Optical Glass

JP7583351B2Active Publication Date: 2024-11-14NIPPON ELECTRIC GLASS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020039803
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-09
Filing Date
2020-03-09
Publication Date
2024-11-14
Estimated Expiration
2040-03-09

AI Technical Summary

Benefits of technology

【0014】 本発明によれば、高屈折率、高分散の光学特性を達成することのできる新規の光学ガラスを提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583351000004
    Figure 0007583351000004
  • Figure 0007583351000001
    Figure 0007583351000001
  • Figure 0007583351000002
    Figure 0007583351000002
Patent Text Reader

Abstract

To provide a novel optical glass that can achieve optical properties of high refractive index and high dispersion.SOLUTION: An optical glass contains, in mol%, La2O3 of 5 to 40%, Nb2O5 of more than 50 to 90%, B2O3 to more than 0 to 30%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical glass used for optical lenses and the like. [Background technology]

[0002] In recent years, with the miniaturization and weight reduction of optical systems used in cameras, microscopes, endoscopes, etc., optical elements such as optical lenses are required to have optical properties of high refractive index and high dispersion. In order to make the glass used in optical elements have a higher refractive index, it is necessary to reduce the content of SiO2 and B2O3, which are the main framework components of the glass, and to contain a large amount of rare earth oxides such as La2O3, Gd2O3, and Ta2O5, or intermediate oxides such as Nb2O5 and TiO2. However, if the framework components are reduced and a large amount of intermediate oxides are contained, the glass-forming ability decreases and vitrification becomes difficult. General optical glass is produced by melting raw materials in a melting vessel such as a crucible and cooling them. Here, in the case of a glass composition with poor glass-forming ability, crystallization tends to proceed from the contact interface with the melting vessel in the conventional production method.

[0003] Even if the composition is difficult to vitrify, it can be vitrified by eliminating contact with the melting vessel and accelerating the cooling rate from the molten state. As such a method, a containerless levitation method (containerless solidification method) is known in which the raw materials are melted and cooled in a suspended state. By using this method, the glass melt hardly comes into contact with the melting vessel and can be cooled rapidly, so that even the composition that is difficult to vitrify as described above can be vitrified. For example, in Patent Document 1, a glass containing only TiO2 and BaO as a glass composition is produced by the containerless levitation method. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 4789086 Summary of the Invention [Problem to be solved by the invention]

[0005] Glasses with a high refractive index exceeding 1.8, including the glass described in Patent Document 1, are relatively prone to devitrification, and therefore it is difficult to make them large (for example, with a diameter of 2 mm or more) even when the containerless levitation method is used.

[0006] In view of the above, an object of the present invention is to provide a novel optical glass capable of achieving optical properties such as a high refractive index and high dispersion. [Means for solving the problem]

[0007] As a result of extensive research, the present inventors have found that the above problems can be solved by an optical glass containing La2O3, Nb2O5 and B2O3 in prescribed ranges as essential components.

[0008] That is, the optical glass of the present invention is characterized by containing, in mole percent, La2O35-40%, Nb2O5 more than 50-90%, and B2O30-30%. The optical glass of the present invention achieves optical properties such as high refractive index and high dispersion by containing a large amount of La2O3 and Nb2O5. If the contents of La2O3 and Nb2O5 are close to each other, La2O3-Nb2O5 crystals are likely to precipitate, so in the present invention, La2O3 is relatively small at 40% or less and Nb2O5 is relatively large at over 50%, thereby suppressing crystallization. In addition, by containing B2O3, which is a glass skeleton component, as an essential component, vitrification is facilitated. Therefore, the optical glass of the present invention achieves optical properties such as high refractive index and high dispersion, and can be made large in diameter.

[0009] The optical glass of the present invention preferably contains, by mol %, 60% or more of La2O3+Nb2O5. In the present invention, "○+○+···" means the total content of each component.

[0010] The optical glass of the present invention preferably contains, in mol %, 80% or more of La2O3+Nb2O5+B2O3.

[0011] The optical glass of the present invention preferably has a refractive index (nd) of 2 to 2.35.

[0012] The optical glass of the present invention preferably has an Abbe number of 5-40.

[0013] The method for producing optical glass of the present invention is a method for producing the above-mentioned optical glass, characterized in that it comprises a step of heating and melting the raw material lump while maintaining it in suspension to obtain molten glass, and then cooling the molten glass. Effect of the Invention

[0014] According to the present invention, it is possible to provide a novel optical glass that can achieve optical properties such as a high refractive index and high dispersion. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of an apparatus for producing an optical glass of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The optical glass of the present invention is characterized by containing, in mole percent, La2O35-40%, Nb2O5 more than 50-90%, and B2O30 more than 30%. The reasons for limiting the glass composition range in this way are explained below. In the following explanation of the content of each component, "%" means "mol %" unless otherwise specified.

[0017] La2O3 is a component that increases the refractive index and enhances the stability of vitrification. It also has the effect of improving weather resistance. The content of La2O3 is 5 to 40%, preferably 7 to 39%, more preferably 10 to 37%, further preferably 15 to 35%, and further preferably 20 to 30%. If the content of La2O3 is too low, it becomes difficult to obtain the above effects. On the other hand, if the content of La2O3 is too high, it becomes difficult to vitrify.

[0018] Nb2O5 is a component that has a large effect of increasing the refractive index and decreasing the Abbe number. As described above, in the glass composition of the present invention, when the content of Nb2O5 is reduced, the content of La2O3 and the content of Nb2O5 become close, and La2O3-Nb2O5 crystals tend to precipitate and make vitrification difficult. On the other hand, when the content of Nb2O5 is too high, vitrification also becomes difficult. Therefore, the content of Nb2O5 is more than 50 to 90%, preferably 51 to 85%, more preferably 52 to 80%, further preferably 53 to 75%, and further preferably 55 to 70%.

[0019] B2O3 is a component that forms a glass skeleton and expands the vitrification range. It also lowers the glass transition point and facilitates press molding. However, if the content of B2O3 is too high, the refractive index decreases and it becomes difficult to obtain the desired optical properties. Therefore, the content of B2O3 is more than 0 to 30%, preferably 0.1 to 20%, and more preferably 1 to 15%.

[0020] In order to obtain desired optical properties, the content of La2O3+Nb2O5 is preferably 60% or more, 70% or more, and particularly 80% or more. The upper limit of the content of La2O3+Nb2O5 is not particularly limited, but taking into consideration the contents of other components, it is preferably less than 100%, 99.9% or less, 99% or less, and particularly 95% or less.

[0021] In order to achieve desired optical properties and a large diameter (e.g., 2 mm or more, 3 mm or more, 4 mm or more, particularly 5 mm or more), the content of La2O3+Nb2O5+B2O3 is preferably 80% or more, 85% or more, particularly 90% or more. There is no particular upper limit to the content of La2O3+Nb2O5+B2O3, and it may be 100%, but when other components are contained, it is preferably less than 100%, 99.9% or less, 99% or less, particularly 95% or less.

[0022] In addition to the above components, the optical glass of the present invention may contain the following components.

[0023] Al2O3 is a component that forms a glass skeleton and expands the vitrification range. However, if the content of Al2O3 is too high, the refractive index decreases and it becomes difficult to obtain the desired optical properties. Therefore, the content of Al2O3 is preferably 0 to 20%, more preferably 0 to 10%.

[0024] SiO2 is a component that forms a glass skeleton and expands the vitrification range. It also has the effect of improving weather resistance. However, if the SiO2 content is too high, the refractive index decreases and it becomes difficult to obtain the desired optical characteristics. Therefore, the SiO2 content is preferably 0 to 20%, more preferably 0 to 10%.

[0025] GeO2 is a component that increases the refractive index and also has the effect of widening the vitrification range. However, if the GeO2 content is too high, the raw material cost tends to be high. Therefore, the GeO2 content is preferably 0 to 10%, more preferably 0 to 5%.

[0026] SnO2 is a component that is highly effective in increasing the refractive index. However, it is prone to cause coloring due to reduction. Therefore, the content of SnO2 is preferably 0 to 5%, more preferably 0 to 3%.

[0027] P2O5 is a component that constitutes the glass skeleton and has the effect of expanding the vitrification range. However, if the content is too high, phase separation is likely to occur. Therefore, the content of P2O5 is preferably 0 to 10%, more preferably 0 to 5%.

[0028] TiO2 is a component that has a large effect of increasing the refractive index, and also has the effect of increasing chemical durability. It also has the effect of decreasing the Abbe number and increasing dispersion. The TiO2 content is preferably 0 to 20%, 0.1 to 18%, 1 to 15%, and particularly preferably 5 to 12%. If the TiO2 content is too high, vitrification becomes difficult. Since TiO2 also has an effect as a colorant, it is preferable to contain TiO2 when the optical glass of the present invention is used for applications requiring coloring, such as color filters described below.

[0029] Ta2O5 is a component that has a large effect of increasing the refractive index. However, if the content of Ta2O5 is too high, it becomes difficult to vitrify and the raw material cost tends to increase. Therefore, the content of Ta2O5 is preferably 0 to 20%, more preferably 0 to 10%.

[0030] Y2O3 is a component that increases the stability of vitrification and increases the refractive index. However, if the content of Y2O3 is too high, vitrification becomes more difficult. Therefore, the content of Y2O3 is preferably 0 to 20%, more preferably 0 to 10%.

[0031] Yb2O3 is a component that increases the refractive index. However, if the content of Yb2O3 is too high, vitrification becomes difficult. In addition, the raw material cost tends to be high. Therefore, the content of Yb2O3 is preferably 0 to 20%, more preferably 0 to 10%.

[0032] ZnO, MgO, CaO, SrO and BaO have the effect of increasing the stability of vitrification and increasing chemical durability. However, if the content is too high, the refractive index decreases and it becomes difficult to obtain the desired optical characteristics. Therefore, the content of each of these components is preferably 0 to 10%, more preferably 0 to 5%.

[0033] Li2O, Na2O, K2O and Cs2O have the effect of lowering the melting temperature, but also lower the refractive index, so the total content is preferably 0 to 10%, and more preferably 0 to 5%.

[0034] Sb2O3 may be contained as a fining agent. However, in order to avoid coloration or from an environmental perspective, the content of Sb2O3 is preferably 0.1% or less, and more preferably substantially none is contained.

[0035] Considering the environmental impact, it is preferable that PbO and F are not substantially contained.

[0036] When the optical glass of the present invention is used for applications such as luminescent materials and color filters, transition metal components and rare earth components that serve as luminescent agents and colorants may be contained. Specifically, examples of transition metal oxides include Cr2O3, Mn2O3, Fe2O3, CoO, NiO, CuO, V2O5, MoO3, RuO2, and the like. Examples of rare earth oxides include CeO2, Nd2O3, Eu2O3, Tb2O3, Dy2O3, Er2O3, and the like. These transition metal oxides and rare earth oxides may be contained alone or in combination of two or more. The content of these transition metal oxides and rare earth oxides (total amount when two or more are contained) is preferably 0 to 5%, 0.001 to 3%, 0.01 to 2%, and particularly preferably 0.02 to 1%.

[0037] In addition, when the above-mentioned transition metal components and rare earth components are added to glasses containing large amounts of La2O3 and Nb2O5, crystallization is easily promoted, and it tends to be difficult to obtain a stable glass. On the other hand, since the present invention contains B2O3, which is a glass skeleton component, as an essential component, crystallization can be suppressed even if a transition metal component or rare earth component is added.

[0038] The refractive index of the optical glass of the present invention is preferably 2 or more, more preferably 2.05 or more. For example, when the optical glass of the present invention is used as a lens, the higher the refractive index, the thinner the lens can be made, which is advantageous for miniaturizing optical devices. The upper limit of the refractive index is preferably 2.35 or less, more preferably 2.3 or less, taking into account the stability of vitrification.

[0039] The Abbe number of the optical glass of the present invention is preferably from 5 to 40, and more preferably from 10 to 30. This makes it suitable as an optical lens for correcting chromatic aberration, for example.

[0040] The optical glass of the present invention can be produced, for example, by a containerless levitation method. Fig. 1 is a schematic cross-sectional view showing an example of a production apparatus for producing a glass material by the containerless levitation method. Hereinafter, the production method of the optical glass of the present invention will be described with reference to Fig. 1.

[0041] The glass material manufacturing apparatus 1 has a molding die 10. The molding die 10 also serves as a melting container. The molding die 10 has a molding surface 10a and a plurality of gas outlets 10b opening on the molding surface 10a. The gas outlets 10b are connected to a gas supply mechanism 11 such as a gas cylinder. Gas is supplied from the gas supply mechanism 11 to the molding surface 10a via the gas outlets 10b. The type of gas is not particularly limited, and may be, for example, air or oxygen, or an inert gas such as nitrogen gas, argon gas, or helium gas.

[0042] When manufacturing a glass material using manufacturing apparatus 1, first, raw material lump 12 prepared to become glass of the above composition is placed on molding surface 10a. Examples of raw material lump 12 include a pressed compact of raw material powder, a sintered compact of raw material powder, and an aggregate of crystals having a composition equivalent to the target glass composition.

[0043] Next, the raw material lump 12 is floated on the forming surface 10a by ejecting gas from the gas ejection holes 10b. That is, the raw material lump 12 is held in a state where it is not in contact with the forming surface 10a. In this state, the raw material lump 12 is irradiated with laser light from the laser light irradiation device 13. As a result, the raw material lump 12 is heated and melted to be vitrified to obtain molten glass. Then, the molten glass is cooled to obtain a glass material. In the process of heating and melting the raw material lump 12 and the process of cooling the molten glass and further the glass material until the temperature is at least below the softening point, it is preferable to continue ejecting at least gas and suppress contact between the raw material lump 12, the molten glass, and further the glass material and the forming surface 10a. In addition to the method of irradiating laser light, the method of heating and melting may be radiation heating. EXAMPLES

[0044] The optical glass of the present invention will be described in detail below using examples, but the present invention is not limited to the following examples.

[0045] Tables 1 to 3 show examples of the present invention (Nos. 1 to 6, 11 to 23) and comparative examples (Nos. 7 to 10).

[0046] [Table 1]

[0047] [Table 2]

[0048] [Table 3]

[0049] First, 0.2 to 0.5 g of raw material powder prepared to have the glass composition shown in Tables 1 to 3 was weighed out, press-molded, and then fired at 800° C. for 6 hours to prepare a raw material lump.

[0050] Using the raw material lump obtained above, roughly spherical glass material (diameter 3 to 7.5 mm) was produced by the containerless levitation method using an apparatus similar to that shown in Figure 1. A 100 W CO2 laser oscillator was used as the heat source. Oxygen gas was used as the gas for levitating the raw material lump, and was supplied at a flow rate of 1 to 15 L / min.

[0051] The refractive index (nd) and Abbe number (νd) of the obtained glass material were measured, and the results are shown in Table 1.

[0052] The refractive index was evaluated by bonding the glass material onto a soda plate substrate having a thickness of 5 mm, polishing it at a right angle, and measuring the refractive index against the d-line (587.6 nm) of a helium lamp using a Shimadzu KPR-2000.

[0053] The Abbe number was calculated from the formula (νd) = {(nd-1) / (nF-nC)} using the refractive index for the d-line and the refractive index for the F-line (486.1 nm) and C-line (656.3 nm) of a hydrogen lamp.

[0054] As shown in Tables 1 to 3, the samples Nos. 1 to 6 and 11 to 23, which are examples, had high refractive indices of 2.11 to 2.27 and low Abbe numbers of 18.1 to 27.4, and were highly dispersed. On the other hand, the samples Nos. 7 to 10, which are comparative examples, did not vitrify. [Explanation of symbols]

[0055] 1: Glass material manufacturing equipment 10: Molding mold 10a: Molding surface 10b: Gas vent 11: Gas supply mechanism 12: Raw material lump 13: Laser light irradiation device

Claims

1. In mole percent, La 2 O 3 20-40%, Nb 2 O 5 Over 50 to 75%, B 2 O 3 The optical glass contains more than 0 to 29% by mass and is free of TiO 2 .

2. In mole percent, La 2 O 3 +Nb 2 O 5 2. The optical glass according to claim 1, containing more than 70%.

3. In mole percent, La 2 O 3 +Nb 2 O 5 +B 2 O 3 3. The optical glass according to claim 1, wherein the content is 80% or more.

4. 4. The optical glass according to claim 1, wherein the refractive index (nd) is from 2 to 2.

35.

5. 5. The optical glass according to claim 1, wherein the Abbe number is 5 to 40.

6. A method for producing the optical glass according to any one of claims 1 to 5, comprising the steps of:

1. A method for producing optical glass, comprising the steps of: heating and melting a raw material lump while holding the raw material lump in a suspended state to obtain molten glass; and then cooling the molten glass.

Citation Information

Patent Citations

  • Optical glass, optical element and method for manufacturing optical glass

    JP2014196236A

  • Optical glass and method for producing the same

    JP2018020934A

  • Optical glass and method for producing the same

    JP2018020935A

  • Method for producing variu-titanium oxide glass by containerless solidification.

    JP4789086B2

  • Glass

    WO2010137276A1