Cathode Material

A one-pot coprecipitation method using urea to form lithium manganese-rich layered oxide cathode materials addresses inefficiencies in existing production methods, resulting in high-capacity and stable cathode materials for lithium-ion batteries.

JP7582864B2Active Publication Date: 2024-11-13COUNCIL FOR SCI IND RES
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020540857
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-10-09
Filing Date
2018-09-27
Publication Date
2024-11-13
Estimated Expiration
2038-09-27

AI Technical Summary

Technical Problem

Current methods for producing lithium manganese-rich layered oxide cathode materials are time-consuming and inefficient, leading to capacity fade, poor rate capability, and high reactivity with electrolytes, making them unsuitable for commercial-scale production.

Method used

A one-pot coprecipitation method using Mn(II) salts and a precipitating agent like urea to form carbonates, followed by calcination and annealing, produces lithium manganese-rich layered oxide cathode materials with improved efficiency and performance.

Benefits of technology

The method results in cathode materials with high initial discharge capacity and stable capacity retention, suitable for high-capacity lithium-ion batteries, achieving capacities of up to 266mAh/g and 95% capacity retention after 30 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582864000001
    Figure 0007582864000001
  • Figure 0007582864000002
    Figure 0007582864000002
  • Figure 0007582864000003
    Figure 0007582864000003
Patent Text Reader

Abstract

A method for producing a lithium manganese-rich layered oxide cathode material or a lithium manganese-rich layered oxide cathode material precursor comprises co-precipitating, from an aqueous solution, a dissolved Li compound and a dissolved Mn salt selected from the group consisting of Mn(CH3COO)2, Mn(NO3)2, MnSO4, and mixtures thereof, in the presence of a precipitating agent that reacts with at least the dissolved Mn salt to form a carbonate salt, thereby providing a precursor comprising MnCO3 and a Li compound as the lithium manganese-rich layered oxide cathode material precursor. The invention extends to a lithium manganese-rich layered oxide cathode material or a lithium manganese-rich layered oxide cathode material precursor, an electrochemical cell, and methods of making and operating the electrochemical cell. [Selected Figure] Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to cathode materials, in particular to processes for producing lithium manganese rich layered oxide cathode materials or precursors to lithium manganese rich layered oxide cathode materials, the lithium manganese rich layered oxide cathode materials or precursors to lithium manganese rich layered oxide cathode materials when produced by said processes, electrochemical cells, methods of making electrochemical cells, and methods of operating electrochemical cells. [Background technology]

[0002] Layered lithium manganese-rich metal oxide composites are promising candidates as cathode materials to achieve higher capacity (>200 mAh / g), voltage stability, and good cycle life to provide the necessary power requirements for a wide range of applications, including electric vehicles and hybrid electric vehicles. The operating voltage window of these materials has been shown to be as high as 2.0 V to 4.8 V. Nevertheless, lithium manganese-rich layered oxide cathode materials, such as lithium manganese-rich layered transition metal oxide composites, have complex structures with inherent drawbacks including large initial irreversible charge capacity, capacity fade upon prolonged cycling, poor continuous charge and discharge rate capability, and high reactivity with electrolytes at high voltages.

[0003] The general chemical formula of lithium manganese rich metal oxides can be represented as xLi2MnO3(1-x)LiMO2, where M=Mn, Ni, Co and x is between 0 and 1. The synthesis methods that have been adopted as the most promising methods for the large-scale production of lithium manganese rich metal oxide materials via carbonate or hydroxide precursors comprise a combination of co-precipitation and solid-state routes, for example by Argonne National Laboratory, Lemont, Illinois, USA (see U.S. Patent 8,492,030). For example, Li 1.2 Mn 0.6 Ni 0.2 To produce O2, Ni 0.25 Mn 0.75 The CO3 precursor is first produced by co-precipitation from a slurry containing nickel and manganese carbonate using Na2CO3 as the precipitant. The slurry is aged for an extended period before filtering to provide a filter cake. The filter cake is then dried, and the dried powder is mixed with Li2CO3 and finally converted to Li by a solid state heating method. 1.2 Mn 0.6 Ni 0.2 This coprecipitation method produces the Li[Ni 1 / 3 Co 1 / 3 Mn 1 / 3 ]O2, lithium-rich layered cathode oxide and spinel-type oxide LiNi 0.5 Mn 1.5 O4, Li 1.05 M 0.05 Mn 1.9 A similar method is used by industry to generate precursors for the commercial production of O4. 0.75 Ni 0.25 via (OH) precursor Li[Li 0.2 Mn 0.6 Ni 0.2 ]O2 cathode materials. However, this method did not produce the final Li[Li 0.2 Mn0.6 Ni 0.2 ]O2. 0.75 Ni 0.25 (OH)2 hydroxide precursor intermediate is Li[Li 0.2 Mn 0.6 Ni 0.2 The material needs to be characterized by SEM and XRD to confirm formation before proceeding to the lithiation step to produce ]O2. Generally, commercially adopted methods for making lithium manganese rich cathode materials, such as those described above, have drawbacks including being time consuming (up to 72 hours) and involving multiple steps that may not be viable for full scale commercialization of these materials.

[0004] A process or method for producing a lithium manganese rich layered oxide cathode material or a lithium manganese rich layered oxide cathode material precursor that addresses at least some of the shortcomings of currently used methods would be advantageous. A fast synthesis method for producing a lithium manganese rich layered oxide cathode material that promises the same or better battery performance than current methods, particularly the lithium manganese rich layered oxide cathode material produced by Argonne National Laboratory, is desirable. Summary of the Invention

[0005] According to one aspect of the invention there is provided a method for producing a lithium manganese rich layered oxide cathode material or a precursor to a lithium manganese rich layered oxide cathode material, the method comprising: co-precipitating a dissolved Li compound and a dissolved Mn salt selected from the group consisting of Mn(CH3COO)2, Mn(NO3)2, MnSO4 and mixtures thereof, from an aqueous solution in the presence of a precipitating agent which reacts with at least the dissolved Mn salt to form a carbonate salt, thereby providing a precipitate comprising MnCO3 and a lithium compound as a lithium manganese rich layered oxide cathode material precursor.

[0006] The method comprises: calcining the precipitate to convert any carbonate materials to oxide materials, thereby providing a calcined material; and and annealing the calcined material to provide a lithium manganese-rich layered oxide cathode material.

[0007] The Mn salt is thus a Mn(II) salt.

[0008] The precipitating agent, which reacts with at least the dissolved Mn salts to form carbonate salts, may be selected from the group consisting of urea, (NH4)2CO3, NH4HCO3, and mixtures thereof.

[0009] Preferably, the precipitant which reacts with at least the dissolved Mn salts to form carbonate salts is urea.

[0010] Preferably, the aqueous solution also comprises a dissolved salt of at least one further metal M, said salt being selected from the group consisting of acetates, nitrates, sulfates, and mixtures thereof.

[0011] The metal M may be selected from the group consisting of Ni, Co, Fe, Al, Mg, Ti, and two or more thereof.

[0012] The dissolved Li compound can be a dissolved Li salt, the Li salt being selected from the group consisting of Li(CH3COO), LiNO3, LiCl, and mixtures thereof; In the presence of a precipitating agent which reacts with at least said Mn salt to form a carbonate, this results in the formation and co-precipitation of Li2CO3 and MnCO3, and carbonates of any metal M other than Li or Mn that may be present in the aqueous solution.

[0013] Alternatively, the dissolved Li compound can be LiOH.

[0014] The precipitate comprising MnCO3 and a lithium compound, such as a precursor of a lithium manganese rich layered oxide cathode material, can be, for example, MnCO3, Li 2 CO 3, and carbonates of other metals M, such as one or more of Ni, Co, Fe, and Al.

[0015] LiOH is less expensive than Li(CH3COO) and is believed to provide better yields than Li(CH3COO). In at least one embodiment of the method of the present invention, LiOH is therefore preferred over Li(CH3COO).

[0016] Coprecipitation can be effected at high precipitation temperatures of the aqueous solutions from about room temperature to about 100°C, preferably from about 60°C to about 80°C, for example about 70°C.

[0017] Typically, coprecipitation involves stirring an aqueous solution, resulting in the formation of a suspension.

[0018] The precipitate, such as a lithium manganese rich layered oxide cathode material precursor, may be calcined in air, during which any organic material, such as acetate, that may be present in the precipitate may be preferably consumed.

[0019] The precipitate may be pretreated at a temperature of about 200°C to about 700°C, for example about 600°C.

[0020] The precipitate may be calcined for a period of about 2 hours to about 10 hours, for example, about 3 hours.

[0021] Annealing of the calcined material may be accomplished at a temperature high enough to crystallize the material. Annealing may be accomplished for a period of time long enough to achieve the desired degree of annealing, i.e., to achieve the desired degree of crystallinity. Annealing may be accomplished in air.

[0022] The calcined material may be annealed at a temperature of about 600°C to about 1000°C, preferably about 800°C to about 1000°C, for example about 900°C.

[0023] The calcined material may be annealed for a period of from about 2 hours to about 24 hours, preferably 12 hours.

[0024] The aqueous solution typically has a pH greater than 7 during co-precipitation of the dissolved Li compounds and the dissolved Mn salts. Preferably, the pH is greater than 9, more preferably between 9.5 and 10.5, e.g., about 10. When the precipitating agent which reacts with at least the dissolved Mn salts to form carbonates is a base, the pH of the aqueous solution may be adjusted by the addition of an excess of precipitating agent, e.g., an excess of urea.

[0025] In one embodiment of the present invention, urea is used in a molar ratio of 1.2, 1.6, or 1.8 times the stoichiometric ratio.

[0026] Alternatively, a stoichiometric amount of the precipitating agent may be used.

[0027] When the dissolved Li compound is LiOH, the method comprises co-dissolving LiOH and a precipitating agent which reacts with at least the Mn salt to form a carbonate salt in water to form a first solution, and adding a second solution having dissolved Mn salt, and preferably at least one further dissolved salt of the metal M as described above, to the first solution to form the aqueous solution and effect co-precipitation.

[0028] Thus, the method includes co-dissolving dissolved LiOH and a precipitant that reacts with at least a Mn salt to form a carbonate salt in water to form a first solution; adding a second solution having a dissolved Mn salt and at least one additional dissolved salt to the first solution to form said aqueous solution and effecting co-precipitation; It may include, The further dissolved salt is selected from the group consisting of acetates, nitrates, sulfates, and mixtures thereof of a metal M selected from the group consisting of Ni, Co, Fe, Al, Mg, Ti, and two or more thereof.

[0029] The method may include separating the precipitate from the aqueous solution, for example by filtration, or by evaporation of the water. In at least one embodiment of the invention, evaporation of the water is preferred.

[0030] In one embodiment of the present invention, the lithium manganese rich layered oxide cathode material is Li 1.2 Mn 0.6 Ni 0.2 It is O2.

[0031] The invention extends to a lithium manganese rich layered oxide cathode material or a precursor to a lithium manganese rich layered oxide cathode material when produced by the process as described above.

[0032] According to a further aspect of the present invention there is provided an electrochemical cell comprising: The electrochemical cell comprises: Cell housing, and Containing a cathode, an anode, and an electrolyte in a cell housing; The cathode is electrically insulated from the anode but electronically coupled to the anode by the electrolyte, and the cathode comprises a lithium manganese rich layered oxide cathode material produced by the method as described above.

[0033] According to another aspect of the present invention, there is provided a method of making an electrochemical cell comprising loading into a cell housing an electrolyte, an anode, a separator and a cathode, the cathode comprising the lithium manganese rich layered oxide cathode material produced by the method as described above.

[0034] The electrochemical cell having a lithium manganese rich layered oxide cathode material has a capacity of at least about 200 mAhg at a current density of 20 mA / g. -1, or at least about 240 mAhg -1 , or at least about 260 mAhg -1 , for example, about 266mAhg -1 The battery may have an initial discharge capacity of 1000 .mu.m.

[0035] The electrochemical cell may exhibit greater than 95%, greater than 96%, or greater than 97% capacity retention at a current density of 20 mA / g after 30 cycles.

[0036] According to yet another aspect of the present invention there is provided a method of operating an electrochemical cell, the method comprising: applying a charging potential to such an electrochemical cell, whereby lithium from the cathode forms at least a portion of the anode; and enabling the discharge potential of the cell to reach 2.0-3.5 V vs. lithium metal with the average manganese valence state being about 3.5+ or greater during charging and discharging of the cell; Includes.

[0037] The charging potential of the cell may be capable of reaching 4.5 to 5.1 V versus lithium metal. The average manganese valence state during charging and discharging of the cell may be about 3.8+ or greater. [Brief description of the drawings]

[0038] The invention will now be described in more detail with reference to the following examples and the accompanying schematic drawings. [Figure 1] FIG. 1 shows the powder XRD patterns of Li1.2Mn0.6Ni0.2O2 cathode materials prepared according to the method of the present invention from four aqueous solutions each having a different pH. [Diagram 2] FIG. 2 shows the first charge / discharge voltage profiles of Li1.2Mn0.6Ni0.2O2 cathode materials made from four aqueous solutions, each having a different pH, according to the method of the present invention and charged from 2.0 V to 4.8 V at a rate of 0.1 C (current density of 20 mA / g). [Diagram 3] FIG. 3 shows a graph of the rate performance (or ratio performance or rate performance or rate performance) of Li1.2Mn0.6Ni0.2O2 cathode material prepared from four aqueous solutions each having a different pH according to the method of the present invention and discharged at 20 mA / g, 50 mA / g, and 100 mA / g for 10 cycles in the voltage range of 2.0 V to 4.8 V, and further cycling performance (or efficiency or cycling performance) at 50 mA / g for 50 cycles. [Figure 4] FIG. 4 shows a graph of the cycling efficiency over 50 cycles of Li1.2Mn0.6Ni0.2O2 cathode materials made from four aqueous solutions, each having a different pH, according to the method of the present invention, discharged at 50 mA / g. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS EXAMPLES

[0039] A facile one-pot co-precipitation synthesis method or process according to the present invention can be used to synthesize lithium manganese-rich metal oxide cathode material Li 1.2 Mn 0.6 Ni 0.2 The Li:Mn:Ni stoichiometry was used to generate the desired Li 1.2 Mn 0.6 Ni 0.2 The O2 layering material remains fixed, but the urea precipitant changes the required stoichiometry by 1.0 to 1.8 times, resulting in Li produced from aqueous solutions with different pH values. 1.2 Mn 0.6 Ni 0.2Four batches of O2 were obtained with pH 9.0 (1.0 x stoichiometric urea ratio), pH 9.5 (1.2 x stoichiometric urea ratio), pH 10.0 (1.6 x stoichiometric urea ratio), and pH 10.5 (1.8 x stoichiometric urea ratio), respectively. The synthesis procedure involved dissolving appropriate stoichiometric amounts of manganese acetate tetrahydrate [Mn(CH3COO)2·4H2O] and nickel acetate tetrahydrate [Ni(CH3COO)·4H2O] in distilled water in a first beaker. Lithium hydroxide [LiOH·H2O] and urea [CO(NH2)2] were dissolved in deionized water in a second beaker, separately from Mn(CH3COO)2·4H2O and Ni(CH3COO)2·4H2O, to form a base solution.

[0040] The solutions in both beakers were stirred at 1000 rpm and 70°C until complete dissolution (10 min dissolution). The acetate solution of the metal ions in the first beaker was then added dropwise to the base solution in the second beaker while stirring at 1000 rpm and 70°C. The aqueous solution in the second beaker gradually turned brown (or dark brown) as a suspension with suspended precipitate formed. The suspension was then left stirring at 70°C for a period of time after which the water was evaporated at 100°C. A fine brown / reddish powder was obtained which was calcined in a first heating step at about 600°C for 2 hours (temperature ramp rate 5°C / min) in an air flow furnace to burn off all the acetate / organics. The second heating step, the annealing step, was carried out at a higher temperature of about 900°C for about 12 hours to promote the formation of the final desired crystalline phase.

[0041] Physicochemical information was obtained using X-ray diffraction (XRD), scanning electron microscopy (SEM), Brunauer-Emmett-Teller (BET) technique, and Maccor battery tester (for electrochemical information). The physical properties of the four produced materials were not significantly different by XRD, SEM, and BET (see Figure 1 showing the XRD patterns of the four materials). The four produced lithium manganese-rich metal oxides were similar to those reported in the literature. As shown in Figure 1, the four Li 1.2 Mn 0.6 Ni 0.2 The XRD patterns of the O2 oxides are all similar and indexed to the layered structure reported in the literature. The materials are in all cases a mixture of cubic and monoclinic crystal structures. Rietveld refinement indicates that these compositions are 90.1%, 93.4%, 94.2% and 94.3% monoclinic for materials produced from aqueous solutions with pH 9, pH 10.5, pH 9.5 and pH 10.0, respectively, as shown in Figure 1.

[0042] However, the electrochemistry of these four materials differed significantly.

[0043] The four cathode materials were loaded into a coin cell, and the four cathode materials were charged to 200 mAhg at a constant current density of 20 mA / g over the voltage range of 2.0–4.8 V. -1 The results show that the 3D-based 3D-LCD displays excellent electrochemical performance, achieving (or delivering) more than 1000 .mu.m.

[0044] The cathode material obtained by coprecipitation from an aqueous solution with a pH of 10.0 had a current density of 266 mAhg at a current density of 20 mA / g, as shown in Figure 3. -1 It achieves high initial discharge capacity of 220mAhg at 50mA / g after 50 cycles. -1 The discharge capacity was maintained at more than 1000mV.

[0045] All four cathodes showed good stability at the starting high potentials of 4.8 V. These materials also showed high discharge capacity at potentials >4.5 V at 20 mA / g. During the first discharge cycle, all four cathodes suffered capacity loss as expected for Li2MnO3-based composites, similar to results reported by other groups studying these types of composites. Another group reported that the large capacity loss during the initial cycles was related to the complete loss of Li2O during activation of the Li2MnO3 component. All electrodes showed a sloping voltage profile below 4.4 V, followed by a relatively long plateau at about 4.5 V during the first charge step. The sloping voltage profile was consistent with the LiMn 0.5 Ni 0.5 Ni in O2 2+ Ni from ions 4+ The voltage profile plateau at 4.5 V is due to oxidation to Li ions. + This results from the simultaneous irreversible removal of ions and oxygen (LiO).

[0046] The process of the present invention produced materials with good performance. The results, as shown in FIG. 2, show that the cathode materials made from aqueous solutions with a pH of 10 each had a capacity of 373 mAhg -1 and 266mAhg -1 had the highest initial charge and discharge capacities.

[0047] Figure 3 shows the results of cells made with various cathode materials at 200mAhg -1 The results show that all of the above were achieved. The cells also exhibited good capacity retention characteristics with approximately 95% capacity retention at 20 mA / g after 30 cycles (see FIG. 4). It is clear from FIG. 3 that the capacity steadily decreases with increasing current density. The materials produced from aqueous solutions with pH 9.5 or pH 10.0 retained 200 mAhg even when charged at a current density of 100 mA / g.-1 Exceeds (>200mAhg -1 ) capacity, and the cathode material achieved stable capacity even at higher current densities.

[0048] All four homogeneous lithium manganese-rich metal oxide cathode materials exhibit stable cycling and good rate capabilities at high potentials, suggesting that they are promising candidates for use in high-capacity lithium-ion battery applications.

[0049] The method of the present invention, which can be described as a facile one-pot co-precipitation synthesis method, can be used to produce lithium manganese rich layered oxide cathode materials or precursors to lithium manganese rich layered oxide cathode materials. Advantageously, the method is fast and uses an inexpensive precipitant such as urea, which can be used in various ratios to produce cathode materials with different electrochemical properties. In at least one embodiment of the present invention, as exemplified, the need for filtration and washing is avoided, potentially saving water.

Claims

1. 1. A method for producing a lithium manganese rich layered oxide cathode material or a lithium manganese rich layered oxide cathode material precursor, the method comprising: Dissolved LiOH and Mn(CH 3 COO) 2 , Mn(NO 3 ) 2 , MnSO 4 and mixtures thereof from an aqueous solution in the presence of a precipitating agent that reacts with at least the dissolved Mn salt to form a carbonate salt, thereby obtaining MnCO as a lithium manganese rich layered oxide cathode material precursor. 3 and providing a precipitate comprising Li2CO3; The precipitating agent is urea, (NH 4 ) 2 CO 3 and mixtures thereof.

2. A method for producing a lithium manganese rich layered oxide cathode material, and calcining the precipitate to convert any carbonate materials to oxide materials, thereby providing a calcined material; and annealing the calcined material to provide a lithium manganese rich layered oxide cathode material. The method of claim 1 , comprising:

3. 3. The method according to claim 1 or 2, wherein the aqueous solution also comprises a dissolved salt of at least one further metal M, the salt being selected from the group consisting of acetates, nitrates, sulfates and mixtures thereof, and / or the metal M being selected from the group consisting of Ni, Co, Fe, Al, Mg, Ti and two or more thereof.

4. The method according to any of claims 1 to 3, wherein the aqueous solution has a pH greater than 9 during co-precipitation of the dissolved Li compounds and the dissolved Mn salts.

5. The method of claim 4, wherein the pH is 9.5 to 10.

5.

6. dissolving the LiOH and the precipitant, which reacts with at least the Mn salt to form a carbonate salt, together in water to form a first solution; and adding a second solution having a dissolved Mn salt and at least one additional dissolved salt to the first solution to form said aqueous solution and effecting co-precipitation; Including, 6. The method according to any of the preceding claims, wherein the further dissolved salt is selected from the group consisting of acetates, nitrates, sulfates and mixtures thereof of a metal M selected from the group consisting of Ni, Co, Fe, Al, Mg, Ti and two or more thereof.

7. The lithium manganese-rich layered oxide cathode material is Li 1.2 Mn 0.6 Ni 0.2 O 2 The method according to any one of claims 1 to 6, wherein

8. 1. An electrochemical cell comprising: A cell housing, and a cathode, an anode, and an electrolyte in the cell housing; Including, the cathode being electrically insulated from the anode but electrochemically bonded to the anode by the electrolyte, the cathode comprising a lithium manganese-rich layered oxide cathode material produced by carrying out the method of any one of claims 1 to 7; and The electrochemical cell exhibits greater than 95% capacity retention at a current density of 20 mA / g of catholyte after 30 cycles.

9. Producing a lithium manganese rich layered oxide cathode material according to the method of claim 2; loading an electrolyte, an anode, a separator, and a cathode into a cell housing; A method of making an electrochemical cell, wherein said cathode comprises said lithium manganese rich layered oxide cathode material.

10. The electrochemical cell having a lithium manganese rich layered oxide cathode material has a current density of at least 200 mAhg at a current density of 20 mA / g of cathode material. -1 9. The electrochemical cell of claim 8 having an initial discharge capacity of the cathode material of

11. The electrochemical cell having a lithium manganese rich layered oxide cathode material has a current density of at least 240 mAhg at a current density of 20 mA / g of cathode material. -1 9. The electrochemical cell of claim 8 having an initial discharge capacity of the cathode material of

12. The electrochemical cell having a lithium manganese rich layered oxide cathode material has a current density of at least 260 mAhg at a current density of 20 mA / g of cathode material. -1 9. The electrochemical cell of claim 8 having an initial discharge capacity of the cathode material of

13. 10. The electrochemical cell of claim 8, wherein the electrochemical cell exhibits greater than 96% capacity retention at a catholyte current density of 20 mA / g after 30 cycles.

14. 10. The electrochemical cell of claim 8, wherein the electrochemical cell exhibits greater than 97% capacity retention at a current density of 20 mA / g of catholyte after 30 cycles.

Citation Information

Patent Citations

  • Lithium secondary battery positive electrode active material and lithium secondary battery

    JP1999307094A

  • Fine particulate manganese carbonate and its production

    JP2000281348A

  • Precursor for lithium-ion secondary battery anode material, its manufacturing method, and manufacturing method of anode material using it

    JP2005285572A

  • Precursor for positive electrode material for lithium ion secondary battery, its manufacturing method, and manufacturing method of positive electrode material using it