Solid electrolyte ceramics and solid-state batteries

The solid electrolyte ceramic with Li, La, Bi, and O, and transition metals like Co, Ni, or Mn, addresses the issue of increased electronic conductivity in garnet-type ceramics, enhancing ionic conductivity and reducing leakage currents in solid-state batteries.

JP7589750B2Active Publication Date: 2024-11-26MURATA MFG CO LTD

Patent Information

Application Number
JP2022563810
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-17
Filing Date
2021-11-17
Publication Date
2024-11-26
Estimated Expiration
2041-11-17

AI Technical Summary

Technical Problem

Conventional solid-state batteries using garnet-type solid electrolyte ceramics face issues with the generation of Li-Bi-O compounds at grain boundaries, leading to increased electronic conductivity and subsequent short circuits and leakage currents during operation.

Method used

A solid electrolyte ceramic composed of Li, La, Bi, and O with additional transition metal elements like Co, Ni, or Mn, maintaining a garnet-type crystal structure, is developed to suppress the increase in electronic conductivity while enhancing ionic conductivity.

Benefits of technology

The proposed ceramic effectively reduces electronic conductivity increases, ensuring stable battery operation with lower leakage currents and improved ionic conductivity, even under high-temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589750000010
    Figure 0007589750000010
  • Figure 0007589750000011
    Figure 0007589750000011
  • Figure 0007589750000001
    Figure 0007589750000001
Patent Text Reader

Abstract

The present invention provides a solid electrolyte ceramic that more sufficiently inhibits a rise in electron conductivity due to the operation of a solid state battery, while also having an excellent ionic conductivity property. The present invention relates to a solid electrolyte ceramic including at least Li (lithium), La (lanthanum), Bi (bismuth), and O (oxygen) and having a garnet-type crystal structure, said solid electrolyte ceramic further including one or more transition metal elements selected from the group consisting of Co (cobalt), Ni (nickel), and Mn (manganese).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solid electrolyte ceramic and a solid-state battery including the solid electrolyte ceramic. [Background technology]

[0002] In recent years, the demand for batteries as power sources for portable electronic devices such as mobile phones and portable personal computers has expanded significantly. As batteries for such applications, development of sintered solid-state secondary batteries (so-called "solid-state batteries") that use a solid electrolyte as the electrolyte and whose other components are also composed of solids is underway.

[0003] A solid-state battery includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer laminated between the positive electrode layer and the negative electrode layer. In particular, the solid electrolyte layer includes a solid electrolyte ceramic, and is responsible for ion conduction between the positive electrode layer and the negative electrode layer. Solid electrolyte ceramics are required to have higher ionic conductivity and lower electronic conductivity. As such solid electrolyte ceramics, attempts have been made to use ceramics obtained by sintering a garnet-type solid electrolyte substituted with Bi from the viewpoint of higher ionic conductivity (for example, Patent Document 1 and Non-Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-050071 A [Non-patent literature]

[0005] [Non-Patent Document 1] Gao et al., SolidState Ionics, 181 (2010) 1415-1419 Summary of the Invention [Problem to be solved by the invention]

[0006] The inventors of the present invention have found that the following problems occur in solid-state batteries using the above-mentioned conventional solid electrolyte ceramics. In particular, in conventional solid-state batteries using garnet-type solid electrolyte ceramics containing Bi, impurities such as Li-Bi-O-based compounds are easily generated at grain boundaries, and these Li-Bi-O-based compounds are reduced during operation of the solid-state battery (i.e., during charging and discharging), increasing the electronic conductivity. When the electronic conductivity increases, the solid-state battery may short-circuit and / or the leakage current may increase.

[0007] An object of the present invention is to provide a solid electrolyte ceramic that has excellent ionic conductivity and that more sufficiently suppresses an increase in electronic conductivity due to the operation of a solid-state battery. [Means for solving the problem]

[0008] The present invention relates to A solid electrolyte ceramic containing at least Li (lithium), La (lanthanum), Bi (bismuth) and O (oxygen) and having a garnet-type crystal structure, A solid electrolyte ceramic further containing one or more transition metal elements selected from the group consisting of Co (cobalt), Ni (nickel) and Mn (manganese). Regarding. Effect of the Invention

[0009] The solid electrolyte ceramic of the present invention has excellent ionic conductivity, while more sufficiently suppressing an increase in electronic conductivity due to the operation of a solid-state battery. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is an enlarged schematic view of a solid electrolyte ceramic for illustrating sintered particles constituting an example of the solid electrolyte ceramic of the present invention and the structure thereof. [Diagram 2]1 shows an electron energy loss spectrum obtained by measuring bulk particles in the solid electrolyte in the solid electrolyte single plate of Example 5A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] [Solid electrolyte ceramics] The solid electrolyte ceramic of the present invention is composed of a sintered body obtained by sintering solid electrolyte particles. The solid electrolyte ceramic of the present invention is a solid electrolyte ceramic containing at least Li (lithium), La (lanthanum), Bi (bismuth) and O (oxygen) and having a garnet-type crystal structure, and further containing one or more transition metal elements selected from the group consisting of Co (cobalt), Ni (nickel) and Mn (manganese) (hereinafter, simply referred to as "predetermined transition metal elements"). In the present invention, the solid electrolyte ceramic containing Li (lithium), La (lanthanum), Bi (bismuth) and O (oxygen) and having a garnet-type crystal structure further contains the predetermined transition metal element, thereby having excellent ion conductivity and more sufficiently suppressing the increase in electronic conductivity. If such a solid electrolyte ceramic does not contain the predetermined transition metal element, the increase in electronic conductivity cannot be sufficiently suppressed. The solid electrolyte ceramic of the present invention is a ceramic made of a solid electrolyte containing at least Li (lithium), La (lanthanum), Bi (bismuth) and O (oxygen) and having a garnet-type crystal structure, and may contain other composite oxides or single oxides within a range that does not impair the effects of the present invention. Also, it is sufficient that at least the sintered particles contained in the solid electrolyte ceramic, which is the main component of the present invention, have a garnet-type crystal structure.

[0012] The form of existence (or the form of inclusion) of the predetermined transition metal element in the solid electrolyte ceramic of the present invention is not particularly limited, and it may be present in the crystal lattice or may be present outside the crystal lattice. For example, the predetermined transition metal element may be present in the bulk, in the grain boundary, or in both in the solid electrolyte ceramic. As an example of the presence of the predetermined transition metal element in the bulk, in the solid electrolyte ceramic of the present invention, the predetermined transition metal element may be present in a metal site (lattice site) constituting a garnet-type crystal structure. The metal site may be any metal site, for example, a Li site, a La site, a Bi site, or two or more of these sites. The solid electrolyte ceramic of the present invention is composed of a plurality of sintered particles, and the predetermined transition metal element may be present in the interface between two or more sintered particles.

[0013] The form of existence (or the form of inclusion) of Bi (bismuth) in the solid electrolyte ceramic of the present invention is not particularly limited, and for example, the specified Bi (bismuth) may be present in the bulk, in the grain boundary, or in both in the solid electrolyte ceramic. From the viewpoint of insulation, it is preferable that Bi is present in the bulk. As an example of Bi being present in the bulk, in the solid electrolyte ceramic of the present invention, the Bi may be present in the metal site (lattice site) constituting the garnet-type crystal structure. It may be present in the sintered particles in the solid electrolyte ceramic of the present invention, or on the surface thereof.

[0014] In the present invention, the specified transition metal and / or Bi (bismuth) may be contained in the ceramic having a garnet-type crystal structure. Furthermore, the specified transition metal and / or Bi (bismuth) may exist as a single oxide of the specified transition metal and / or Bi (bismuth). Also, the specified transition metal and / or Bi (bismuth) may exist as a complex oxide containing elements constituting the solid electrolyte ceramic. The oxide may be present at the interface between sintered particles of the ceramic having a garnet-type crystal structure, which is the main component of the present invention.

[0015] In the solid electrolyte ceramics of the present invention, Li (lithium) and La (lanthanum) may be present in the bulk, and more specifically, in the solid electrolyte ceramics of the present invention, they may be present in the Li site and La site as metal sites (lattice sites) constituting the garnet-type crystal structure, for example. In this case, Li (lithium) and La (lanthanum) may be present in part in the grain boundary, either independently or as a composite oxide.

[0016] The transition metal element contained in the solid electrolyte ceramic of the present invention preferably contains Co, from the viewpoint of more sufficiently suppressing the increase in electronic conductivity.

[0017] The solid electrolyte ceramic of the present invention preferably has a chemical composition represented by the following general formula (I), and further contains the predetermined transition metal element in the above-mentioned form.

[0018] [ka]

[0019] In formula (I), A is one or more elements selected from the group consisting of Li (lithium), Ga (gallium), Al (aluminum), Mg (magnesium), Zn (zinc) and Sc (scandium), and includes at least Li. B is one or more elements selected from the group consisting of La (lanthanum), Ca (calcium), Sr (strontium), Ba (barium), and lanthanoid elements, including at least La. Examples of lanthanoid elements include Ce (cerium), Pr (praseodymium), Nd (neodymium), Pm (promethium), Sm (samarium), Eu (europium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holminium), Er (erbium), Tm (thulium), Yb (ytterbium), and Lu (lutetium). D represents one or more elements selected from the group consisting of transition elements capable of forming 6-coordinated bonds with oxygen and typical elements belonging to groups 12 to 15. Examples of transition elements capable of forming 6-coordinated bonds with oxygen include Sc (scandium), Zr (zirconium), Ti (titanium), Ta (tantalum), Nb (niobium), Hf (hafnium), Mo (molybdenum), W (tungsten), and Te (tellurium). Examples of typical elements belonging to groups 12 to 15 include In (indium), Ge (germanium), Sn (tin), Pb (lead), Sb (antimony), and Bi (bismuth). D includes at least Bi.

[0020] In formula (I), α, β, γ, and ω satisfy the following relations: 5.0≦α≦8.0, 2.5≦β≦3.5, 1.5≦γ≦2.5, and 11≦ω≦13, respectively. From the viewpoint of more sufficient suppression of an increase in electronic conductivity, α preferably satisfies 5.5≦α≦7.0, more preferably 6.0≦α≦6.8, even more preferably 6.2≦α≦6.8, and particularly preferably 6.2≦α≦6.6. From the viewpoint of more sufficient suppression of an increase in electronic conductivity, β preferably satisfies 2.5≦β≦3.3, more preferably 2.5≦β≦3.1, and further preferably 2.8≦β≦3.0. From the viewpoint of more sufficient suppression of an increase in electronic conductivity, γ preferably satisfies 1.8≦γ≦2.5, more preferably 1.8≦γ≦2.3, and further preferably 1.9≦γ≦2.3. From the viewpoint of more sufficient suppression of an increase in electronic conductivity, ω preferably satisfies 11≦ω≦12.5, and more preferably satisfies 11.5≦ω≦12.5.

[0021] The total content of the predetermined transition metal elements in the solid electrolyte ceramic of the present invention is usually the content of B in the general formula (I) (for example, La and B in the general formula (II) described later). 1 When the total amount of the cations (the total number of cations and cations) is taken as 100 mol%, the cation content is more than 0 mol% and not more than 3.50 mol% (for example, 0.01 mol% or more and 1.80 mol% or less), and from the viewpoint of better ionic conductivity and more sufficient suppression of an increase in electronic conductivity during operation, the cation content is preferably more than 0 mol% and not more than 1.20 mol% (for example, 0.01 mol% or more and 1.00 mol% or less), and more preferably more than 0 mol% and not more than 0.25 mol% (for example, 0.01 mol% or more and 0.20 mol% or less).

[0022] The content of a predetermined transition metal element can be measured by performing inductively coupled plasma (ICP) emission spectroscopy (ICP analysis) of the solid electrolyte ceramic to obtain the average chemical composition of the material. In detail, the average chemical composition is obtained based on the ICP analysis, and the contents of Co, Mn and Ni are calculated based on the average chemical composition, and the contents of B in the general formula (I) (for example, La and B in the general formula (II) described later) are calculated based on the average chemical composition. 1 The total number of the above (total number of the above) is taken as 100 mol %. The amount of the above may be measured and calculated using ICP-AES (inductively coupled plasma atomic emission spectroscopy), LA-ICP-MS (laser ablation inductively coupled plasma mass spectrometry), TEM-EDX (energy dispersive X-ray spectroscopy), WDX (wavelength dispersive X-ray spectroscopy) and / or X-ray photoelectron spectroscopy (XPS: X-ray Photoelectron Spectroscopy).

[0023] The content of Bi (bismuth) is usually more than 0 mol% and not more than 50 mol%, and from the viewpoint of better ionic conductivity and more sufficient suppression of an increase in electronic conductivity during operation, the content of Bi is preferably more than 0 mol% and not more than 35 mol%, more preferably 0.5 mol% or more and 20 mol% or less, and even more preferably 2.5 mol% or more and 17.5 mol% or less, when the content of D is 100 mol%.

[0024] The Bi content can be measured by performing inductively coupled plasma (ICP) emission spectroscopy (ICP analysis) of the solid electrolyte ceramic to obtain the average chemical composition of the material, in the same manner as the content of a specific transition metal element. In detail, the average chemical composition is obtained based on the ICP analysis, and the Bi content is calculated based on the average chemical composition by subtracting the D content in the general formula (I) (for example, the Bi and D content in the general formula (II) described later). 1 The total number of the above (total number of the above) is taken as 100 mol %. The amount of the above may be measured and calculated using ICP-AES (inductively coupled plasma atomic emission spectroscopy), LA-ICP-MS (laser ablation inductively coupled plasma mass spectrometry), TEM-EDX (energy dispersive X-ray spectroscopy), WDX (wavelength dispersive X-ray spectroscopy) and / or X-ray photoelectron spectroscopy (XPS: X-ray Photoelectron Spectroscopy).

[0025] In the present invention, the solid electrolyte ceramic having a garnet-type crystal structure means not only that the solid electrolyte ceramic has a "garnet-type crystal structure" but also that the solid electrolyte ceramic has a "garnet-like crystal structure". Specifically, the solid electrolyte ceramic of the present invention has a crystal structure that can be recognized as a garnet-type or garnet-like crystal structure by a person skilled in the field of solid batteries in X-ray diffraction. More specifically, the solid electrolyte ceramic of the present invention may show one or more main peaks corresponding to Miller indices specific to the so-called garnet-type crystal structure (diffraction pattern: ICDD Card No. 01-080-6142) at a predetermined incident angle in X-ray diffraction, or may show one or more main peaks having different incident angles (i.e., peak positions or diffraction angles) and intensity ratios (i.e., peak intensities or diffraction intensity ratios) from one or more main peaks corresponding to Miller indices specific to the so-called garnet-type crystal structure due to differences in composition as a garnet-like crystal structure. A representative diffraction pattern of a garnet-like crystal structure is, for example, ICDD Card No. 00-045-0109, etc. In addition, at least the sintered particles contained in the solid electrolyte ceramic, which is the main component of the present invention, should have a garnet-type crystal structure.

[0026] As a specific embodiment, the solid electrolyte ceramic of the present invention may have a chemical composition represented by the general formula (II). More specifically, the solid electrolyte ceramic may have a chemical composition represented by the general formula (II). In this case, the solid electrolyte ceramic of the present invention has the chemical composition represented by the general formula (II) and further contains a predetermined transition metal element as described above.

[0027] [ka]

[0028] In formula (II), A 1 A refers to a metallic element that occupies the Li site in the garnet-type crystal structure. 1is an element corresponding to A in the general formula (I) and may be one or more elements selected from the group consisting of elements other than Li among the elements exemplified as A. 1 is usually one or more elements selected from the group consisting of Ga (gallium), Al (aluminum), Mg (magnesium), Zn (zinc) and Sc (scandium). 1 is preferably one or more elements selected from the group consisting of Ga (gallium) and Al (aluminum), and more preferably two elements, Ga and Al, from the viewpoints of better ionic conductivity and more sufficient suppression of an increase in electronic conductivity during operation.

[0029] In formula (II), B 1 indicates a metal element that occupies the La site in the garnet-type crystal structure. 1 is an element corresponding to B in the general formula (I) and may be one or more elements selected from the group consisting of elements other than La among the elements exemplified as B. 1 is usually one or more elements selected from the group consisting of Ca (calcium), Sr (strontium), Ba (barium), and the lanthanide elements.

[0030] In formula (II), D 1 refers to a metal element that occupies a 6-coordinate site in a garnet-type crystal structure. The 6-coordinate site of a garnet-type crystal structure is, for example, Li5La3Nb2O 12 (ICDD Card No. 00-045-0109) Nb-occupied site, Li7La3Zr2O 12 (ICDD Card. No. 01-078-6708) is the site occupied by Zr. D 1 is an element corresponding to D in the general formula (I) and may be one or more elements selected from the group consisting of elements other than Bi among the elements exemplified as D. 1is usually at least one element selected from the group consisting of Zr (zirconium), Sn (tin), Sb (antimony), Ti (titanium), Ta (tantalum), Nb (niobium), Hf (hafnium), Mo (molybdenum), W (tungsten) and Te (tellurium). From the viewpoint of more excellent ion conductivity and more sufficient suppression of the increase in electron conductivity during operation, it preferably contains at least one element selected from the group consisting of Zr (zirconium) and Ta (tantalum), more preferably contains Zr (zirconium) and Ta (tantalum), and still more preferably contains Zr (zirconium) and Ta (tantalum).

[0031] In formula (II), x satisfies 0 < x ≤ 1.00. From the viewpoint of more excellent ion conductivity and more sufficient suppression of the increase in electron conductivity during operation, it preferably satisfies 0.01 ≤ x ≤ 0.70, more preferably satisfies 0.02 ≤ x ≤ 0.40, still more preferably satisfies 0.05 ≤ x ≤ 0.40, and particularly preferably satisfies 0.05 ≤ x ≤ 0.35. y satisfies 0 ≤ y ≤ 0.50. From the viewpoint of more excellent ion conductivity and more sufficient suppression of the increase in electron conductivity during operation, it preferably satisfies 0 ≤ y ≤ 0.40, more preferably satisfies 0 ≤ y ≤ 0.30, still more preferably satisfies 0 ≤ y ≤ 0.20, and particularly preferably y = 0. β satisfies 2.5 ≤ β ≤ 3.3. From the viewpoint of more excellent ion conductivity and more sufficient suppression of the increase in electron conductivity during operation, it is preferably 2.5 ≤ β ≤ 3.1, and more preferably 2.8 ≤ β ≤ 3.0 z satisfies 0 ≤ z ≤ 2.00. From the viewpoint of more excellent ion conductivity and more sufficient suppression of the increase in electron conductivity during operation, it preferably satisfies 0 ≤ z ≤ 1.00, more preferably satisfies 0 ≤ z ≤ 0.50, and still more preferably z = 0. γ satisfies 1.5 ≤ γ ≤ 2.5. From the viewpoint of more excellent ion conductivity and more sufficient suppression of the increase in electron conductivity during operation, it preferably satisfies 1.8 ≤ γ ≤ 2.5, more preferably satisfies 1.8 ≤ γ ≤ 2.3, and still more preferably satisfies 1.9 ≤ γ ≤ 2.3.

[0032] In formula (II), p usually satisfies 6.0≦p≦7.0, and from the viewpoints of better ionic conductivity and more sufficient suppression of an increase in electronic conductivity during operation, preferably satisfies 6.0≦p≦6.6, and more preferably 6.25≦p≦6.55. a is A 1 is the average valence of A 1 The average valence of is A 1 For example, if there are n1 elements X with a valence of a+, n2 elements Y with a valence of b+, and n3 elements Z with a valence of c+, then the value is expressed as (n1×a+n2×b+n3×c) / (n1+n2+n3). b is B 1 is the average valence of B 1 The average valence of B 1 For example, when n1 element X having a valence of a+, n2 element Y having a valence of b+, and n3 element Z having a valence of c+ are recognized, the above-mentioned A 1 This is the same value as the average valence of. c is D 1 is the average valence of D 1 The average valence of D 1 For example, when n1 element X having a valence of a+, n2 element Y having a valence of b+, and n3 element Z having a valence of c+ are recognized, the above-mentioned A 1 This is the same value as the average valence of. δ indicates the amount of oxygen vacancy, and may be 0. δ usually satisfies 0≦δ<1. The amount of oxygen vacancy δ cannot be quantitatively analyzed even with the latest equipment, so it may be considered to be 0. The molar ratio of each element in the chemical composition of the solid electrolyte ceramic of the present invention does not necessarily coincide with, for example, the molar ratio of each element in formula (II) and tends to deviate from that depending on the analytical method. However, as long as the composition deviation is not so large as to cause a change in the characteristics, the effect of the present invention can be achieved.

[0033] In the present invention, the chemical composition of the solid electrolyte ceramic may be the composition of the entire ceramic material determined by ICP (inductively coupled plasma analysis). It may be measured and calculated by ICP-AES (inductively coupled plasma atomic emission spectroscopy) or LA-ICP-MS (laser ablation inductively coupled plasma mass spectrometry). The chemical composition may be measured and calculated by XPS analysis, or may be determined by TEM-EDX (energy dispersive X-ray spectroscopy) and / or WDX (wavelength dispersive X-ray spectroscopy). Furthermore, the chemical composition may be obtained by performing quantitative analysis (composition analysis) of 100 arbitrary points of each of 100 arbitrary sintered particles and calculating the average value.

[0034] The content of a predetermined transition metal element (i.e., Co, Ni, Mn) in the solid electrolyte ceramic of the present invention [for example, the content of B in the general formula (I) (or the content of La and B in the general formula (II)] 1 The molar ratio when the total number of the elements (moles) is taken as 100 mol % may be calculated by the following method. In the present invention, the chemical composition of the solid electrolyte ceramic can be determined by ICP analysis (inductively coupled plasma method), LA-ICP-MS (laser ablation ICP mass spectrometry) analysis, etc. Also, it may be measured and calculated by XPS analysis, or TEM-EDX (energy dispersive X-ray spectrometry) or WDX (wavelength dispersive X-ray spectrometry). Furthermore, the chemical composition may be obtained by quantitatively analyzing (compositionally analyzing) any 100 points of each of any 100 sintered particles and calculating the average value.

[0035] For example, the analysis by EDX or WDX measures the cross section of a solid-state battery. The cross section of a solid-state battery is a cross section parallel to the lamination direction of the positive electrode layer, the solid electrolyte layer, and the negative electrode layer. The cross section of a solid-state battery can be exposed by embedding the solid-state battery in resin and then polishing it. There is no particular limitation on the method of polishing the cross section, but the solid electrolyte layer can be exposed by cutting it with a dicer or the like and then polishing it with abrasive paper, chemical mechanical polishing, ion milling, or the like. The molar ratios of Co, Ni, and Mn to B can be calculated by quantitatively analyzing the exposed cross section (solid electrolyte layer) with EDX or WDX (wavelength dispersive X-ray fluorescence analyzer).

[0036] For example, in TEM-EELS measurement, the electrode layer or solid electrolyte layer of a solid battery is exfoliated using FIB (focused ion beam) or the like, and then the solid electrolyte portion is measured using TEM-EELS (transmission electron microscope-electron energy loss spectroscopy). This makes it possible to detect elements contained in B, as well as Co, Ni, and Mn, and calculate the molar ratios of Co, Ni, and Mn relative to the B content.

[0037] In the electron energy loss spectroscopy (EELS spectrum) of the solid electrolyte ceramic (LLZ) of the present invention, as shown in the EELS spectrum of Fig. 2, the energy position of the Co L-edge peak in the solid electrolyte ceramic (LLZ) of the present invention is lower than the energy position of the Co L-edge peak of LiCoO2 (LCO). In detail, the shift width sw of these peaks (see Fig. 2) is usually 0.1 to 3 eV, preferably 0.3 to 2 eV. Fig. 2 shows an electron energy loss spectroscopy spectrum obtained by measuring bulk particles in the solid electrolyte in the solid electrolyte single plate produced in the example.

[0038] Specific examples of the chemical composition of the solid electrolyte ceramic of the present invention include the following chemical compositions. In the chemical compositions shown below, the transition metal element following the hyphen (-) may be present in the bulk and / or grain boundaries, as described above. Li<h2 style=";text-align:left;direction:ltr"> 6.3 <h2 style=";text-align:left;direction:ltr"> La3(Zr<h2 style=";text-align:left;direction:ltr"> 1.30 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.40 <h2 style=";text-align:left;direction:ltr"> Bi<h2 style=";text-align:left;direction:ltr"> 0.30 <h2 style=";text-align:left;direction:ltr"> )O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> -0.001Co<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.3 <h2 style=";text-align:left;direction:ltr"> La3(Zr<h2 style=";text-align:left;direction:ltr"> 1.30 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.40 <h2 style=";text-align:left;direction:ltr"> Bi<h2 style=";text-align:left;direction:ltr"> 0.30 <h2 style=";text-align:left;direction:ltr"> )O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> -0.003Co<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.3 <h2 style=";text-align:left;direction:ltr"> La3(Zr<h2 style=";text-align:left;direction:ltr"> 1.30 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.40 <h2 style=";text-align:left;direction:ltr"> Bi<h2 style=";text-align:left;direction:ltr"> 0.30 <h2 style=";text-align:left;direction:ltr"> )O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> -0.005Co<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.3 <h2 style=";text-align:left;direction:ltr"> La3(Zr<h2 style=";text-align:left;direction:ltr"> 1.30 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.40 <h2 style=";text-align:left;direction:ltr"> Bi<h2 style=";text-align:left;direction:ltr"> 0.30 <h2 style=";text-align:left;direction:ltr"> )O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> -0.010Co<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.3 <h2 style=";text-align:left;direction:ltr"> La3(Zr<h2 style=";text-align:left;direction:ltr"> 1.30 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.40 <h2 style=";text-align:left;direction:ltr"> Bi<h2 style=";text-align:left;direction:ltr"> 0.30 <h2 style=";text-align:left;direction:ltr"> )O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> -0.025Co<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.3 <h2 style=";text-align:left;direction:ltr"> La3(Zr<h2 style=";text-align:left;direction:ltr"> 1.30 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.40 <h2 style=";text-align:left;direction:ltr"> Bi<h2 style=";text-align:left;direction:ltr"> 0.30 <h2 style=";text-align:left;direction:ltr"> )O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> -0.050Co<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.3 <h2 style=";text-align:left;direction:ltr"> La3(Zr<h2 style=";text-align:left;direction:ltr"> 1.30 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.40 <h2 style=";text-align:left;direction:ltr"> Bi<h2 style=";text-align:left;direction:ltr"> 0.30 <h2 style=";text-align:left;direction:ltr"> )O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> -0.001Mn<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.3 <h2 style=";text-align:left;direction:ltr"> La3(Zr<h2 style=";text-align:left;direction:ltr"> 1.30 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.40 <h2 style=";text-align:left;direction:ltr"> Bi<h2 style=";text-align:left;direction:ltr"> 0.30 <h2 style=";text-align:left;direction:ltr"> )O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> -0.005Mn<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.3 <h2 style=";text-align:left;direction:ltr"> La3(Zr<h2 style=";text-align:left;direction:ltr"> 1.30 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.40 <h2 style=";text-align:left;direction:ltr"> Bi<h2 style=";text-align:left;direction:ltr"> 0.30 <h2 style=";text-align:left;direction:ltr"> )O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> -0.010Mn<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> 6.3 <h2 style=";text-align:left;direction:ltr"> La3(Zr<h2 style=";text-align:left;direction:ltr"> 1.30 <h2 style=";text-align:left;direction:ltr"> Ta<h2 style=";text-align:left;direction:ltr"> 0.40 <h2 style=";text-align:left;direction:ltr"> Bi<h2 style=";text-align:left;direction:ltr"> 0.30 <h2 style=";text-align:left;direction:ltr"> )O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> -0.001Ni<h2 style=";text-align:left;direction:ltr"> <h2 style=";text-align:left;direction:ltr"> Li6.3 La3(Zr 1.30 Ta 0.40 Bi 0.30 )O 12 -0.005Ni Li 6.3 La3(Zr 1.30 Ta 0.40 Bi 0.30 )O 12 -0.010Ni Li 6.3 La3(Zr 1.30 Ta 0.40 Bi 0.30 )O 12 -0.005Co-0.005Ni-0.005Mn Li 6.5 La3(Zr 1.53 Ta 0.4 Bi 0.07 )O 12 -0.005Co Li 6.5 La3(Zr 1.46 Ta 0.4 Bi 0.14 )O 12 -0.005Co Li 6.3 La3(Zr 1.30 Ta 0.40 Bi 0.30 )O 12 -0.005Co Li 6.1 La3(Zr 1.10 Ta 0.40 Bi 0.50 )O 12 -0.005Co

[0039] As long as the solid electrolyte ceramic of the present invention contains a predetermined transition metal element, each sintered particle constituting the solid electrolyte ceramic may contain Bi anywhere between the grain boundary vicinity portion described below and the particle interior. Furthermore, the Bi concentration may be approximately uniform between the grain boundary vicinity portion described below and the particle interior, or the Bi concentration may have a gradient. The former and latter solid electrolyte ceramics of the present invention can be called "solid electrolyte ceramics with uniform Bi concentration structure" and "solid electrolyte ceramics with gradient Bi concentration structure", respectively.

[0040] In one embodiment of the present invention, the solid electrolyte ceramic of the present invention may be a "Bi concentration gradient structure type solid electrolyte ceramic" containing the above-mentioned predetermined transition metal element while having a Bi concentration gradient between the grain boundary vicinity and the grain interior in each sintered particle. Note that the Bi concentration gradient structure type solid electrolyte ceramic of the present invention preferably has a chemical composition represented by the above general formula (I) or (II) in the grain boundary vicinity and the entire grain interior in each sintered particle.

[0041] In each sintered particle constituting the Bi concentration gradient structure type solid electrolyte ceramic of the present invention, specifically, the Bi concentration in the vicinity of the grain boundary is higher than the Bi concentration inside the particle. More specifically, as shown in FIG. 1, the solid electrolyte ceramic 10 of the present invention is composed of a plurality of sintered particles 1, and in each sintered particle 1, the Bi concentration in the grain boundary vicinity 3 close to the grain boundary 2 is higher than the Bi concentration in the particle interior 4 surrounded by the grain boundary vicinity 3. By containing a predetermined transition metal element while having such a Bi concentration gradient in the Bi concentration gradient structure type solid electrolyte ceramic of the present invention, the effect of containing the predetermined transition metal element in the present invention (particularly the effect of suppressing the increase in electronic conductivity during operation) can be more fully exhibited. FIG. 1 shows an enlarged schematic diagram of the solid electrolyte ceramic for explaining the sintered particles constituting the Bi concentration gradient structure type solid electrolyte ceramic of the present invention and their structure. In FIG. 1, only three sintered particles 1 are shown, but usually many sintered particles exist around them while forming grain boundaries between adjacent sintered particles.

[0042] The grain boundary vicinity 3 is a region (i.e., a grain boundary vicinity region) that is located at a distance from the grain boundary 2 (i.e., the distance from the grain boundary 2 toward the grain interior 4) of 50 nm or less. Therefore, the grain boundary vicinity 3 is disposed on the outer edge of the sintered particle (for example, in a cross-sectional view) and surrounds the particle interior 4 described below.

[0043] The Bi concentration in the grain boundary vicinity portion 3 refers to the average Bi amount (x1) in the grain boundary vicinity region as described above. In this specification, the Bi concentration in the grain boundary vicinity portion 3 is calculated by point analysis of 10 points in the grain boundary vicinity portion 3 using TEM-EDX (energy dispersive X-ray spectroscopy) and using the average value. In detail, for each of 10 arbitrary sintered particles, composition analysis is performed by point analysis at 10 arbitrary points in the grain boundary vicinity portion 3 to obtain the Bi / D ratio. The Bi amount x in the above general formula (I) is calculated from the Bi / D ratio, and the average value is used. The grain boundary vicinity portion 3 of one sintered particle forms a grain boundary 2 between them together with the grain boundary vicinity portions 3 of one or more mutually adjacent sintered particles.

[0044] The grain interior 4 is a region whose distance from the grain boundary 2 (i.e., the distance from the grain boundary 2 toward the grain interior 4) is more than 50 nm. More specifically, the grain interior 4 is an inner region surrounded by the grain boundary vicinity portion 3 (for example, in a cross-sectional view).

[0045] The Bi concentration in the particle interior 4 refers to the average Bi amount (x2) in the particle interior 4 as described above. In this specification, the Bi concentration in the particle interior 4 is calculated by point analysis of 10 points in the particle interior 4 using TEM-EDX (energy dispersive X-ray spectroscopy) and using the average value. In detail, for each of 10 arbitrary sintered particles, composition analysis is performed by point analysis at any 10 points in the particle interior 4 to obtain the Bi / D ratio. The Bi amount x in the above general formula (I) is calculated from the Bi / D ratio, and the average value is used.

[0046] In the present invention, in a solid electrolyte ceramic material having a garnet-type crystal structure, Bi can occupy a 6-coordinated site in the garnet-type crystal structure. In a preferred embodiment, when the amount of Bi x is twice the molar ratio of Bi in such a 6-coordinated site, the amount of Bi x in the grain boundary vicinity 3 (referred to as "x1" in this specification) and the amount of Bi x in the grain interior 4 (referred to as "x2" in this specification) are expressed by the following relationship: x2 <x1 Meet the following. In the present invention, the 6-coordinate site in the garnet-type crystal structure refers to, for example, the site occupied by D in the chemical composition of the general formula (I). In another specific example, the 6-coordinate site in the garnet-type crystal structure is, for example, Li5La3Nb2O 12 (ICDD Card No. 00-045-0109), the site occupied by Nb, also in the garnet-type crystal structure Li7La3Zr2O 12 This refers to the site occupied by Zr in (ICDD Card. No. 01-078-6708).

[0047] From the viewpoint of more excellent ionic conductivity and more sufficient suppression of an increase in electronic conductivity during operation, the Bi amount x1 in the grain boundary vicinity portion 3 and the Bi amount x2 in the particle interior 4 preferably satisfy the following relational expression p1, more preferably the following relational expression p2, further preferably the following relational expression p3, and particularly preferably the following relational expression p4:

[0048] Embodiment p1: 0 <x1≦0.80;および 0≦x2≦0.30.

[0049] Embodiment p2: 0.20≦x1≦0.60; and 0.01≦x2≦0.25.

[0050] Embodiment p3: 0.30≦x1≦0.50; and 0.05≦x2≦0.20.

[0051] Embodiment p4: 0.35≦x1≦0.45; and 0.08≦x2≦0.16.

[0052] From the viewpoint of more excellent ionic conductivity and more sufficient suppression of an increase in electronic conductivity during operation, the Bi amount x1 in the grain boundary vicinity portion 3 and the Bi amount x2 in the particle interior 4 preferably satisfy the following relational expression q1, more preferably the following relational expression q2, further preferably the following relational expression q3, and particularly preferably the following relational expression q4:

[0053] Implementation example q1: 0.01≦x1-x2.

[0054] Implementation example q2: 0.01≦x1-x2≦0.50.

[0055] Implementation example q3: 0.10≦x1-x2≦0.40.

[0056] Implementation example q4: 0.15≦x1-x2≦0.35.

[0057] The average particle size of the sintered particles constituting the solid electrolyte ceramic is usually more than 100 nm and not more than 100 μm, particularly not less than 200 nm and not more than 10 μm.

[0058] The average grain size of the sintered grains is the average grain size of the sintered grains whose outer periphery is defined by the grain boundaries. In this specification, the average particle size of the sintered particles is determined by performing particle analysis using a TEM image and image analysis software (e.g., "A-zo-kun" (manufactured by Asahi Kasei Engineering Co., Ltd.) and calculating the circle equivalent diameter, and using the average value of 100 random particles.

[0059] [Method of manufacturing solid electrolyte ceramics] The solid electrolyte ceramics of the present invention can be obtained by mixing a compound containing a predetermined metal element (i.e., starting material) with water, drying, and then heat-treating (for example, at least sintering). The compound containing the predetermined metal element is usually a mixture of compounds containing one metal element selected from the group consisting of Li (lithium), La (lanthanum), Bi (bismuth) and a predetermined transition metal element. Examples of the compound containing the predetermined metal element (i.e., starting material) include lithium hydroxide monohydrate LiOH·H2O, lanthanum hydroxide La(OH)3, zirconium oxide ZrO2, tantalum oxide Ta2O5, bismuth oxide Bi2O3, cobalt oxide Co3O4, basic nickel carbonate hydrate NiCO3·2Ni(OH)2·4H2O, manganese carbonate MnCO3, and the like. The mixing ratio of the compound containing the predetermined metal element may be such that the solid electrolyte ceramics of the present invention has a predetermined chemical composition after heat treatment. The heat treatment temperature is usually from 500° C. to 1200° C., preferably from 600° C. to 1000° C. The heat treatment time is usually from 10 minutes to 1440 minutes, particularly preferably from 60 minutes to 600 minutes.

[0060] The Bi concentration gradient structure type solid electrolyte ceramic of the present invention can be obtained by heat treatment (for example, at least sintering) in a state where a Bi-containing solid electrolyte layer as a shell layer is present around a Bi-free solid electrolyte particle as a core particle. In detail, it can be obtained by elementally diffusing Bi from the shell layer to the core particle. More specifically, a solution in which the core particle and a material for forming the shell layer are dissolved is prepared, and the two are mixed. Thereafter, the solvent is evaporated, and then heat treatment is performed to obtain a solid electrolyte particle in which the core particle is covered with a shell layer. Furthermore, the solid electrolyte ceramic of the present invention can be obtained by heat treatment of the solid electrolyte particle covered with the shell layer. However, the above manufacturing method is one example of how the Bi concentration gradient structure type solid electrolyte ceramic material of the present invention can be obtained, and it may be produced by other manufacturing methods.

[0061] The core particles are Bi-free solid electrolyte particles, and for example, particles made of a solid electrolyte having a garnet-type crystal structure that does not contain Bi are used. The core particles may be a solid electrolyte having a garnet-type crystal structure containing Bi, as long as the Bi concentration gradient structure type solid electrolyte ceramics of the present invention can be obtained. As the solid electrolyte used as the core particles, for example, a material similar to the solid electrolyte having the chemical composition represented by the above general formula (II) can be mentioned, except that x is within the range of 0≦x<1.0. x is preferably within the same range as x2 in the above embodiments p1 to p4. The core particles can be manufactured by the same method as the Bi concentration uniform structure type solid electrolyte ceramics of the present invention.

[0062] The chemical composition of the solid electrolyte constituting the core particle is not particularly limited, and for example, the solid electrolyte ceramic of the present invention may have a chemical composition as a whole represented by the general formula (I) or (II).

[0063] The average particle size of the core particles is usually more than 50 nm and not more than 100 μm, particularly not less than 100 nm and not more than 10 μm.

[0064] In this specification, the average particle size of the core particles is a value measured by the same method as that for the average particle size of the sintered particles.

[0065] The material for forming the shell layer is a material for forming a Bi-containing solid electrolyte layer as the shell layer, and is, for example, a material mixture for forming a layer composed of a solid electrolyte having a Bi-containing garnet-type crystal structure. The mixing ratio in the material mixture may be such that the shell layer and the solid electrolyte ceramic of the present invention have a predetermined chemical composition after sintering. As the Bi-containing solid electrolyte as the shell layer, for example, a material similar to the solid electrolyte having the average chemical composition represented by the above general formula (II) can be mentioned, except that x is within the same range as x1 in the above embodiments p1 to p4.

[0066] The chemical composition of the solid electrolyte constituting the shell layer is not particularly limited, and may be, for example, such that the solid electrolyte ceramic of the present invention as a whole has the chemical composition represented by the general formula (I) or (II).

[0067] The average thickness of the shell layer is usually more than 10 nm and not more than 10 μm, particularly from 20 nm to 1 μm.

[0068] In this specification, the average thickness of the shell layer can be calculated by subjecting a core particle having a shell layer to TEM measurement, measuring the thickness of the shell layer at any 20 points, and averaging the measurements.

[0069] The content of the shell layer forming material in the slurry is not particularly limited as long as the solid electrolyte ceramic of the present invention is obtained, and may be, for example, 1 mol % or more and 70 mol % or less, particularly 10 mol % or more and 50 mol % or less, relative to 100 mol % of the core particles.

[0070] The solvent is not particularly limited as long as it can dissolve the material for forming the shell layer, and for example, a solvent that can be used in the production of a positive electrode layer, a negative electrode layer, or a solid electrolyte layer in the field of solid-state batteries is used. The solvent is usually a solvent that can be used with the binder described below. Examples of such solvents include alcohols such as 2-methoxyethanol.

[0071] The sintering conditions for forming the shell layer are not particularly limited as long as the Bi concentration gradient structure type solid electrolyte ceramics of the present invention can be obtained. For example, if the sintering conditions are too strong, the Bi amount inside the particles becomes too high, and the Bi concentration gradient structure type solid electrolyte ceramics of the present invention cannot be obtained. Also, for example, if the sintering conditions are too weak, elemental diffusion of Bi from the shell layer to the core particles does not occur, and the Bi concentration gradient structure type solid electrolyte ceramics of the present invention cannot be obtained. The sintering temperature may be, for example, 600°C or more and 1100°C or less, particularly 700°C or more and 950°C or less. The sintering time may be, for example, 10 minutes or more and 1440 minutes or less, particularly 60 minutes or more and 600 minutes or less.

[0072] As the sintering aid that may be contained in the solid electrolyte ceramics of the present invention, which have a uniform Bi concentration structure and a gradient Bi concentration structure, any sintering aid known in the field of solid-state batteries can be used. The composition of such a sintering aid preferably contains at least Li (lithium), B (boron), and O (oxygen), and the molar ratio of Li to B (Li / B) is preferably 2.0 or more. Specific examples of such sintering aids include, for example, Li3BO3, (Li 2.7 Al 0.3 )BO3, Li 2.8 (B 0.8 C 0.2 )O3, LiBO2.

[0073] In particular, when the Bi concentration gradient structure type solid electrolyte ceramic of the present invention contains a sintering aid, the content of the sintering aid is preferably as small as possible from the viewpoint of elemental diffusion of Bi, and is preferably 0% or more and 10% or less, and more preferably 0% or more and 5% or less, relative to the volume ratio of the garnet-type solid electrolyte.

[0074] [Solid battery] In the present specification, the term "solid-state battery" refers in a broad sense to a battery whose components (particularly the electrolyte layer) are made of solids, and in a narrow sense to an "all-solid-state battery" whose components (particularly all components) are made of solids. In the present specification, the term "solid-state battery" includes so-called "secondary batteries" that can be repeatedly charged and discharged, and "primary batteries" that can only be discharged. The "solid-state battery" is preferably a "secondary battery." The term "secondary battery" is not excessively limited by its name, and may also include electrochemical devices such as "electricity storage devices."

[0075] The solid-state battery of the present invention includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer, and usually has a laminated structure in which the positive electrode layer and the negative electrode layer are laminated with a solid electrolyte layer interposed therebetween. The positive electrode layer and the negative electrode layer may each be laminated in two or more layers as long as a solid electrolyte layer is provided between them. The solid electrolyte layer is in contact with the positive electrode layer and the negative electrode layer and is sandwiched between them. The positive electrode layer and the solid electrolyte layer may be integrally sintered as sintered bodies, and / or the negative electrode layer and the solid electrolyte layer may be integrally sintered as sintered bodies. The term "integrally sintered as sintered bodies" means that two or more adjacent or contacting members (particularly layers) are joined by sintering. Here, the two or more members (particularly layers) may be sintered as sintered bodies, but may be integrally sintered.

[0076] The above-mentioned solid electrolyte ceramics of the present invention are useful as a solid electrolyte for solid-state batteries. Therefore, the solid-state battery of the present invention contains the above-mentioned solid electrolyte ceramics of the present invention as a solid electrolyte. More specifically, the solid electrolyte ceramics of the present invention are contained as a solid electrolyte in at least one layer selected from the group consisting of a positive electrode layer, a negative electrode layer, and a solid electrolyte layer. From the viewpoint of more excellent ion conductivity in the solid electrolyte layer and more sufficient suppression of an increase in electronic conductivity during operation, it is preferable that the solid electrolyte ceramics of the present invention are contained at least in the solid electrolyte layer.

[0077] (Positive electrode layer) In the solid-state battery of the present invention, the positive electrode layer is not particularly limited. For example, the positive electrode layer may contain a positive electrode active material and may further contain the solid electrolyte ceramic of the present invention. By containing the solid electrolyte ceramic of the present invention in the positive electrode layer, it is possible to suppress short-circuiting of the solid-state battery. The positive electrode layer may have the form of a sintered body containing positive electrode active material particles. The positive electrode layer may be a layer capable of absorbing and releasing ions (particularly lithium ions).

[0078] The positive electrode active material is not particularly limited, and positive electrode active materials known in the field of solid-state batteries can be used. Examples of the positive electrode active material include lithium-containing phosphate compound particles having a Nasicon structure, lithium-containing phosphate compound particles having an olivine structure, lithium-containing layered oxide particles, and lithium-containing oxide particles having a spinel structure. Specific examples of lithium-containing phosphate compounds having a Nasicon structure that are preferably used include Li3V2(PO4)3, etc. Specific examples of lithium-containing phosphate compounds having an olivine structure that are preferably used include Li3Fe2(PO4)3, LiMnPO4, etc. Specific examples of lithium-containing layered oxide particles that are preferably used include LiCoO2, LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 Specific examples of lithium-containing oxides having a spinel structure that are preferably used include LiMn2O4, LiNi 0.5 Mn 1.5 O4, Li4Ti5O 12 From the viewpoint of reactivity during co-sintering with the garnet-type solid electrolyte used in the present invention, LiCoO2, LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 It is more preferable to use a lithium-containing layered oxide such as O2. Only one type of these positive electrode active material particles may be used, or a mixture of two or more types may be used.

[0079] The positive electrode active material in the positive electrode layer has a Nasicon structure, which means that the positive electrode active material (particularly its particles) has a Nasicon crystal structure, and in a broader sense, means that the positive electrode active material has a crystal structure that can be recognized as a Nasicon crystal structure by those skilled in the art of solid-state batteries. In a narrower sense, the positive electrode active material in the positive electrode layer has a Nasicon structure, which means that the positive electrode active material (particularly its particles) shows one or more main peaks in X-ray diffraction at a specified incident angle, which correspond to Miller indices specific to the so-called Nasicon crystal structure. The compounds exemplified above are preferably used as positive electrode active materials having a Nasicon structure.

[0080] The positive electrode active material in the positive electrode layer has an olivine structure, which means that the positive electrode active material (particularly its particles) has an olivine crystal structure, and in a broad sense, means that the positive electrode active material has a crystal structure that can be recognized as an olivine crystal structure by those skilled in the art of solid-state batteries. In a narrow sense, the positive electrode active material in the positive electrode layer has an olivine structure, which means that the positive electrode active material (particularly its particles) shows one or more main peaks corresponding to Miller indices specific to the so-called olivine crystal structure at a predetermined incidence angle in X-ray diffraction. The above-mentioned compounds can be given as examples of the positive electrode active material having an olivine structure that is preferably used.

[0081] The positive electrode active material in the positive electrode layer has a spinel structure, which means that the positive electrode active material (particularly its particles) has a spinel crystal structure, and in a broad sense, means that the positive electrode active material has a crystal structure that can be recognized as a spinel crystal structure by a person skilled in the field of solid-state batteries. In a narrow sense, the positive electrode active material in the positive electrode layer has a spinel structure, which means that the positive electrode active material (particularly its particles) shows one or more main peaks corresponding to Miller indices specific to the so-called spinel crystal structure at a predetermined incidence angle in X-ray diffraction. The above-mentioned compounds can be given as examples of the positive electrode active material having a spinel structure that is preferably used.

[0082] The chemical composition of the positive electrode active material may be an average chemical composition. The average chemical composition of the positive electrode active material means the average value of the chemical composition of the positive electrode active material in the thickness direction of the positive electrode layer. The average chemical composition of the positive electrode active material can be analyzed and measured by breaking the solid-state battery and performing composition analysis by EDX (energy dispersive X-ray spectroscopy) in a field of view that includes the entire thickness direction of the positive electrode layer using SEM-EDX.

[0083] The positive electrode active material can be produced, for example, by the following method, or can be obtained as a commercial product. When producing the positive electrode active material, first, a raw material compound containing a predetermined metal atom is weighed so that the chemical composition is a predetermined chemical composition, and water is added and mixed to obtain a slurry. The slurry is then dried, calcined at 700°C to 1000°C for 1 hour to 30 hours, and pulverized to obtain the positive electrode active material.

[0084] The chemical composition and crystal structure of the positive electrode active material in the positive electrode layer may typically change due to elemental diffusion during sintering. The positive electrode active material may have the above-mentioned chemical composition and crystal structure in the solid-state battery after sintering with the negative electrode layer and the solid electrolyte layer.

[0085] The average particle size of the positive electrode active material is not particularly limited and may be, for example, 0.01 μm or more and 10 μm or less, and preferably 0.05 μm or more and 4 μm or less.

[0086] The average particle size (arithmetic mean) of the positive electrode active material can be determined, for example, by randomly selecting 10 to 100 particles from an SEM image and simply averaging their particle sizes. The particle diameter is the diameter of a spherical particle when the particle is assumed to be a perfect sphere. Such a particle diameter can be obtained, for example, by cutting out a cross section of a solid-state battery, taking a cross-sectional SEM image using a SEM, calculating the cross-sectional area S of the particle using image analysis software (for example, "A-zo-kun" (manufactured by Asahi Kasei Engineering Co., Ltd.)), and then calculating the particle diameter R using the following formula.

[0087]

number

[0088] The average particle size of the positive electrode active material in the positive electrode layer can be automatically measured by specifying the positive electrode active material by its composition when measuring the average chemical composition described above.

[0089] The average particle size of the positive electrode active material in the positive electrode layer may usually change due to sintering during the manufacturing process of the solid-state battery. The positive electrode active material may have the above-mentioned average particle size in the solid-state battery after sintering with the negative electrode layer and the solid electrolyte layer.

[0090] The volume ratio of the positive electrode active material in the positive electrode layer is not particularly limited, and may be, for example, 30% or more and 90% or less, and particularly 40% or more and 70% or less.

[0091] The positive electrode layer may contain the solid electrolyte ceramic of the present invention as a solid electrolyte, and / or may contain a solid electrolyte other than the solid electrolyte ceramic of the present invention. The positive electrode layer may further include a sintering aid and / or a conductive material.

[0092] When the positive electrode layer contains the solid electrolyte ceramic of the present invention, the volume ratio of the solid electrolyte ceramic of the present invention may usually be 20% or more and 60% or less, particularly 30% or more and 45% or less.

[0093] As the sintering aid in the positive electrode layer, compounds similar to the sintering aids that may be contained in the solid electrolyte ceramics can be used.

[0094] The volume ratio of the sintering aid in the positive electrode layer is not particularly limited, and is, for example, preferably from 0.1% to 20%, and more preferably from 1% to 10%.

[0095] The conductive material in the positive electrode layer can be a conductive material known in the field of solid-state batteries. Preferred conductive materials include metal materials such as Ag (silver), Au (gold), Pd (palladium), Pt (platinum), Cu (copper), Sn (tin), and Ni (nickel); and carbon materials such as acetylene black, Ketjen black, Super P (registered trademark), and carbon nanotubes such as VGCF (registered trademark). The shape of the carbon material is not particularly limited, and any shape such as spherical, plate, and fibrous may be used.

[0096] The volume ratio of the conductive material in the positive electrode layer is not particularly limited, and is, for example, preferably from 10% to 50%, and more preferably from 20% to 40%.

[0097] The thickness of the positive electrode layer is usually 0.1 to 30 μm, for example, preferably 1 to 20 μm. The thickness of the positive electrode layer is the average value of thicknesses measured at any 10 points in an SEM image.

[0098] In the positive electrode layer, the porosity is not particularly limited, but is preferably 20% or less, more preferably 15% or less, and further preferably 10% or less.

[0099] The porosity of the positive electrode layer was measured from an SEM image after FIB cross-section processing.

[0100] The positive electrode layer is a layer that may be called a “positive electrode active material layer.” The positive electrode layer may have a so-called positive electrode current collector or positive electrode current collector layer.

[0101] (Negative electrode layer) In the solid-state battery of the present invention, the negative electrode layer is not particularly limited. For example, the negative electrode layer may contain a negative electrode active material and may further contain the solid electrolyte ceramic of the present invention. By containing the solid electrolyte ceramic of the present invention in the negative electrode layer, it is possible to suppress short-circuiting of the solid-state battery. The negative electrode layer may have the form of a sintered body containing negative electrode active material particles. The negative electrode layer may be a layer capable of absorbing and releasing ions (particularly lithium ions).

[0102] The negative electrode active material is not particularly limited, and any negative electrode active material known in the field of solid-state batteries can be used. Examples of the negative electrode active material include carbon materials such as graphite, graphite-lithium compounds, lithium metal, lithium alloy particles, phosphoric acid compounds having a Nasicon structure, Li-containing oxides having a spinel structure, β II -Li3VO4 type structure, γ II The negative electrode active material is an oxide having a lithium metal, β II-Li3VO4 type structure, γ II It is preferable to use a Li-containing oxide having a -Li3VO4 type structure.

[0103] In the negative electrode layer, the oxide is β II -Li3VO4 type structure means that the oxide (particularly the particles) is β II -Li3VO4 type crystal structure, and in a broad sense, it is understood by those skilled in the art of solid-state batteries to have a β II -Li3VO4 type crystal structure. In the narrow sense, the oxide in the negative electrode layer is β II The term "having a -Li3VO4 type structure" means that the oxide (particularly the particles) is a so-called β II It means that the β-Li3VO4 type crystal structure exhibits one or more major peaks corresponding to Miller indices specific to the β-Li3VO4 type crystal structure at a given incidence angle. II An example of the Li-containing oxide having a -Li3VO4 type structure is Li3VO4.

[0104] In the negative electrode layer, the oxide is γ II -Li3VO4 type structure means that the oxide (particularly the particles) is γ II -Li3VO4 type crystal structure, and in a broad sense, it is known by those skilled in the art of solid-state batteries as γ II In the narrow sense, the oxide in the negative electrode layer is γ II The term "having a -Li3VO4 type structure" means that the oxide (particularly the particles) is a so-called γ II - means that the crystal structure of Li3VO4 type shows one or more major peaks corresponding to Miller indices specific to the Li3VO4 type crystal structure at a given angle of incidence (x-axis). II As the Li-containing oxide having the Li-Li3VO4 type structure, Li 3.2 V 0.8 S 0.2 O4 is an example.

[0105] The chemical composition of the negative electrode active material may be an average chemical composition. The average chemical composition of the negative electrode active material means the average value of the chemical composition of the negative electrode active material in the thickness direction of the negative electrode layer. The average chemical composition of the negative electrode active material can be analyzed and measured by breaking the solid-state battery and performing composition analysis by EDX (energy dispersive X-ray spectroscopy) in a field of view that includes the entire thickness direction of the negative electrode layer using SEM-EDX.

[0106] The negative electrode active material can be produced, for example, by the same method as that for the positive electrode active material, or can be obtained as a commercially available product.

[0107] The chemical composition and crystal structure of the anode active material in the anode layer may usually be changed by elemental diffusion during sintering in the manufacturing process of the solid-state battery. The anode active material may have the average chemical composition and crystal structure described above in the solid-state battery after sintering with the cathode layer and the solid electrolyte layer.

[0108] The volume ratio of the negative electrode active material in the negative electrode layer is not particularly limited, and is, for example, preferably 50% or more (particularly 50% or more and 99% or less), more preferably 70% or more and 95% or less, and even more preferably 80% or more and 90% or less.

[0109] The negative electrode layer may contain the solid electrolyte ceramic of the present invention as a solid electrolyte, and / or may contain a solid electrolyte other than the solid electrolyte ceramic of the present invention. The negative electrode layer may further include a sintering aid and / or a conductive material.

[0110] When the negative electrode layer contains the solid electrolyte ceramic of the present invention, the volume ratio of the solid electrolyte ceramic of the present invention may usually be 20% or more and 60% or less, particularly 30% or more and 45% or less.

[0111] As the sintering aid in the negative electrode layer, the same compounds as the sintering aid in the positive electrode layer can be used. As the conductive material in the negative electrode layer, the same compounds as the conductive material in the positive electrode layer can be used.

[0112] The thickness of the negative electrode layer is usually 0.1 to 30 μm, and preferably 1 to 20 μm. The thickness of the negative electrode layer is determined by averaging thicknesses measured at any ten points in an SEM image.

[0113] In the negative electrode layer, the porosity is not particularly limited, but is preferably 20% or less, more preferably 15% or less, and further preferably 10% or less.

[0114] The porosity of the negative electrode layer is a value measured in the same manner as the porosity of the positive electrode layer.

[0115] The negative electrode layer is a layer that may be called a “negative electrode active material layer.” The negative electrode layer may have a so-called negative electrode current collector or negative electrode current collector layer.

[0116] (Solid electrolyte layer) In the solid state battery of the present invention, the solid electrolyte layer preferably contains the above-mentioned solid electrolyte ceramic of the present invention from the viewpoints of superior ion conductivity and more sufficient suppression of an increase in electronic conductivity during operation.

[0117] The volume ratio of the solid electrolyte ceramic of the present invention in the solid electrolyte layer is not particularly limited, and from the viewpoint of better ion conductivity and more sufficient suppression of an increase in electronic conductivity during operation, it is preferably from 10% to 100%, more preferably from 20% to 100%, and even more preferably from 30% to 100%.

[0118] When the solid electrolyte layer contains the solid electrolyte ceramic of the present invention, it is sufficient that the solid electrolyte ceramic of the present invention having the above-mentioned chemical composition is present at least in the center of the thickness direction of the solid electrolyte layer (particularly at least 5 points, preferably at least 8 points, more preferably at least 10 points out of any 10 points). This is because the solid electrolyte layer is sandwiched between the positive electrode layer and the negative electrode layer, and element diffusion from the positive electrode layer and the negative electrode layer to the solid electrolyte layer and / or element diffusion from the solid electrolyte layer to the positive electrode layer and the negative electrode layer may occur due to sintering during the manufacturing process of the solid battery.

[0119] The solid electrolyte layer may contain, in addition to the garnet-type solid electrolyte ceramic of the present invention, one or more materials selected from a solid electrolyte composed of at least Li, Zr, and O, a solid electrolyte having a γ-Li3VO4 structure, and an oxide glass ceramic-based lithium ion conductor. An example of a solid electrolyte composed of at least Li, Zr, and O is Li2ZrO3.

[0120] An example of a solid electrolyte having a γ-Li3VO4 structure is a solid electrolyte having an average chemical composition represented by the following general formula (III).

[0121] [ka]

[0122] In formula (III), A is one or more elements selected from the group consisting of Na, K, Mg, Ca, Al, Ga, Zn, Fe, Cr, and Co. B is one or more elements selected from the group consisting of V and P. D is one or more elements selected from the group consisting of Zn, Al, Ga, Si, Ge, Sn, As, Ti, Mo, W, Fe, Cr, and Co. x satisfies 0≦x≦1.0, in particular 0≦x≦0.2. The value of y satisfies 0≦y≦1.0, and in particular 0.20≦y≦0.50. a is the average valence of A. The average valence of A is the value expressed as (n1×a+n2×b+n3×c) / (n1+n2+n3) when, for example, A contains n1 element X with a valence of a+, n2 element Y with a valence of b+, and n3 element Z with a valence of c+. c is the average valence of D. The average valence of D is the same as the average valence of A described above when, for example, n1 element X with a valence a+, n2 element Y with a valence b+, and n3 element Z with a valence c+ are recognized as D.

[0123] Specific examples of solid electrolytes having a γ-Li3VO4 structure include Li 3.2 (V 0.8 S 0.2 )O4, Li 3.5 (V 0.5 Ge 0.5 )O4, Li 3.4 (P 0.6 Si0.4)O4, Li 3.5 (P 0.5 Ge 0.5 )O4, etc.

[0124] As the oxide glass ceramic-based lithium ion conductor, for example, a phosphate compound containing lithium, aluminum, and titanium as constituent elements (LATP) or a phosphate compound containing lithium, aluminum, and germanium as constituent elements (LAGP) can be used.

[0125] The solid electrolyte layer may further contain, in addition to the solid electrolyte, for example, a sintering aid. As the sintering aid in the solid electrolyte layer, the same compounds as the sintering aid in the positive electrode layer can be used.

[0126] The volume proportion of the sintering aid in the solid electrolyte layer is not particularly limited, and from the viewpoint of better ion conductivity and more sufficient suppression of an increase in electronic conductivity during operation, it is preferably from 0% to 20%, and more preferably from 1% to 10%.

[0127] The thickness of the solid electrolyte layer is usually 0.1 to 30 μm, and preferably 1 to 20 μm from the viewpoint of better ion conductivity and more sufficient suppression of an increase in electronic conductivity during operation. The thickness of the solid electrolyte layer is the average value of thicknesses measured at any 10 points in an SEM image.

[0128] In the solid electrolyte layer, the porosity is not particularly limited, and from the viewpoint of better ion conductivity and more sufficient suppression of an increase in electronic conductivity during operation, it is preferably 20% or less, more preferably 15% or less, and even more preferably 10% or less.

[0129] The porosity of the solid electrolyte layer is a value measured in the same manner as the porosity of the positive electrode layer.

[0130] [Solid-state battery manufacturing method] The solid-state battery can be manufactured, for example, by the so-called green sheet method, the printing method or a combination of these methods.

[0131] The green sheet method will now be described. First, a paste is prepared by appropriately mixing a solvent, a binder, etc. with a positive electrode active material. The paste is applied onto a sheet and dried to form a first green sheet for forming a positive electrode layer. The first green sheet may contain a solid electrolyte, a conductive material, and / or a sintering aid, etc.

[0132] A paste is prepared by appropriately mixing the negative electrode active material with a solvent, a binder, etc. The paste is applied onto a sheet and dried to form a second green sheet for forming the negative electrode layer. The second green sheet may contain a solid electrolyte, a conductive material, and / or a sintering aid, etc.

[0133] A paste is prepared by appropriately mixing the solid electrolyte with a solvent, a binder, etc. The paste is applied and dried to prepare a third green sheet for forming the solid electrolyte layer. The third green sheet may contain a sintering aid, etc.

[0134] The solvent for producing the first to third green sheets is not particularly limited, and for example, a solvent that can be used in the manufacture of a positive electrode layer, a negative electrode layer, or a solid electrolyte layer in the field of solid state batteries is used. As the solvent, a solvent that can be used with the binder described below is usually used. As such a solvent, for example, alcohol such as 2-propanol is included.

[0135] The binder for producing the first to third green sheets is not particularly limited, and for example, a binder that can be used in the manufacture of a positive electrode layer, a negative electrode layer, or a solid electrolyte layer in the field of solid state batteries is used. Examples of such binders include butyral resin, acrylic resin, etc.

[0136] Next, the first to third green sheets are appropriately laminated to prepare a laminate. The laminate thus prepared may be pressed. A preferred pressing method is a hydrostatic pressing method. Thereafter, the laminate is sintered at, for example, 600 to 800° C. to obtain a solid-state battery.

[0137] The printing method will be explained. The printing method is similar to the green sheet method, except for the following: Prepare ink for each layer having the same composition as the paste for each layer used to obtain the green sheet, except that the amounts of solvent and resin are suitable for use as an ink. · Each layer is printed using ink and laminated to create a laminate.

[0138] The present invention will be described in more detail below based on specific examples. However, the present invention is not limited to the following examples and can be modified as appropriate within the scope of the present invention. EXAMPLES

[0139] <Experimental Example 1: Solid electrolyte ceramics with uniform Bi concentration structure> <Examples 1A to 14A, 1B to 3B, and 1C to 4C, and Comparative Example 1> [Manufacturing of solid electrolyte ceramics] The raw materials are lithium hydroxide monohydrate (LiOH·H2O), lanthanum hydroxide (La(OH)3), Zirconium oxide ZrO2, tantalum oxide Ta2O5, bismuth oxide Bi2O3, cobalt oxide Co3O4, basic nickel carbonate hydrate NiCO3·2Ni(OH)2·4H2O, and manganese carbonate MnCO3 were used. Each starting material was weighed out so as to have a chemical composition as shown in Table 1, Table 2 or Table 3. Water was added, the mixture was placed in a polyethylene pot, and the pot was rotated at 150 rpm for 16 hours to mix the raw materials. In addition, lithium hydroxide monohydrate (LiOH·H2O), the Li source, was charged in an amount 3 wt% in excess of the target composition, taking into account Li deficiency during sintering. The obtained slurry was evaporated and dried, and then calcined in O2 at 900°C for 5 hours to obtain the target phase. A mixed solvent of toluene and acetone was added to the calcined powder and pulverized in a planetary ball mill for 12 hours. The pulverized powder was confirmed to have no compositional deviation by ICP measurement. The average particle size of the pulverized powder was 150 nm.

[0140] [Manufacturing of solid electrolyte single plate] As an evaluation sample of the solid electrolyte ceramics, a solid electrolyte single plate was produced by the following method.

[0141] The obtained pulverized powder was mixed with butyral resin, alcohol, and a binder to produce a slurry. The slurry was molded onto a PET film using a doctor blade method to obtain a sheet. The sheets were laminated until the sheet thickness reached 200 μm, then cut into a square shape measuring 10 mm x 10 mm. The binder was removed at 400°C, and the sheet was sintered at 950°C for 300 minutes under a pressure of 100 MPa to produce a solid electrolyte single plate. The porosity of the solid electrolyte single plate was 10% or less, and it was confirmed that the sintering had progressed sufficiently. The surface of the obtained sintered body was polished to obtain a garnet solid electrolyte substrate.

[0142] [Crystal structure of solid electrolyte single plate] In all of the Examples and Comparative Examples, it was confirmed that X-ray diffraction patterns attributable to a crystal structure similar to that of a garnet type were obtained by X-ray diffraction of the solid electrolyte single plate (ICDD Card No. 00-045-0109).

[0143] [Chemical composition of solid electrolyte plate] The solid electrolyte single plate was subjected to ICP-AES analysis to obtain the average chemical composition of the solid electrolyte single plate. The contents of Co, Mn and Ni in the average chemical composition of the entire solid electrolyte single plate were calculated as a percentage of the content of B in the above general formula (I) of the garnet-type crystal structure (for example, the total number of La and B in the above general formula (II)) taken as 100 mol%. In Example 2A, quantitative analysis was also performed using LA-ICP-MS, and it was confirmed that the results were equivalent. Furthermore, in Examples 4A, 5A, 13A, and 14A, quantitative analysis was performed using WDX, and it was confirmed that the results were equivalent.

[0144] [Electronic conductivity measurement (before and after storage test)] An Au electrode was sputtered onto one side of the obtained single plate to make it the working electrode. Li metal with the same area as the Au electrode was attached to the other side. Finally, the cell was sealed in a 2035 size coin cell to make it the evaluation cell. All of the above operations were carried out in a dry room with a dew point of -40°C or less. A voltage of 2 V was applied to the working electrode relative to Li at room temperature, and the transient current was observed. The current that flowed 10 hours after the voltage application was read as the leakage current before the storage test. The leakage current value before the storage test was approximately 1×10 -10 ~6×10 -7 It was confirmed that the electrical conductivity was within the range of S / cm. After that, the cell was stored at 90°C for about one month, and the above test was performed again to read the leakage current after the storage test. The electronic conductivity was calculated from the leakage current using the following formula. Electronic conductivity = (I / V) x (L / A) (I: leakage current, V: applied voltage, L: solid electrolyte plate thickness, A: electrode area) The electronic conductivity after the storage test was evaluated according to the following criteria. ◎: Electronic conductivity <1.0×10 -8 S / cm(excellent); ○;1.0×10 -8 S / cm≦Electronic conductivity<1.0×10 -7 S / cm(good); △;1.0×10 -7 S / cm≦Electronic conductivity<1.0×10 -6 S / cm (Acceptable) (No problem in practical use); ×;1.0×10 -6 S / cm ≦ Electronic conductivity (unacceptable) (problems in practical use).

[0145] [Ionic conductivity measurement] A gold (Au) layer was formed on both sides of the solid electrolyte plate as a current collector by sputtering, and then the plate was sandwiched and fixed between SUS current collectors. The sintered tablets of each solid electrolyte were subjected to AC impedance measurement at room temperature (25°C) in the range of 0.1Hz to 10MHz (±50mV) to evaluate the ionic conductivity. ◎:5.0×10 -4 S / cm ≤ ionic conductivity (excellent); ○;1.0×10 -4 S / cm≦Ionic conductivity<5.0×10 -4 S / cm(good); △;5.0×10 -5 S / cm≦Ionic conductivity<1.0×10 -4 S / cm (Acceptable) (No problem in practical use); ×; ionic conductivity < 5.0 × 10 -5 S / cm (not possible) (problems in practical use).

[0146] [Table 1]

[0147] [Table 2]

[0148] [Table 3]

[0149] The following is clear from Table 1. As can be seen from Comparative Example 1, when a storage test is performed at 90°C with Li attached to the Bi-substituted garnet-type solid electrolyte, the electronic conductivity increases rapidly. This is thought to be because the Bi-substituted garnet-type solid electrolyte is prone to forming Li-Bi-O-based compounds as heterogeneous phases at the grain boundaries, and these Li-Bi-O-based compounds are reduced by Li to exhibit electronic conductivity. A comparison between Comparative Example 1 and Examples 1A to 12A shows that the Bi-substituted garnet-type solid electrolyte containing one or more transition metal elements selected from Co, Mn, and Ni significantly reduces the electronic conductivity after the storage test. This is believed to be because the Bi-substituted garnet-type solid electrolyte containing one or more transition metal elements selected from Co, Mn, and Ni suppresses the formation of Li-Bi-O-based compounds that are the cause of electronic conductivity. From the above, it is possible to construct an all-solid-state battery with low leakage current even when maintained at high temperatures by including a Bi-substituted garnet-type solid electrolyte containing one or more transition metal elements selected from Co, Mn, and Ni. From the comparison of Examples 1A to 6A, it is found that the leakage current after the storage test also changes depending on the Co content. It is found that the Co content is preferably more than 0 mol% and not more than 1.20 mol%, more preferably more than 0 mol% and not more than 0.25 mol%. That is, it is found that the electronic conductivity increases even if the Co content is too high. This is considered to be because, although an increase in the Co content suppresses the formation of Li-Bi-O-based compounds, an excessive increase in the Co amount generates a heterogeneous phase having Li-La-Co-O-based electronic conductivity. Measurement of electronic conductivity before storage also showed that if the amount of Co added is too large, the electronic conductivity before storage becomes high, so the total content of transition metal elements is preferably more than 0 mol% and not more than 1.20 mol%, more preferably more than 0 mol% and not more than 0.50 mol% (e.g., 0.01 mol% or more and 0.50 mol% or less), and even more preferably more than 0 mol% and not more than 0.25 mol% (e.g., 0.01 mol% or more and 0.20 mol% or less), when the content of B is 100 mol%. From a comparison of Examples 4A to 12A, it is clear that when the Bi-substituted garnet-type solid electrolyte contains Co among Ni, Mn, and Co, the effect of reducing the electronic conductivity is particularly large.

[0150] The following is clear from Table 2. From Examples 3A and 1B to 3B, it can be seen that the Bi substitution amount in the garnet-type solid electrolyte affects the electronic conductivity after the storage test. From the viewpoint of reducing the electronic conductivity after the storage test, it can be seen that a smaller Bi substitution amount is preferable. It was found that the electronic conductivity increased significantly in Example 3B. This is thought to be because if the Bi substitution amount in the garnet-type solid electrolyte increases too much, not only is it easy to form Li-Bi-O-based compounds, but the garnet-type solid electrolyte itself is also easily reduced and decomposed.

[0151] The following is clear from Table 3. From Examples 1C to 4C, the effects of the present invention can be obtained even when γ in general formula (I) has various values.

[0152] <Experimental Example 2: Bi-uniform structure type and Bi-gradient structure type solid electrolyte ceramics> <Example 1D and Comparative Example 2> The solid electrolyte ceramics with a uniform Bi concentration structure and the solid electrolyte single plate were produced, the crystal structure and chemical composition of the solid electrolyte single plate were evaluated, and the electronic conductivity and ionic conductivity were measured in the same manner as in Example 1A, except that the starting materials were weighed so that the chemical compositions were as shown in Table 3. In these Examples and Comparative Examples, it was confirmed that, by X-ray diffraction of the solid electrolyte single plate, an X-ray diffraction pattern that can be assigned to a crystal structure similar to that of a garnet type was obtained (ICDD Card No. 00-045-0109).

[0153] <Example 2D and Comparative Example 3> The solid electrolyte single plate was produced, the crystal structure and chemical composition of the solid electrolyte single plate were evaluated, and the electronic conductivity and ionic conductivity were measured in the same manner as in Example 1A, except that a Bi concentration gradient structure type solid electrolyte ceramic produced by the following method was used. In these examples and comparative examples, it was confirmed by X-ray diffraction of the solid electrolyte single plate that the X-ray diffraction pattern of the ceramic single plate can be attributed to a crystal structure similar to that of a garnet type (ICDD Card No. 00-045-0109). In addition, it was confirmed by TEM-EDX that the Bi concentration gradient structure was formed.

[0154] [Fabrication of solid electrolyte ceramics with Bi concentration gradient structure] Core particles and shell layers were prepared for producing solid electrolyte ceramics with a Bi concentration gradient structure.

[0155] (Production of core particles) As the core particles, a garnet-type solid electrolyte powder was produced as follows. The raw materials are lithium hydroxide monohydrate (LiOH·H2O), lanthanum hydroxide (La(OH)3), Zirconium oxide ZrO2, tantalum oxide Ta2O5, bismuth oxide Bi2O3, and cobalt oxide Co3O4 were used. The chemical composition of each raw material is Li in Comparative Example 3. 6.6 La3(Zr 1.6 Ta 0.4 )O 12 In Example 2D, Li 6.6 La3(Zr 1.6 Ta 0.4 )O 12 The raw materials were weighed out so that the total amount was -0.0050Co, water was added, and the mixture was sealed in a 100 ml polyethylene pot and rotated on a pot rack at 150 rpm for 16 hours to mix the raw materials. In addition, lithium hydroxide monohydrate LiOH·H2O, the Li source, was charged in an amount 3 wt% in excess of the target composition, taking into account Li deficiency during sintering. The resulting slurry was evaporated and dried, and then calcined at 900°C for 5 hours to obtain the target phase. A mixed solvent of toluene and acetone was added to the calcined powder obtained, and the mixture was ground in a planetary ball mill for 6 hours. The pulverized powder was dried to obtain a solid electrolyte powder. It was confirmed by ICP measurement that the powder had no composition deviation. The average particle size of the core particles was 150 nm. In the examples and comparative examples, the primary particle size of the material was not changed, and the structure and composition were controlled by the composition, molar ratio, and firing time of the core and shell phases.

[0156] (Production of powder with core particles coated with a shell layer) A powder in which core particles were coated with a garnet-type solid electrolyte as a shell layer was produced as follows. The raw materials used were lithium nitrate LiNO3, lanthanum nitrate hexahydrate La(NO3)3·6H2O, bismuth nitrate pentahydrate Bi(NO3)3·5H2O, zirconium(IV) isopropoxide Zr(OC3H7)4, tantalum(V) ethoxide Ta(OC2H5)5, cobalt nitrate hexahydrate Co(NO3)2·6H2O, and ethyl acetoacetate. 6.0 La3(Zr 1.0 Ta 0.4 Bi 0.6 )O 12 In Example 2D, Li 6.0 La3(Zr 1.0 Ta0.4 Bi 0.6 )O 12 The mixture was weighed so as to satisfy the chemical composition of -0.0050Co. Ethyl acetoacetate was weighed so as to have a molar amount four times that of each alkoxide. First, each alkoxide and ethyl acetoacetate were placed in a glass container and stirred with a stirrer piece for 30 minutes (referred to as solution A). Next, each nitrate and 2-methoxyethanol were placed in a glass container and the nitrate was dissolved (referred to as solution B). Solution A was gradually dropped into solution B to prepare a uniform solution C. After mixing a specific core particle with solution C, the mixture was mixed for 5 hours using a stirrer piece, and then the solvent was evaporated at 100 ° C. The obtained dried powder was heat-treated at 700 ° C for 5 hours to obtain a garnet-type solid electrolyte powder having a shell layer on the core particle. Solution C alone was dried and then heat-treated at 700° C. for 5 hours to obtain a shell layer powder. XRD measurement of the above shell layer powder confirmed that a garnet-type solid electrolyte was obtained. Furthermore, ICP measurement of the above powder confirmed that there was no composition deviation in the shell layer.

[0157] [measurement] (Bi content in the vicinity of grain boundaries (x1)) After processing the solid electrolyte single plate into a thin piece by FIB processing, quantitative analysis (composition analysis) was performed by EDX point analysis of 20 arbitrary points in the vicinity of the grain boundary of each of 10 arbitrary sintered particles to obtain the Bi / D ratio in the vicinity of the grain boundary. The Bi amount x in formula (I) was calculated from the Bi / D ratio in the vicinity of the grain boundary, and this was defined as the Bi amount (x1) in the vicinity of the grain boundary.

[0158] (Bi content inside particle (x2)) After processing the solid electrolyte single plate into a thin piece by FIB processing, quantitative analysis (composition analysis) was performed by EDX (energy dispersive X-ray spectroscopy) at 20 arbitrary points inside each of 10 arbitrary sintered particles to obtain the Bi / D ratio inside the particle. The Bi amount x in formula (I) was calculated from the Bi / D ratio inside the particle, and this was used as the Bi amount (x2) near the grain boundary.

[0159] [Table 4]

[0160] The following is clear from Table 3. Comparative Examples 2 and 3 have the same average chemical composition, but Comparative Example 3 shows the electronic conductivity after the storage test of a garnet-type solid electrolyte in which the Bi substitution amount is increased near the grain boundary. Comparison between Comparative Example 2 and Comparative Example 3 and comparison between Example 1D and Example 2D shows that the electronic conductivity after the storage test is increased in the solid electrolyte in which the Bi substitution amount is increased near the grain boundary compared to the solid electrolyte in which Bi is uniformly dissolved. This is considered to be because the increase in the Bi substitution amount near the grain boundary makes it easier to form a Li-Bi-O-based heterogeneous phase at the grain boundary. Comparison between Comparative Example 3 and Example 2D shows that the electronic conductivity after the storage test is significantly improved even in the garnet-type solid electrolyte in which the Bi substitution amount is increased near the grain boundary by the solid electrolyte containing Co. Also, it is shown that the effect of Co inclusion is particularly large in the garnet-type solid electrolyte in which the Bi substitution amount is increased near the grain boundary (Example 2D) compared to the solid electrolyte in which Bi is uniformly dissolved (Comparative Example 2, Example 1D). Thus, it is clear that the effect of the present invention is particularly effective for garnet-type solid electrolytes in which the amount of Bi substitution is increased in the vicinity of the grain boundaries.

[0161] (TEM-EELS measurement) The solid electrolyte used in Example 5A and lithium cobalt oxide LiCoO2 were weighed out so that the volume ratio was 1:1 to prepare a mixed powder. The resulting mixed powder was kneaded with butyral resin, alcohol, and a binder to produce a slurry. The slurry was cast into a sheet on a PET film by a doctor blade method to obtain a positive electrode sheet. The solid electrolyte sheets prepared in the same manner as in Example 5A were laminated to a thickness of 200 μm to prepare a solid electrolyte laminate. The above-prepared positive electrode sheets were laminated to a thickness of 30 μm to prepare a positive electrode laminate. The obtained solid electrolyte laminate and positive electrode laminate were laminated and then pressed together to obtain a positive electrode / solid electrolyte sheet laminate. The sheets were cut into a square shape of 10 mm×10 mm in size, and the binder was removed at 400° C., followed by pressure sintering at 800° C. for 120 minutes under a pressure of 100 MPa to prepare a positive electrode / solid electrolyte co-fired body. A positive electrode half cell was prepared by attaching Li metal to the surface opposite to the positive electrode of the obtained positive electrode / solid electrolyte co-fired body. The positive electrode layer of the prepared positive electrode half cell was exfoliated by FIB processing, and EELS measurements were performed on the solid electrolyte particles in the positive electrode layer using a TEM (JEOL-JEM-ARM200F NEOARMex) and an EELS (Gatan Continuum ER). Figure 2 shows the EELS spectrum of the bulk particles in the solid electrolyte. A peak originating from the L-end of Co was detected, indicating that Co is contained in the solid electrolyte particles. It was also found that the peak position (LLZ) was observed on the lower energy side compared to the peak position of LiCoO2 (lithium cobalt oxide) (LCO) of the reference material. For Example 5A, the shift width sw (see Figure 2) between the Co L-end peak position in the solid electrolyte ceramic (LLZ) of the present invention and the Co L-end peak position of LiCoO2 (LCO) was 0.9 eV. The first derivative peak intensity of the obtained EELS spectrum was used as the quantification method. Specifically, the maximum value I max and the minimum value I min and calculate the difference between them (I max -I min ) was used as the peak intensity, and the Co / La ratio was calculated by dividing the Co L-end peak intensity by the La M-end peak intensity. In this way, EELS measurements were performed at five arbitrary points in the solid electrolyte grain, the Co / La ratio was calculated for each, and the Co / La ratio was obtained by averaging these values. As a result, the Co / La ratio was 0.8%, which was found to be approximately the same as the value measured by ICP. [Industrial Applicability]

[0162] A solid-state battery including the solid electrolyte ceramic of the present invention can be used in various fields where battery use or power storage is expected. By way of example only, a solid-state battery according to an embodiment of the present invention can be used in the field of electronics packaging. The solid-state battery according to an embodiment of the present invention can also be used in the electrical, information, and communication fields in which mobile devices and the like are used (e.g., electrical and electronic devices fields including small electronic devices such as mobile phones, smartphones, smart watches, notebook computers, digital cameras, activity meters, arm computers, electronic paper, wearable devices, RFID tags, card-type electronic money, and smart watches, or mobile device fields), household and small industrial applications (e.g., power tools, golf carts, household, nursing care, and industrial robots), large industrial applications (e.g., forklifts, elevators, and port cranes), transportation systems (e.g., hybrid cars, electric cars, buses, trains, electrically assisted bicycles, and electric motorcycles), power system applications (e.g., various power generation, road conditioners, smart grids, and general household storage systems), medical applications (medical devices such as earphones and hearing aids), pharmaceutical applications (medical management systems), IoT, and space and deep sea applications (e.g., space probes, submersible research vessels, and the like).

Claims

1. Contains at least Li (lithium), La (lanthanum), Bi (bismuth) and O (oxygen), A solid electrolyte ceramic having a garnet-type crystal structure, further comprising one or more transition metal elements selected from the group consisting of Co (cobalt), Ni (nickel) and Mn (manganese), The solid electrolyte ceramic further includes one or more elements D selected from the group consisting of transition elements capable of forming 6-coordination with oxygen and typical elements belonging to groups 12 to 15, the element D including at least Bi (bismuth); The content of the Bi (bismuth) is more than 0 mol % and 25 mol % or less when the content of the element D is 100 mol %.

2. The solid electrolyte ceramic according to claim 1, wherein the solid electrolyte ceramic has a chemical composition represented by the following general formula (I) and further contains one or more transition metal elements: 【Chemistry 1】 (In formula (I), A is one or more elements selected from the group consisting of Li (lithium), Ga (gallium), Al (aluminum), Mg (magnesium), Zn (zinc) and Sc (scandium), and includes at least Li (lithium); B is one or more elements selected from the group consisting of La (lanthanum), Ca (calcium), Sr (strontium), Ba (barium), and lanthanoid elements, including at least La (lanthanum); D is the element D and includes at least Zr (zirconium), Ta (tantalum) and Bi (bismuth); α satisfies 5.0≦α≦8.0; β satisfies 2.5≦β≦3.5; γ satisfies 1.5≦γ≦2.5; (ω satisfies 11≦ω≦13).

3. The solid electrolyte ceramic according to claim 2, wherein the total content of the one or more transition metal elements is more than 0 mol % and not more than 3.50 mol % when the content of B is 100 mol %.

4. The solid electrolyte ceramic according to claim 2, wherein the total content of the one or more transition metal elements is more than 0 mol % and 1.20 mol % or less when the content of B is 100 mol %.

5. 3. The solid electrolyte ceramic according to claim 2, wherein the total content of the one or more transition metal elements is more than 0 mol % and 0.25 mol % or less when the content of B is 100 mol %.

6. The solid electrolyte ceramic according to any one of claims 1 to 5, wherein the one or more transition metal elements include Co.

7. 7. The solid electrolyte ceramic according to claim 1, wherein the Bi concentration in the vicinity of grain boundaries is higher than the Bi concentration inside the grains.

8. The Bi content in the grain boundary vicinity portion is x (hereinafter, referred to as “x”), where x is twice the molar ratio of Bi in the D in the garnet-type crystal structure. 1 ") and the Bi content x inside the particle (hereinafter referred to as "x 2 ") is expressed by the following relationship: x 2 <x 1 The solid electrolyte ceramic according to claim 7, which satisfies the above.

9. The amount of Bi in the vicinity of the grain boundary x 1 and the amount of Bi inside the particle x 2 The solid electrolyte ceramic according to claim 8, which satisfies the following relational expression: 0<x 1 ≦0.80; and 0≦x 2 ≦0.30。

10. The amount of Bi in the vicinity of the grain boundary x 1 and the amount of Bi inside the particle x 2 The solid electrolyte ceramic according to claim 8 or 9, which satisfies the following relational expression: 0.01≦x 1 -x 2 。

11. In the electron energy loss spectrum of the solid electrolyte ceramic, the peak position of the Co L edge is LiCoO 2 The solid electrolyte ceramic according to any one of claims 1 to 10, wherein the peak position of Co L edge is lower than that of Co L edge.

12. A solid-state battery comprising the solid electrolyte ceramic according to any one of claims 1 to 11.

13. the solid-state battery includes a positive electrode layer, a negative electrode layer, and a solid electrolyte layer laminated between the positive electrode layer and the negative electrode layer, The solid-state battery according to claim 12 , wherein the positive electrode layer and the negative electrode layer are layers capable of absorbing and releasing lithium ions.

14. The solid-state battery according to claim 13 , wherein the solid electrolyte layer is integrally sintered with the positive electrode layer and the negative electrode layer.

15. The solid-state battery according to any one of claims 12 to 14, wherein the solid electrolyte ceramic is contained in a solid electrolyte layer of the solid-state battery.

Citation Information

Patent Citations

  • Solid electrolyte ceramics material

    JP2015050071A

  • Stabilizing Coatings for Solid-State Batteries

    JP2019530963A

Cited By

  • Solid-state battery

    WO2026204110A1