Adhesive and antenna device
The adhesive with metal particles addresses the challenge of maintaining precise air cavity gaps in antenna devices, improving communication speed and quality by ensuring minimal gap and strength changes during repeated heating.
Patent Information
- Application Number
- JP2020556996
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-19
- Filing Date
- 2020-09-08
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-09-08
AI Technical Summary
Conventional antenna devices fail to maintain high communication speed and quality due to the inability to control the gap between air cavities within the antenna with precision, especially when subjected to repeated heating during manufacturing processes.
An adhesive comprising metal particles is used to bond substrates, ensuring a gap change rate of 10% or less and a gap-to-particle diameter ratio of 0.70 to 0.97, maintaining adhesive strength change at 10% or less, thereby controlling the air cavity gap with high precision even under repeated heating.
The adhesive enables precise control of air cavity gaps, enhancing communication speed and quality in antenna devices by maintaining consistent gap distances and adhesive strength, even after multiple heating cycles.
Smart Images

Figure 0007583613000002 
Figure 0007583613000003 
Figure 0007583613000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive for bonding two substrates, and also to an antenna device using the adhesive. [Background technology]
[0002] Various adhesives are used to bond two adherends together. In addition, spacers such as gap materials are sometimes mixed into the adhesive to make the thickness of the adhesive layer formed by the adhesive uniform and to control the distance (gap) between the two adherends.
[0003] In recent years, the rapid spread of smartphones, tablet devices, etc. has led to a surge in traffic, which has become an issue. For this reason, the 5th generation mobile communication system (5G) is being studied as a successor to communication systems such as LTE (Long Term Evolution) and LTE-A (LTE-Advanced) by the Third Generation Partnership Project (3GPP), as well as a new wireless communication system.
[0004] For example, in the fifth generation mobile communication system (5G), in order to realize high-speed transmission using a wider band, it is being considered to communicate using a higher carrier frequency compared to LTE and LTE-A. However, when communicating at a high carrier frequency, there is a possibility that a conventional antenna device cannot fully demonstrate its performance. A conventional antenna device is disclosed, for example, in Patent Document 1 below.
[0005] The following Patent Document 1 discloses an antenna device including an antenna and a multilayer high-frequency substrate. The antenna has a power supply conductor on the back surface. The multilayer high-frequency substrate is configured by stacking a plurality of strip lines with lands on the front surface. The lands are electrically connected to the strip conductors via through holes. In the multilayer high-frequency substrate, the lands of the stacked strip lines are bonded together with an anisotropic conductive adhesive. In the antenna device, the power supply conductor of the antenna and the lands on the front surface of the multilayer high-frequency substrate are bonded together with an anisotropic conductive adhesive. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-185550 A Summary of the Invention [Problem to be solved by the invention]
[0007] For the fifth generation mobile communication system (5G), antennas for base stations and terminals are required to have improved communication speeds and communication quality. In order to achieve these improvements, the provision of an air cavity (space) within the antenna is being considered. By providing an air cavity (space) within the antenna, it is possible to improve the bandwidth and reduce electromagnetic noise. As a result, it is possible to improve the communication speed and communication quality of the antenna.
[0008] In conventional antenna devices, high levels of communication speed and quality are not required, and an air cavity (space) may not be provided in the antenna. The air cavity (space) is formed, for example, by keeping the distance (gap) between the high-frequency board and the board constituting the antenna uniform and constant. In order to improve the communication speed and quality of the antenna, it is required to control the distance (gap) of the air cavity (space) with high precision.
[0009] In addition, when an antenna device is obtained by bonding two substrates with an adhesive to form an air cavity (space) in the antenna, the antenna device may be repeatedly heated. When the antenna device is repeatedly heated, the gap of the air cavity (space) cannot be controlled with high precision, and it may be difficult to improve the communication speed and communication quality of the antenna.
[0010] An object of the present invention is to provide an adhesive that can control the gap of the air cavity with high precision even when repeatedly heated, and to provide an antenna device using the adhesive. [Means for solving the problem]
[0011] According to a broad aspect of the present invention, there is provided an adhesive for bonding a first metal portion and a second metal portion in a first substrate having a first metal portion on its surface and a second substrate having a second metal portion on its surface, wherein the adhesive has a rate of change in the gap between the substrates calculated by evaluation test 1a described below of 10% or less.
[0012] Evaluation test 1a: A first substrate having a first metal part on its surface, a second substrate having a second metal part on its surface, and an adhesive are prepared. The adhesive is placed on the first metal part of the first substrate, and the second substrate is placed on the surface of the adhesive opposite to the first substrate side so that the first metal part and the second metal part face each other. Thereafter, the first substrate and the second substrate are bonded together by performing a reflow process under reflow conditions specified in JEDEC J-STD-020 to obtain a laminate. The gap between the substrates of the obtained laminate is measured and defined as the gap before heating. Thereafter, the obtained laminate is subjected to four reflow processes under reflow conditions specified in JEDEC J-STD-020, and the gap between the substrates of the laminate after the reflow process is measured and defined as the gap after heating. The rate of change in the gap is calculated from the gap before and after heating using the following formula (1).
[0013] Gap change rate = [(gap before heating - gap after heating) / gap before heating] x 100 Formula (1)
[0014] In a particular aspect of the adhesive according to the present invention, the adhesive contains metal particles.
[0015] According to a broad aspect of the present invention, there is provided an adhesive for bonding a first metal portion and a second metal portion in a first substrate having a first metal portion on a surface thereof and a second substrate having a second metal portion on a surface thereof, the adhesive containing metal particles, and a ratio of the gap after heating calculated by the evaluation test 1b described below to the average particle diameter of the metal particles is provided that is 0.70 or more and 0.97 or less.
[0016] Assessment Test 1b: A first substrate having a first metal portion on its surface, a second substrate having a second metal portion on its surface, and an adhesive are prepared. The adhesive is placed on the first metal portion of the first substrate, and the second substrate is placed on the surface of the adhesive opposite to the first substrate side such that the first metal portion and the second metal portion face each other. Thereafter, the first substrate and the second substrate are bonded together by performing a reflow process under the reflow conditions specified in JEDEC J-STD-020 to obtain a laminate. The obtained laminate is subjected to a reflow process four times under the reflow conditions specified in JEDEC J-STD-020, and the gap between the substrates of the laminate after the reflow process is measured and defined as the gap after heating.
[0017] In a particular aspect of the adhesive according to the present invention, the metal particles have a base particle and a metal layer disposed on a surface of the base particle.
[0018] In a particular aspect of the adhesive of the present invention, the metal layer has a second metal layer disposed on a surface of the base particle and a first metal layer disposed on a surface of the second metal layer, and the first metal layer is a solder layer.
[0019] In a particular aspect of the adhesive according to the present invention, the rate of change in adhesive strength between the substrates, as calculated by the following Evaluation Test 2, is 10% or less.
[0020] Evaluation test 2: A first substrate having a first metal part on its surface, a second substrate having a second metal part on its surface, and an adhesive are prepared. The adhesive is placed on the first metal part of the first substrate, and the second substrate is placed on the surface of the adhesive opposite to the first substrate side so that the first metal part and the second metal part face each other. Thereafter, the first substrate and the second substrate are bonded together by performing a reflow process under reflow conditions specified in JEDEC J-STD-020 to obtain a laminate. The obtained laminate is used to measure the adhesive strength between the substrates under conditions conforming to MIL STD-883G, which is defined as the adhesive strength before heating. The obtained laminate is then subjected to four reflow processes under reflow conditions specified in JEDEC J-STD-020, and the laminate after the reflow process is used to measure the adhesive strength between the substrates under conditions conforming to MIL STD-883G, which is defined as the adhesive strength after heating. The rate of change in adhesive strength before and after heating is calculated using the following formula (2).
[0021] Rate of change in adhesive strength = [(adhesive strength before heating - adhesive strength after heating) / adhesive strength before heating] x 100 Formula (2)
[0022] In a specific aspect of the adhesive according to the present invention, the first substrate is a glass epoxy substrate or a ceramic substrate, and the second substrate is a glass epoxy substrate, a ceramic substrate, or a silicon substrate.
[0023] In a particular aspect of the adhesive according to the present invention, the first metal portion is formed of copper or formed by nickel / gold plating, and the second metal portion is formed of copper or formed by nickel / gold plating.
[0024] According to a broad aspect of the present invention, there is provided an antenna device comprising a first substrate having a first metal portion on its surface, a second substrate having a second metal portion on its surface, and an adhesive portion bonding the first substrate and the second substrate, wherein the material of the adhesive portion is the adhesive described above, the first metal portion and the second metal portion are bonded by the adhesive portion, and an air cavity is formed by the first substrate, the second substrate, and the adhesive portion.
[0025] In a specific aspect of the antenna device according to the present invention, the first substrate is a glass epoxy substrate or a ceramic substrate, and the second substrate is a glass epoxy substrate, a ceramic substrate, or a silicon substrate.
[0026] In a particular aspect of the antenna device according to the present invention, the first metal portion is formed of copper or formed with nickel / gold plating, and the second metal portion is formed of copper or formed with nickel / gold plating. Effect of the Invention
[0027] The adhesive according to the present invention is an adhesive for bonding a first metal part and a second metal part in a first substrate having a first metal part on its surface and a second substrate having a second metal part on its surface. In the adhesive according to the present invention, the rate of change in the gap between the substrates calculated by the evaluation test 1a is 10% or less. Since the adhesive according to the present invention has the above configuration, the gap of the air cavity can be controlled with high precision even when repeatedly heated.
[0028] The adhesive according to the present invention is an adhesive for bonding a first metal part and a second metal part in a first substrate having a first metal part on a surface thereof and a second substrate having a second metal part on a surface thereof. The adhesive according to the present invention contains metal particles. In the adhesive according to the present invention, the ratio of the gap after heating calculated by the evaluation test 1b to the average particle size of the metal particles is 0.70 or more and 0.97 or less. Since the adhesive according to the present invention has the above configuration, the gap of the air cavity can be controlled with high precision even when repeatedly heated. [Brief description of the drawings]
[0029] [Figure 1] FIG. 1 is a cross-sectional view showing a first example of metal particles that can be used in an adhesive according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a second example of metal particles that can be used in the adhesive according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view showing an example of an antenna device using the adhesive according to the present invention. [Figure 4] FIG. 4 is an enlarged cross-sectional view showing an adhesive portion between a metal particle and a metal portion in the antenna device shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] The present invention will be described in detail below.
[0031] (glue) The adhesive according to the present invention is an adhesive for bonding a first metal part and a second metal part in a first substrate having the first metal part on its surface and a second substrate having the second metal part on its surface. In the adhesive according to the present invention, the rate of change in the gap between the substrates calculated by the following evaluation test 1a is 10% or less.
[0032] Evaluation test 1a: A first substrate having a first metal part on its surface, a second substrate having a second metal part on its surface, and an adhesive are prepared. The adhesive is placed on the first metal part of the first substrate, and the second substrate is placed on the surface of the adhesive opposite to the first substrate side so that the first metal part and the second metal part face each other. Thereafter, the first substrate and the second substrate are bonded together by performing a reflow process under reflow conditions specified in JEDEC J-STD-020 to obtain a laminate. The gap between the substrates of the obtained laminate is measured and defined as the gap before heating. That is, the gap before heating means the gap before the laminate is heated. Then, the obtained laminate is subjected to a reflow process four times under reflow conditions specified in JEDEC J-STD-020, and the gap between the substrates of the laminate after the reflow process is measured and defined as the gap after heating. That is, the gap after heating means the gap after the laminate is heated four times. From the gap before and after heating, the rate of change of the gap is calculated using the following formula (1).
[0033] Gap change rate = [(gap before heating - gap after heating) / gap before heating] x 100 Formula (1)
[0034] In the evaluation test 1a, the adhesive is preferably disposed so that the gap before heating is 60 μm or more, and more preferably 850 μm or less.
[0035] The adhesive of the present invention is an adhesive for bonding a first metal part and a second metal part in a first substrate having a first metal part on a surface thereof and a second substrate having a second metal part on a surface thereof. The adhesive of the present invention contains metal particles. In the adhesive of the present invention, the ratio of the gap after heating calculated by the following evaluation test 1b to the average particle size of the metal particles is 0.70 or more and 0.97 or less.
[0036] Assessment Test 1b: A first substrate having a first metal part on its surface, a second substrate having a second metal part on its surface, and an adhesive are prepared. The adhesive is placed on the first metal part of the first substrate, and the second substrate is placed on the surface of the adhesive opposite to the first substrate side so that the first metal part and the second metal part face each other. Thereafter, the first substrate and the second substrate are bonded together by performing a reflow process under the reflow conditions specified in JEDEC J-STD-020 to obtain a laminate. The obtained laminate is subjected to a reflow process four times under the reflow conditions specified in JEDEC J-STD-020, and the gap between the substrates of the laminate after the reflow process is measured and defined as the gap after heating.
[0037] In the above evaluation test 1b, it is preferable that the adhesive is arranged so that the gap between the substrates of the laminate (laminate before reflow treatment) is 60 μm or more, and it is preferable that the adhesive is arranged so that the gap is 850 μm or less.
[0038] Since the adhesive according to the present invention has the above-mentioned configuration, the gap of the air cavity can be controlled with high precision even when repeatedly heated.
[0039] When an antenna device is obtained by bonding two substrates with an adhesive to form an air cavity (space) in the antenna, the antenna device may be repeatedly heated. In an antenna device obtained using a conventional adhesive, the antenna device is repeatedly heated, so that the gap of the air cavity (space) cannot be controlled with high precision, and it may be difficult to improve the communication speed and communication quality of the antenna.
[0040] In contrast, the adhesive according to the present invention has the above-mentioned configuration, and therefore, even when repeatedly heated, the gap between the substrates can be controlled with high precision, and the gap of the air cavity can be controlled with high precision, thereby further improving the communication speed and communication quality of the antenna.
[0041] The adhesive according to the present invention is an adhesive for bonding a first metal portion and a second metal portion in a first substrate having a first metal portion on a surface thereof and a second substrate having a second metal portion on a surface thereof. The adhesive according to the present invention is an adhesive for bonding two substrates. The adhesive according to the present invention is preferably an adhesive for bonding metal portions in two substrates.
[0042] In the adhesive according to the present invention, the rate of change of the gap between the substrates calculated by the evaluation test 1a is 10% or less. The rate of change of the gap between the substrates calculated by the evaluation test 1a is preferably 5% or less, more preferably 3% or less. When the rate of change of the gap between the substrates calculated by the evaluation test 1a is equal to or less than the upper limit, the gap of the air cavity can be controlled with high precision even when repeatedly heated.
[0043] In the adhesive according to the present invention, the ratio of the gap after heating calculated by the evaluation test 1b to the average particle size of the metal particles (gap after heating calculated by the evaluation test 1b / average particle size of the metal particles) is 0.70 or more and 0.97 or less. The ratio (gap after heating calculated by the evaluation test 1b / average particle size of the metal particles) is preferably 0.75 or more, more preferably 0.80 or more, and preferably 0.95 or less, more preferably 0.90 or less. When the ratio (gap after heating calculated by the evaluation test 1b / average particle size of the metal particles) is equal to or more than the lower limit and equal to or less than the upper limit, the gap of the air cavity can be controlled with high precision even when repeatedly heated.
[0044] In the above adhesive, the rate of change in adhesive strength between the substrates calculated by the following Evaluation Test 2 is preferably 10% or less, more preferably 5% or less, and even more preferably 3% or less. When the rate of change in adhesive strength between the substrates calculated by the following Evaluation Test 2 is equal to or less than the above upper limit, the adhesive strength between the substrates can be maintained even when repeatedly heated, and the air cavity gap can be controlled with high precision.
[0045] Evaluation test 2: A first substrate having a first metal part on its surface, a second substrate having a second metal part on its surface, and an adhesive are prepared. The adhesive is placed on the first metal part of the first substrate, and the second substrate is placed on the surface of the adhesive opposite to the first substrate side so that the first metal part and the second metal part face each other. Thereafter, the first substrate and the second substrate are bonded together by performing a reflow process under reflow conditions specified in JEDEC J-STD-020 to obtain a laminate. The obtained laminate is used to measure the adhesive strength between the substrates under conditions conforming to MIL STD-883G, which is defined as the adhesive strength before heating. The obtained laminate is then subjected to four reflow processes under reflow conditions specified in JEDEC J-STD-020, and the laminate after the reflow process is used to measure the adhesive strength between the substrates under conditions conforming to MIL STD-883G, which is defined as the adhesive strength after heating. The rate of change in adhesive strength before and after heating is calculated using the following formula (2).
[0046] Rate of change in adhesive strength = [(adhesive strength before heating - adhesive strength after heating) / adhesive strength before heating] x 100 Formula (2)
[0047] In the above evaluation test 2, it is preferable that the adhesive is arranged so that the gap between the substrates of the laminate (laminate before reflow treatment) is 60 μm or more, and it is preferable that the adhesive is arranged so that the gap is 850 μm or less.
[0048] In the evaluation test 2, the adhesive strength before heating is preferably 1.5 kgf or more, more preferably 2.0 kgf or more. When the adhesive strength before heating is equal to or more than the lower limit, the adhesive strength between the substrates can be maintained even when the substrates are repeatedly heated, and the gap of the air cavity can be controlled with high precision.
[0049] In Evaluation Test 1a, Evaluation Test 1b, and Evaluation Test 2, the first substrate is preferably a glass epoxy substrate or a ceramic substrate. In Evaluation Test 1a, Evaluation Test 1b, and Evaluation Test 2, the second substrate is preferably a glass epoxy substrate, a ceramic substrate, or a silicon substrate.
[0050] In the evaluation tests 1a, 1b, and 2, the first metal part is preferably made of copper or is formed by nickel / gold plating. In the evaluation tests 1a, 1b, and 2, the second metal part is preferably made of copper or is formed by nickel / gold plating.
[0051] The evaluation tests 1a, 1b, and 2 are performed to calculate the rate of change of the gap, the ratio (gap after heating calculated by evaluation test 1b / average particle size of metal particles), and the rate of change of the adhesive strength. When the adhesive is actually used, it does not have to be processed under the conditions specified in evaluation test 1a, 1b, and 2. For example, when the adhesive is actually used, it does not have to be reflow processed under the reflow conditions specified in JEDEC J-STD-020.
[0052] From the viewpoint of controlling the gap of the air cavity with high precision even when repeatedly heated, the adhesive preferably contains metal particles. The adhesive may or may not contain components other than the metal particles. From the viewpoint of controlling the gap of the air cavity with even higher precision even when repeatedly heated, the adhesive preferably contains only the metal particles, and is preferably a particle group of a plurality of metal particles.
[0053] The adhesive is capable of adhering, for example, two adherends. The adherend is preferably a substrate, more preferably a substrate having a metal portion on its surface. The adhesive is preferably used to adhere two substrates. The adhesive is preferably used to adhere two metal portions together. Furthermore, the adhesive is preferably used to control the gap between the two substrates. The adhesive is preferably used to control the gap between the two substrates.
[0054] The adhesive may or may not be used for conductive connection. The adhesive is preferably used in an antenna device. The adhesive is preferably used to form an air cavity. The adhesive is preferably used in an antenna device to form an air cavity. The adhesive is preferably used in an antenna device to keep a uniform and constant distance (gap) between a high-frequency board and a board constituting the antenna. The adhesive is preferably used in an antenna device to form an air cavity and improve the communication speed and communication quality of the antenna.
[0055] (metal particles) The adhesive according to the present invention preferably contains metal particles. The metal particles refer to particles containing a metal. The metal particles may contain components other than metal. The metal particles preferably have a role of regulating the distance (gap) between two substrates, for example. The metal particles are preferably not solder particles formed only from solder. The metal particles preferably have a base particle and a metal layer disposed on the surface of the base particle. The metal layer may have a single layer structure or a multi-layer structure of two or more layers.
[0056] The metal particles preferably have solder on the outer surface portion of the metal layer. The base particles preferably are not solder particles formed only by solder. In addition, when the metal particles are solder particles in which both the center portion and the outer surface portion of the metal layer are formed by solder, it may be difficult to control the gap of the air cavity when repeatedly heated because the solder spreads due to heating. When the metal particles are metal particles having a base particle not formed by solder and a metal layer (solder layer) arranged on the surface of the base particle, excessive spreading of the solder due to heating can be suppressed even when repeatedly heated, so that the gap of the air cavity can be controlled with high precision. Therefore, it is preferable that the metal particles are not solder particles formed by solder. It is preferable that the metal particles are not solder particles in which both the center portion and the outer surface portion of the metal layer are formed by solder.
[0057] The average particle size of the metal particles is not particularly limited. The average particle size of the metal particles can be appropriately selected according to the gap of the target air cavity. The average particle size of the metal particles may be, for example, 80 μm or more, or 900 μm or less.
[0058] The average particle size of the metal particles is preferably a number average particle size. The average particle size of the metal particles is obtained, for example, by observing 50 arbitrary metal particles with an electron microscope or optical microscope, and calculating the average particle size of each metal particle, or by performing laser diffraction particle size distribution measurement. In the observation with an electron microscope or optical microscope, the particle size of each metal particle is obtained as a particle size of a circle equivalent diameter. In the observation with an electron microscope or optical microscope, the average particle size of 50 arbitrary metal particles with a circle equivalent diameter is almost equal to the average particle size of a sphere equivalent diameter. In the laser diffraction particle size distribution measurement, the particle size of each metal particle is obtained as a particle size of a sphere equivalent diameter.
[0059] The coefficient of variation (CV value) of the particle size of the metal particles is preferably 10% or less, and more preferably 5% or less. When the coefficient of variation of the particle size of the metal particles is equal to or less than the upper limit, the gap of the air cavity can be controlled with even higher accuracy.
[0060] The coefficient of variation (CV value) can be measured as follows.
[0061] CV value (%) = (ρ / Dn) × 100 ρ: Standard deviation of metal particle diameter Dn: average particle size of metal particles
[0062] The shape of the metal particles is not particularly limited, and may be spherical or a shape other than spherical, such as flat.
[0063] Next, specific examples of metal particles will be described with reference to the drawings.
[0064] FIG. 1 is a cross-sectional view showing a first example of metal particles that can be used in an adhesive according to an embodiment of the present invention.
[0065] 1 has a base particle 2 and a metal layer 3 disposed on the surface of the base particle 2. The metal layer 3 coats the surface of the base particle 2. The metal particle 1 is a coated particle in which the surface of the base particle 2 is coated with the metal layer 3.
[0066] The metal layer 3 has a second metal layer 3A and a solder layer 3B (first metal layer). The metal particle 1 has the second metal layer 3A between the base particle 2 and the solder layer 3B. Therefore, the metal particle 1 has the base particle 2, the second metal layer 3A arranged on the surface of the base particle 2, and the solder layer 3B arranged on the outer surface of the second metal layer 3A. In this way, the metal layer 3 may have a multi-layer structure of two or more layers, or may have a multi-layer structure.
[0067] FIG. 2 is a cross-sectional view showing a second example of metal particles that can be used in the adhesive according to an embodiment of the present invention.
[0068] The metal layer 3 of the metal particle 1 in Fig. 1 has a two-layer structure. The metal particle 1A shown in Fig. 2 has a solder layer 4 as a single metal layer. The metal particle 1A includes a base particle 2 and a solder layer 4 disposed on the surface of the base particle 2.
[0069] Other details of the metal particles will be described below.
[0070] Base material particles: The base particles include resin particles, inorganic particles other than metal-containing particles, organic-inorganic hybrid particles, and metal-containing particles. The base particles are preferably base particles other than metal-containing particles, and more preferably resin particles, inorganic particles other than metal-containing particles, or organic-inorganic hybrid particles. The base particles may be core-shell particles having a core and a shell disposed on the surface of the core. The core may be an organic core, and the shell may be an inorganic shell.
[0071] As the material of the resin particles, various organic substances are suitably used. As the material of the resin particles, polyolefin resins such as polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, polyisobutylene, and polybutadiene; acrylic resins such as polymethyl methacrylate and polymethyl acrylate; polycarbonate, polyamide, phenol formaldehyde resin, melamine formaldehyde resin, benzoguanamine formaldehyde resin, urea formaldehyde resin, phenol resin, melamine resin, benzoguanamine resin, urea resin, epoxy resin, unsaturated polyester resin, saturated polyester resin, polyethylene terephthalate, polysulfone, polyphenylene oxide, polyacetal, polyimide, polyamideimide, polyether ether ketone, polyether sulfone, divinylbenzene polymer, and divinylbenzene copolymer. As the divinylbenzene copolymer, divinylbenzene-styrene copolymer and divinylbenzene-(meth)acrylic acid ester copolymer are exemplified. The material of the resin particles is preferably a polymer obtained by polymerizing one or more types of polymerizable monomers having an ethylenically unsaturated group, since this allows the hardness of the resin particles to be easily controlled within a suitable range.
[0072] When the resin particles are obtained by polymerizing a polymerizable monomer having an ethylenically unsaturated group, the polymerizable monomer having an ethylenically unsaturated group may be a non-crosslinkable monomer or a crosslinkable monomer.
[0073] Examples of the non-crosslinkable monomer include styrene-based monomers such as styrene and α-methylstyrene; carboxyl group-containing monomers such as (meth)acrylic acid, maleic acid, and maleic anhydride; alkyl (meth)acrylate compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate; and 2-hydroxyethyl (meth)acrylate, glycerol (meth)acrylate. nitrile-containing monomers such as (meth)acrylonitrile; vinyl ether compounds such as methyl vinyl ether, ethyl vinyl ether, and propyl vinyl ether; acid vinyl ester compounds such as vinyl acetate, vinyl butyrate, vinyl laurate, and vinyl stearate; unsaturated hydrocarbons such as ethylene, propylene, isoprene, and butadiene; and halogen-containing monomers such as trifluoromethyl (meth)acrylate, pentafluoroethyl (meth)acrylate, vinyl chloride, vinyl fluoride, and chlorostyrene.
[0074] Examples of the crosslinkable monomer include tetramethylolmethane tetra(meth)acrylate, tetramethylolmethane tri(meth)acrylate, tetramethylolmethane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, glycerol tri(meth)acrylate, glycerol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, and (poly)propylene glycol di(meth)acrylate. Examples of suitable (meth)acrylate compounds include polyfunctional (meth)acrylate compounds such as glycol di(meth)acrylate, (poly)tetramethylene glycol di(meth)acrylate, and 1,4-butanediol di(meth)acrylate; triallyl (iso)cyanurate, triallyl trimellitate, divinylbenzene, diallyl phthalate, diallyl acrylamide, diallyl ether, and silane-containing monomers such as γ-(meth)acryloxypropyltrimethoxysilane, trimethoxysilylstyrene, and vinyltrimethoxysilane.
[0075] The term "(meth)acrylate" refers to acrylate and methacrylate. The term "(meth)acrylic" refers to acrylic and methacrylic. The term "(meth)acryloyl" refers to acryloyl and methacryloyl.
[0076] The resin particles can be obtained by polymerizing the polymerizable monomer having an ethylenically unsaturated group by a known method, such as a suspension polymerization method in the presence of a radical polymerization initiator, or a method in which a monomer is swelled and polymerized together with a radical polymerization initiator using non-crosslinked seed particles.
[0077] When the base particle is an inorganic particle other than a metal-containing particle or an organic-inorganic hybrid particle, examples of the inorganic material for forming the base particle include silica, alumina, barium titanate, zirconia, and carbon black. The inorganic material is preferably not a metal. The particle formed by the silica is not particularly limited, but examples thereof include particles obtained by hydrolyzing a silicon compound having two or more hydrolyzable alkoxysilyl groups to form a crosslinked polymer particle, and then baking the particle as necessary. The organic-inorganic hybrid particle includes an organic-inorganic hybrid particle formed by a crosslinked alkoxysilyl polymer and an acrylic resin.
[0078] The organic-inorganic hybrid particles are preferably core-shell type organic-inorganic hybrid particles having a core and a shell disposed on the surface of the core. The core is preferably an organic core. The shell is preferably an inorganic shell. From the viewpoint of more effectively reducing the connection resistance between electrodes, the base particle is preferably an organic-inorganic hybrid particle having an organic core and an inorganic shell disposed on the surface of the organic core.
[0079] Examples of the material for the organic core include the materials for the resin particles described above.
[0080] The material of the inorganic shell may be any of the inorganic substances listed as the material of the base particle. The material of the inorganic shell is preferably silica. The inorganic shell is preferably formed by forming a shell-like material from a metal alkoxide on the surface of the core by a sol-gel method, and then firing the shell-like material. The metal alkoxide is preferably a silane alkoxide. The inorganic shell is preferably formed from a silane alkoxide.
[0081] When the base particle is a metal-containing particle, examples of the metal that is the material of the metal-containing particle include silver, copper, nickel, silicon, gold, and titanium.
[0082] The particle diameter of the base particle is not particularly limited. The particle diameter of the base particle can be appropriately selected according to the gap of the target air cavity. The particle diameter of the base particle may be, for example, 80 μm or more, or 900 μm or less.
[0083] The particle size of the base particle refers to the diameter when the base particle is a perfect sphere, and refers to the sphere-equivalent diameter when the base particle is not a perfect sphere.
[0084] The particle diameter of the base particle is preferably a number average particle diameter. The particle diameter of the base particle is determined using a particle size distribution measuring device or the like. The particle diameter of the base particle is preferably determined by observing 50 arbitrary base particles with an electron microscope or optical microscope and calculating the average value. In the observation with an electron microscope or optical microscope, the particle diameter of each base particle is determined as the particle diameter of a circle equivalent diameter. In the observation with an electron microscope or optical microscope, the average particle diameter of 50 arbitrary base particles with a circle equivalent diameter is almost equal to the average particle diameter of a sphere equivalent diameter. In the laser diffraction type particle size distribution measurement, the particle diameter of each base particle is determined as the particle diameter of a sphere equivalent diameter.
[0085] Metal layer: The metal particles preferably have a base particle and a metal layer disposed on the surface of the base particle. The metal layer may be a single-layer structure or a multi-layer structure of two or more layers. When the metal layer has a multi-layer structure of two or more layers, the metal particles preferably have a base particle, a second metal layer disposed on the surface of the base particle, and a solder layer (first metal layer) disposed on the surface of the second metal layer. The metal particles preferably have solder on the outer surface portion of the metal layer.
[0086] The metal layer includes a metal. The metal constituting the metal layer is not particularly limited. Examples of the metal include gold, silver, copper, platinum, palladium, zinc, lead, aluminum, cobalt, indium, nickel, chromium, titanium, antimony, bismuth, germanium, and cadmium, as well as alloys thereof. In addition, tin-doped indium oxide (ITO) and solder may be used as the metal. Only one of the metals may be used, or two or more of them may be used in combination. From the viewpoint of controlling the gap of the air cavity with higher precision and from the viewpoint of further increasing the adhesive strength between the substrates, the metal included in the outermost metal layer is preferably solder.
[0087] The melting point of the base particle is preferably higher than the melting point of the metal layer. The melting point of the base particle is preferably higher than 160°C, more preferably higher than 300°C, even more preferably higher than 400°C, and particularly preferably higher than 450°C. The melting point of the base particle may be lower than 400°C. The melting point of the base particle may be lower than 160°C. The softening point of the base particle is preferably higher than 260°C. The softening point of the base particle may be lower than 260°C.
[0088] The metal particles may have a single layer of solder layer. The metal particles may have multiple layers of metal layers (a second metal layer and a solder layer (a first metal layer)). That is, the metal particles may have two or more metal layers stacked together. When the metal layer has two or more layers, the metal particles preferably have solder on the outer surface portion of the metal layer.
[0089] The solder is preferably a metal (low melting point metal) having a melting point of 450°C or less. The solder layer is preferably a metal layer (low melting point metal layer) having a melting point of 450°C or less. The low melting point metal layer is a layer containing a low melting point metal. The solder in the metal particles is preferably a metal (low melting point metal) having a melting point of 450°C or less. The low melting point metal refers to a metal having a melting point of 450°C or less. The melting point of the low melting point metal is preferably 300°C or less, more preferably 220°C or less.
[0090] The melting point of the low melting point metal can be determined by differential scanning calorimetry (DSC). An example of a differential scanning calorimetry (DSC) device is "EXSTAR DSC7020" manufactured by SII Corporation.
[0091] In addition, the solder in the metal particles preferably contains tin. In 100% by weight of the metal contained in the solder in the metal particles, the content of tin is preferably 30% by weight or more, more preferably 40% by weight or more, even more preferably 70% by weight or more, and particularly preferably 90% by weight or more. When the content of tin contained in the solder in the metal particles is equal to or more than the lower limit, the adhesive strength between the substrates can be further increased.
[0092] The tin content can be measured using a high-frequency inductively coupled plasma atomic emission spectrometer ("ICP-AES" manufactured by Horiba, Ltd.) or a fluorescent X-ray analyzer ("EDX-800HS" manufactured by Shimadzu Corporation).
[0093] When an adhesive containing metal particles having the solder on the outer surface of a metal layer is used to bond metal parts formed on two substrates, the solder can be melted and bonded to the metal parts. For example, the solder and the metal parts tend to come into surface contact rather than point contact, so that the adhesive strength between the substrates can be further increased and the contact area between the metal particles and the metal parts can be sufficiently increased.
[0094] The low melting point metal constituting the solder in the solder layer and the metal particles is not particularly limited. The low melting point metal is preferably tin or an alloy containing tin. Examples of the alloy include a tin-silver alloy, a tin-copper alloy, a tin-silver-copper alloy, a tin-bismuth alloy, a tin-zinc alloy, and a tin-indium alloy. Since it has excellent wettability with respect to the metal part, the low melting point metal is preferably tin, a tin-silver alloy, a tin-silver-copper alloy, a tin-bismuth alloy, or a tin-indium alloy.
[0095] The material constituting the solder in the solder layer and the metal particles is preferably a filler metal having a liquidus of 450° C. or less based on JIS Z3001: Welding Terminology. Examples of the composition of the solder include metal compositions containing zinc, gold, silver, lead, copper, tin, bismuth, indium, etc.
[0096] In order to further increase the bonding strength between the solder and the metal part in the metal particles, the solder in the metal particles may contain metals such as nickel, copper, antimony, aluminum, zinc, iron, gold, titanium, phosphorus, germanium, tellurium, cobalt, bismuth, manganese, chromium, molybdenum, and palladium. In order to further increase the bonding strength between the solder and the metal part in the metal particles, the solder in the metal particles preferably contains nickel, copper, or antimony. In order to further increase the bonding strength between the solder and the metal part in the metal particles, the content of these metals for increasing the bonding strength is preferably 0.001% by weight or more, and preferably 1% by weight or less, based on 100% by weight of the solder in the metal particles.
[0097] The metal particle preferably has a base particle, a second metal layer disposed on a surface of the base particle, and a solder layer disposed on a surface of the second metal layer.
[0098] The melting point of the second metal layer is preferably higher than that of the solder layer. The melting point of the second metal layer is preferably higher than 220°C, more preferably higher than 300°C, even more preferably higher than 400°C, even more preferably higher than 450°C, particularly preferably higher than 500°C, and most preferably higher than 600°C. The solder layer has a low melting point, so it is preferably melted when forming an air cavity. The second metal layer is preferably not melted when forming an air cavity. The metal particles are preferably used by melting the solder, preferably by melting the solder layer, and preferably by melting the solder layer and not melting the second metal layer. Since the melting point of the second metal layer is higher than that of the solder layer, it is possible to melt only the solder layer without melting the second metal layer when forming an air cavity.
[0099] The absolute value of the difference between the melting point of the solder layer and the melting point of the second metal layer exceeds 0°C, preferably 5°C or more, more preferably 10°C or more, even more preferably 30°C or more, particularly preferably 50°C or more, and most preferably 100°C or more.
[0100] The second metal layer includes a metal. The metal constituting the second metal layer is not particularly limited. Examples of the metal include gold, silver, copper, platinum, palladium, zinc, lead, aluminum, cobalt, indium, nickel, chromium, titanium, antimony, bismuth, germanium, and cadmium, as well as alloys thereof. In addition, tin-doped indium oxide (ITO) may be used as the metal. Only one of the above metals may be used, or two or more of them may be used in combination.
[0101] The second metal layer is preferably a nickel layer, a palladium layer, a copper layer or a gold layer, more preferably a nickel layer, a gold layer or a copper layer, and even more preferably a copper layer. The metal particles preferably have a nickel layer, a palladium layer, a copper layer or a gold layer, more preferably a nickel layer, a gold layer or a copper layer, and even more preferably a copper layer. By bonding two substrates using an adhesive containing metal particles having these preferred metal layers, the gap of the air cavity can be controlled with even higher precision. In addition, a solder layer can be formed more easily on the surface of these preferred metal layers.
[0102] The thickness of the metal layer is preferably 3.5 μm or more, more preferably 8 μm or more, and is preferably 80 μm or less, more preferably 65 μm or less, and even more preferably 50 μm or less. When the thickness of the metal layer is equal to or more than the lower limit and equal to or less than the upper limit, the adhesive strength between the substrates can be further increased.
[0103] The thickness of the second metal layer is preferably 0.5 μm or more, more preferably 3 μm or more, and is preferably 30 μm or less, more preferably 25 μm or less, and further preferably 20 μm or less. When the thickness of the second metal layer is equal to or more than the lower limit and equal to or less than the upper limit, the adhesive strength between the substrates can be further increased.
[0104] The thickness of the solder layer (first metal layer) is preferably 3 μm or more, more preferably 5 μm or more, and is preferably 50 μm or less, more preferably 40 μm or less, and further preferably 30 μm or less. When the thickness of the solder layer is equal to or more than the lower limit and equal to or less than the upper limit, the adhesive strength between the substrates can be further increased.
[0105] The thickness of the metal layer, the thickness of the second metal layer, and the thickness of the solder layer can be measured, for example, by observing the cross section of a metal particle using a transmission electron microscope (TEM).
[0106] The method of forming the metal layer on the surface of the base particle is not particularly limited. Examples of the method of forming the metal layer include electroless plating, electroplating, physical collision, mechanochemical reaction, physical vapor deposition or physical adsorption, and a method of coating the surface of the base particle with a metal powder or a paste containing a metal powder and a binder. The method of forming the metal layer is preferably electroless plating, electroplating, or a physical collision method. Examples of the physical vapor deposition method include vacuum deposition, ion plating, and ion sputtering. In addition, in the physical collision method, for example, a sheeter composer (manufactured by Tokuju Kosakusho Co., Ltd.) is used.
[0107] (Antenna device) The antenna device according to the present invention comprises a first substrate having a first metal portion on its surface, a second substrate having a second metal portion on its surface, and an adhesive portion bonding the first substrate and the second substrate. In the antenna device according to the present invention, the material of the adhesive portion is the adhesive described above. In the antenna device according to the present invention, the first metal portion and the second metal portion are bonded by the adhesive portion. In the antenna device according to the present invention, an air cavity is formed by the first substrate, the second substrate, and the adhesive portion.
[0108] The first substrate is preferably a glass epoxy substrate or a ceramic substrate. The second substrate is preferably a glass epoxy substrate, a ceramic substrate or a silicon substrate. The substrate may be a high-frequency substrate, a substrate constituting an antenna, or the like. The first metal portion is preferably made of copper or is formed by nickel / gold plating. The second metal portion is preferably made of copper or is formed by nickel / gold plating. The first metal portion and the second metal portion may be made of copper or may be formed by nickel / gold plating.
[0109] FIG. 3 is a cross-sectional view showing an example of an antenna device using the adhesive according to the present invention.
[0110] The antenna device 11 shown in Fig. 3 includes a first substrate 12, a second substrate 13, and an adhesive portion bonding the first substrate 12 and the second substrate 13 together. The material of the adhesive portion is the adhesive described above. In this embodiment, the material of the adhesive portion is metal particles 1. The adhesive portion is preferably formed from the metal particles.
[0111] The first substrate 12 has a plurality of first metal parts 12a on its surface (upper surface). The second substrate 13 has a plurality of second metal parts 13a on its surface (lower surface). The first metal parts 12a and the second metal parts 13a are bonded together by one or more metal particles 1 (adhesive part). In the antenna device 11, an air cavity 14 is formed by the first substrate 12, the second substrate 13, and the metal particles 1 (adhesive part). The metal particles 1 (adhesive part) keep the distance (gap) between the first substrate 12 and the second substrate 13 constant. The metal particles 1 (adhesive part) control the gap of the air cavity 14.
[0112] The gap in the antenna device may be set in accordance with the frequency band that the antenna device targets.
[0113] The method for manufacturing the antenna device is not particularly limited. As an example of the method for manufacturing the antenna device, the adhesive is placed between the first metal part and the second metal part to obtain a laminate, and then the laminate is heated and pressurized. The pressure of the pressurization is 9.8×10 4 Pa~4.9×10 6The heating temperature is about 120° C. to 250° C. From the viewpoint of controlling the air cavity gap with even greater precision, it is preferable not to apply pressure during the manufacture of the antenna device. By not applying pressure during the manufacture of the antenna device, the solder layer of the molten metal particles does not excessively wet and spread over the first metal portion and the second metal portion, so that the air cavity gap can be controlled with even greater precision.
[0114] FIG. 4 is an enlarged cross-sectional view showing an adhesive portion between a metal particle and a metal portion in the antenna device shown in FIG.
[0115] As shown in FIG. 4, in the antenna device 11, the laminate is heated, and then the solder layer 3B of the metal particles 1 melts, and the molten solder layer portion 3Ba comes into sufficient contact with the first metal portion 12a and the second metal portion 13a. By using the metal particles 1 whose outermost layer is a solder layer, the contact area between the metal particles 1 and the first metal portion 12a and the second metal portion 13a can be increased, and the gap of the air cavity can be controlled with even higher precision, compared to the case where the metal particles whose outermost layer is a metal such as nickel, gold, or copper are used. In addition, by using the metal particles 1 that are not solder particles formed by solder, excessive wetting and spreading of the solder due to heating can be suppressed even when repeatedly heated, and the gap of the air cavity can be controlled with even higher precision, compared to the case where the solder particles whose central portion and the outer surface portion of the metal layer are both formed by solder are used.
[0116] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0117] (metal particle 1) 50 parts by weight of divinylbenzene and 50 parts by weight of tetramethylolmethane tetraacrylate were copolymerized to produce base particles (average particle diameter 240 μm, CV value 1.85%) which are resin particles. The obtained base particles were electroless nickel plated to form a 0.3 μm thick undercoat nickel plating layer on the surface of the base particles. Next, the base particles on which the undercoat nickel plating layer was formed were electrolytic copper plated to form a 10 μm thick copper layer. Further, electrolytic plating was performed to form a 25 μm thick solder layer containing tin. In this way, metal particles 1 (average particle diameter 310 μm, CV value 2.85%) were produced in which a 10 μm thick copper layer was formed on the surface of the base particles and a 25 μm thick solder layer (tin: silver = 96.5 wt %: 3.5 wt %) was formed on the surface of the copper layer.
[0118] (metal particles 2) Base particles (average particle diameter 260 μm, CV value 1.92%), which are resin particles, were prepared in the same manner as metal particles 1. The obtained base particles were electroless nickel plated to form a 0.3 μm thick undercoat nickel plating layer on the surface of the base particles. Next, the base particles on which the undercoat nickel plating layer was formed were electrolytic copper plated to form a 5 μm thick copper layer. Further, electrolytic plating was performed to form a 20 μm thick solder layer containing tin. In this way, metal particles 2 (average particle diameter 310 μm, CV value 2.76%) were prepared in which a 5 μm thick copper layer was formed on the surface of the base particles and a 20 μm thick solder layer (tin:silver=96.5 wt %:3.5 wt %) was formed on the surface of the copper layer.
[0119] (metal particles 3) Base particles (average particle diameter 210 μm, CV value 1.68%), which are resin particles, were prepared in the same manner as metal particles 1. The obtained base particles were electroless nickel plated to form a 0.3 μm thick undercoat nickel plating layer on the surface of the base particles. Next, the base particles on which the undercoat nickel plating layer was formed were electrolytic copper plated to form a 10 μm thick copper layer. Further, electrolytic plating was performed to form a 40 μm thick solder layer containing tin. In this way, metal particles 3 (average particle diameter 310 μm, CV value 3.21%) were prepared in which a 10 μm thick copper layer was formed on the surface of the base particles and a 40 μm thick solder layer (tin:silver=96.5 wt %:3.5 wt %) was formed on the surface of the copper layer.
[0120] (Metal particles X1) Solder balls formed from a solder containing tin, silver and copper ("M705" manufactured by Senju Metal Industry Co., Ltd., tin:silver:copper=96.5% by weight:3% by weight:0.5% by weight) were used as metal particles X1 (average particle diameter 300 μm).
[0121] (Average particle size of metal particles) The average particle size of the metal particles was measured by the above-mentioned method using a digital microscope ("VHX-5000" manufactured by Keyence Corporation).
[0122] Example 1 No adhesive component other than the metal particles 1 was used, and the obtained metal particles 1 themselves were used as an adhesive.
[0123] (Production of antenna device A) A glass epoxy substrate having 20 metal parts (first metal parts) made of copper was prepared as the first substrate. A glass epoxy substrate having 20 metal parts (second metal parts) made of copper was prepared as the second substrate. The metal parts are metal parts for forming an antenna circuit. Flux (WS-9160-M7 manufactured by Cookson Electronics) was applied to the surface of the first metal part of the first substrate. Metal particles 1 were then placed on the surface of the applied flux, and reflow treatment (heating temperature 250°C and heating time 30 seconds) was performed to bond the metal particles 1 and the first metal part. Solder paste (M705-GRN360-K2-V manufactured by Senju Metal Industry Co., Ltd.) was then applied to the surface of the second metal part of the second substrate. The bonded structure of the first substrate and the metal particles 1 and the second substrate coated with the solder paste were arranged so that the first metal part and the second metal part faced each other, and a reflow process (heating temperature 250°C, heating time 30 seconds) was performed. In this way, an antenna device A was produced in which the first metal part and the second metal part were bonded via the adhesive part formed by the metal particles 1.
[0124] (Fabrication of antenna device B) Antenna device B was manufactured in the same manner as antenna device A, except that a glass epoxy substrate having 20 metal parts (second metal parts) formed by nickel / gold plating was used as the second substrate.
[0125] (Fabrication of antenna device C) Antenna device C was manufactured in the same manner as antenna device A, except that a glass epoxy substrate having 20 metal portions (second metal portions) formed by nickel / gold plating was used as the first substrate and the second substrate.
[0126] Example 2 Antenna devices A, B, and C were produced in the same manner as in Example 1, except that metal particles 2 were used instead of metal particles 1 as the adhesive.
[0127] Example 3 Antenna devices A, B, and C were produced in the same manner as in Example 1, except that metal particles 3 were used instead of metal particles 1 as the adhesive.
[0128] Comparative Example 1 Antenna devices A, B, and C were produced in the same manner as in Example 1, except that metal particles X1 were used instead of metal particles 1 as the adhesive.
[0129] (evaluation) (1) Rate of change of gap between substrates (evaluation test 1a) (1-1) The obtained metal particles (adhesive) were prepared. A first substrate (glass epoxy substrate) having a first metal part made of copper on its surface was prepared. A second substrate (glass epoxy substrate) having a second metal part made of copper on its surface was prepared. Using the prepared metal particles (adhesive), first substrate, and second substrate, the rate of change of the gap between the substrates was calculated by the method described above.
[0130] (1-2) The obtained metal particles (adhesive) were prepared. A first substrate (glass epoxy substrate) having a first metal portion formed of copper on its surface was prepared. A second substrate (glass epoxy substrate) having a second metal portion formed of nickel / gold plating on its surface was prepared. Using the prepared metal particles (adhesive), first substrate, and second substrate, the rate of change of the gap between the substrates was calculated by the method described above.
[0131] (1-3) The obtained metal particles (adhesive) were prepared. A first substrate (glass epoxy substrate) having a first metal portion formed on its surface by nickel / gold plating was also prepared. A second substrate (glass epoxy substrate) having a second metal portion formed on its surface by nickel / gold plating was also prepared. Using the prepared metal particles (adhesive), first substrate, and second substrate, the rate of change of the gap between the substrates was calculated by the method described above.
[0132] [Criteria for determining the rate of change of the gap between boards] ○: Gap change rate is 10% or less ×: Gap change rate exceeds 10%
[0133] (2) Ratio (gap after heating / average particle size of metal particles) (Evaluation Test 1b) (2-1) The obtained metal particles (adhesive) were prepared. A first substrate (glass epoxy substrate) having a first metal part made of copper on its surface was prepared. A second substrate (glass epoxy substrate) having a second metal part made of copper on its surface was prepared. Using the prepared metal particles (adhesive), first substrate, and second substrate, the ratio (gap after heating / average particle size of metal particles) was calculated by the method described above.
[0134] (2-2) The obtained metal particles (adhesive) were prepared. A first substrate (glass epoxy substrate) having a first metal part formed of copper on its surface was prepared. A second substrate (glass epoxy substrate) having a second metal part formed of nickel / gold plating on its surface was prepared. Using the prepared metal particles (adhesive), first substrate, and second substrate, the ratio (gap after heating / average particle size of metal particles) was calculated by the method described above.
[0135] (2-3) The obtained metal particles (adhesive) were prepared. A first substrate (glass epoxy substrate) having a first metal portion formed on its surface by nickel / gold plating was also prepared. A second substrate (glass epoxy substrate) having a second metal portion formed on its surface by nickel / gold plating was also prepared. Using the prepared metal particles (adhesive), first substrate, and second substrate, the ratio (gap after heating / average particle size of metal particles) was calculated by the method described above.
[0136] [Ratio (gap after heating / average particle size of metal particles) criteria] ○: Ratio (gap after heating / average particle size of metal particles) is 0.70 or more and 0.97 or less ×: Ratio (gap after heating / average particle size of metal particles) is less than 0.70 or exceeds 0.97
[0137] (3) Rate of change in adhesive strength between substrates (Evaluation Test 2) (3-1) The obtained metal particles (adhesive) were prepared. A first substrate (glass epoxy substrate) having a first metal part formed of copper on its surface was prepared. A second substrate (glass epoxy substrate) having a second metal part formed of copper on its surface was prepared. Using the prepared metal particles (adhesive), first substrate, and second substrate, the rate of change in adhesive strength between the substrates was calculated by the method described above.
[0138] (3-2) The obtained metal particles (adhesive) were prepared. A first substrate (glass epoxy substrate) having a first metal part formed of copper on its surface was prepared. A second substrate (glass epoxy substrate) having a second metal part formed of nickel / gold plating on its surface was prepared. Using the prepared metal particles (adhesive), first substrate, and second substrate, the rate of change in adhesive strength between the substrates was calculated by the method described above.
[0139] (3-3) The obtained metal particles (adhesive) were prepared. A first substrate (glass epoxy substrate) having a first metal portion formed on its surface by nickel / gold plating was also prepared. A second substrate (glass epoxy substrate) having a second metal portion formed on its surface by nickel / gold plating was also prepared. Using the prepared metal particles (adhesive), first substrate, and second substrate, the rate of change in adhesive strength between the substrates was calculated by the method described above.
[0140] [Criteria for determining the rate of change in adhesive strength between substrates] ○: Change in adhesive strength is 10% or less ×: The rate of change in adhesive strength exceeds 10%
[0141] (4) Gap controllability The thickness of the air cavity of the five antenna devices A obtained was measured using a stereo microscope (Nikon's "SMZ-10"), and the average thickness of the air cavity of each of the five antenna devices A was calculated. The gap controllability was judged according to the following criteria from the difference between the maximum average thickness and the minimum average thickness. The same evaluation was also performed on the obtained antenna devices B and C.
[0142] [Gap control criteria] ○: The difference between the maximum and minimum average thicknesses of the air cavities is less than 10 μm ×: The difference between the maximum and minimum average thicknesses of the air cavities is 10 μm or more.
[0143] (5) Gap control after reflow processing Using the five antenna devices A after the evaluation of the above (4) gap controllability, four reflow processes were performed under the reflow conditions specified in JEDEC J-STD-020. The antenna devices A after the reflow process were evaluated in the same manner as the above (4) gap controllability. The gap controllability after the reflow process was judged according to the following criteria. The same evaluation was also performed on the obtained antenna devices B and C.
[0144] [Criteria for determining gap control after reflow processing] ○: The difference between the maximum and minimum average thicknesses of the air cavities is less than 10 μm ×: The difference between the maximum and minimum average thicknesses of the air cavities is 10 μm or more.
[0145] (6) Antenna communication quality Using the antenna device A after the evaluation of the gap controllability after the reflow process (5) above, it was confirmed whether the antenna operates with good accuracy. The communication quality of the antenna was judged according to the following criteria. The obtained antenna devices B and C were also evaluated in the same way.
[0146] [Criteria for determining antenna communication quality] ○: The antenna device operates stably without any variation. ×: There is variation in the operation of the antenna device.
[0147] The results are shown in Table 1 below.
[0148] [Table 1]
[0149] A similar tendency was observed even when a ceramic substrate or a silicon substrate was used as the first substrate and the second substrate instead of the glass epoxy substrate. [Explanation of symbols]
[0150] 1,1A…metal particles 2...Base material particles 3...Metal layer 3A…Second metal layer 3B: Solder layer (first metal layer) 3Ba: Molten solder layer 4...Solder layer 11...Antenna device 12...First substrate 12a…First metal part 13...Second board 13a…Second metal part 14…Air cavity
Claims
1. an adhesive for bonding a first metal portion and a second metal portion to each other in a first substrate having a first metal portion on a surface thereof and a second substrate having a second metal portion on a surface thereof, the combination of the first substrate and the second substrate is a combination of a high-frequency substrate and a substrate constituting an antenna, the adhesive is used in an antenna device to maintain a uniform and constant distance between the high-frequency board and a board constituting the antenna; An adhesive in which the rate of change in the gap between substrates, as calculated by the following evaluation test 1a, is 10% or less. Evaluation test 1a: A first substrate having a first metal portion on its surface, a second substrate having a second metal portion on its surface, and an adhesive are prepared. The adhesive is placed on the first metal part of the first substrate, and the second substrate is placed on the surface of the adhesive opposite to the first substrate side such that the first metal part and the second metal part face each other. Thereafter, the first substrate and the second substrate are bonded together by performing a reflow process under the reflow conditions specified in JEDEC J-STD-020 to obtain a laminate. The gap between the substrates of the obtained laminate is measured and defined as the gap before heating. Thereafter, the obtained laminate is subjected to four reflow processes under the reflow conditions specified in JEDEC J-STD-020, and the gap between the substrates of the laminate after the reflow process is measured and defined as the gap after heating. The rate of change in the gap is calculated from the gap before and after heating using the following formula (1). Gap change rate=[(gap before heating−gap after heating) / gap before heating]×100 Formula (1)
2. The adhesive of claim 1 comprising metal particles.
3. an adhesive for bonding a first metal portion and a second metal portion to each other in a first substrate having a first metal portion on a surface thereof and a second substrate having a second metal portion on a surface thereof, the combination of the first substrate and the second substrate is a combination of a high-frequency substrate and a substrate constituting an antenna, the adhesive is used in an antenna device to maintain a uniform and constant distance between the high-frequency board and a board constituting the antenna; the adhesive comprises metal particles; An adhesive, in which the ratio of the gap after heating calculated by the following evaluation test 1b to the average particle size of the metal particles is 0.70 or more and 0.97 or less. Evaluation test 1b: A first substrate having a first metal portion on its surface, a second substrate having a second metal portion on its surface, and an adhesive are prepared. The adhesive is placed on the first metal part of the first substrate, and the second substrate is placed on the surface of the adhesive opposite to the first substrate side such that the first metal part and the second metal part face each other. Thereafter, the first substrate and the second substrate are bonded together by performing a reflow process under the reflow conditions specified in JEDEC J-STD-020 to obtain a laminate. The obtained laminate is subjected to a reflow process four times under the reflow conditions specified in JEDEC J-STD-020, and the gap between the substrates of the laminate after the reflow process is measured and regarded as the gap after heating.
4. The adhesive of claim 2 or 3, wherein the metal particles have a substrate particle and a metal layer disposed on a surface of the substrate particle.
5. the metal layer has a second metal layer disposed on a surface of the base particle and a first metal layer disposed on a surface of the second metal layer; The adhesive of claim 4 , wherein the first metal layer is a solder layer.
6. 6. The adhesive according to claim 1, wherein the rate of change in adhesive strength between substrates calculated by the following Evaluation Test 2 is 10% or less. Evaluation test 2: A first substrate having a first metal portion on its surface, a second substrate having a second metal portion on its surface, and an adhesive are prepared. The adhesive is placed on the first metal part of the first substrate, and the second substrate is placed on the surface of the adhesive opposite to the first substrate side so that the first metal part and the second metal part face each other. Thereafter, the first substrate and the second substrate are bonded together by performing a reflow process under reflow conditions specified in JEDEC J-STD-020 to obtain a laminate. The obtained laminate is used to measure the adhesive strength between the substrates under conditions conforming to MIL STD-883G, which is defined as the adhesive strength before heating. The obtained laminate is then subjected to four reflow processes under reflow conditions specified in JEDEC J-STD-020, and the laminate after the reflow process is used to measure the adhesive strength between the substrates under conditions conforming to MIL STD-883G, which is defined as the adhesive strength after heating. The rate of change in adhesive strength is calculated from the adhesive strength before and after heating using the following formula (2). Rate of change in adhesive strength=[(adhesive strength before heating−adhesive strength after heating) / adhesive strength before heating]×100 Formula (2)
7. the first substrate is a glass epoxy substrate or a ceramic substrate, The adhesive according to any one of claims 1 to 6, wherein the second substrate is a glass epoxy substrate, a ceramic substrate or a silicon substrate.
8. The first metal portion is formed of copper or is formed by nickel / gold plating, The adhesive according to any one of claims 1 to 7, wherein the second metal portion is formed of copper or formed by nickel / gold plating.
9. A first substrate having a first metal portion on a surface thereof; a second substrate having a second metal portion on a surface thereof; an adhesive portion that bonds the first substrate and the second substrate; The material of the adhesive part is the adhesive according to any one of claims 1 to 8, the first metal portion and the second metal portion are bonded together by the adhesive portion, the combination of the first substrate and the second substrate is a combination of a high-frequency substrate and a substrate constituting an antenna, the gap between the high-frequency board and the board constituting the antenna is maintained uniform and constant by the adhesive part; An antenna device, wherein an air cavity is formed by the first substrate, the second substrate, and the adhesive portion.
10. the first substrate is a glass epoxy substrate or a ceramic substrate, The antenna device according to claim 9 , wherein the second substrate is a glass epoxy substrate, a ceramic substrate or a silicon substrate.
11. The first metal portion is formed of copper or is formed by nickel / gold plating, 11. The antenna device according to claim 9, wherein the second metal portion is made of copper or is plated with nickel / gold.
Citation Information
Patent Citations
Multilayer high-frequency substrate, and antenna device
JP2015185550A
Conductive particles and method and device for manufacturing the same, anisotropic conductive adhesive and conductive connection structure, and electronic circuit components and method of manufacturing the same