Manufacturing method of hollow fiber membrane
A non-uniform structured hollow fiber membrane with high cellulose ester content and specific properties addresses the issue of strength loss during cryopreservation, ensuring structural integrity and improved cell survival.
Patent Information
- Application Number
- JP2022559146
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-30
- Filing Date
- 2021-10-26
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-10-26
AI Technical Summary
Hollow fiber membranes made of cellulose esters, such as cellulose acetate, lose strength and are prone to damage due to exposure to extremely low temperatures during cryopreservation, leading to potential structural failure.
A hollow fiber membrane with a non-uniform structure in the thickness direction, high cellulose ester content, and specific properties such as breaking strength, pore diameter, and surface smoothness is developed to maintain strength during cryopreservation.
The membrane effectively suppresses strength loss and maintains structural integrity during freezing and thawing, enhancing cell survival rates during cryopreservation.
Smart Images

Figure 0007582322000009 
Figure 0007582322000010 
Figure 0007582322000011
Abstract
Description
[Technical field]
[0001] The present invention relates to a hollow fiber membrane for cryopreservation of cells. [Background technology]
[0002] Vitrification is known as a method for freezing and preserving cells such as egg cells and embryo cells. In vitrification, an instrument called Cryotop (registered trademark) is used. Cryotop is a specialized instrument with a very thin, rectangular sheet attached to the end of a handle. Cells are placed on the sheet at the end of the Cryotop together with a freezing liquid such as a vitrification liquid, and are frozen and preserved using liquid nitrogen or the like.
[0003] In recent years, a method using hollow fiber membranes (hollow fiber cryopreservation method) has been investigated for the cryopreservation of such cells. In the hollow fiber cryopreservation method, cells are frozen and preserved while being contained inside a hollow fiber membrane made of cellulose acetate. This method is expected to improve the survival rate of cells after freezing.
[0004] However, hollow fiber membranes are relatively fragile materials and may be damaged when used for cryopreservation, which makes them difficult to handle. For example, Patent Document 1 (Japanese Patent No. 5252556), Patent Document 2 (Japanese Patent No. 5051716), and Patent Document 3 (Japanese Patent No. 6667903) disclose hollow fiber support devices and the like for improving the handleability of hollow fibers during cryopreservation.
[0005] As a conventional hollow fiber membrane, for example, a hollow fiber membrane made of cellulose acetate used in hemodialysis, hemodiafiltration, etc., as disclosed in Patent Document 4 (Japanese Patent No. 5440332) and Patent Document 5 (Japanese Patent No. 5212837), is known. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 5252556 [Patent Document 2] Patent No. 5051716 [Patent Document 3] Patent No. 6667903 [Patent Document 4] Patent No. 5440332 [Patent Document 5] Patent No. 5212837 Summary of the Invention [Problem to be solved by the invention]
[0007] As described above, hollow fiber membranes made of cellulose esters such as cellulose acetate are at risk of losing strength and being damaged when exposed to extremely low temperatures such as those used in the cryopreservation of cells, or due to volume changes during freezing and subsequent thawing.
[0008] Therefore, an object of the present invention is to suppress a decrease in strength of a hollow fiber membrane made of cellulose ester for cell cryopreservation when used for the cryopreservation of cells. [Means for solving the problem]
[0009] (1) A hollow fiber membrane for cell cryopreservation comprising a cellulose ester, A hollow fiber membrane, the breaking strength of which when thawed after being frozen by a vitrification freezing method is 80% or more of its breaking strength in a wet state before freezing.
[0010] (2) The hollow fiber membrane according to (1), which has a non-uniform structure in the thickness direction.
[0011] (3) The hollow fiber membrane according to (1) or (2), wherein the average pore size of the outer surface of the hollow fiber membrane is 1.1 times or more the average pore size of the inner surface.
[0012] (4) The hollow fiber membrane according to any one of (1) to (3), wherein the average area ratio of the cross section in the thickness direction is 40% or more and 70% or less.
[0013] (5) The hollow fiber membrane according to any one of (1) to (4), wherein the variation in the area ratio of the thickness direction cross section in the thickness direction is less than 5%.
[0014] (6) The hollow fiber membrane according to any one of (1) to (3), wherein the arithmetic mean roughness of the inner surface of the hollow fiber membrane measured by an atomic force microscope is 20 nm or less. Effect of the Invention
[0015] According to the present invention, in a hollow fiber membrane made of cellulose ester for cell cryopreservation, it is possible to suppress a decrease in strength when used for the cryopreservation of cells. [Brief description of the drawings]
[0016] [Figure 1] 1 is a graph showing the measurement results of the inner diameter of a hollow fiber membrane. [Diagram 2] 1 is a graph showing the measurement results of the membrane thickness of a hollow fiber membrane. [Diagram 3] 1 is a graph showing the measurement results of the breaking strength of a hollow fiber membrane. [Figure 4] 1 is a graph showing the measurement results of the breaking elongation of a hollow fiber membrane. [Diagram 5] 1 is a graph showing the measurement results of the yield strength of a hollow fiber membrane. [Figure 6] FIG. 2 is a schematic diagram for explaining an example of a method for producing a hollow fiber membrane. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, the embodiments of the present invention will be described, but the present invention is not limited thereto. In this specification, the expression in the form of "A to B" means the upper and lower limits of a range (i.e., A or more and B or less), and when no unit is described for A and only a unit is described for B, the unit of A is the same as the unit of B.
[0018] <Hollow fiber membrane> The hollow fiber membrane of this embodiment can be suitably used for cryopreservation of cells. The target cells include egg cells (fertilized eggs, etc.), embryonic cells, pluripotent stem cells including iPS cells and ES cells, and artificial tissues (cell clumps) such as organoids derived from pluripotent stem cells. The cell clumps may be composed of multiple cell types. The cells are cryopreserved while placed inside the hollow fiber membrane. A cell suspension containing individual cells may be cryopreserved inside the hollow fiber membrane.
[0019] (Cellulose ester) The hollow fiber membrane of the present embodiment contains cellulose ester. The ratio of cellulose ester in the material constituting the hollow fiber membrane is preferably 90% by mass or more, more preferably 95% by mass or more, and further preferably 98% by mass or more. The hollow fiber membrane may be composed of only cellulose ester. The hollow fiber membrane preferably has a transparency sufficient to allow the cells contained therein to be seen. Since cellulose ester is a highly transparent material, it is preferable that the ratio of cellulose ester in the material constituting the hollow fiber membrane is high. It is also preferable that the hollow fiber membrane does not dissolve in the vitrification liquid and that the resin component does not elute into the vitrification liquid, and from this viewpoint, it is preferable that the ratio of cellulose ester in the material constituting the hollow fiber membrane is high.
[0020] Examples of cellulose esters include cellulose acetate, cellulose phthalate, and cellulose succinate. The cellulose ester is preferably cellulose acetate. Cellulose acetate is resistant to chlorine, a bactericide, and can be sterilized with chlorine.
[0021] Examples of cellulose acetate include cellulose triacetate, cellulose monoacetate, cellulose diacetate, cellulose acetate butyrate, cellulose acetate propionate, etc. From the viewpoint of durability, etc., the cellulose acetate is preferably cellulose triacetate.
[0022] As cellulose acetate, for example, various cellulose acetates (L-20, 30, 40, 50, 70, LT-35, 55, 105, etc.) with different degrees of acetylation and polymerization are commercially available from Daicel Chemical Industries, Ltd. It is preferable to use cellulose acetate with a relatively low viscosity (a polymer with a relatively low viscosity) having a 6% viscosity of more than 140 mPa s and less than 200 mPa s.
[0023] The acetylation degree of cellulose acetate is preferably 53 to 62%, more preferably 55 to 61.5%, and further preferably 58 to 61.5%. The acetylation degree indicates the degree of substitution of hydroxyl groups in cellulose with acetate groups. Although the theoretical upper limit of the acetylation degree is 62.5%, if the acetylation degree is too high, there is a possibility that the solubility and moldability may decrease.
[0024] (Strength and elongation such as breaking strength) The breaking strength of the hollow fiber membrane of this embodiment, when thawed after being frozen by the vitrification freezing method, is 80% or more, preferably 90% or more, and more preferably 95% or more of the breaking strength when wet before freezing.
[0025] Furthermore, the breaking elongation of the hollow fiber membrane of this embodiment when thawed after being frozen by the vitrification freezing method is preferably 80% or more, more preferably 90% or more, and even more preferably 95% or more of the breaking elongation when wet before freezing.
[0026] Furthermore, the hollow fiber membrane of this embodiment has a yield strength when thawed after being frozen by the vitrification freezing method, which is preferably 80% or more, more preferably 90% or more, and even more preferably 95% or more of the yield strength in a wet state before freezing.
[0027] As described above, the hollow fiber membrane containing the cellulose ester of this embodiment is suppressed from decreasing in strength when used for cryopreservation of cells.
[0028] The breaking strength, breaking elongation and yield strength are measured by the method for measuring strength and elongation (breaking strength, breaking elongation and yield strength) in the examples described later.
[0029] Vitrification is a method of freezing cells in an amorphous glassy state by rapidly lowering the temperature by, for example, immersing the cells in liquid nitrogen, thereby preventing the crystallization of water, which is said to easily occur at -60°C to -15°C. This method is superior to the slow freezing method in that it does not cause damage to cells due to the formation of ice crystals, takes a short time to process, does not require special equipment, and allows for good long-term storage of cells. Many specific methods for vitrification of cells have been developed, and one example is a method in which cells are immersed in a freeze-resistant storage solution and rapidly frozen at -80°C or lower, more preferably -190°C or lower, in liquid nitrogen or an ultra-low temperature freezer.
[0030] The conditions of the vitrification freezing method when comparing the above strength and elongation (breaking strength, breaking elongation and yield strength) before and after freezing and thawing are as follows.
[0031] [Conditions for vitrification freezing method] (Equilibrium liquid) Composition: ethylene glycol (7.5% by mass), dimethyl sulfoxide (7.5% by mass) and water Immersion time: 4 minutes (vitrification fluid) Composition: ethylene glycol (15% by weight), dimethyl sulfoxide (15% by weight), sucrose (0.5 M in vitrification solution) and water. Immersion time: 30 seconds (Crozen storage conditions) Freezing method: Immersion in liquid nitrogen (LN2) Storage method: Store in liquid nitrogen (LN2) for one week. (Method of melting) Immerse in melting solution (1M sucrose solution) for 1 minute Immerse in diluent (0.5M sucrose solution) for 3 minutes Immerse in a cleaning solution (commercially available TCM199 medium (GIBCO)) for 5 minutes, then immerse in another cleaning solution of the same composition for 5 minutes.
[0032] (Shape of hollow fiber membrane, etc.) The inner diameter of the hollow fiber membrane is preferably 30 μm or more and 300 μm or less, and more preferably 35 μm or more and 260 μm or less. The thickness of the hollow fiber membrane is preferably 20 to 200 μm, and more preferably 30 to 150 μm. The membrane thickness can be calculated by "(outer diameter - inner diameter) / 2".
[0033] The hollow fiber membrane (hollow fiber type membrane) is preferably composed of a semipermeable membrane. For cells contained in the hollow fiber membrane and cryopreserved, the membrane does not allow the cells to pass through, but allows the culture medium, cryopreservation solution, and cryoprotectants contained in the preservation solution to pass through, so that the state in which the cells are contained in the internal space of the hollow fiber membrane can be maintained. In other words, this has the advantage that the culture medium, intracellular fluid, etc. in the internal space of the hollow fiber membrane can be easily replaced with the cryopreservation solution.
[0034] The hollow fiber membrane preferably has a hollow ratio of 10 to 65%, and more preferably 12 to 55%. The hollow ratio is the ratio of the area of the hollow part in the cross section of the hollow fiber membrane and is expressed as "hollow part cross-sectional area / (membrane part cross-sectional area+hollow part cross-sectional area)×100(%)".
[0035] The average pore size of the hollow fiber membrane (average pore size of the micropores in the entire membrane) is preferably 10 μm or less. Examples of methods for measuring the average pore size include the bubble point method and mercury intrusion method.
[0036] The hollow fiber membrane of this embodiment is preferably a membrane having a non-uniform structure (asymmetric structure) in the thickness direction. When the hollow fiber membrane has an asymmetric structure, it is considered that the effect of suppressing the decrease in strength of the hollow fiber membrane due to the extremely low temperature used for cryopreservation of cells, freezing and the volume change during subsequent thawing is high. Although the reason is not clear, one possible reason is that the buffer capacity of the polymer chain is higher in the non-uniform structure than in the uniform structure, and the hollow fiber membrane is less susceptible to the influence of the volume change, etc.
[0037] Examples of hollow fiber membranes having an asymmetric structure include hollow fiber membranes having different densities (porosity, cross-sectional aperture ratio) in the thickness direction. Examples of such hollow fiber membranes include membranes having a dense layer on one surface side, which is essentially a separation active layer that defines the pore size of the hollow fiber membrane, and a membrane having a lower density on the other surface side than the dense layer.
[0038] In a hollow fiber membrane having an asymmetric structure, it is preferable that the porosity of one surface is different from that of the other surface. The porosity of the surface having a larger porosity is preferably 1.1 times or more, more preferably 1.3 times or more, of the porosity of the other surface. It is believed that such an asymmetric structure allows heat to be transferred quickly from the solution outside the hollow fiber membrane to the solution inside the hollow fiber membrane during vitrification freezing, thereby suppressing the generation of ice crystals and suppressing damage to the membrane structure and cells. In measuring the porosity of the membrane surface, first, the hollow fiber membrane is imaged using a scanning electron microscope (SEM) at 10,000x magnification. From the obtained image, an area of 762 pixels vertical x 620 pixels horizontal is cut out, and then image analysis software (e.g., WinROOF2013) is used to binarize the image into black and white, and the porosity of the inner and outer surfaces of the hollow fiber membrane is determined. This is performed for 10 fields of view, and the average is calculated to determine the surface porosity.
[0039] The area ratio of a hollow fiber membrane is the area ratio of the solid part (the part where the membrane exists) other than the pore part in the cross section (transverse section) in the thickness direction of the hollow fiber membrane. The area ratio is determined by analyzing an image of the cross section of the hollow fiber membrane taken by SEM. Specifically, As described belowThe membrane is divided into three regions, and the area ratio is measured for each region. The three regions are region A including the outer surface, region B including the inner surface, and a region (center region C) between regions A and B. The magnification of the SEM may be any magnification that allows the pores and solid parts to be recognized, and for example, 5000 to 20000 times is appropriate for measuring the hollow fiber membrane of the present invention. The area ratio is calculated by a method using image analysis. Specifically, the pores and solid parts (polymer parts) are binarized using image analysis software (e.g., WinROOF2013). After the binarization, the area ratio is calculated from the ratio of the total area of the pores to the total area of the polymer parts.
[0040] In this embodiment, the hollow fiber membrane has the above-mentioned asymmetric structure, while being characterized in that the bulk density (area ratio in the cross section in the thickness direction) varies little (preferably is almost constant) in the thickness direction of the membrane. Although the reason is unclear, it is believed that the above-mentioned structural feature allows the membrane to withstand sudden temperature changes and volume changes in the vitrification liquid. Therefore, it is believed that the hollow fiber membrane structure can be prevented from becoming brittle or being destroyed by freezing and melting, and the membrane strength can be maintained. The small variation in area ratio in the thickness direction cross section means, for example, that the difference in area ratio (%) is small for the area A including the outer surface, the area B including the inner surface, and the central area C (the area between the area A and the area B) in the thickness direction cross section. Specifically, when the area ratios of the areas A, B, and C are measured, in all combinations of two area ratios selected from a (area ratio of the area A), b (area ratio of the area B), and c (area ratio of the area C), the absolute value of the difference between the two area ratios is preferably less than 5%, and more preferably less than 3% (see the following formula). For example, the area A is the area from the outer surface to a depth of 30% of the film thickness, and the area B is the area from the inner surface to a depth of 30% of the film thickness. Preferably, |ab|<5%, |bc|<5%, and |ca|<5% More preferably, |ab|<3%, |bc|<3%, and |ca|<3%
[0041] The average area ratio (for example, "(a+b+c) / 3") of the cross section in the thickness direction is preferably 40% or more and 70% or less (see the formula below). 40%≦(a+b+c) / 3≦70%
[0042] In the present invention, the hollow fiber membrane preferably has a highly smooth inner surface. With a highly smooth inner surface, even if an egg cell or embryo cell comes into contact with the inner surface of the hollow fiber membrane, the risk of inflicting damage on the cell surface can be minimized. Here, "highly smooth" means that the arithmetic mean roughness Ra value is 20 nm or less. Since the higher the smoothness, the less damage to cells, the more preferable the Ra value is 10 nm or less, and even more preferable that it is 1 nm or more and less than 8 nm. The arithmetic mean roughness Ra value can be measured using an atomic force microscope (AFM).
[0043] <Manufacturing method of hollow fiber membrane> The present invention also relates to a method for producing a hollow fiber membrane containing the above-mentioned cellulose ester.
[0044] The method for producing the hollow fiber membrane of this embodiment is, for example, the following method. The method for producing the hollow fiber membrane includes the steps of: The method includes a spinning process in which a spinning dope and an inner liquid are discharged from a double-tube nozzle through an air-running portion into a coagulation liquid, the spinning dope is coagulated in the coagulation liquid, and the coagulated product of the spinning dope is pulled out of the coagulation liquid to obtain a hollow fiber membrane, The spinning dope contains a resin raw material containing a cellulose ester, a solvent and a non-solvent, The internal liquid includes water, The temperature of the spinning dope in the nozzle is 70 to 110°C, and the temperature of the internal liquid is 40 to 70°C, The above Spinning solution the ratio of the amount of the solvent to the amount of the non-solvent is 60 / 40 to 80 / 20; The manufacturing method has a nozzle draft ratio of 0.4 to 0.9.
[0045] The concentration of the cellulose ester in the spinning dope is preferably 10 to 30% by mass. In the spinning dope, the ratio of the amount of the solvent to the total amount of the solvent and the non-solvent is preferably 60 to 80% by mass. The solvent is preferably an aprotic polar solvent. The non-solvent is preferably a glycol ester. The linear distance of the air gap is preferably 10 to 50 mm.
[0046] [Spinning process] 6, in the spinning process, spinning dope 10a and inner liquid 10b are discharged from a double-tube nozzle 11 through an air gap 20 into a coagulating liquid 21, the spinning dope is coagulated in the coagulating liquid 21, and the coagulated product of the spinning dope is pulled out of the coagulating liquid 21 to obtain a hollow fiber membrane 16. The hollow fiber membrane is pulled out by, for example, a submerged guide 12 and rollers 13, 14, and 15.
[0047] The nozzle 11 has a double tube shape and includes an outer tube and an inner tube provided inside the outer tube. The fiberizable liquid is discharged from a gap (slit) between the outer tube and the inner tube, and the inner liquid is discharged from inside the inner tube. inner tube Diameter of slit Inner diameter ) for outer tube Diameter of slit Outside diameter ) is preferably 110 to 300%, more preferably 110 to 200%. The diameter of the outer tube is preferably 220 to 400 μm, more preferably 220 to 330 μm. The diameter of the inner tube is preferably 150 to 330 μm, more preferably 150 to 270 μm. The diameter of the inner tube is preferably approximately the same as the diameter of the hollow fiber membrane. The ratio of the cross-sectional area of the inner tube to the cross-sectional area of the slit is preferably 80 to 120%. By using such a nozzle, the linear discharge speed of the membrane-forming solution can be made approximately equal to the take-up speed, so that it is possible to reduce the interfacial friction between the discharged membrane-forming solution and the inner liquid, and to prevent roughening of the inner surface of the hollow fiber membrane. The linear discharge velocity of the film-forming solution was calculated by multiplying the discharge amount of the film-forming solution by the cross-sectional area of the nozzle slit [π(a / 2) 2 -π(b / 2) 2 ] can be calculated (see formula below). Discharge linear velocity of film-forming raw solution [m / min] = Discharge amount of film-forming raw solution / Cross-sectional area of slit The take-up speed is the rotation speed (surface speed) of a roller 13 provided at the outlet of the coagulation bath (see FIG. 6). discharge line Speed vs. Pick-up The nozzle draft ratio, which is the ratio of the speeds (take-up speed / discharge linear speed), is 0.4 to 0.9, and preferably 0.5 to 0.9. In this way, by increasing the discharge linear speed relative to the take-up speed of the membrane-forming dope, a characteristic membrane structure of the hollow fiber of the present invention can be obtained.
[0048] The linear distance of the air travel section 20 (the distance between the tip of the nozzle 11 and the liquid surface of the solidifying liquid 21) is preferably 10 to 50 mm, and more preferably 10 to 40 mm.
[0049] The hollow fiber membrane obtained by the spinning step may be further subjected to a washing step (water washing step) with pure water. In the water washing step, the water preferably flows in the opposite direction to the movement direction of the hollow fiber membrane (countercurrent), but may also flow in the same direction as the movement direction of the hollow fiber membrane (co-current).
[0050] (Spinning solution) The spinning dope 10a contains a resin raw material containing the cellulose ester, a solvent and a non-solvent.
[0051] The temperature (set temperature) of the spinning dope in the nozzle 11 is 70 to 110°C, and preferably 70 to 100°C.
[0052] The concentration of the cellulose ester in the spinning dope is preferably 10 to 30% by mass, more preferably 10 to 25% by mass. If the concentration of the cellulose ester is too low, the strength of the hollow fiber membrane will be low. On the other hand, if the concentration of the cellulose ester is too high, the viscosity of the spinning dope will be too high, which may make it difficult to carry out spinning.
[0053] The solvent is a liquid capable of dissolving the cellulose ester. The solvent is preferably a polar solvent, and is preferably soluble in water. The polar solvent is Non Protic polar solvents are preferred. Examples of aprotic polar solvents include N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMA), dimethylsulfoxide (DMSO), and acetonitrile.
[0054] The non-solvent is a liquid (except water) that does not dissolve cellulose ester. Examples of the non-solvent include glycol ester, glycerin, alcohols, etc., and preferably glycol ester. Examples of the glycol ester include ethylene glycol, triethylene glycol (TEG), polyethylene glycol (polyethylene glycol 200, polyethylene glycol 400, etc.), and propylene glycol.
[0055] In the spinning dope, the ratio of the amount of the solvent (S) to the amount of the non-solvent (NS) (S / NS ratio) is 60 / 40 to 80 / 20, and more preferably 65 / 35 to 75 / 25. If the S / NS ratio in the spinning dope is too small, the dissolution of the cellulose ester becomes unstable, so that the spinning stability may decrease or the asymmetric structure suitable for the application of the present invention may not be obtained. If the S / NS ratio is too large, a hollow fiber membrane with an asymmetric structure may not be obtained or the spinning stability may decrease. The spinning dope may further contain water in addition to the solvent and non-solvent.
[0056] The order of addition of the materials and the mixing method when mixing the resin raw material containing the cellulose ester that is the constituent material of the hollow fiber membrane, the solvent, and the non-solvent are not particularly limited.
[0057] (Internal fluid) The internal liquid contains water. The content of water in the internal liquid is 95 to 100% by mass, and preferably 98 to 100% by mass. It is preferable that the inner surface of the hollow fiber membrane is highly smooth, since this reduces damage caused by contact with the cells to be cryopreserved. In order to improve the smoothness of the inner surface of the hollow fiber membrane, it is preferable to quickly solidify (fix) the inner surface after the spinning dope is discharged from the nozzle before it is affected by external disturbances, thereby preventing excessive phase separation. It is also preferable to prevent external forces such as stretching from being applied to the inner surface during and after solidification, thereby minimizing fluctuations in the inner diameter after the hollow fiber membrane structure is fixed.
[0058] In order to quickly solidify the inner surface, a highly coagulable inner liquid 10b is used in comparison with the spinning dope 10a, or a spinning dope composition and temperature conditions that are easy to solidify are adopted. Or It is preferable to do so. For this reason, in the production method of this embodiment, an inner liquid containing water having a high coagulability is used for the spinning dope containing cellulose ester. In addition to water, ethylene glycol, triethylene glycol, polyethylene glycol 200 or 400, glycerin, propylene glycol, and the like, which are generally used as non-solvents for cellulose esters, can be used alone or in combination. When using an internal liquid mainly made of water, the non-solvents and solvents for cellulose triacetate polymers, such as N-methylpyrrolidone, dimethylacetamide, dimethylformamide, and dimethylsulfoxide, can be added as components other than water up to an upper limit of 5% by weight.
[0059] The temperature (set temperature) of the internal liquid in the nozzle 11 is 40 to 70° C., and preferably 45 to 65° C. As described above, the temperature (set temperature) of the spinning dope in the nozzle 11 is 70 to 110° C., but the internal liquid is preferably set to a temperature lower than this. The temperature of the internal liquid in the nozzle 11 is preferably 10° C. or more lower than the temperature of the spinning dope in the nozzle 11, more preferably 20° C. or more lower, and even more preferably 30° C. or more lower. When the spinning dope 10a and the inner liquid 10b are discharged from the double-tube nozzle 11, it is preferable to provide a temperature difference between the spinning dope and the inner liquid in order to increase the coagulation property (coagulation speed) of the inner surface of the spinning dope (hollow fiber membrane). By increasing the coagulation speed of the inner surface, a hollow fiber membrane having an asymmetric structure (ununiform structure in the thickness direction) can be obtained. In addition, the temperature of the inner liquid can be set within a specific range, and the composition of the coagulation liquid described below can be adjusted within a specific range, or the nozzle draft can be adjusted. ratio Adjusting the above is one of the factors that can increase the smoothness of the inner surface of the hollow fiber membrane and reduce the change in bulk density (area ratio) in the thickness direction of the membrane in the membrane cross section, despite the asymmetric structure. In order to provide a temperature difference between the spinning dope and the inner liquid, it is preferable to use a nozzle having a structure that can separately control the temperatures of the spinning dope and the inner liquid until just before discharge.
[0060] (coagulation liquid) The solidification liquid preferably contains a solvent and a non-solvent (excluding water). In this case, the solidification liquid may further contain water in addition to the solvent and non-solvent. The ratio of the total amount of the solvent and the non-solvent in the coagulation liquid (concentration of the coagulation liquid) is 60 to 90 mass %, and preferably 65 to 90 mass %, which makes it possible to obtain the characteristic structure of the hollow fiber membrane of the present invention.
[0061] The temperature of the coagulation liquid is preferably 20 to 60°C, and more preferably 30 to 50°C. EXAMPLES
[0062] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0063] Example 1 The hollow fiber membrane of Example 1 was produced under the following conditions by the method for producing a hollow fiber membrane described in the embodiment.
[0064] (Composition of spinning solution) Raw resin (cellulose ester): Cellulose triacetate (CTA) (LT75, Daicel Chemical Industries, Ltd.) Raw resin concentration (polymer concentration): 17.5% by mass (in spinning solution) Solvent: N-methylpyrrolidone (NMP) Non-solvent: Triethylene glycol (TEG) [Solvent / non-solvent (S / NS) ratio = 7 / 3] Internal fluid: water
[0065] (Preparation of spinning solution) The above raw resin powder was mixed with other materials to prepare a spinning dope to be used in the spinning process.
[0066] (Composition of coagulation liquid) Solvent(S): NMP Non-solvent (NS): TEG water Concentration of coagulation liquid [(mass of S + mass of NS) / mass of coagulation liquid]: 78% by mass The S / NS ratio is the same as that of the spinning dope.
[0067] (Spinning process conditions) Discharge temperature of spinning dope (set temperature): 93℃ Discharge temperature of internal liquid (water) (set temperature): 55℃ Nozzle: Double tubular nozzle (outer tube diameter: 270 μm, inner tube diameter: 200 μm) Air gap length: 25m m Aerial travel time: 0.025 seconds Coagulation liquid temperature: 43℃ Pulling speed: 60m / min Nozzle draft ratio: 0.78
[0068] [Conditions for the washing process] Flow in the washing tank: Countercurrent Temperature 98℃
[0069] [Examples 2 and 3] The nozzle draft ratio was changed as shown in Table 1. Other than that, the hollow fiber membranes of Examples 2 and 3 were produced in the same manner as in Example 1. The arithmetic mean roughness and area ratio of the inner surface of the obtained hollow fiber membrane were measured, and the results are shown in Table 2.
[0070] [Comparative Examples 1 and 2] As shown in Table 1, the compositions of the spinning dope, inner liquid, and coagulation liquid, as well as the manufacturing conditions, were changed. Liquid paraffin was used as the inner liquid, and the set temperature of the inner liquid was not particularly controlled but was approximately the same as the temperature of the spinning dope. Other than that, the hollow fiber membranes of Comparative Example 1 and Comparative Example 2 were manufactured in the same manner as in Example 1.
[0071] [Table 1]
[0072] [Measurement of area ratio] A wet hollow fiber membrane was immersed in liquid nitrogen to freeze, then removed from the liquid nitrogen and immediately folded and cut to obtain a sample with a smooth cross section (cross section in the thickness direction). The sample was fixed to a sample stage so that the cross section could be observed, and carbon deposition was performed on the cross section of the sample. The cross section of the sample after deposition was imaged using a scanning electron microscope (Hitachi S-2500) at an acceleration voltage of 5 kV and a magnification of 10,000 times. In the obtained image, the central areas of the regions corresponding to each of the above-mentioned regions A to C (region A including the outer surface, region B including the inner surface, and central region C between regions A and B) were binarized using image analysis software WinROOF2013 to binarize the pores and polymer parts. After the binarization, the area ratio was calculated from the ratio of the pores and polymer parts. Here, region A is the region from the outer surface to a depth of 30% of the film thickness, and region B is the region from the inner surface to a depth of 30% of the film thickness. In addition, since the structure may become unclear due to the fracture or dissolution of part of the cross section by the electron beam, in such cases, measurements were performed using a part with a clear structure, or the sample was changed and the photograph was taken again. The results of the area ratio measurements are shown in Table 2.
[0073] [Measurement of arithmetic mean roughness] A hollow fiber membrane was prepared as a sample by opening it (cutting it diagonally in the longitudinal direction) so that the inner surface of the hollow fiber membrane could be observed. Observations were made in air in DFM mode using an atomic force microscope E-Sweep (Hitachi High-Technologies Corporation). Si-DF3 was used as the cantilever and a 20 μm scanner was used as the scanner. The observation field was set to 2 μm square, and the arithmetic mean roughness (Ra) of the inner surface of the hollow fiber membrane was measured at 256 × 256 pixels. The measurement results of the arithmetic mean roughness (Ra) are shown in Table 2.
[0074] [Table 2]
[0075] <Freezing storage test> A cryopreservation test using a vitrification freezing method was carried out on the hollow fiber membranes of Examples 1 to 3 and Comparative Examples 1 and 2. The conditions for the vitrification freezing method were the same as those for measuring the breaking strength (breaking strength when thawed after being frozen by the vitrification freezing method) described above. For each of the hollow fiber membranes of Examples 1 to 3 and Comparative Examples 1 and 2 in the frozen storage test, the following measurements were performed in the initial dry state ("dry state"), in the water-wet state ("wet state"), in the equilibrium liquid-infiltrated state ("equilibrium liquid"), in the vitrification liquid-infiltrated state ("vitrification liquid"), and in the frozen and then thawed state ("post-thawing").
[0076] [Measurement of inner diameter, outer diameter and membrane thickness of hollow fiber membrane] The inner diameter, outer diameter and membrane thickness were measured by the following method.
[0077] An appropriate number of hollow fiber membranes are passed through a hole with a diameter of 3 mm drilled in the center of a slide glass so that the hollow fiber membranes do not fall out, and the hollow fiber membranes are cut with a razor along the top and bottom surfaces of the slide glass to obtain a cross-sectional sample of the hollow fiber membrane. The inner and outer diameters of the obtained cross-sectional sample of the hollow fiber membrane are measured using a projector (Nikon PROFILE PROJECTOR V-12). Specifically, the dimensions of the outer surface of the hollow fiber membrane in the XX and YY directions (two perpendicular directions on the cross section) were measured for each hollow fiber membrane cross section, and the arithmetic average of these values was used as the outer diameter of each hollow fiber membrane cross section. In addition, the dimensions of the hollow part in the XX and YY directions (two perpendicular directions on the cross section) were measured for each hollow fiber membrane cross section, and the arithmetic average was used as the inner diameter of each hollow fiber membrane cross section. Note that similar measurements were performed for 10 cross sections, and the average values were used as the inner and outer diameters. The membrane thickness (average value) is calculated from the measurement results (average value) of the inner diameter and the inner diameter of the hollow fiber membrane by the formula "(outer diameter-inner diameter) / 2".
[0078] The measurement results (average values) of the inner diameters of the hollow fiber membranes are shown in Table 3 (Fig. 1), and the measurement results (average values) of the membrane thicknesses are shown in Table 4 (Fig. 2). Note that for the comparative examples, the strength of the hollow fiber membranes was low after melting, and it was not possible to prepare a cross-sectional sample of the hollow fiber membrane, so the inner diameter and membrane thickness could not be measured.
[0079] [Table 3]
[0080] [Table 4]
[0081] [Measurement of strength and elongation] For the hollow fiber membranes of Examples 1 to 3 and Comparative Examples 1 and 2, the strength and elongation (breaking strength, breaking elongation, and yield strength) were measured by the following method.
[0082] The strength and elongation of the hollow fiber membrane was measured using a tensile testing machine (UTMII manufactured by Toyo Baldwin Co., Ltd.) by cutting one hollow fiber membrane to a length of approximately 15 cm and attaching it between chucks (distance of approximately 10 cm) so that there was no slack. The hollow fiber membrane was then pulled at a crosshead speed of 10 cm / min in a temperature and humidity environment of 20±5°C and 60±10% Rh. From the obtained SS curve, the load (breaking strength) and elongation (breaking elongation) per single fiber at the breaking point of the hollow fiber membrane, and the load (yield strength) and elongation (yield elongation) per single fiber at the yield point were read. Specifically, the load and elongation were obtained using the method shown in
[0061] of JP2011-212638A. The measurement results of breaking strength, breaking elongation and yield strength are shown in Tables 5 to 7 (FIGS. 3 to 5). For each of the examples and comparative examples, the measurements were carried out five times, and the average values are shown as the measured values.
[0083] [Table 5]
[0084] [Table 6]
[0085] [Table 7]
[0086] As shown in Table 5 (FIG. 3), in the hollow fiber membranes of the comparative examples, the breaking strength is significantly reduced in the state after thawing after freezing compared to the values before freezing ("dry state", "wet state", "equilibrium liquid", and "vitrification liquid" in the table and figures). In contrast, in the case of the hollow fiber membranes of the examples, the breaking strength is hardly reduced even in the state after thawing compared to the values before freezing. In addition, in the hollow fiber membranes of the examples, the breaking strength in the thawed state after freezing by the vitrification freezing method is 95% or more of the breaking strength in the wet state before freezing ("wet state").
[0087] Furthermore, as shown in Tables 6 and 7 (FIGS. 4 and 5), in the hollow fiber membranes of the comparative examples, the breaking elongation and yield strength are significantly lower after freezing and thawing than the values before freezing. In contrast, in the hollow fiber membranes of the examples, the breaking elongation and yield strength are hardly lowered even after thawing than the values before freezing. In the hollow fiber membranes of the examples, the breaking elongation or yield strength in the thawed state after freezing by the vitrification freezing method is 95% or more of the breaking elongation or yield strength in the wet state before freezing ("wet state").
[0088] These results show that the hollow fiber membrane of the present invention can suppress a decrease in strength when used for cryopreservation of cells.
[0089] <Evaluation of cell viability> Using the hollow fiber membranes of Examples 1 to 3 and Comparative Example 1, cells (pig-derived embryonic cells) were frozen by vitrification freezing method (hollow fiber cryopreservation method), and after thawing, the number of viable cells was measured and the survival rate (the ratio of the number of viable cells to the number of test cells) was calculated.
[0090] In addition, cells were frozen by vitrification freezing method (cryotop method) using Cryotop (registered trademark, manufactured by Kitasato Corporation), a commercially available cell cryopreservation device, and after thawing, the number of viable cells was counted and the survival rate was calculated.
[0091] The results of the evaluation of the viability, together with the number of test cells (the number of cells subjected to the test) and the number of viable cells, are shown in Table 8. The conditions for the vitrification freezing method were the same as those for measuring the strength and elongation described above, and in the hollow fiber membrane cryopreservation method, the cells were cryopreserved while being contained inside the hollow fiber membrane.
[0092] [Table 8]
[0093] As shown in Table 8, when cells were cryopreserved using the hollow fiber membranes of Examples 1 to 3, the ratio of surviving cells after thawing (viability) was higher than that of the commercially available product and the comparative example. This result shows that the hollow fiber membranes of Examples 1 to 3 can be suitably used for cell cryopreservation. [Explanation of symbols]
[0094] 10a spinning dope, 10b inner liquid, 11 nozzle, 12 submerged guide, 13, 14, 15 rollers, 16 hollow fiber membrane, 20 air-passing portion, 21 coagulating liquid.
Claims
1. A method for producing a hollow fiber membrane, comprising the steps of: The method includes a spinning process in which a spinning dope and an inner liquid are discharged from a double-tube nozzle through an air-running portion into a coagulation liquid, the spinning dope is coagulated in the coagulation liquid, and the coagulated product of the spinning dope is pulled out of the coagulation liquid to obtain a hollow fiber membrane, The spinning dope contains a resin raw material containing a cellulose ester, a solvent and a non-solvent, the coagulation liquid comprises the solvent and the non-solvent; The internal liquid includes water, The temperature of the spinning dope at the nozzle is 70 to 110° C. The temperature of the internal liquid at the nozzle is 40 to 70° C. The ratio of the amount of the solvent to the amount of the non-solvent in the spinning dope is 60 / 40 to 80 / 20; The nozzle draft ratio is 0.4 to 0.
9. The hollow fiber membrane is for cryopreservation of cells containing a cellulose ester, the breaking strength of the hollow fiber membrane when thawed after being frozen by a vitrification freezing method is 80% or more of the breaking strength of the hollow fiber membrane when wet before freezing; The method for producing a hollow fiber membrane, wherein the hollow fiber membrane has an average area ratio of 40% or more and 70% or less in the thickness direction cross section.
2. The method for producing a hollow fiber membrane according to claim 1, wherein the concentration of the cellulose ester in the spinning dope is 10 to 30% by mass.
3. The method for producing a hollow fiber membrane according to claim 1 or 2, wherein a ratio of a total amount of the solvent and the non-solvent in the coagulation liquid is 60 to 90 mass%.
4. the solvent is an aprotic polar solvent, The method for producing a hollow fiber membrane according to any one of claims 1 to 3, wherein the non-solvent is a glycol ester.
5. The method for producing a hollow fiber membrane according to any one of claims 1 to 4, wherein a temperature of the inner liquid in the nozzle is lower by 10°C or more than a temperature of the spinning dope in the nozzle.
6. The method for producing a hollow fiber membrane according to any one of claims 1 to 5, wherein a linear distance of the air-tight portion is 10 to 50 mm.
Citation Information
Patent Citations
JP1975051716A
Electrophotographic light sensitive composition
JP1977012837A
Semiconductor switch unit
JP1977052556A
Connection of pressure fluid feed pipes
JP1979040332A
Cellulose derivative hollow fiber membrane
JP2002306937A