Cleaning composition and cleaning method
A cleaning composition with tetra(hydrocarbon) ammonium fluoride and alkylene glycol dialkyl ether effectively removes polysiloxane adhesive residue on semiconductor substrates, ensuring high efficiency and substrate integrity.
Patent Information
- Application Number
- JP2023011409
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-02-15
- Filing Date
- 2023-01-27
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-02-14
AI Technical Summary
Existing cleaning compositions for removing polysiloxane adhesive residue on semiconductor substrates are inefficient and can corrode the substrate, failing to provide effective cleaning without damaging the surface.
A cleaning composition comprising tetra(hydrocarbon) ammonium fluoride and an organic solvent, specifically alkylene glycol dialkyl ether and a lactam compound, is used to clean polysiloxane adhesive residue, ensuring high efficiency and substrate integrity.
The composition allows for rapid and thorough removal of adhesive residue without corroding the substrate, maintaining substrate quality and efficiency in cleaning processes.
Smart Images

Figure 0007583377000001 
Figure 0007583377000002 
Figure 0007583377000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a cleaning composition and a cleaning method used for removing adhesive residues after peeling off a temporary adhesive layer formed on a semiconductor substrate using a polysiloxane adhesive, for example. [Background technology]
[0002] Conventionally, semiconductor wafers have been integrated in a two-dimensional plane, but for the purpose of further integration, there is a demand for semiconductor integration technology that integrates (stacks) the plane in a three-dimensional direction. This three-dimensional stacking is a technology that integrates multiple layers while connecting them with through silicon vias (TSVs). When integrating multiple layers, each wafer to be integrated is thinned by polishing the side opposite the circuit surface (i.e., the back side), and the thinned semiconductor wafers are stacked.
[0003] Semiconductor wafers before thinning (also simply called wafers here) are bonded to a support in order to be polished by a polishing device. The bond at that time must be easily peeled off after polishing, so it is called temporary bonding. This temporary bonding must be easily removed from the support, and if a large force is applied to remove it, the thinned semiconductor wafer may be cut or deformed, so it is easily removed to prevent such things from happening. However, it is not preferable for the semiconductor wafer to come off or shift due to the polishing stress when polishing the back surface. Therefore, the performance required for the temporary bonding is to withstand the stress during polishing and to be easily removed after polishing. For example, it is required to have a high stress (strong adhesive force) in the planar direction during polishing and a low stress (weak adhesive force) in the vertical direction during removal. In addition, the processing process may reach high temperatures of 150°C or more, so heat resistance is also required.
[0004] Under these circumstances, in the semiconductor field, polysiloxane adhesives that can provide these properties are mainly used as temporary adhesives. In polysiloxane-based adhesion using a polysiloxane adhesive, adhesive residues often remain on the substrate surface after peeling off the thinned substrate. In order to avoid problems in the subsequent process, cleaning compositions have been developed to remove these residues and clean the semiconductor substrate surface (e.g., Patent Documents 1 and 2), and there is a constant demand for new cleaning compositions in the semiconductor field these days. Patent Document 1 discloses a siloxane resin remover containing a polar aprotic solvent and a quaternary ammonium hydroxide, and Patent Document 2 discloses a cured resin remover containing an alkyl ammonium fluoride, but the emergence of a more effective cleaning composition is desired. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2014 / 092022 [Patent Document 2] U.S. Patent No. 6,818,608 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a cleaning agent composition and a cleaning method which, when cleaning a substrate such as a semiconductor substrate, can provide good cleaning properties for adhesive residues after peeling off a temporary adhesion formed by an adhesive layer obtained by using a polysiloxane-based adhesive, and can clean the substrate highly efficiently without corroding the substrate. [Means for solving the problem]
[0007] The present inventors have conducted intensive research to solve the above problems, and as a result have found that, when cleaning a substrate such as a semiconductor substrate to which adhesive residue remains after peeling off a temporary adhesion formed by an adhesive layer obtained using a polysiloxane-based adhesive, by using a cleaning composition containing tetra(hydrocarbon)ammonium fluoride and an organic solvent, where the organic solvent contains an alkylene glycol dialkyl ether and a lactam compound represented by formula (1), the substrate can be cleaned highly efficiently and satisfactorily in a short time without corroding the substrate, and have completed the present invention. Incidentally, Patent Documents 1 and 2 contain no description that teaches or suggests the specific configuration of the cleaning composition of the present invention.
[0008] That is, the present invention provides 1. A cleaning composition used to remove a polysiloxane-based adhesive remaining on a substrate, the cleaning composition comprising a tetra(hydrocarbon)ammonium fluoride and an organic solvent, the organic solvent comprising an alkylene glycol dialkyl ether and a lactam compound represented by formula (1); [ka] (In the formula, R 101 represents an alkyl group having 1 to 6 carbon atoms, R 102 represents an alkylene group having 1 to 6 carbon atoms. 2. The cleaning composition according to 1, wherein the lactam compound includes at least one selected from N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone. 3. The cleaning composition according to 1 or 2, wherein the alkylene glycol dialkyl ether comprises at least one selected from ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dipropyl ethane, ethylene glycol dibutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, and propylene glycol dipropyl ether; 4. The cleaning composition according to any one of 1 to 3, wherein the tetra(hydrocarbon)ammonium fluoride includes at least one selected from the group consisting of tetramethylammonium fluoride, tetraethylammonium fluoride, tetrapropylammonium fluoride, and tetrabutylammonium fluoride. 5. Any of the cleaning composition according to 1 to 4, wherein the ratio of the alkylene glycol dialkyl ether to the lactam compound is, in terms of mass ratio, alkylene glycol dialkyl ether:lactam compound=30:70 to 80:20. 6. The cleaning composition according to 1, wherein the lactam compound comprises at least one selected from N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone, the alkylene glycol dialkyl ether comprises at least one selected from ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dipropyl ethane, ethylene glycol dibutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether and propylene glycol dipropyl ether, and the tetra(hydrocarbon)ammonium fluoride comprises at least one selected from tetramethylammonium fluoride, tetraethylammonium fluoride, tetrapropylammonium fluoride and tetrabutylammonium fluoride. 7. The cleaning composition according to 6, wherein the ratio of the alkylene glycol dialkyl ether to the lactam compound is, in terms of mass ratio, alkylene glycol dialkyl ether:lactam compound=30:70 to 80:20. 8. The cleaning composition according to any one of 1 to 7, wherein the polysiloxane-based adhesive remaining on the substrate is an adhesive residue of an adhesive layer obtained from an adhesive composition containing a component (A) that cures by a hydrosilylation reaction. 9. A cleaning method comprising removing an adhesive residue remaining on a substrate by using any one of the cleaning compositions according to 1 to 8. 10. A method for producing a processed semiconductor substrate, comprising: a first step of producing a laminate comprising a semiconductor substrate, a support substrate, and an adhesive layer obtained from an adhesive composition; a second step of processing the semiconductor substrate of the obtained laminate; a third step of peeling off the semiconductor substrate after processing; and a fourth step of cleaning and removing adhesive residue remaining on the peeled semiconductor substrate with a cleaning composition, characterized in that any of the cleaning compositions 1 to 8 is used as the cleaning composition. to provide. Effect of the Invention
[0009] The cleaning composition of the present invention makes it possible to clean substrates such as semiconductor substrates to which adhesive residue remains after peeling off a temporary adhesion formed by an adhesive layer obtained using a polysiloxane-based adhesive, in a short time and with high efficiency without corroding the substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will now be described in further detail. The cleaning composition of the present invention is a cleaning composition used for removing a polysiloxane-based adhesive remaining on a substrate such as a semiconductor substrate, and contains tetra(hydrocarbon)ammonium fluoride and an organic solvent, where the organic solvent contains an alkylene glycol dialkyl ether and a lactam compound represented by formula (1).
[0011] [ka] (In the formula, R 101 represents an alkyl group having 1 to 6 carbon atoms, R 102 represents an alkylene group having 1 to 6 carbon atoms.
[0012] Specific examples of the hydrocarbon group in the tetra(hydrocarbon)ammonium fluoride include an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, and an aryl group having 6 to 20 carbon atoms.
[0013] In a preferred embodiment of the invention, the tetra(hydrocarbon)ammonium fluoride comprises a tetraalkylammonium fluoride. Specific examples of tetraalkylammonium fluoride include, but are not limited to, tetramethylammonium fluoride, tetraethylammonium fluoride, tetrapropylammonium fluoride, tetrabutylammonium fluoride, etc. Among these, tetrabutylammonium fluoride is preferred. The tetra(hydrocarbon)ammonium fluoride may be in the form of a hydrate. The tetra(hydrocarbon)ammonium fluoride may be used alone or in combination of two or more kinds.
[0014] The amount of tetra(hydrocarbon)ammonium fluoride is not particularly limited as long as it dissolves in the solvent contained in the cleaning composition, but is usually 0.1 to 30% by mass based on the cleaning composition.
[0015] Specific examples of alkylene glycol dialkyl ethers include, but are not limited to, ethylene glycol dimethyl ether (also called dimethoxyethane, the same applies below), ethylene glycol diethyl ether (diethoxyethane), ethylene glycol dipropyl ethane (dipropoxyethane), ethylene glycol dibutyl ether (dibutoxyethane), propylene glycol dimethyl ether (dimethoxypropane), propylene glycol diethyl ether (diethoxypropane), propylene glycol dipropyl ether (dipropoxypropane), and the like. The alkylene glycol dialkyl ethers can be used alone or in combination of two or more.
[0016] The amount of the alkylene glycol dialkyl ether is 1 to 98.9% by mass based on the cleaning agent composition.
[0017] In the above formula (1), specific examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, etc., and specific examples of the alkylene group having 1 to 6 carbon atoms include a methylene group, an ethylene group, a trimethylene group, a tetramethylene, a pentamethylene group, a hexamethylene group, etc., but are not limited to these.
[0018] Specific examples of the lactam compound represented by the above formula (1) include α-lactam compounds, β-lactam compounds, γ-lactam compounds, δ-lactam compounds, etc., which can be used alone or in combination of two or more.
[0019] In a preferred embodiment of the present invention, the lactam compound represented by the above formula (1) comprises 1-alkyl-2-pyrrolidone (N-alkyl-γ-butyrolactam), in a more preferred embodiment, N-methylpyrrolidone (NMP) or N-ethylpyrrolidone (NEP), and in an even more preferred embodiment, N-methylpyrrolidone (NMP).
[0020] The amount of the lactam compound represented by the above formula (1) is usually 1 to 98.9% by mass based on the cleaning composition.
[0021] The ratio (mass ratio) of the alkylene glycol dialkyl ether to the lactam compound represented by the above formula (1) is arbitrary, but is preferably alkylene glycol dialkyl ether:lactam compound represented by the above formula (1)=30:70 to 80:20, more preferably 35:65 to 76:24, even more preferably 40:60 to 73:27, and still more preferably 45:55 to 70:30.
[0022] In the present invention, the cleaning composition contains only an organic solvent as a solvent, which reduces the occurrence of metal contamination and metal corrosion caused by water and enables substrates to be cleaned reproducibly and appropriately. Therefore, the cleaning composition of the present invention usually contains only an organic solvent as a solvent. Note that "only an organic solvent" means that only the organic solvent is used intentionally as a solvent, and does not deny the presence of water contained in the organic solvent or other components.
[0023] In a preferred embodiment of the present invention, the cleaning composition of the present invention contains only the above alkylene glycol dialkyl ether and the lactam compound represented by the above formula (1) as the organic solvent.
[0024] In the present invention, the tetra(hydrocarbon)ammonium fluoride is dissolved in a solvent contained in the cleaning composition.
[0025] The cleaning composition of the present invention is obtained by mixing the above-mentioned tetra(hydrocarbon)ammonium fluoride, the above-mentioned alkylene glycol dialkyl ether, the lactam compound represented by the above formula (1), and other components as necessary. The order of mixing the components can be any order as long as there is no problem such as precipitation or liquid separation that would prevent the object of the present invention from being achieved. That is, among all the components of the cleaning composition, a part of them may be mixed in advance, and then the remaining components may be mixed, or all the components may be mixed at once. In addition, if necessary, the cleaning composition may be filtered. Furthermore, when the components used are, for example, hygroscopic or deliquescent, all or a part of the preparation of the cleaning composition may be carried out under an inert gas.
[0026] The cleaning composition of the present invention as described above has good cleaning properties for polysiloxane adhesives, and is excellent in both cleaning speed and cleaning durability. Specifically, regarding the cleaning speed, when an adhesive layer obtained from an adhesive composition is contacted with the cleaning composition of the present invention for 5 minutes at room temperature (23° C.), the etching rate [μm / min] calculated by measuring the decrease in film thickness before and after contact and dividing the decrease by the cleaning time is usually 5.0 [μm / min] or more, in a preferred embodiment 7.0 [μm / min] or more, in a more preferred embodiment 7.5 [μm / min] or more, in an even more preferred embodiment 8.0 [μm / min] or more, and in an even more preferred embodiment 9.0 [μm / min] or more. As for cleaning durability, when 1 g of an adhesive solid obtained from the adhesive composition is contacted with 2 g of the cleaning composition of the present invention at room temperature (23° C.), the cleaning composition of the present invention usually dissolves most of the adhesive solid within 12 to 24 hours, and in a preferred embodiment, completely dissolves the adhesive solid within 2 to 12 hours, and in a more preferred embodiment, completely dissolves the adhesive solid within 1 to 2 hours.
[0027] According to the present invention, by using the above-mentioned cleaning composition to clean and remove the polysiloxane-based adhesive remaining on a substrate such as a semiconductor substrate, the substrate can be cleaned in a short time, and substrates such as semiconductor substrates can be cleaned efficiently and satisfactorily. The cleaning composition of the present invention is used for cleaning the surfaces of various substrates such as semiconductor substrates, and the objects to be cleaned are not limited to silicon semiconductor substrates, but also include various substrates such as germanium substrates, gallium arsenide substrates, gallium phosphide substrates, gallium arsenide-aluminum substrates, aluminum-plated silicon substrates, copper-plated silicon substrates, silver-plated silicon substrates, gold-plated silicon substrates, titanium-plated silicon substrates, silicon substrates with a silicon nitride film formed thereon, silicon substrates with a silicon oxide film formed thereon, silicon substrates with a polyimide film formed thereon, glass substrates, quartz substrates, liquid crystal substrates and organic EL substrates.
[0028] A suitable method for using the cleaning composition of the present invention in a semiconductor process includes use in a method for producing thinned substrates used in semiconductor packaging techniques such as TSV. Specifically, the cleaning composition of the present invention is used as the cleaning composition in a production method including: a first step of producing a laminate including a semiconductor substrate, a support substrate, and an adhesive layer obtained from the adhesive composition; a second step of processing the semiconductor substrate of the obtained laminate; a third step of peeling off the semiconductor substrate after processing; and a fourth step of cleaning and removing adhesive residue remaining on the peeled semiconductor substrate with the cleaning composition.
[0029] The adhesive composition used to form the adhesive layer in the first step can typically be at least one selected from silicone-based, acrylic resin-based, epoxy resin-based, polyamide-based, polystyrene-based, polyimide-based, and phenol resin-based adhesives. In particular, the cleaning composition of the present invention is effective for cleaning polysiloxane-based adhesives. In particular, the cleaning composition of the present invention is effective for cleaning and removing adhesive residues from polysiloxane-based adhesives containing component (A) that cures by a hydrosilylation reaction. Therefore, the following describes a method for producing a thinned substrate using a polysiloxane-based adhesive (adhesive composition) containing component (A) that cures via a hydrosilylation reaction and the cleaning composition of the present invention, but the present invention is not limited thereto.
[0030] First, a first step for producing a laminate including a semiconductor substrate, a supporting substrate, and an adhesive layer obtained from an adhesive composition will be described. The component (A) contained in the adhesive composition that cures by a hydrosilylation reaction is, for example, a siloxane unit (Q unit) represented by SiO2, R 1 R 2 R 3 SiO 1 / 2 Siloxane unit (M unit) represented by R 4 R 5 SiO 2 / 2 Siloxane units (D units) represented by the formula 6 SiO 3 / 2and a platinum group metal catalyst (A2), wherein the polysiloxane (A1) contains one or more units selected from the group consisting of siloxane units (T units) represented by SiO2, siloxane units (Q' units) represented by R 1 'R 2 'R 3 'SiO 1 / 2 Siloxane unit (M' unit) represented by R 4 'R 5 'SiO 2 / 2 Siloxane units (D' units) represented by the formula 6 'SiO 3 / 2 and at least one unit selected from the group consisting of M' units, D' units and T' units; and a polyorganosiloxane (a1) having siloxane units (Q" units) represented by SiO2, R 1 "R 2 "R 3 "SiO 1 / 2 Siloxane unit (M” unit) represented by R 4 "R 5 "SiO 2 / 2 Siloxane units (D" units) represented by the formula 6 "SiO 3 / 2 and a polyorganosiloxane (a2) containing one or more units selected from the group consisting of siloxane units (T″ units) represented by the following formula:
[0031] R 1 ~R 6 are groups or atoms bonded to a silicon atom, and each independently represents an alkyl group, an alkenyl group, or a hydrogen atom. R 1 '~R 6 R ′ is a group bonded to a silicon atom, and each independently represents an alkyl group or an alkenyl group. 1 '~R 6 At least one of is an alkenyl group. R 1 ”~R 6" are groups or atoms bonded to the silicon atom, and each independently represents an alkyl group or a hydrogen atom, but R 1 ”~R 6 At least one of " is a hydrogen atom.
[0032] The alkyl group may be linear, branched, or cyclic, but is preferably a linear or branched alkyl group. The number of carbon atoms is not particularly limited, but is usually 1 to 40, preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less.
[0033] Specific examples of linear or branched alkyl groups include methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, s-butyl, t-butyl, n-pentyl, 1-methyl-n-butyl, 2-methyl-n-butyl, 3-methyl-n-butyl, 1,1-dimethyl-n-propyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, and 3-methyl-n-pentyl. Examples of the aryl group include, but are not limited to, a 4-methyl-n-pentyl group, a 1,1-dimethyl-n-butyl group, a 1,2-dimethyl-n-butyl group, a 1,3-dimethyl-n-butyl group, a 2,2-dimethyl-n-butyl group, a 2,3-dimethyl-n-butyl group, a 3,3-dimethyl-n-butyl group, a 1-ethyl-n-butyl group, a 2-ethyl-n-butyl group, a 1,1,2-trimethyl-n-propyl group, a 1,2,2-trimethyl-n-propyl group, a 1-ethyl-1-methyl-n-propyl group, and a 1-ethyl-2-methyl-n-propyl group. Of these, a methyl group is preferred.
[0034] Specific examples of the cyclic alkyl group include a cyclopropyl group, a cyclobutyl group, a 1-methyl-cyclopropyl group, a 2-methyl-cyclopropyl group, a cyclopentyl group, a 1-methyl-cyclobutyl group, a 2-methyl-cyclobutyl group, a 3-methyl-cyclobutyl group, a 1,2-dimethyl-cyclopropyl group, a 2,3-dimethyl-cyclopropyl group, a 1-ethyl-cyclopropyl group, a 2-ethyl-cyclopropyl group, a cyclohexyl group, a 1-methyl-cyclopentyl group, a 2-methyl-cyclopentyl group, a 3-methyl-cyclopentyl group, a 1-ethyl-cyclobutyl group, a 2-ethyl-cyclobutyl group, a 3-ethyl-cyclobutyl group, a 1,2-dimethyl-cyclobutyl group, a 1,3-dimethyl-cyclobutyl group, a 2,2-dimethyl-cyclobutyl group, a 2,3-dimethyl-cyclobutyl group, a 2,4-dimethyl cycloalkyl groups such as aryl-cyclobutyl group, 3,3-dimethyl-cyclobutyl group, 1-n-propyl-cyclopropyl group, 2-n-propyl-cyclopropyl group, 1-i-propyl-cyclopropyl group, 2-i-propyl-cyclopropyl group, 1,2,2-trimethyl-cyclopropyl group, 1,2,3-trimethyl-cyclopropyl group, 2,2,3-trimethyl-cyclopropyl group, 1-ethyl-2-methyl-cyclopropyl group, 2-ethyl-1-methyl-cyclopropyl group, 2-ethyl-2-methyl-cyclopropyl group, and 2-ethyl-3-methyl-cyclopropyl group; and bicycloalkyl groups such as bicyclobutyl group, bicyclopentyl group, bicyclohexyl group, bicycloheptyl group, bicyclooctyl group, bicyclononyl group, and bicyclodecyl group, but are not limited to these.
[0035] The alkenyl group may be either linear or branched, and the number of carbon atoms therein is not particularly limited, but is usually 2 to 40, preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less.
[0036] Specific examples of the alkenyl group include ethenyl, 1-propenyl, 2-propenyl, 1-methyl-1-ethenyl, 1-butenyl, 2-butenyl, 3-butenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, 1-ethylethenyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, 1-n-propylethenyl, 1-methyl-1-butenyl, 1-methyl-2-butenyl, 1-methyl-3-butenyl, 2-ethyl-2- propenyl, 2-methyl-1-butenyl, 2-methyl-2-butenyl, 2-methyl-3-butenyl, 3-methyl-1-butenyl, 3-methyl-2-butenyl, 3-methyl-3-butenyl, 1,1-dimethyl-2-propenyl, 1-i-propylethenyl, 1,2-dimethyl-1-propenyl, 1,2-dimethyl-2-propenyl, 1-cyclopentenyl, 2-cyclopentenyl, 3-cyclopentenyl, 1-hexenyl, 2-hexenyl, 3-hexenyl, 4-hexenyl, 5-hexenyl, 1-methyl-1- pentenyl group, 1-methyl-2-pentenyl group, 1-methyl-3-pentenyl group, 1-methyl-4-pentenyl group, 1-n-butylethenyl group, 2-methyl-1-pentenyl group, 2-methyl-2-pentenyl group, 2-methyl-3-pentenyl group, 2-methyl-4-pentenyl group, 2-n-propyl-2-propenyl group, 3-methyl-1-pentenyl group, 3-methyl-2-pentenyl group, 3-methyl-3-pentenyl group, 3-methyl-4-pentenyl group, 3-ethyl-3-butenyl group, 4-methyl-1-pentenyl group, 4-methyl-2-pentenyl group, 4 -Methyl-3-pentenyl, 4-methyl-4-pentenyl, 1,1-dimethyl-2-butenyl, 1,1-dimethyl-3-butenyl, 1,2-dimethyl-1-butenyl, 1,2-dimethyl-2-butenyl, 1,2-dimethyl-3-butenyl, 1-methyl-2-ethyl-2-propenyl, 1-s-butylethenyl, 1,3-dimethyl-1-butenyl, 1,3-dimethyl-2-butenyl, 1,3-dimethyl-3-butenyl, 1-i-butylethenyl, 2,2-dimethyl-3-butenyl, 2,3-dimethyl-1-butenyl, 2,3-dimethyl-2-butenyl group, 2,3-dimethyl-3-butenyl group, 2-i-propyl-2-propenyl group, 3,3-dimethyl-1-butenyl group, 1-ethyl-1-butenyl group, 1-ethyl-2-butenyl group, 1-ethyl-3-butenyl group, 1-n-propyl-1-propenyl group, 1-n-propyl-2-propenyl group, 2-ethyl-1-butenyl group, 2-ethyl-2-butenyl group, 2-ethyl-3-butenyl group, 1,1,2-trimethyl-2-propenyl group, 1-t-butylethenyl group, 1-methyl-1-ethyl-2-propenyl group, 1-ethyl-2-methyl-1-propenyl group, 1-ethyl-2-methyl-2-propenyl group, 1-i-propyl-1-propenyl group, 1-i-propyl- Examples of the cyclopentyl group include, but are not limited to, a 2-propenyl group, a 1-methyl-2-cyclopentenyl group, a 1-methyl-3-cyclopentenyl group, a 2-methyl-1-cyclopentenyl group, a 2-methyl-2-cyclopentenyl group, a 2-methyl-3-cyclopentenyl group, a 2-methyl-4-cyclopentenyl group, a 2-methyl-5-cyclopentenyl group, a 2-methylene-cyclopentyl group, a 3-methyl-1-cyclopentenyl group, a 3-methyl-2-cyclopentenyl group, a 3-methyl-3-cyclopentenyl group, a 3-methyl-4-cyclopentenyl group, a 3-methyl-5-cyclopentenyl group, a 3-methylene-cyclopentyl group, a 1-cyclohexenyl group, a 2-cyclohexenyl group, and a 3-cyclohexenyl group. Of these, ethenyl and 2-propenyl are preferred.
[0037] As described above, the polysiloxane (A1) contains the polyorganosiloxane (a1) and the polyorganosiloxane (a2), and the alkenyl group contained in the polyorganosiloxane (a1) and the hydrogen atom (Si-H group) contained in the polyorganosiloxane (a2) form a crosslinked structure through a hydrosilylation reaction in the presence of a platinum group metal catalyst (A2), thereby curing.
[0038] The polyorganosiloxane (a1) contains one or more units selected from the group consisting of Q' units, M' units, D' units and T' units, and also contains at least one unit selected from the group consisting of M' units, D' units and T' units. As the polyorganosiloxane (a1), a combination of two or more polyorganosiloxanes satisfying such conditions may be used.
[0039] Preferred combinations of two or more selected from the group consisting of Q' units, M' units, D' units and T' units include, but are not limited to, (Q' units and M' units), (D' units and M' units), (T' units and M' units), and (Q' units, T' units and M' units).
[0040] In addition, when the polyorganosiloxane (a1) contains two or more types of polyorganosiloxanes, combinations of (Q' units and M' units) and (D' units and M' units), combinations of (T' units and M' units) and (D' units and M' units), and combinations of (Q' units, T' units and M' units) and (T' units and M' units) are preferred, but are not limited to these.
[0041] The polyorganosiloxane (a2) contains one or more units selected from the group consisting of Q″ units, M″ units, D″ units, and T″ units, and also contains at least one unit selected from the group consisting of M″ units, D″ units, and T″ units. As the polyorganosiloxane (a2), a combination of two or more polyorganosiloxanes satisfying such conditions may be used.
[0042] Preferred combinations of two or more selected from the group consisting of Q″ units, M″ units, D″ units and T″ units include, but are not limited to, (M″ units and D″ units), (Q″ units and M″ units), and (Q″ units, T″ units and M″ units).
[0043] The polyorganosiloxane (a1) is composed of siloxane units having alkyl and / or alkenyl groups bonded to the silicon atoms thereof.1 '~R 6 The proportion of alkenyl groups in all the substituents represented by R 1 '~R 6 ' can be an alkyl group.
[0044] The polyorganosiloxane (a2) is composed of siloxane units in which an alkyl group and / or a hydrogen atom is bonded to the silicon atom. 1 ”~R 6 The proportion of hydrogen atoms in all the substituents and substituted atoms represented by R 1 ”~R 6 " can be an alkyl group.
[0045] The polysiloxane (A1) contains a polyorganosiloxane (a1) and a polyorganosiloxane (a2). In a preferred embodiment of the present invention, the molar ratio of the alkenyl groups contained in the polyorganosiloxane (a1) to the hydrogen atoms constituting the Si-H bonds contained in the polyorganosiloxane (a2) can be in the range of 1.0:0.5 to 1.0:0.66.
[0046] The weight average molecular weight of each of the polyorganosiloxane (a1) and the polyorganosiloxane (a2) is usually from 500 to 1,000,000, and preferably from 5,000 to 50,000.
[0047] The weight average molecular weight can be measured, for example, using a GPC apparatus (EcoSEC, HLC-8320GPC, manufactured by Tosoh Corporation) and a GPC column (Shodex (registered trademark), KF-803L, KF-802, and KF-801, manufactured by Showa Denko K.K.), setting the column temperature to 40° C., using tetrahydrofuran as an eluent (elution solvent), setting the flow rate (flow velocity) to 1.0 mL / min, and using polystyrene (manufactured by Sigma-Aldrich Co.) as a standard sample.
[0048] The polyorganosiloxane (a1) and polyorganosiloxane (a2) contained in the adhesive composition react with each other by hydrosilylation to form a cured film, and the curing mechanism is therefore different from that via, for example, silanol groups, and therefore neither siloxane needs to contain a silanol group or a functional group capable of forming a silanol group by hydrolysis, such as an alkyloxy group.
[0049] Component (A) contains a platinum group metal catalyst (A2). Such a platinum-based metal catalyst is a catalyst for promoting the hydrosilylation reaction between the alkenyl groups of the polyorganosiloxane (a1) and the Si-H groups of the polyorganosiloxane (a2).
[0050] Specific examples of platinum-based metal catalysts include platinum black, platinic chloride, chloroplatinic acid, a reaction product of chloroplatinic acid with a monohydric alcohol, a complex of chloroplatinic acid with an olefin, platinum bisacetoacetate, and other platinum-based catalysts, but are not limited to these. An example of a complex of platinum with an olefin is, but is not limited to, a complex of divinyltetramethyldisiloxane with platinum.
[0051] The amount of the platinum group metal catalyst (A2) is usually in the range of 1.0 to 50.0 ppm based on the total amount of the polyorganosiloxane (a1) and the polyorganosiloxane (a2).
[0052] Component (A) may contain a polymerization inhibitor (A3). In other words, by including a polymerization inhibitor in the adhesive composition, it becomes possible to suitably control the curing caused by heating during lamination, and it is possible to reproducibly obtain an adhesive composition that gives an adhesive layer with excellent adhesion and peelability.
[0053] The polymerization inhibitor is not particularly limited as long as it can inhibit the progress of the hydrosilylation reaction. Specific examples include, but are not limited to, alkynylalkyl alcohols which may be substituted with an aryl group, such as 1-ethynyl-1-cyclohexanol and 1,1-diphenyl-2-propyn-1-ol.
[0054] The amount of the polymerization inhibitor is usually 1000.0 ppm or more based on the polyorganosiloxane (a1) and the polyorganosiloxane (a2) from the viewpoint of obtaining the effect thereof, and is 10000.0 ppm or less from the viewpoint of preventing excessive inhibition of the hydrosilylation reaction.
[0055] The adhesive composition may contain at least one component (B) selected from the group consisting of a component containing an epoxy-modified polyorganosiloxane, a component containing a methyl group-containing polyorganosiloxane, and a component containing a phenyl group-containing polyorganosiloxane. By including such a component (B) in the adhesive composition, the resulting adhesive layer can be peeled off with good reproducibility.
[0056] Examples of epoxy-modified polyorganosiloxane include R 210 R 220 SiO 2 / 2 The siloxane unit (D 200 units), preferably R 11 R 12 SiO 2 / 2 The siloxane unit (D 10 Examples include those containing the unit.
[0057] R 11 is a group bonded to a silicon atom and represents an alkyl group; R 12 is a group bonded to a silicon atom, and represents an epoxy group or an organic group containing an epoxy group. Specific examples of the alkyl group include those listed above.
[0058] Furthermore, the epoxy group in the organic group containing an epoxy group may be an independent epoxy group that is not condensed with other rings, or may be an epoxy group that forms a condensed ring with other rings, such as a 1,2-epoxycyclohexyl group.
[0059] Specific examples of organic groups containing an epoxy group include, but are not limited to, 3-glycidoxypropyl and 2-(3,4-epoxycyclohexyl)ethyl. In the present invention, a preferred example of the epoxy-modified polyorganosiloxane is epoxy-modified polydimethylsiloxane, but is not limited thereto.
[0060] The epoxy-modified polyorganosiloxane is a polyorganosiloxane having the above-mentioned siloxane unit (D 10 D 10 In addition to the units, the above Q units, M units and / or T units may be included.
[0061] In a preferred embodiment, specific examples of the epoxy-modified polyorganosiloxane include D 10 Polyorganosiloxane consisting of only units, D 10 Polyorganosiloxanes containing D units and Q units; 10 Polyorganosiloxanes containing D units and M units; 10 Polyorganosiloxanes containing D units and T units; 10 Polyorganosiloxanes containing units, Q units and M units, D 10 Polyorganosiloxanes containing units, M units and T units, D 10 and polyorganosiloxanes containing Q units, M units and T units.
[0062] The epoxy-modified polyorganosiloxane is preferably an epoxy-modified polydimethylsiloxane having an epoxy value of 0.1 to 5. The weight average molecular weight is usually 1,500 to 500,000, but from the viewpoint of suppressing precipitation in the adhesive composition, it is preferably 100,000 or less.
[0063] Specific examples of epoxy-modified polyorganosiloxanes include CMS-227 (manufactured by Gelest Co., Ltd., weight average molecular weight 27,000) represented by formula (A-1), ECMS-327 (manufactured by Gelest Co., Ltd., weight average molecular weight 28,800) represented by formula (A-2), KF-101 (manufactured by Shin-Etsu Chemical Co., Ltd., weight average molecular weight 31,800) represented by formula (A-3), and KF-1001 (manufactured by Shin-Etsu Chemical Co., Ltd., weight average molecular weight 55,600) represented by formula (A-4). Examples of the polyimide copolymer include, but are not limited to, trade name KF-1005 (manufactured by Shin-Etsu Chemical Co., Ltd., weight average molecular weight 11,500) represented by formula (A-5), trade name X-22-343 (manufactured by Shin-Etsu Chemical Co., Ltd., weight average molecular weight 2,400) represented by formula (A-6), trade name BY16-839 (manufactured by Dow Corning Corporation, weight average molecular weight 51,700) represented by formula (A-7), and trade name ECMS-327 (manufactured by Gelest Pharmaceuticals, weight average molecular weight 28,800) represented by formula (A-8).
[0064] [ka] (m and n are the numbers of repeating units.)
[0065] [ka] (m and n are the numbers of repeating units.)
[0066] [ka] (m and n are the numbers of repeating units, and R is an alkylene group having 1 to 10 carbon atoms.)
[0067] [ka] (m and n are the numbers of repeating units, and R is an alkylene group having 1 to 10 carbon atoms.)
[0068] [ka] (m, n, and o are the numbers of repeating units, and R is an alkylene group having 1 to 10 carbon atoms.)
[0069] [ka] (m and n are the numbers of repeating units, and R is an alkylene group having 1 to 10 carbon atoms.)
[0070] [ka] (m and n are the numbers of repeating units, and R is an alkylene group having 1 to 10 carbon atoms.)
[0071] [ka] (m and n are the numbers of repeating units.)
[0072] Examples of the methyl group-containing polyorganosiloxane include R 210 R 220 SiO 2 / 2 The siloxane unit (D 200 units), preferably R 21 R 21 SiO 2 / 2 The siloxane unit (D 20 Examples include those containing the unit.
[0073] R 210 and R 220 are groups bonded to a silicon atom, and each independently represents an alkyl group, with at least one being a methyl group. Specific examples of the alkyl group include those listed above. R 21 is a group bonded to a silicon atom, and represents an alkyl group. Specific examples of the alkyl group include those listed above. 21 As the alkyl group, a methyl group is preferable. A preferred example of the methyl group-containing polyorganosiloxane is polydimethylsiloxane, but is not limited thereto.
[0074] The methyl group-containing polyorganosiloxane is a polyorganosiloxane having the above-mentioned siloxane unit (D 200 Unit or D 20 D 200 Units and D 20 In addition to the units, the above Q units, M units and / or T units may be included.
[0075] In one embodiment, specific examples of the methyl group-containing polyorganosiloxane include D 200 Polyorganosiloxane consisting of only units, D 200 Polyorganosiloxanes containing D units and Q units; 200 Polyorganosiloxanes containing D units and M units; 200 Polyorganosiloxanes containing D units and T units; 200 Polyorganosiloxanes containing units, Q units and M units, D 200 Polyorganosiloxanes containing units, M units and T units, D 200 Examples of suitable polyorganosiloxanes include polyorganosiloxanes containing Q, M, and T units. In a preferred embodiment, specific examples of the methyl group-containing polyorganosiloxane include D 20 Polyorganosiloxane consisting of only units, D 20 Polyorganosiloxanes containing D units and Q units; 20 Polyorganosiloxanes containing D units and M units; 20 Polyorganosiloxanes containing D units and T units; 20 Polyorganosiloxanes containing units, Q units and M units, D 20 Polyorganosiloxanes containing units, M units and T units, D 20 Examples of suitable polyorganosiloxanes include polyorganosiloxanes containing Q, M, and T units.
[0076] The viscosity of methyl group-containing polyorganosiloxane is usually 1,000 to 2,000,000 mm2 / s, but preferably 10,000 to 1,000,000 mm 2 / s. The methyl group-containing polyorganosiloxane is typically a dimethyl silicone oil made of polydimethylsiloxane. This viscosity value is indicated as a kinetic viscosity, and is expressed as centistokes (cSt) = mm 2 / s. Kinematic viscosity can be measured with a kinematic viscometer. Viscosity (mPa s) can also be converted to density (g / cm 3 It can also be calculated by dividing by the viscosity (mm 2 / s)=viscosity (mPa s) / density (g / cm 3 ) can be calculated from the formula:
[0077] Specific examples of methyl group-containing polyorganosiloxanes include WACKER (registered trademark SILICONE FLUID AK series) manufactured by Wacker GmbH, dimethyl silicone oils (KF-96L, KF-96A, KF-96, KF-96H, KF-69, KF-965, KF-968) manufactured by Shin-Etsu Chemical Co., Ltd., and cyclic dimethyl silicone oil (KF-995), but are not limited to these.
[0078] Examples of the phenyl group-containing polyorganosiloxane include R 31 R 32 SiO 2 / 2 The siloxane unit (D 30 Examples include those containing the unit.
[0079] R 31 is a group bonded to a silicon atom and represents a phenyl group or an alkyl group; R 32 is a group bonded to a silicon atom and represents a phenyl group. Specific examples of the alkyl group include those listed above, with a methyl group being preferred.
[0080] The phenyl group-containing polyorganosiloxane is a polyorganosiloxane having the above-mentioned siloxane unit (D 30 D 30In addition to the units, the above Q units, M units and / or T units may be included.
[0081] In a preferred embodiment, specific examples of the phenyl group-containing polyorganosiloxane include D 30 Polyorganosiloxane consisting of only units, D 30 Polyorganosiloxanes containing D units and Q units; 30 Polyorganosiloxanes containing D units and M units; 30 Polyorganosiloxanes containing D units and T units; 30 Polyorganosiloxanes containing units, Q units and M units, D 30 Polyorganosiloxanes containing units, M units and T units, D 30 Examples of suitable polyorganosiloxanes include polyorganosiloxanes containing Q, M, and T units.
[0082] The weight average molecular weight of the phenyl group-containing polyorganosiloxane is usually 1,500 to 500,000, but from the viewpoint of inhibiting precipitation in the adhesive composition, it is preferably 100,000 or less.
[0083] A specific example of the phenyl group-containing polyorganosiloxane is PMM-1043 (trade name, manufactured by Gelest, Inc., weight average molecular weight 67,000, viscosity 30,000 mm), represented by formula (C-1). 2 / s), and PMM-1025 (trade name, manufactured by Gelest, Inc., weight average molecular weight 25,200, viscosity 500 mm 2 / s), the trade name KF50-3000CS (manufactured by Shin-Etsu Chemical Co., Ltd., weight average molecular weight 39,400, viscosity 3000 mm 2 / s), and the product name TSF431 (manufactured by MOMENTIVE Co., Ltd., weight average molecular weight 1,800, viscosity 100 mm 2 / s), and the product name TSF433 (manufactured by MOMENTIVE, weight average molecular weight 3,000, viscosity 450 mm 2 / s), and PDM-0421 (trade name, manufactured by Gelest, Inc., weight average molecular weight 6,200, viscosity 100 mm2 / s), and PDM-0821 (manufactured by Gelest, Inc., weight average molecular weight 8,600, viscosity 125 mm 2 / s), but are not limited to these.
[0084] [ka] (m and n represent the number of repeating units.)
[0085] [ka] (m and n represent the number of repeating units.)
[0086] [ka] (m and n represent the number of repeating units.)
[0087] [ka] (m and n represent the number of repeating units.)
[0088] [ka] (m and n represent the number of repeating units.)
[0089] [ka] (m and n represent the number of repeating units.)
[0090] [ka] (m and n represent the number of repeating units.)
[0091] The polysiloxane-based adhesive composition may contain component (A) and component (B) in any ratio. Taking into consideration the balance between adhesion and releasability, the ratio of component (A) to component (B) by mass is preferably 99.995:0.005 to 30:70, and more preferably 99.9:0.1 to 75:25.
[0092] Such an adhesive composition may contain a solvent for the purpose of adjusting the viscosity, etc., and specific examples of the solvent include, but are not limited to, aliphatic hydrocarbons, aromatic hydrocarbons, ketones, etc.
[0093] More specifically, examples of the solvent include, but are not limited to, hexane, heptane, octane, nonane, decane, undecane, dodecane, isododecane, menthane, limonene, toluene, xylene, mesitylene, cumene, MIBK (methyl isobutyl ketone), butyl acetate, diisobutyl ketone, 2-octanone, 2-nonanone, 5-nonanone, etc. Such solvents may be used alone or in combination of two or more.
[0094] When such an adhesive composition contains a solvent, the content of the solvent is appropriately set taking into consideration the desired viscosity of the adhesive composition, the coating method to be used, the thickness of the thin film to be produced, etc., but is in the range of about 10 to 90 mass % of the entire adhesive composition.
[0095] The viscosity of the adhesive composition at 25° C. is usually 500 to 20,000 mPa s, and preferably 1,000 to 5,000 mPa s, and can be adjusted by changing the types of organic solvents used, their ratios, the concentrations of the film-constituting components, etc., taking into consideration various factors such as the coating method used and the desired film thickness. Here, film-constituting components refer to components other than the solvent.
[0096] The adhesive composition used in the present invention can be produced by mixing the membrane constituent components and a solvent. However, when the solvent is not included, the adhesive composition used in the present invention can be produced by mixing the membrane constituent components.
[0097] Specifically, the first step includes a pre-step of applying the adhesive composition to the surface of a semiconductor substrate or a support substrate to form an adhesive coating layer, and a post-step of bonding the semiconductor substrate and the support substrate via the adhesive coating layer, applying a load in the thickness direction of the semiconductor substrate and the support substrate while performing at least one of a heat treatment and a decompression treatment, thereby bonding the semiconductor substrate, the adhesive coating layer, and the support substrate, and then performing a post-heat treatment. The post-heat treatment in the post-step finally cures the adhesive coating layer appropriately to become an adhesive layer, and a laminate is produced.
[0098] Here, for example, the semiconductor substrate is a wafer and the support substrate is a support body, and the adhesive composition may be applied to either or both of the semiconductor substrate and the support substrate. Examples of the wafer include, but are not limited to, silicon wafers and glass wafers having a diameter of about 300 mm and a thickness of about 770 μm. The support (carrier) is not particularly limited, but may be, for example, a silicon wafer having a diameter of about 300 mm and a thickness of about 700 μm, but is not limited thereto.
[0099] The thickness of the adhesive coating layer is usually 5 to 500 μm, but from the viewpoint of maintaining the film strength, it is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more, and from the viewpoint of avoiding non-uniformity due to a thick film, it is preferably 200 μm or less, more preferably 150 μm or less, even more preferably 120 μm or less, and even more preferably 70 μm or less.
[0100] The coating method is not particularly limited, but is usually a spin coating method. Note that a method of forming a coating film by a separate spin coating method or the like and attaching a sheet-like coating film may also be adopted, and this method is also referred to as coating or coating film.
[0101] The temperature of the heat treatment is usually 80° C. or higher, and from the viewpoint of preventing excessive curing, preferably from 150° C. or lower. The time of the heat treatment is usually 30 seconds or more, preferably 1 minute or more, from the viewpoint of ensuring the expression of temporary adhesive ability, but is usually 10 minutes or less, preferably 5 minutes or less, from the viewpoint of suppressing deterioration of the adhesive layer and other members.
[0102] The reduced pressure treatment can be carried out by exposing the two substrates and the adhesive coating layer therebetween to an atmospheric pressure of 10 to 10,000 Pa. The reduced pressure treatment time is usually 1 to 30 minutes.
[0103] In a preferred embodiment of the invention, the two substrates and the layer therebetween are laminated together, preferably by heat treatment, more preferably by a combination of heat treatment and reduced pressure treatment.
[0104] The load in the thickness direction of the semiconductor substrate and the support substrate is not particularly limited as long as it does not adversely affect the semiconductor substrate, the support substrate, and the layers therebetween and can firmly adhere to them, but is usually within the range of 10 to 1,000 N.
[0105] The post-heating temperature is preferably 120° C. or higher from the viewpoint of obtaining a sufficient curing speed, and is preferably 260° C. or lower from the viewpoint of preventing deterioration of the substrate and adhesive. The heating time is usually 1 minute or more from the viewpoint of realizing suitable bonding of the wafer by curing, and preferably 5 minutes or more from the viewpoint of stabilizing the physical properties of the adhesive, and is usually 180 minutes or less, preferably 120 minutes or less from the viewpoint of avoiding adverse effects on the adhesive layer due to excessive heating. Heating can be performed using a hot plate, an oven, or the like. One purpose of the post-heating treatment is to more suitably cure the component (A).
[0106] Next, a second step of processing the semiconductor substrate of the stack obtained by the method described above will be described. An example of the processing applied to the laminate used in the present invention is processing of the back surface opposite to the circuit surface of the semiconductor substrate, typically thinning the wafer by polishing the back surface of the wafer. Using such a thinned wafer, through-silicon vias (TSVs) and the like are formed, and then the thinned wafer is peeled off from the support to form a wafer stack, which is then three-dimensionally mounted. In addition, before and after that, wafer back electrodes and the like are also formed. During the wafer thinning and TSV process, heat of 250 to 350°C is applied while the wafer is attached to the support, and the adhesive layer contained in the laminate used in the present invention has heat resistance against that heat. For example, a wafer with a diameter of 300 mm and a thickness of about 770 μm can be thinned to a thickness of about 80 μm to 4 μm by polishing the back surface opposite the front circuit surface.
[0107] Next, a third step of peeling off the semiconductor substrate made of the semiconductor substrate after processing will be described. The method for peeling the laminate used in the present invention includes, but is not limited to, solvent peeling, laser peeling, mechanical peeling using a tool having a sharp part, peeling between a support and a wafer, etc. Peeling is usually performed after processing such as thinning. In the third step, the adhesive is not necessarily completely attached to the supporting substrate and peeled off, and some of the adhesive may be left behind on the processed substrate. Therefore, in the fourth step, the surface of the substrate to which the remaining adhesive is attached is cleaned with the above-mentioned cleaning composition of the present invention, whereby the adhesive on the substrate can be sufficiently cleaned and removed.
[0108] Finally, the fourth step of cleaning and removing adhesive residue remaining on the peeled semiconductor substrate with a cleaning composition will be described. The fourth step is a step of cleaning and removing adhesive residue remaining on the substrate after peeling with the cleaning composition of the present invention. Specifically, for example, the thinned substrate on which adhesive remains is immersed in the cleaning composition of the present invention, and, if necessary, ultrasonic cleaning or other means are also used to clean and remove the adhesive residue. When ultrasonic cleaning is used, the conditions are appropriately determined taking into consideration the state of the surface of the substrate, but usually, adhesive residue remaining on the substrate can be sufficiently removed by cleaning at 20 kHz to 5 MHz for 10 seconds to 30 minutes.
[0109] The method for producing a thinned substrate of the present invention includes the above-mentioned steps 1 to 4, but may also include steps other than these. For example, in step 4, before cleaning with the cleaning composition of the present invention, adhesive residues may be removed by immersing the substrate in various solvents or by tape peeling, as necessary.
[0110] Moreover, the above-mentioned constituent elements and methodological elements relating to the first to fourth steps may be modified in various ways without departing from the gist of the present invention. EXAMPLES
[0111] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The following apparatuses were used in the present invention. (1) Agitator (rotating / revolving mixer): Thinky Corporation Rotating / revolving mixer ARE-500 (2) Viscometer: Rotational viscometer TVE-22H manufactured by Toki Sangyo Co., Ltd. (3) Agitator: AS ONE Mix Rotor Variable 1-1186-12 (4) Mixer H: AS ONE heated rocking mixer HRM-1 (5) Contact-type film thickness meter: Tokyo Seimitsu Co., Ltd. Wafer thickness measuring device WT-425
[0112] [1] Preparation of adhesive composition [Preparation Example 1] A 600 mL stirring vessel dedicated to the planetary centrifugal mixer was charged with 150 g of a base polymer (manufactured by Wacker Chemical Industries, Ltd.) consisting of a vinyl-containing linear polydimethylsiloxane and a vinyl-containing MQ resin with a viscosity of 200 mPa s as (a1), 15.81 g of a SiH-containing linear polydimethylsiloxane with a viscosity of 100 mPa s as (a2), and 0.17 g of 1-ethynyl-1-cyclohexanol (manufactured by Wacker Chemical Industries, Ltd.) as (A3), and the mixture was stirred for 5 minutes with the planetary centrifugal mixer. To the resulting mixture, 0.33 g of platinum catalyst (A2) (manufactured by Wacker Chemical Co.) and 9.98 g of vinyl-containing linear polydimethylsiloxane (a1) with a viscosity of 1000 mPa·s (manufactured by Wacker Chemical Co.) were added in a 50 mL screw tube, and 0.52 g of the mixture obtained by stirring for 5 minutes in a planetary centrifugal mixer was added. The mixture was stirred for 5 minutes in a planetary centrifugal mixer, and the resulting mixture was filtered through a 300 mesh nylon filter to obtain an adhesive composition. The viscosity of the adhesive composition measured using a rotational viscometer was 9900 mPa·s.
[0113] [Preparation Example 2] To a 600 mL stirring vessel dedicated to the planetary centrifugal mixer, 95 g of vinyl group-containing MQ resin (manufactured by Wacker Chemie) as (a1), 93.4 g of p-menthane (manufactured by Nippon Terpene Chemical Co., Ltd.) as a solvent, and 0.41 g of 1,1-diphenyl-2-propyn-1-ol (manufactured by Tokyo Chemical Industry Co., Ltd.) were added, and the mixture was stirred for 5 minutes with the planetary centrifugal mixer. The mixture thus obtained was mixed with 29.5 g of a linear polydimethylsiloxane containing a SiH group and having a viscosity of 100 mPa·s (manufactured by Wacker Chemical Co.) as (a2), 29.5 g of a linear polydimethylsiloxane containing a vinyl group and having a viscosity of 200 mPa·s (manufactured by Wacker Chemical Co.) as (a1), and 100 g of a linear polydimethylsiloxane containing a vinyl group and having a viscosity of 1,000,000 mm 2 To the mixture were added 0.41 g of a polyorganosiloxane (manufactured by Wacker Chemical Industries, trade name AK1000000) having a molecular weight of 100 / s and 0.41 g of 1-ethynyl-1-cyclohexanol (manufactured by Wacker Chemical Industries, Ltd.) as (A3), and the mixture was stirred for an additional 5 minutes using a planetary centrifugal mixer. Then, 14.9 g of a mixture obtained by stirring 0.20 g of platinum catalyst (A2) (manufactured by Wacker Chem.) and 17.7 g of vinyl-containing linear polydimethylsiloxane (a1) with a viscosity of 1000 mPa·s (manufactured by Wacker Chem.) separately for 5 minutes in a 50 mL screw tube was added to the mixture, which was further stirred for 5 minutes in the planetary mixer. The mixture was filtered through a 300 mesh nylon filter to obtain an adhesive composition. The viscosity of the adhesive composition measured using a rotational viscometer was 4600 mPa·s.
[0114] [2] Preparation of cleaning composition [ test Example 1] A mixed solvent of 47.5 g of N-methyl-2-pyrrolidone dehydrate (manufactured by Kanto Chemical Co., Ltd.) and 47.5 g of 1,2-diethoxyethane (manufactured by Tokyo Chemical Industry Co., Ltd.) was added to 5 g of tetrabutylammonium fluoride trihydrate (manufactured by Kanto Chemical Co., Ltd.) as a solvent, and the resulting mixture was stirred to obtain a cleaning composition.
[0115] [ test Example 2] The amount of N-methyl-2-pyrrolidone dehydrate was changed to 33 g, and the amount of 1,2-diethoxyethane was changed to 62 g. test A cleaning composition was obtained in the same manner as in Example 1.
[0116] [ test Example 3] The amount of N-methyl-2-pyrrolidone dehydrate was changed to 38 g, and the amount of 1,2-diethoxyethane was changed to 57 g. test A cleaning composition was obtained in the same manner as in Example 1.
[0117] [ test Example 4] The amount of N-methyl-2-pyrrolidone dehydrate was 43 g, and the amount of 1,2-diethoxyethane was 52 g. test A cleaning composition was obtained in the same manner as in Example 1.
[0118] [ test example 5 ] To 5 g of tetrabutylammonium fluoride trihydrate was added 95 g of dehydrated N-methyl-2-pyrrolidone, and the resulting mixture was stirred to obtain a cleaning composition.
[0119] [ test example 6 ] Except for using diethylene glycol diethyl ether (Tokyo Chemical Industry Co., Ltd.) instead of 1,2-diethoxyethane, test A cleaning composition was obtained in the same manner as in Example 1.
[0120] [ test example 7 ] Except for using diethylene glycol dibutyl ether (Tokyo Chemical Industry Co., Ltd.) instead of 1,2-diethoxyethane, test A cleaning composition was obtained in the same manner as in Example 1.
[0121] [ test example 8 ] test Except for using 95 g of 1,2-diethoxyethane instead of the mixed solvent used in Example 1, test An attempt was made to prepare a cleaning composition in the same manner as in Example 1, but tetrabutylammonium fluoride trihydrate remained undissolved.
[0122] [ test example 9 ] A commercially available silicone cleaner "KSR-1" (manufactured by Kanto Chemical Co., Ltd.) was used as the cleaning liquid composition.
[0123] [3] Performance evaluation of cleaning agent compositions A good cleaning composition needs to have a high cleaning speed that dissolves adhesive residues immediately after contact with them, and good cleaning power to maintain that speed, so the following evaluations were carried out. By combining a higher cleaning speed with good cleaning power, more effective cleaning can be expected. [3-1] Etching rate measurement The etching rate was measured to measure the cleaning speed of the obtained cleaning composition. The adhesive composition obtained in Preparation Example 1 was applied to a 12-inch silicon wafer with a spin coater to a thickness of 100 μm, and cured at 150° C. / 15 minutes and 190° C. / 10 minutes. The wafer after the film formation was cut into chips of 4 cm square, and the film thickness was measured using a contact film thickness meter. The chip was then placed in a stainless steel petri dish with a diameter of 9 cm, 7 mL of the obtained cleaning composition was added, and the dish was covered, and then the dish was placed on a stirrer H and stirred and washed at 23° C. for 5 minutes. After washing, the chip was taken out, washed with isopropanol and pure water, and dry baked at 150° C. for 1 minute, and the film thickness was measured again with a contact film thickness meter. The film thickness reduction was measured before and after washing, and the etching rate [μm / min] was calculated by dividing the reduction by the washing time, which was used as an index of cleaning power. The results are shown in Table 1.
[0125] [Table 1]
[0126] As shown in Table 1, the cleaning composition of the present invention containing an alkylene glycol dialkyl ether (1,2-diethoxyethane) and a specific lactam compound (N-methyl-2-pyrrolidone) was more effective than the cleaning composition containing only a lactam compound (N-methyl-2-pyrrolidone) as a solvent ( test example 5 ) or cleaning compositions containing structurally similar glycol compounds as solvents ( test example 6 ~ 7 ), it showed a higher etching rate and excellent cleaning power durability (good solubility).
[0127] [3-3] Evaluation of corrosiveness test A silicon wafer was immersed in each of the cleaning compositions obtained in Examples 1 to 4 for 5 minutes. As a result, no corrosion of the silicon wafer was observed in any of the compositions.
Claims
1. A cleaning composition used for removing a polysiloxane-based adhesive remaining on a substrate, the polysiloxane-based adhesive comprising a component (A) that cures by a hydrosilylation reaction, The component (A) is SiO 2 Siloxane units (Q units) represented by the formula: R 1 R 2 R 3 SiO 1/2 Siloxane units (M units) represented by the formula: R 4 R 5 SiO 2/2 Siloxane units (D units) represented by the formula: 6 SiO 3/2 Polysiloxane (A1) containing one or more units selected from the group consisting of siloxane units (T units) represented by the following formula: 1 ~R 6 are groups or atoms bonded to a silicon atom, and each independently represents an alkyl group, an alkenyl group, or a hydrogen atom, A cleaning composition comprising a tetra(hydrocarbon)ammonium fluoride and a solvent consisting of only an organic solvent, the organic solvent containing a lactam compound represented by formula (1) and further containing a glycol compound. 【Chemistry 1】 (In the formula, R 101 represents an alkyl group having 1 to 6 carbon atoms; R 102 represents an alkylene group having 1 to 6 carbon atoms.
2. 2. The cleaning composition according to claim 1, wherein the lactam compound comprises at least one selected from the group consisting of N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone.
3. 3. The cleaning composition according to claim 1, wherein the tetra(hydrocarbon)ammonium fluoride comprises at least one selected from the group consisting of tetramethylammonium fluoride, tetraethylammonium fluoride, tetrapropylammonium fluoride and tetrabutylammonium fluoride.
4. The cleaning composition according to any one of claims 1 to 3, wherein the organic solvent further comprises an alkylene glycol dialkyl ether.
5. 5. The cleaning agent composition according to claim 4, wherein the alkylene glycol dialkyl ether comprises at least one selected from ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dipropyl ethane, ethylene glycol dibutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, and propylene glycol dipropyl ether.
6. 6. The cleaning composition according to claim 4, wherein the ratio of the alkylene glycol dialkyl ether to the lactam compound is, in terms of mass ratio, alkylene glycol dialkyl ether:lactam compound=30:70 to 80:
20.
7. The cleaning composition according to any one of claims 1 to 6, wherein the organic solvent further comprises diethylene glycol diethyl ether or diethylene glycol dibutyl ether.
8. The cleaning composition according to any one of claims 1 to 7, wherein the cleaning rate of the cleaning composition is 5.0 [µm / min] or more, and the cleaning rate is determined as follows. (Cleaning speed) At room temperature (23° C.), an adhesive layer obtained from the adhesive composition is brought into contact with the cleaning composition for 5 minutes, and the reduction in film thickness is measured before and after the contact. The etching rate [μm / min] calculated by dividing the reduction by the cleaning time is defined as the cleaning speed.
9. A cleaning method comprising removing adhesive residue remaining on a substrate by using the cleaning composition according to any one of claims 1 to 8.
10. A first step of producing a laminate including a semiconductor substrate, a support substrate, and an adhesive layer obtained from an adhesive composition; A second step of processing the semiconductor substrate of the obtained laminate; A third step of peeling off the semiconductor substrate after processing; and A fourth step of cleaning and removing adhesive residue remaining on the peeled semiconductor substrate with a cleaning composition. A method for manufacturing a processed semiconductor substrate, comprising: A method for producing a processed semiconductor substrate, comprising using the cleaning composition according to any one of claims 1 to 8 as the cleaning composition.
11. A method for producing a cleaning composition used to remove a polysiloxane-based adhesive remaining on a substrate, the method comprising the steps of: mixing, under an inert gas, tetra(hydrocarbon)ammonium fluoride with a solvent consisting essentially of an organic solvent; and wherein the organic solvent contains a lactam compound represented by formula (1) and further contains a glycol compound. 【Chemistry 2】 (In the formula, R 101 represents an alkyl group having 1 to 6 carbon atoms; R 102 represents an alkylene group having 1 to 6 carbon atoms.
12. The method for producing a cleaning composition according to claim 11, wherein the organic solvent comprises an alkylene glycol dialkyl ether.
13. The method for producing a cleaning composition according to claim 11 or 12, wherein the organic solvent comprises diethylene glycol diethyl ether or diethylene glycol dibutyl ether.
14. The method for producing the cleaning composition according to any one of claims 11 to 13, wherein the cleaning rate of the cleaning composition is 5.0 [µm / min] or more, and the cleaning rate is determined as follows. (Cleaning speed) At room temperature (23° C.), an adhesive layer obtained from the adhesive composition is brought into contact with the cleaning composition for 5 minutes, and the reduction in film thickness is measured before and after the contact. The etching rate [μm / min] calculated by dividing the reduction by the cleaning time is defined as the cleaning speed.
15. A cleaning composition used for removing a polysiloxane-based adhesive remaining on a substrate, the polysiloxane-based adhesive comprising: a component (A) that cures by a hydrosilylation reaction; and a component (B) that contains a methyl group-containing polyorganosiloxane; The component (A) is SiO 2 Siloxane units (Q units) represented by the formula: R 1 R 2 R 3 SiO 1/2 Siloxane units (M units) represented by the formula: R 4 R 5 SiO 2/2 Siloxane units (D units) represented by the formula: 6 SiO 3/2 Polysiloxane (A1) containing one or more units selected from the group consisting of siloxane units (T units) represented by the following formula: 1 ~R 6 are groups or atoms bonded to a silicon atom, and each independently represents an alkyl group, an alkenyl group, or a hydrogen atom, A cleaning composition comprising a tetra(hydrocarbon)ammonium fluoride and a solvent consisting of only an organic solvent, the organic solvent containing a lactam compound represented by formula (1) and further containing a glycol compound. 【Chemistry 3】 (In the formula, R 101 represents an alkyl group having 1 to 6 carbon atoms; R 102 represents an alkylene group having 1 to 6 carbon atoms.
Citation Information
Patent Citations
Method for producing polar polymer and organic silicon compound
JP2008274214A
Silicone solubilizer
JP2015505886A
Composition for removing silicone polymer and manufacturing method of thin film substrate using the same
KR1020160087089A
Composition for removing silicone resins and method of thinning substrate by using the same
US20170158888A1
Cured polymers dissolving compositions
US6818608B2