Oxides, solid electrolytes, and all-solid-state lithium-ion secondary batteries

LLZ-based oxides with substituent elements like Zn, Bi, Nb, and Hf enhance ionic conductivity and structural stability, addressing the need for improved solid electrolytes in all-solid-state lithium-ion secondary batteries, achieving high lithium ion conductivity and density.

JP7583730B2Active Publication Date: 2024-11-14KANEKA CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021548753
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-27
Filing Date
2020-09-07
Publication Date
2024-11-14
Estimated Expiration
2040-09-07

AI Technical Summary

Technical Problem

There is a need for new solid electrolyte materials in all-solid-state lithium-ion secondary batteries that offer higher ionic conductivity and lithium ion stability to meet the demands of automotive applications.

Method used

The development of LLZ-based oxides with substituent elements such as Zn, Bi, Nb, and Hf, which improve the ionic conductivity and structural stability by altering the crystal structure and reducing defects in the garnet-type oxide.

Benefits of technology

The LLZ-based oxides exhibit enhanced lithium ion conductivity, reaching up to 5.0×10⁻⁴ S/cm, and higher density, thereby improving the performance of all-solid-state lithium-ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583730000002
    Figure 0007583730000002
  • Figure 0007583730000003
    Figure 0007583730000003
  • Figure 0007583730000004
    Figure 0007583730000004
Patent Text Reader

Abstract

An LLZ oxide according to one embodiment of the present invention is a garnet oxide that contains Li, La, Zr and O as main constituent elements, while containing substituent elements such as Zn in addition to the main constituent elements. The substituent elements may comprise Bi, Nb, Hf and the like in addition to Zn. This LLZ oxide is used, for example, as a solid electrolyte for an all-solid-state lithium ion secondary battery. An all-solid-state lithium ion secondary battery according to the present invention is provided with: a positive electrode; a negative electrode; and a solid electrolyte layer that is arranged between the positive electrode and the negative electrode.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an oxide, and a solid electrolyte and an all-solid-state lithium ion secondary battery each containing the oxide. [Background technology]

[0002] Lithium-ion secondary batteries are becoming popular as power sources for mobile phones and laptops. At present, liquid electrolytes (electrolytic solutions) are widely used in lithium-ion secondary batteries, but in order to expand their use to in-vehicle devices, etc., development is underway on all-solid-state secondary batteries that use solid electrolytes as secondary batteries with high safety and higher capacity and output.

[0003] As a candidate for the solid electrolyte of all-solid-state lithium-ion secondary batteries, the garnet-type oxide Li7La3Zr2O 12 Garnet-type oxides are generally classified as A3B2C3O 12 It has a cubic crystal structure. In LLZ, the A site (dodecahedral coordination) is occupied by La 3+ , B site (hexahedral coordination) Zr 4+ , C sites (tetrahedral coordination) and interstitial sites (octahedral coordination) are occupied by Li + The structure is dominated by a lattice constant of 1,000,000,000 Li, which is occupied by 1,000,000 Li. Compared to typical garnet-type structures, this structure contains an excess of Li. This unique crystal structure is believed to be one of the reasons why the material exhibits high lithium-ion conductivity in the solid state.

[0004] Furthermore, LLZ-based oxides in which various additive elements are introduced into LLZ have been reported. For example, Patent Document 1 reports that the denseness and lithium ion conductivity are improved by adding Al as a substitution element in addition to the basic elements of LLZ, Li, La, and Zr. Patent Document 2 reports that the lithium ion conductivity is further improved by adding Nb and / or Ta as a substitution element. [Prior art documents] [Patent documents]

[0005] Patent Document 1 Japanese Patent Application Laid-Open No. 2011-51800 Patent Document 2 Japanese Patent Application Laid-Open No. 2011-73962 Summary of the Invention Problems to be Solved by the Invention

[0006] As a solid electrolyte material, the development of new materials is required from the viewpoints of higher ionic conductivity, lithium ion stability, etc. Means for Solving the Problems

[0007] LLZ-based oxides are garnet-type oxides mainly composed of Li, La, Zr, and O, and contain substitution elements such as Zn in addition to the main constituent elements.

[0008] The substitution element of the LLZ-based oxide may contain Bi in addition to Zn. For example, Li (7-2j) Zn j La (3-k) Bi k Zr2O (12-δ) It may have a composition represented by (0 < j < 3.5, 0 < k < 3, 0 ≦ δ < 1).

[0009] The substitution element of the LLZ-based oxide may contain one or more elements selected from the group consisting of Nb and Hf in addition to Zn. For example, Li (7-4x+z) Hf x La (3-2y / 3) Zn y Zr (2-z) Nb z O (12-δ) It may have a composition represented by (0 < x < 1.75, 0 ≦ y < 3, 0 ≦ z < 2, 0 ≦ δ < 1, provided that at least one of y and z is not 0). Advantages of the Invention

[0010] The above-mentioned LLZ-based oxide can be used as a solid electrolyte for an all-solid-state lithium-ion secondary battery. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional SEM image of an oxide sintered body of an example. [Diagram 2] 1 is a cross-sectional SEM image of an oxide sintered body of an example. [Diagram 3] 1 is an X-ray diffraction chart of an oxide sintered body of an example. [Figure 4] 1 is an X-ray diffraction chart of an oxide sintered body of an example. [Diagram 5] 1 is an X-ray diffraction chart of an oxide sintered body of an example. [Figure 6] 1 is an X-ray diffraction chart of an oxide sintered body of an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] [Oxide] One embodiment of the present invention is a garnet-type oxide whose main constituent elements are Li, La, Zr, and O. The crystal structure of the garnet-type oxide is a cubic system, but the composition formula is Li7La3Zr2O 12±δ Garnet-type oxides (LLZ) represented by the formula (1) have a cubic phase and a tetragonal phase. It is known that the cubic phase may have a low-temperature cubic phase and a high-temperature cubic phase depending on the formation conditions, thermal history, and the like. Therefore, the crystal structure of LLZ and oxides in which a part of the metal elements of LLZ is replaced with other metal elements (LLZ-based oxides) may have a garnet-like crystal structure in addition to a general garnet-type crystal structure. In this specification, the term "garnet-type oxide" is used to refer to the case where the oxide has a garnet-like crystal structure. The garnet-type oxide may be a single phase or a mixed phase of two or more phases.

[0013] LLZ may have oxygen vacancies. The formula is Li7La3Zr2O 12-δIn this case, δ represents the amount of oxygen deficiency. δ may be 0. Although it is difficult to precisely measure the amount of oxygen deficiency δ, generally δ is less than 1. The LLZ-based oxide having a substitution element may also have oxygen deficiency.

[0014] The LLZ-based oxide of the present invention contains at least Zn as a substitution element in addition to Li, La, Zr, and O as main constituent elements. Zn as a substitution element is considered to be introduced into the Li site and / or the Zr site of LLZ. By introducing Zn as a substitution element, the ionic conductivity of the oxide tends to improve.

[0015] The LLZ-based oxide may contain substitution elements other than Zn. Examples of substitution elements other than Zn include Bi, Nb, Ta, Na, K, Rb, Mg, Ca, Ba, Sr, Ce, B, Al, Ti, V, Cr, Fe, Ni, Sn, Ga, Ge, In, Sc, Y, Lu, Hf, Pr, Nd, Pm, Sm, Eu, W, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, etc.

[0016] In the first embodiment of the LLZ-based oxide of the present invention, Bi is included as a substitution element other than Zn. Bi as a substitution element is considered to be introduced into the La site. When Zn and Bi are included as substitution elements, Zn is considered to be preferentially introduced into the Li site. Therefore, the LLZ-based oxide of the first embodiment containing Zn and Bi as substitution elements has the composition formula Li (7-2j) Zn j La (3-k) Bi k Zr2O (12-δ) and can be represented by. Here, 0 < j < 3.5 and 0 < k < 3. δ is the amount of oxygen deficiency, and generally it is less than 1 as described above.

[0017] From the perspective of enhancing the substitution effect by Zn, the substitution amount j of Zn is preferably 0.05 or more, more preferably 0.08 or more, still more preferably 0.1 or more, and may be 0.12 or more or 0.15 or more. On the other hand, when the substitution amount by Zn becomes excessively large, the ionic conductivity may decrease as the amount of Li in the oxide decreases. Therefore, j is preferably 1 or less, more preferably 0.7 or less, still more preferably 0.5 or less, and may be 0.4 or less, 0.3 or less, or 0.2 or less.

[0018] 8 - coordinated Bi 3+ (Ionic radius: 1.17 Å) and 8 - coordinated La 3+ (Ionic radius: 1.16 Å) Since their ionic radii are substantially equal, even if the substitution amount k of Bi changes, there is no significant difference in the crystal structure of the LLZ - type oxide. Therefore, the substitution amount k of Bi can be in any range less than 3. k may be 0.05 or more, 0.075 or more, 0.1 or more, or 0.12 or more, and may also be 1 or less, 0.75 or less, 0.5 or less, 0.3 or less, or 0.2 or less.

[0019] In the second embodiment of the LLZ - type oxide of the present invention, as a substitution element other than Zn, it contains Nb and / or Hf. Nb as a substitution element is considered to be introduced into the Zr site. Hf as a substitution element is considered to be introduced into the Li site. When including Zn and Nb and / or Hf as substitution elements, Zn is considered to be preferentially introduced into the La site. Therefore, the LLZ - type oxide of the second embodiment containing Nb and / or Hf in addition to Zn as a substitution element has the composition formula Li (7-4x+z) Hf x La (3-2y / 3) Zn y Zr (2-z) Nb z O (12-δ) It can be represented by. Here, 0 < x < 1.75, 0 ≤ y < 3, 0 ≤ z < 2. However, at least one of y and z is not 0. When including Hf as a substitution element, x > 0, and when including Nb as a substitution element, z > 0. δ is the amount of oxygen deficiency and is generally less than 1 as described above.

[0020] From the viewpoint of enhancing the effect of substitution with Zn, the amount of substitution y of Zn is preferably 0.05 or more, more preferably 0.08 or more, even more preferably 0.1 or more, and may be 0.12 or more or 0.15 or more. On the other hand, if the amount of substitution with Zn becomes too large, the ion conductivity may decrease with the decrease in the amount of Li in the oxide. Therefore, y is preferably 1 or less, more preferably 0.7 or less, even more preferably 0.5 or less, and may be 0.4 or less, 0.3 or less, or 0.2 or less.

[0021] Since Hf has a smaller ionic radius than Li, it is considered that as the substitution amount x of Hf increases, the lattice spacing tends to become smaller, and the diffusion path of lithium ions becomes narrower. In addition, as the substitution amount x of Hf increases, the ion conductivity may decrease with the decrease in the amount of Li in the oxide. Therefore, x is preferably 1 or less, more preferably 0.7 or less, and even more preferably 0.5 or less, and may be 0.4 or less, 0.3 or less, or 0.2 or less. From the viewpoint of obtaining the substitution effect of Hf, the substitution amount x of Hf may be 0.01 or more, 0.05 or more, 0.08 or more, or 0.1 or more.

[0022] When the Nb substitution amount z increases, the ion conductivity may improve with an increase in the Li amount in the oxide. On the other hand, when the Nb substitution amount z increases, the lattice spacing tends to become smaller, and it is considered that the diffusion path of lithium ions becomes narrower. The Nb substitution amount z may be 0.01 or more, 0.05 or more, 0.1 or more, 0.2 or more, 0.3 or more, or 0.4 or more, or 1 or less, 0.8 or less, 0.7 or less, or 0.6 or less.

[0023] As described above, it is believed that the ionic conductivity of the LLZ-based oxide changes when the LLZ-based oxide contains Zn, Bi, Hf, Nb, etc. as a substitution element, and the crystal structure (crystal phase and lattice constant) changes and the Li ion content changes. It is preferable that the LLZ-based oxide is a cubic crystal. directionLLZ-based oxides having a crystal structure tend to exhibit high ionic conductivity, and the ionic conductivity tends to be high especially when the crystal structure is a single phase.

[0024] In addition, the inclusion of a substitution element may suppress the occurrence of defects such as voids and abnormal grain growth in the sintered body. In other words, the substitution element such as Zn acts as a sintering aid or grain growth inhibitor, and the density of the sintered body of the LLZ-based oxide increases, which is also thought to contribute to the improvement of the ionic conductivity.

[0025] The density of LLZ oxide is 3.5g / cm 3 It is preferable that the content is 3.8 g / cm or more. 3 More than 4.0g / cm 3 More than 4.2g / cm 3 or more than 4.4g / cm 3 The density of the oxide can be calculated based on the mass and volume of the pellet. For example, in the case of a cylindrical pellet, the diameter of the pellet is measured at several points with a micrometer and the average value is calculated, and the thickness is also measured at several points with a micrometer and the average value is calculated, and the volume is calculated from these values.

[0026] The lithium ion conductivity of LLZ oxide is 5.0×10 ‐5 S / cm or more is preferable, and 1.0×10 ‐4 S / cm or more is preferable, and 3.0×10 ‐4 S / cm or more is more preferable. The lithium ion conductivity can be measured by an AC impedance method. When the ion conductivity of an oxide sintered body is measured by an AC impedance method, multiple resistance components may be detected. For example, when the resistance of the grain boundary is large, a bulk resistance indicating the resistance of the grain portion and a grain boundary resistance indicating the resistance of the grain boundary portion are detected. In this case, the ion conductivity can be calculated by considering the bulk resistance (which generally indicates a relatively low resistance) as the resistance component of the oxide.

[0027] [Method of producing oxide] The above-mentioned LLZ-based oxide is obtained by mixing and firing the Li compound, La compound, and Zr compound, which are the main constituent element sources, and compounds containing substitution elements such as Zn. As an example, a method of producing a sintered body of an oxide by mixing raw materials, calcining them, forming them, and then calcining (sintering) them will be described.

[0028] First, the starting materials containing each element are weighed out so as to obtain the stoichiometric ratio of the composition formula of the target oxide. The starting materials may be oxides, hydroxides, chlorides, carbonates, sulfates, nitrates, oxalates, etc. of each element. The mixing method may be dry mixing and grinding, or wet mixing and grinding with a solvent added. For mixing, a planetary mill, an attritor, a ball mill, etc. may be used. When wet mixing and grinding is performed, a solvent in which Li is difficult to dissolve is preferably used, and for example, an organic solvent such as ethanol may be used.

[0029] The mixed powder is preferably pre-fired at a temperature equal to or higher than the temperature at which the state of the starting materials changes (for example, gas generation or phase change) and lower than the sintering temperature. Specifically, the pre-fire temperature is preferably about 800 to 1200° C. Pre-fire is generally performed in an air atmosphere (oxidizing atmosphere).

[0030] The material obtained by the calcination is molded into a predetermined shape. Before molding, the material after the calcination may be pulverized and mixed. Examples of the molding method include a method in which a binder is added to the powder and then molding in a mold, cold isostatic pressing (CIP), hot isostatic pressing (HIP), hot pressing, etc. Sintering may be performed in an air atmosphere or in an inert gas atmosphere such as nitrogen or argon. If necessary, firing may be performed in a reducing atmosphere. The sintering temperature may be higher than the calcination temperature, and specifically, it is preferably 1100°C or higher, and more preferably 1150°C or higher.

[0031] The above method is an example, and LLZ-based oxides can be obtained by other methods. For example, raw material powders and flux can be mixed, and LLZ-based oxides having a desired composition can be produced by a mechanochemical method.

[0032] [Uses of oxides] The above-mentioned LLZ-based oxide can be used as a solid electrolyte of an all-solid-state battery, and is particularly preferably used as a solid electrolyte of an all-solid-state lithium-ion secondary battery. The all-solid-state battery includes a positive electrode, a negative electrode, and a solid electrolyte, and contains the above-mentioned oxide as the solid electrolyte. The solid electrolyte may be contained in a separator disposed between the positive electrode and the negative electrode, or may be contained in the positive electrode and / or the negative electrode.

[0033] The positive electrode and the negative electrode each contain an active material. Any active material known as an active material for an all-solid-state battery can be used as the active material. For example, the active material for a lithium all-solid-state battery is LiCoO2; LiNi x Co 1-x O2(0 <x<1);LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2;LiMnO2;Li-Mn spinel with different elements;Lithium titanate;Lithium metal phosphate;Transition metal oxide;TiS2 ; These include carbon materials such as graphite and hard carbon, LiCoN, SiO2, Li2SiO3, Li4SiO4, metallic lithium, lithium alloys such as LiSn, LiSi, LiAl, LiGe, LiSb, and LiP, and lithium-storing intermetallic compounds such as Mg2Sn, Mg2Ge, Mg2Sb, and Cu3Sb. In a lithium solid-state battery, two substances with different potentials (charge / discharge potentials) for absorbing and releasing lithium ions are selected, and the substance showing the more noble potential is used as the positive electrode active material, and the substance showing the more base potential is used as the negative electrode active material.

[0034] The electrode mixture constituting the positive electrode and the negative electrode may contain, in addition to the active material, a solid electrolyte, a conductive assistant, a binder, and the like. The above-mentioned LLZ-based oxide may be used as the solid electrolyte contained in the electrode mixture. In addition, LLZ-based oxides other than the above and sulfide-based solid electrolytes may be used. As the conductive assistant, for example, carbon materials such as vapor-grown carbon fiber, acetylene black, ketjen black, carbon nanotubes, and carbon nanofibers, as well as metal materials that can withstand the environment when the all-solid-state battery is used, are used. Examples of binders include rubber-based polymers such as acrylonitrile butadiene rubber, butadiene rubber, polyvinylidene fluoride, and styrene butadiene rubber.

[0035] The positive electrode and the negative electrode each have a current collector. As the current collector, metals such as Cu, Ni, Al, V, Au, Pt, Mg, Fe, Ti, Co, Cr, Zn, Ge, In, or alloy materials containing two or more of these elements are preferable. The shape of the current collector is not particularly limited, and may be a foil or mesh. The positive electrode and the negative electrode are formed, for example, by applying a slurry-like electrode mixture composition to the surface of the current collector and then drying it. The positive electrode and the negative electrode may be produced by dry molding the electrode mixture and the current collector.

[0036] As described above, the all-solid-state battery may contain a solid electrolyte in the positive electrode and the negative electrode. The all-solid-state battery also includes a solid electrolyte layer as a separator between the positive electrode and the negative electrode. This solid electrolyte layer also preferably contains the above-mentioned LLZ-based oxide. The solid electrolyte layer may also contain a binder. The solid electrolyte layer can be produced by either a wet method or a dry method. EXAMPLES

[0037] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0038] [Sample preparation] As raw material components, lithium oxide, lanthanum oxide, zirconium oxide, zinc oxide, hafnium oxide, niobium oxide and bismuth oxide were blended in the amounts shown in Table 1. After the raw materials were mixed and pulverized by a rolling ball mill, they were press-molded into cylindrical pellets using a mold. The pellets were placed in an alumina crucible and covered with powder of cubic Li7La3Zr2O 12 (LLZ) for the purpose of suppressing Li volatilization during firing. Firing was carried out at 1100 °C for 12 hours in an atmosphere with flowing dry nitrogen. The fired pellets were crushed and mixed in a mortar and then press-molded again into cylindrical pellets using a mold. The molded body was placed in an alumina crucible, covered with powder of cubic LLZ in the same manner as during firing, and held at 1230 °C for 20 hours in an atmosphere with flowing dry nitrogen to obtain sintered compacts (Samples 1 to 13).

[0039] [Evaluation] [Observation of Cross Section of Sintered Compact] For Samples 1 to 11, the cross sections were observed by a scanning electron microscope (SEM). The SEM images of Samples 1 to 7 are shown in Fig. 1, and the SEM images of Samples 8 to 11 are shown in Fig. 2.

[0040] [X-ray Diffraction] For Samples 1 to 11, X-ray diffraction measurements were performed using CuKα as the radiation source. The X-ray diffraction charts of Samples 1 to 7 are shown in Figs. 3 and 4, and the X-ray diffraction charts of Samples 8 to 11 are shown in Figs. 5 and 6. Figs. 3 and 5 are X-ray diffraction charts in the range of 2θ = 10 to 60°, and Figs. 4 and 6 are X-ray diffraction charts in the range of 2θ = 30 to 40°.

[0041] [Lithium Ion Conductivity] Electrodes with a diameter of 8 mm were formed on both sides of Samples 1 to 13 by Au sputtering to prepare samples for ion conductivity measurement. This sample was set in a full solid-state battery evaluation cell (manufactured by Takizawa Co., Ltd.) in a glove box under an argon atmosphere, and a potentiogalvanostat TaThe ionic conductivity was evaluated by AC impedance measurement. The conditions for the AC impedance measurement were a frequency of 0.01 Hz to 1 MHz and a voltage of 50 mV. When two resistance components (bulk resistance and grain boundary resistance) were observed during the measurement, the ionic conductivity of the bulk resistance σ Bulk was adopted.

[0042] The amount and composition of raw materials used for samples 1 to 13, and the lithium ion conductivity σ Bulk is shown in Table 1. [Table 1]

[0043] Samples 1 to 13 were all 10 -5 S / cm order or 10 -4 It exhibits lithium ion conductivity on the order of 10 S / cm. By introducing substitution elements, it is possible to obtain a lithium ion conductivity of 10 S / cm. -6 S / cm~10 -7 The conductivity was improved compared to that of the SiO2-based ...

[0044] Among samples 1 to 7 containing Zn, Hf and Nb as substitution elements, sample 1 showed the highest lithium ion conductivity. Samples 2 and 3, which had a higher substitution amount of Hf than sample 1, had a lower conductivity than sample 1. From FIG. 1, it can be seen that samples 2 and 3 had larger voids than sample 1. From the X-ray diffraction chart in FIG. 4, it can be seen that the diffraction peaks of samples 2 and 3 are shifted to the high angle side (the lattice constant is smaller) compared to sample 1. This is considered to be due to the substitution of Li with Hf, which has a relatively small ionic radius. In samples 2 and 3, it is considered that the conductivity is lower than that of sample 1 because the lattice constant becomes smaller and the diffusion path of lithium ions becomes narrower with the increase in the substitution amount of Hf, and the Li content decreases.

[0045] Samples 4 and 5, in which the amount of Zn substitution was increased compared to sample 1, also had lower conductivity compared to sample 1. In the X-ray diffraction chart of Figure 4, the diffraction peaks of samples 4 and 5 are shifted to the higher angle side compared to sample 1, and it is considered that one of the reasons for the lower conductivity compared to sample 1 is that the diffusion path of lithium ions is narrower.

[0046] Samples 6 and 7, which had a higher Nb substitution than Sample 1, showed a slight decrease in conductivity compared to Sample 1. When Zr was substituted with Nb, the Li content increased to compensate for the charge difference, and it was expected that the conductivity would increase, but this phenomenon was not observed. In the X-ray diffraction chart of Figure 4, the diffraction peaks of Samples 6 and 7 were slightly shifted to the higher angle side compared to Sample 1. Six-coordinate Zr 4+ and 6-coordinate Nb 3+ Although there is no difference in the ionic radius between the two, the high angle shifts observed in samples 6 and 7, which have a large amount of Nb substitution, are believed to be due to the fact that part or all of the Nb introduced as a substitution element was introduced into the La site and / or Nb was introduced into the Zr site. 5+ It is estimated that 8-coordinate Nb 5+ is an 8-coordinate La 3+ The ionic radius is smaller than that of 6-coordinated Nb 5+ is 6-coordinate Zr 4+ Since the ionic radius is smaller than that of Nb 5+ is introduced into the La site and / or Zr site. R It is believed that the lattice constant becomes smaller when Nb is added. 5+ The decrease in Li content due to the introduction of Li as a cation may also be a factor in the decrease in ionic conductivity.

[0047] The X-ray diffraction charts of samples 1 to 7 (Figs. 3 and 4) show that all samples are cubic crystals, but while sample 1 is a single phase, multiple phases were confirmed in samples 2 to 7. It is presumed that the high ionic conductivity of sample 1 is related to the fact that the LLZ garnet-type structure was maintained.

[0048] Among samples 8 to 13, which contain Zn and Bi as substitution elements, sample 8 showed the highest ionic conductivity. Sample 9, which has a higher amount of Zn substitution than sample 8, and samples 12 and 13, which have a lower amount of Zn substitution, showed lower conductivity than sample 8. It is believed that the effect of introducing the substitution element Zn is small in samples 12 and 13. In the X-ray diffraction chart of Figure 6, the diffraction peak of sample 9 is shifted to the high angle side compared to sample 8, and it is believed that one of the causes of the lower conductivity is the smaller lattice constant and the narrower diffusion path of Li ions.

[0049] In samples 10 and 11, in which the amount of Bi substitution was increased compared to sample 8, the diffraction peaks tended to shift to higher angles as the amount of Bi substitution increased. Also, sample 8 was a single phase, whereas multiple phases were confirmed in samples 9 to 11. The fact that the LLZ garnet structure was maintained in sample 8 is also presumably related to the high ionic conductivity.

[0050] As shown in the evaluation results of the above samples 1 to 13, the LLZ-based oxides containing Zn as a substituting element have excellent lithium ion conductivity. In addition, there is a possibility that the lithium conductivity can be further improved by adjusting the amount of Zn substituted and the type and amount of the substituting element other than Zn.

Claims

1. A garnet-type oxide having Li, La, Zr and O as main constituent elements, The main constituent element includes Zn and Bi as substitution elements, An oxide having a composition represented by Li(7-2j)ZnjLa(3-k)BikZr2O(12-δ) (0.15≦j≦0.45, 0.05≦k≦1, 0≦δ<1).

2. A garnet-type oxide having Li, La, Zr and O as main constituent elements, The main constituent element includes Zn, Nb, and Hf as substitution elements, An oxide having a composition represented by Li(7-4x+z)HfxLa(3-2y / 3)ZnyZr(2-z)NbzO(12-δ) (0.05≦x<1.75, 0.15≦y≦0.45, 0.3≦z<2, 0≦δ<1).

3. A solid electrolyte comprising the oxide according to claim 1 or 2.

4. A battery comprising a positive electrode, a negative electrode, and a solid electrolyte layer disposed between the positive electrode and the negative electrode; An all-solid-state lithium ion secondary battery, wherein the solid electrolyte layer comprises the oxide according to claim 1 or 2.

Citation Information

Patent Citations

  • Multi-doping pomegranate-shaped solid electrolyte material and preparation method thereof

    CN109888374A

  • Ceramic material and process for producing the same

    JP2011051800A

  • Ceramic material and preparation method therefor

    JP2011073962A

  • Method of manufacturing cathode-solid electrolyte assembly

    JP2013243111A

  • Garnet-type lithium ion conductive oxide

    JP2016171068A