Monomer composition, molded body, dental material composition, dental material, and method for producing (meth)acrylate (A)
A (meth)acrylate compound with thiol and (meth)acryloyloxy groups, combined with a thiol compound, addresses the mechanical property deficiencies in dental materials by enhancing the bending strength of cured products.
Patent Information
- Application Number
- JP2020024508
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-17
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-02-17
AI Technical Summary
Existing dental materials lack sufficient mechanical properties, necessitating the development of (meth)acrylates that can enhance the mechanical strength of cured products when used alone or in combination with other polymerizable compounds.
A (meth)acrylate compound with two or more thiol groups and (meth)acryloyloxy groups, combined with a thiol compound, forming a reactant with a structure represented by specific formulas, which includes a urethane bond and has a bending strength of 80 MPa or more, is used to improve mechanical properties.
The proposed (meth)acrylate composition results in cured products with enhanced mechanical properties, such as improved bending strength, when incorporated into dental materials.
Smart Images

Figure 0007582781000022 
Figure 0007582781000023 
Figure 0007582781000024
Abstract
Description
[Technical field]
[0001] This disclosure , Mo Nomer composition, molded body, dental material composition, dental material and a method for producing the (meth)acrylate (A) Regarding. [Background technology]
[0002] Composite resins, which are a representative example of dental material compositions, typically contain a monomer composition containing a monomer, a filler, a polymerization initiator, a polymerization inhibitor, a pigment, and the like. In recent years, composite resins with higher mechanical properties have been demanded, and the properties of the cured product of the monomer composition contained in the composite resin have a significant effect on the properties of the cured product of the composite resin containing the monomer composition. For this reason, various studies have been conducted on the monomers contained in the monomer composition, and for example, polyfunctional (meth)acrylates such as those shown in Patent Documents 1 to 4 are known as monomers. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2000-204069 A [Patent Document 2] Special Publication No. 2013-544823 [Patent Document 3] Japanese Patent Application Publication No. 11-315059 [Patent Document 4] International Publication No. 2012 / 157566 Summary of the Invention [Problem to be solved by the invention]
[0004] As described above, in order to expand the range of application of dental compositions containing monomers, such as composite resins, it is necessary to improve the mechanical properties of the cured product. Therefore, there is a demand for (meth)acrylates that can give cured products with excellent mechanical properties when used alone or in combination with other polymerizable compounds.
[0005] An object of the present disclosure is to provide a (meth)acrylate, a monomer composition, and a dental material composition capable of producing a cured product having excellent mechanical properties, as well as a molded body and a dental material having excellent mechanical properties. [Means for solving the problem]
[0006] Means for solving the above problems include the following aspects. <1> A (meth)acrylate which is a reaction product of a thiol compound (1) having two or more thiol groups and a (meth)acrylate compound (2) having two or more (meth)acryloyloxy groups, the flexural strength of which when cured alone is 80 MPa or more. <2> Contains a (meth)acryloyloxy group, a urethane bond, and a structure represented by the following formula (B): <1> The (meth)acrylate according to claim 1. [ka] In formula (B), R 2 is a hydrogen atom or a methyl group, and * indicates the bonding position. <3> Represented by the following formula (3): <1> or <2> The (meth)acrylate according to claim 1. [ka] In formula (3), X is a structure represented by formula (3-1) or a structure represented by formula (3-2). n is an integer of 2 to 4. 2 , R 3 and R 4may be the same or different. In formula (3-1) and formula (3-2), * represents a bonding position. In formula (3), when X is a structure represented by formula (3-1), R 1 is a residue obtained by removing n thiol groups from a thiol compound (1) having n or more thiol groups, and R 2 is a hydrogen atom or a methyl group, R 3 is a residue obtained by removing one (meth)acryloyloxy group and one hydroxyl group from an alcohol having a (meth)acryloyloxy group. In formula (3-1), R 4 is the residue obtained by removing two isocyanate groups from a diisocyanate. In formula (3), when X is a structure represented by formula (3-2), R 1 is a residue obtained by removing n thiol groups from a thiol compound (1) having n or more thiol groups, and R 2 is a hydrogen atom or a methyl group, R 3 is a residue obtained by removing one (meth)acryloyloxy group and one isocyanate group from an isocyanate having a (meth)acryloyloxy group. In formula (3-2), R 4 is the residue obtained by removing two hydroxyl groups from a diol. <4> R 1 The molecular weight is 100 to 500. <3> The (meth)acrylate according to claim 1. <5> R 1 is a group represented by the following formula (4), (5), (6), (7), (8-1), (8-2), (8-3), (9), (10), (11) or (12): <3> or <4> The (meth)acrylate according to claim 1. [ka] [ka] [ka] In the formulas (4) to (12), * represents a bonding position. In formula (10), R 5 is a divalent hydrocarbon group having 1 to 10 carbon atoms. In formula (11), R 6 , R 7 and R 8 are each independently a divalent hydrocarbon group having 1 to 10 carbon atoms. In formula (12), R 9 , R 10 and R 11 each independently represents a divalent hydrocarbon group having 1 to 10 carbon atoms; Y 1 and Y 2 are each independently an oxygen atom or a sulfur atom. <6> R 4 contains at least one selected from a linear or branched divalent acyclic hydrocarbon group having 4 to 20 carbon atoms and a divalent cyclic hydrocarbon group having 4 to 20 carbon atoms. <3> ~ <5> 13. The (meth)acrylate according to any one of the above items. <7> R 3 is an alkylene group having 1 to 6 carbon atoms <3> ~ <6> 13. The (meth)acrylate according to any one of the above items. <8> The thiol compound (1) has 6 to 20 carbon atoms. <1> ~ <7> 13. The (meth)acrylate according to any one of the above items. <9> The thiol compound (1) has at least one bond selected from a sulfide bond, an ether bond, and an ester bond. <1> ~ <8> 13. The (meth)acrylate according to any one of the above items. <10> Viscosity at 65℃ is 1mPa·s to 10,000mPa·s <1> ~ <9> 13. The (meth)acrylate according to any one of the above items. <11> <1> ~ <10> A monomer composition comprising the (meth)acrylate according to any one of the above items. <12> For dental materials <11> The monomer composition according to claim 1. <13> <11> or <12> 2. A molded article obtained by curing the monomer composition according to claim 1. <14> <11> or <12> 2. A dental composition comprising the monomer composition according to claim 1, a polymerization initiator, and a filler. <15> <14> A dental material obtained by hardening the dental material composition described in claim 1. Effect of the Invention
[0007] According to one embodiment of the present disclosure, it is possible to provide a (meth)acrylate, a monomer composition, and a dental material composition capable of producing a cured product having excellent mechanical properties, as well as a molded body and a dental material having excellent mechanical properties. [Brief description of the drawings]
[0008] [Figure 1] 1 is an IR spectrum of the (meth)acrylate (A-1) obtained in Example 1. [Diagram 2] 1 is an IR spectrum of the (meth)acrylate (A-2) obtained in Example 2. [Diagram 3] 1 is an IR spectrum of the (meth)acrylate (A-3) obtained in Example 3. [Figure 4] 1 is an IR spectrum of the (meth)acrylate (A-4) obtained in Example 4. [Diagram 5] 1 is an IR spectrum of the (meth)acrylate (A-5) obtained in Example 5. [Figure 6] 1 is an IR spectrum of the (meth)acrylate (A-6) obtained in Example 6. [Figure 7] 1 is an IR spectrum of the (meth)acrylate (A-7) obtained in Example 7. [Figure 8] 1 is an IR spectrum of the (meth)acrylate (A-8) obtained in Example 8. [Figure 9] 1 is an IR spectrum of the (meth)acrylate (A-9) obtained in Example 9. [Figure 10] 1 is an IR spectrum of the (meth)acrylate (A-10) obtained in Example 10. [Figure 11] 1 is an IR spectrum of the (meth)acrylate (A-11) obtained in Example 11. [Figure 12] 1 is an IR spectrum of the (meth)acrylate (A-12) obtained in Example 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The contents of the present disclosure will be described in detail below. The following description of the configuration elements may be based on representative embodiments of the present disclosure, but the present disclosure is not limited to such embodiments.
[0010] In the present disclosure, the use of "to" indicating a numerical range means that the numerical values before and after it are included as the lower limit and upper limit. In the present disclosure, in the ranges of numerical values described stepwise, the upper limit or lower limit of one numerical range may be replaced with the upper limit or lower limit of another numerical range of numerical values described stepwise. In addition, in the ranges of numerical values described in the present disclosure, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. In this disclosure, when referring to the amount of each component in a composition, if multiple substances corresponding to each component are present in the composition, it means the total amount of multiple substances present in the composition, unless otherwise specified. In this disclosure, "(meth)acryloyl" means acryloyl or methacryloyl, and "(meth)acrylate" means acrylate or methacrylate.
[0011] (Meth)acrylate The (meth)acrylate of the present disclosure is a reaction product of a thiol compound (1) having two or more thiol groups and a (meth)acrylate compound (2) having two or more (meth)acryloyloxy groups, the bending strength of which when cured alone is 80 MPa or more. By using this (meth)acrylate, a cured product having excellent mechanical properties can be produced. Hereinafter, the (meth)acrylate of the present disclosure will also be referred to as (meth)acrylate (A) of the present disclosure.
[0012] The (meth)acrylate (A) of the present disclosure is a reaction product of a thiol compound (1) having two or more thiol groups and a (meth)acrylate compound (2) having two or more (meth)acryloyloxy groups, the bending strength of which when cured alone is 80 MPa or more. When a cured product is produced using the (meth)acrylate (A) of the present disclosure, the mechanical properties of the resulting cured product can be improved.
[0013] The reactant contained in the monomer composition of the present disclosure may have a structure obtained by reacting a thiol group of the thiol compound (1) with a (meth)acryloyloxy group of the (meth)acrylate compound (2). The reactant may have no thiol group but may have a (meth)acryloyloxy group. The reactant may have a sulfide bond, or may have a sulfide bond and an ester bond. The thiol groups, sulfide bonds, and ester bonds in the reaction product can be confirmed, for example, by FT-IR (Fourier Transform Infrared) measurement.
[0014] The (meth)acrylate of the present disclosure preferably contains a (meth)acryloyloxy group, a urethane bond, and a structure represented by the following formula (B): By using this (meth)acrylate, a cured product having excellent mechanical properties can be produced.
[0015] [ka]
[0016] In formula (B), R 2represents a hydrogen atom or a methyl group. * represents a bonding position. For example, the bonding position may be a residue of the thiol compound (1) from which one or more thiol groups have been removed, a residue of the (meth)acrylate compound (2) from which one (meth)acryloyloxy group has been removed, or the like. The bonding position may be adjacent to the sulfur atom in formula (B) to which a residue of the thiol compound (1) from which one or more thiol groups have been removed, or the bonding position may be adjacent to the oxygen atom in formula (B) to which a residue of the (meth)acrylate compound (2) from which one (meth)acryloyloxy group has been removed may be bonded.
[0017] The reaction product may or may not have a thiol group. For example, in the reaction between the thiol group of the thiol compound (1) and the (meth)acryloyloxy group of the (meth)acrylate compound (2), all of the thiol groups of the thiol compound (1) may react, or some of the thiol groups may remain in the reaction product without reacting. The presence or absence of a thiol group can be confirmed, for example, by FT-IR measurement.
[0018] The reaction product may have a thiol group, and may further have a (meth)acryloyloxy group. For example, in the reaction between the thiol group of the thiol compound (1) and the (meth)acryloyloxy group of the (meth)acrylate compound (2), all of the thiol groups of the thiol compound (1) may react, and some of the (meth)acryloyloxy groups of the (meth)acrylate compound (2) may remain in the reaction product without reacting. The presence or absence of the (meth)acryloyloxy group can be confirmed, for example, by FT-IR measurement.
[0019] <Thiol compound (1)> The thiol compound (1) has two or more thiol groups. Examples of the thiol compound (1) include an aliphatic polythiol compound, an aromatic polythiol compound, and a heterocyclic polythiol compound. The thiol compound (1) preferably has 6 to 20 carbon atoms. The thiol compound (1) preferably has at least one bond selected from a sulfide bond, an ether bond, and an ester bond.
[0020] The thiol compound (1) is not particularly limited, and examples thereof include 1,3-propanedithiol, 1,4-butanedithiol, 1,6-hexanedithiol, 2,5-hexanedithiol, 1,8-octanedithiol, 1,9-nonanedithiol, 3,6-dioxa-1,8-octanedithiol, 3,7-dithia-1,9-nonanedithiol, 1,4-butanediol bis(thioglycolate), bis(3-mercaptopropionic acid)ethylene glycol, 1,4-bis(3-mercaptobutyryloxy)butane, 1,2,3-propanetrithiol, Tetrakis(mercaptomethyl)methane, trimethylolpropane tris(2-mercaptoacetate), trimethylolpropane tris(3-mercaptopropionate), trimethylolethane tris(2-mercaptoacetate), trimethylolethane tris(3-mercaptopropionate), pentaerythritol tetrakis(2-mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptopropionate), 1,2,3-tris(mercaptomethyl)methane 1,2,3-tris(2-mercaptoethylthio)propane, 1,2,3-tris(3-mercaptopropylthio)propane, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, tetrakis(mercaptomethylthio)propane, aliphatic polythiol compounds such as 1,1,3,3-tetrakis(mercaptomethylthio)propane, 1,1,2,2-tetrakis(mercaptomethylthio)ethane, tris(mercaptomethylthio)methane, and tris(mercaptoethylthio)methane; bis(2,3-dimercaptopropyl)sulfide, and esters of these thioglycolic acids or mercaptopropionic acids; aliphatic polythiol compounds such as 1,1,3,3-tetrakis(mercaptomethylthio)propane, 1,1,2,2-tetrakis(mercaptomethylthio)ethane, tris(mercaptomethylthio)methane, and tris(mercaptoethylthio)methane;Examples of the aromatic polythiol compounds include 1,3,5-trimercaptobenzene, 1,3,5-tris(mercaptomethyl)benzene, 1,3,5-tris(mercaptomethyleneoxy)benzene, and 1,3,5-tris(mercaptoethyleneoxy)benzene; and heterocyclic polythiol compounds such as 2,4,6-trimercapto-s-triazine, 2,4,6-trimercapto-1,3,5-triazine, and tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate.
[0021] As the thiol compound (1), from the viewpoint of producing a (meth)acrylate (A) capable of producing a cured product having excellent mechanical properties, 1,4-butanedithiol, 1,8-octanedithiol, 3,6-dioxa-1,8-octanedithiol, 3,7-dithia-1,9-nonanedithiol, 1,4-butanediol bis(thioglycolate), ethylene glycol bis(3-mercaptopropionate), 1,4-bis(3-mercaptobutyryloxy)butane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-di Preferred are mercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 1,1,3,3-tetrakis(mercaptomethylthio)propane, trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(2-mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, and the like.
[0022] <(Meth)acrylate compound (2)> The (meth)acrylate compound (2) alone has a flexural strength of at least 80 MPa when cured, and has two or more (meth)acryloyloxy groups.
[0023] (Bending strength) The (meth)acrylate compound (2) alone has a flexural strength of 80 MPa or more when cured. This can improve the bending strength of the cured product obtained by curing the (meth)acrylate (A) of the present disclosure. From the above viewpoint, the (meth)acrylate compound (2) preferably has a bending strength of 90 MPa or more, and more preferably 100 MPa or more. In the present disclosure, the flexural strength of a cured product is measured in accordance with ISO 4049, except that test pieces for measurement are obtained according to the following procedure. First, the compound or composition to be measured is placed in a stainless steel mold of 2 mm x 2 mm x 25 mm, and a visible light irradiation device is used to irradiate each side for 3 minutes, for a total of 6 minutes on both sides, to obtain a cured product. Next, the cured product is removed from the stainless steel mold and heat-treated at 130°C for 2 hours. After the heat treatment, the cured product is cooled to room temperature, immersed in distilled water, and held at 37°C for 24 hours. The cured product after the heat treatment is used as a test piece and a bending test is performed. The preparation of the test specimens and the measurement of the bending strength will be described in detail later in the Examples.
[0024] The upper limit of the bending strength of the (meth)acrylate compound (2) is not particularly limited, but may be, for example, 400 MPa or less, or 350 MPa or less.
[0025] In the present disclosure, the bending strength of a cured product of the (meth)acrylate compound (2) alone can be measured by carrying out a three-point bending test using a testing machine (for example, Autograph EZ-S manufactured by Shimadzu Corporation).
[0026] The (meth)acrylate compound (2) is not particularly limited, and examples thereof include tricyclodecane dimethanol di(meth)acrylate, 2,2-bis[4-(3-(meth)acryloyloxy-2-hydroxypropoxy)phenyl]propane, 2,2-bis(4-methacryloxypolyethoxyphenyl)propane, ethylene oxide-modified bisphenol A di(meth)acrylate, and propylene oxide-modified bisphenol A di(meth)acrylate.
[0027] Specifically, the following compounds may be used as the (meth)acrylate compound (2).
[0028] [ka]
[0029] From the viewpoint of handleability when mixed with a main component monomer to form a monomer composition, the (meth)acrylate (A) of the present disclosure may have a viscosity at 65°C of 1 mPa·s to 10,000 mPa·s, 10 mPa·s to 7,000 mPa·s, 50 mPa·s to 5,000 mPa·s, or 100 mPa·s to 3,000 mPa·s. The viscosity in the present disclosure is a value measured at 65°C using an E-type viscometer (TVE-22H manufactured by Toki Sangyo Co., Ltd.).
[0030] Furthermore, the viscosity at 65°C of a mixture of the (meth)acrylate (A) and an unreacted component which is at least one of the thiol compound (1) and the (meth)acrylate compound (2) used in the production of the (meth)acrylate (A) may be 1 mPa·s to 10,000 mPa·s, 10 mPa·s to 7,000 mPa·s, 50 mPa·s to 5,000 mPa·s, or 100 mPa·s to 3,000 mPa·s.
[0031] Furthermore, the reaction product may be one in which all of the thiol groups of the thiol compound (1) have reacted, and some of the (meth)acryloyloxy groups of the (meth)acrylate compound (2) remain unreacted, as described above.
[0032] The (meth)acrylate of the present disclosure is preferably represented by the following formula (3).
[0033] [ka]
[0034] In formula (3), X is a structure represented by formula (3-1) or a structure represented by formula (3-2). n is an integer of 2 to 4. 2 , R 3 and R 4 may be the same or different. In formula (3-1) and formula (3-2), * represents a bonding position. In formula (3), when X is a structure represented by formula (3-1), R 1 is a residue obtained by removing n thiol groups from a thiol compound (1) having n or more thiol groups, and R 2 is a hydrogen atom or a methyl group, R 3 is a residue obtained by removing one (meth)acryloyloxy group and one hydroxyl group from an alcohol having a (meth)acryloyloxy group. In formula (3-1), R 4 is the residue obtained by removing two isocyanate groups from a diisocyanate.
[0035] In formula (3), when X is a structure represented by formula (3-2), R 1 is a residue obtained by removing n thiol groups from a thiol compound (1) having n or more thiol groups, and R 2 is a hydrogen atom or a methyl group, R 3 is a residue obtained by removing one (meth)acryloyloxy group and one isocyanate group from an isocyanate having a (meth)acryloyloxy group. In formula (3-2), R 4is the residue obtained by removing two hydroxyl groups from a diol.
[0036] In the formula (3), the thiol compound (1) may be the above-mentioned thiol compound (1), and the alcohol having a (meth)acryloyloxy group may be the above-mentioned alcohol derived from the (meth)acrylate compound (2).
[0037] In formula (3), R 1 is preferably a residue obtained by removing all thiol groups from a difunctional to tetrafunctional thiol compound having 2 to 20 carbon atoms and at least one bond selected from a sulfide bond, an ester bond, an ether bond, and an alkylene group. The thiol compound is preferably a compound having 2 to 20 carbon atoms and having at least one bond selected from a sulfide bond, an ester bond, an ether bond, and an alkylene group, more preferably a compound having 2 to 20 carbon atoms and having one or more sulfide bonds, ester bonds, ether bonds, or alkylene groups, still more preferably a compound having 2 to 20 carbon atoms and having two or more sulfide bonds, ester bonds, or ether bonds, or a compound having an alkylene group and having no sulfide bonds, ester bonds, or ether bonds, and particularly preferably a compound having 2 to 20 carbon atoms and having two or three sulfide bonds, a compound having 2 to 20 carbon atoms and having three or four ester bonds, a compound having 2 to 20 carbon atoms and having two ether bonds, or a compound having an alkylene group having 2 to 20 carbon atoms and having no sulfide bonds, ester bonds, or ether bonds.
[0038] In formula (3), R 1 may be a residue obtained by removing all thiol groups from a trifunctional or tetrafunctional thiol compound, and n may be 3 or 4.
[0039] In formula (3), the R 1 The molecular weight of the copolymer is preferably 100 to 500.
[0040] R 1 is preferably a group represented by the following formula (4), (5), (6), (7), (8-1), (8-2), (8-3), (9), (10), (11) or (12).
[0041] [ka]
[0042] [ka]
[0043] [ka]
[0044] In formulas (4) to (12), * represents a bonding position. More specifically, it represents a bonding position with the sulfur atom shown in formula (3). In formula (10), R 5 In formula (11), R is a divalent hydrocarbon group having 1 to 10 carbon atoms. 6 , R 7 and R 8 are each independently a divalent hydrocarbon group having 1 to 10 carbon atoms. 9 , R 10 and R 11 each independently represents a divalent hydrocarbon group having 1 to 10 carbon atoms; Y 1 and Y 2 are each independently an oxygen atom or a sulfur atom. Examples of the divalent hydrocarbon group having 1 to 10 carbon atoms include the divalent noncyclic hydrocarbon groups and divalent cyclic hydrocarbon groups described below.
[0045] In formula (3), R 2 are each independently a hydrogen atom or a methyl group, and 2 is preferably a hydrogen atom or a methyl group.
[0046] In formula (3), X is a structure represented by formula (3-1) or a structure represented by formula (3-2). X is preferably a structure represented by formula (3-1). In the formula (3), when X is a structure represented by the formula (3-1), the (meth)acrylate of the present disclosure may be produced using an alcohol having a (meth)acryloyloxy group and a diisocyanate. R 3 When X is a structure represented by formula (3-1), R is a residue obtained by removing one (meth)acryloyloxy group and one hydroxyl group from an alcohol having a (meth)acryloyloxy group. 4 is the residue obtained by removing two isocyanate groups from a diisocyanate.
[0047] In the formula (3), when X is a structure represented by the formula (3-2), the compound may be produced using an isocyanate and diol having a (meth)acryloyloxy group according to the present disclosure. R 3 When X is a structure represented by formula (3-2), R is a residue obtained by removing one (meth)acryloyloxy group and one isocyanate group from an isocyanate having a (meth)acryloyloxy group. 4 is the residue obtained by removing two hydroxyl groups from a diol.
[0048] In formula (3), R 3 is not particularly limited, and examples thereof include a group obtained by removing two hydrogen atoms from an alkane, a group obtained by removing two hydrogen atoms from an arene, a group having one or more -C(=O)-, -SO2-, -NR- (R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, preferably a hydrogen atom) bonded to the above group, and a group consisting of a combination of the above groups. In the group obtained by removing two hydrogen atoms from an alkane, a portion of the hydrocarbon group may be substituted with -C(=O)-, -SO2-, -NR- (R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, preferably a hydrogen atom) or the like. R 3 Among these, a group in which two hydrogen atoms have been removed from an alkane is preferable.
[0049] The number of carbon atoms in the alkane is preferably 1 to 20, more preferably 1 to 10, and further preferably 1 to 6. The alkane may have a substituent or may be unsubstituted. The alkane may be linear, branched, or cyclic. The cyclic alkane may be monocyclic or polycyclic. Specific examples of the alkane include methane, ethane, propane, butane, 2-methylpropane, heptane, 2-methylbutane, and 2,2-dimethylpropane.
[0050] The number of carbon atoms in the arene is preferably 6 to 18, more preferably 6 to 14, and further preferably 6 to 10. Specific examples of the arene include benzene and condensed polycyclic aromatic compounds in which two or more aromatic rings are condensed.
[0051] R 3 is preferably an alkylene group having 1 to 6 carbon atoms.
[0052] In addition, in formula (3-1) and formula (3-2), R 4 is preferably a divalent linear or branched acyclic hydrocarbon group having 1 to 50 carbon atoms, a divalent cyclic hydrocarbon group having 3 to 50 carbon atoms, or a divalent organic group having 1 to 50 carbon atoms and containing an oxygen atom in the main chain.
[0053] The divalent cyclic hydrocarbon group having 3 to 50 carbon atoms may be composed only of a cyclic hydrocarbon portion, or may be a combination of a cyclic hydrocarbon portion and a non-cyclic hydrocarbon portion. Here, examples of the divalent non-cyclic hydrocarbon group include an alkylene group, an alkenylene group, and an alkynylene group, and examples of the divalent cyclic hydrocarbon group include a cycloalkylene group, a cycloalkenylene group, a cycloalkynylene group, and an arylene group.
[0054] In addition, the divalent organic group containing an oxygen atom in the main chain preferably does not have a structure in which oxygen atoms are consecutively present in the main chain, for example, "-OO-", and the structure other than the oxygen atom is preferably a hydrocarbon group. In addition, the hydrogen atoms in the non-cyclic hydrocarbon group and the hydrocarbon group may be substituted with a halogen atom such as a chlorine atom or a bromine atom, an alkoxy group, a nitro group, a hydroxy group, a carbonyl group, etc., and the hydrogen atoms in the cyclic ... a alkyl group, etc.
[0055] As the linear or branched divalent acyclic hydrocarbon group having 1 to 50 carbon atoms, a linear or branched divalent acyclic hydrocarbon group having 1 to 20 carbon atoms is preferred, a linear or branched divalent acyclic hydrocarbon group having 4 to 20 carbon atoms is more preferred, a linear or branched divalent acyclic hydrocarbon group having 4 to 10 carbon atoms is even more preferred, and a linear or branched divalent acyclic hydrocarbon group having 6 to 10 carbon atoms is particularly preferred.
[0056] As the divalent cyclic hydrocarbon group having 3 to 50 carbon atoms, a divalent cyclic hydrocarbon group having 3 to 30 carbon atoms is preferable, a divalent cyclic hydrocarbon group having 4 to 25 carbon atoms is more preferable, a divalent cyclic hydrocarbon group having 4 to 20 carbon atoms is even more preferable, and a divalent cyclic hydrocarbon group having 5 to 12 carbon atoms is particularly preferable.
[0057] R 4 It is preferable that the divalent hydrocarbon group contains at least one selected from a linear or branched divalent acyclic hydrocarbon group having 4 to 20 carbon atoms and a divalent cyclic hydrocarbon group having 4 to 20 carbon atoms.
[0058] The divalent organic group having 1 to 50 carbon atoms and containing an oxygen atom in the main chain is preferably an oxyalkylene group having 1 to 50 carbon atoms, more preferably an oxyalkylene group having 2 to 30 carbon atoms.
[0059] In formula (3-1) and formula (3-2), R 4may each independently be one substituent selected from the residue obtained by removing two (meth)acryloyloxy groups from the (meth)acrylate compound (2) exemplified above, and a plurality of R 4 is preferably one substituent selected from the residue obtained by removing two (meth)acryloyloxy groups from the (meth)acrylate compound (2) exemplified above.
[0060] (Method for producing (meth)acrylate (A)) The method for producing the (meth)acrylate (A) of the present disclosure will be described below. The method for producing the (meth)acrylate (A) of the present disclosure is obtained by reacting a thiol compound (1) with a (meth)acrylate compound (2). The thiol compound (1) and the (meth)acrylate compound (2) used in this production method include the compounds described above.
[0061] In order to efficiently produce the (meth)acrylate (A) when the thiol compound (1) is reacted with the (meth)acrylate compound (2), the ratio (b / a) of the mass b of the (meth)acrylate compound (2) to the mass a of the thiol compound (1) is preferably in the range of 0.5 to 35, more preferably in the range of 2 to 15, and even more preferably in the range of 3 to 10. In addition, the ratio of the number of moles of thiol groups in the thiol compound (1) to the number of moles of (meth)acryloyloxy groups in the (meth)acrylate compound (2) (number of moles of (meth)acryloyloxy groups / number of moles of thiol groups) is preferably 0.5 to 20, more preferably 1 to 15, and even more preferably 1.5 to 10, from the viewpoint of efficiently producing the (meth)acrylate (A).
[0062] When reacting the thiol compound (1) with the (meth)acrylate compound (2), a catalyst may be added to increase the reaction rate. As the catalyst, a known catalyst that accelerates the reaction between the thiol group contained in the thiol compound (1) and the (meth)acryloyloxy group contained in the (meth)acrylate compound (2), i.e., the enethiol reaction, can be used.
[0063] As the catalyst, a phosphine compound is preferably used. Examples of the phosphine compound include trialkylphosphine compounds such as trimethylphosphine, triethylphosphine, triisopropylphosphine, tri-n-propylphosphine, tri-tert-butylphosphine, triisobutylphosphine, tri-n-butylphosphine, tri-n-hexylphosphine, tri-n-octylphosphine, and tricyclohexylphosphine, methyldiphenylphosphine, dimethylphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, diethylphenylphosphine, dichloro(ethyl)phosphine, dichloro(phenyl)phosphine, and chlorodiphenylphosphine. These may be used alone or in combination of two or more. Among these catalysts, trialkylphosphine compounds are preferred because they suppress gelation and allow the reaction to proceed smoothly. The trialkylphosphine compound is preferably a trialkylphosphine compound such as tri-n-butylphosphine, tri-n-hexylphosphine, tricyclohexylphosphine, tri-n-octylphosphine, etc. The trialkylphosphine compound may be used alone or in combination of two or more.
[0064] The amount of the catalyst used is preferably 0.001% by mass to 0.5% by mass, more preferably 0.002% by mass to 0.3% by mass, still more preferably 0.01% by mass to 0.3% by mass, particularly preferably 0.01% by mass to 0.2% by mass, and even more preferably 0.05% by mass to 0.2% by mass, based on 100% by mass of the total of the thiol compound (1) and the (meth)acrylate compound (2), from the viewpoints of reaction regulation and catalytic effect. The catalyst may be added in its entirety at the start of the reaction, or may be added to the reaction system successively or in portions as necessary.
[0065] The reaction temperature is not particularly limited, and from the viewpoint of shortening the reaction time and suppressing the generation of by-products, it is preferably 0°C to 100°C, more preferably 20°C to 80°C, even more preferably 30°C to 60°C, and particularly preferably 35°C to 50°C. The reaction time is not particularly limited, and from the viewpoint of suppressing the generation of by-products, it is preferably 1 hour to 10 hours, more preferably 1.5 hours to 6 hours, and even more preferably 2 hours to 5 hours.
[0066] When reacting the thiol compound (1) with the (meth)acrylate compound (2), a polymerization inhibitor may be used to suppress a polymerization reaction between the (meth)acrylate compounds (2). The polymerization inhibitor is not particularly limited, and examples thereof include dibutylhydroxytoluene (BHT), hydroquinone (HQ), hydroquinone monomethyl ether (MEHQ), and phenothiazine (PTZ).
[0067] The amount of the polymerization inhibitor used may be 0.001% by mass to 0.5% by mass, 0.002% by mass to 0.3% by mass, 0.005% by mass to 0.3% by mass, 0.005% by mass to 0.1% by mass, or 0.01% by mass to 0.1% by mass, relative to 100% by mass in total of the thiol compound (1) and the (meth)acrylate compound (2).
[0068] <Monomer composition> The monomer composition of the present disclosure includes the (meth)acrylate (A) of the present disclosure. The monomer composition of the present disclosure may be for dental materials and may include a (meth)acrylate compound (B) other than the (meth)acrylate (A) of the present disclosure.
[0069] In general, when a main component monomer capable of improving the strength of the cured product is selected, the viscosity of the monomer composition increases, which may decrease the handleability.
[0070] In order to reduce the viscosity of the monomer composition and improve its ease of handling, a diluent monomer may be added to the main monomer. The diluent monomer may contain a (meth)acrylate compound (B) other than the (meth)acrylate (A) of the present disclosure.
[0071] Examples of the (meth)acrylate compound (B) include neopentyl di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,8-octanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, poly ... Examples of the methacrylates include triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 2,2-bis[4-(3-(meth)acryloyloxy-2-hydroxypropoxy)phenyl]propane, ethylene oxide-modified bisphenol A di(meth)acrylate, propylene oxide-modified bisphenol A di(meth)acrylate, and 2,2,4-trimethylhexamethylenebis(2-carbamoyloxyethyl)dimethacrylate (urethane dimethacrylate: UDMA). The (meth)acrylate compound (B) may be used alone or in combination of two or more. For example, a viscosity adjusting monomer such as triethylene glycol dimethacrylate may be used to adjust the viscosity of the monomer composition to a low level, and urethane dimethacrylate may be further used in combination to obtain high mechanical strength. When the viscosity adjusting monomer and urethane dimethacrylate are used in combination, the viscosity adjusting monomer and urethane dimethacrylate may be used in a mass ratio of 1:0.8 to 1.2.
[0072] In the monomer composition of the present disclosure, when the monomer composition contains a (meth)acrylate (B), from the viewpoint of improving the handleability of the monomer composition and suppressing a decrease in the functionality of the main component monomer, the content of the (meth)acrylate (B) is preferably 5% by mass or more and less than 50% by mass, more preferably 10% by mass to 40% by mass, and even more preferably 15% by mass to 30% by mass, relative to the total amount of the monomer composition.
[0073] In the monomer composition of the present disclosure, when the (meth)acrylate (B) is contained, the content of the (meth)acrylate (A) is preferably more than 50 mass% and not more than 95 mass%, more preferably 60 mass% to 90 mass%, and even more preferably 70 mass% to 85 mass%, based on the total amount of the monomer composition, from the viewpoint of improving the handleability of the monomer composition and suppressing a decrease in the functionality of the main component monomer.
[0074] The monomer composition of the present disclosure preferably contains an oxide of a phosphine-based compound. As the oxide of a phosphine compound, an oxide of a trialkylphosphine compound is preferable, tri-n-butylphosphine oxide, tri-n-hexylphosphine oxide, tricyclohexylphosphine oxide, tri-n-octylphosphine oxide is more preferable, and tri-n-butylphosphine oxide is even more preferable.
[0075] When the monomer composition of the present disclosure contains an oxide of a phosphine-based compound, the content of the oxide of the phosphine-based compound is preferably 0.001 mass% to 0.5 mass%, more preferably 0.002 mass% to 0.3 mass%, even more preferably 0.01 mass% to 0.3 mass%, particularly preferably 0.01 mass% to 0.2 mass%, and even more preferably 0.05 mass% to 0.2 mass%, relative to the mass of the entire monomer composition.
[0076] (Method of producing monomer composition) The method for producing a monomer composition of the present disclosure may include a step of obtaining a (meth)acrylate (A) by the method for producing a (meth)acrylate of the present disclosure, and a step of mixing the (meth)acrylate (A) with a (meth)acrylate (B) that is a (meth)acrylate other than the (meth)acrylate (A) to produce a monomer composition.
[0077] <Molded body> The molded article of the present disclosure is obtained by curing the monomer composition of the present disclosure. That is, the molded article of the present disclosure is a cured product of the dental material monomer composition of the present disclosure. For example, by curing a monomer composition containing (meth)acrylate (A) and (meth)acrylate (B) which is a compound represented by general formula (A), a cured product having excellent heat resistance, solvent resistance, and impact resistance can be obtained.
[0078] <Dental material composition> The dental material composition of the present disclosure contains the monomer composition of the present disclosure, a polymerization initiator, and a filler. This dental composition has room temperature polymerizability, heat polymerizability, or photopolymerizability, and can be preferably used, for example, as a dental restorative material.
[0079] The amount of the monomer composition to be mixed is preferably 20% by mass to 80% by mass, and more preferably 20% by mass to 50% by mass, relative to 100% by mass of the dental material composition.
[0080] As the polymerization initiator, a general polymerization initiator used in the dental field can be used, and is usually selected taking into consideration the polymerizability and polymerization conditions of the polymerizable compounds such as (meth)acrylate (A) and (meth)acrylate (B) contained in the dental material composition.
[0081] In the case of performing room temperature polymerization, the polymerization initiator is preferably, for example, a redox-based polymerization initiator in which an oxidizing agent and a reducing agent are combined. When using a redox-based polymerization initiator, the oxidizing agent and the reducing agent are packaged separately, and the two are mixed just before use.
[0082] The oxidizing agent is not particularly limited, and examples thereof include organic peroxides such as diacyl peroxides, peroxy esters, dialkyl peroxides, peroxy ketals, ketone peroxides, and hydroperoxides. Examples of the organic peroxides include diacyl peroxides such as benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, and m-toluoyl peroxide; peroxy esters such as t-butyl peroxybenzoate, bis-t-butylperoxyisophthalate, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, t-butylperoxy-2-ethylhexanoate, and t-butylperoxyisopropyl carbonate; dialkyl peroxides such as dicumyl peroxide, di-t-butyl peroxide, and lauroyl peroxide; peroxy ketals such as 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane; ketone peroxides such as methyl ethyl ketone peroxide; and hydroperoxides such as t-butyl hydroperoxide.
[0083] The reducing agent is not particularly limited, and a tertiary amine is usually used. Examples of the tertiary amine include N,N-dimethylaniline, N,N-dimethyl-p-toluidine, N,N-dimethyl-m-toluidine, N,N-diethyl-p-toluidine, N,N-dimethyl-3,5-dimethylaniline, N,N-dimethyl-3,4-dimethylaniline, N,N-dimethyl-4-ethylaniline, N,N-dimethyl-4-i-propylaniline, N,N-dimethyl-4-t-butylaniline, and N,N-dimethyl-3,5-di-t-butylaniline. n-aniline, N,N-bis(2-hydroxyethyl)-p-toluidine, N,N-bis(2-hydroxyethyl)-3,5-dimethylaniline, N,N-bis(2-hydroxyethyl)-3,4-dimethylaniline, N,N-bis(2-hydroxyethyl)-4-ethylaniline, N,N-bis(2-hydroxyethyl)-4-i-propylaniline, N,N-bis(2-hydroxyethyl)-4-t-butylaniline, N,N-di(2-hydroxyethyl) )-3,5-di-i-propylaniline, N,N-bis(2-hydroxyethyl)-3,5-di-t-butylaniline, ethyl 4-dimethylaminobenzoate, n-butoxyethyl 4-dimethylaminobenzoate, (2-methacryloyloxy)ethyl 4-dimethylaminobenzoate, trimethylamine, triethylamine, N-methyldiethanolamine, N-ethyldiethanolamine, Nn-butyldiethanolamine, N-lauryldiethanolamine, triethanolamine, (2-dimethylamino)ethyl methacrylate, N,N-bis(methacryloyloxyethyl)-N-methylamine, N,N-bis(methacryloyloxyethyl)-N-ethylamine, N,N-bis(2-hydroxyethyl)-N-methacryloyloxyethylamine, N,N-bis(methacryloyloxyethyl)-N-(2-hydroxyethyl)amine, tris(methacryloyloxyethyl)amine, and the like.
[0084] In addition to these organic peroxide / amine systems, cumene hydroperoxide / thiourea systems and ascorbic acid / Cu systems are also available. 2+Redox-based polymerization initiators such as salt-based and organic peroxide / amine / sulfinic acid (or its salt)-based polymerization initiators can be used. In addition, tributylborane, organic sulfinic acid, etc. can also be suitably used as the polymerization initiator.
[0085] When thermal polymerization is carried out by heating, a polymerization initiator such as a peroxide or an azo compound is preferred. The peroxide is not particularly limited, and examples thereof include benzoyl peroxide, t-butyl hydroperoxide, cumene hydroperoxide, etc. The azo compound is not particularly limited, and examples thereof include azobisisobutyronitrile, etc.
[0086] When photopolymerization is performed by irradiation with visible light, redox initiators such as α-diketone / tertiary amine, α-diketone / aldehyde, and α-diketone / mercaptan are preferred. The photopolymerization initiator is not particularly limited, and examples thereof include α-diketone / reducing agent, ketal / reducing agent, and thioxanthone / reducing agent. Examples of α-diketones include camphorquinone, benzil, and 2,3-pentanedione. Examples of ketals include benzil dimethyl ketal and benzil diethyl ketal. Examples of thioxanthones include 2-chlorothioxanthone and 2,4-diethylthioxanthone. Examples of reducing agents include tertiary amines such as Michler's ketone, 2-(dimethylamino)ethyl methacrylate, N,N-bis[(meth)acryloyloxyethyl]-N-methylamine, ethyl N,N-dimethylaminobenzoate, butyl 4-dimethylaminobenzoate, butoxyethyl 4-dimethylaminobenzoate, N-methyldiethanolamine, 4-dimethylaminobenzophenone, N,N-bis(2-hydroxyethyl)-p-toluidine, and dimethylaminophenanthol; aldehydes such as citronellal, lauryl aldehyde, phthaldialdehyde, dimethylaminobenzaldehyde, and terephthalaldehyde; and compounds having a thiol group such as 2-mercaptobenzoxazole, decanethiol, 3-mercaptopropyltrimethoxysilane, 4-mercaptoacetophenone, thiosalicylic acid, and thiobenzoic acid. A system in which an organic peroxide is added to these redox systems, such as an α-diketone / organic peroxide / reducing agent, can also be suitably used.
[0087] When photopolymerization is performed by irradiation with ultraviolet light, photopolymerization initiators such as benzoin alkyl ether, benzyl dimethyl ketal, etc. are preferred. Photopolymerization initiators such as (bis)acylphosphine oxides are also preferably used.
[0088] Among the (bis)acylphosphine oxides, examples of the acylphosphine oxides include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylmethoxyphenylphosphine oxide, 2,4,6-trimethylbenzoylethoxyphenylphosphine oxide, 2,3,5,6-tetramethylbenzoyldiphenylphosphine oxide, and benzoyldi-(2,6-dimethylphenyl)phosphonate. Examples of bisacylphosphine oxides include bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,4,6-trimethylbenzoyl)phenylphosphine oxide, (2,5,6-trimethylbenzoyl)-2,4,4-trimethylpentylphosphine oxide, and the like. These (bis)acylphosphine oxide photopolymerization initiators may be used alone or in combination with reducing agents such as various amines, aldehydes, mercaptans, sulfinates, etc. These (bis)acylphosphine oxide photopolymerization initiators may also be used in combination with the above-mentioned visible light photopolymerization initiators.
[0089] The polymerization initiator may be used alone or in combination of two or more kinds. The blending amount of the polymerization initiator is preferably 0.01% by mass to 20% by mass, and more preferably 0.1% by mass to 5% by mass, based on 100% by mass of the dental material composition.
[0090] The filler may be any filler commonly used in the dental field. Fillers are generally classified into organic fillers and inorganic fillers. Examples of the organic filler include fine powders of polymethyl methacrylate, polyethyl methacrylate, methyl methacrylate-ethyl methacrylate copolymer, crosslinked polymethyl methacrylate, crosslinked polyethyl methacrylate, ethylene-vinyl acetate copolymer, styrene-butadiene copolymer, and the like.
[0091] Examples of inorganic fillers include fine powders of various glasses (mainly composed of silicon dioxide and optionally containing oxides of heavy metals, boron, aluminum, etc.), various ceramics, diatomaceous earth, kaolin, clay minerals (montmorillonite, etc.), activated clay, synthetic zeolite, mica, calcium fluoride, ytterbium fluoride, calcium phosphate, barium sulfate, zirconium dioxide, titanium dioxide, and hydroxyapatite. Specific examples of such inorganic fillers include barium borosilicate glass (Kimble Raysorb T3000, Schott 8235, Schott GM27884, Schott GM39923, etc.), strontium boroaluminosilicate glass (Raysorb T4000, Schott G018-093, Schott GM32087, etc.), lanthanum glass (Schott GM31684, etc.), fluoroaluminosilicate glass (Schott G018-091, Schott G018-117, etc.), and boroaluminosilicate glass containing zirconium, cesium, etc. (Schott G018-307, G018-308, G018-310, etc.).
[0092] Alternatively, an organic-inorganic composite filler may be used which is obtained by adding a polymerizable compound to an inorganic filler in advance, forming the inorganic filler into a paste, polymerizing and curing the paste, and pulverizing the paste. In addition, in the dental material composition, a composition containing microfillers with a particle size of 0.1 μm or less is one of the preferred embodiments for dental composite resin. As the material of such a filler with a small particle size, silica (for example, Aerosil), alumina, zirconia, titania, etc. are preferable. The incorporation of such an inorganic filler with a small particle size is advantageous in obtaining polishing lubricity of the cured product of the composite resin.
[0093] These fillers may be surface-treated with a surface treatment agent such as a silane coupling agent depending on the purpose. As the surface treatment agent, a known silane coupling agent, for example, an organic silicon compound such as methacryloxyalkyltrimethoxysilane (the number of carbon atoms between the methacryloxy group and the silicon atom: 3 to 12), methacryloxyalkyltriethoxysilane (the number of carbon atoms between the methacryloxy group and the silicon atom: 3 to 12), vinyltrimethoxysilane, vinylethoxysilane, vinyltriacetoxysilane, etc. is used. The amount of the surface treatment agent is preferably 0.1% by mass to 20% by mass, more preferably 1% by mass to 10% by mass, based on 100% by mass of the filler before the surface treatment.
[0094] These fillers may be used alone or in combination of two or more. The amount of the filler may be appropriately determined in consideration of the operability (viscosity) of the dental material composition (e.g., composite resin paste) and the mechanical properties of the hardened product, and is preferably 10 to 2000 parts by mass, more preferably 50 to 1000 parts by mass, and even more preferably 100 to 600 parts by mass, relative to 100 parts by mass of all components other than the filler contained in the dental material composition.
[0095] The dental material composition of the present disclosure may contain components other than the monomer composition, polymerization initiator, and filler of the present disclosure, as appropriate, depending on the purpose. For example, it may contain the above-mentioned polymerization inhibitor to improve storage stability. It may also contain a colorant such as a known pigment or dye to adjust the color tone. Furthermore, it may contain a reinforcing material such as a known fiber to improve the strength of the cured product. In addition, the dental material composition of the present disclosure may contain additives such as a bactericide, disinfectant, stabilizer, and preservative as necessary, as long as the effects of the present invention are achieved.
[0096] The dental material composition of the present disclosure can be cured under appropriate conditions by the polymerization method of the polymerization initiator described above. For example, in the case of the dental material composition of the present disclosure containing a photopolymerization initiator by irradiation with visible light, the dental material composition can be processed into a predetermined shape, and then irradiated with visible light for a predetermined time using a known light irradiation device to obtain a desired cured product. The conditions such as irradiation intensity and irradiation strength can be appropriately changed according to the curing property of the dental material composition. In addition, the cured product cured by irradiation with light, including visible light, may be further heat-treated under appropriate conditions to improve the mechanical properties of the cured product.
[0097] The cured product of the dental composition of the present disclosure obtained as described above can be suitably used as a dental material. The method of using the dental material composition of the present disclosure is not particularly limited as long as it is a method generally known as a method of using dental materials. For example, when the dental material composition of the present disclosure is used as a composite resin for filling caries cavities, the dental material composition is filled into a cavity in the oral cavity, and then photocured using a known light irradiation device, thereby achieving the purpose. When used as a composite resin for crowns, the dental material composition is processed into an appropriate shape, then photocured using a known light irradiation device, and then heat-treated under a specified condition, thereby obtaining a desired crown material.
[0098] The dental composition and dental material of the present disclosure can be preferably used as, for example, a dental restorative material, a denture base resin, a denture base lining material, an impression material, a luting material (resin cement, resin-added glass ionomer cement, etc.), a dental adhesive (orthodontic adhesive, cavity application adhesive, etc.), a fissure sealant, a CAD / CAM resin block, a temporary crown, an artificial tooth material, etc. In addition, dental restorative materials can be classified according to the scope of application into composite resins for crowns, composite resins for filling caries cavities, composite resins for core construction, composite resins for filling and restoring, etc.
[0099] (Method of manufacturing dental composition) The method for producing a dental material composition of the present disclosure includes a step of obtaining a (meth)acrylate (A) by the method for producing a (meth)acrylate of the present disclosure, and a step of producing a dental material composition by mixing the (meth)acrylate (A), the (meth)acrylate (B), a polymerization initiator, and a filler. The obtained dental material composition has room temperature polymerizability, heat polymerizability, or photopolymerizability, and can be preferably used, for example, as a dental restorative material. The method for producing a dental material composition of the present disclosure may also include a step of obtaining a monomer composition by the method for producing a monomer composition of the present disclosure, and a step of producing a dental material composition by mixing the monomer composition, a polymerization initiator, and a filler.
[0100] <Dental materials> The dental material of the present disclosure is obtained by hardening the dental material composition of the present disclosure. That is, the dental material of the present disclosure is a hardened product of the dental composition of the present disclosure. The hardening conditions of the dental composition may be appropriately determined depending on the composition of the dental composition, the application of the dental material, and the like.
[0101] (Manufacturing method of dental materials) The method for producing a dental material of the present disclosure includes a step of obtaining a dental material composition by the method for producing a dental material composition of the present disclosure, and a step of hardening the dental material composition to produce a dental material. The hardening conditions may be appropriately determined depending on the composition of the dental material composition, the use of the dental material, etc. EXAMPLES
[0102] Hereinafter, one embodiment of the present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to the following examples as long as it does not deviate from the gist of the disclosure. In addition, unless otherwise specified, "parts" are based on mass.
[0103] The abbreviations for the compounds used in the examples of the present invention are shown below. HEA: 2-hydroxyethyl acrylate HEMA: 2-hydroxyethyl methacrylate TCDDM: Tricyclodecanedimethanol TMHDI: A mixture of 2,2,4-trimethylhexamethylene diisocyanate and 2,4,4-trimethylhexamethylene diisocyanate NBDI: A mixture of 2,5-bis(isocyanatomethyl)bicyclo[2.2.1]heptane and 2,6-bis(isocyanatomethyl)bicyclo[2.2.1]heptane AOI: 2-isocyanatoethyl acrylate DBTDL: Dibutyltin dilaurate BHT: Dibutyl hydroxytoluene DOOT: 3,6-dioxa-1,8-octanedithiol TMMP: Trimethylolpropane tris(3-mercaptopropionate) CQ: Camphorquinone DMAB2-BE: 2-butoxyethyl 4-(dimethylamino)benzoate
[0104] TBP: Tributylphosphine NPG: Neopentyl dimethacrylate 2,6E: 2,2-bis(4-methacryloxypolyethoxyphenyl)propane UDMA: Urethane dimethacrylate UDA1: Urethane diacrylate 1 UDA2: Urethane diacrylate 2 Bis-GMA: Bisphenol A dimethacrylate DCP: Tricyclodecane dimethanol dimethacrylate
[0105] [IR spectrum measurement method] The IR spectrum of the compound obtained in each example was measured using a Fourier transform infrared spectrometer, Spectrum Two / UATR (Universal Attenuated Total Reflectance), manufactured by PerkinElmer Japan Co., Ltd. The compound obtained in each Example was allowed to stand at 20°C for 24 hours, and then the infrared absorption spectrum of the compound was measured at 20°C.
[0106] [Bending test method] The bending test method in the examples and comparative examples of the present invention is shown below.
[0107] ~Preparation of bending test specimen α~ To 10 parts by mass of the (meth)acrylate compound (2,6E, UDMA, UDA1 or UDA2) as the raw material before the reaction, 0.05 parts by mass of CQ and 0.05 parts by mass of DMAB2-BE were added, and the mixture was stirred at room temperature until it became uniform, and then defoamed to prepare a raw material strength confirmation composition. The obtained raw material strength confirmation composition was placed in a stainless steel mold of 2 mm x 2 mm x 25 mm, and irradiated with light for 3 minutes on each side and 6 minutes on both sides in total using a visible light irradiation device (Solidify Light V, manufactured by Matsukaze Co., Ltd.) to form a cured product. The cured product removed from the stainless steel mold was then heat-treated in an oven at 130°C for 2 hours. The cured product removed from the oven was cooled to room temperature, and then immersed in distilled water in a sealable sample bottle and held at 37°C for 24 hours to be used as test piece α (bending test piece).
[0108] ~Preparation of test piece β for bending test~ To 10 parts by mass of the monomer composition obtained in each Example and Comparative Example, 0.05 parts by mass of CQ and 0.05 parts by mass of DMAB2-BE were added, and the mixture was stirred at room temperature until it was uniform. Further, 15 parts by mass of silica glass (Fuselex-X (manufactured by Tatsumori Co., Ltd.)) was added, and the mixture was stirred in a mortar until it was uniform, and then degassed to prepare a dental material composition. The obtained dental material composition was placed in a stainless steel mold of 2 mm x 2 mm x 25 mm, and irradiated with light for 3 minutes on each side and 6 minutes on both sides in total using a visible light irradiation device (Solidify Light V, manufactured by Matsukaze Co., Ltd.) to form a cured product. The cured product removed from the stainless steel mold was then heat-treated in an oven at 130°C for 2 hours. The cured product removed from the oven was cooled to room temperature, and then immersed in distilled water in a sealable sample bottle and held at 37°C for 24 hours to be used as a test piece β (test piece for bending test).
[0109] (Bending test) The test piece α or test piece β prepared by the above method was subjected to a three-point bending test using a testing machine (Autograph EZ-S manufactured by Shimadzu Corporation) with a support distance of 20 mm and a crosshead speed of 1 mm / min, to measure the breaking strength.
[0110] [Refractive index measurement method] In each of the Examples and Comparative Examples, the refractive index was measured using an Abbe type full digital refractometer (Abbemat550 manufactured by Anton Paar). The temperature was controlled at 25°C.
[0111] [Method of measuring viscosity] In each of the Examples and Comparative Examples, the viscosity of the (meth)acrylate was measured using an E-type viscometer (TVE-22H manufactured by Toki Sangyo Co., Ltd.) The temperature was controlled at 65° C. using a circulating thermostatic water bath.
[0112] [Production method of (meth)acrylate compounds (UDMA)] In a 200 mL four-neck flask equipped with a thoroughly dried stirring blade and a thermometer, 0.2 parts by mass of DBTDL, 0.1 parts by mass of BHT, and 44.68 parts by mass of TMHDI were charged and dissolved to form a homogeneous solution, and then the temperature of this solution was raised to 80°C, and 55.32 parts by mass of HEMA were added dropwise over 1 hour. During the dropwise addition, the internal temperature rose due to the heat of reaction, so the amount of addition was controlled so that it would be below 90°C. After the entire amount of HEMA was added dropwise, the reaction temperature was kept at 90°C and the reaction was carried out for 5 hours. At this time, the progress of the reaction was tracked by HPLC analysis to confirm the end point of the reaction. By discharging the product from the reactor, 100 g of urethane dimethacrylate (UDMA) represented by the following general formula was obtained as a (meth)acrylate compound. The obtained (meth)acrylate compound had a viscosity of 170 mPa·s at 65°C and a refractive index of 1.4836 at 25°C.
[0113] [ka]
[0114] [Production method of (meth)acrylate compounds (UDA1)] In a 200 mL four-neck flask equipped with a thoroughly dried stirring blade and a thermometer, 0.2 parts by mass of DBTDL, 0.1 parts by mass of BHT, and 41.02 parts by mass of TCDDM were charged and dissolved to form a homogeneous solution, and the temperature of this solution was raised to 80°C, and 58.98 parts by mass of AOI were added dropwise over 1 hour. During the dropwise addition, the internal temperature rose due to the heat of reaction, so the amount of dropwise addition was controlled so that the temperature was below 90°C. After the entire amount of AOI was added dropwise, the reaction temperature was kept at 90°C and the reaction was carried out for 8 hours. At this time, the progress of the reaction was tracked by HPLC analysis to confirm the end point of the reaction. By discharging the product from the reactor, 100 g of urethane diacrylate 1 (UDA1) represented by the following general formula was obtained as a (meth)acrylate compound. The obtained (meth)acrylate compound had a viscosity of 1640 mPa·s at 65°C and a refractive index of 1.5108 at 25°C.
[0115] [ka]
[0116] [Production method of (meth)acrylate compounds (UDA2)] In a 200 mL four-neck flask equipped with a thoroughly dried stirring blade and a thermometer, 0.2 parts by mass of DBTDL, 0.1 parts by mass of BHT, and 47.03 parts by mass of NBDI were charged and dissolved to form a homogeneous solution, and then the solution was heated to 80°C, and 52.67 parts by mass of HEA were added dropwise over 1 hour. During the dropwise addition, the internal temperature rose due to the heat of reaction, so the amount of dropwise addition was controlled so that the temperature was 90°C or less. After the entire amount of HEA was added dropwise, the reaction temperature was kept at 90°C and the reaction was carried out for 8 hours. At this time, the progress of the reaction was tracked by HPLC analysis to confirm the end point of the reaction. By discharging the product from the reactor, 100 g of urethane diacrylate 2 (UDA2) represented by the following general formula was obtained as a (meth)acrylate compound. The resulting (meth)acrylate compound had a viscosity of 910 mPa·s at 65°C and a refractive index of 1.5049 at 25°C.
[0117] [ka]
[0118] [Example 1] A raw material strength confirmation composition and test piece α (test piece for bending test) were obtained from the raw material compound UDMA before the reaction according to the methods described in the sections (Preparation of test piece α for bending test) and (Bending test). A bending test was carried out, and the breaking strength was 175 MPa.
[0119] In a 100 mL four-neck flask equipped with a thoroughly dried stirring blade and a thermometer, 0.04 parts by mass of TBP, 2.5 parts by mass of DOOT, which is a thiol compound, and 47.5 parts by mass of UDMA, which is a (meth)acrylate compound, were charged and dissolved to form a homogeneous solution, and then the temperature was raised to 50°C. After the temperature was raised, the reaction temperature was kept at 50°C and the reaction was carried out for 3 hours. At this time, the progress of the reaction was tracked by IR analysis to confirm the end point of the reaction. The product was discharged from the reactor to obtain 50 g of (meth)acrylate (A-1). The obtained (meth)acrylate (A-1) had a viscosity of 295 mPa·s at 65° C. and a refractive index of 1.4879 at 25° C. The IR spectrum of the (meth)acrylate (A-1) is shown in FIG. 10.5 parts by mass of the obtained (meth)acrylate (A-1) and 4.5 parts by mass of NPG were placed in a container and stirred at 50° C. until homogenized, to obtain a monomer composition. A dental material composition and a test piece β (test piece for bending test) were obtained from the obtained monomer composition according to the methods described in the sections (Preparation of test piece β for bending test) and (Bending test), and a bending test was performed, whereupon the breaking strength was 185 MPa.
[0120] [Examples 2 to 12] A raw material strength confirmation composition and test piece α (test piece for bending test) were obtained and a bending test was carried out in the same manner as in Example 1, except that the (meth)acrylate compound before the reaction was changed to the compound shown in Table 1. The measured breaking strengths are shown in Table 1.
[0121] 50 g of (meth)acrylates (A-2) to (A-12) were obtained in the same manner as in Example 1, except that the thiol compound and (meth)acrylate compound were changed to the compounds shown in Table 1. The viscosities at 65° C. and the refractive indices at 25° C. of the obtained (meth)acrylates (A-2) to (A-12) are as shown in Table 1. The IR spectra of the (meth)acrylates (A-2) to (A-12) are shown in FIG. 2 to FIG. 12, respectively. In addition, monomer compositions were obtained in the same manner as in Example 1, except that (meth)acrylate (A-1) was changed to (meth)acrylates (A-2) to (A-12), respectively. Then, dental compositions and test pieces β (test pieces for bending tests) were obtained from the obtained monomer compositions according to the methods described in the sections (Preparation of test pieces β for bending tests) and (Bending tests), and bending tests were performed. The measured breaking strengths are shown in Table 1.
[0122] [Comparative Example 1] 12.0 parts by mass of UDMA and 3.0 parts by mass of NPG were placed in a container and stirred at 50°C until homogenous, to obtain a monomer composition. A dental material composition and a test piece β (test piece for bending test) were obtained from the obtained monomer composition according to the methods described in the sections (Preparation of test piece β for bending test) and (Bending test), and a bending test was performed, whereupon the breaking strength was 139 MPa. Furthermore, UDMA had a viscosity of 170 mPa s at 65°C and a refractive index of 1.4836 at 25°C.
[0123] [Comparative Example 2] 12.0 parts by mass of UDA1 and 3.0 parts by mass of NPG were placed in a container and stirred at 50°C until homogenous, to obtain a monomer composition. A dental material composition and a test piece β (test piece for bending test) were obtained from the obtained monomer composition according to the methods described in the sections (Preparation of test piece β for bending test) and (Bending test), and a bending test was performed, whereupon the breaking strength was 182 MPa. Furthermore, UDA1 had a viscosity of 1640 mPa s at 65°C and a refractive index of 1.5109 at 25°C.
[0124] [Comparative Example 3] 12.0 parts by mass of UDA2 and 3.0 parts by mass of NPG were placed in a container and stirred at 50°C until homogenous, to obtain a monomer composition. A dental material composition (11) and a test piece β (test piece for bending test) were obtained from the obtained monomer composition according to the methods described in the sections (Preparation of test piece β for bending test) and (Bending test), and a bending test was performed, whereupon the breaking strength was 201 MPa. Furthermore, UDA2 had a viscosity of 907 mPa s at 65°C and a refractive index of 1.5049 at 25°C.
[0125] [Comparative Example 4] 12.0 parts by mass of 2,6E and 3.0 parts by mass of NPG were placed in a container and stirred at 50°C until homogenous, to obtain a monomer composition. A dental material composition and a test piece β (test piece for bending test) were obtained from the obtained monomer composition according to the methods described in the sections (Preparation of test piece β for bending test) and (Bending test), and a bending test was performed, whereupon the breaking strength was 140 MPa. In addition, 2,6E had a viscosity of 1000 mPa s at 65°C and a refractive index of 1.5400 at 25°C.
[0126] [Comparative Example 5] 12.0 parts by mass of Bis-GMA and 3.0 parts by mass of NPG were placed in a container and stirred at 50°C until homogenous, to obtain a monomer composition. A dental material composition and a test piece β (test piece for bending test) were obtained from the obtained monomer composition according to the methods described in the sections (Preparation of test piece β for bending test) and (Bending test), and a bending test was performed, whereupon the breaking strength was 138 MPa. In addition, the viscosity of Bis-GMA at 65°C was 1500 mPa s, and the refractive index at 25°C was 1.5524.
[0127] [Comparative Example 6] 12.0 parts by mass of DCP and 3.0 parts by mass of NPG were placed in a container and stirred at 50°C until homogenous, to obtain a monomer composition. A dental material composition and a test piece β (test piece for bending test) were obtained from the obtained monomer composition according to the methods described in the sections (Preparation of test piece β for bending test) and (Bending test), and a bending test was performed, whereupon the breaking strength was 124 MPa. DCP had a viscosity of 5 mPa s at 65°C and a refractive index of 1.5004 at 25°C.
[0128] [Table 1]
[0129] As shown in Table 1, the bending strength of the cured product of the thiol compound (1) having two or more thiol groups and the (meth)acrylate compound (2) having two or more (meth)acryloyloxy groups in the examples was 80 MPa or more, and the (meth)acrylate in the examples, which was a reaction product of the thiol compound (1) having two or more thiol groups, had excellent breaking strength. On the other hand, the (meth)acrylate according to the comparative example, which did not use the thiol compound (1) having two or more thiol groups, was inferior in breaking strength.
Claims
1. (Meth)acrylate and an oxide of a trialkylphosphine compound, The (meth)acrylate is Represented by the following formula (3), or A thiol compound (1) having two or more thiol groups; the bending strength of the cured product alone is 80 MPa or more, and the (meth)acrylate compound (2) has two or more (meth)acryloyloxy groups, and is a reaction product of the (meth)acrylate compound (2) which is selected from the group consisting of tricyclodecane dimethanol di(meth)acrylate, 2,2-bis[4-(3-(meth)acryloyloxy-2-hydroxypropoxy)phenyl]propane, 2,2-bis(4-methacryloxypolyethoxyphenyl)propane, ethylene oxide modified bisphenol A di(meth)acrylate, and propylene oxide modified bisphenol A di(meth)acrylate; Monomer composition. 【Chemistry 1】 In formula (3), X is a structure represented by formula (3-1) or a structure represented by formula (3-2). n is an integer of 2 to 4. 2 , R 3 and R 4 may be the same or different. In formula (3-1) and formula (3-2), * represents a bonding position. In formula (3), R 1 is a residue obtained by removing n thiol groups from a thiol compound (1) having n or more thiol groups, R 2 is a hydrogen atom or a methyl group, R 3 represents a group obtained by removing two hydrogen atoms from an alkane having 1 to 20 carbon atoms, a group obtained by removing two hydrogen atoms from an arene having 6 to 18 carbon atoms, and a group obtained by removing -C(=O)-, -SO 2 A group having one or more -, -NR- (R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms) bonded thereto, or a group consisting of a combination of the above groups. In formula (3-1) and formula (3-2), R 4 is a divalent non-cyclic hydrocarbon group having 1 to 50 carbon atoms which is linear or branched, a divalent cyclic hydrocarbon group having 3 to 50 carbon atoms, or a divalent hydrocarbon group having 1 to 50 carbon atoms which contains an oxygen atom in the main chain.
2. The monomer composition according to claim 1 , wherein the (meth)acrylate contains a (meth)acryloyloxy group, a urethane bond, and a structure represented by the following formula (B): 【Chemistry 2】 In formula (B), R 2 is a hydrogen atom or a methyl group, and * indicates the bonding position.
3. The R 1 3. The monomer composition according to claim 1 or 2, wherein the molecular weight of said monomer is from 100 to 500.
4. The R 1 is a group represented by the following formula (4), (5), (6), (7), (8-1), (8-2), (8-3), (9), (10), (11) or (12): 【Chemistry 3】 【Chemistry 4】 【Chemistry 5】 In formulas (4) to (12), * represents a bonding position. In formula (10), R 5 is a divalent hydrocarbon group having 1 to 10 carbon atoms. In formula (11), R 6 , R 7 and R 8 are each independently a divalent hydrocarbon group having 1 to 10 carbon atoms. In formula (12), R 9 , R 10 and R 11 each independently represents a divalent hydrocarbon group having 1 to 10 carbon atoms; Y 1 and Y 2 are each independently an oxygen atom or a sulfur atom.
5. The R 4 The monomer composition according to any one of claims 1 to 4, wherein the monomer group is selected from the group consisting of a linear or branched divalent acyclic hydrocarbon group having 4 to 20 carbon atoms and a divalent cyclic hydrocarbon group having 4 to 20 carbon atoms.
6. The R 3 The monomer composition according to any one of claims 1 to 5, wherein is an alkylene group having 1 to 6 carbon atoms.
7. The monomer composition according to any one of claims 1 to 6, wherein the thiol compound (1) has 6 to 20 carbon atoms.
8. The monomer composition according to any one of claims 1 to 7, wherein the thiol compound (1) has at least one bond selected from a sulfide bond, an ether bond, and an ester bond.
9. The monomer composition according to any one of claims 1 to 8, having a viscosity at 65°C of 1 mPa·s to 10,000 mPa·s.
10. The monomer composition according to any one of claims 1 to 9, which is used as a dental material.
11. A molded article obtained by curing the monomer composition according to any one of claims 1 to 10.
12. A dental composition comprising the monomer composition according to any one of claims 1 to 10, a polymerization initiator, and a filler.
13. A dental material obtained by hardening the dental composition according to claim 12.
14. Using a trialkylphosphine compound as a catalyst, A thiol compound (1) having two or more thiol groups; a (meth)acrylate compound (2) having two or more (meth)acryloyloxy groups and having a bending strength of 80 MPa or more when cured alone, The (meth)acrylate compound (2) is tricyclodecane dimethanol di(meth)acrylate, 2,2-bis[4-(3-(meth)acryloyloxy-2-hydroxypropoxy)phenyl]propane, 2,2-bis(4-methacryloxypolyethoxyphenyl)propane, ethylene oxide-modified bisphenol A di(meth)acrylate, or propylene oxide-modified bisphenol A di(meth)acrylate. A method for producing a (meth)acrylate (A) which is a reaction product of a thiol compound (1) having two or more thiol groups and a (meth)acrylate compound (2) having two or more (meth)acryloyloxy groups and having a bending strength of 80 MPa or more when cured alone.
15. Using a trialkylphosphine compound as a catalyst, A thiol compound (1) having two or more thiol groups; (2) a (meth)acrylate compound having two or more (meth)acryloyloxy groups and having a bending strength of 80 MPa or more when cured alone; A method for producing a (meth)acrylate (A) represented by the following formula (3), which is a reaction product of a thiol compound (1) having two or more thiol groups and a (meth)acrylate compound (2) having two or more (meth)acryloyloxy groups and having a bending strength of 80 MPa or more when cured alone: 【Chemistry 6】 In formula (3), X is a structure represented by formula (3-1) or a structure represented by formula (3-2). n is an integer of 2 to 4. A plurality of R 2 , R 3 , and R 4 may be the same or different. In formulas (3-1) and (3-2), * represents a bonding position. In formula (3), R 1 is a residue obtained by removing n thiol groups from a thiol compound (1) having n or more thiol groups, R 2 is a hydrogen atom or a methyl group; R 3 is a group obtained by removing two hydrogen atoms from an alkane having 1 to 20 carbon atoms, a group obtained by removing two hydrogen atoms from an arene having 6 to 18 carbon atoms, a group having one or more -C(═O)-, -SO 2 -, or -NR- (wherein R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms) bonded to any of these groups, or a group consisting of a combination of the aforementioned groups. In formula (3-1) and formula (3-2), R 4 is a divalent linear or branched acyclic hydrocarbon group having 1 to 50 carbon atoms, a divalent cyclic hydrocarbon group having 3 to 50 carbon atoms, or a divalent hydrocarbon group having 1 to 50 carbon atoms and containing an oxygen atom in the main chain.
Citation Information
Patent Citations
Urethane dimethacrylate derivative of 1,3-bis(1-isocyanato-1-methylethyl)Benzene
JP1999315059A
Polymerizably unsaturated bond-containing n-substituted amide compound
JP2000204069A
Multifunction thio(METH)acrylate resin, active energy ray curable hard coat resin composition comprising the same, cured film obtained by curing the same, plastic film having cured film laminated thereon, plastic injection molding using the plastic film, and processed product
JP2013213200A
High-strength dental materials
JP2013544823A
Dental curable composition
JP2014152107A