Manufacturing method of press-molded products
A two-step press-forming method with convex portions in the first step addresses the issue of ridgeline cracking in high-strength steel press-formed products, ensuring structural integrity by reducing tensile forces and thickness reduction.
Patent Information
- Application Number
- JP2024500468
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-12-07
- Filing Date
- 2023-09-27
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2043-09-27
AI Technical Summary
Existing methods fail to effectively suppress cracks at the ridgeline connections in press-formed products with T-shaped or L-shaped top plate portions, particularly when using high-strength steel plates, due to tensile forces during the press-forming process.
A two-step press-forming method is employed, where an intermediate molded product with convex portions is formed in the first step to reduce tensile forces, followed by shaping into the final product, ensuring the ridgeline connections are strengthened to prevent cracking.
The method significantly reduces the occurrence of cracks at the ridgeline ends of press-formed products, even with high-strength steel, by minimizing tensile forces and material thickness reduction, thereby enhancing the structural integrity of vehicle body parts.
Smart Images

Figure 0007582548000007 
Figure 0007582548000008 
Figure 0007582548000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a press-formed product having at least a top plate portion, a vertical wall portion, and a ridge portion which is a connection portion between the top plate portion and the vertical wall portion. [Background technology]
[0002] As automobile crash safety standards become stricter, progress is being made in improving the crash safety of car bodies, but in light of recent carbon dioxide emission regulations, it is also necessary to reduce the weight of car bodies. Therefore, in order to achieve both crash safety performance and weight reduction of car bodies, metal plates with even higher strength than before are being used for car bodies. Recently, efforts have been made to apply ultra-high tensile steel plates of 1.5 GPa class or higher. However, high-strength metal plates generally have poor ductility, so when press-formed products are manufactured as car body parts, cracks are likely to occur from the edges during the press forming process.
[0003] Conventionally, methods for preventing cracks in press-formed products have been adopted. For example, Patent Document 1 discloses a method for preventing cracks occurring in a connection portion between a wall portion continuing from a connecting side portion and a flange portion continuing from the wall portion when a T-shaped part having a T-shaped top plate portion in which a vertical side portion and a horizontal side portion are connected by a connecting side portion is press-formed. In addition, Patent Document 2 discloses a method for preventing cracks caused by stretch flange forming of a press-formed product having a flat plate portion having a concave outer peripheral edge portion in which a part of the outer peripheral edge is concave inward, and a flange portion bent along the concave outer peripheral edge portion. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-13952 A [Patent Document 2] JP 2016-104492 A Summary of the Invention [Problem to be solved by the invention]
[0005] The method disclosed in Patent Document 1 first forms an intermediate part in a first forming step, which has a convex part formed on the vertical side of the connecting side of the top plate, and a curved R part formed by lifting up the bottom R part connecting the wall part and the flange part continuing from the connecting side. Then, in a second forming step, the convex part and the curved R part of the intermediate part are crushed to form a T-shaped part of the target shape. This is said to allow material to flow into the wall part continuing to the connecting side, preventing cracks from occurring in the connecting part between the wall part and the flange part.
[0006] In addition, the method disclosed in Patent Document 2 involves applying plastic deformation to a portion of a blank material that corresponds to a flat portion, and drawing the material into the portion that has been plastically deformed, thereby drawing the material to a portion that corresponds to a bent portion of a flange portion, and providing excess material to the portion that corresponds to the bent portion. The blank material with the excess material is then bent to form a press-formed product having a flange portion. This is said to effectively prevent the occurrence of stretch flange cracking without reducing the formability of the bent portion of the flange portion of the press-formed product.
[0007] Thus, the methods disclosed in Patent Documents 1 and 2 were intended to prevent cracks in the portion of the press-formed product subjected to stretch flange deformation. On the other hand, for example, in a press-formed product having a top plate portion having a horizontal side portion and a vertical side portion and being substantially T-shaped or substantially L-shaped in top view, cracks may occur at the end of the ridge portion connecting the vertical wall portion and the horizontal side portion at the tip side of the horizontal side portion, unlike cracks caused by stretch flange deformation. However, the methods disclosed in Patent Documents 1 and 2 above could not suppress cracks at the end of the ridge portion connecting the vertical wall portion and the horizontal side portion of such a press-formed product having a top plate portion having a substantially T-shaped or substantially L-shaped shape.
[0008] Furthermore, even in press molding of a press-formed product having a top plate portion, a vertical wall portion continuing to the top plate portion via a ridge portion, and a vertical flange portion continuing to the vertical wall portion, it was difficult to suppress cracks that occurred at the end of the ridge portion.
[0009] Furthermore, even in press molding of a press-molded product that has a top plate portion and a vertical wall portion that continues to the top plate portion via a ridge portion, where the top plate portion or a part of it is curved when viewed from above, and the vertical wall portion continues to the inside of the curvature in the top plate portion, it was also difficult to suppress cracks that occur at the end of the ridge portion.
[0010] The present invention has been made in consideration of the above-mentioned problems, and its object is to provide a method for manufacturing a press-molded product having a top plate portion and a vertical wall portion continuing to the top plate portion via a ridge portion, which suppresses the occurrence of cracks during press molding. [Means for solving the problem]
[0011] In order to solve the above problems and achieve the objectives, (1) The manufacturing method of a press-formed product of the present invention is a manufacturing method of a press-formed product having at least a top plate portion, a vertical wall portion, and a ridge portion which is a connection portion between the top plate portion and the vertical wall portion, and includes a first forming process of press-forming a metal plate blank into an intermediate formed product having an intermediate top plate portion, an intermediate vertical wall portion, and an intermediate ridge portion connecting the intermediate top plate portion and the intermediate vertical wall portion, and having a convex portion higher than a reference height of the top plate surface at one or more locations on the intermediate top plate portion including the intermediate ridge portion, and a second forming process of press-forming the intermediate formed product into the press-formed product.
[0012] (2) The manufacturing method of the press-molded product according to the present invention, in the invention of (1) above, is characterized in that, in the shape of the press-molded product, the top plate portion has a horizontal side portion, a vertical side portion, and a connecting R portion where the horizontal side portion and the vertical side portion are connected, and is approximately T-shaped or approximately L-shaped in a top view, and is provided with a ridge portion that connects to the top plate portion from the horizontal side portion of the top plate portion to the connecting R portion and the vertical side portion, a vertical wall portion that continues via the ridge portion from the horizontal side portion of the top plate portion to the connecting R portion and the vertical side portion, and a bottom flange portion that continues from the vertical wall portion, The plate portion has an intermediate horizontal side portion, an intermediate vertical side portion, and an intermediate connection R portion connecting the intermediate horizontal side portion and the intermediate vertical side portion, and is approximately T-shaped or approximately L-shaped when viewed from above, and the height of the intermediate vertical side portion of the intermediate top plate portion is lower than the height of the vertical side portion in the target product shape.Further, in the first molding process, the intermediate molded product is press-molded into an intermediate molded product having a convex portion higher than the height of the vertical side portion at the end of the intermediate horizontal side portion of the intermediate top plate portion including the intermediate ridge portion of the intermediate molded product and / or at the intermediate connection R portion of the intermediate top plate portion including the intermediate ridge portion of the intermediate molded product.
[0013] (3) In the manufacturing method of the press-molded product of the present invention, in the above-mentioned (2) invention, in the first molding process, the intermediate molded product is press-molded to have a convex portion whose height gradually increases toward the tip side of the intermediate horizontal side portion of the intermediate top plate portion including the intermediate ridge portion, the convex portion having a height that gradually increases toward the tip side of the intermediate horizontal side portion.
[0014] (4) In the manufacturing method of the press-molded product of the present invention, in the above-mentioned (2) invention, in the first molding process, the intermediate molded product is press-formed into the intermediate horizontal side portion of the intermediate top plate portion including the intermediate ridge portion, having the convex portion whose height is constant up to the tip side of the intermediate horizontal side portion.
[0015] (5) In the manufacturing method of the press-molded product of the present invention, in the above-mentioned (2) invention, in the first molding step, the convex portion is formed in the intermediate connection R portion including the intermediate ridge portion, and further, the intermediate molded product is press-molded to have the intermediate horizontal edge portion of the intermediate top plate portion whose height matches the height of the convex portion of the intermediate connection R portion.
[0016] (6) In the manufacturing method of a press-molded product of the present invention, in the above-mentioned (1) invention, in the first molding process, the intermediate molded product is press-molded to have a convex portion higher than a reference height of the top plate surface at one or more locations of the intermediate top plate portion including the end portion of the intermediate ridge portion.
[0017] (7) In the manufacturing method of a press-formed product of the present invention, in the above-mentioned (6), the press-formed product has a vertical flange portion continuous with the vertical wall portion, and in the first forming process, the intermediate top plate portion including the intermediate ridge portion is press-formed into an intermediate formed product having the convex portion at the end portion on the vertical flange portion side of the press-formed product.
[0018] (8) The manufacturing method of a press-molded product of the present invention is the same as that of the above-mentioned (6), in which the press-molded product has a top plate portion or a portion of the top plate portion that is curved when viewed from above, and the vertical wall portion continues on the inside of the curvature in the top plate portion, and in the first molding step, the press-molded product is press-molded into an intermediate molded product having the convex portion on the intermediate top plate portion including the end portion of the intermediate ridge portion. Effect of the Invention
[0019] In the present invention, a press-formed product having a top plate portion and a vertical wall portion continuing to the top plate portion through a ridge portion can be manufactured while suppressing the occurrence of cracks during press forming. In particular, for a press-formed product having a top plate portion having a horizontal side portion and a vertical side portion and having an approximately T-shaped or approximately L-shaped top plate portion in a top view, cracks at the ridge portion at the tip side of the horizontal side portion can be suppressed. Also, for a press-formed product having a top plate portion, a vertical wall portion continuing to the top plate portion through the ridge portion, and a vertical flange portion continuing to the vertical wall portion, cracks at the end of the ridge portion close to the vertical flange side can be suppressed. Furthermore, for a press-formed product having a top plate portion and a vertical wall portion continuing to the top plate portion through the ridge portion, the top plate portion or a part of the top plate portion is curved in a top view, and the vertical wall portion is continuous to the inside of the curve of the top plate portion, cracks at the end of the ridge portion can be suppressed. [Brief description of the drawings]
[0020] [Figure 1] Figure 1 shows an example of a manufacturing method for a press-formed product according to embodiment 1 of the present invention, in which the ridge portion on the tip side of the horizontal side and the entire horizontal side portion of the top plate are made higher as convex portions, and is a diagram illustrating a first forming process in which the press-formed product is press-formed into an intermediate shape in which the vertical wall height at the vertical side portion of the top plate is lower than the target shape, a second forming process in which the press-formed product has the vertical wall height of the target shape, and why cracks at the end portion of the ridge portion on the horizontal side of the press-formed product of the target shape can be suppressed ((a) first forming process, (b) second forming process). [Diagram 2] Figure 2 is a diagram illustrating an example of a manufacturing method for a press-formed product according to embodiment 1 of the present invention in which the convex portion is only a connecting R portion, and which illustrates a first forming process in which the press-formed product is press-formed into an intermediate shape in which the vertical wall height at the vertical side portion of the top plate is lower than the target shape, a second forming process in which the press-formed product has the vertical wall height of the target shape, and the reason why cracks at the end portion of the horizontal side ridge portion of the press-formed product of the target shape can be suppressed ((a) first forming process, (b) second forming process). [Diagram 3]FIG. 3 is a diagram showing an example of a press-formed product having a top plate portion that is substantially T-shaped when viewed from above, which is an object to be manufactured in the present invention, in which the tip of the horizontal side portion of the top plate is only slightly rounded. [Figure 4] FIG. 4 is a diagram showing an example of a press-formed product having a top plate portion that is substantially T-shaped when viewed from above, which is an object to be manufactured in the present invention, in which the tip of the horizontal side portion of the top plate is largely rounded. [Diagram 5] FIG. 5 is a diagram showing an example of a press-molded product to be manufactured in the present invention, which has a top plate portion that is substantially L-shaped when viewed from above. [Figure 6] FIG. 6 is a diagram for explaining a conventional manufacturing method for press-forming a press-formed product having a substantially T-shape in top view in two steps ((a) a first forming step, (b) a second forming step). [Figure 7] FIG. 7 is a contour diagram showing the results of determining the sheet thickness change rate at the bottom dead center of the intermediate shape and the target shape of a roughly T-shaped press-formed product press-formed in a conventional two-step process ((a) intermediate shape, (b) target shape). [Figure 8] FIG. 8 is a diagram illustrating locations where cracks occur in a press-molded product having a substantially T-shaped top plate portion press-molded by a conventional manufacturing method, and the reasons for this. [Figure 9] Figure 9 is a diagram showing an example of a punch used in press molding of an intermediate-shaped press-formed product in which a convex portion is formed in the top plate portion in the first molding process in the manufacturing method of a press-formed product according to embodiment 1 of the present invention. It is a diagram showing a specific example of a punch that forms a "convex portion" of uniform height on the ridge portion that continues from the position where the horizontal side portion of the top plate portion extends, and further molds into an intermediate molded product having a top plate horizontal side portion whose height matches the height of the convex portion. [Figure 10] Figure 10 is a diagram showing an example of a punch used in press forming an intermediate-shaped press-formed product in which a convex portion is formed in the top plate portion in the first forming process in the manufacturing method of a press-formed product according to embodiment 1 of the present invention. It is a diagram showing a specific example of a punch that forms a ``convex portion'' on the ridge portion that continues from the position where the lateral side portion of the top plate portion extends, so that the convex portion gradually becomes higher toward the tip of the ridge portion, and further forms an intermediate molded product having a top plate lateral side portion that has a height that matches the height of the convex portion. [Figure 11] FIG. 11 is a diagram showing an example of a punch used in press molding of an intermediate-shaped press-molded product in which a convex portion is formed in the top plate portion in the first molding process in a manufacturing method of a press-molded product relating to embodiment 1 of the present invention, and is a diagram showing a specific example of a punch that forms a convex portion in the joint R portion of the top plate portion. [Figure 12] FIG. 12 is a contour diagram showing the results of determining the sheet thickness change rate at the bottom dead center of the intermediate shape and the target shape of a substantially T-shaped press-formed product press-formed by the manufacturing method of the press-formed product using the punch shown in FIG. 10(a) according to the first embodiment of the present invention ((a) intermediate shape, (b) target shape). [Figure 13] FIG. 13 is a contour diagram showing the results of determining the sheet thickness change rate at the bottom dead center of the intermediate shape and the target shape of a roughly T-shaped press-formed product press-formed in two conventional steps when the product target shape is as shown in FIG. 4 ((a) intermediate shape, (b) target shape). [Figure 14] FIG. 14 is a contour diagram showing the results of determining the sheet thickness change rate at the bottom dead center of the intermediate shape and the target shape of a substantially T-shaped press-formed product press-formed by the manufacturing method of the press-formed product using the punch (convex portion) shown in FIG. 11(a) according to the first embodiment of the present invention ((a) intermediate shape, (b) target shape). [Figure 15] FIG. 15 is a contour diagram showing the results of determining the sheet thickness change rate at the bottom dead center of the intermediate shape and the target shape of a substantially T-shaped press-formed product press-formed by the manufacturing method of the press-formed product using the punch (height Up of the convex portion + horizontal side portion) shown in FIG. 11(b) according to the first embodiment of the present invention ((a) intermediate shape, (b) target shape). [Figure 16] FIG. 16 shows the results of the plate thickness change rate obtained for the intermediate shape and the target shape of a press-formed product having a roughly L-shaped top plate portion press-formed by a conventional method ((a) intermediate shape, (b) target shape). [Figure 17]FIG. 17 is a diagram showing the results of the plate thickness change rate obtained for the intermediate shape and the target shape of a press-formed product having a substantially L-shaped top plate portion press-formed by the method according to the first embodiment of the present invention ((a) intermediate shape, (b) target shape). [Figure 18] FIG. 18 is an explanatory diagram of a method for producing a press-molded product according to the second embodiment of the present invention. [Figure 19] FIG. 19 is an explanatory diagram of an intermediate punch used in a manufacturing method for a press-formed product according to the second embodiment of the present invention. [Figure 20] FIG. 20 is an explanatory diagram of an intermediate molded product according to the second embodiment of the present invention. [Figure 21] FIG. 21 is a diagram illustrating the sheet thickness reduction rate of a press-formed product formed according to the second embodiment of the present invention. [Figure 22] FIG. 22 is an explanatory view of another aspect of the intermediate punch according to the second embodiment of the present invention. [Diagram 23] FIG. 23 is an explanatory diagram of a press-formed product having a target shape according to the second embodiment of the present invention. [Figure 24] FIG. 24 is an explanatory diagram of a conventional method for press-forming the press-formed product shown in FIG. 23 in one step. [Diagram 25] FIG. 25 is an explanatory diagram of the sheet thickness reduction rate when press forming is performed by the conventional method shown in FIG. [Figure 26] FIG. 26 is an explanatory diagram of a method for producing a press-molded product according to the third embodiment of the present invention. [Figure 27] FIG. 27 is an explanatory diagram of an intermediate punch used in a manufacturing method for a press-molded product according to the third embodiment of the present invention. [Figure 28] FIG. 28 is an explanatory diagram of an intermediate molded product according to the third embodiment of the present invention. [Figure 29] FIG. 29 is a diagram illustrating the sheet thickness reduction rate of a press-formed product formed according to the third embodiment of the present invention. [Diagram 30] FIG. 30 is an explanatory diagram of a press-formed product having a target shape according to the third embodiment of the present invention. [Diagram 31]FIG. 31 is an explanatory diagram of a conventional method for press-forming the press-formed product shown in FIG. 30 in one step. [Diagram 32] FIG. 32 is an explanatory diagram of the sheet thickness reduction rate when press forming is performed by the conventional method shown in FIG. [Diagram 33] FIG. 33 is an explanatory diagram for explaining the mechanism by which cracks occur in the press-formed product press-formed by the conventional method shown in FIG. [Diagram 34] FIG. 34 is a diagram for explaining the inclination angle of the tip side of the horizontal side portion in the press-formed product of the intermediate shape in Example 1. As shown in FIG. [Diagram 35] FIG. 35 is a diagram for explaining a height increment for uniformly increasing the height of a portion on the tip side of a horizontal side portion in a press-formed product of an intermediate shape in Example 1. In FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] (Embodiment 1) Before describing the manufacturing method of the press-formed product according to the first embodiment of the present invention, the press-formed product to which the present invention is applied and the occurrence of cracks in the press-formed product will be described below. Note that the same or similar components are denoted by the same reference numerals, and duplicated descriptions will be omitted.
[0022] <Press-molded products targeted by the present invention> FIG. 3 shows a press-molded product 1 having a top plate portion 3, a vertical wall portion 5, and a bottom flange portion 7, as an example of a press-molded product to be manufactured in the present invention.
[0023] 3, the top panel 3 has a horizontal side 3a and a vertical side 3b and is generally T-shaped when viewed from above. Furthermore, the top panel 3 has an arc-shaped connecting R portion 3c extending from the horizontal side 3a to the vertical side 3b.
[0024] 3, the vertical wall portion 5 is continuous from the horizontal side portion 3a to the vertical side portion 3b of the top plate portion 3 via a ridge portion 9. The vertical wall portion 5 has a horizontal side vertical wall portion 5a that is continuous from the horizontal side portion 3a via the horizontal side ridge portion 9a, and a vertical side vertical wall portion 5b that is continuous from the vertical side portion 3b via the vertical side ridge portion 9b. Furthermore, the vertical wall portion 5 has a connection R side vertical wall portion 5c that is continuous from the connection R portion 3c via the connection R side ridge portion 9c and connects the horizontal side vertical wall portion 5a and the vertical side vertical wall portion 5b.
[0025] As shown in Figure 3, the bottom flange portion 7 is continuous with the vertical wall portion 5, and is formed continuous with each of the horizontal side vertical wall portion 5a, the vertical side vertical wall portion 5b, and the connection R side vertical wall portion 5c.
[0026] Conventionally, such a press-formed product 1 has been press-formed in two steps, a first forming step and a second forming step, as shown in FIG.
[0027] First, in the first forming step, as shown in Fig. 6(a), a blank 11, which is a metal plate, is sandwiched between a punch 13 and a pad 15, and a die 17 is moved relatively toward the punch 13 to press-form an intermediate-shaped press-formed product 21 (see Fig. 6(b)) having a lower vertical wall height than the target shape. Here, a top plate portion 23 of the intermediate-shaped press-formed product 21 is press-formed into the same shape as the top plate portion 3 (see Fig. 3) of the press-formed product 1 having the target shape.
[0028] Then, in the subsequent second forming process, as shown in Figure 6 (b), the top plate portion 23 of the intermediate-shaped press-formed product 21 is clamped between a punch 31 and a pad 33, and the die 35 is moved relatively toward the punch 31 to press-form a press-formed product 1 of the target shape having a vertical wall height higher than that of the intermediate shape.
[0029] However, when the press-formed product 21 in the intermediate shape is press-formed into the press-formed product 1 in the target shape (FIG. 3) in the second forming step, cracks may occur at the end of the horizontal edge 9a connecting the horizontal edge 3a and the horizontal vertical wall 5a. The end of the horizontal edge 9a refers to the portion on the tip side of the horizontal edge 9a in the direction in which the horizontal edge 3a extends.
[0030] In order to determine the cause of cracks occurring at the end of the horizontal edge ridge portion 9a of the press-formed product 1 having such an approximately T-shaped top plate portion 3, a finite element method analysis (FEM analysis) was performed on each process of press-forming the press-formed product 1 into a target shape in two steps, as shown in Figure 6.
[0031] FIG. 7 shows the sheet thickness change rate at the bottom dead center of the intermediate shape press-formed product 21 and the target shape press-formed product 1, which are obtained by FEM analysis for each of the first forming process and the second forming process. The results shown in FIG. 7 are for a case where a steel plate having a sheet thickness of 1.2 mm and a tensile strength of 780 MPa is used as the blank 11, the vertical wall height of the intermediate shape press-formed product 21 is 20 mm, and the vertical wall height of the target shape press-formed product 1 is 30 mm. The sheet thickness change rate shown in FIG. 7 is a value obtained by dividing the difference between the sheet thickness at each part of the intermediate shape press-formed product 21 or the press-formed product 1 and the sheet thickness of the metal sheet which is the blank 11 by the sheet thickness of the blank 11. In this specification and drawings, when the sheet thickness change rate is a positive value, it is called the sheet thickness increase rate, and when the sheet thickness change rate is a negative value, it is called the sheet thickness decrease rate. The larger the absolute value of the sheet thickness decrease rate, the more likely it is that cracks will occur.
[0032] Fig. 7(a) shows the sheet thickness change rate at the bottom dead point of the intermediate shape press-formed product 21 press-formed in the first forming step shown in Fig. 6(a), where the sheet thickness reduction rate at the end of the horizontal edge 29a was -4.7%. Fig. 7(b) shows the sheet thickness change rate at the bottom dead point of the press-formed product 1 of the target shape press-formed in the second forming step shown in Fig. 6(b), where the sheet thickness reduction rate at the end of the horizontal edge 9a was -16.9%. Thus, the sheet thickness reduction rate at the end of the horizontal edge 9a of the target shape has a large absolute value, and as a result, the sheet thickness is greatly reduced at the end of the horizontal edge 9a in the second forming step, making it easy for cracks to occur.
[0033] The reason why the plate thickness reduction rate at the end of the horizontal edge 9a of the press-formed product 1 of the target shape is large will be described with reference to FIG. 8. Conventionally, as described above, in the first forming process, a press-formed product 21 of an intermediate shape with a vertical wall height lower than that of the target shape is press-formed, and in the subsequent second forming process, the press-formed product 21 of the intermediate shape is press-formed into a press-formed product 1 of the target shape with a vertical wall height. In this case, in the second forming process, as shown in FIG. 8, the horizontal edge 29a is stretched, and a large tensile force acts on the horizontal edge 9a. As a result, due to this large tensile force, the absolute value of the plate thickness reduction rate at the end of the horizontal edge 9a of the target shape becomes large as shown in FIG. 7(b) described above, leading to the occurrence of cracks.
[0034] Therefore, the inventors have studied a method for reducing the tensile force acting on the horizontal edge 9a in the process of press-molding the press-molded product 1 of the target shape in two steps. As a result, as shown in Fig. 1 and Fig. 2, in the first molding step, the vertical wall height of the tip of the horizontal edge 23a in the top plate 23 of the press-molded product 21 of the intermediate shape in Fig. 1 is formed higher than the vertical wall height of the vertical edge 23b, and the convex portion 23d lifted upward is formed in the region from the horizontal edge 23a to the vertical edge 23b including the connecting R portion 23c in the top plate 23 of the press-molded product 21 of the intermediate shape in Fig. 2. As explained with reference to Fig. 2, when the convex portion 23d lifted upward is crushed in the subsequent second molding step to form the connecting R portion 3c which becomes the top plate portion of the target shape, the material flows from the convex portion 23d lifted upward to the tip of the horizontal edge 9a. It has been found that this reduces the tensile force acting on the horizontal edge portion 9a and suppresses cracks at the end of the horizontal edge portion 9a. The present invention has been made based on the above-mentioned investigation results, and the specific configuration is as follows.
[0035] <Method of manufacturing press molded products> The manufacturing method of the press-molded product of embodiment 1 involves press-molding the press-molded product 1 shown in Figure 2 described above into an intermediate shape in which the vertical wall height of the vertical side portion of the top plate is lower than the target shape in a first molding process, and then press-molding it to the vertical wall height of the target shape in the subsequent second molding process.
[0036] In the manufacturing method of the press-formed product according to the first embodiment, in the first forming step, as shown in FIG. 1(a), the vertical wall height of the horizontal side portion 23a of the top plate portion 23 of the press-formed product 21 in the intermediate shape is formed to include a "protrusion" that is higher than the vertical wall height of the vertical side portion. In the first forming step, the intermediate shape press-formed product 21 may be press-formed using a punch 71 including an area higher than the area where the vertical side portion 23b is formed for the part where the horizontal side portion 23a of the top plate portion 23 is formed, as shown in FIG. 9 and FIG. 10. Alternatively, in the manufacturing method of the press-formed product according to the first embodiment, in the first forming step, as shown in FIG. 2(a), a protrusion 23d higher than the surrounding height (reference height of the top plate surface) is formed in the area from the horizontal side portion 23a including the connecting R portion 23c to the vertical side portion 23b. Here, the protrusion 23d is formed to be higher than the vertical side portion 23b of the top plate portion 23 in the intermediate shape. In the first forming step, as illustrated in Fig. 11(a), a punch 71 having a convex portion forming portion 73d provided in a region extending from a horizontal side forming portion 73a including a connection R forming portion 73c of a top plate forming portion 73 to a vertical side forming portion 73b may be used to press-form an intermediate shaped press-formed product 21. In the first forming step, as illustrated in Fig. 11(b), a punch 61 having a convex portion forming portion in a region extending from a convex portion forming portion 63d of the top plate forming portion to a horizontal side tip side forming portion 63a1 may be used to press-form an intermediate shaped press-formed product 21.
[0037] Furthermore, in the manufacturing method of the press-molded product according to the first embodiment, in the subsequent second molding step, the intermediate product formed in the first molding step is press-molded into the top plate portion 3 having a target shape.
[0038] <Reasons why cracks can be prevented> The reason why the method for manufacturing a press-formed product according to the first embodiment can suppress the occurrence of cracks at the ends of the horizontal side ridge lines 9a of the press-formed product 1 having a target shape will be described with reference to Figs.
[0039] In the first embodiment, as described above, in the first forming step, press forming is performed to form an intermediate-shaped press-formed product 21 including a "protrusion" in which the horizontal side 23a of the intermediate-shaped top plate portion 23 is higher than the vertical side 23b (FIG. 1(a)). Alternatively, in the first forming step, press forming is performed to form an intermediate-shaped press-formed product 21 in which a protrusion 23d that is higher than the vertical side 23b of the intermediate-shaped top plate portion 23 is formed on the top plate portion 23 (FIG. 2(a)).
[0040] When the press-formed product 21 of such an intermediate shape is press-formed into the press-formed product 1 of the target shape in the second forming process, the material flows from the high part of the intermediate shape to the horizontal edge portion 9a, as shown in Fig. 1(b) and Fig. 2(b). This makes it possible to reduce the tensile force generated in the horizontal edge portion 9a of the press-formed product 1 of the target shape. As a result, the reduction in the plate thickness at the end of the horizontal edge portion 9a is reduced, and cracks can be suppressed.
[0041] <Mode of horizontal side> In the above description, the first forming step is to uniformly raise the tip end portion in the direction in which the horizontal side portion 23a of the intermediate press-formed product 21 extends, as shown in FIG. 1(a). Examples of this embodiment are shown in FIG. 9(a) and FIG. 9(b). FIG. 9(a) is a schematic diagram of a punch (die) that uniformly raises the tip end portion of the horizontal side forming portion 73a higher than the boundary line between the region in which the vertical side forming portion 73b of the top plate forming portion 73 is extended toward the horizontal side forming portion 73a and the horizontal side forming portion 73a. FIG. 9(b) is a schematic diagram of a punch (die) that uniformly raises the region from the boundary line between the region in which the vertical side forming portion 73b of the top plate forming portion 73 is extended toward the horizontal side forming portion 73a and the horizontal side forming portion 73a to the tip. In this way, there is no particular limitation on the range in which the tip end portion of the horizontal side forming portion 73a is uniformly raised. However, from the viewpoint of suppressing wrinkles in the vicinity of the connecting R portion 3c in the second forming step, it is preferable to make the tip side portion of the intermediate shape horizontal side forming portion 73a higher than the boundary line with the region to which the vertical side forming portion 73b is extended. Therefore, only the tip side portion of the horizontal side forming portion 73a may be made uniformly higher than that shown in FIG. 9(a) (not shown).
[0042] In addition, in the first forming step, when the tip end portion of the horizontal side portion 23a is uniformly high, the increment in height of the tip end portion is preferably 0.05 or more and 0.5 or less in ratio to the vertical wall height of the horizontal side vertical wall portion 25a of the intermediate shape press-formed product 21. If the increment in height of the tip end portion of the horizontal side portion 23a is smaller than 0.05, the height of the horizontal side portion 23a (see FIG. 8) is insufficient, and the absolute value of the thickness reduction rate at the end of the horizontal side ridge portion 9a of the target shape is only slightly reduced, and it may be difficult to prevent cracks. In addition, if the increment in height of the tip end portion of the horizontal side portion 23a is larger than 0.5, the vertical wall height of the tip end of the horizontal side portion 23a becomes too high in the first forming step, and the horizontal side ridge portion 29a is stretched, and the absolute value of the thickness reduction rate increases, and the risk of cracks occurring in the first forming step may increase.
[0043] Furthermore, in the present invention, in the first forming step, as exemplified in FIG. 10, the intermediate lateral side forming portion 73a may be inclined so as to gradually become higher toward the tip end in the extending direction.
[0044] Fig. 12 shows the results of obtaining the plate thickness change rate for each of the intermediate-shaped press-formed product 21 and the press-formed product 1 of the target shape, which is produced in the first forming process and has a horizontal side portion 23a inclined so that the tip side is gradually higher. The results shown in Fig. 12 are obtained when a steel plate having a plate thickness of 1.2 mm and a tensile strength of 780 MPa class is used as the blank 11. Furthermore, the vertical wall height of the intermediate shape is 20 mm, the vertical wall height of the target shape is 30 mm, the inclination angle on the tip side of the horizontal side portion 23a in the press-formed product 21 of the intermediate shape is 15.4°, and the height increment at the tip is 5.5 mm.
[0045] As shown in Fig. 12(a), in the press-formed product 21 of the intermediate shape, the sheet thickness reduction rate at the tip of the horizontal side ridge portion 29a is -9.1%, which is an absolute value that is greater than that of the conventional method (-4.7%) shown in Fig. 7(a) described above. However, as shown in Fig. 12(b), in the press-formed product 1 of the target shape, the sheet thickness reduction rate at the tip of the horizontal side ridge portion 9a is -11.9%, which is an absolute value that is less than that of the conventional method (-16.9%) shown in Fig. 7(b) described above. This result shows that even when the tip side of the horizontal side portion 23a is inclined in the press-formed product 21 of the intermediate shape, cracks at the end of the horizontal side ridge portion 9a of the press-formed product 1 of the target shape can be suppressed.
[0046] Specific examples of inclining the tip side of the horizontal side portion 23a of the intermediate shape are shown in Figures 10(a) and 10(b). Figure 10(a) shows an example in which the vertical side molding portion 73b in the top plate molding portion 73 is inclined from the boundary between the region where the vertical side molding portion 73b is extended to the horizontal side molding portion 73a side and the horizontal side molding portion 73a as the starting point, and the inclination is gradually higher toward the tip in the direction in which the horizontal side molding portion 73a extends. Figure 10(b) shows an example in which the vertical side molding portion 73b is inclined from the extended region side of the vertical side molding portion 73b relative to the boundary between the region where the vertical side molding portion 73b is extended to the horizontal side molding portion 73a side and the horizontal side molding portion 73a as the starting point, and the inclination is gradually higher toward the tip in the direction in which the horizontal side molding portion 73a extends.
[0047] In this way, there is no particular limitation on the starting position for tilting the tip portion of the horizontal side molding portion 73a, and the tilt may be started from the tip side of the boundary line between the extended region of the vertical side molding portion 73b and the horizontal side molding portion 73a (not shown).
[0048] Furthermore, as shown in Figures 10(a) and 10(b), when inclining the tip side of the horizontal side molding portion 73a in the intermediate shaped press-formed product 21, the inclination angle based on the horizontal side portion 3a of the target shape is preferably greater than or equal to 3 degrees and less than 25 degrees.
[0049] If the inclination angle is less than 3 degrees, the absolute value of the thickness reduction rate of the horizontal edge 9a in the press-formed product 1 of the target shape is only slightly reduced, and it may be difficult to prevent cracks. If the inclination angle is more than 25 degrees, the horizontal edge 29a between the horizontal edge 23a and the horizontal vertical wall 25a is stretched in the first forming step (see FIG. 12(a)), and the absolute value of the thickness reduction rate increases, which may increase the risk of cracks occurring in the first forming step.
[0050] 9(a) and 9(b) and 10(a) and 10(b) show examples of specific shapes of a punch (die) that forms the horizontal side portion 23a of the intermediate-shaped press-formed product 21, but the present invention is not limited to these shapes. As long as the punch (die) forms the height of the tip side of the horizontal side portion of the top plate portion of the intermediate shape higher than the vertical side portion of the top plate portion of the intermediate shape, it may have a shape other than the horizontal side forming portion 73a shown in FIGS. 9 and 10.
[0051] For example, in the first forming step, the height of a region of the horizontal side of the intermediate shape that is an extension of the vertical side may be made higher than the height of the vertical side of the intermediate shape.
[0052] The above description has been directed to the press-molded product 1 having the top plate portion 3 that is substantially T-shaped in top view. However, the present invention may also be directed to a press-molded product 41 that includes a top plate portion 43 that is substantially L-shaped in top view and has a horizontal side portion 43a and a vertical side portion 43b, a vertical wall portion 45, and a bottom flange portion 47, as shown in Fig. 5.
[0053] Conventionally, the press-formed product 41 having a top plate portion 43 of a substantially L-shape was also manufactured by press-forming into an intermediate shape with a low vertical wall height in the first forming process, and then press-forming into the vertical wall height of the target shape in the subsequent second forming process, as shown in FIG. 16. Therefore, like the press-formed product 1 having a top plate portion 3 of a substantially T-shape, the horizontal side vertical wall portion 55a of the press-formed product 51 of the intermediate shape in FIG. 16(a) is stretched in the vertical wall height direction in the second forming process in FIG. 16(b). This causes a large tensile force to act on the horizontal side vertical wall portion 45a and the horizontal side ridge portion 49a of the target shape. As a result, the absolute value of the sheet thickness reduction rate at the end of the horizontal side ridge portion 49a becomes large (17.7%) due to this large tensile force, leading to the occurrence of cracks.
[0054] 17(a), in the first forming step, the tip end portion of the horizontal side portion 53a of the top plate is raised so that the tip end portion of the horizontal side portion 53a is higher than the vertical side portions. In the subsequent second forming step, the tip end portion of the horizontal side portion 53a of the intermediate shape is set to the height of the target shape.
[0055] As a result, as in the case of manufacturing a press-molded product 1 having the aforementioned approximately T-shaped top plate portion 3, the absolute value of the plate thickness reduction rate at the end of the horizontal side ridge portion 49a of the target shape can be reduced (-12.6%), and cracking can be suppressed.
[0056] 17(a), the height of the tip end portion of the horizontal side portion 53a of the top plate portion is uniformly higher than the tip end portion of the vertical side portion 53b of the top plate portion. However, even when manufacturing a press-molded product 41 having a substantially L-shape, the tip end portion of the horizontal side portion 53a of the intermediate shape may be inclined so as to gradually become higher toward the tip end in the direction in which the horizontal side portion 53a connects to the vertical wall portion and extends.
[0057] Next, FEM analysis was performed to verify that the reduction in plate thickness at the end of the horizontal edge ridge portion 9a is reduced by performing intermediate forming using the punch shape shown in Figure 11, for each process of press-forming the press-formed product 1 into the target shape through the first forming process and the second forming process.
[0058] Fig. 14 shows the results of the sheet thickness change rate at the bottom dead center of the intermediate-shape press-formed product 21 and the target-shape press-formed product 1, which was obtained by FEM analysis of the first forming step and the second forming step according to the first embodiment. The results shown in Fig. 14 are for a case where a 780 MPa-class steel plate is used as the blank 11, the vertical wall height of the intermediate-shape press-formed product 21 is 20 mm, and the vertical wall height of the target-shape press-formed product 1 is 30 mm. The sheet thickness change rate is a value obtained by dividing the difference between the sheet thickness at each portion of the press-formed product 1 or the intermediate-shape press-formed product 21 and the sheet thickness of the metal sheet that is the blank 11 by the sheet thickness of the blank 11.
[0059] In the intermediate-shaped press-formed product 21, the sheet thickness reduction rate at the end of the horizontal edge 29a was -1.8%, as shown in Fig. 14(a). The absolute value of this sheet thickness reduction rate is slightly increased compared to the sheet thickness reduction rate (=-1.2%, see Fig. 13(a)) of the intermediate-shaped press-formed product 21 press-formed by the conventional method.
[0060] On the other hand, the sheet thickness reduction rate of the press-formed product 1 having the target shape press-formed in the second forming step shown in Fig. 14(b) was -8.1%. This value is smaller in absolute value than the sheet thickness reduction rate (=-11.0%, see Fig. 13(b)) at the end of the horizontal edge ridge portion 9a of the press-formed product 1 press-formed by the conventional method. As a result, it is found that cracks at the end of the horizontal edge portion 9a of the press-formed product 1 having the target shape can be suppressed.
[0061] As described above, in the manufacturing method of the press-formed product according to the first embodiment, in the second forming step, the convex portion 23d is crushed to form the top plate portion 3 in the target shape. This reduces the tensile force acting on the horizontal edge portion 9a continuing from the horizontal edge portion 3a in the top plate portion 3 in the target shape, and makes it possible to suppress cracks at the end portion of the horizontal edge portion 9a.
[0062] In addition, the height increment of the convex portion 23d formed on the intermediate-shaped top plate portion 23 in the first molding process (the height to the apex of the convex portion 23d when the vertical side portion 23b of the intermediate-shaped top plate portion 23 is used as the reference) may be 5% to 50% of the width of the horizontal side vertical wall portion 25a.
[0063] If the height increment of the protrusion 23d is less than 5%, the flow of material to the horizontal edge 9a caused by crushing the protrusion 23d in the second molding step is insufficient, and cracks may not be sufficiently suppressed. Also, if the height increment of the protrusion 23d exceeds 50%, the flow of material to the horizontal edge 9a caused by crushing the protrusion 23d in the second molding step is excessive, and although cracks can be suppressed, there may be a problem of excess material causing wrinkles.
[0064] In the present invention, as long as a protrusion is formed at a connecting R portion that connects a horizontal side portion to a vertical side portion of a top plate portion in an intermediate shape, the protrusion may have a shape other than that of the protrusion 23d shown in FIG. 2(a).
[0065] As another aspect of the first embodiment, the first forming step may be a step of press-forming an intermediate-shaped press-formed product 21 as illustrated in FIG. 15(a). Here, the intermediate-shaped press-formed product 21 has a convex portion 23d formed on the top plate portion 23, and a portion 23a1 on the tip side of the horizontal side portion 23a is higher than the vertical side portion 23b of the top plate portion 23 of the intermediate shape. In this case, in the first forming step, for example, as shown in FIG. 11(b), a punch 61 having a horizontal side tip side forming portion 63a1 that forms the intermediate-shaped portion 23a1 uniformly higher than the vertical side portion 23b in addition to the convex portion forming portion 63d may be used. Then, in the subsequent second forming step, the convex portion 23d is crushed, and the intermediate-shaped portion 23a1 is set to the height of the target shape.
[0066] FIG. 15(a) is a diagram showing the results of FEM analysis of the sheet thickness change rate at the bottom dead point of the intermediate-shaped press-formed product 51 according to another aspect of the first embodiment. FIG. 15(b) is a diagram showing the results of FEM analysis of the sheet thickness change rate at the bottom dead point of the press-formed product 1 of the target shape according to another aspect of the first embodiment. The results shown in FIG. 15 are for a case where a 780 MPa-class steel plate is used as the blank 11, the vertical wall height of the intermediate-shaped press-formed product 51 is 20 mm, and the vertical wall height of the target-shaped press-formed product 1 is 30 mm. The sheet thickness change rate shown in FIG. 15 is a value obtained by dividing the difference between the sheet thickness at each part of the intermediate-shaped press-formed product 51 or the press-formed product 1 and the sheet thickness of the metal sheet which is the blank 11 by the sheet thickness of the blank 11.
[0067] In the intermediate-shaped press-formed product 51, as shown in Fig. 15(a), the sheet thickness reduction rate at the end of the horizontal edge ridge portion 29a was -2.5%. The absolute value of this sheet thickness reduction rate is increased compared to the sheet thickness reduction rate (=-1.2%) (see Fig. 13(a)) of the intermediate-shaped press-formed product 51 press-formed by the conventional method.
[0068] On the other hand, when the press-formed product 51 of the intermediate shape shown in FIG. 15(a) is press-formed into the press-formed product 1 of the target shape in the second forming step, the sheet thickness reduction rate at the end of the horizontal edge 9a is -4.7%, as shown in FIG. 15(b). This value is a significantly reduced absolute value compared to the sheet thickness reduction rate by the conventional method (=-11.0%, see FIG. 13(b)). Furthermore, the absolute value is reduced compared to the sheet thickness reduction rate when only the convex portion 23d is formed (=-8.1%, FIG. 14(b)). For this reason, it is preferable to form the convex portion 23d on the press-formed product 51 of the intermediate shape in the first forming step and to raise the portion 23a1 on the tip side of the horizontal edge 23a, so that the sheet thickness reduction at the end of the horizontal edge 9a can be further suppressed.
[0069] When the intermediate-shaped press-formed product 21 is press-formed, if the portion 23a1 at the tip of the horizontal side portion 23a is made higher, the height increment is preferably set to be equal to or smaller than the height increment of the protrusion 23d. By making the protrusion 23d higher than the portion 23a1, the protrusion 23d can be crushed during the press-formation into the target shape, causing material to flow to the horizontal side ridge portion 9a.
[0070] In addition, the intermediate-shape press-molded product 21 shown in Figure 15 has the vertical side portion 23b higher from the extended area side of the vertical side portion 23b than the boundary line between the area extended toward the horizontal side portion 23a and the horizontal side portion 23a, and the portion 23a1 from the boundary line to the tip side of the horizontal side portion 23a is uniformly higher.
[0071] However, in the present invention, other than making the convex portion 23d higher than the portion 23a1, there is no particular limitation on the form or range in which the portion on the tip side of the horizontal side portion in the intermediate shape press-formed product press-formed in the first forming step is raised.
[0072] Furthermore, the present invention may be a press-molded product 41 having a top plate portion 43 that is approximately L-shaped when viewed from above and has a horizontal side portion 43a and a vertical side portion 43b, a vertical wall portion 45, and a bottom flange portion 47, as shown as an example in Figures 5 and 16(b).
[0073] In the case of a press-formed product 41 having an approximately L-shaped top plate portion 43, in the conventional method, when the product was press-formed into an intermediate shape with a low vertical wall height in the first forming process and then press-formed into the target vertical wall height in the second forming process, cracks were likely to occur at the end of the horizontal side ridge portion 49a.
[0074] Therefore, in the present invention, as in the above-mentioned substantially T-shaped press-formed product 1, in the first forming step, a convex portion higher than the height (reference height of the top surface) of the vertical side portion 53b of the intermediate-shaped top plate portion 53 is formed in the connecting R portion that connects the horizontal side portion and the vertical side portion of the top plate portion. Then, in the subsequent second forming step, the convex portion is crushed to form the top plate portion in the target shape.
[0075] This makes it possible to reduce the reduction in plate thickness at the end of the horizontal edge 49a of the target shape and suppress cracks, even when manufacturing a press-formed product 41 having a generally L-shaped top plate portion 43. Furthermore, in the first forming step, a convex portion may be formed on the top plate portion of the intermediate shape, and the portion on the tip side of the horizontal edge portion may be made higher than the vertical edge portion of the top plate portion of the intermediate shape.
[0076] According to the manufacturing method for a press-formed product of the first embodiment, even when a high-strength steel plate is used, cracks at the end of the horizontal edge ridge portion 9a of the press-formed product 1 having a target shape can be suppressed. Therefore, the press-formed product 1 manufactured using a high-tensile steel plate by the manufacturing method for a press-formed product of the first embodiment can be manufactured as a vehicle body part.
[0077] (Embodiment 2) The target shape of the press-formed product targeted in the second embodiment will be described with reference to Fig. 23. The press-formed product 101 includes a top plate portion 103, a top plate flange portion 105 extending from one longitudinal end of the top plate portion 103, and a vertical wall portion 109 continuing from the top plate portion 103 via a ridge portion 107. The press-formed product 101 also includes a vertical flange portion 111 bent outward on one longitudinal end side of the vertical wall portion 109, and a horizontal flange portion 113 bent outward on the lower end of the vertical wall portion 109.
[0078] The process by which the invention according to the second embodiment has been arrived at will be described below by taking the press-molded product 101 as an example. Figure 24 is an explanatory diagram of a conventional manufacturing method for press-molding the press-molded product 101 shown in Figure 23 in one step.
[0079] The blank 115 to be formed into the press-molded product 101 shown in Figure 23 is made of a metal plate, and as shown in Figure 24, its overall shape is approximately rectangular, with a top plate flange equivalent portion 117 formed on one end and vertical flange equivalent portions 119 formed on both sides of the top plate flange equivalent portion 117.
[0080] The die 121 used in the conventional manufacturing method of the press-formed product 101 includes a punch 123, a pad 125 for pressing the blank 115, and a die 127 for forming the top plate portion 103, the vertical wall portion 109, the horizontal flange portion 113, and the vertical flange portion 111 in cooperation with the punch 123. The punch 123 includes a top plate forming surface portion 129 for mainly forming the top plate portion 103. The punch 123 includes a top plate horizontal side forming surface portion 168 for forming the horizontal side of the top plate forming surface portion 129, a punch side vertical wall forming surface portion 131 for forming the vertical wall portion 109 continuously with the vertical side, and a punch side horizontal flange forming surface portion 133 for forming the flange portion continuously with the punch side vertical wall forming surface portion 131. The punch 123 also includes a punch side vertical flange forming surface portion 135 for forming the vertical flange portion 111 continuously with the horizontal side of the top plate forming surface portion 129.
[0081] The pad 125 has a shape corresponding to a top plate forming surface portion 129 of the punch 123. The die 127 consists of a pair of left and right die portions, and includes a die side vertical wall forming surface portion 137, a die side horizontal flange forming surface portion 139, and a die side vertical flange forming surface portion 141.
[0082] In a conventional manufacturing method of the press-formed product 101, a blank 115 is sandwiched between a pad 125 and a punch 123, a die 127 is moved relatively to the punch 123, and the top plate portion 103, the vertical wall portion 109, and the horizontal flange portion 113 are press-formed, and the vertical flange portion 111 is bent laterally to form the press-formed product into a target shape. Regarding the conventional manufacturing method of the press-formed product 101, a press forming analysis was performed by the finite element method (FEM) for a case where a metal plate having a tensile strength of 1.5 GPa class was used, and the plate thickness reduction rate of the press-formed product 101 after forming was obtained.
[0083] FIG. 25 shows the thickness reduction rate at the bottom dead center of forming as a contour, with the lighter colored areas indicating a larger thickness reduction rate. In the following explanation, the thickness reduction rate is expressed as a value (ratio) obtained by dividing the difference between the thickness of the metal plate that is the blank 115 and the thickness of each area after press forming by the thickness of the metal plate that is the blank 115. As the thickness reduction rate increases, cracks become more likely to occur. As shown in the partially enlarged view of FIG. 25, the end of the ridge line portion 107 on the side where the vertical flange portion 111 is formed (hereinafter simply referred to as "end portion 142 of ridge line portion 107") has a thickness reduction rate of 8.9%, which shows that the thickness reduction rate is the largest and cracks are more likely to occur.
[0084] The reason why the sheet thickness reduction rate of the end 142 of the ridgeline portion 107 is large will be explained with reference to Fig. 25. The arrows in Fig. 25 indicate the tensile forces generated during the forming process. When the vertical wall portion 109 is formed via the ridgeline portion 107, a tensile force as shown by the arrow (i) in Fig. 25 acts on the sheet surface of the ridgeline portion 107. Furthermore, when the vertical flange portion 111 is bent laterally, a tensile force as shown by the arrow (ii) is further applied to the end 142 of the ridgeline portion 107. In this way, both the tensile force during the forming of the vertical wall portion 109 and the tensile force during the laterally bending of the vertical flange portion 111 act on the end 142 of the ridgeline portion 107, so that the sheet thickness reduction rate becomes large and cracks are likely to occur.
[0085] Therefore, the inventors have studied a method for reducing the tensile force acting on the end 142 of the ridgeline portion 107. As a result, when press-molding a press-molded product 101 having a target shape shown in FIG. 23, press molding is performed in two steps, a first molding step and a second molding step, and a convex part higher than the surrounding height (reference height of the top plate surface) is formed at the end of the ridgeline portion of the intermediate molded product molded in the first molding step on the side close to the intermediate vertical flange portion, and the convex part is crushed to the height of the target molded product in the second molding step. It has been found that this makes it possible to reduce the tensile force on the end 142 of the ridgeline portion 107 and to prevent wrinkles from occurring in the top plate portion 103 or the vertical wall portion 109. The present invention is based on such findings, and a manufacturing method of the press-molded product 101 according to embodiment 2 will be described with reference to FIG. 18.
[0086] The manufacturing method of the press-molded product 101 according to the second embodiment includes a first molding step (FIG. 18(a)) and a second molding step (FIG. 18(b)). The first molding step is a step of press-molding an intermediate molded product 149 (see FIG. 20(a)) having an intermediate top plate portion 143, an intermediate vertical wall portion 145 continuing to the intermediate top plate portion 143 via an intermediate ridge portion 144, and a convex portion 147 higher than the surrounding height (reference height of the top plate surface) formed on the end portion 142 on the side closer to the intermediate vertical flange portion 153 of the intermediate ridge portion 144. The intermediate molded product 149 also has an intermediate horizontal flange portion 151 and an intermediate vertical flange portion 153. The second molding step is a step of press-molding the intermediate molded product 149 into the press-molded product 101, which is a target shape. Each step will be described below in detail.
[0087] <1st molding process> In the first forming step, as shown in Fig. 18(a), a blank 115 is press-formed by an intermediate punch 155, an intermediate pad 157, and an intermediate die 159 to manufacture an intermediate formed product 149 shown in Fig. 20. The blank 115 is similar to that shown in Fig. 24. As shown in Figs. 18 and 19, the intermediate punch 155 has a T-shaped intermediate top plate forming surface portion 161 having vertical and horizontal sides in a plan view, a punch-side intermediate vertical wall forming surface portion 163 that forms the intermediate vertical wall portion 145, a punch-side intermediate horizontal flange forming surface portion 165 that forms the intermediate horizontal flange portion 151, and a punch-side intermediate vertical flange forming surface portion 167 that forms the intermediate vertical flange portion 153.
[0088] A convex portion forming portion 169 for forming the convex portion 147 is formed on both sides of the end of the intermediate top plate forming surface portion 161 in the width direction. In the intermediate punch 155 shown in FIG. 19, the convex portion forming portion 169 extends toward the top plate flange portion 105 (see FIG. 20) side, and the overall height of the intermediate top plate forming surface portion 161 is high. The punch side intermediate vertical wall forming surface portion 163 has a gentler inclination angle than the conventional punch side vertical wall forming surface portion 131 shown in FIG. 24. In addition, the angle between the punch side intermediate horizontal flange forming surface portion 165 and the punch side intermediate vertical wall forming surface portion 163 is set to be the same angle as the angle between the vertical wall portion 109 of the target shape and the horizontal flange portion 113 of the target shape.
[0089] 18 has a shape corresponding to the intermediate top plate forming surface portion 161 of the intermediate punch 155. The intermediate die 159 has a die side intermediate vertical wall forming surface portion 171 shaped corresponding to the punch side intermediate vertical wall forming surface portion 163, and a die side intermediate horizontal flange forming surface portion 173 shaped corresponding to the punch side intermediate horizontal flange forming surface portion 165. The intermediate die 159 also has a die side intermediate vertical flange forming surface portion 175 shaped corresponding to the punch side intermediate vertical flange forming surface portion 167.
[0090] The intermediate molded product 149 shown in Fig. 20(a) is manufactured by the intermediate punch 155, the intermediate pad 157, and the intermediate die 159. As described above, the intermediate molded product 149 has the intermediate top plate portion 143, the intermediate vertical wall portion 145, the top plate flange portion 105, the intermediate horizontal flange portion 151, and the intermediate vertical flange portion 153. In addition, a convex portion 147 is formed at the end portion 146 of the intermediate ridge portion 144 in the intermediate molded product 149.
[0091] 20(b) shows the AA cross section of the intermediate product 149 in FIG. 20(a) in comparison with the press-formed product 1 (FIG. 21) (two-dot chain line) of the target shape. As shown in FIG. 20(b), a convex portion 147 is formed at the end of the ridge in the intermediate product 149, so that the end 146 of the intermediate ridge 144 is raised, and the bending radius of the top plate 103 and the vertical wall 109 is made larger than the target shape, thereby reducing the tensile force when bending the top plate 103 and the vertical wall 109 in the first forming step. As shown in FIG. 20(a), the sheet thickness reduction rate of the end 146 of the intermediate ridge 144 is 2.8%, which is smaller than the 8.9% of the conventional press-formed product 101 shown in FIG. 25.
[0092] <Second molding process> The second forming step is a step of press-forming the intermediate product 149 into a target shape, that is, the press-formed product 101. The punch 123, pad 125, and die 127 used in the second forming step have the same shapes as the conventional punch 123, pad 125, and die 127 shown in FIG.
[0093] In the second forming step, by crushing the convex portion 147 of the end 146 of the intermediate ridge line portion 144 shown in Fig. 20 to form the target shape, a material flow is generated toward the end 146 of the intermediate ridge line portion 144, reducing the tensile force and preventing cracking of the end 142 of the ridge line portion 107 of the press-formed product 101, which has the target shape, shown in Fig. 23. In addition, because the convex portion 147 is provided only to the end 146 of the intermediate ridge line portion 144 and not to the entire area, no excess material flow is generated in the second forming step, and no wrinkles are generated in the top plate portion 103 or vertical wall portion 109 of the press-formed product 101, which has the target shape.
[0094] A press-formed product 101 formed by the second forming process is shown in Fig. 21. As shown in Fig. 21, the sheet thickness reduction rate of end 142 of ridge line portion 107 in press-formed product 101 formed by the second forming process after passing through the first forming process was 4.1%. As such, compared to the sheet thickness reduction rate of 8.9% (see Fig. 25) of end 142 of ridge line portion 107 in the prior art shown in Fig. 25, it is found that the sheet thickness reduction rate is smaller in the present invention, making it possible to prevent cracks.
[0095] The shape of the intermediate punch 155 in the first forming step is not limited to that shown in Fig. 19, and may be, for example, that shown in Fig. 22(a) and Fig. 22(b). In the one shown in Fig. 22(a), the convex portion forming portion 169 is formed only on both sides in the width direction of the end of the intermediate top plate forming surface portion 161, and in the one shown in Fig. 22(b), the convex portion forming portion 169 extends to the top plate side-side forming surface portion 168, but other areas of the side of the top plate side-side forming surface portion 168 are not elevated.
[0096] Further, the press-formed product 101 having a target shape in the second embodiment has a vertical flange portion 111, but the press-formed product having a target shape of the present invention includes a product not having a vertical flange.
[0097] (Embodiment 3) The target shape of the press-formed product targeted in the third embodiment will be described with reference to Fig. 30. The press-formed product 177 has a top plate portion 179 having a curved portion when viewed from above, and a vertical wall portion 183 continuing from a part of the inside of the curve of the top plate portion 179 via a ridge portion 181, and an end portion 185 of the ridge portion 181 has an R-shape.
[0098] The background to the invention according to embodiment 3 will be described below by taking a press-molded product 177 as an example. Fig. 31 is an explanatory diagram of a conventional method for manufacturing a press-molded product 177 shown in Fig. 30, in which the press-molded product 177 is press-molded in one step.
[0099] Blank 187 formed into press-molded product 177 is made of a metal plate, and top plate equivalent portion 189 formed into top plate portion 179 is curved in an arc shape as shown in Fig. 31. Vertical wall equivalent portions 191 are formed inside the curvature of top plate equivalent portion 189, at positions located inward in the longitudinal direction from both ends of top plate equivalent portion 189. Ends 193 of vertical wall equivalent portions 191 are formed in an R shape.
[0100] In a conventional manufacturing method of the press-formed product 177, the blank 187 is sandwiched between a pad 199 and a punch 197 of a metal mold 195, the die 201 is moved relative to the punch 197, and the top plate portion 179 and the vertical wall portion 183 are press-formed into a target shape. Regarding such a conventional manufacturing method of the press-formed product 177, a press forming analysis was performed by the finite element method (FEM) when a metal plate having a tensile strength of 980 MPa was used for the blank 187, and the plate thickness reduction rate of the press-formed product 177 after forming was obtained.
[0101] Fig. 32 shows the thickness reduction rate at the bottom dead center of forming as a contour plot, with the lighter the color, the greater the thickness reduction rate. As shown in Fig. 32, the thickness reduction rate at end 185 of ridge line 181 is 10.8%, which is the largest thickness reduction rate and is therefore prone to cracking.
[0102] The reason why the sheet thickness reduction rate at end 185 of ridgeline portion 181 is large will be explained with reference to Figure 33. The arrows in Figure 33 indicate the tensile forces generated during the forming process. When vertical wall portion 183 is formed via ridgeline portion 181, a tensile force acts on the sheet surface of ridgeline portion 181 as shown by arrow (iii) in Figure 33. Also, as shown by arrow (iv), a tensile force is generated at end 185 of the ridgeline portion as vertical wall portion 183 is pulled inward. Also, end 185 of the ridgeline portion has a notch shape, and as shown by arrow (v), tensile forces are concentrated and large tensile forces act, which increases the sheet thickness reduction rate and makes it easier for cracks to occur.
[0103] Therefore, the inventors have studied a method for reducing the tensile force acting on the end 185 of the ridgeline portion. As a result, they have decided to perform press molding in two steps, a first molding step and a second molding step. In the first molding step, a convex portion higher than the surrounding height (reference height of the top plate surface) is given to the end of the ridgeline portion of the intermediate molded product to be molded, and in the second molding step, the convex portion is crushed to the height of the target molded product. It has been found that this makes it possible to reduce the tensile force of the end 185 of the ridgeline portion 181, and furthermore, wrinkles are not generated in the top plate portion 179 or the vertical wall portion 183. The present invention is based on such findings, and a manufacturing method of the press-molded product 177 according to the third embodiment will be described with reference to FIG. 26.
[0104] The manufacturing method of the press-molded product 177 according to the third embodiment includes a first molding step (FIG. 26(a)) and a second molding step (FIG. 26(b)). The first molding step is a step of press-molding an intermediate product 211 (see FIG. 28) having an intermediate top plate portion 203, an intermediate vertical wall portion 207 continuing to the intermediate top plate portion 203 via an intermediate ridge portion 205, and a protrusion portion 209 formed at an end portion 206 of the intermediate ridge portion 205 and higher than the surrounding height (reference height of the top plate surface). The second molding step is a step of press-molding the intermediate product 211 into a press-molded product 177 (FIG. 29). Each step will be described in detail below.
[0105] <1st molding process> In the first forming step, as shown in Fig. 26(a), a blank 187 is press-formed by an intermediate punch 213, an intermediate pad 215, and an intermediate die 217 to manufacture an intermediate formed product 211 shown in Fig. 28. The blank 187 is similar to that shown in Fig. 31. As shown in Fig. 26(a) and Fig. 27 which shows a schematic diagram of the intermediate punch 213 in Fig. 26(a), the intermediate punch 213 is provided with an intermediate top plate forming surface portion 219 and a punch-side intermediate vertical wall forming surface portion 221 which forms the intermediate ridge portion 205.
[0106] A punch-side convexity forming portion 223 for forming the convexity 209 is formed on both sides in the width direction of the end of the intermediate top plate forming surface portion 219. The punch shown in Figures 26(a) and 27 is arranged so that the central position of the punch-side convexity forming portion 223 overlaps with the end portion 206 of the intermediate ridge portion 205.
[0107] The intermediate pad 215 has a shape corresponding to the intermediate top plate forming surface portion 219 of the intermediate punch 213. The intermediate die 217 is provided with a die side intermediate vertical wall forming surface portion 225 having a shape corresponding to the punch side intermediate vertical wall forming surface portion 221, and a die side convex portion forming portion 226 having a shape corresponding to the punch side convex portion forming portion 223.
[0108] Fig. 28(b) shows the BB section of Fig. 28(a) in comparison with the section of the target press-formed product shape (two-dot chain line). As shown in Fig. 28(b), the end of the ridge line in the intermediate formed product 211 is formed with a convex portion 209, so that the end 206 of the intermediate ridge line portion 205 rises, and the bending radius of the intermediate top plate portion 203 and the intermediate vertical wall portion 207 is made larger than the target shape, thereby reducing the tensile force when bending the intermediate top plate portion 203 and the intermediate vertical wall portion 207 in the first forming step. As shown in Fig. 28(a), the sheet thickness reduction rate of the end 206 of the intermediate ridge line portion 205 is 5.5%, which is smaller than the 10.8% of the conventional press-formed product 177 shown in Fig. 32.
[0109] <Second molding process> The second forming process is a process of press-forming the intermediate product 211 into a target shape, that is, the press-formed product 177. The punch 197, pad 199, and die 201 used in the second forming process have the same shapes as the conventional punch 197, pad 199, and die 201 shown in FIG.
[0110] 28 is pressed into the target shape, material flows toward the end 206 of the intermediate ridgeline portion 205, reducing the tensile force and preventing cracking of the end 185 of the ridgeline portion 181 of the press-formed product 177, which has the target shape. In addition, because the protrusion 209 is provided only to the end 206 of the intermediate ridgeline portion 205, not the entire area, no excess material flows and no wrinkles are formed in the top plate portion 179 or vertical wall portion 183 of the press-formed product 177, which has the target shape.
[0111] Fig. 29 shows a press-formed product 177 formed by the second forming step. As shown in Fig. 29, the sheet thickness reduction rate of end 185 of ridgeline portion 181 in press-formed product 177 formed by the second forming step after passing through the first forming step was 7.0%. As described above, this is a large reduction compared to the sheet thickness reduction rate of 10.8% (see Fig. 32) of end 185 of ridgeline portion 181 when press-formed in a conventional one-step process, and it is understood that cracks can be prevented.
[0112] The shape of the intermediate punch 213 in the first forming step is not limited to that shown in Fig. 27(a) and may be, for example, that shown in Fig. 27(b). In the one shown in Fig. 27(a), the top position of the punch side convexity forming portion 223 is disposed so as to extend to the outside of the end portion 206 of the intermediate ridge portion 205, while in the one shown in Fig. 27(b), the punch side convexity forming portion 223 extends along the ridge portion to the end of the intermediate top plate forming surface portion 219.
[0113] 29, the curvature of the ridgeline 181 of the top plate 179 and the vertical wall 183 does not necessarily have to be constant, and a part of it may be straight. Also, the angle of the intermediate vertical wall 207 of the intermediate molded product 211 does not have to be the same as the angle of the target shape, and it may be gentler than the target shape, or it may not be inclined at all. EXAMPLES
[0114] An analysis was carried out to verify the effects of the present invention, which will be described below. Example 1 In Example 1, the targets were a press-molded product 1 having a generally T-shaped top plate portion 3 shown in Fig. 3, and a press-molded product 41 having a generally L-shaped top plate portion 43 shown in Fig. 5. Each of the press-molded product 1 and the press-molded product 41 was manufactured by the first molding step and the second molding step of the manufacturing method for a press-molded product according to the first embodiment described above.
[0115] In the analysis, a steel plate having a thickness of 1.2 mm and a tensile strength of 780 MPa was used as the blank metal plate. Then, FEM analysis was performed for each of the first forming process and the second forming process, and the effect of suppressing cracking at the ends of the horizontal edge 9a (approximately T-shaped press-formed product 1) and the horizontal edge 49a (approximately L-shaped press-formed product 41) in the target shape was examined. Here, the effect of suppressing cracking was evaluated by the plate thickness reduction rate. As described above, the plate thickness reduction rate is a negative value of the plate thickness change rate obtained by dividing the difference between the plate thickness at each part of the press-formed product in the intermediate shape or the target shape and the plate thickness of the blank metal plate by the plate thickness of the blank.
[0116] In Example 1, the height of the tip side of the horizontal side portion 23a of the top plate portion of the intermediate shape is made higher than the height of the vertical side portion of the top plate portion of the intermediate shape in the first forming step, which is an example of the invention. In the example of the invention, the horizontal side forming portion of the top plate forming portion formed into the intermediate shape in the first forming step is shaped as shown in Figures 34 and 35. In Figure 34, the tip side of the horizontal side portion of the top plate portion of the intermediate shape is inclined so that it gradually becomes higher toward the tip in the direction in which the horizontal side portion extends. Here, the inclination angle of the press-formed product of the intermediate shape in which the tip side of the horizontal side portion is inclined is changed to various angles.
[0117] On the other hand, Fig. 35 shows a top plate portion of an intermediate shape in which the tip end of the horizontal side portion is uniformly higher in the direction in which the horizontal side portion extends. Furthermore, in the intermediate shape in which the tip end of the horizontal side portion is uniformly higher, a protrusion 23d is formed that is raised upward from the horizontal side portion to the vertical side portion so as to straddle the connecting R portion of the approximately T-shape or approximately L-shape. Here, for the intermediate shape in which the tip end of the horizontal side portion is uniformly higher, the height increment of the tip end portion of the horizontal side portion is changed in various ways, and the height of the protrusion 23d is set to the same height as the tip end portion of the horizontal side portion.
[0118] In Example 1, as a comparative example, a conventional example was used in which the height of the tip end side of the horizontal side portions 23a, 53a of the top plate portions 23, 53 of the press-formed products 21, 51 in the intermediate shape was set to the height of the top plate portions 3, 43 in the target shape as shown in Fig. 7(a) or Fig. 16(a) described above. For the conventional example as well, FEM analysis was performed for each of the first forming step and the second forming step, as in the examples of the invention, and the sheet thickness reduction rate was obtained for each of the press-formed products in the intermediate shape and the target shape at the bottom dead center of forming.
[0119] Table 1 shows the results of the inclination angle of the tip end of the horizontal side portion 23a or the tip end of the horizontal side portion 53a in the top plate portion of the intermediate shape, and the sheet thickness reduction rate at the end of the horizontal side ridge portion 9a of the press-formed product of the target shape or the horizontal side ridge portion 49a of the press-formed product 41. Note that the sheet thickness reduction rate decreases as the absolute value of the value increases.
[0120] [Table 1]
[0121] In the conventional example of No. 1, the inclination of the tip side of horizontal side portion 23a (approximately T-shaped) or the tip side of horizontal side portion 53a (approximately L-shaped) in the top plate portion of the intermediate shape is set to 0°. The sheet thickness reduction rate at the end of horizontal side ridge portion 9a (approximately T-shaped) of the target shape in No. 1 is -16.9%, and the sheet thickness reduction rate at the end of horizontal side ridge portion 49a (approximately L-shaped) is -17.7%, and these absolute values are large, so it is thought that cracks will occur.
[0122] In contrast, in Nos. 2 to 9, the inclination angle of the tip of horizontal side portion 23a or the tip of horizontal side portion 53a in the top plate portion of the intermediate shape is set to 3.8° to 23.7°. It can be seen that the absolute value of the sheet thickness reduction rate at the end of horizontal side ridge portion 9a or horizontal side ridge portion 49a of the target shape in Nos. 2 to 9 is reduced compared to the conventional example (-17.7%). In particular, in No. 7, which had an inclination angle of 18.3°, the sheet thickness reduction rate was -10.6%, and the absolute value was significantly reduced and favorable.
[0123] Table 2 shows the height of the tip side of horizontal side portion 23a or the tip side of horizontal side portion 53a in the top plate portion of the intermediate shape, and the plate thickness reduction rate at the end of horizontal side ridge portion 9a or horizontal side ridge portion 49a of the press-molded product of the target shape.
[0124] [Table 2]
[0125] In the conventional example No. 1, the height increment on the tip side of horizontal side portion 23a (approximately T-shaped) or the tip side of horizontal side portion 53a (approximately L-shaped) of the top plate portion of the intermediate shape is 0 mm. The sheet thickness reduction rate at the end of horizontal side ridge portion 9a (approximately T-shaped) of the target shape in No. 1 is -16.9%, and the sheet thickness reduction rate at the end of horizontal side ridge portion 49a (approximately L-shaped) is -17.7%, and these absolute values are large, so it is thought that cracks will occur.
[0126] In contrast, in Nos. 11 to 17, the height increment of the tip of the horizontal side portion 23a (generally T-shaped) or the tip of the horizontal side portion 53a (generally L-shaped) in the intermediate shape top plate portion is set to 3 mm to 25 mm. It can be seen that the sheet thickness reduction rate at the end of the horizontal side ridge portion 9a (generally T-shaped) or the horizontal side ridge portion 49a (generally L-shaped) of the target shape in Nos. 11 to 17 is reduced compared to the conventional example. In particular, in No. 17, in which the height increment was set to 25 mm, the sheet thickness reduction rate was -8.0%, and the absolute value was significantly reduced and favorable.
[0127] As described above, it has been shown that the method of the present invention can suppress cracks at the end of the horizontal edge portion when manufacturing a press-formed product having an approximately T-shaped or approximately L-shaped top plate portion by press molding in two steps.
[0128] Example 2 In Example 2, a press-molded product 1 having an approximately T-shaped top plate portion 3 with the dimensions shown in Figure 4 was targeted, and was press-molded through the first and second molding steps of the manufacturing method for a press-molded product related to the above-mentioned embodiment 1.
[0129] A steel plate having a thickness of 1.2 mm and a tensile strength of 780 MPa was used as the blank. An FEM analysis was performed on the first and second forming steps to examine the effect of suppressing cracking at the end of the horizontal edge 9a of the target shape. The effect of suppressing cracking was evaluated based on the thickness reduction rate of the press-formed product of the target shape obtained by the FEM analysis. As described above, the thickness reduction rate is a negative value of the thickness change rate obtained by dividing the difference between the thickness at each part of the press-formed product of the intermediate shape or the target shape and the thickness of the metal plate that is the blank by the thickness of the blank.
[0130] In the examples of the invention, in the first forming process, the punch 71 shown in Figure 11(a) or the punch 61 shown in Figure 11(b) was used to press-form an intermediate-shaped press-formed product 21 (Figure 2(a)) or an intermediate-shaped press-formed product 51 (Figure 15(a)).
[0131] By changing the height of the protrusion forming portion 73d of the punch 71 shown in FIG. 11(a), the height increment of the protrusion 23d was variously changed.
[0132] Moreover, the heights of the convex forming portion 63d and the horizontal side tip forming portion 63a1 of the punch 61 shown in FIG. 11(b) are made equal to each other, but the heights are changed, thereby varying the height increment of the convex portion 23d.
[0133] For comparison, a conventional example was prepared in which no protrusion was formed on the connection R portion 23c of the top plate portion 23 of the press-formed product 21 of an intermediate shape as shown in Fig. 13. As with the examples of the invention, FEM analysis was performed on the first and second forming steps of the conventional example to determine the sheet thickness reduction rate of the press-formed product 1 of the target shape at the bottom dead center of forming. In this embodiment, it was previously determined by actual press forming and press forming analysis that cracks would occur if the absolute value of the sheet thickness reduction rate exceeded 10%.
[0134] Table 3 shows the height increment at the convex portion 23d of the press-formed product 21 having the intermediate shape shown in Fig. 2(a) or Fig. 13(a) and the sheet thickness reduction rate at the end of the horizontal side ridge portion 9a of the press-formed product 1 having the target shape. Note that the greater the absolute value of the sheet thickness reduction rate, the greater the sheet thickness reduction.
[0135] [Table 3]
[0136] In the conventional example of No. 21, no protrusions were formed in the intermediate-shape press-formed product 21, and the height increment at the protrusions was set to 0 mm. The sheet thickness reduction rate at the end of the horizontal side ridge portion 9a of the target shape in No. 21 was -11.0%, and the absolute value was large, so that cracks occurred.
[0137] In contrast, in the invention examples No. 22 to No. 25, a convex portion 23d is formed on the top plate portion 23 of the intermediate shape, and the height increment is set to 3 mm to 10 mm. It can be seen that the absolute value of the sheet thickness reduction rate at the end of the horizontal side ridge portion 9a of the target shape in No. 22 to No. 25 is reduced compared to the conventional example (-11.0%). In particular, in No. 25, where the height increment is 10 mm, the sheet thickness reduction rate is -8.1%, and the absolute value is greatly reduced.
[0138] Table 4 shows the height increments at the protrusions 23d and the tip end portions 23a1 of the horizontal side portions 23a of the press-formed product 21 having the intermediate shape shown in Fig. 15 or 13, and the sheet thickness reduction rates at the ends of the horizontal side ridge portions 9a of the press-formed product 1 having the target shape. As in Table 3, the greater the absolute value of the sheet thickness reduction rate, the greater the reduction in sheet thickness.
[0139] [Table 4]
[0140] In the conventional example No. 21, as in Table 3 described above, the sheet thickness reduction rate at the end of the horizontal side ridge portion 9a of the target shape was -11.0%, which was a large absolute value and caused cracks.
[0141] In contrast, in the invention examples No. 31 to No. 34, the height increment at the intermediate shape protrusion 23d and the portion 23a1 at the tip side of the horizontal side portion 23a is set to 3 mm to 10 mm. It can be seen that the absolute value of the sheet thickness reduction rate at the end of the horizontal side ridge portion 9a of the target shape in No. 31 to No. 34 is reduced compared to the conventional example. In particular, in No. 34 where the height increment is set to 10 mm, the sheet thickness reduction rate was -4.7%, which was favorable.
[0142] As described above, the method of the present invention has been shown to be able to suppress cracks at the end of the horizontal edge when manufacturing a press-formed product having an approximately T-shaped top plate portion by press forming in two steps.
[0143] Example 3 In Example 3, a 1.5 GPa-class material having a thickness of 1.2 mm was used as the metal plate of the blank 115, and press-forming was performed by the method of the present invention, the comparative method, and the conventional method for the press-formed product 101 having the target dimensions shown in FIG.
[0144] In the method of the present invention, an intermediate punch 155 shown in Fig. 19 is used in the first forming step to change the height h of the convex portion forming portion 169 of the intermediate punch 155, thereby press-forming into an intermediate formed product 149 in which the height increment Δh of the end portion 146 of the intermediate ridge portion 144 shown in Fig. 20 is changed, and then in the second forming step, press-forming is performed into the target press-formed product 101 shown in Fig. 23. The comparative method is a method of manufacturing a press-formed product in two steps, but in which the convex portion 147 is not formed in the first step. The conventional method is press-formed in one step, as shown in Fig. 24.
[0145] The thickness reduction rate of the end 142 of the ridgeline portion 107 (see FIG. 23) was obtained by FEM analysis. The thickness reduction rate is the value (ratio) obtained by dividing the difference between the thickness of the metal plate that is the blank and the thickness of each portion of the formed product by the thickness of the metal plate that is the blank 115. Table 5 shows the ridgeline portion end height increment Δh and the maximum thickness reduction rate of the target press-formed product 101. Note that it has been found in advance by actual press forming and press forming analysis that cracks will occur in the target press-formed product 101 of Example 3 when the maximum thickness reduction rate is 7.0% or more.
[0146] [Table 5]
[0147] In the conventional example No. 41, which was press-formed in one process, the height increment Δh at the ridge end was 0, and the maximum thickness reduction rate was as large as 8.9%, which caused cracks. In the comparative example No. 42, which was press-formed in two processes, the height increment Δh at the ridge end was 0, and the maximum thickness reduction rate was as large as 7.2%, which caused cracks. In contrast, Nos. 43 to 50 had reduced maximum thickness reduction rates, which indicated that cracks were suppressed. In particular, No. 44 had a maximum thickness reduction rate of 3.9%, which was less than half, and was remarkably good.
[0148] Example 4 In Example 4, a 980 MPa grade material having a thickness of 1.4 mm was used as a blank metal plate, and press-formed product 177 with target dimensions shown in FIG. 30 was press-formed by the method of the present invention, the comparative method, and the conventional method. In the method of the present invention, an intermediate punch 213 shown in FIG. 27(a) was used in the first forming step, and the height H of the punch side convex portion forming portion 223 of the intermediate punch 213 was changed to press-form an intermediate formed product 211 in which the height increment ΔH of the end portion 206 of the intermediate ridge line portion 205 shown in FIG. 28(a) was changed, and then in the second forming step, the target press-formed product 177 shown in FIG. 30 was press-formed. The comparative method is a method for manufacturing a press-formed product 101 in which a convex portion 209 is not formed in the first step, although press-formed in two steps. In the conventional method, press-formed in one step as shown in FIG. 31.
[0149] The thickness reduction rate of the end 185 of the ridgeline 181 (see FIG. 30) was obtained by FEM analysis. Table 6 shows the ridgeline end height increment ΔH and the maximum thickness reduction rate of the target press-formed product 177. Note that it was previously known from actual press forming and press forming analysis that cracks would occur in the target press-formed product 229 of Example 4 when the maximum thickness reduction rate was 10.5% or more.
[0150] [Table 6]
[0151] In the conventional example No. 51, which was press-formed in one process, the height increment ΔH of the ridge end was 0, and the maximum thickness reduction rate was as large as 10.8%, which caused cracks. In the comparative example No. 52, which was press-formed in two processes, the height increment ΔH of the ridge end was 0, and the maximum thickness reduction rate was as large as 10.5%, which caused cracks. In contrast, Nos. 53 to 59 had reduced maximum thickness reduction rates, which indicated that cracks were suppressed. In particular, No. 58 had a maximum thickness reduction rate of 4.6%, which was less than half, and was remarkably good. [Industrial Applicability]
[0152] The present invention can provide a method for manufacturing a press-molded product that can suppress the occurrence of cracks when manufacturing a press-molded product having a generally T-shaped or generally L-shaped top plate portion by press molding. [Explanation of symbols]
[0153] 1 Press-molded products 3 Top plate 3a Side part 3b Vertical side 3c Connection R section 5 Vertical wall section 5a Vertical wall on horizontal side 5b Vertical side vertical wall 5c Connection R side vertical wall 7 Bottom flange 9 Ridge 9a Horizontal side ridgeline part 9b Vertical side ridge 9c Connection R side ridge 11 Blank 13 Punch 15 Pad 17 Die 21 Intermediate shaped press-molded products 23 Top plate 23a Side part 23a1 Tip side part 23b Vertical side 23c Connection R part 23d Convex 25a Horizontal side vertical wall part 29a Lateral side ridgeline part 31 Punch 33 Pad 35 Die 41 Press-molded product (approximately L-shaped) 43 Top plate 43a Side part 43b Vertical side 45 Vertical wall section 45a Horizontal side vertical wall part 47 Bottom flange 49a Side ridgeline 51 Intermediate shaped press-molded product (approximately L-shaped) 53 Top plate 53a Side part 53b Vertical side 55a Horizontal side vertical wall part 61 Punch 63a1 Side edge side molding part 63b Vertical side forming part 63d Convex forming part 71 Punch 73 Top plate molding section 73a Side molding part 73b Vertical side molding part 73c Connection R molding part 73d Convex forming part 101 Press-molded products 103 Top plate 105 Top plate flange 107 Ridge 109 Vertical wall section 111 Vertical flange 113 Horizontal flange section 115 Blank 117 Top plate flange equivalent part 119 Vertical flange equivalent part 121 Mold 123 Punch 125 Pad 127 Die 129 Top plate molding surface section 131 Punch side vertical wall forming surface part 133 Punch side horizontal flange forming surface 135 Punch side vertical flange forming surface 137 Die side vertical wall forming surface 139 Die side horizontal flange forming surface 141 Die side vertical flange forming surface 142 Edge of ridge 143 Intermediate top plate 144 Middle Ridge 145 Intermediate vertical wall 146 End of intermediate ridge 147 Convex 149 Intermediate molded products 151 Intermediate horizontal flange section 153 Intermediate vertical flange 155 Middle Punch 157 Middle Pad 159 Intermediate Die 161 Intermediate top plate molding surface section 163 Punch side intermediate vertical wall forming surface 165 Punch side intermediate horizontal flange forming surface 167 Punch side intermediate vertical flange forming surface 168 Top plate horizontal molding surface 169 Convex forming part 171 Die side intermediate vertical wall forming surface portion 173 Die side intermediate horizontal flange forming surface 175 Die side intermediate vertical flange forming surface 177 Press-molded products 179 Top plate 181 Ridge 183 Vertical wall section 185 Edge of ridge 187 Blank 189 Top plate equivalent part 191 Vertical wall equivalent 193 End of vertical wall 195 Molds 197 Punch 199 Pad 201 Die 203 Intermediate top plate 205 Middle Ridge 206 End of intermediate ridge 207 Intermediate vertical wall 209 Convex 211 Intermediate molded products 213 Middle Punch 215 Middle Pad 217 Intermediate Die 219 Intermediate top plate molding surface section 221 Punch side intermediate vertical wall forming surface 223 Punch side convex forming section 225 Die side intermediate vertical wall forming surface 226 Die side convex forming section 229 Press-molded products
Claims
1. A method for manufacturing a press-molded product having at least a top plate portion, a vertical wall portion, and a ridge portion which is a connection portion between the top plate portion and the vertical wall portion, a first forming process for press-forming a metal sheet blank into an intermediate formed product having an intermediate top plate portion, an intermediate vertical wall portion, and an intermediate ridge portion connecting the intermediate top plate portion and the intermediate vertical wall portion, and having a convex portion higher than a reference height of the top plate surface at one or more locations of the intermediate top plate portion including the intermediate ridge portion; A second molding step of press-molding the intermediate molded product into the press-molded product; It is equipped with In the shape of the press-molded product, The top plate portion has a horizontal side portion, a vertical side portion, and a connection R portion where the horizontal side portion and the vertical side portion are connected, and is substantially T-shaped or substantially L-shaped when viewed from above, the ridge portion that connects to the top plate portion from the horizontal side portion of the top plate portion to the connecting R portion and the vertical side portion; the vertical wall portion extending from the horizontal side portion of the top plate portion to the connecting R portion and the vertical side portion via the ridge portion; A bottom flange portion continuing from the vertical wall portion; It is equipped with In the first molding step, The intermediate top panel portion has an intermediate horizontal side portion, an intermediate vertical side portion, and an intermediate connection R portion where the intermediate horizontal side portion and the intermediate vertical side portion are connected, and is substantially T-shaped or substantially L-shaped when viewed from above, The intermediate molded product is press-molded into the intermediate vertical side portion of the intermediate top plate portion, the height of which is lower than the height of the vertical side portion in a target product shape; Furthermore, in the first molding step, The intermediate molded product is press-molded to have a convex portion that is higher than the height of the vertical side portion at an end portion of the intermediate horizontal side portion of the intermediate top plate portion including the intermediate ridge line portion of the intermediate molded product and / or at an intermediate connection R portion of the intermediate top plate portion including the intermediate ridge line portion of the intermediate molded product. A manufacturing method for press-molded products.
2. In the first molding step, The intermediate horizontal side portion of the intermediate top plate portion including the intermediate ridge line portion is press-formed into the intermediate molded product having the convex portion whose height gradually increases toward the tip side of the intermediate horizontal side portion. A method for producing the press-molded product according to claim 1.
3. In the first molding step, The intermediate horizontal side portion of the intermediate top plate portion including the intermediate ridge line portion is press-formed into the intermediate molded product having the convex portion having a constant height up to the tip side of the intermediate horizontal side portion. A method for producing the press-molded product according to claim 1.
4. In the first molding step, forming the convex portion at the intermediate connection R portion including the intermediate ridge line portion; Further, the intermediate shaped product is press-molded to have the intermediate horizontal side portion of the intermediate top plate portion having a height that matches the height of the protrusion of the intermediate connection R portion. A method for producing the press-molded product according to claim 1.
Citation Information
Patent Citations
Method for forming partial overlap
JP2007029966A
Press molding method
JP2016104492A
Press molding method
JP2019013952A
Manufacturing method for press component, metal plate for press molding, and high-tensile steel plate
JP2021176646A
Blank, and method for producing press-molded article
WO2015174353A1
Cited By
Press forming method
JP2026130447A