Soluble germicidal glass and method for preparing soluble germicidal glass

A soluble sterilizing glass with controlled ternary oxide compositions regulates silver ion release, addressing the sustained release issues of conventional antibacterial glass, providing stable bactericidal performance for home appliances.

JP7582713B2Active Publication Date: 2024-11-13WUXI LITTLE SWAN ELECTRIC CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023537414
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-31
Filing Date
2021-05-17
Publication Date
2024-11-13
Estimated Expiration
2041-05-17

AI Technical Summary

Technical Problem

Conventional silver-supported antibacterial glass materials suffer from insufficient sustained release performance of silver ions, leading to inconsistent bactericidal effects over time.

Method used

A soluble sterilizing glass composed of ternary oxides, including boron oxide, calcium oxide, and phosphorus oxide, with controlled ratios to regulate the release rate of silver ions, along with optional additives like cerium oxide for enhanced bactericidal efficiency and colorants for customization.

Benefits of technology

The glass effectively controls the release rate and efficiency of silver ions, ensuring long-term bactericidal action with stable performance and improved production efficiency, suitable for applications in home appliances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582713000001
    Figure 0007582713000001
  • Figure 0007582713000002
    Figure 0007582713000002
  • Figure 0007582713000003
    Figure 0007582713000003
Patent Text Reader

Abstract

The present application relates to a soluble germicidal glass and a method for preparing the soluble germicidal glass. The material of the soluble germicidal glass includes 0.1 to 5 parts by mass of silver oxide, 1 to 20 parts by mass of boron oxide, 10 to 30 parts by mass of calcium oxide, and 30 to 70 parts by mass of phosphorus oxide. The prepared soluble germicidal glass can improve the sustained release performance of silver ions as a germicide in the soluble germicidal glass and can release silver ions at a reasonable speed, thereby improving the germicidal efficiency and germicidal effect of the soluble germicidal glass.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims priority to a Chinese patent application filed with the State Intellectual Property Office of the People's Republic of China on December 31, 2020, bearing application number 20202011635297.0 and entitled "Soluble germicidal glass and method for preparing soluble germicidal glass," the entire contents of which are incorporated herein by reference.

[0002] The present application relates to the technical field of inorganic antimicrobial materials, and in particular to a soluble germicidal glass and a method for preparing the soluble germicidal glass. [Background technology]

[0003] Antibacterial materials are functional materials with bactericidal and antibacterial properties, and their antibacterial action is mainly achieved by adding antibacterial agents. Antibacterial agents are mainly classified into three types: natural organisms, organic, and inorganic antibacterial agents.

[0004] Natural antibacterial agents such as chitosan and sorbic acid have been extensively studied. These agents are safe, environmentally friendly, and have excellent antibacterial properties. However, they have poor heat resistance, a short effective period, and limited production conditions, making their industrialization difficult.

[0005] Organic antibacterial agents contain organic substances such as organic acids, phenols, quaternary ammonium salts, and benzimidazoles as antibacterial ingredients, and are effective in inhibiting the growth of harmful bacteria and mold. However, they are unstable, easily decomposed, and usually highly toxic.

[0006] Inorganic antibacterial agents are mainly obtained by adding antibacterial metals or their ions to porous materials such as zeolite and silica gel, or materials such as glass. Inorganic antibacterial materials have the characteristics of longer-lasting effectiveness, broad-spectrum antibacterial properties, good heat resistance, and safety compared to organic and biological antibacterial materials.

[0007] Among many inorganic antibacterial agents, silver is one of the antibacterial agents with relatively good performance and relatively wide use. Silver-loaded antibacterial glass materials have excellent antibacterial effect and good safety, so extensive application research is being conducted.

[0008] However, one of the drawbacks of the conventional technology is that the sustained release performance of the silver-loaded antibacterial glass material is insufficient. Summary of the Invention

[0009] The present application aims to solve at least one of the above technical problems.

[0010] Therefore, a first object of the present application is to provide a soluble germicidal glass.

[0011] A second object of the present application is to provide a method for preparing a soluble germicidal glass.

[0012] In order to achieve the first object of the present application, an embodiment of the present application provides a soluble germicidal glass, the material of the soluble germicidal glass including 0.1 to 5 parts by weight of silver oxide, 1 to 20 parts by weight of boron oxide, 10 to 30 parts by weight of calcium oxide, and 30 to 70 parts by weight of phosphorus oxide.

[0013] The present technical solution provides a ternary oxide soluble sterilizing glass mainly composed of boron oxide, calcium oxide and phosphorus oxide, in order to rationally control the sustained release rate and sustained release efficiency of silver ions in the soluble sterilizing glass. By adding phosphorus oxide and boron oxide and controlling the proportion, silver ions can be sustained release at a reasonable speed in the boron calcium phosphorus ternary oxide soluble sterilizing glass. Specifically, the applicant, regardless of any theory, has found in the process of realizing the present application that the addition of phosphorus oxide can increase the dissolution rate of silver ions to promote the release of silver ions. Conversely, the addition of boron oxide can reduce the dissolution rate of silver ions to inhibit the release of silver ions. Therefore, the present technical solution controls the addition amount and specific ratio of phosphorus oxide and boron oxide (i.e., the content of phosphorus oxide is 30 parts by weight to 70 parts by weight, and the content of boron oxide is 1 part by weight to 20 parts by weight). As a result, the present technical solution can rationally control the sustained release rate and sustained release efficiency of silver ions in the soluble sterilizing glass. In addition, the addition of calcium oxide can appropriately lower the melting temperature of the soluble sterilizing glass, reduce the manufacturing cost of the soluble sterilizing glass, and improve the production efficiency of the soluble sterilizing glass.

[0014] In addition, the technical solutions provided by the above embodiments of the present application have the following additional technical features:

[0015] In the above technical solution, the soluble sterilizing glass further includes 0.0001 to 0.0008 parts by weight of a colorant.

[0016] The purpose of adding coloring agents is to adjust and control the color of the soluble germicidal glass to meet the various needs of users.

[0017] In any of the above technical solutions, the colorant includes at least one of cobalt oxide, manganese oxide, iron oxide, copper oxide, and cadmium sulfide, or a combination thereof.

[0018] The colorant used in this technical solution is specifically a metal oxide colorant, which has stable performance, is resistant to high temperatures, and is not easily decomposed.

[0019] In any of the above technical solutions, the soluble sterilizing glass further contains 0.0001 to 0.0006 parts by weight of cerium oxide.

[0020] The addition of cerium oxide to the soluble germicidal glass can increase the proportion of high-valent silver ions in the silver ions as germicide, and therefore can improve the germicidal effect and germicidal efficiency of the soluble germicidal glass according to the examples of the present application.

[0021] In any of the above technical solutions, the silver ions in the soluble sterilizing glass include divalent silver ions and / or trivalent silver ions.

[0022] Since divalent silver ions and / or trivalent silver ions have a higher bactericidal effect and bactericidal efficiency than monovalent silver ions, a soluble bactericidal glass containing divalent silver ions and / or trivalent silver ions has an excellent bactericidal effect as well as a sustained-release effect.

[0023] In any of the above technical solutions, the soluble sterilizing glass further includes at least one of lithium oxide, sodium oxide, potassium oxide, magnesium oxide, silicon oxide, and aluminum oxide, or a combination thereof.

[0024] Alkali metal oxides or alkaline earth metal oxides, including lithium oxide, sodium oxide, and potassium oxide, have relatively active physicochemical properties and can effectively lower the melting point of soluble sterilized glass. The addition of silicon oxide and aluminum oxide promotes the formation of glass and improves the viscosity and mechanical strength of soluble sterilized glass. Magnesium oxide increases the clarity of the molten glass and the gloss and refractive index of the soluble sterilized glass after molding.

[0025] In any of the above technical solutions, the amount of silver ions eluted from the soluble sterilizing glass is 1 mg silver ions / g water to 500 mg silver ions / g water.

[0026] This technical solution can effectively control the release concentration and speed of silver ions in the soluble germicidal glass, and ensure that the soluble germicidal glass can achieve a long-term and effective germicidal effect.

[0027] In any of the above technical solutions, the thickness range of the soluble germicidal glass is 3mm to 5mm, and / or the length range of the soluble germicidal glass is 5mm to 8mm.

[0028] The soluble sterilized glass of the above size can meet the production and processing needs of many household appliances, and has a relatively reasonable sustained release period and good sustained release efficiency. In addition, the soluble sterilized glass of the above size can be cooled immediately under natural conditions, is not likely to explode or break into pieces, has a high yield rate during molding, has small internal stress, and has good mechanical strength and thermal stability without the need for an annealing process.

[0029] In order to achieve the second object of the present application, an embodiment of the present application provides a method for preparing a soluble sterilizing glass, including the steps of weighing and mixing raw materials in a mass ratio of silver oxide:boron oxide:calcium oxide:phosphorus oxide=(0.1-5):(1-20):(10-30):(30-70) to obtain a mixture, melting the mixture to obtain a glass liquid, and cooling and forming the glass liquid to obtain a soluble sterilizing glass.

[0030] The preparation method of the soluble germicidal glass according to the embodiments of the present application can obtain the soluble germicidal glass according to any one of the embodiments of the present application, and the preparation method of the soluble germicidal glass according to the embodiments of the present application has all the beneficial effects of the soluble germicidal glass according to any one of the embodiments of the present application, so no further mention will be made here.

[0031] In the above technical solution, melting the mixture to obtain a glass liquid includes melting the mixture within a temperature range of 950°C to 1350°C for 0.5 to 2 hours to obtain a glass liquid.

[0032] The above temperature control ensures sufficient melting of each metal oxide and ensures that a homogeneous, clear, soluble, sterilized glass can be obtained in this embodiment.

[0033] The above technical solution further includes pre-heating the mixture before melting the mixture to obtain a glass liquid.

[0034] The purpose of the pre-heating process is to more effectively remove impurities and gases from the raw materials, prevent the glass liquid from generating excessive bubbles during the melting process, and ensure that the soluble sterilized glass material is firm and dense.

[0035] In the above technical solution, preheating the mixture includes preheating the mixture within a temperature range of 250°C to 350°C for 0.5 hours to 1.5 hours.

[0036] The above preheating conditions can effectively remove impurities and gases in the raw material.

[0037] In the above technical solution, the step of cooling and forming the glass liquid to obtain the soluble sterilized glass includes the steps of preheating a metal mold, pouring the glass liquid into the metal mold and naturally cooling and forming the glass to obtain the soluble sterilized glass.

[0038] By pre-heating the metal mold before cooling and forming, the glass liquid can be prevented from bursting during the process of tipping and forming.

[0039] In the above technical solution, preheating the metal mold includes preheating the metal mold to a temperature range of 200℃ to 300℃.

[0040] The above-mentioned temperature control for preheating the metal mold can effectively prevent the glass from exploding during cooling and forming, and can improve the yield.

[0041] In the above technical solution, the raw materials include a silver source raw material including at least one of silver nitrate, silver chloride, silver sulfate, silver carbonate, silver bromide, silver iodide, silver oxide, or a combination thereof, and / or a boron source raw material including boric acid, and / or a calcium source raw material including at least one of calcium carbonate, calcium nitrate, calcium sulfate, calcium phosphate, calcium chloride, calcium oxide, or a combination thereof, and / or a phosphorus source raw material including at least one of calcium phosphate, ammonium phosphate, phosphorus oxide, or a combination thereof.

[0042] Raw materials containing silver, boron, calcium, and phosphorus may be added directly as oxides or as salt compounds. Among these, using metal salt compounds as raw materials can improve the homogeneity and clarity of glass compared to using metal oxides as raw materials.

[0043] Additional aspects and advantages of the present application will be set forth in the description which follows, or may be learned by practice of the present application. [Brief description of the drawings]

[0044] The above and / or additional aspects and advantages of the present application will become apparent and understandable from the following detailed description of the embodiments in conjunction with the drawings, in which:

[0045] [Figure 1] 1 is a step flow chart of a method for preparing a soluble sterilizing glass according to an embodiment of the present application; [Diagram 2] 2 is a step flow chart of a method for preparing a soluble sterilizing glass according to an embodiment of the present application; [Diagram 3] 3 is a flow chart showing step 3 of a method for preparing a soluble sterilizing glass according to an embodiment of the present application; [Figure 4] 4 is a flow chart showing step 4 of a method for preparing a soluble germicidal glass according to an embodiment of the present application. [Diagram 5] 5 is a step flow chart of a method for preparing a soluble germicidal glass according to an embodiment of the present application; [Figure 6] 6 is a flow chart showing step 6 of a method for preparing a soluble germicidal glass according to an embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0046] In order to make the above-mentioned objects, features and advantages of the present application more clearly understandable, the present application will be described in more detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other without conflict.

[0047] In the following description, many specific details are set forth in order to fully understand the present application; however, the present application may be implemented in other ways different from the description, and therefore the scope of protection of the present application is not limited by the specific examples disclosed below.

[0048] Hereinafter, soluble germicidal glass and a method for preparing the soluble germicidal glass according to some embodiments of the present application will be described with reference to Figs. 1 to 6.

[0049] The material of the soluble sterilizing glass of this embodiment includes 0.1 to 5 parts by weight of silver oxide (AgO and / or Ag2O), 1 to 20 parts by weight of boron oxide (B2O3), 10 to 30 parts by weight of calcium oxide (CaO), and 30 to 70 parts by weight of phosphorus oxide (P2O5).

[0050] For example, the material of the soluble germicidal glass of this embodiment specifically contains 0.1 parts by weight of silver oxide, 19.9 parts by weight of boron oxide, 10 parts by weight of calcium oxide, and 70 parts by weight of phosphorus oxide.

[0051] Further, for example, the material of the soluble germicidal glass of this embodiment specifically contains 5 parts by weight of silver oxide, 20 parts by weight of boron oxide, 30 parts by weight of calcium oxide, and 45 parts by weight of phosphorus oxide.

[0052] The embodiment of the present application aims to provide a soluble glass. Here, the soluble glass refers to a soluble, sterilizable glass that can slowly and steadily release one or more functional ions in a liquid, such as water. The functional ions in the embodiment of the present application are specifically silver ions (Ag + and / or Ag 2+ Silver ions have good bactericidal and disinfecting effects, and occupy the lattice of metal oxide glass in the form of a dope. When immersed in liquid or scoured, they are steadily released over time, achieving a long-term bactericidal effect.

[0053] Soluble germicidal glass containing silver ions can be applied to home appliances such as washing machines and air conditioners to sterilize the washing water of the washing machine and the indoor space the air conditioner is installed in. However, one of the problems in the conventional technology is that the sustained release performance of silver ions that realize the germicidal function is insufficient.

[0054] Specifically, it is difficult to control the sustained release performance of silver ions in the soluble germicidal glass of the related art. Take the silver ion-doped soluble germicidal glass placed in a washing machine as an example. In a certain washing procedure and washing time range, if the release speed of silver ions in the soluble germicidal glass is too fast, the silver ions will be released early, and the germicidal effect during the later use of the washing machine will be reduced, and even the germicidal effect will be lost. If the release speed of silver ions in the soluble germicidal glass is too slow, the germicidal effect during the entire use of the washing machine will be insufficient, making it difficult to effectively sterilize clothes and home textiles.

[0055] Regardless of any theory, the applicant has found that in the process of realizing the embodiments of the present application, the release rate of silver ions is influenced by the amount of silver ions added and the components and compounding ratio of the soluble glass as the base material. Therefore, the embodiments of the present application provide a ternary oxide soluble sterilizing glass mainly composed of boron oxide, calcium oxide and phosphorus oxide, in order to rationally control the release rate and release efficiency of silver ions in the soluble sterilizing glass. However, the mass ratio of boron oxide, calcium oxide and phosphorus oxide is boron oxide:calcium oxide:phosphorus oxide=(1-20):(10-30):(30-70). The raw materials with the above components and compounding ratios can be within the glass-forming region. By adding and proportionally controlling phosphorus oxide and boron oxide, silver ions can be released at a reasonable speed in the boron calcium phosphorus ternary oxide soluble sterilizing glass. The addition of phosphorus oxide increases the dissolution rate of silver ions to promote the release of silver ions, while the addition of boron oxide reduces the dissolution rate of silver ions to suppress the release of silver ions.Therefore, in this embodiment, the compounding ratio between phosphorus and boron can be controlled to rationally control the release rate and release efficiency of silver ions in the soluble sterilizing glass.In addition, the addition of calcium oxide can appropriately reduce the melting temperature of the soluble sterilizing glass, reduce the production cost of the soluble sterilizing glass, and improve the production efficiency of the soluble sterilizing glass.

[0056] In some embodiments of the examples of the present application, the soluble sterilizing glass further includes 0.0001 to 0.0008 parts by weight of a colorant. For example, the content of the colorant in the soluble sterilizing glass of this embodiment may be 0.0001 parts by weight, 0.0004 parts by weight, or 0.0008 parts by weight. The purpose of adding the colorant is to adjust and control the color of the soluble sterilizing glass. Here, those skilled in the art can flexibly select and adjust the amount and specific type of the colorant added within the above range. The colorant can be added and mixed together with the substrate raw material such as boron oxide, calcium oxide, and phosphorus oxide during the raw material blending process, and the colorant can be uniformly distributed in the molten glass liquid during the process of the soluble sterilizing glass entering the melting and heating process, and a soluble sterilizing glass with a uniform color can be obtained after melting and cooling.

[0057] In some embodiments of the present application, the colorant includes at least one of cobalt oxide (Co2O3), manganese oxide (MnO2), iron oxide (Fe2O3 and / or Fe3O4), copper oxide (CuO), and cadmium sulfide (CdS), or a combination thereof. The colorant of this embodiment is specifically a metal oxide colorant. The metal oxide colorant has stable performance, is resistant to high temperatures, and is not easily decomposed.

[0058] In some embodiments of the examples of the present application, the soluble sterilizing glass further contains 0.0001 to 0.0006 parts by weight of cerium oxide. For example, the content of cerium oxide in the soluble sterilizing glass of the present examples may be 0.0001 parts by weight, 0.0003 parts by weight, or 0.0006 parts by weight. The rare earth element cerium ion (Ce 3+ ) is characterized by having a rich energy level and a high atomic valence. By adding cerium oxide to the boron-calcium-phosphorus ternary oxide soluble bactericidal glass, the proportion of high-valence silver ions (i.e., divalent silver ions or trivalent silver ions) in the silver ions serving as a bactericide can be increased. Therefore, the addition of cerium oxide can improve the bactericidal effect and bactericidal efficiency of the soluble bactericidal glass according to the examples of the present application.

[0059] In some embodiments of the examples of the present application, the silver ions in the soluble sterilizing glass include divalent silver ions and / or trivalent silver ions. As described above, divalent silver ions and / or trivalent silver ions have higher bactericidal effect and bactericidal efficiency than monovalent silver ions, so the soluble sterilizing glass containing divalent silver ions and / or trivalent silver ions has excellent bactericidal effect as well as sustained release effect.

[0060] In some embodiments of the present application, the soluble sterilized glass further comprises at least one of lithium oxide, sodium oxide, potassium oxide, magnesium oxide, silicon oxide, and aluminum oxide, or a combination thereof. Alkali metal oxides or alkaline earth metal oxides, including lithium oxide, sodium oxide, and potassium oxide, have relatively active physicochemical properties and can effectively lower the melting point (i.e., melting temperature) of the soluble sterilized glass. The addition of silicon oxide and aluminum oxide promotes the formation of glass and improves the viscosity and mechanical strength of the soluble sterilized glass. Magnesium oxide increases the clarity of the molten glass liquid and the gloss and refractive index of the soluble sterilized glass after molding.

[0061] In some embodiments of the examples of the present application, the amount of silver ions eluted in the soluble sterilized glass is 1 mg silver ions / g water to 500 mg silver ions / g water. In this embodiment, the amount of silver ions eluted is tested by a method of preparing a measurement sample by filtering the silver ion eluate with 5C filter paper. After preparing the measurement sample, the silver ion concentration in the sample is measured using a test analysis device capable of measuring the silver ion concentration, such as a silver ion meter, an atomic absorption spectrometer, or an inductively coupled plasma mass spectrometry device (ICP-MS). The amount of silver ions eluted under a temperature condition of 30°C and a test time of 24 hours obtained in the test of this embodiment is XX mg silver ions / g water to XX mg silver ions / g water, that is, 1 (mg / (g·1L·24Hrs·30°C)) to 500 (mg / (g·1L·24Hrs·30°C)).

[0062] In some embodiments of the examples of the present application, the thickness range of the soluble sterilizing glass is 3mm to 5mm. The length range of the soluble sterilizing glass is 5mm to 8mm. The size and shape of the soluble sterilizing glass are consistent with the size and shape of the molding die employed. The soluble sterilizing glass of this embodiment may be prepared in a sheet, plate, or block shape, or may be prepared in a spherical or approximately spherical shape. The sustained release efficiency and sustained release period of silver ions are affected by the size and shape of the soluble sterilizing glass. The soluble sterilizing glass manufactured using a molding die having a thickness range of 3mm to 5mm and a length range of 5mm to 8mm can meet the production and processing needs of many home appliances, and has a relatively reasonable sustained release period and excellent sustained release efficiency. In addition, the soluble sterilizing glass having a thickness range of 3mm to 5mm and a length range of 5mm to 8mm can be cooled immediately under natural conditions, is unlikely to explode or separate into fragments, has a high yield during molding, has small internal stress, and has good mechanical strength and thermal stability without the need for an annealing process.

[0063] FIG. 1 is a step flow chart of a method for preparing soluble germicidal glass according to an embodiment of the present application. As shown in FIG. 1, the method for preparing soluble germicidal glass according to an embodiment of the present application includes: Step S102 of weighing and mixing raw materials in a mass ratio of silver oxide:boron oxide:calcium oxide:phosphorus oxide=(0.1-5):(1-20):(10-30):(30-70) to obtain a mixture; Step S104 of melting the mixture to obtain a glass liquid; and step S106 of cooling and forming the glass liquid to obtain a soluble sterilized glass.

[0064] In the soluble sterilizing glass according to the embodiment of the present application, the content of silver oxide as a sterilizing agent is 0.1 wt% to 5 wt%, the content of boron oxide is 1 wt% to 20 wt%, the content of calcium oxide is 10 wt% to 30 wt%, and the content of phosphorus oxide is 30 wt% to 70 wt%, based on 100 parts by mass (100 wt%) of the total mass of the soluble sterilizing glass. In this embodiment, the ratio relationship of each oxide in the soluble sterilizing glass is limited by mass fraction. When the oxide of each element is directly used as a raw material, in this embodiment, the load bearing capacity of the raw material can be directly measured based on the proportional relationship in step S102. When the salt compound of each element is directly used as a raw material, in this embodiment, the original weighing proportion can be determined from the conversion relationship between the molar mass and mass fraction of each raw material. When a liquid raw material is used, in this embodiment, the original weighing proportion can be determined from the conversion relationship between the volume concentration and mass fraction. Those skilled in the art are aware of the above conversion and weighing methods, and the examples of this application do not refer to them.

[0065] In addition, in this embodiment, in addition to the main raw materials including silver oxide, boron oxide, calcium oxide, and phosphorus oxide, other metal oxide secondary materials can also be added. For example, in this embodiment, silver nitrate (AgNO3), calcium phosphate (Ca(H2PO4)2), sodium phosphate (NaH2PO4), ammonium phosphate (NH4H2PO4), boric acid (H3BO3), zinc oxide (ZnO), copper oxide (CuO), cobalt oxide (Co2O3), and cerium oxide CeO2 can be used as raw materials. Here, assuming the total mass of all raw materials is 100 wt%, the mass ratio of each raw material to the total raw materials is as follows: silver nitrate occupies 3 wt%, calcium phosphate occupies 78 wt%, sodium phosphate occupies 8.7 wt%, ammonium phosphate occupies 0.9 wt%, boric acid occupies 5.9 wt%, zinc oxide occupies 2.55 wt%, copper oxide occupies 0.4 wt%, cobalt oxide occupies 0.05 wt%, and cerium oxide occupies 0.5 wt%. When preparing a less soluble sterilized glass, the weighing process in the embodiment of the present application can be realized by using an analytical balance, and the raw materials are mixed and ground in a small mixing equipment such as an agate mortar or a planetary ball mill, and the mixture placed in a platinum crucible is melted in an electric resistance furnace or a muffle furnace, and finally the glass liquid in the platinum crucible is tilted onto an aluminum plate mold or an iron plate mold for cooling and forming.

[0066] When preparing a large amount of soluble sterilizing glass in actual production, the weighing process in the embodiment of the present application can be realized by using a large platform scale, the mixing mill realizes the mixing and grinding of the raw materials, and the large equipment such as a kiln realizes the melting and cooling of the mixture.

[0067] The cooling and forming step in step S106 may be performed by natural cooling, furnace cooling, or water quenching.

[0068] The melting process in step S104 may be performed in an air atmosphere, a reducing atmosphere, or an inert gas atmosphere.

[0069] After cooling, the present embodiment can also carry out an annealing process to remove the internal stress of the soluble sterilized glass. The temperature range of the annealing process is 200°C to 500°C, and the annealing period is 2 hours to 4 hours.

[0070] The preparation method of the soluble germicidal glass according to the embodiment of the present application can obtain the soluble germicidal glass according to any one of the embodiments of the present application, which is doped with a silver ion germicidal agent with excellent sustained release performance and reasonably controllable sustained release efficiency. The preparation method of the soluble germicidal glass according to the embodiment of the present application has all the beneficial effects of the soluble germicidal glass according to any one of the embodiments of the present application, and will not be further mentioned here.

[0071] In some embodiments of the examples of the present application, melting the mixture to obtain a glass liquid includes melting the mixture at a temperature range of 950°C to 1350°C for 0.5 hours to 2 hours to obtain a glass liquid. Figure 2 is a step flow chart 2 of a method for preparing a soluble sterilizing glass according to one embodiment of the present application. As shown in Figure 2, the method for preparing a soluble sterilizing glass of this embodiment includes the following steps: A step S202 of weighing and mixing raw materials in a mass ratio of silver oxide:boron oxide:calcium oxide:phosphorus oxide=(0.1-5):(1-20):(10-30):(30-70) to obtain a mixture; Step S204 of melting the mixture at a temperature range of 950° C. to 1350° C. for 0.5 to 2 hours to obtain a glass liquid; and step S206 of cooling and forming the glass liquid to obtain a soluble sterilized glass.

[0072] The temperature control in the melting process adopted in step S204 of the present embodiment ensures that each metal oxide is melted sufficiently, and that the present embodiment can obtain a homogeneous and clear soluble sterilized glass.

[0073] In some embodiments of the examples of the present application, the preparation method further includes a step of preheating the mixture before melting the mixture to obtain a glass liquid. Figure 3 is a step flow chart of a preparation method for soluble germicidal glass according to an embodiment of the present application. As shown in Figure 3, the preparation method for soluble germicidal glass of this embodiment includes: Step S302 of weighing and mixing raw materials in a mass ratio of silver oxide:boron oxide:calcium oxide:phosphorus oxide=(0.1-5):(1-20):(10-30):(30-70) to obtain a mixture; A step S304 of preheating the mixture; Step S306 of melting the mixture to obtain a glass liquid; and step S308 of cooling and forming the glass liquid to obtain a soluble sterilized glass.

[0074] The purpose of the pre-heating process is to more effectively remove impurities and gases from the raw materials, prevent the glass liquid from generating excessive bubbles during the melting process, and ensure that the soluble sterilized glass material is firm and dense.

[0075] In some embodiments of the examples of the present application, preheating the mixture includes preheating the mixture within a temperature range of 250°C to 350°C for 0.5 hours to 1.5 hours. FIG. 4 is step 4 of a flowchart of a method for preparing a soluble germicidal glass according to an example of the present application. As shown in FIG. 4, the method for preparing a soluble germicidal glass of this embodiment includes the following steps: Step S402: weighing and mixing raw materials in a mass ratio of silver oxide:boron oxide:calcium oxide:phosphorus oxide=(0.1-5):(1-20):(10-30):(30-70) to obtain a mixture; Step S404 of preheating the mixture within a temperature range of 250° C. to 350° C. for 0.5 hours to 1.5 hours; Step S406 of melting the mixture to obtain a glass liquid; and step S408 of cooling and forming the glass liquid to obtain a soluble sterilized glass.

[0076] In this embodiment, the mixture is preheated within the temperature range of 250°C to 350°C, and the preheating time is more than 0.5 hours and less than 1.5 hours. The above preheating conditions can effectively remove impurities and gases in the raw materials.

[0077] In some embodiments of the examples of the present application, cooling and forming the glass liquid to obtain a soluble sterilized glass includes preheating a metal mold, pouring the glass liquid into the metal mold and naturally cooling and forming it to obtain a glass liquid. Figure 5 is a step flow chart of a method for preparing a soluble sterilized glass according to an embodiment of the present application. As shown in Figure 5, the method for preparing a soluble sterilized glass of this embodiment includes: Step S502: weighing and mixing raw materials in a mass ratio of silver oxide:boron oxide:calcium oxide:phosphorus oxide=(0.1-5):(1-20):(10-30):(30-70) to obtain a mixture; Step S504 of melting the mixture to obtain a glass liquid; A step S506 of preheating the metal mold; and step S508 of pouring the glass liquid into a metal mold and allowing it to cool naturally to obtain a soluble sterilized glass.

[0078] The metal mold of this embodiment may be a metal mold having excellent heat resistance and thermal conductivity, such as an aluminum mold or an iron mold. The purpose of preheating the metal mold before cooling and forming is to prevent the glass liquid from falling and exploding during the forming process. Natural cooling forming refers to placing the metal mold containing the glass liquid in a room temperature environment (for example, between 20°C and 30°C) and naturally cooling it until the liquid glass liquid becomes a solid lump glass body.

[0079] In some embodiments of the examples of the present application, preheating the metal mold includes preheating the metal mold to a temperature range of 200°C to 300°C. FIG. 6 is step 6 of a flowchart of a method for preparing soluble germicidal glass according to an embodiment of the present application. As shown in FIG. 6, the method for preparing soluble germicidal glass of this embodiment includes the following steps: Step S602: weighing and mixing raw materials in a mass ratio of silver oxide:boron oxide:calcium oxide:phosphorus oxide=(0.1-5):(1-20):(10-30):(30-70) to obtain a mixture; Step S604 of melting the mixture to obtain a glass liquid; Step S606: preheating the metal mold to a temperature range of 200°C to 300°C; and step S608 of pouring the glass liquid into a metal mold and allowing it to cool naturally to obtain a soluble sterilized glass.

[0080] In this embodiment, the mold is preheated within a temperature range of 200°C to 300°C, and the preheating time is 1 hour to 2 hours. For example, in this embodiment, melting of the raw material and preheating of the metal mold can be realized by using two electric resistance furnaces, respectively. The temperature rise rate of the raw material heating and the temperature rise rate of the metal mold preheating can be selected and adjusted by those skilled in the art according to the performance of the heating equipment. However, in this embodiment, the electric resistance furnace for preheating the metal mold is opened after the raw material approaches or reaches the melting temperature so that the preheating is completed and the metal mold with the appropriate temperature can be immediately taken out and used after the mixture is melted to obtain a glass liquid.

[0081] In some embodiments of the examples of the present application, the raw material comprises a silver source raw material, the silver source raw material comprising at least one of silver nitrate (AgNO3), silver chloride (AgCl), silver sulfate (Ag2SO4), silver carbonate (Ag2CO3), silver bromide (AgBr), silver iodide (AgI), silver oxide (Ag2O), or a combination thereof.

[0082] In some embodiments of the examples of the present application, the raw material comprises a boron source material, and the boron source material comprises boric acid (H3BO3).

[0083] In some embodiments of the examples of the present application, the raw material comprises a calcium source material, the calcium source material comprising at least one of calcium carbonate (CaCO), calcium nitrate (Ca(NO)), calcium sulfate (CaSO), calcium phosphate (Ca(HPO) or CaHPO), calcium chloride (CaCl), calcium oxide (CaO), or a combination thereof.

[0084] In some embodiments of the examples of the present application, the raw material comprises a phosphorus source raw material, the phosphorus source raw material comprises at least one of calcium phosphate (Ca(H2PO4)2 or CaHPO4), ammonium phosphate (NH4)3PO4), phosphorus oxide (PO5), or a combination thereof.

[0085] The silver source raw material is a raw material for supplying silver oxide. Accordingly, the boron source raw material, calcium source raw material, and phosphorus source raw material are in the order of raw material for supplying boron oxide, raw material for supplying calcium oxide, and raw material for supplying phosphorus oxide. The raw materials containing silver, boron, calcium, and phosphorus may be added directly as oxides (i.e., silver oxide, boron oxide, calcium oxide, and phosphorus oxide may be added directly as raw materials), or may be added as salt compounds (for example, substances such as silver chloride, boric acid, calcium carbonate, various phosphates, and calcium phosphates may be added as raw materials). Here, when salt compounds are used as raw materials, each salt compound containing silver, boron, calcium, and phosphorus is oxidized under high temperature conditions to become an oxide, and an oxide glass is obtained after melting. Among them, using metal salt compounds as raw materials can improve the homogeneity and clarity of glass compared to using metal oxides as raw materials.

[0086] From the above, the beneficial effects of the embodiments of the present application are as follows:

[0087] 1. In the embodiments of the present application, by selecting the materials of the soluble germicidal glass and adjusting the compounding ratio, the release concentration and speed of silver ions in the soluble germicidal glass can be effectively controlled, so as to ensure that the soluble germicidal glass can achieve a long-term and effective germicidal effect.

[0088] 2. In the embodiments of the present application, by adjusting the processing steps of the soluble germicidal glass, a soluble germicidal glass with high mechanical strength, high clarity and high silver ion loading can be obtained.

[0089] In the description herein, the term "one embodiment," "some embodiments," "specific embodiments," and the like means that the specific features, structures, materials, or characteristics described in connection with the embodiment or example are included in at least one embodiment or example of the present application. In the present specification, general expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.

[0090] The above is only a preferred embodiment of the present application, and does not limit the present application. Those skilled in the art can make various modifications and variations to the present application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.

Claims

1. A silver ion doped soluble germicidal glass, comprising: The material of the soluble germicidal glass is 0.1 parts by mass to 5 parts by mass of silver oxide, 1 part by mass to 20 parts by mass of boron oxide, 10 parts by mass to 30 parts by mass of calcium oxide, 30 parts by mass to 70 parts by mass of phosphorus oxide, cerium oxide 0.0001 part by mass to 0.0006 part by mass, Contains 0.0001 parts by weight to 0.0008 parts by weight of a colorant; The colorant is copper oxide, The silver ions in the silver ion-doped soluble germicidal glass include divalent silver ions and / or trivalent silver ions. A silver ion doped soluble germicidal glass characterized by:

2. The colorant further comprises at least one of cobalt oxide, manganese oxide, iron oxide, cadmium sulfide, or a combination thereof.

2. The silver ion doped soluble germicidal glass of claim 1.

3. Further comprising at least one of lithium oxide, sodium oxide, potassium oxide, magnesium oxide, silicon oxide, aluminum oxide, or a combination thereof.

2. The silver ion doped soluble germicidal glass of claim 1.

4. The amount of silver ions eluted from the soluble sterilizing glass is 1 mg silver ion / g water to 500 mg silver ion / g water.

4. A soluble, bactericidal glass doped with silver ions according to claim 1.

5. the thickness range of said soluble germicidal glass is between 3 mm and 5 mm; and / or The length of the soluble germicidal glass ranges from 5 mm to 8 mm.

4. A soluble, bactericidal glass doped with silver ions according to claim 1.

6. A method for preparing a silver ion doped soluble germicidal glass comprising the steps of: A step of weighing and mixing raw materials in a mass ratio of silver oxide:boron oxide:calcium oxide:phosphorus oxide=(0.1-5):(1-20):(10-30):(30-70) to obtain a mixture; melting the mixture to obtain a glass liquid; and cooling and forming the glass liquid to obtain the soluble sterilized glass. The silver ions in the soluble sterilizing glass include divalent silver ions and / or trivalent silver ions, The raw material is a silver source source comprising at least one of silver nitrate, silver chloride, silver sulfate, silver carbonate, silver bromide, silver iodide, silver oxide, or a combination thereof; and / or a boron source material comprising boric acid; and / or a calcium source material comprising at least one of calcium carbonate, calcium nitrate, calcium sulfate, calcium phosphate, calcium chloride, calcium oxide, or a combination thereof; and / or The phosphorus source material includes at least one of calcium phosphate, ammonium phosphate, phosphorus oxide, or a combination thereof.

1. A method for preparing a silver ion-doped soluble bactericidal glass, comprising:

7. The step of melting the mixture to obtain a glass liquid includes: The mixture is melted at a temperature in the range of 950° C. to 1350° C. for 0.5 to 2 hours to obtain the glass liquid.

7. The method for preparing silver ion doped soluble germicidal glass according to claim 6.

8. The method further includes a step of preheating the mixture before melting the mixture to obtain a glass liquid.

7. The method for preparing silver ion doped soluble germicidal glass according to claim 6.

9. The step of preheating the mixture includes preheating the mixture within a temperature range of 250° C. to 350° C. for 0.5 hours to 1.5 hours.

9. The method for preparing silver ion doped soluble germicidal glass according to claim 8.

10. The step of cooling and forming the glass liquid to obtain the soluble sterilized glass comprises: preheating a metal mold; and pouring the glass liquid into the metal mold and allowing it to cool naturally to obtain a soluble sterilized glass.

7. The method for preparing silver ion doped soluble germicidal glass according to claim 6.

11. The step of preheating the metal mold includes preheating the metal mold to a temperature range of 200° C. to 300° C.

11. A method for preparing silver ion doped soluble germicidal glass according to claim 10.

Citation Information

Patent Citations

  • Water-treating agent made from glass

    JP1989317133A

  • Antibacterial glass composition

    JP1996048539A

  • Antibacterial phosphate glass with adjusted refractive index

    JP2005255517A

  • Antibacterial glass and method of manufacturing the same

    JP2013155114A

  • Antibacterial glass and method for production thereof

    WO2002028792A1