Resin composition, optical fiber, and method for producing optical fiber
The resin composition for optical fibers, containing a hydroxyl group-containing urethane compound and photopolymerizable compounds, addresses the issue of slipperiness loss, enhancing productivity by providing superior slipperiness and wear resistance.
Patent Information
- Application Number
- JP2021570682
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-14
- Filing Date
- 2020-12-08
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-12-08
AI Technical Summary
The surface slipperiness of the secondary coating on optical fibers decreases due to external forces, leading to meandering during winding and reduced productivity.
A resin composition for secondary coating comprising a hydroxyl group-containing urethane compound with a specific molecular weight range, a photopolymerizable compound, and a photopolymerization initiator, which forms a secondary resin layer with excellent surface slipperiness and wear resistance.
The resin composition enhances the productivity of optical fibers by maintaining surface slipperiness and wear resistance, improving handling and reducing winding abnormalities.
Smart Images

Figure 0007582210000003 
Figure 0007582210000001 
Figure 0007582210000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a resin composition for a secondary coating of an optical fiber, an optical fiber, and a method for making an optical fiber. This application claims priority to Japanese Application No. 2020-003518 filed on January 14, 2020, and incorporates by reference all of the contents of said Japanese application. [Background technology]
[0002] In general, optical fibers are provided with a coating resin layer for protecting the glass fiber, which is an optical transmission medium. The coating resin layer is composed of two layers, for example, a primary resin layer in contact with the glass fiber and a secondary resin layer formed on the outer surface of the primary resin layer. The secondary resin layer is required to have surface slipperiness, scratch resistance, anti-tack properties, etc., in order to prevent external damage to the optical fiber and to improve the handleability of the optical fiber.
[0003] For example, Patent Documents 1 and 2 disclose that a resin layer is formed using a resin composition containing a silicone compound to improve surface slipperiness. Patent Documents 3 and 4 disclose that a resin layer is formed using a resin composition containing a specific urethane (meth)acrylate to improve tack prevention. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-278850 [Patent Document 2] Japanese Patent Application Publication No. 9-328632 [Patent Document 3] JP 2006-36989 A [Patent Document 4] JP 2005-89586 A Summary of the Invention
[0005] A resin composition for a secondary coating of an optical fiber according to one embodiment of the present disclosure is a resin composition containing a hydroxyl-containing urethane compound having a number average molecular weight of 10,000 or more and 40,000 or less, a photopolymerizable compound, and a photopolymerization initiator, wherein the content of the hydroxyl-containing urethane compound is 0.05 parts by mass or more and 10 parts by mass or less based on 100 parts by mass of the total amount of the resin composition, and the hydroxyl-containing urethane compound is a reaction product of a polyol having a number average molecular weight of 1,800 or more and 4,500 or less and a diisocyanate. [Brief description of the drawings]
[0006] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of an optical fiber according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] [Problem that this disclosure aims to solve] In optical fiber production lines, the surface slipperiness of the coating resin layer gradually deteriorates due to contact with guide rollers, screening tests (a test in which a tensile load of several kg is applied to the optical fiber to remove low-strength parts in advance), etc., which can cause the optical fiber to meander when wound onto a bobbin, resulting in reduced productivity of the optical fiber. In order to improve the productivity of optical fiber, the secondary resin layer is required to have excellent surface slipperiness and abrasion resistance when an external force is applied to the optical fiber.
[0008] An object of the present disclosure is to provide a resin composition for a secondary coating of an optical fiber that has excellent surface slip properties and abrasion resistance when an external force is applied to the optical fiber, and an optical fiber that has excellent productivity.
[0009] [Effects of this disclosure] According to the present disclosure, it is possible to provide a resin composition for a secondary coating of an optical fiber that has excellent surface slipperiness and abrasion resistance when an external force is applied to the optical fiber, and an optical fiber that has excellent productivity.
[0010] [Description of the embodiments of the present disclosure] First, the contents of the embodiments of the present disclosure will be listed and described. A resin composition for a secondary coating of an optical fiber according to one aspect of the present disclosure is a resin composition containing a hydroxyl group-containing urethane compound having a number average molecular weight of 10,000 to 40,000, a photopolymerizable compound, and a photopolymerization initiator, the content of the hydroxyl group-containing urethane compound being 0.05 parts by mass to 10 parts by mass based on a total amount of 100 parts by mass of the resin composition, and the hydroxyl group-containing urethane compound being a reaction product of a polyol having a number average molecular weight of 1,800 to 4,500 and a diisocyanate.
[0011] Such a resin composition can form a secondary resin layer having excellent surface slip properties and abrasion resistance when an external force is applied to the optical fiber, thereby improving the productivity of the optical fiber.
[0012] In order to impart appropriate toughness to the secondary resin layer, the photopolymerizable compound may contain urethane (meth)acrylate having a number average molecular weight of 1,000 or more and 6,000 or less.
[0013] In order to form a tougher resin layer, the urethane (meth)acrylate may be a reaction product of a polyol having a number average molecular weight of 350 or more and 2500 or less, a diisocyanate, and a hydroxyl group-containing (meth)acrylate.
[0014] The photopolymerizable compound may further contain an epoxy (meth)acrylate in order to provide the secondary resin layer with appropriate toughness. The epoxy (meth)acrylate may have an aromatic ring in order to further improve abrasion resistance.
[0015] An optical fiber according to one aspect of the present disclosure includes a glass fiber including a core and a cladding, a primary resin layer that contacts the glass fiber and coats the glass fiber, and a secondary resin layer that coats the primary resin layer, the secondary resin layer including a cured product of the resin composition. Such an optical fiber has excellent surface slipperiness and abrasion resistance, and can improve the productivity of the optical fiber.
[0016] The method for producing an optical fiber according to an embodiment of the present disclosure includes a coating step of coating the resin composition on the outer periphery of a glass fiber including a core and a cladding, and a curing step of curing the resin composition by irradiating the resin composition with ultraviolet light after the coating step, thereby making it possible to produce an optical fiber having excellent surface slip properties and abrasion resistance.
[0017] [Details of the embodiment of the present disclosure] Specific examples of the resin composition and optical fiber according to the present embodiment will be described with reference to the drawings as necessary. Note that the present disclosure is not limited to these examples, but is intended to include all modifications within the scope of the claims and meaning equivalent thereto. In the following description, the same elements in the description of the drawings will be given the same reference numerals, and duplicated descriptions will be omitted.
[0018] (Resin composition) The resin composition according to the present embodiment contains a hydroxyl group-containing urethane compound, a photopolymerizable compound, and a photopolymerization initiator.
[0019] The hydroxyl-containing urethane compound according to this embodiment has a number average molecular weight (Mn) of 10,000 or more and 40,000 or less, and is a urethane compound having a hydroxyl group (hereinafter referred to as "hydroxyl-containing urethane compound (A)"). The Mn of the hydroxyl-containing urethane compound (A) is preferably 11,000 or more and 40,000 or less, and more preferably 12,000 or more and 39,000 or less. If the Mn of the hydroxyl-containing urethane compound (A) is less than 10,000, the surface slip properties and abrasion resistance tend to decrease, and if the Mn exceeds 40,000, the resin composition tends to become cloudy.
[0020] The hydroxyl group-containing urethane compound (A) is a reaction product between a polyol having an Mn of 1800 or more and 4500 or less and a diisocyanate. The hydroxyl group-containing urethane compound (A) has a urethane structure based on the reaction between a polyol having an Mn of 1800 or more and 4500 or less and a diisocyanate, and a hydroxyl group bonded to the end of the urethane structure. The hydroxyl group-containing urethane compound (A) is a compound that does not have a photopolymerizable group such as a (meth)acryloyl group.
[0021] Examples of the polyol include polytetramethylene glycol, polyethylene glycol, polypropylene glycol, polyester polyol, polycaprolactone polyol, polycarbonate polyol, polybutadiene polyol, and bisphenol A-ethylene oxide addition diol. Among them, it is preferable to use polypropylene glycol as the polyol.
[0022] Examples of diisocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, 1,5-naphthalene diisocyanate, norbornene diisocyanate, 1,5-pentamethylene diisocyanate, tetramethylxylylene diisocyanate, and trimethylhexamethylene diisocyanate.
[0023] The hydroxyl-containing urethane compound (A) can be obtained by reacting a polyol with a diisocyanate at a molar ratio (OH / NCO) of the hydroxyl groups (OH) of the polyol to the isocyanate groups (NCO) of the diisocyanate of 1.1 to 1.8. When the OH / NCO ratio is within the above range, the proportion of urethane bonds contained in the hydroxyl-containing urethane compound (A) increases, so that hydrogen bonds between the hydroxyl-containing urethane compounds (A) or between the compounds and other materials become stronger, and good surface properties can be maintained even after an external force is applied to the optical fiber.
[0024] Since it is easy to synthesize the hydroxyl-containing urethane compound (A) with an adjusted ratio of urethane bonds, the Mn of the polyol constituting the hydroxyl-containing urethane compound (A) is 1800 or more, preferably 2000 or more, and more preferably 2500 or more. Since the ratio of urethane bonds contained in the hydroxyl-containing urethane compound (A) increases and it becomes easier to form a secondary resin layer having good surface properties, the Mn of the polyol is 4500 or less, preferably 4000 or less, and more preferably 3500 or less.
[0025] The preparation of the hydroxyl group-containing urethane compound (A) will be described below with a specific example. For example, polypropylene glycol is used as the polyol, and 2,4-tolylene diisocyanate is used as the diisocyanate. Polypropylene glycol and 2,4-tolylene diisocyanate are reacted in a molar ratio of OH / NCO of 1.1 to 1.8 to synthesize a urethane compound having a hydroxyl group at the end. The hydroxyl group-containing urethane compound (A) can be represented by the following formula (1). HO-(PUIU)mP-OH (1) Here, HO and OH represent hydroxyl groups, U represents a urethane bond, I represents a residue of 2,4-tolylene diisocyanate, P represents a residue of polypropylene glycol, and m is an integer of 1 or more. By changing m (OH / NCO), the ratio of urethane bonds in the urethane compound can be changed. The smaller the OH / NCO, the larger m becomes, and the larger the OH / NCO, the smaller m becomes.
[0026] From the viewpoint of improving the slipperiness and abrasion resistance of the surface, the content of the hydroxyl group-containing urethane compound (A) is 0.05 parts by mass or more, preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.3 parts by mass or more, based on the total amount (100 parts by mass) of the resin composition. From the viewpoint of suppressing the decrease in the Young's modulus of the secondary resin layer, the content of the hydroxyl group-containing urethane compound (A) is 10 parts by mass or less, preferably 8 parts by mass or less, more preferably 6 parts by mass or less, and even more preferably 5 parts by mass or less, based on the total amount of the resin composition.
[0027] From the viewpoint of forming a tough secondary resin layer, the photopolymerizable compound according to this embodiment may contain a urethane (meth)acrylate (hereinafter referred to as "urethane (meth)acrylate (B)") having an Mn of 1000 or more and 6000 or less. The Mn of the urethane (meth)acrylate (B) is preferably 1050 or more and 5800 or less, and more preferably 1100 or more and 5500 or less. When the Mn of the urethane (meth)acrylate (B) is 1000 or more, it becomes easy to form a tough secondary resin layer, and when it is 6000 or less, it becomes easy to increase the Young's modulus of the secondary resin layer.
[0028] Here, (meth)acrylate means acrylate or the corresponding methacrylate. The same applies to other similar expressions such as (meth)acryloyl.
[0029] The urethane (meth)acrylate (B) may be a reaction product of a polyol having an Mn of 350 or more and 2500 or less, a diisocyanate, and a hydroxyl group-containing (meth)acrylate. The urethane (meth)acrylate (B) preferably has a urethane structure based on a reaction between a polyol having an Mn of 350 or more and 2500 or less and a diisocyanate, and a (meth)acryloyl group bonded to an end of the urethane structure.
[0030] Examples of hydroxyl group-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, caprolactone (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, 2-hydroxy-O-phenylphenolpropyl (meth)acrylate, 2-hydroxy-3-methacrylpropyl acrylate, trimethylolpropane di(meth)acrylate, and pentaerythritol tri(meth)acrylate.
[0031] The urethane (meth)acrylate (B) can be obtained by reacting a polyol having an Mn of 350 or more and 2500 or less with a diisocyanate at an NCO / OH ratio of 1.5 or more and 4 or less, and then reacting with an OH-containing (meth)acrylate. When the NCO / OH ratio is within the above range, a tough secondary resin layer can be easily formed.
[0032] The preparation of the urethane (meth)acrylate (B) will be described below with a specific example. For example, polypropylene glycol is used as the polyol, 2,4-tolylene diisocyanate is used as the diisocyanate, and 2-hydroxyethyl acrylate is used as the hydroxyl group-containing (meth)acrylate. First, polypropylene glycol and 2,4-tolylene diisocyanate are reacted to synthesize an NCO-terminated prepolymer. Next, the NCO-terminated prepolymer and 2-hydroxyethyl acrylate are reacted to synthesize a urethane acrylate. The urethane acrylate (B) can be represented by the following formula (2). A-(UIUP)nUIUA (2) Here, A represents a residue of 2-hydroxyethyl acrylate, U represents a urethane bond, I represents a residue of 2,4-tolylene diisocyanate, P represents a residue of polypropylene glycol, and n is an integer of 1 or more. By changing n, the ratio of urethane bonds in the urethane acrylate can be changed. The smaller the NCO / OH, the larger n becomes, and the larger the NCO / OH, the smaller n becomes.
[0033] From the viewpoint of improving the toughness of the secondary resin layer, Mn of the polyol constituting the urethane (meth)acrylate (B) is more preferably 400 or more and 2,200 or less, and further preferably 500 or more and 2,000 or less.
[0034] From the viewpoint of improving the toughness of the secondary resin layer, the content of the urethane (meth)acrylate (B) is preferably from 5 to 60 parts by mass, more preferably from 10 to 50 parts by mass, based on the total amount of the resin composition.
[0035] An organic tin compound or an amine compound is used as a catalyst when synthesizing the hydroxyl group-containing urethane compound (A) and the urethane (meth)acrylate (B). Examples of organic tin compounds include dibutyltin dilaurate, dibutyltin diacetate, dibutyltin maleate, dibutyltin bis(2-ethylhexyl mercaptoacetate), dibutyltin bis(isooctyl mercaptoacetate), and dibutyltin oxide. In terms of easy availability or catalytic performance, it is preferable to use dibutyltin dilaurate or dibutyltin diacetate as a catalyst.
[0036] In order to impart appropriate toughness to the secondary resin layer, the photopolymerizable compound according to this embodiment may further contain an epoxy (meth)acrylate. The epoxy (meth)acrylate is a compound obtained by reacting an epoxy compound having two or more glycidyl groups with a compound having a (meth)acryloyl group.
[0037] In order to further improve the abrasion resistance, it is preferable that the epoxy (meth)acrylate has an aromatic ring. Examples of the epoxy (meth)acrylate having an aromatic ring include novolac epoxy (meth)acrylate, trade name "Viscoat #540" manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name "Epoxy Ester 3002M", "Epoxy Ester 3002A", "Epoxy Ester 3000MK", and "Epoxy Ester 3000A" manufactured by Kyoeisha Chemical Co., Ltd.
[0038] In order to impart flexibility to the secondary resin layer, the photopolymerizable compound according to the present embodiment may further contain an epoxy (meth)acrylate having no aromatic ring. Examples of the epoxy (meth)acrylate having no aromatic ring include those available under the trade names "EPOXY ESTER 40EM", "EPOXY ESTER 70PA", "EPOXY ESTER 200PA" and "EPOXY ESTER 80MFA" manufactured by Kyoeisha Chemical Co., Ltd.
[0039] The content of the epoxy (meth)acrylate may be 5 parts by mass or more, 10 parts by mass or more, or 20 parts by mass or more, and may be 70 parts by mass or less, 65 parts by mass or less, or 60 parts by mass or less, based on the total amount of the resin composition.
[0040] The photopolymerizable compound according to the present embodiment may further include a photopolymerizable compound (hereinafter referred to as "monomer") other than urethane (meth)acrylate and epoxy (meth)acrylate. As the monomer, a monofunctional monomer having one photopolymerizable ethylenically unsaturated group, or a polyfunctional monomer having two or more ethylenically unsaturated groups may be used. Two or more types of monomers may be mixed and used.
[0041] Examples of monofunctional monomers include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, isoamyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, phenoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, (Meth)acrylate monomers such as acrylate, nonylphenol polyethylene glycol (meth)acrylate (for example, trade name "SR504" manufactured by Sartomer), nonylphenoxy polyethylene glycol (meth)acrylate, isobornyl (meth)acrylate, 3-phenoxybenzyl (meth)acrylate, methylphenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, m-phenoxybenzyl (meth)acrylate, 2-(2-ethoxyethoxy)ethyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl acrylate; carboxyl group-containing monomers such as (meth)acrylic acid, (meth)acrylic acid dimer, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, and ω-carboxy-polycaprolactone (meth)acrylate;N-Acryloylmorpholine, N-Vinylpyrrolidone, N-Vinylcaprolactam, 3-(3-pyridinyl)propyl (meth)acrylate, N,N-Dimethylacrylamide, N-Hydroxyethylacrylamide, N,N-Diethylacrylamide, N-Isopropylacrylamide, N,N-Dimethylaminopropylacrylamide, N,N-Dimethylaminopropylacrylamide·Methyl chloride salt, Diacetoneacrylamide, N-Acryloylpiperidine, N-Methacryloylpiperidine, N-Acryloylpyrrolidine, Maleimide, Nitrogen-containing monomers such as N-cyclohexylmaleimide, N-phenylmaleimide, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide, aminoethyl(meth)acrylate, aminopropyl(meth)acrylate, N,N-dimethylaminoethyl(meth)acrylate, and t-butylaminoethyl(meth)acrylate are included.
[0042] Examples of polyfunctional monomers include ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, 1,6-hexyl bifunctional monomers such as sandiol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, 1,14-tetradecanediol di(meth)acrylate, 1,16-hexadecanediol di(meth)acrylate, 1,20-eicosanediol di(meth)acrylate, isopentyldiol di(meth)acrylate, 3-ethyl-1,8-octanediol di(meth)acrylate, tricyclodecanol di(meth)acrylate, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene di(meth)acrylate, and EO adduct di(meth)acrylate of bisphenol A (for example, trade name "Viscoat #700HV" manufactured by Osaka Organic Chemical Industry Co., Ltd.);Trimethylolpropane tri(meth)acrylate, trimethylol octane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, trimethylolpropane polypropoxy tri(meth)acrylate, trimethylolpropane polyethoxy polypropoxy tri(meth)acrylate, tris[(meth)acryloyloxyethyl]isocyanurate, pentaerythritol tri(meth)acrylate, pentaerythritol polyethoxy tetra(meth)acrylate ) acrylate, pentaerythritol polypropoxy tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, caprolactone-modified tris[(meth)acryloyloxyethyl]isocyanurate, and other trifunctional or higher monomers;
[0043] The photopolymerization initiator can be appropriately selected from known radical photopolymerization initiators. Examples of the photopolymerization initiator include 1-hydroxycyclohexyl phenyl ketone (Omnirad 184, manufactured by IGM Resins), 2,2-dimethoxy-2-phenylacetophenone (Omnirad 651, manufactured by IGM Resins), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO, manufactured by IGM Resins), ethyl (2,4,6-trimethylbenzoyl)-phenylphosphinate (Omnirad TPO-L, manufactured by IGM Resins), 2-benzoyl-2-dimethylamino-4'-morpholinobutyrophenone (Omnirad TPO369, manufactured by IGM Resins), 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one (Omnirad TPO379, manufactured by IGM Resins), and 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one (Omnirad TPO379, manufactured by IGM Resins). Examples of suitable amines include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, IGM Resins), bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, IGM Resins), and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (Omnirad 907, IGM Resins).
[0044] Two or more kinds of photopolymerization initiators may be mixed for use. The photopolymerization initiator preferably contains 2,4,6-trimethylbenzoyldiphenylphosphine oxide, since this has excellent rapid curing properties for the resin composition.
[0045] The content of the photopolymerization initiator is preferably 0.2 parts by mass or more and 5 parts by mass or less, more preferably 0.4 parts by mass or more and 3 parts by mass or less, and even more preferably 0.5 parts by mass or more and 2 parts by mass or less, based on the total amount of the resin composition.
[0046] The resin composition according to the present embodiment may further contain a photoacid generator, a leveling agent, an antifoaming agent, an antioxidant, and the like.
[0047] The photoacid generator is A + B -Examples of the photoacid generator include sulfonium salts such as CPI-100P and 110P (manufactured by San-Apro Co., Ltd.), Omnicat 270 and 290 (manufactured by IGM Resins), and iodonium salts such as Omnicat 250 (manufactured by IGM Resins), WPI-113, 116, 124, 169 and 170 (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.).
[0048] (Optical Fiber) 1 is a schematic cross-sectional view showing an example of an optical fiber according to the present embodiment. The optical fiber 10 includes a glass fiber 13 including a core 11 and a cladding 12, and a coating resin layer 16 including a primary resin layer 14 and a secondary resin layer 15 provided on the outer periphery of the glass fiber 13.
[0049] The cladding 12 surrounds the core 11. The core 11 and the cladding 12 mainly contain glass such as silica glass, and for example, the core 11 can be made of silica glass doped with germanium or pure silica glass, and the cladding 12 can be made of pure silica glass or silica glass doped with fluorine.
[0050] 1, for example, the outer diameter (D2) of the glass fiber 13 is about 100 μm to 125 μm, and the diameter (D1) of the core 11 constituting the glass fiber 13 is about 7 μm to 15 μm.
[0051] The thickness of the coating resin layer 16 is usually about 60 μm to 70 μm. The thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be about 20 μm to 40 μm, for example, the thickness of the primary resin layer 14 may be 35 μm and the thickness of the secondary resin layer 15 may be 25 μm. When a large number of optical fibers are assembled into a cable, it is preferable that the coating diameter of the optical fibers is small. In that case, the total thickness of the coating resin layer 16 is preferably 30 μm to 40 μm, and the thickness of each of the primary resin layer and the secondary resin layer may be 10 μm to 30 μm.
[0052] By applying the resin composition according to this embodiment to the secondary resin layer, an optical fiber with excellent productivity can be produced.
[0053] The method for manufacturing an optical fiber according to this embodiment includes a coating step of coating the above-mentioned resin composition onto the outer periphery of a glass fiber including a core and a cladding, and a curing step of curing the resin composition by irradiating it with ultraviolet light after the coating step.
[0054] From the viewpoint of improving the microbending resistance of the optical fiber, the Young's modulus of the secondary resin layer is preferably 500 MPa or more, and more preferably 800 MPa or more, at 23° C.±2° C. Although there is no particular upper limit to the Young's modulus of the secondary resin layer, from the viewpoint of imparting appropriate toughness to the secondary resin layer, it may be 3000 MPa or less, 2500 MPa or less, 2000 MPa or less, or 1500 MPa or less at 23° C.±2° C.
[0055] The Young's modulus of the secondary resin layer can be measured by the following method. First, the optical fiber is immersed in a mixed solvent of acetone and ethanol, and only the coating resin layer is extracted in a cylindrical shape. At this time, the primary resin layer and the secondary resin layer are integrated, but since the Young's modulus of the primary resin layer is 1 / 1000 to 1 / 10000 of that of the secondary resin layer, the Young's modulus of the primary resin layer can be ignored. Next, the solvent is removed from the coating resin layer by vacuum drying, and then a tensile test (tensile speed 1 mm / min) is performed at 23°C, and the Young's modulus can be obtained by the secant equation with 2.5% strain.
[0056] The primary resin layer 14 can be formed by curing a resin composition containing, for example, urethane (meth)acrylate, a monomer, a photopolymerization initiator, and the like. The resin composition forming the primary resin layer has a different composition from the resin composition for the secondary coating. The resin composition for the primary coating can be prepared using a conventionally known technique.
[0057] The Young's modulus of the primary resin layer is preferably 0.5 MPa or less. If the Young's modulus of the primary resin layer exceeds 0.5 MPa, external forces are easily transmitted to the glass fiber, and the increase in transmission loss due to microbending may become significant.
[0058] In some cases, optical fibers are arranged in parallel and integrated with a ribbon resin to form an optical fiber ribbon. The resin composition according to the present disclosure can also be used as a ribbon resin. This can improve the surface slipperiness and abrasion resistance when an external force is applied to the optical fiber ribbon, just like with optical fibers. EXAMPLES
[0059] The present disclosure will be described in more detail below by showing the results of evaluation tests using examples and comparative examples according to the present disclosure. Note that the present disclosure is not limited to these examples.
[0060] [Synthesis of hydroxyl-containing urethane compounds] (A-1) Polypropylene glycol (PPG4000) with Mn4000 and 2,4-tolylene diisocyanate (TDI) were mixed so that the molar ratio of NCO to OH (OH / NCO) was 1.8, and 200 ppm of dibutyltin dilaurate was added as a catalyst to the final total charge. PPG4000 and TDA were reacted at 80°C for 1 hour to obtain a hydroxyl group-containing urethane compound (A-1) with Mn10700.
[0061] (A-2) A hydroxyl-containing urethane compound (A-2) with Mn of 13100 was obtained in the same manner as in the synthesis of (A-1), except that polypropylene glycol (PPG3000) with Mn of 3000 and TDI were mixed so that the OH / NCO ratio was 1.5.
[0062] (A-3) A hydroxyl-containing urethane compound (A-3) with Mn of 15600 was obtained in the same manner as in the synthesis of (A-1), except that polypropylene glycol (PPG2000) with Mn of 2000 and TDI were mixed so that the OH / NCO ratio was 1.2.
[0063] (A-4) A hydroxyl-containing urethane compound (A-4) with Mn of 37800 was obtained in the same manner as in the synthesis of (A-1), except that PPG3000 and TDI were mixed so that the OH / NCO ratio was 1.1.
[0064] (Z-1) A hydroxyl-containing urethane compound (Z-1) with Mn of 6500 was obtained in the same manner as in the synthesis of (A-1), except that PPG3000 and TDI were mixed so that the OH / NCO ratio was 2.0.
[0065] (Z-2) A hydroxyl-containing urethane compound (Z-2) with Mn of 8100 was obtained in the same manner as in the synthesis of (A-1), except that PPG4000 and TDI were mixed so that the OH / NCO ratio was 2.0.
[0066] [Synthesis of urethane acrylate] (B-1) Polypropylene glycol (PPG400) with Mn400 and isophorone diisocyanate (IPDI) were reacted at NCO / OH ratio of 1.5 to prepare an NCO-terminated prepolymer. As a catalyst, dibutyltin dilaurate was added at 200 ppm relative to the final total amount charged. Next, 2-hydroxyethyl acrylate (HEA) was added so that the molar ratio of OH of HEA to NCO of the NCO-terminated prepolymer was 1.05, and the reaction was carried out at 80°C for 1 hour to obtain urethane acrylate (B-1) with Mn1900.
[0067] (B-2) A urethane acrylate (B-2) with Mn of 2200 was obtained in the same manner as in the synthesis of (B-1), except that polypropylene glycol (PPG600) with Mn of 600 and TDI were reacted at an NCO / OH ratio of 2.0 to prepare an NCO-terminated prepolymer.
[0068] (B-3) A urethane acrylate (B-3) with Mn of 1100 was obtained in the same manner as in the synthesis of (B-1), except that PPG600 and TDI were reacted at an NCO / OH ratio of 4.0 to prepare an NCO-terminated prepolymer.
[0069] (B-4) A urethane acrylate (B-4) with Mn of 5400 was obtained in the same manner as in the synthesis of (B-1), except that PPG2000 and TDI were reacted at an NCO / OH ratio of 2.0 to prepare an NCO-terminated prepolymer.
[0070] (B-5) A urethane acrylate (B-5) with Mn of 10,800 was obtained in the same manner as in the synthesis of (B-1), except that PPG3000 and IPDI were reacted at an NCO / OH ratio of 1.5 to prepare an NCO-terminated prepolymer.
[0071] The Mn of the hydroxyl group-containing urethane compound and the urethane acrylate were measured using a Waters ACQUITY APC RI system under the following conditions: sample concentration: 0.2 mass% THF solution, injection amount: 20 μL, sample temperature: 15°C, mobile phase: THF, XT column for organic solvents: particle diameter 2.5 μm, pore size 450 Å, column inner diameter 4.6 × column length 150 mm + particle diameter 2.5 μm, pore size 125 Å, column inner diameter 4.6 × column length 150 mm + particle diameter 1.7 μm, pore size 45 Å, column inner diameter 4.6 × column length 150 mm, column temperature: 40°C, flow rate: 0.8 mL / min.
[0072] [Resin composition for secondary coating] Resin compositions for secondary coating in each of the Examples and Comparative Examples were prepared by mixing a hydroxyl group-containing urethane compound, urethane acrylate, tripropylene glycol diacrylate (TPGDA), neopentyl glycol diacrylate (NPGDA), EO adduct diacrylate of bisphenol A (Viscoat #700HV), epoxy acrylate having an aromatic ring (Viscoat #540), and 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO) in the amounts (parts by mass) shown in Table 1 or Table 2. However, the resin composition of Comparative Example 1 became cloudy and could not be used to form a secondary resin layer.
[0073] (Resin composition for primary coating) A resin composition for primary coating was obtained by mixing 70 parts by weight of urethane acrylate (B-5), 19 parts by weight of nonylphenol polyethylene glycol acrylate (manufactured by Sartomer, product name "SR504"), 10 parts by weight of isobornyl acrylate, and 1 part by weight of Omnirad TPO.
[0074] [Fabrication of optical fiber] A resin composition for primary coating and a resin composition for secondary coating were each applied to the outer peripheral surface of the glass fiber 13. Next, each resin composition was cured by irradiating with ultraviolet light to form a coating resin layer 16 including a primary resin layer 14 and a secondary resin layer 15, thereby producing the optical fiber 10. The thickness of the primary resin layer 14 was 35 μm, and the thickness of the secondary resin layer 15 was 25 μm.
[0075] (Frequency of optical fiber winding abnormalities) To evaluate the productivity of optical fiber, the frequency of winding defects was measured. At a drawing speed of 1000 m / min, the optical fiber was rewound for 500 km (50 km x 10 bobbins), and the longitudinal transmission loss of each bobbin was evaluated using an OTDR (optical time domain reflectometer). The measurement wavelength was 1550 nm. Optical fiber with 5 or fewer points per 500 km where point discontinuities exceeded 0.05 dB (winding defect frequency) was deemed to have passed.
[0076] [Table 1]
[0077] [Table 2] [Explanation of symbols]
[0078] 10 Optical Fiber 11 cores 12 Clad 13 Glass Fiber 14 Primary resin layer 15 Secondary resin layer 16 Resin coating layer
Claims
1. A resin composition comprising a hydroxyl group-containing urethane compound having a number average molecular weight of 10,000 or more and 40,000 or less, a photopolymerizable compound, and a photopolymerization initiator, A resin composition for secondary coating of optical fiber, wherein the content of the hydroxyl group-containing urethane compound is 0.05 parts by mass or more and 10 parts by mass or less based on 100 parts by mass of a total amount of the resin composition, and the hydroxyl group-containing urethane compound is a reaction product of a polyol having a number average molecular weight of 1,800 to 4,500 and a diisocyanate.
2. The resin composition according to claim 1 , wherein the photopolymerizable compound comprises a urethane (meth)acrylate having a number average molecular weight of 1,000 or more and 6,000 or less.
3. The resin composition according to claim 2, wherein the urethane (meth)acrylate is a reaction product of a polyol having a number average molecular weight of 350 or more and 2500 or less, a diisocyanate, and a hydroxyl group-containing (meth)acrylate.
4. The resin composition according to claim 2 or 3, wherein the photopolymerizable compound further comprises an epoxy (meth)acrylate.
5. The resin composition according to claim 4 , wherein the epoxy (meth)acrylate has an aromatic ring.
6. a glass fiber including a core and a cladding; a primary resin layer that is in contact with and covers the glass fiber; A secondary resin layer that covers the primary resin layer, An optical fiber, wherein the secondary resin layer comprises a cured product of the resin composition according to claim 1 .
7. A coating step of coating an outer periphery of a glass fiber including a core and a clad with the resin composition according to any one of claims 1 to 5; a curing step of curing the resin composition by irradiating the resin composition with ultraviolet light after the coating step; A method for manufacturing an optical fiber, comprising:
Citation Information
Patent Citations
Resin composition for secondary coating of optical glass fiber
JP1988085030A
Liquid curable resin composition
JP1997278850A
Resin composition for coating optical fiber and optical fiber or unit
JP1997328632A
Liquid curable resin composition
JP2005089586A
Liquid state, curable resin composition
JP2006036989A