Nickel-based lithium metal composite oxide, its manufacturing method, and lithium secondary battery including positive electrode containing the same

A nickel-based lithium metal composite oxide with controlled nickel content and particle sizes in secondary particles addresses the issues of overfiring and incomplete calcination, enhancing structural stability and battery performance.

JP7582911B2Active Publication Date: 2024-11-13SAMSUNG SDI CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2021106545
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-30
Filing Date
2021-06-28
Publication Date
2024-11-13
Estimated Expiration
2041-06-28

AI Technical Summary

Technical Problem

The existing methods for producing nickel-based lithium metal composite oxides with a mixture of large and small secondary particles face issues of overfiring or incomplete calcination, leading to performance deterioration and increased manufacturing complexity and cost due to multiple heat treatment steps.

Method used

A nickel-based lithium metal composite oxide is developed with secondary particles comprising aggregates of primary particles, where the nickel content is 50 mol% or more, and the large secondary particles have a particle size of 10 μm or more and small secondary particles 5 μm or less, with controlled nickel content differences between them, allowing simultaneous heat treatment to improve structural stability and reduce manufacturing complexity.

Benefits of technology

The solution results in a nickel-based lithium metal composite oxide with enhanced structural stability, leading to improved efficiency and lifespan of lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582911000016
    Figure 0007582911000016
  • Figure 0007582911000017
    Figure 0007582911000017
  • Figure 0007582911000018
    Figure 0007582911000018
Patent Text Reader

Abstract

To provide a nickel-based lithium metal composite oxide and a manufacturing method thereof, and a lithium secondary battery having a positive electrode that contains the nickel-based lithium metal composite oxide.SOLUTION: A nickel-based lithium metal composite oxide, a manufacturing method thereof, and a lithium secondary battery having a positive electrode containing the nickel-based lithium metal composite oxide are disclosed. The nickel-based lithium metal composite oxide comprises primary particles, and secondary particles including aggregates of the primary particles. In the nickel-based lithium metal composite oxide, a nickel content is 50 mol% or more to a transition metal total content. The secondary particles include large secondary particles of 10 μm or more in particle size, and small secondary particles of 5 μm or less in particle size. The large secondary particles are larger than the small secondary particles in nickel content.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nickel-based lithium metal composite oxide, a method for producing the same, and a lithium secondary battery including a positive electrode containing the same. [Background technology]

[0002] Due to the development of portable electronic devices and communication devices, there is an increasing need to develop high-energy density lithium secondary batteries.

[0003] When a lithium metal composite oxide is used as a positive electrode active material for a lithium secondary battery, if large secondary particles and small secondary particles are mixed, the collapse of the active material is suppressed even during pressing, and excellent performance can be exhibited, making it possible to manufacture a lithium secondary battery with a high energy density.

[0004] When manufacturing a lithium metal composite oxide containing a mixture of large and small secondary particles, the large and small secondary particles are simultaneously heat-treated. However, since the large and small secondary particles have different characteristics, if they are simultaneously heat-treated, the small or large secondary particles may be over-fired or incompletely fired, resulting in a decrease in performance. Therefore, the large and small secondary particles are separately heat-treated, and then the heat-treated mixture is heat-treated. However, since multiple heat treatment processes are performed, the manufacturing process of the positive electrode active material becomes complicated and the manufacturing cost increases, and an improvement is required. Summary of the Invention [Problem to be solved by the invention]

[0005] The problem to be solved by the present invention is to provide a nickel-based lithium metal composite oxide having improved structural stability.

[0006] Another problem to be solved by the present invention is to provide a method for producing the nickel-based lithium metal composite oxide, which can obtain the nickel-based lithium metal composite oxide at low production cost and through a simplified production process.

[0007] Another problem to be solved by the present invention is to provide a lithium secondary battery having a positive electrode containing the above-mentioned nickel-based lithium metal composite oxide and having improved efficiency and life span. [Means for solving the problem]

[0008] According to one aspect, there is provided a nickel-based lithium metal composite oxide comprising secondary particles including aggregates of primary particles, the nickel content being 50 mol % or more based on the total transition metal content in the nickel-based lithium metal composite oxide, the secondary particles comprising large secondary particles having a particle size of 10 μm or more and small secondary particles having a particle size of 5 μm or less, and the nickel content of the large secondary particles being higher than the nickel content of the small secondary particles.

[0009] The present invention provides a nickel-based lithium metal composite oxide having a positive electrode containing the nickel-based lithium metal composite oxide, in which the ratio (A2 / A1) of the discharge peak intensity (A2) to the charge peak intensity (A1) shown at a voltage of 4.1 V to 4.25 V at a current of 1 C in a dq / dv charge / discharge differential curve is 1.1 or more.

[0010] In another aspect, there is provided a method for producing a nickel-based lithium metal composite oxide, the method including the steps of mixing a large-particle nickel-based metal hydroxide having a nickel content of 50 mol % or more, based on the total transition metal content in the large-particle nickel-based metal hydroxide, a small-particle nickel-based metal hydroxide having a nickel content of 50 mol % or more, based on the total transition metal content in the small-particle nickel-based metal hydroxide, and a lithium precursor to obtain a precursor mixture, and then performing a heat treatment to obtain the nickel-based lithium metal composite oxide.

[0011] In yet another aspect, there is provided a lithium secondary battery including a positive electrode comprising the nickel-based lithium metal composite oxide described above. Effect of the Invention

[0012] The nickel-based lithium metal composite oxide according to an embodiment has excellent structural stability, and a lithium secondary battery having improved life and high rate characteristics can be manufactured by using a positive electrode including the nickel-based lithium metal composite oxide. [Brief description of the drawings]

[0013] [Figure 1] 1 is a graph showing dQ / dV charge / discharge differential curves after the first cycle in the lithium secondary batteries of Preparation Example 1 and Comparative Preparation Examples 1 and 2. [Diagram 2] 1 is a graph showing dQ / dV charge / discharge differential curves after 30 cycles in the lithium secondary batteries of Preparation Example 1 and Comparative Preparation Example 2. [Diagram 3] 1 is a graph showing dQ / dV charge / discharge differential curves after 50 cycles in the lithium secondary batteries of Preparation Example 1 and Comparative Preparation Example 2. [Figure 4] 1 is a graph showing dQ / dV charge / discharge differential curves for the lithium secondary battery of Preparation Example 1 at the first cycle, after 30 cycles, and after 50 cycles. [Diagram 5] 1 is a graph showing dQ / dV charge / discharge differential curves for the lithium secondary battery of Comparative Preparation Example 2 at the first cycle, after 30 cycles, and after 50 cycles. [Figure 6] 1 is an X-ray diffraction analysis graph relating to the composite positive electrode active material obtained in Example 1. [Figure 7] 1 is a schematic diagram illustrating a structure of a lithium secondary battery according to an embodiment. [Figure 8] 1 is a graph showing the life characteristics of the lithium secondary batteries of Production Examples 1 and 2 and the lithium secondary battery of Comparative Production Example 1. [Figure 9]1 is a graph showing charge / discharge characteristics of coin cells manufactured according to Manufacturing Example 1 and Comparative Manufacturing Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Exemplary nickel-based lithium metal composite oxides, methods for producing same, and lithium secondary batteries having positive electrodes containing same are described in further detail below with reference to the accompanying drawings.

[0015] The nickel-based lithium metal composite oxide includes secondary particles including aggregates of primary particles, and has a nickel content of 50 mol % or more based on the total transition metal content in the nickel-based lithium metal composite oxide, the secondary particles include large secondary particles having a particle size of 10 μm or more and small secondary particles having a particle size of 5 μm or less, and the nickel content of the large secondary particles is higher than the nickel content of the small secondary particles. The particle size indicates the average particle size when the particles are spherical, and indicates the length of the major axis when the particles are non-spherical. The particle size can be measured by a particle size analyzer, a scanning electron microscope, and / or a transmission electron microscope. The particle size indicates, for example, the average particle size (D50).

[0016] In this specification, unless otherwise defined, the average particle size (D50) means the average diameter of particles whose cumulative volume corresponds to 50% by volume in the particle size distribution, and means the value of the particle size corresponding to 50% from the smallest particle when the total number of particles is 100% in a distribution curve in which particle sizes are accumulated in order from the smallest particle to the largest particle. The average particle size (D50) can be measured by a method widely known to those skilled in the art, for example, by using a particle size analyzer (e.g., HORIBA, LA-950 Laser particle size analyzer) or from a TEM or SEM photograph. As another method, it can be measured using a measuring device using dynamic light-scattering, data analysis is performed to count the number of particles for each particle size range, and then the average particle size (D50) value can be easily obtained through calculation.

[0017] In the nickel-based lithium metal composite oxide, the nickel content is 60 mol % or more, 75 mol % or more, or 75 mol % to 99 mol %.

[0018] The nickel-based lithium metal composite oxide has a differential capacity dQ / dV charge / discharge differential curve for a lithium secondary battery having a positive electrode containing the nickel-based lithium metal composite oxide, and the ratio (A2 / A1) of the discharge peak intensity (A2) to the charge peak intensity (A1) shown at a current of 1 C and a voltage of 4.1 V to 4.25 V is 1.1 or more.

[0019] The dQ / dV charge / discharge differential curves were obtained in the voltage range of 3.0V to 4.3V, for example, 3.0V to 4.25V.

[0020] In the dQ / dV charge / discharge differential curve, V represents the voltage relative to the lithium metal negative electrode, and Q represents the charge / discharge capacity of the lithium secondary battery. In the dQ / dV charge / discharge differential curve, the X-axis represents the voltage V, and the Y-axis represents the value (dQ / dV) obtained by differentiating the charge / discharge capacity with respect to the voltage.

[0021] In order to manufacture a lithium secondary battery having excellent capacity characteristics using this nickel-based lithium metal composite oxide, it is common to manufacture the battery by heat treating a large-particle nickel-based lithium metal composite oxide precursor, a small-particle nickel-based lithium metal composite oxide precursor, and a lithium precursor.

[0022] The large-particle nickel-based lithium metal composite oxide precursor and the small-particle nickel-based lithium metal composite oxide precursor have different properties, and therefore, they are individually calcined, and then mixed with a lithium precursor and subjected to secondary calcination to obtain the desired nickel-based lithium metal composite oxide. Thus, three calcination steps are required to obtain the nickel-based lithium metal composite oxide, which results in high production costs and complicated production processes, and thus requires improvement.

[0023] To this end, the inventors have solved the above-mentioned problems and completed the present invention, which relates to a nickel-based lithium metal composite oxide having excellent structural stability and excellent capacity characteristics, which is produced by simultaneously heat-treating a large-particle nickel-based lithium metal composite oxide precursor, a small-particle nickel-based lithium metal composite oxide precursor, and a lithium precursor once while controlling the particle size and nickel content of the large-particle nickel-based lithium metal composite oxide precursor and a small-particle nickel-based lithium metal composite oxide precursor within a predetermined range.

[0024] The large-particle nickel-based lithium metal composite oxide precursor is, for example, a large-particle nickel-based metal hydroxide, and the small-particle nickel-based lithium metal composite oxide precursor is, for example, a small-particle nickel-based metal hydroxide.

[0025] In the large-particle nickel-based metal hydroxide and the small-particle nickel-based metal hydroxide, the nickel content is 50 mol % or more, 60 mol % or more, 75 mol % or more, or 75 mol % to 99 mol % based on the total transition metal content in the large-particle nickel-based metal hydroxide and the small-particle nickel-based metal hydroxide.

[0026] The nickel content difference between the large-particle nickel-based lithium metal composite oxide precursor and the small-particle nickel-based lithium metal precursor is 10 mol% or more, 11 mol% or more, 11 mol% to 24 mol%, for example, 11 to 20 mol%, 11 to 18 mol%, or 12 to 16 mol%. When the nickel content difference between the large-particle nickel-based lithium metal composite oxide precursor and the small-particle nickel-based lithium metal precursor is within the above-mentioned range, a nickel-based lithium metal composite oxide having excellent structural stability and energy density can be obtained.

[0027] The nickel content difference between the large-particle secondary particles and the small-particle secondary particles contained in the nickel-based lithium metal composite oxide obtained from the above-mentioned precursor is maintained the same as the nickel content difference between the large-particle nickel-based lithium metal composite oxide precursor and the small-particle nickel-based lithium metal precursor.

[0028] The nickel content difference between the large secondary particles and the small secondary particles contained in the nickel-based lithium metal composite oxide is 10 mol% or more, 11 mol% or more, for example, 11 to 20 mol%, 11 to 18 mol%, or 12 to 16 mol%. When the nickel content difference between the large secondary particles and the small secondary particles is within the above-mentioned range, the large nickel-based lithium metal precursor and the small nickel-based lithium metal precursor for obtaining them can be simultaneously heat-treated to obtain a nickel-based lithium metal composite oxide with excellent structural stability and energy density.

[0029] In the large secondary particles, the nickel content is 85 to 99 mol%, for example, 85 to 95 mol%, for example, 88 to 95 mol%, based on the total content of the transition metals, and in the small secondary particles, the nickel content is 75 to 89 mol%, for example, 80 to 85 mol%, for example, 75 to 85 mol%, based on the total content of the transition metals.

[0030] The particle size of the large-grain nickel-based lithium metal composite oxide precursor is 10 μm to 17 μm, for example, 12 to 15 μm. The particle size of the small-grain nickel-based lithium metal composite oxide precursor is 2 μm to 5 μm, for example, 3 to 4 μm. The particle size of the large-grain secondary particles contained in the nickel-based lithium metal (NCA) composite oxide obtained from such a precursor is 10 μm or more, 12 μm or more, 14 μm or more, 15 μm or more, for example, 12 to 17 μm.

[0031] The large secondary particles have a particle size of 10 to 15 μm, for example, 12 to 17 μm, and the small secondary particles have a particle size of 2 to 5 μm, for example, 3 to 4 μm, in one embodiment.

[0032] When the particle sizes of the large and small secondary particles are within the above-mentioned ranges, the large-particle nickel-based lithium metal composite oxide precursor and the small-particle nickel-based lithium metal composite oxide precursor for obtaining them can be simultaneously heat-treated to obtain a nickel-based lithium metal composite oxide having excellent structural stability and energy density. The content of the large-particle nickel-based lithium metal composite oxide precursor is 30 to 90 parts by weight, 50 to 90 parts by weight, 60 to 90 parts by weight, or 80 to 90 parts by weight, based on 100 parts by weight of the total content of the large-particle nickel-based lithium metal composite oxide precursor and the small-particle nickel-based lithium metal composite oxide precursor.

[0033] In the nickel-based lithium metal composite oxide of the present invention, the content of the large secondary particles is 30 to 90 parts by weight, 50 to 90 parts by weight, 60 to 90 parts by weight, or 80 to 90 parts by weight, based on 100 parts by weight of the total content of the large secondary particles and the small secondary particles.

[0034] When the mixing weight ratio of the large-grain secondary particles to the small-grain secondary particles is within the aforementioned range, the large-grain nickel-based lithium metal precursor and the small-grain nickel-based lithium metal precursor for obtaining them can be simultaneously heat-treated to obtain a nickel-based lithium metal composite oxide having excellent structural stability and excellent energy density.

[0035] In a lithium secondary battery having a positive electrode including the nickel-based lithium metal composite oxide according to an embodiment, the ratio (A2 / A1) of the discharge peak intensity (A2) to the charge peak intensity (A1) is 1.1 or more, for example, 1.1 to 1.5, in a dQ / dV charge / discharge differential curve at a current of 1C and a voltage of 4.3V to 3.0V. The charge peak and discharge peak are shown at a current of 1C and a voltage of 4.1V to 4.25V.

[0036] The charging and discharging conditions for the lithium secondary battery having the above-mentioned positive electrode are as follows.

[0037] The lithium secondary battery is charged at a constant current of 1 C until it reaches 4.3 V, and then charged at a constant voltage of 0.05 C. After the battery is fully charged, it is left to rest for about 10 minutes, and then it is discharged at a constant current of 1 C until the voltage reaches 3 V. This cycle is repeated several times and then evaluated.

[0038] The dQ / dV charge / discharge differential curves are for the first 100 charge / discharge cycles, the first 80 charge / discharge cycles, or the first 50 charge / discharge cycles. The charge / discharge cycles can be repeated a total of 50 times, for example.

[0039] The aforementioned charging peak is indicated, for example, between 4.17V and 4.25V, for example, at 4.19V, and the aforementioned discharging peak is indicated, for example, between 4.14V and 4.17V, for example, at 4.16V.

[0040] The dQ / dV charge / discharge differential curve indicates the capacity characteristics of the working ions of the positive active material at different voltages. The position, intensity difference, and area of ​​the main peak may vary depending on the type and physical properties of the positive active material.

[0041] dQ / dV is a graph showing the results of measuring the dq / dv distribution under a discharge condition of 1 C rate for a lithium battery including a positive electrode containing the nickel-based lithium metal composite oxide of the present invention and a lithium metal negative electrode. The nickel-based lithium metal composite oxide is, for example, lithium nickel oxide (NCA).

[0042] The dQ / dV distribution has three to six, e.g., five, main peaks, of which the peak at about 3.65 V corresponds to the main peak of NCA related to the phase transition from a hexagonal structure to a monoclinic structure, and the peaks in the voltage range of 4.1 V to 4.25 V indicate structural changes due to degradation of NCA.

[0043] The ratio (A2 / A1) of the discharge peak intensity (A2) to the dQ / dV charge peak intensity (A1) is 1.1 to 1.5. The amount of electrical energy stored in the lithium secondary battery can be known from the charge peak intensity, and the amount of structural change can be known from the discharge peak intensity. When the ratio (A2 / A1) of the discharge peak intensity (A2) to the dQ / dV charge peak intensity (A1) is within the above range, it is related to the Ni content difference and Co content difference between large and small particles. When it is within such a range, the NCA has low surface resistance, and by utilizing this, a lithium secondary battery with excellent high-temperature life characteristics and storage characteristics can be manufactured.

[0044] The above-mentioned dQ / dV charge / discharge differential curves relate to the first charge / discharge cycle to the 50th charge / discharge cycle of the lithium secondary battery, for example, the first charge / discharge cycle, the 30th charge / discharge cycle, or the 50th charge / discharge cycle. The evaluation conditions for the charge / discharge cycle are as described in Evaluation Example 1 below.

[0045] In the dQ / dV charge / discharge differential curve of the nickel-based lithium metal composite oxide according to an embodiment, the charge peak shown at a voltage of 3.5V to 3.8V has a gentle slope.

[0046] The nickel-based lithium metal composite oxide is also a compound represented by the following chemical formula 1:

[0047] [ka]

[0048] In the above formula 1, M is manganese (Mn), aluminum (Al), or a combination thereof; M' is boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr), or a combination thereof; 0.95≦a≦1.3, 0 <x<0.5、0<y<0.5、0≦z<0.5、0<x+y+z≦0.5である。

[0049] The sum of x+y+z is, for example, 0.01 to 0.2, 0.01 to 0.12, 0.04 to 0.1, or 0.04 to 0.08.

[0050] In the compound of Chemical Formula 1, the content of nickel is 50 mol % or more, which is higher than the content of each of the transition metals such as cobalt, M, and M'. By using a positive electrode containing such a nickel-based lithium metal composite oxide, it is possible to manufacture a lithium secondary battery having a high lithium diffusion rate, good conductivity, and a larger capacity at the same voltage.

[0051] In Chemical Formula 1, 0.95 ≦ a ≦ 1.3, 0 < x ≦ 0.3, 0 ≦ y ≦ 0.5, 0 ≦ z ≦ 0.05, and 0.5 ≦ 1 - x - y - z ≦ 0.95. In the aforementioned Chemical Formula 1, a is, for example, 1 to 1.1, x is 0.05 to 0.3, or 0.05 to 0.1, y is 0.05 to 0.3, z is 0, or z is 0.001 to 0.01.

[0052] According to one embodiment, in Chemical Formula 1, z is 0.

[0053] The compound of Chemical Formula 1 is, for example, Li 1.1 Ni 0.92 Co 0.05 Al 0.03 O 2、 LiNi 0.8 Co 0.1 MnAl 0.1 O2, LiNi 0.85 Co 0.1 Al 0.05 O2, Li 1.1 Ni 0.92 Co 0.05 Mn 0.03 O 2、 LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.85 Co 0.1 Mn 0.05 O2, Li 1.1 Ni 0.94 Co 0.03 Mn 0.03 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.94 Co 0.03 Al 0.03 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.96 Co 0.02 Al 0.02 O2, etc.

[0054] According to an embodiment, the large secondary particles are a compound of Formula 1, where 0.88≦1-xyz≦0.95, 0.01≦x≦0.08, 0.001≦y≦0.05, and 0≦z≦0.01. And the small secondary particles are a compound of Formula 1, where 0.75≦1-xyz≦0.85, 0.01≦x≦0.15, 0.001≦y≦0.05, and 0≦z≦0.01.

[0055] According to an embodiment, the large secondary particles are a compound represented by the following Formula 1-1, and the small secondary particles are a compound represented by the following Formula 1-2.

[0056] [ka]

[0057] In the above formula 1-1, M is boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr), or a combination thereof; 0.95≦a≦1.3, 0 <x<0.5、0<y<0.5、0≦z<0.5である。

[0058] In the chemical formula 1-1, 0.88≦1-xyz≦0.96, 0.01≦x≦0.08, 0.001≦y≦0.05, and 0≦z≦0.01;

[0059] [ka]

[0060] In the above formula 1-2, M is boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr), or a combination thereof; 0.95≦a≦1.3, 0 <x<0.5、0<y<0.5、0≦z<0.5である。

[0061] In chemical formula 1-2, 0.75≦1-xyz≦0.85, 0.01≦x≦0.05, 0.001≦y≦0.05, and 0≦z≦0.01.

[0062] The large secondary particles of formula 1-1 are, for example, Li 1.1 Ni 0.92 Co 0.05 Al 0.03 O 2、 LiNi 0.94 Co 0.03 Al 0.03 O2, LiNi 0.88 Co 0.08 Al 0.04 O2, LiNi 0.90 Co 0.05 Al 0.05 O2, LiNi 0.96 Co 0.02 Al 0.02 O2, LiNi 0.88 Co 0.06 Al 0.06 O2, etc., and the small secondary particles of chemical formula 1-2 are LiNi 0.8 Co 0.15 Al 0.05 O 2、 LiNi 0.75 Co 0.20 Al 0.05 O2, etc.

[0063] The specific surface area of ​​the large secondary particles is 0.1 to 1 m 2 / g, for example, 0.3 to 0.8 m 2 / g, and the specific surface area of ​​the small secondary particles is 2 to 15 m 2 / g, for example, 2 to 10 m 2 When the specific surface area of ​​the large secondary particles and the small secondary particles is within the above-mentioned range, a positive electrode and a lithium secondary battery excellent in capacity characteristics, life characteristics, and high-temperature storage characteristics can be produced. The specific surface area is the BET specific surface area measured by the Brunauer-Emmett-Teller method (BET method).

[0064] The compound of Chemical Formula 1 has a structure in which primary particles are aggregated to form spherical secondary particles, and the average particle size of the secondary particles is 1 to 25 μm, for example, 5 to 25 μm.

[0065] Hereinafter, a method for preparing a composite positive electrode active material according to an embodiment will be described.

[0066] A composite positive electrode active material can be obtained by mixing a nickel-based metal hydroxide, which is a large secondary particle, a nickel-based metal hydroxide, which is a small secondary particle, and a lithium precursor to obtain a precursor mixture, which is then heat-treated.

[0067] The nickel-based metal hydroxide is a precursor of a nickel-based lithium metal composite oxide.

[0068] The particle size of the nickel-based metal hydroxide which is the large secondary particles is 10 μm or more, for example, 12 to 17 μm, and the particle size of the nickel-based metal hydroxide which is the small secondary particles is 5 μm or less, for example, 2 to 5 μm.

[0069] The nickel-based metal hydroxide is also a compound represented by the following chemical formula 2.

[0070] [ka]

[0071] In the above formula 2, M is manganese (Mn), aluminum (Al), or a combination thereof; M' is boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr), or a combination thereof; and <x<0.5、0<y<0.5、0≦z<0.5、0<x+y+z≦0.5である。

[0072] In Chemical Formula 2, 0 < x ≤ 0.3, 0 ≤ y ≤ 0.5, and 0 ≤ z ≤ 0.05. In Chemical Formula 2, x + y + z is from 0.01 to 0.25, for example, from 0.04 to 0.25.

[0073] The nickel-based metal hydroxide is also a compound represented by the following Chemical Formula 2-1.

[0074]

Chemical Formula

[0075] In the aforementioned Chemical Formula 2-1, M is an element selected from the group consisting of boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), and zirconium (Zr), where 0 < x < 0.5, 0 < y < 0.5, 0 ≤ z < 0.5, and 0 < x + y + z ≤ 0.50.

[0076] In Chemical Formula 2-1, for example, 0 < x ≤ 0.3, 0 ≤ y ≤ 0.5, and 0 ≤ z ≤ 0.05. In Chemical Formula 2-1, x + y + z is from 0.01 to 0.25, for example, from 0.04 to 0.25.

[0077] The nickel-based metal hydroxide according to an embodiment is, for example, Ni 0.92 Co 0.05 Al 0.03 (OH)2, Ni 0.94 Co 0.03 Al 0.03 (OH)2, Ni 0.88 Co 0.06 Al 0.06 (OH)2, Ni 0.96 Co 0.02 Al 0.02 (OH)2, Ni 0.93 Co 0.04 Al 0.03 (OH)2, Ni 0.8 Co 0.15 Al 0.05 O2(OH) 2、 Ni 0.75 Co 0.20 Al0.05 (OH) 2、 Ni 0.92 Co 0.05 Mn 0.03 (OH)2, Ni 0.94 Co 0.03 Mn 0.03 (OH)2, Ni 0.88 Co 0.06 Mn 0.06 (OH)2, Ni 0.96 Co 0.02 Mn 0.02 (OH)2, Ni 0.93 Co 0.04 Mn 0.03 (OH)2, Ni 0.8 Co 0.15 Mn 0.05 O2(OH) 2、 Ni 0.75 Co 0.20 Mn 0.05 (OH)2, or a combination thereof.

[0078] In this specification, the compositions of the large-particle and small-particle nickel-based metal hydroxide are controlled to correspond to the compositions of the large-particle and small-particle nickel-based metal composite oxide.

[0079] The lithium precursor may be, for example, lithium hydroxide, lithium fluoride, lithium carbonate, Li2COOH, or a mixture thereof, and the content of the lithium precursor is controlled so that the molar ratio (Li / M) of the lithium in the lithium precursor to the transition metal in the nickel-based metal hydroxide is 0.95 or more, for example, more than 1.0, for example, 1.05 to 1.3, for example, 1.1 to 1.2.

[0080] The transition metal of the nickel-based metal hydroxide refers to a combination of Ni, Co, Mn, M and M' in Chemical Formula 2. The content of the lithium precursor and the nickel-based metal hydroxide is stoichiometrically adjusted so as to produce the nickel-based lithium metal composite oxide of Chemical Formula 1.

[0081] The above-mentioned mixing may be a dry mixing, and may be carried out using a mixer or the like.

[0082] The above-mentioned heat treatment is carried out in an oxidizing gas atmosphere.

[0083] The oxidizing gas atmosphere utilizes an oxidizing gas such as oxygen or air, for example, the oxidizing gas is composed of 10 to 20 volume % of oxygen or air and 80 to 90 volume % of an inert gas.

[0084] The heat treatment is suitably carried out at a temperature within a range not exceeding a densification temperature at which the reaction between the lithium precursor and the nickel-based metal hydroxide proceeds, where the densification temperature means a temperature at which crystallization is sufficiently performed and the active material can realize a charging capacity. The heat treatment is carried out at a temperature between 650°C and 800°C, 700°C and 750°C, for example, 700°C and 720°C.

[0085] The heat treatment time varies depending on the heat treatment temperature, etc.

[0086] The mixing weight ratio of the nickel-based metal hydroxide which is the large secondary particles and the nickel-based metal hydroxide which is the small secondary particles is 9:1 to 8:2.

[0087] The nickel-based metal hydroxide which is the large secondary particle and the nickel-based metal hydroxide which is the small secondary particle can be produced by a general method. For example, the nickel-based metal hydroxide which is the large secondary particle and the nickel-based metal hydroxide which is the small secondary particle differ only in the reaction time of the precursor (raw material) of the nickel-based metal hydroxide and the drying process of the product obtained after the reaction, and the remaining processes can be carried out in the same manner.

[0088] In the case of large nickel-based metal hydroxide, the reaction time to obtain nickel-based metal hydroxide is, for example, in the range of 90 to 130 hours, and drying is performed at 180 to 200°C, 185 to 200°C, 190 to 200°C, for example, 200°C. In the case of small nickel-based metal hydroxide, the reaction time of the precursor (raw material) of nickel-based metal hydroxide is shorter than that of large nickel-based metal hydroxide, for example, 20 to 30 hours, for example, 20 to 28 hours. The product after the reaction is dried at a temperature in the range of 200 to 220°C.

[0089] By using the method for preparing a nickel-based lithium metal composite oxide according to an embodiment, a positive electrode active material having high capacity, improved charge / discharge efficiency, and improved life span can be obtained.

[0090] Hereinafter, a method for manufacturing a lithium secondary battery having a positive electrode including a nickel-based lithium metal composite oxide according to an embodiment as a positive electrode active material, a negative electrode, a non-aqueous electrolyte containing a lithium salt, and a separator will be described.

[0091] The positive electrode and the negative electrode are prepared by coating a positive electrode active material layer forming composition and a negative electrode active material layer forming composition on a current collector, respectively, and drying the composition. The positive electrode active material forming composition is prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent, and the positive electrode active material according to an embodiment is used as the positive electrode active material.

[0092] The binder is a component that helps to bond the active material to the conductive agent and the like, and the active material to the current collector, and is added in an amount of 1 to 50 parts by weight based on 100 parts by weight of the total weight of the positive electrode active material. Non-limiting examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene butadiene rubber, fluororubber, and various copolymers. The content is 2 to 5 parts by weight based on 100 parts by weight of the total weight of the positive electrode active material. When the content of the binder is within the above range, the binding force of the active material layer to the current collector is good.

[0093] The conductive agent is not particularly limited as long as it has conductivity without inducing a chemical change in the battery, and examples of the conductive agent that can be used include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber and metal fiber; carbon fluoride; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0094] The content of the conductive agent is 2 to 5 parts by weight based on 100 parts by weight of the total weight of the positive electrode active material. When the content of the conductive agent is within the above range, the finally obtained electrode has excellent conductivity characteristics.

[0095] A non-limiting example of the solvent is N-methylpyrrolidone. The content of the solvent is 100 to 3,000 parts by weight based on 100 parts by weight of the positive electrode active material. When the content of the solvent is within the above range, the operation for forming the active material layer is easy.

[0096] The positive electrode current collector is not particularly limited as long as it has a thickness of 3 to 500 μm, does not induce chemical changes in the battery, and has high conductivity, and may be, for example, stainless steel, aluminum, nickel, titanium, heat-treated carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The current collector may have fine irregularities on its surface to increase the adhesive strength of the positive electrode active material, and may be in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.

[0097] Separately, a negative electrode active material, a binder, a conductive agent, and a solvent are mixed to prepare a composition for forming a negative electrode active material layer.

[0098] The negative electrode active material is a material capable of absorbing and releasing lithium ions. Non-limiting examples of the negative electrode active material include carbon-based materials such as graphite and carbon; lithium metal and its alloys; silicon oxide-based materials, etc. According to one embodiment of the present invention, silicon oxide is used.

[0099] The binder may be, but is not limited to, polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyacrylic acid, and polymers in which hydrogen is substituted with Li, Na, or Ca, or various copolymers. The binder may be added in an amount of 1 to 50 parts by weight based on 100 parts by weight of the total weight of the negative electrode active material. Non-limiting examples of such binders include the same type as that of the positive electrode.

[0100] The negative electrode active material layer forming composition may further include a conductive agent. The conductive agent is not particularly limited as long as it is conductive without inducing a chemical change in the battery, and may be, for example, graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; conductive fiber such as carbon fiber or metal fiber; conductive tube such as carbon nanotube; metal powder such as fluorocarbon, aluminum, or nickel powder; conductive whisker such as zinc oxide or potassium titanate; conductive metal oxide such as titanium oxide; or conductive material such as polyphenylene derivative. The conductive agent is preferably carbon black, and more specifically, carbon black having an average particle size of several tens of nm.

[0101] The conductive agent is present in an amount of 0.01 to 10 parts by weight, 0.01 to 5 parts by weight, or 0.1 to 2 parts by weight, based on 100 parts by weight of the total weight of the negative electrode active material layer.

[0102] The negative electrode active material layer forming composition may further include a thickener, which may be at least one of carboxymethyl cellulose (CMC), carboxyethyl cellulose, starch, regenerated cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, and polyvinyl alcohol.

[0103] The content of the solvent is 100 to 3,000 parts by weight based on 100 parts by weight of the total weight of the negative electrode active material. When the content of the solvent is within the above range, the process for forming the negative electrode active material layer is easy. The solvent may be the same as that used in the preparation of the positive electrode.

[0104] The negative electrode current collector is generally made to a thickness of 3 to 500 μm. Such a negative electrode current collector is not particularly limited as long as it is conductive without inducing a chemical change in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, heat-treated carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, like the positive electrode current collector, the surface can be formed with fine irregularities to strengthen the binding force of the negative electrode active material, and it can be used in various forms such as a film, sheet, foil, net, porous body, foam, and nonwoven fabric.

[0105] A separator is interposed between the positive electrode and the negative electrode prepared by the above process.

[0106] The above-mentioned separator has a pore size of 0.01 to 10 μm and a thickness of 5 to 300 μm. Specific examples include sheets or nonwoven fabrics made of olefin polymers such as polypropylene and polyethylene, or glass fibers. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte can also serve as the separator.

[0107] The lithium salt-containing non-aqueous electrolyte is composed of a non-aqueous electrolyte solution and a lithium salt. The non-aqueous electrolyte may be a non-aqueous electrolyte solution, an organic solid electrolyte, an inorganic solid electrolyte, or the like.

[0108] As the non-aqueous electrolyte, non-protonic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, N,N-formamide, N,N-dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ether, methyl propionate, and ethyl propionate may be used.

[0109] Examples of the organic solid electrolyte that can be used include, but are not limited to, polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate ester polymers, polyester sulfide, polyvinyl alcohol, and polyvinylidene fluoride.

[0110] In the above-mentioned inorganic solid electrolyte, non-limiting examples include Li nitrides, halides, and sulfates such as Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, and Li3PO4-Li2S-SiS2.

[0111] The lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte, and non-limiting examples thereof include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, (FSO2)2NLi, etc. may be used.

[0112] FIG. 7 is a cross-sectional view illustrating a typical structure of a lithium secondary battery according to an embodiment.

[0113] Referring to FIG. 7, the lithium secondary battery 21 includes a positive electrode 23, a negative electrode 22, and a separator 24. The positive electrode 23, the negative electrode 22, and the separator 24 are wound or folded and housed in a battery case 25. Next, an organic electrolyte is injected into the battery case 25 and sealed with a cap assembly 26 to complete the lithium secondary battery 20. The battery case 25 may be cylindrical, rectangular, thin-film, or the like. For example, the lithium secondary battery 20 may be a large-sized thin-film battery. The lithium secondary battery may be a lithium-ion battery. A separator may be disposed between the positive electrode and the negative electrode to form a battery structure. The battery structures are stacked in a bi-cell structure, and then impregnated with an organic electrolyte, and the resultant product is housed in a pouch and sealed to complete a lithium-ion polymer battery. In addition, a plurality of the battery structures are stacked to form a battery pack, and the battery pack may be used in all devices that require high capacity and high output. For example, they are also used in notebook computers, smartphones, electric vehicles (EVs), and the like.

[0114] In addition, the lithium secondary battery has excellent storage stability, life characteristics, and high rate characteristics at high temperatures, and can be used in electric vehicles, for example, hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs).

[0115] The present invention will be described in more detail through the following examples and comparative examples. However, the examples are given for illustrative purposes and are not intended to be limiting.

[0116] (Production of nickel-based metal hydroxides)

[0117] Production Example 1: Production of large nickel-based metal hydroxide particles The coprecipitation method described below was used to obtain large nickel-based metal hydroxide (Ni 0.94 Co 0.03 Al 0.03 (OH)2).

[0118] Ammonia water was added to the reactor, and the raw material of nickel-based metal hydroxide was added thereto while controlling the stoichiometry, and the pH of the mixture in the reactor was adjusted using sodium hydroxide. Next, the mixture was reacted with stirring until it reached the desired size, after which the introduction of the raw material solution was stopped and the product was obtained through a drying process. The specific manufacturing process is as follows.

[0119] As raw materials for nickel-based metal hydroxide, nickel sulfate (NiSO4·6H2O), cobalt sulfate (CoSO4·7H2O), and aluminum sulfate (Al2(SO4)3·H2O) were dissolved in distilled water as a solvent in a molar ratio of 94:3:3 to prepare a mixed solution. To form a complex compound, ammonia water (NH4OH) dilution solution and sodium hydroxide (NaOH) as a precipitant were prepared. Then, the metal raw material mixed solution, ammonia water, and sodium hydroxide were each put into the reactor. Sodium hydroxide was put in to maintain the pH inside the reactor. Next, the reaction was carried out for about 95 hours while stirring, and then the putting in of the raw material solution was stopped.

[0120] The slurry solution in the reactor was filtered, washed with high-purity distilled water, and then dried in a hot air oven at 200°C for 24 hours to obtain large-grain nickel-based metal hydroxide (Ni 0.94 Co 0.03 Al 0.03 (OH)2) powder was obtained.

[0121] Production Example 2: Production of small nickel-based metal hydroxide Small nickel-based metal hydroxide (Ni 0.8 Co 0.15 Al 0.05The same process as in Preparation Example 1 was carried out, except that the contents of nickel sulfate (NiSO4·6H2O), cobalt sulfate (CoSO4·7H2O) and aluminum sulfate (Al2(SO4)3·H2O) were stoichiometrically controlled to obtain small nickel-based metal hydroxide (Ni(OH)2) having a size of about 3 μm, the precursor was dried in a hot air oven at 210°C for 24 hours instead of in a hot air oven at 200°C for 24 hours, and the reaction time was changed to 25 hours. 0.8 Co 0.15 Al 0.05 (OH)2) powder was obtained.

[0122] Production Example 3: Production of large nickel-based metal hydroxide particles As large-grain nickel-based metal hydroxide, Ni 0.96 Co 0.02 Al 0.02 The same process as in Preparation Example 1 was carried out, except that the contents of nickel sulfate (NiSO4·6H2O), cobalt sulfate (CoSO4·7H2O), and aluminum sulfate (Al2(SO4)3·H2O) were stoichiometrically controlled to obtain large particles of nickel-based metal hydroxide (Ni(OH)2) having a size of about 12 μm. 0.96 Co 0.02 Al 0.02 (OH)2) powder was obtained.

[0123] Production Example 4: Production of large nickel-based metal hydroxide particles Large nickel-based metal hydroxide particles (Ni 0.94 Co 0.03 Al 0.03 Instead of (OH)2), large particles of nickel-based metal hydroxide (Ni 0.94 Co 0.03 Al 0.03 The same procedure as in Preparation Example 1 was followed, except that the reaction time was changed to about 90 hours while stirring after sodium hydroxide was added to maintain the pH inside the reactor so as to obtain 2-(2-methyl-2-propanediol (OH)2).

[0124] Production Example 5: Production of large nickel-based metal hydroxide particles Large nickel-based metal hydroxide particles (Ni 0.94 Co 0.03 Al 0.03 Instead of (OH)2), large nickel-based metal hydroxide (Ni 0.94 Co 0.03 Al 0.03 The same procedure as in Preparation Example 1 was followed, except that the reaction time was changed to about 130 hours while stirring after sodium hydroxide was added to maintain the pH inside the reactor so as to obtain 2-(2-methyl-2-propanediol (OH)2).

[0125] Production Example 6: Production of small nickel-based metal hydroxide Small nickel-based metal hydroxide (Ni 0.8 Co 0.15 Al 0.05 Instead of (OH)2), small nickel-based metal hydroxide (Ni 0.8 Co 0.15 Al 0.05 The same procedure as in Preparation Example 2 was followed, except that the reaction time was changed to about 22 hours while stirring was performed after sodium hydroxide was added to maintain the pH inside the reactor so as to obtain 2-(OH)2).

[0126] Production Example 7: Production of small nickel-based metal hydroxide Small nickel-based metal hydroxide (Ni 0.8 Co 0.15 Al 0.05 Instead of (OH)2), small nickel-based metal hydroxide (Ni 0.8 Co 0.15 Al 0.05 The same procedure as in Preparation Example 2 was followed, except that the reaction time was changed to about 28 hours while stirring was performed after sodium hydroxide was added to maintain the pH inside the reactor so as to obtain 2-(OH)2).

[0127] (Production of nickel-based lithium metal composite oxide)

[0128] Example 1 The large-particle nickel-based metal hydroxide having a size of 12 μm obtained in Production Example 1 and the small-particle nickel-based metal hydroxide having a size of 3 μm obtained in Production Example 2 were mixed in a mixing ratio by weight of 80:20.

[0129] The large-particle nickel-based metal hydroxide, the small-particle nickel-based metal hydroxide mixture, and lithium hydroxide (LiOH) were mixed in a dry ratio of 1:1.05 using a Henschel mixer, and heat-treated in an oxygen atmosphere at about 720°C for 10 hours to produce a nickel-based lithium metal composite oxide Li containing large and small secondary particles. 1.05 Ni 0.92 Co 0.05 Al 0.03 The average particle size (D50) of the large secondary particles was 12 μm, the average particle size (D50) of the small secondary particles was 3 μm, the mixing weight ratio of the large secondary particles to the small secondary particles was 80:20, and the difference in nickel content between the large secondary particles and the small secondary particles was 14 mol %.

[0130] Example 2 The same procedure as in Example 1 was carried out, except that the mixing weight ratio of the large nickel-based metal hydroxide having a size of 12 μm obtained in Preparation Example 1 and the small nickel-based metal hydroxide having a size of 3 μm obtained in Preparation Example 2 was changed to a weight ratio of 90:10, and heat treatment was performed in an oxygen atmosphere at about 720° C. for 10 hours, to obtain a nickel-based lithium metal composite oxide containing large secondary particles and small secondary particles as shown in Table 1 below. The large secondary particles had an average particle size (D50) of 12 μm, the small secondary particles had an average particle size (D50) of 3 μm, the mixing weight ratio of the large secondary particles to the small secondary particles was 90:10, and the difference in nickel content between the large secondary particles and the small secondary particles was 14 mol %.

[0131] [Table 1]

[0132] Examples 3 to 6 As shown in Table 2 below, the nickel-based lithium metal composite oxide was obtained in the same manner as in Example 1, except that the heat treatment temperature of the nickel-based metal hydroxide was changed.

[0133] [Table 2]

[0134] Example 7 Instead of the large nickel-based metal hydroxide particles having a size of 12 μm obtained in Production Example 1, the nickel-based metal hydroxide particles obtained in Production Example 3 (nickel-based metal hydroxide (Ni 0.96 Co 0.02 Al 0.02 The same procedure as in Example 1 was carried out except that (OH)2) was used, and a nickel-based lithium metal composite oxide satisfying the conditions in Table 3 below was obtained.

[0135] [Table 3]

[0136] Example 8 The same procedure as in Example 1 was carried out, except that the large-particle nickel-based metal hydroxide of Preparation Example 4 and the small-particle nickel-based metal hydroxide of Preparation Example 2 were used, to obtain a nickel-based lithium metal composite oxide satisfying the conditions in Table 4 below.

[0137] Example 9 The same procedure as in Example 1 was carried out, except that the large-particle nickel-based metal hydroxide of Production Example 5 and the small-particle nickel-based metal hydroxide of Production Example 2 were used, to obtain a nickel-based lithium metal composite oxide satisfying the conditions in Table 4 below.

[0138] Example 10 The same procedure as in Example 1 was carried out, except that the large-particle nickel-based metal hydroxide of Production Example 1 and the small-particle nickel-based metal hydroxide of Production Example 6 were used, to obtain a nickel-based lithium metal composite oxide satisfying the conditions in Table 4 below.

[0139] Example 11 The same procedure as in Example 1 was carried out, except that the large-particle nickel-based metal hydroxide of Production Example 1 and the small-particle nickel-based metal hydroxide of Production Example 7 were used, to obtain a nickel-based lithium metal composite oxide satisfying the conditions in Table 4 below.

[0140] [Table 4]

[0141] Comparative Example 1 The large-particle nickel-based metal hydroxide obtained in Production Example 1 was Ni 0.94 Co 0.03 Al 0.03 The small nickel-based metal hydroxide obtained in Production Example 3 was prepared by using Ni(OH)2. 0.96 Co 0.02 Al 0.02 The same procedure as in Example 1 was carried out, except that (OH)2 was used, to obtain a nickel-based lithium metal composite oxide.

[0142] Comparative Example 2 The large-particle nickel-based metal hydroxide obtained in Production Example 1 and lithium hydroxide (LiOH) were mixed in a dry manner in a molar ratio of 1:1.05 using a Henschel mixer, and subjected to a primary heat treatment in an oxygen atmosphere at about 740°C for 10 hours to obtain large-particle secondary particles of a nickel-based lithium metal composite oxide. The average particle size (D50) of the large-particle secondary particles is 12 μm.

[0143] Separately, the small nickel-based metal hydroxide particles having a size of 3 μm obtained in Preparation Example 2 and lithium hydroxide (LiOH) were mixed in a molar ratio of 1:1.01 in a dry manner using a Henschel mixer, and a secondary heat treatment was performed in an oxygen atmosphere at about 680°C for 10 hours to obtain small secondary particles of nickel-based lithium metal composite oxide. The small secondary particles have an average particle size (D50) of 3 μm.

[0144] The large secondary particles and the small secondary particles were mixed in a weight ratio of 80:20, and then a tertiary heat treatment was performed at about 700°C to obtain a nickel-based lithium metal composite oxide containing the large secondary particles and the small secondary particles.

[0145] According to Comparative Example 2, three heat treatment steps must be performed to obtain NCA, which increases the production cost and time, making it difficult to practically apply this method.

[0146] (manufacturing lithium secondary batteries)

[0147] Example 1 The nickel-based lithium metal composite oxide secondary particles obtained in Example 1 were used as the positive electrode active material to produce a lithium secondary battery as follows.

[0148] A mixture of 96 g of the nickel-based lithium metal composite oxide secondary particles obtained in Example 1, 2 g of polyvinylidene fluoride, 47 g of N-methylpyrrolidone as a solvent, and 2 g of carbon black as a conductive agent was mixed in a mixer to remove air bubbles, thereby producing a uniformly dispersed slurry for forming a positive electrode active material layer.

[0149] The slurry prepared by the above process was coated on an aluminum foil using a doctor blade to form a thin plate, which was then dried at 135°C for more than 3 hours, rolled, and vacuum dried to prepare a positive electrode.

[0150] A 2032-type coin cell was manufactured using the above-mentioned positive electrode and a lithium metal counter electrode as a counter electrode. A separator (thickness: about 16 μm) made of a porous polyethylene (PE) film was placed between the above-mentioned positive electrode and the above-mentioned lithium metal counter electrode, and an electrolyte was injected to manufacture a 2032-type coin cell. At this time, the electrolyte used was a solution containing 1.1M LiPF6 dissolved in a solvent made by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:5.

[0151] The chemical conversion process for the coin cell manufactured by the above process was carried out as follows.

[0152] The first charge and discharge cycle was performed after a 10-hour rest period, with a constant current charge of 0.2C until the voltage reached 4.25V, and then a constant voltage charge of 0.05C until the voltage reached 3V. The coin cell that had been fully charged was then given a rest period of about 10 minutes, after which a constant current discharge of 0.2C until the voltage reached 3V (first cycle). After a further rest period of about 10 minutes, the second charge and discharge cycle was performed after a constant current charge of 0.2C until the voltage reached 4.25V, and then a constant voltage charge of 0.05C until the current reached 3V. The coin cell that had been fully charged was given a rest period of about 10 minutes, after which a constant current discharge of 0.2C until the voltage reached 3V (second cycle).

[0153] Examples 2 to 11 A lithium secondary battery was prepared in the same manner as in Preparation Example 1, except that the nickel-based lithium metal composite oxide prepared in Examples 2 to 11 was used instead of the nickel-based lithium metal composite oxide prepared in Example 1.

[0154] Comparative production examples 1 and 2 Lithium secondary batteries were fabricated in the same manner as in Preparation Example 1, except that the nickel-based lithium metal composite oxides prepared in Comparative Preparation Examples 1 and 2 were used instead of the nickel-based lithium metal composite oxide prepared in Example 1.

[0155] Evaluation example 1: dQ / dV analysis The coin cells produced in Production Example 1 and Comparative Production Examples 1 and 2 were evaluated for charge / discharge characteristics and the like using a charger / discharger (manufacturer: TOYO, model: TOYO-3100).

[0156] The charge / discharge characteristic evaluation process will be described in more detail as follows.

[0157] The cells were charged at a constant current of 1 C until the voltage reached 4.3 V, and then charged at a constant voltage of 0.05 C until the voltage reached 3 V. After a rest period of about 10 minutes, the cells that had been charged were discharged at a constant current of 1 C until the voltage reached 3 V (first cycle). Such charge / discharge cycles were repeated a total of 50 times.

[0158] After the first cycle, after 30 cycles, and after 50 cycles, the ratios (A2 / A1) of the discharge peak intensity (A2) to the charge peak intensity (A1) were measured for the dQ / dV charge / discharge differential curve distributions shown in the voltage range of 4.1 V to 4.25 V. The results are shown in Table 5 below and in Figures 1 to 5.

[0159] The charging peak is the peak shown between 4.17V and 4.25V, and the aforementioned discharging peak is the peak shown between 4.14V and 4.17V.

[0160] FIG. 1 shows the dQ / dV charge / discharge differential curves after the first cycle for the lithium batteries of Preparation Example 1 and Comparative Preparation Examples 1 and 2, and FIG. 2 shows the dQ / dV charge / discharge differential curves after 30 cycles for the lithium batteries of Preparation Example 1 and Comparative Preparation Example 2.

[0161] Fig. 3 shows the dQ / dV charge / discharge differential curves after 50 cycles for the lithium batteries of Preparation Example 1 and Comparative Preparation Example 2, Fig. 4 shows the dQ / dV charge / discharge differential curves after the first cycle, 30 cycles, and 50 cycles for the lithium battery of Preparation Example 1, and Fig. 5 shows the dQ / dV charge / discharge differential curves after the first cycle, 30 cycles, and 50 cycles for the lithium battery of Comparative Preparation Example 2.

[0162] [Table 5]

[0163] 1 to 5 and Table 5, the lithium secondary battery of Preparation Example 1 exhibited a characteristic that A2 / A1 was 1.1 or more after the first cycle, 30 cycles, and 50 cycles, while the lithium batteries of Comparative Preparation Examples 1 and 2 exhibited a characteristic that A2 / A1 was less than 1.0 after the first cycle, 30 cycles, and 50 cycles. Furthermore, the lithium battery of Preparation Example 1 exhibited a reduced A2 / A1 change rate compared to Comparative Preparation Examples 1 and 2. The A2 / A1 change rate indicates the ratio of A2 / A1 at 50 cycles to A2 / A1 at 1 cycle, and the reduced A2 / A1 change rate indicates that the lithium battery of Preparation Example 1 has less structural change due to deterioration after charge / discharge cycles.

[0164] Evaluation example 2: X-ray diffraction analysis X-ray diffraction analysis was carried out on the nickel-based lithium metal composite oxide of Example 1 using X'pert pro (PANalytical) utilizing Cu Kα radiation (1.54056 Å). The results of the X-ray diffraction analysis are shown in FIG.

[0165] Referring to FIG. 6, it was found that the nickel-based lithium metal composite oxide of Example 1 was free of impurities and formed an ordered layered structure.

[0166] Evaluation example 3: Charge / discharge efficiency and capacity retention rate The charge / discharge efficiency and capacity retention rate of the coin cells manufactured according to Manufacturing Examples 1 to 6 and Comparative Manufacturing Example 1 were evaluated as follows using a charger / discharger (manufacturer: TOYO, model: TOYO-3100).

[0167] (1)Charge / discharge efficiency Each coin cell was charged at a constant current of 0.2 C at 25°C until it reached 4.25 V, and then charged at a constant voltage of 0.05 C. After the charged cells were rested for about 10 minutes, they were discharged at a constant current of 0.2 C until the voltage reached 3 V, and this cycle was repeated 50 times for evaluation.

[0168] (2) Capacity retention rate (CRR) Each coin cell was charged at a constant current of 1 C at 45°C until it reached 4.3 V, and then charged at a constant voltage of 0.05 C. After the charged cells were rested for about 10 minutes, they were discharged at a constant current of 1 C until the voltage reached 3 V, and this cycle was repeated 50 times for evaluation.

[0169] The capacity retention ratio (CRR) was calculated from the following Equation 1, and the initial charge / discharge efficiency was calculated from the following Equation 2. Some of the capacity retention ratio and initial charge / discharge efficiency characteristics were investigated and are shown in Table 6 and Figure 8. Figure 8 shows the capacity retention ratio characteristics of Preparation Examples 1 and 2 and Comparative Preparation Example 1.

[0170]

number

[0171]

number

[0172] [Table 6]

[0173] 8, it can be seen that the coin cells manufactured according to Preparation Examples 1 to 6 have improved capacity retention characteristics compared to Comparative Preparation Example 1. In addition, the coin cells of Preparation Examples 1 to 6 have improved initial charge / discharge efficiency characteristics compared to Comparative Preparation Example 1.

[0174] The coin cell of Comparative Example 2 showed excellent capacity retention characteristics. However, in the coin cell of Comparative Example 2, the positive electrode uses the nickel-based lithium metal composite oxide of Comparative Example 2 obtained by firing large particles and small particles in separate processes and firing three times, and the nickel-based lithium metal composite oxide of Comparative Example 2 must be subjected to three heat treatment processes, which requires high manufacturing costs and time, making this method difficult to apply in practice.

[0175] The charge-discharge characteristics of the coin cells of Preparation Examples 7 to 11 were evaluated in the same manner as in the coin cell of Preparation Example 1 described above.

[0176] As a result of the evaluation, the charge / discharge characteristics of the coin cells of Preparation Examples 7 to 11 were at a similar level to the charge / discharge characteristics of the coin cell of Preparation Example 1 described above.

[0177] Evaluation example 4: Charge / discharge characteristics The charge / discharge characteristics of the coin cells manufactured according to Preparation Example 1 and Comparative Preparation Example 1 were evaluated under the following conditions.

[0178] For charge / discharge characteristics, each coin cell was charged at 25°C with a current of 0.2 C until it reached 4.25 V, and then it was charged with a constant voltage of 0.05 C. After the cells were fully charged, they were rested for about 10 minutes, and then they were discharged at a constant current of 0.2 C until the voltage reached 3 V.

[0179] The above evaluation results are shown in FIG.

[0180] As shown in FIG. 9, the coin cell of Preparation Example 1 had improved charge / discharge characteristics compared to the coin cell of Comparative Example 1.

[0181] Although an embodiment has been described above with reference to the drawings and examples, they are merely illustrative, and a person skilled in the art will understand that various modifications and equivalent embodiments are possible therefrom. Therefore, the scope of protection of the present invention is defined by the claims. [Explanation of symbols]

[0182] 21 Lithium secondary battery 22 Negative electrode 23 Positive electrode 24 Separator 25 Battery case 26 Cap Assembly

Claims

1. A nickel-based lithium metal composite oxide comprising secondary particles including aggregates of primary particles, the nickel content being 50 mol % or more based on the total transition metal content in the nickel-based lithium metal composite oxide, The secondary particles include large secondary particles having an average particle size (D50) of 10 μm or more and small secondary particles having an average particle size (D50) of 5 μm or less, A nickel-based lithium metal composite oxide, wherein the large secondary particles have a higher nickel content than the small secondary particles, The large secondary particles are a compound represented by the following chemical formula 1-1, and the small secondary particles are a compound represented by the following chemical formula 1-2, A nickel-based lithium metal composite oxide, wherein the small secondary particles have a specific surface area of ​​2 to 15 m 2 / g, the large secondary particles have a specific surface area of ​​0.1 to 1 m 2 / g, the small secondary particles have a specific surface area that is at least twice as large as the large secondary particles, and the specific surface areas are BET specific surface areas measured by a BET method: 【Chemistry 1-1】 In the formula 1-1, M is boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr), or a combination thereof; 0.95≦a≦1.3, 0.88≦1−x−y−z≦0.96, 0.01≦x≦0.08, 0.001≦y≦0.05, and 0≦z≦0.01, 【Chemistry 1-2】 In the formula 1-2, M is boron (B), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), zirconium (Zr), or a combination thereof; 0.95≦a≦1.3, 0.75≦1-x-y-z≦0.85, 0.01≦x≦0.05, 0.001≦y≦0.05, and 0≦z≦0.

01.

2. The nickel-based lithium metal composite oxide according to claim 1, wherein in a dQ / dV charge / discharge differential curve relating to a lithium secondary battery having a positive electrode containing the nickel-based lithium metal composite oxide, the ratio (A2 / A1) of the discharge peak intensity (A2) to the charge peak intensity (A1) shown at a voltage of 4.1 V to 4.25 V at a current of 1 C is 1.1 or more.

3. 3. The nickel-based lithium metal composite oxide according to claim 2, wherein the charge peak is a peak indicated at 4.17 V to 4.25 V, and the discharge peak is a peak indicated at 4.14 V to 4.17 V.

4. 3. The nickel-based lithium metal composite oxide according to claim 2, wherein the ratio (A2 / A1) of the discharge peak intensity (A2) to the dQ / dV charge peak intensity (A1) is 1.1 to 1.

5.

5. 2. The nickel-based lithium metal composite oxide according to claim 1, wherein the difference in nickel content between the large secondary particles and the small secondary particles is 10 mol % or more.

6. 2. The nickel-based lithium metal composite oxide according to claim 1, wherein the large secondary particles have a nickel content of 85 to 99 mol % based on the total content of transition metals.

7. 2. The nickel-based lithium metal composite oxide according to claim 1, wherein the small secondary particles have a nickel content of 75 to 89 mol % based on the total transition metal content of the small secondary particles.

8. 2. The nickel-based lithium metal composite oxide according to claim 1, wherein the large secondary particles have an average particle size (D50) of 10 μm to 17 μm.

9. 2. The nickel-based lithium metal composite oxide according to claim 1, wherein the small secondary particles have an average particle size (D50) of 2 μm to 5 μm.

10. 2. The nickel-based lithium metal composite oxide according to claim 1, wherein the content of the large secondary particles is 30 to 90 parts by weight based on 100 parts by weight of the total content of the large secondary particles and the small secondary particles.

11. A large-particle nickel-based metal hydroxide having a nickel content of 50 mol % or more based on the total transition metal content in the large-particle nickel-based metal hydroxide, a small-particle nickel-based metal hydroxide having a nickel content of 50 mol % or more based on the total transition metal content in the small-particle nickel-based metal hydroxide, and a lithium precursor are mixed to obtain a precursor mixture, and then heat-treated; A method for producing a nickel-based lithium metal composite oxide, comprising the step of obtaining the nickel-based lithium metal composite oxide according to any one of claims 1 to 10.

12. The method for producing a nickel-based lithium metal composite oxide according to claim 11, wherein the heat treatment is performed at a temperature of 650°C to 800°C.

13. The method for producing a nickel-based lithium metal composite oxide according to claim 11, wherein the large-particle nickel-based metal hydroxide has a higher nickel content than the small-particle nickel-based metal hydroxide, and the difference in nickel content is 10 mol % or more.

14. The nickel content of the large-grain nickel-based metal hydroxide is 85 to 99 mol% based on the total content of transition metals in the large-grain nickel-based metal hydroxide; 12. The method for producing a nickel-based lithium metal composite oxide according to claim 11, wherein the nickel content of the small nickel-based metal hydroxide is 75 to 89 mol% based on the total transition metal content of the small nickel-based metal hydroxide.

15. 12. The method for producing a nickel-based lithium metal composite oxide according to claim 11, wherein the lithium precursor is lithium hydroxide, lithium fluoride, lithium carbonate, or a mixture thereof.

16. 11. A lithium secondary battery comprising a positive electrode, a negative electrode, and an electrolyte interposed between the positive electrode and the negative electrode, each containing the nickel-based lithium metal composite oxide according to claim 1.

Citation Information

Patent Citations

  • Cathode active material for secondary battery, preparation method therefor, and lithium secondary battery comprising same

    WO2019151834A1