sieve. During pulverization, wet pulverization in the presence of water or an organic solvent such as hexane can also be used. As a classification method, a sieve, an air classifier, etc. are used as necessary for both the dry and wet methods.
[0024] The content of the positive electrode active material in the positive electrode active material layer is preferably 50% by mass to 99% by mass, more preferably 70% by mass to 98% by mass, and even more preferably 80% by mass to 95% by mass. By setting the content of the positive electrode active material in the above range, both high energy density and manufacturability of the positive electrode active material layer can be achieved.
[0025] The conductive agent is preferably carbon black. When the conductive agent is carbon black, the electronic conductivity of the conductive agent and the coatability of the positive electrode mixture paste are improved. Examples of the carbon black include furnace black, acetylene black, and ketjen black. Among these, acetylene black is preferable. In addition, one or more types of carbon black may be used in combination.
[0026] The conductive agent may contain other conductive agents other than carbon black. The other conductive agents are not particularly limited as long as they are conductive materials. Examples of such conductive agents include carbonaceous materials, metals, conductive ceramics, and the like. Examples of carbonaceous materials include graphite, other non-graphitic carbons other than carbon black, graphene-based carbon, and the like. Examples of other non-graphitic carbons include carbon nanofibers and pitch-based carbon fibers. Examples of graphene-based carbons include graphene, carbon nanotubes (CNTs), fullerenes, and the like. Examples of the conductive agent include powder and fiber. As the conductive agent, one of these materials may be used alone, or two or more of them may be mixed and used. In addition, these materials may be used in a composite form.
[0027] The lower limit of the conductive agent content in the positive electrode active material layer is preferably 1 mass %, more preferably 2 mass %. Meanwhile, the upper limit of the conductive agent content is preferably 8 mass %, more preferably 6 mass %. By setting the total conductive agent content within the above range, it is possible to suppress the increase in current collection resistance accompanying the charge / discharge cycle of the energy storage element and to increase the energy density.
[0028] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, polyimide, etc.; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, etc.; polysaccharide polymers, etc.
[0029] The content of the binder in the positive electrode active material layer is preferably from 1% by mass to 10% by mass, more preferably from 2% by mass to 9% by mass. By setting the content of the binder in the above range, the active material can be stably held.
[0030] Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC), methyl cellulose, etc. When the thickener has a functional group that reacts with lithium or the like, this functional group may be deactivated in advance by methylation or the like.
[0031] The filler is not particularly limited. Examples of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, poorly soluble ion crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, and mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof.
[0032] The positive electrode active material layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.
[0033] In the Log differential pore volume distribution of the positive electrode active material layer, the lower limit of the sum of the maximum value A of the differential pore volume in the first range of pore diameters of 0.04 μm or more and 0.1 μm or less and the maximum value B of the differential pore volume in the second range of pore diameters of more than 0.1 μm and 1.0 μm or less is 0.60 cm 3 / g, 0.63 cm 3 / g is more preferable. When the lower limit of the total of the differential pore volume and the maximum differential pore volume is within the above range, the dispersibility of the positive electrode active material and the conductive material is good, so that the conductive path between the active materials is maintained even if the positive electrode active material layer expands with charge / discharge cycles. As a result, the positive electrode for a storage element can suppress an increase in current collection resistance with charge / discharge cycles of the storage element.
[0034] The lower limit of the maximum differential pore volume A in the first range is 0.05 cm 3 / g is preferred, and 0.23 cm 3 / g is more preferable, and 0.30 cm 3 The lower limit of the maximum value B of the differential pore volume in the second range is preferably 0.05 cm3 / g. 3 / g is preferred, and 0.33 cm 3 / g is more preferable, and 0.38 cm 3 / g is more preferable. By setting the lower limit of the maximum value A of the differential pore volume in the first range and the lower limit of the maximum value B of the differential pore volume in the second range within the above ranges, the positive electrode for an energy storage element can further improve the effect of suppressing the increase in current collection resistance accompanying the charge / discharge cycle of the energy storage element. On the other hand, the upper limit of the maximum value A of the differential pore volume in the first range is preferably 1.0 cm 3 The upper limit of the maximum value B of the differential pore volume in the second range is preferably 1.6 cm 3 By setting the maximum value A and the maximum value B to be equal to or less than the upper limit, the pore volume of the positive electrode active material layer does not become excessively large, so that it is possible to suppress peeling of the electrode plate due to a decrease in adhesion of the positive electrode active material layer.
[0035] The Log differential pore volume of the positive electrode active material layer is measured by mercury intrusion porosimetry according to the following procedure. The pore volume distribution is measured by mercury intrusion using AutoPore9400 (Micromeritics). The contact angle of mercury is set to 130° and the surface tension to 484 dynes / cm. The pore diameter range to be measured is from 6 nm to 20 μm. The pore diameter is plotted on the horizontal axis and the pore volume on the vertical axis to obtain a cumulative pore volume curve. Next, the differential volume dV between the measurement points is divided by the logarithmic differential value d(logD) of the pore diameter to obtain a value, and the log differential pore volume curve is obtained by plotting this value against the average pore diameter of each interval. The "maximum value of the differential pore volume in the pore diameter range of 0.04 μm to 0.1 μm" is the maximum value of the log differential pore volume in the average pore diameter range of 0.04 μm to 0.1 μm. "The maximum value of the differential pore volume in the range of pore diameters exceeding 0.1 μm and not exceeding 1.0 μm" refers to the maximum value of the Log differential pore volume in the range of average pore diameters exceeding 0.1 μm and not exceeding 1.0 μm. The sample of the positive electrode active material layer to be used for measuring the pore volume distribution is prepared by the following method. The storage element is discharged at a constant current of 0.1 C to the discharge end voltage during normal use. Here, "normal use" refers to the case where the storage element is used under the discharge conditions recommended or specified for the storage element. The storage element is disassembled, the positive electrode is removed and used as the working electrode, and a single-electrode battery is assembled using metallic Li as the counter electrode, and the positive electrode potential is set to 3.0 V (vs. Li / Li) at a current of 0.1 C. + ) The single-electrode battery is disassembled, and the removed positive electrode is thoroughly washed with dimethyl carbonate and then dried under reduced pressure at room temperature. The dried positive electrode is cut to a specified size (e.g., 2 x 2 cm) and used as a sample for measuring the pore volume distribution. The operations from disassembling the energy storage element to cutting the positive electrode to the specified size are carried out in a dry air atmosphere with a dew point of -40°C or less.
[0036] The porosity of the positive electrode active material layer may be, for example, 30% to 50%, preferably 35% to 47%, and more preferably 37% to 45%. By setting the porosity of the positive electrode active material layer in the above range, it is possible to increase the maximum value A of the differential pore volume in the first range and the maximum value B of the differential pore volume in the second range, and the increase in the current collection resistance due to the charge / discharge cycles of the energy storage element can be further suppressed.
[0037] The positive electrode for an electric storage device can suppress an increase in current collection resistance that occurs with charge / discharge cycles of the electric storage device.
[0038] <Electricity storage element> The electric storage element according to one embodiment of the present invention includes an electrode assembly having a positive electrode, a negative electrode, and a separator, a non-aqueous electrolyte, and a case that accommodates the electrode assembly and the non-aqueous electrolyte. The electrode assembly is usually a laminated type in which a plurality of positive electrodes and a plurality of negative electrodes are laminated with a separator interposed therebetween, or a wound type in which a positive electrode and a negative electrode are laminated with a separator interposed therebetween and wound. The non-aqueous electrolyte exists in a state in which it is impregnated in the positive electrode, the negative electrode, and the separator. As an example of an electric storage element, a non-aqueous electrolyte secondary battery (hereinafter, also simply referred to as a "secondary battery") will be described.
[0039] [Positive electrode] The positive electrode of the electricity storage element is as described above.
[0040] [Negative electrode] The negative electrode has a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The configuration of the intermediate layer is not particularly limited and can be selected from the configurations exemplified for the positive electrode.
[0041] (Negative electrode substrate) The negative electrode substrate has electrical conductivity. Metals such as copper, nickel, stainless steel, nickel-plated steel, and aluminum, or alloys thereof, carbonaceous materials, etc. are used as the material of the negative electrode substrate. Among these, copper or copper alloys are preferred. Examples of the negative electrode substrate include foils, vapor deposition films, meshes, and porous materials, and foils are preferred from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.
[0042] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, further preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate and to increase the energy density per volume of the secondary battery.
[0043] (Negative electrode active material layer) The negative electrode active material layer contains a negative electrode active material. The negative electrode active material layer contains optional components such as a conductive agent, a binder, a thickener, a filler, etc., as necessary. The optional components such as a conductive agent, a binder, a thickener, a filler, etc. can be selected from the materials exemplified for the positive electrode above.
[0044] The negative electrode active material layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.
[0045] The negative electrode active material can be appropriately selected from known negative electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the negative electrode active material for lithium ion secondary batteries. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li4Ti5O 12 , LiTiO 2、 Examples of the material include titanium-containing oxides such as TiNb2O7, polyphosphate compounds, silicon carbide, and carbon materials such as graphite and non-graphitic carbon (easily graphitized carbon or non-graphitizable carbon). Among these materials, graphite and non-graphitic carbon are preferred. In the negative electrode active material layer, one of these materials may be used alone, or two or more of them may be used in combination.
[0046] "Graphite" refers to graphite that has an average lattice spacing (d002 ) is 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. Artificial graphite is preferred from the viewpoint of availability of materials with stable physical properties.
[0047] "Non-graphitic carbon" refers to carbon that has an average lattice spacing (d 002 ) is 0.34 nm or more and 0.42 nm or less. Examples of non-graphitizable carbon include non-graphitizable carbon and graphitizable carbon. Examples of non-graphitizable carbon include resin-derived materials, petroleum pitch or petroleum pitch-derived materials, petroleum coke or petroleum coke-derived materials, plant-derived materials, and alcohol-derived materials.
[0048] Here, the "discharged state" refers to a state in which the negative electrode active material carbon material is discharged so that lithium ions that can be absorbed and released during charging and discharging are sufficiently released. For example, in a single-electrode battery using a negative electrode containing a carbon material as a negative electrode active material as a working electrode and metallic Li as a counter electrode, the state is one in which the open circuit voltage is 0.7 V or more.
[0049] "Non-graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.36 nm or more and 0.42 nm or less.
[0050] "Graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.34 nm or more and less than 0.36 nm.
[0051] The negative electrode active material is usually a particle (powder). The average particle size of the negative electrode active material can be, for example, 1 nm or more and 100 μm or less. When the negative electrode active material is a carbon material, a titanium-containing oxide, or a polyphosphate compound, the average particle size may be 1 μm or more and 100 μm or less. When the negative electrode active material is Si, Sn, Si oxide, Sn oxide, or the like, the average particle size may be 1 nm or more and 1 μm or less. By setting the average particle size of the negative electrode active material to the above lower limit or more, the negative electrode active material can be easily manufactured or handled. By setting the average particle size of the negative electrode active material to the above upper limit or less, the electronic conductivity of the active material layer is improved. In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, or the like is used. The pulverization method and the powder classification method can be selected from, for example, the methods exemplified for the positive electrode. When the negative electrode active material is a metal such as metallic Li, the negative electrode active material may be in the form of a foil.
[0052] The content of the negative electrode active material in the negative electrode active material layer is preferably 60% by mass to 99% by mass, more preferably 90% by mass to 98% by mass. By setting the content of the negative electrode active material in the above range, both high energy density and manufacturability of the negative electrode active material layer can be achieved.
[0053] [Separator] The separator can be appropriately selected from known separators. For example, a separator consisting of only a base layer, a separator in which a heat-resistant layer containing heat-resistant particles and a binder is formed on one or both sides of the base layer, etc. can be used as the separator. Examples of the material of the base layer of the separator include woven fabric, nonwoven fabric, and porous resin film. Among these materials, a porous resin film is preferable from the viewpoint of strength, and a nonwoven fabric is preferable from the viewpoint of the liquid retention of the non-aqueous electrolyte. As the material of the base layer of the separator, polyolefins such as polyethylene and polypropylene are preferable from the viewpoint of shutdown function, and polyimide and aramid are preferable from the viewpoint of oxidation decomposition resistance. A material obtained by combining these resins may be used as the base layer of the separator.
[0054] The heat-resistant particles contained in the heat-resistant layer preferably have a mass loss of 5% or less when heated from room temperature to 500°C under an air atmosphere at 1 atmosphere, and more preferably have a mass loss of 5% or less when heated from room temperature to 800°C. Examples of materials with a mass loss of a predetermined amount or less include inorganic compounds. Examples of inorganic compounds include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, barium titanate, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; sparingly soluble ion crystals such as calcium fluoride and barium fluoride; covalent crystals such as silicon and diamond; mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof. As the inorganic compound, these substances may be used alone or in the form of a complex, or two or more of them may be mixed and used. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of the safety of the energy storage element.
[0055] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, "porosity" refers to a volume-based value measured with a mercury porosimeter.
[0056] As the separator, a polymer gel composed of a polymer and a non-aqueous electrolyte may be used. Examples of the polymer include polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinylpyrrolidone, and polyvinylidene fluoride. The use of the polymer gel has an effect of suppressing leakage. As the separator, the above-mentioned porous resin film or nonwoven fabric may be used in combination with the polymer gel.
[0057] [Non-aqueous electrolyte] The nonaqueous electrolyte may be appropriately selected from known nonaqueous electrolytes. The nonaqueous electrolyte may be a nonaqueous electrolyte solution. The nonaqueous electrolyte solution includes a nonaqueous solvent and an electrolyte salt dissolved in the nonaqueous solvent.
[0058] The non-aqueous solvent can be appropriately selected from known non-aqueous solvents. Examples of the non-aqueous solvent include cyclic carbonates, chain carbonates, carboxylates, phosphates, sulfonates, ethers, amides, and nitriles. As the non-aqueous solvent, those in which some of the hydrogen atoms contained in these compounds are substituted with halogens may be used.
[0059] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinylethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Among these, EC is preferred.
[0060] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, trifluoroethyl methyl carbonate, bis(trifluoroethyl) carbonate, etc. Among these, EMC is preferable.
[0061] As the non-aqueous solvent, it is preferable to use a cyclic carbonate or a chain carbonate, and it is more preferable to use a combination of a cyclic carbonate and a chain carbonate. By using a cyclic carbonate, it is possible to promote dissociation of the electrolyte salt and improve the ionic conductivity of the non-aqueous electrolyte. By using a chain carbonate, it is possible to keep the viscosity of the non-aqueous electrolyte low. When using a cyclic carbonate and a chain carbonate in combination, it is preferable that the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate:chain carbonate) is, for example, in the range of 5:95 to 50:50.
[0062] The electrolyte salt can be appropriately selected from known electrolyte salts. Examples of the electrolyte salt include lithium salts, sodium salts, potassium salts, magnesium salts, onium salts, etc. Among these, lithium salts are preferred.
[0063] Examples of the lithium salt include inorganic lithium salts such as LiPF6, LiPO2F2, LiBF4, LiClO4, and LiN(SO2F)2, lithium oxalate salts such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP), and lithium salts having a halogenated hydrocarbon group such as LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), LiC(SO2CF3)3, and LiC(SO2C2F5)3. Among these, inorganic lithium salts are preferred, and LiPF6 is more preferred.
[0064] The electrolyte salt content in the non-aqueous electrolyte is 0.1 mol / dm at 20°C and 1 atmosphere. 3 More than 2.5mol / dm 3 It is preferable that the value is 0.3 mol / dm or less. 3 More than 2.0mol / dm 3 More preferably, it is 0.5 mol / dm or less. 3 More than 1.7mol / dm 3 More preferably, it is 0.7 mol / dm or less. 3More than 1.5mol / dm 3 By setting the content of the electrolyte salt within the above range, the ionic conductivity of the nonaqueous electrolyte can be increased.
[0065] The non-aqueous electrolyte may contain additives in addition to the non-aqueous solvent and the electrolyte salt. Examples of additives include halogenated carbonates such as fluoroethylene carbonate (FEC) and difluoroethylene carbonate (DFEC); oxalates such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); imide salts such as lithium bis(fluorosulfonyl)imide (LiFSI); biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, cyclohexyl, and the like. Aromatic compounds such as benzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the above aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; vinylene carbonate, methylvinylene carbonate, ethylvinylene carbonate, succinic anhydride, Glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, cyclohexanedicarboxylic anhydride; ethylene sulfite, propylene sulfite, dimethyl sulfite, propane sultone, propene sultone, butane sultone, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2- dioxo-1,3,2-dioxathiolane), 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, 1,3-propene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tristrimethylsilyl borate, tristrimethylsilyl phosphate, tetrakistrimethylsilyl titanate, lithium monofluorophosphate, lithium difluorophosphate, and the like.These additives may be used alone or in combination of two or more.
[0066] The content of the additive contained in the non-aqueous electrolyte is preferably 0.01% by mass to 10% by mass, more preferably 0.1% by mass to 7% by mass, even more preferably 0.2% by mass to 5% by mass, and particularly preferably 0.3% by mass to 3% by mass. By setting the content of the additive within the above range, it is possible to improve the capacity retention performance or cycle performance after high-temperature storage, and to further improve safety.
[0067] The non-aqueous electrolyte may be a solid electrolyte, or a non-aqueous electrolyte solution and a solid electrolyte may be used in combination.
[0068] The solid electrolyte can be selected from any material that has ionic conductivity such as lithium, sodium, calcium, etc., and is solid at room temperature (e.g., 15° C. to 25° C.). Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, oxynitride solid electrolytes, polymer solid electrolytes, etc.
[0069] Examples of sulfide solid electrolytes include Li2S-P2S5, LiI-Li2S-P2S5, and Li 10 Ge-P2S 12 etc.
[0070] [Specific configuration of the energy storage element] The shape of the energy storage element of this embodiment is not particularly limited, and examples thereof include a cylindrical battery, a square battery, a flat battery, a coin battery, and a button battery.
[0071] FIG 1 shows an energy storage element 1 as an example of a prismatic battery. Note that this figure is a see-through view of the inside of the case. An electrode body 2 having a positive electrode and a negative electrode wound with a separator sandwiched between them is housed in a prismatic case 3. The positive electrode is electrically connected to a positive electrode terminal 4 via a positive electrode lead 41. The negative electrode is electrically connected to a negative electrode terminal 5 via a negative electrode lead 51.
[0072] [Configuration of the power storage device] The energy storage element of this embodiment can be mounted as an energy storage device formed by assembling a plurality of energy storage elements 1 in a power source for an automobile such as an electric vehicle (EV), a hybrid vehicle (HEV), or a plug-in hybrid vehicle (PHEV), a power source for electronic devices such as a personal computer or a communication terminal, or a power storage power source, etc. In this case, it is sufficient that the technology of the present invention is applied to at least one energy storage element included in the energy storage device. 2 shows an example of an energy storage device 30 in which energy storage units 20, each of which is an assembly of two or more electrically connected energy storage elements 1, are further assembled. The energy storage device 30 may include a bus bar (not shown) that electrically connects the two or more energy storage elements 1, a bus bar (not shown) that electrically connects the two or more energy storage units 20, and the like. The energy storage units 20 or the energy storage device 30 may include a status monitoring device (not shown) that monitors the status of the one or more energy storage elements.
[0073] [Method of manufacturing the energy storage element] The manufacturing method of the electric storage element of this embodiment can be appropriately selected from known methods except for using the positive electrode described above as the positive electrode. The manufacturing method includes, for example, preparing an electrode body, preparing a nonaqueous electrolyte, and housing the electrode body and the nonaqueous electrolyte in a case. The preparation of the electrode body includes preparing the positive electrode and the negative electrode, and forming the electrode body by stacking or rolling the positive electrode and the negative electrode via a separator. The positive electrode can be produced, for example, by applying a positive electrode mixture paste directly or via an intermediate layer to a positive electrode substrate and drying it. After drying, pressing or the like may be performed as necessary. The positive electrode mixture paste includes each component constituting the positive electrode active material layer, such as a positive electrode active material, a conductive agent, and an optional binder. The positive electrode mixture paste usually further includes a dispersion medium. In the Log differential pore volume distribution of the positive electrode active material layer, the maximum value A of the differential pore volume in the first range and the maximum value B of the differential pore volume in the second range can be adjusted by the particle size and specific surface area of the positive electrode active material, the particle size and specific surface area of the conductive agent, the composition, thickness and area of the positive electrode active material layer, the kneading conditions of the positive electrode mixture paste during production, the press strength of the positive electrode active material layer, and the like.
[0074] The method of housing the non-aqueous electrolyte in the case can be appropriately selected from known methods. For example, when a non-aqueous electrolyte solution is used as the non-aqueous electrolyte, the non-aqueous electrolyte solution may be injected through an injection port formed in the case, and then the injection port may be sealed.
[0075] According to the energy storage element, by including the positive electrode, an increase in current collection resistance due to charge / discharge cycles can be suppressed.
[0076] <Other embodiments> The energy storage element of the present invention is not limited to the above-described embodiment, and various modifications may be made without departing from the scope of the present invention. For example, the configuration of one embodiment may be added to the configuration of another embodiment, and a part of the configuration of one embodiment may be replaced with the configuration of another embodiment or a well-known technique. Furthermore, a part of the configuration of one embodiment may be deleted. Also, a well-known technique may be added to the configuration of one embodiment.
[0077] In the above embodiment, the case where the storage element is used as a chargeable and dischargeable non-aqueous electrolyte secondary battery (for example, a lithium ion secondary battery) has been described, but the type, shape, size, capacity, etc. of the storage element are arbitrary. The present invention can also be applied to various secondary batteries, electric double layer capacitors, lithium ion capacitors, and other capacitors.
[0078] In the above embodiment, the electrode assembly in which the positive electrode and the negative electrode are stacked with a separator interposed therebetween has been described, but the electrode assembly may not include a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other in a state in which a non-conductive layer is formed on the active material layer of the positive electrode or the negative electrode. EXAMPLES
[0079] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0080] [Examples 1 to 4 and Comparative Examples 1 to 6] (Preparation of positive electrode) The positive electrode active material is LiNi with a particle size of 4 μm. 1 / 3 Co 1 / 3 Mn 1 / 3 A lithium transition metal composite oxide consisting of O2(NCM111) was used. Carbon black of the type shown in Table 1 was used as the conductive agent. Polyvinylidene fluoride was used as the binder.
[0081] Using N-methylpyrrolidone (NMP) as a dispersion medium, the positive electrode active material, conductive agent, and binder were kneaded under the conditions of Table 1 using a high-speed mixer "Filmix" manufactured by Primix Corporation so that the mass ratio (solid content equivalent) of the positive electrode active material layer in the positive electrode active material layer was 93.5:4.5:2, to obtain a positive electrode mixture paste. Next, the positive electrode mixture paste was applied to both sides of an aluminum foil as a positive electrode substrate, leaving a non-coated portion (a portion where the positive electrode active material layer is not formed), dried at 100°C, and roll-pressed to form a positive electrode active material layer on the positive electrode substrate. The amount of the positive electrode mixture paste applied was 10 mg / cm in solid content. 2In this manner, the positive electrodes of Examples 1 to 4 and Comparative Examples 1 to 6 were obtained.
[0082] (Preparation of negative electrode) Graphite was used as the negative electrode active material, styrene-butadiene rubber (SBR) as the binder, and carboxymethyl cellulose (CMC) as the thickener. The negative electrode active material, binder, and thickener were mixed in a mass ratio (solid content equivalent) of 98:1:1, and an appropriate amount of water was added as a dispersion medium to adjust the viscosity to prepare a negative electrode mixture paste. This negative electrode mixture paste was applied to both sides of copper foil, which is the negative electrode substrate, leaving uncoated areas (areas where the negative electrode active material layer is not formed), and dried to form a negative electrode active material layer. Then, roll pressing was performed to obtain a negative electrode.
[0083] (Preparation of non-aqueous electrolyte) A mixed solvent of EC, DMC, and EMC in a volume ratio of 30:35:35 was added with LiPF6 at 1.2 mol / dm 3 A non-aqueous electrolyte was prepared by dissolving the aqueous solution in the above-mentioned solution at a concentration of 1:1.
[0084] (Fabrication of Energy Storage Element) Next, the positive electrode and the negative electrode were laminated via a separator made of a polyethylene base material and an inorganic layer formed on the polyethylene base material to prepare an electrode body. This electrode body was housed in an aluminum case (rectangular battery case), and a positive electrode terminal and a negative electrode terminal were attached. The nonaqueous electrolyte was poured into the case (rectangular battery case), and the case was sealed to obtain the storage elements of the examples and comparative examples.
[0085] (Initial charge / discharge) Each of the above storage elements was charged at a constant current of 0.2C to 4.1V at 25°C, and then charged at a constant voltage of 4.1V. The charge was terminated when the total charge time reached 7 hours. After a 10-minute pause after charging, the elements were discharged at a constant current of 0.2C to 2.5V at 25°C. A 10-minute pause was then provided after discharging. The above cycle was repeated twice. For each storage element after the initial charge and discharge, the AC resistance at 1kHz was measured using a 1kHz AC impedance meter 10 minutes or more after the end of discharge.
[0086] (Measurement of Log Differential Pore Volume) For each energy storage element after the initial charge and discharge, the Log differential pore volume distribution of the positive electrode active material layer was measured by the method described above, and the sum of the maximum differential pore volume A in the first range of pore diameters of 0.04 μm or more and 0.1 μm or less and the maximum differential pore volume B in the second range of pore diameters of more than 0.1 μm and 1.0 μm or less was calculated. The results are shown in Table 1.
[0087] (Charge-discharge cycle test) After the initial charging and discharging, each storage element was stored in a thermostatic chamber at 55°C for 3 hours, and then it was charged at a constant current of 4C to 4.1V, and then, without a rest period, it was discharged at a constant current of 4C to 2.5V. This charging and discharging process was counted as one cycle, and this cycle was repeated 1500 times. Both charging and discharging were performed in a thermostatic chamber at 55°C.
[0088] (AC resistance (ACR) increase rate after charge / discharge cycle test) The AC resistance increase rate of the storage element after the above charge-discharge cycle test was evaluated. The AC resistance at 1 kHz was measured for each storage element after the above charge-discharge cycle test by the above method. The increase rate (%) of the AC resistance at 1 kHz after the charge-discharge cycle test relative to the AC resistance at 1 kHz after the initial charge-discharge test was calculated by the following formula. The obtained AC resistance increase rate is shown in Table 1. AC resistance increase rate (%) = (ACR after charge-discharge cycle test / ACR after initial charge-discharge) x 100
[0089] The evaluation results are shown in Table 1 below.
[0090] [Table 1]
[0091] As shown in Table 1 and FIG. 3, in the Log differential pore volume distribution of the positive electrode active material layer, the sum of the maximum value A of the differential pore volume in the pore diameter range of 0.04 μm or more and 0.1 μm or less and the maximum value B of the differential pore volume in the pore diameter range of more than 0.1 μm and 1.0 μm or less is 0.60 cm 3 / g or more, the increase rate of AC resistance after the charge-discharge cycle test was reduced as compared with Comparative Example 1 to Comparative Example 6, in which the sum of the maximum differential pore volumes was outside the above range.
[0092] The above results show that the positive electrode for an energy storage element can suppress an increase in current collection resistance that occurs with the charge / discharge cycles of the energy storage element. [Industrial Applicability]
[0093] The positive electrode for an electric storage device can be applied to an electric storage device used as a power source for electronic devices such as personal computers and communication terminals, and automobiles. [Explanation of symbols]
[0094] 1 Energy storage element 2 Electrode body 3 Cases 4 Positive terminal 41 Positive lead 5 Negative terminal 51 Negative lead 20 Energy Storage Unit 30 Energy storage device
Claims
1. A positive electrode active material layer containing a positive electrode active material and a conductive agent, In the Log differential pore volume distribution of the positive electrode active material layer, the maximum value of the differential pore volume in the pore diameter range of 0.04 μm or more and 0.1 μm or less is defined as A, When the maximum value of the differential pore volume in the pore diameter range of more than 0.1 μm and not more than 1.0 μm is B, The sum of A and B is 0.60 cm 3 / g or more, The above B is greater than the above A, The above A is 0.23 cm 3 / g or more, The positive electrode for a storage element, wherein B is 0.33 cm 3 / g or more.
2. 2. The positive electrode for a storage element according to claim 1, wherein the conductive agent is carbon black.
3. An electric storage element comprising the positive electrode according to claim 1 or 2.
Citation Information
Patent Citations
Lithium secondary battery
JP2012216500A
Electrode for nonaqueous electrolyte battery, nonaqueous electrolyte battery, battery pack, and vehicle
JP2017059394A
Power storage element
JP2018055801A
Lithium-ion battery manufacturing method and lithium-ion battery
JP2020057523A
Electrode for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and automobile, power tool or stationary device equipped with same
WO2006129756A1