Electrode and method for producing same, battery and electric device

A gas-permeable current collector layer with a porous structure addresses gas-related cell expansion in batteries, improving performance and stability by allowing gas to escape, thus preventing deformation.

JP7583907B2Active Publication Date: 2024-11-14CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023501834
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-18
Publication Date
2024-11-14
Estimated Expiration
2041-09-18

AI Technical Summary

Technical Problem

The generation of gas during the charging and discharging process in batteries due to electrolyte and electrode interactions leads to cell expansion and deformation, affecting battery performance and lifespan.

Method used

Incorporating a gas-permeable current collector layer with a porous structure and a conductive layer to allow gas to escape, reducing cell expansion and improving battery performance.

Benefits of technology

The design effectively vents generated gas, preventing cell deformation and enhancing battery performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583907000001
    Figure 0007583907000001
  • Figure 0007583907000002
    Figure 0007583907000002
  • Figure 0007583907000003
    Figure 0007583907000003
Patent Text Reader

Abstract

This application discloses an electrode, a manufacturing method thereof, a battery, and an electric device. The electrode includes a porous, gas-permeable current collector layer, and an active material layer laminated on at least a portion of the surface of the current collector layer and disposed outside the pores of the porous structure.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of batteries, and in particular to electrodes and methods for their manufacture, batteries and electrical devices. [Background technology]

[0002] Energy saving and emission reduction are the keys to the sustainable development of the automotive industry, and electric vehicles have become an important part of the sustainable development of the automotive industry due to their energy saving and environmental protection advantages. In electric vehicles, battery technology is one of the key factors related to their development.

[0003] When a battery is charged or discharged, chemical reactions can occur due to contact between the electrolyte and the positive and negative electrodes, generating gases that can affect the use of the battery. Summary of the Invention [Problem to be solved by the invention]

[0004] In view of the above-mentioned problems, the present application provides an electrode having improved gas permeability, capable of mitigating cell expansion due to gas generation during use of the battery, and further improving the overall performance of the battery, a manufacturing method thereof, a battery, and an electric device. [Means for solving the problem]

[0005] In a first aspect, the present application provides an electrode including a current collector layer having a porous structure and being gas permeable, and an active material layer laminated on at least a portion of a surface of the current collector layer and disposed outside the pores of the porous structure.

[0006] In the technical solution of the embodiment of the present application, the current collector layer is gas permeable, and with this design, when gas is generated in the battery due to contact between the electrolyte and the positive and negative electrodes, the gas can smoothly overflow outside the cell through the current collector layer, avoiding deformation and structural failure caused by gas expansion inside the cell, and further improving the performance of the battery.

[0007] In some embodiments, the material of the current collector layer includes a conductive material, such as a metal material, a carbon-based conductive material, a conductive polymer material, or a combination thereof. By adopting the conductive material, the current collector layer has a relatively good electrical conductivity.

[0008] In some embodiments, the current collector layer includes a porous matrix and a conductive layer covering at least a portion of the surface of the porous matrix. The current collector of the present embodiment has a composite structure including a porous matrix and a conductive layer. The porous matrix serves to support the current collector structure, and the conductive layer serves to conduct electricity, and both have their own advantages and function synergistically to provide the current collector layer with improved overall performance.

[0009] In some embodiments, the electrical conductivity of the conductive layer is greater than that of the porous matrix, and such a design allows the conductive layer to adopt a material with a relatively high electrical conductivity and the porous matrix to adopt a material with a relatively low electrical conductivity, thereby reducing the amount of high electrical conductivity material used and reducing costs, while essentially not affecting the electrical conductivity of the current collector surface and not affecting the electron transport at the interface between the current collector and the active material.

[0010] In some embodiments, the density of the porous matrix is ​​less than that of the conductive layer. With this design, the conductive layer adopts a material with a relatively high electrical conductivity (e.g., a metal material) and the porous matrix adopts a material with a relatively low density (e.g., a polymer material), thereby reducing the density of the entire current collector layer while essentially not affecting the electrical conductivity of the current collector surface and not affecting electron transport at the interface between the current collector and the active material.

[0011] In some embodiments, the material of the porous matrix includes a polymer. Optionally, the polymer is selected from one or more of polyamide, polyimide, polyester, polyolefin, polyalkyne, siloxane polymer, polyether, polyalcohol, polysulfone, polysaccharide polymer, amino acid polymer, polysulfur nitride, aromatic ring polymer, aromatic heterocyclic polymer, epoxy resin, phenolic resin, derivatives thereof, crosslinked products thereof, and copolymers thereof, or combinations thereof. Such a design can reduce the density of the entire current collector layer.

[0012] In some embodiments, the material of the conductive layer includes a metal, and optionally, the metal is selected from aluminum, copper, nickel, iron, titanium, silver, nickel, or an alloy of any one of them. Such a design can improve the conductive performance of the current collector layer.

[0013] In some embodiments, the porosity of the current collector layer is 20% or more, for example, 20% to 95%. When the porosity of the current collector layer is 20% to 95%, the electrode has good gas permeability as well as good structural strength and stability.

[0014] In some embodiments, the thickness of the current collector layer is 4 μm or more, for example, 4 μm to 500 μm. By making the thickness of the current collector layer 4 μm or more, the current collector has good structural strength and stability. When the thickness of the current collector layer is 4 μm to 500 μm, the electrode has good structural strength and stability, and has a relatively low weight and volume fraction in the battery, and further, the battery has a high volumetric energy density or gravimetric energy density.

[0015] In some embodiments, the gas permeability of the current collector layer is 1000 to 5000 cm 3 / m 2 24h 0.1Mpa (e.g., 1000~2000cm 3 / m 2 24h 0.1Mpa, 2000~3000cm3 / m 2 24h 0.1Mpa, 3000~4000cm 3 / m 2 24h 0.1Mpa or 4000~5000cm 3 / m 2 ·24h·0.1Mpa). This design allows the current collector to have high gas permeability, which is helpful for gas discharge. The test standard can be found in GB / T1038-2000 "Test method for gas permeability of plastic films and sheets by differential pressure method".

[0016] In some embodiments, the tortuosity of the current collector layer is ≧1, for example, 1.0-6.0 (for example, 1.0-2.0, 2.0-3.0, 3.0-4.0, 4.0-5.0, or 5.0-6.0). With this design, the electrode is easily infiltrated by the electrolyte, and the electrolyte is easily raised along the electrode. The tortuosity test criterion is based on the Bruggeman relationship: τ=ε α where τ is the tortuosity, ε is the porosity, and α is the Bruggeman coefficient (-1≦α≦-0.5).

[0017] In some embodiments, the electrode further includes an electrical connection member (e.g., a tab) attached to the current collector layer and electrically connected to the current collector layer, in which the electrical connection member is a member for conducting electrode current.

[0018] In some embodiments, at least one side of the porous matrix includes at least one edge region, and the area other than the edge region is covered by the conductive layer. In this solution, the edge region is not covered by the conductive layer, and the edge region is non-conductive. The edge region is not covered by the active material layer, and the edge region can prevent the active material layer from directly contacting the battery end cap and protect the active material layer. In addition, since the tab is usually attached to the edge of the current collector layer, the non-conductive edge region protects the tab while preventing the tab from contacting the opposite electrode and shorting out.

[0019] In some embodiments, the surface of the current collector layer includes an active material region and a support region, the active material layer is laminated on the active material region of the current collector layer, and the electrode further includes a support layer, the support layer is laminated on the support region of the surface. In some embodiments, the material of the support layer includes ceramics (e.g., a coating layer containing ceramic particles). In this solution, the support layer has a role of structural reinforcement, and such a design can improve the structural strength and structural stability of the electrode.

[0020] In some embodiments, the active material layer comprises an electrochemical active material, and optionally the electrochemical active material is selected from a lithium ion battery positive electrode active material or a lithium ion battery negative electrode active material, and optionally the lithium ion battery positive electrode active material is selected from a lithium-containing phosphate having an olivine structure, a lithium transition metal oxide, or a combination thereof, and optionally the lithium ion battery negative electrode active material is selected from artificial graphite, natural graphite, soft carbon, hard carbon, a silicon-based material, a tin-based material, lithium titanate, lithium metal, or a combination thereof. In this solution, the electrode according to the present application can be used in combination with each electrochemical active material.

[0021] In a second aspect, the present application provides a method for producing an electrode, the method comprising: providing a current collector layer having a porous matrix and being gas permeable; providing an active material layer; and laminating the active material layer on at least a portion of a surface of the current collector layer such that the active material layer is disposed outside the pores of the porous matrix. The electrode obtained by the method has improved gas permeability.

[0022] In some embodiments, a method of making an electrode includes the steps of producing a current collector layer comprising providing a porous matrix and depositing a conductive layer on at least a portion of a surface of the porous matrix, optionally wherein the deposition is selected from electroplating, electroless plating, vapor deposition, magnetron spackling, or a combination thereof, and the resulting electrode has improved gas permeability.

[0023] In some embodiments, the electrical conductivity of the porous matrix is ​​less than the electrical conductivity of the conductive layer, such that the electrode obtained by the method has improved electrical conductivity.

[0024] In some embodiments, the density of the porous matrix is ​​less than the density of the conductive layer, resulting in an electrode having a low density.

[0025] In a third aspect, the present application provides a battery including the electrode according to any of the above-mentioned embodiments or the electrode obtained by the method according to any of the above-mentioned embodiments.

[0026] In a fourth aspect, the present application provides an electric device including a battery according to any of the above-described embodiments for supplying electric energy.

[0027] The above description is only an outline of the technical solution of the present application, which can be implemented in accordance with the contents of this specification in order to more clearly understand the technical means of the present application, and to make the above and other objects, features and advantages more obvious and easy to understand, specific embodiments of the present application are specifically listed below. [Brief description of the drawings]

[0028] Various other advantages and merits will become apparent to those skilled in the art upon reading the following detailed description of the preferred embodiments. The drawings are only for the purpose of illustrating the preferred embodiments and are not to be construed as limiting the present application. In the drawings, like parts are designated by like reference numerals throughout.

[0029] [Figure 1] FIG. 1 is a structural schematic diagram of a vehicle according to some embodiments of the present application. [Diagram 2] FIG. 2 is a schematic exploded view of a battery according to some embodiments of the present application. [Diagram 3] FIG. 1 is a schematic diagram of a battery cell according to some embodiments of the present application. [Figure 4] FIG. 2 is an exploded schematic diagram of a battery cell according to some embodiments of the present application. [Diagram 5] FIG. 5 is a cross-sectional view taken along the xz plane of FIG. 4, showing a battery cell according to some embodiments of the present application employing a roll-up electrode assembly. [Figure 6] FIG. 5 is a cross-sectional view taken along the xz plane of FIG. 4 employing a laminated electrode assembly according to some embodiments of the present application. [Figure 7] 1 is a cross-sectional view of an electrode according to some embodiments of the present application; [Figure 8] 11A-11C are cross-sectional views of electrodes according to some other embodiments of the present application. [Figure 9] 11A-11C are cross-sectional views of electrodes according to some other embodiments of the present application. [Figure 10] 13A-13C are top views of electrodes according to some other embodiments of the present application. [Figure 11] 13A-13C are top views of electrodes according to some other embodiments of the present application. [Figure 12] 11A-11C are cross-sectional views of electrodes according to some other embodiments of the present application. [Figure 13] 11A-11C are electrode top views of some other embodiments of the present application. [Figure 14] 13A-13C are top views of electrodes according to some other embodiments of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings. The following examples are merely illustrative and are not to be construed as limiting the scope of protection of the present invention.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application pertains. The terms used herein are only for describing specific examples and are not intended to limit the present application. The terms "including" and "having" and any variations thereof in the specification, claims, and the brief description of the drawings above are intended to cover a non-exclusive inclusion.

[0032] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are used merely to distinguish different objects, and should not be understood as indicating or suggesting relative importance, or implying the number, particular order, or hierarchical relationship of technical features. In the description of the embodiments of the present application, "plurality" means two or more, unless otherwise specified.

[0033] The term "embodiment" as used herein means that a combination of a particular feature, structure, or characteristic described in the embodiment may be included in at least one embodiment of the present application. The term appears in various places in the present specification not all necessarily referring to the same embodiment, nor does it mean an embodiment that is mutually exclusive, independent, or an alternative to other embodiments. Those skilled in the art can understand, either explicitly or implicitly, that the embodiment described in this specification may be combined with other embodiments.

[0034] In the description of the embodiments of the present application, the term "and / or" merely describes the relationship between related objects, and means that there are three possible relationships. For example, "A and / or B" can mean three cases: simply A, both A and B, and simply B. In addition, " / " in the text generally indicates that the related objects before and after it have an "or" relationship.

[0035] In describing the embodiments of the present application, the term "multiple" means two or more (including two); similarly, "multiple sets" means two or more sets (including two sets), and "multiple sheets" means two or more sheets (including two sheets).

[0036] In describing the embodiments of the present application, the orientations and positional relationships indicated by technical terms such as "center," "longitudinal," "lateral," "length," "width," "thickness," "up," "down," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial direction," "radial," "circumferential," and the like are based on the orientations and positional relationships in the drawings, and are merely intended to facilitate and simplify the description of the embodiments of the present application, and do not indicate or imply that the devices or elements shown must have a specific orientation or be configured and operated in a specific orientation, and therefore should not be construed as limiting the embodiments of the present application.

[0037] In the description of the embodiments of the present application, unless otherwise specified or limited, the technical terms "attach," "connect," "join," "connect," "fix," etc. should be understood in a broad sense. For example, they may be fixedly connected, detachably connected, or integrated, may be mechanically connected or electrically connected, may be directly connected or indirectly connected via an intermediate medium, may be internally connected to both elements, or may be in an interactive relationship between both elements. Those skilled in the art can understand the specific meanings of these terms described in the embodiments of the present application according to the specific circumstances.

[0038] At present, in view of the development of the market situation, the application of power batteries is becoming more and more widespread. Power batteries are not only widely used in energy storage power systems such as hydroelectric, thermal, wind and solar power stations, but also in electric transportation such as electric bicycles, electric motorcycles, electric cars, military equipment and aerospace, and many other fields. As the application fields of power batteries expand, the market demand for them is also constantly expanding.

[0039] A battery cell generally includes a stack of multiple layers of electrodes, or a winding of multiple layers of electrodes. The inventors have noticed that as the charge / discharge cycle of the battery progresses, a side reaction (e.g., oxidative decomposition of the electrolyte) may occur near the electrodes, generating gas. If the generated gas is not quickly exhausted from the stack or winding of the multi-layer electrodes, the local air pressure in the cell may become too large, which may further cause the expansion and deformation of the cell, and further adversely affect the performance and service life of the battery. For example, the expansion and deformation of the cell may increase the distance between some electrodes, causing a loss of battery capacity.

[0040] In view of the above, in order to solve the problem of expansion and deformation of the cell due to a gas generation side reaction occurring near the electrode, the inventors conducted detailed studies and designed an electrode including a current collector layer and an active material layer, wherein the current collector layer has a porous matrix, the current collector layer is gas permeable, the active material layer is laminated on at least a part of the surface of the current collector layer, and the active material layer is disposed outside the pores of the porous matrix.

[0041] In such a battery cell, the current collector layer has a porous matrix and is gas permeable, so that gas generated near the electrode can be effectively discharged, thereby preventing gas expansion in the cell due to blocking of gas discharge, and further preventing expansion and deformation of the cell.

[0042] The battery cells disclosed in the embodiments of the present application can be used in electric devices such as, but not limited to, vehicles, ships, and aircraft. The battery cells and batteries disclosed in the present application can be used to configure a power supply system for the electric device. This is advantageous in mitigating and automatically adjusting the deterioration of the expansion force of the electric cell, compensating for the consumption of the electrolyte, and improving the stability of the battery performance and the battery life.

[0043] The present embodiment provides an electric device that uses a battery as a power source, and the electric device may be, but is not limited to, a mobile phone, a tablet, a laptop, an electric toy, a power tool, a battery car, an electric car, a ship, a spacecraft, etc. Among them, the electric toy may include stationary or mobile electric toys, such as a game console, an electric car toy, an electric ship toy, an electric plane toy, etc., and the spacecraft may include an aircraft, a rocket, a space shuttle, a spaceship, etc.

[0044] In the following embodiment, for convenience of explanation, a vehicle 1000 will be taken as an example to describe an electric device according to one embodiment of the present application.

[0045] Please refer to FIG. 1, which is a structural schematic diagram of a vehicle 1000 provided in some embodiments of the present application. The vehicle 1000 can be a gasoline vehicle, a gas vehicle, or a new energy vehicle, and the new energy vehicle can be a pure electric vehicle, a hybrid vehicle, or a range extender vehicle, etc. A battery 100 is provided inside the vehicle 1000, and the battery 100 can be disposed in the lower part, the front part, or the rear part of the vehicle 1000. The battery 100 is used to supply power to the vehicle 1000, for example, the battery 100 is used as the operating power source of the vehicle 1000. The vehicle 1000 may further include a controller 200 and a motor 300, and the controller 200 is used to control the power supply from the battery 100 to the motor 300, for example, for starting the vehicle 1000, navigation, and working power demand during driving.

[0046] In some embodiments of the present application, the battery 100 is used not only as an operating power source for the vehicle 1000, but also as a driving power source for the vehicle 1000, and can replace or partially replace fuel or natural gas to provide driving power for the vehicle 1000.

[0047] Please refer to FIG. 2, which is an explosion diagram of a battery 100 provided in some embodiments of the present application. The battery 100 includes a housing 10 and a battery cell 20, and the battery cell 20 is accommodated in the housing 10. The housing 10 is used to provide an accommodation space for the battery cell 20, and the housing 10 can adopt various structures. In some embodiments, the housing 10 may include a first part 11 and a second part 12, and the first part 11 and the second part 12 cover each other, and the first part 11 and the second part 12 jointly define an accommodation space for accommodating the battery cell 20. The second part 12 may be a hollow structure with an opening at one end, and the first part 11 may be a plate-like structure, and the first part 11 may cover the open side of the second part 12, and the first part 11 and the second part 12 may jointly define an accommodation space. Both the first part 11 and the second part 12 have a hollow structure with an opening on one side, and the opening side of the first part 11 may cover the opening side of the second part 12. Of course, the housing 10 formed by the first part 11 and the second part 12 may have various shapes, such as a cylinder or a rectangular parallelepiped.

[0048] In the battery 100, the battery cell 20 may be multiple, and the multiple battery cells 20 may be connected in series, parallel, or series-parallel, and the series-parallel connection means that the multiple battery cells 20 are connected both in series and in parallel. The multiple battery cells 20 may be directly connected in series, parallel, or series-parallel, and the entire battery cells 20 may be housed in the housing 10. Of course, the battery 100 may be formed by connecting the multiple battery cells 20 in series, parallel, or series-parallel to form a battery module, and the multiple battery modules may be further connected in series, parallel, or series-parallel to form a whole body and housed in the housing 10. The battery 100 may further include other structures, for example, the battery 100 may further include a bus component for realizing electrical connection between the multiple battery cells 20.

[0049] Each battery cell 20 may be a secondary battery or a primary battery, including but not limited to a lithium-sulfur battery, a sodium-ion battery, or a magnesium-ion battery, and may be cylindrical, flat, rectangular, or have other shapes.

[0050] FIG. 3 is a structural schematic diagram of a single battery cell, and FIG. 4 is an exploded schematic diagram of a single battery cell. Each battery cell 20 includes a case 21 and an electrode assembly 22 provided in the case 21. The case 21 may have a hexahedral shape or other shapes and has an opening. The electrode assembly 22 is accommodated in the case 21. A cover plate assembly 24 covers the opening of the case 21. The cover plate assembly 24 includes a cover plate 241 and two electrode terminals provided on the cover plate, the two electrode terminals being a first electrode terminal 242 and a second electrode terminal 243, respectively. The first electrode terminal 242 may be a positive electrode terminal, and the second electrode terminal 243 may be a negative electrode terminal. In another embodiment, the first electrode terminal 242 may be a negative electrode terminal, and the second electrode terminal 243 may be a positive electrode terminal. An adapter 23 is provided between the cover plate assembly 24 and the electrode assembly 22, and the tabs of the electrode assembly 22 are electrically connected to electrode terminals on the cover plate 241 through the adapter 23. In this embodiment, there are two adapters 23, namely, a positive adapter and a negative adapter.

[0051] 4, two electrode assemblies 22 are provided in the case 21, and the two electrode assemblies 22 are stacked along the height direction (z direction) of the battery cell 20, where the height direction of the battery cell 20 coincides with the height direction of the battery pack. Of course, in other embodiments, one electrode assembly 22 may be provided in the case 21, or three or more electrode assemblies 22 may be provided in the case 21. The multiple electrode assemblies 22 are stacked along the height direction (z direction) of the battery cell 20.

[0052] As shown in FIG. 5 and FIG. 6, the electrode assembly 22 includes a first electrode 221, a second electrode 222, and a separator 223 disposed between the first electrode 221 and the second electrode 222. The first electrode 221 may be a positive electrode, and the second electrode 222 may be a negative electrode. In another embodiment, the first electrode 221 may be a negative electrode, and the second electrode 222 may be a positive electrode. The separator 223 is an insulator interposed between the first electrode 221 and the second electrode 222. The active material of the positive electrode may be coated on the coating area of ​​the positive electrode, and the active material of the negative electrode may be coated on the coating area of ​​the negative electrode. The part protruding from the coating area of ​​the positive electrode is a positive electrode tab, and the part protruding from the coating area of ​​the negative electrode is a negative electrode tab. The positive electrode tab is connected to the positive electrode terminal of the cover plate assembly 24 by a positive electrode adapter, and similarly, the negative electrode tab is connected to the negative electrode terminal of the cover plate assembly 24 by a negative electrode adapter.

[0053] As shown in FIG. 5, the electrode assembly 22 has a winding structure. The first electrode 221, the separator 223, and the second electrode 222 are all strip-shaped, and the first electrode 221, the separator 223, and the second electrode 222 are sequentially stacked and wound up two or more times to form the electrode assembly 22, which is flat. When manufacturing the electrode assembly 22, the electrode assembly 22 may be directly wound up in a flat shape, or may be first wound up into a hollow cylindrical structure and then pressed into a flat shape after winding. FIG. 8 is a schematic diagram of the outline of the electrode assembly 22, in which the outer surface of the electrode assembly 22 includes two flat surfaces 224, which are arranged opposite to each other along the height direction (z direction) of the battery cell 20. Here, the electrode assembly 22 has an approximately hexahedral structure, and the flat surface 224 is approximately parallel to the winding axis and is the outer surface with the largest area. The flat surface 224 may be any relatively flat surface, and does not necessarily have to be a pure plane.

[0054] 6, the electrode assembly 22 has a laminate structure, that is, the electrode assembly 22 includes a plurality of first electrodes 221 and a plurality of second electrodes 222, and a separator 223 is provided between the first electrodes 221 and the second electrodes 222. The first electrodes 221 and the second electrodes 222 are provided in a laminated manner along the height direction (z direction) of the battery cell 20.

[0055] According to some embodiments of the present application, referring to Fig. 7, the present application provides an electrode including a current collector layer 710 and a first active material layer 721. The current collector layer 710 has a porous structure 715, and the current collector layer is gas permeable. The first active material layer 721 is laminated on at least a part of the surface of the current collector layer 710, and the first active material layer 721 is located outside the pores of the porous structure 715.

[0056] Current collector layer 710 is, for example, any conductive substrate capable of carrying electrical current to and from the active material layers.

[0057] The porous structure 715 refers to, for example, pore channels that connect from one side to the other side of the current collector layer 710. The porous structure is, for example, a through-hole structure, for example, a three-dimensional network structure.

[0058] Gas permeable means that the material has a higher gas permeability than metal foil (for example, copper foil having a thickness of 4 to 8 μm).

[0059] The first active material layer 721 refers to a layer containing an electrochemically active material. The electrochemically active material can be a positive electrode active material or a negative electrode active material.

[0060] The negative electrode active material may be a battery negative electrode active material well known in the art. For example, the negative electrode active material may include at least one of artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based material, tin-based material, and lithium titanate. The silicon-based material may be at least one selected from elemental silicon, silicon oxide, silicon carbon composite, silicon nitrogen composite, and silicon alloy. The tin-based material may be at least one selected from elemental tin, tin oxide, and tin alloy. However, the present application is not limited to these materials, and other traditional materials used as battery negative electrode active materials may be used. These negative electrode active materials may be used alone or in combination of two or more.

[0061] The positive electrode active material may be a positive electrode active material for batteries well known in the art. For example, the positive electrode active material may be a positive electrode active material for batteries well known in the art. For example, the positive electrode active material may include at least one of lithium-containing phosphates having an olivine structure, lithium transition metal oxides, and their modified compounds. However, the present application is not limited to these materials, and other traditional materials used as positive electrode active materials for batteries may be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides include lithium cobalt oxide (e.g., LiCoO2), lithium nickel oxide (e.g., LiNiO2), lithium manganese oxide (e.g., LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (sometimes abbreviated as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (sometimes abbreviated as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2(NCM 211(sometimes abbreviated as "LiNi") 0.6 Co 0.2 Mn 0.2 O2(NCM 622 (sometimes abbreviated as "LiNi") 0.8 Co 0.1 Mn 0.1 O2(NCM 811 Lithium nickel cobalt aluminum oxide (LiNi 0.85 Co 0.15 Al 0.05 Examples of lithium-containing phosphates having an olivine structure include, but are not limited to, at least one of lithium iron phosphate (e.g., LiFePO4 (sometimes abbreviated as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (e.g., LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon.

[0062] The active material layer optionally contains a binder, which may be at least one selected from styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0063] In the technical proposal of the embodiment of the present application, the current collector layer is gas permeable. Moreover, the active material layers are located outside the pores of the porous structure and do not penetrate into the porous matrix layer of the current collector layer, so that the porous structure is not clogged and the gas permeability of the current collector layer is enhanced. With this design, when gas is generated due to contact between the electrolyte and the positive and negative electrodes, the gas can smoothly overflow outside the cell through the current collector layer, which can avoid deformation and structural failure caused by gas expansion inside the cell, and further improve the performance of the battery.

[0064] In some embodiments, the current collector layer is gas and liquid permeable, in which the current collector is not only gas permeable and has improved exhaust performance, but also electrolyte permeable, thereby shortening the infiltration time of the electrolyte into the electrode material layer and improving the infiltration effect of the electrolyte into the electrode material layer.

[0065] In some embodiments, the material of the current collector layer includes a conductive material, such as a metal material, a carbon-based conductive material, a conductive polymer material, or a combination thereof. By adopting the conductive material, the current collector has a relatively good electrical conductivity.

[0066] A conductive material has an electrical conductivity of 10 siemens / meter (S / m) or more, e.g., 10 3 Siemens / meter (S / m) or more, e.g. 10 6 The conductive material is a material having a conductivity of Siemens / meter (S / m) or more. The metallic material is, for example, aluminum, copper, nickel, iron, titanium, silver, nickel, or an alloy of any one of them. The carbon-based conductive material is, for example, graphite, carbon fiber, carbon nanotube, graphene. The conductive polymer material is, for example, polypyrrole, polythiophene, polyphenylene vinylene.

[0067] According to some embodiments of the present application, referring to Fig. 8, the current collector layer 710 includes a porous matrix 711 and a conductive layer 712, and the conductive layer 712 covers at least a part of the surface of the porous matrix 711. The current collector of the embodiment of the present application has a composite structure including the porous matrix 711 and the conductive layer 712. The porous matrix 711 plays a role of supporting the current collector structure, and the conductive layer 712 plays a role of electrical conduction, and both have their own advantages and work synergistically to provide the current collector layer with improved overall performance.

[0068] In the above-mentioned solution, the porous matrix 711 has a porous structure, i.e., a pore channel that runs from one side to the other. The porous matrix is, for example, a matrix with a through-hole structure, for example, a matrix with a three-dimensional network structure. The porous matrix 711 can be made of a non-conductive material.

[0069] In some embodiments, the conductive layer 712 coats the inner surfaces of the pores of the porous matrix, leaving the pore structure of the porous matrix intact after coating, and the current collector layer 710 has a porous structure 715.

[0070] In some embodiments, the conductive layer 712 coats both the exterior and interior pore surfaces of the porous matrix, and by such design, all surfaces of the porous matrix have improved electrical conductivity.

[0071] In some embodiments, the electrical conductivity of the conductive layer 712 is higher than the electrical conductivity of the porous matrix 711. In this design, the conductive layer 712 is made of a material with a relatively high electrical conductivity, and the porous matrix 711 is made of a material with a relatively low electrical conductivity, so that the amount of high electrical conductivity material used is reduced, reducing costs, and the electrical conductivity of the current collector surface is essentially unaffected, and the electron transport at the interface between the current collector and the active material is also unaffected.

[0072] In some embodiments, the density of the porous matrix 711 is less than the density of the conductive layer 712. In this design, the conductive layer 712 employs a material with a relatively high electrical conductivity (e.g., a metal material) and the porous matrix 711 employs a material with a relatively low density (e.g., a polymer material), so that the density of the entire current collector layer 710 is reduced while the electrical conductivity of the surface of the current collector layer 710 is essentially not affected, and the electron transport at the interface between the current collector layer 710 and the active material layer 721 is not affected.

[0073] In some embodiments, the material of the porous matrix 711 includes a polymer. Optionally, the polymer is selected from one or more of polyamide, polyimide, polyester, polyolefin, polyalkyne, siloxane polymer, polyether, polyalcohol, polysulfone, polysaccharide polymer, amino acid polymer, polysulfur nitride, aromatic ring polymer, aromatic heterocyclic polymer, epoxy resin, phenolic resin, derivatives thereof, crosslinked products thereof, and copolymers thereof, or combinations thereof. Such a design can reduce the density of the entire current collector layer.

[0074] In some embodiments, the material of the conductive layer 712 includes a metal. Optionally, the metal is selected from aluminum, copper, nickel, iron, titanium, silver, nickel, or an alloy of any one of these. Such a design can improve the conductivity of the current collector layer.

[0075] In some embodiments, the porosity of the current collector layer 710 is 20% or more, for example, 20% to 95%. When the porosity of the current collector layer is 20% to 95%, the electrode has relatively good gas permeability and good structural strength and stability. The porosity of the current collector layer 710 is 20% to 30%, 30% to 40%, 40% to 50%, 50% to 60%, 60% to 70%, 70% to 80%, 80% to 90%, or 90% to 95%. The porosity of the current collector layer is measured according to GB / T 33052-2016 "Method for measuring porosity of microporous functional films by cetane absorption method".

[0076] In some embodiments, the thickness of the current collector layer 710 is 4 μm or more, for example, 4 μm to 500 μm. By providing the current collector layer with a thickness of 4 μm or more, the current collector has good structural strength and stability. By providing the current collector layer with a thickness of 4 μm to 500 μm, the electrode has good structural strength and stability, a relatively low weight and volume fraction in the battery, and the battery has a high volumetric or gravimetric energy density.

[0077] In some embodiments, the gas permeability of the current collector layer 710 is 1000 to 5000 cm3 / m 2 ·24h·0.1MPa. This design makes the collector electrode have high gas permeability and is favorable for gas discharge. The test standard can refer to GB / T1038-2000 "Test method for gas permeability of plastic film and sheet by differential pressure method".

[0078] In some embodiments, the tortuosity of the current collector layer 710 is ≧1, for example, 1.0-6.0 (for example, 1.0-2.0, 2.0-3.0, 3.0-4.0, 4.0-5.0, or 5.0-6.0). This design makes it easier for the electrode to be infiltrated by the electrolyte, and the electrolyte is easier to rise along the electrode. The test criterion for the tortuosity is based on the Bruggeman relationship: τ=ε α (where τ is the tortuosity, ε is the porosity, and α is the Bruggeman coefficient) (-1≦α≦-0.5) is used to determine the tortuosity.

[0079] In some embodiments, Fig. 9 shows a cross-sectional view of an electrode according to some embodiments, as shown in Fig. 9, the electrode includes a current collector layer 710, the current collector layer 710 has a porous structure 715, the current collector layer is gas permeable, the electrode further includes a first active material layer 721 and a second active material layer 722, the first active material layer 721 and the second active material layer 722 are respectively laminated on both sides of the current collector layer 710, and the first active material layer 721 and the second active material layer 722 are located outside the pores of the porous structure 715. The current collector layer 710 includes a porous matrix 711 and a conductive layer 712, and the conductive layer 712 covers at least a part of the surface of the porous matrix 711.

[0080] 9, an electrode further includes an electrical connection member 810 (e.g., a tab), which is attached to and electrically connected to the current collector layer 710. For example, the electrical connection member 810 may be attached to the current collector layer 710 by a transfer welding process, and the electrical connection member 810 may be electrically connected to the current collector layer 710 via a connection region 815.

[0081] In this solution, the electrical connection member 810 is a component for conducting electrode current. The electrical connection member 810 protrudes and extends from the edge of the current collector layer 710 to serve as an input or output for current.

[0082] 9, at least one side (e.g., both sides) of the porous matrix 711 includes at least one edge region 713, and the conductive layer 712 covers the area other than the edge region 713. Optionally, some or all of the edges of the porous matrix 711 are provided with edge regions. Optionally, for a rectangular porous matrix 711, one, two, three or four edges of the porous matrix 711 are provided with edge regions. Optionally, two opposing edges of the porous matrix 711 are provided with edge regions.

[0083] In this solution, the edge region 713 is not covered by the conductive layer 712, and the edge region 713 is non-conductive. The edge region 713 is also not covered by the first active material layer 721 or the second active material layer 722, and the edge region of the current collector layer 710 serves as a buffer protection to prevent the first active material layer 721 or the second active material layer 722 laminated on the current collector layer 710 from directly contacting the battery end cap. It also serves to protect the active material layer. In addition, since the tab 810 is usually attached to the edge of the current collector layer 710, the non-conductive edge region 713 serves to protect the tab 810, while preventing the tab 810 from contacting the opposite electrode and causing a short circuit.

[0084] In one embodiment, Figs. 10 and 11 each show a top view of one electrode. To allow for viewing of the layers of the electrode from the top, in Figs. 10 and 11, a portion of the surface of the porous matrix 711 is not covered by the conductive layer 712, and a portion of the surface of the current collector layer 710 is not covered by the first active material layer 721. It should be understood that these uncovered areas are depicted in this manner for ease of viewing, unless otherwise noted. It should be noted that a portion of the edge region 713 of the current collector layer 710 is not covered by the conductive layer 712, nor is it covered by the first active material layer 721 or the second active material layer 722. In this embodiment, the edge region 713 serves as a buffer protection to prevent the conductive layer 712, the first active material layer 721, or the second active material layer 722 from directly contacting the battery end cap.

[0085] 10, a direction perpendicular to the protruding direction of the electrical connection member 810 is defined as a first direction, and a ratio d:D of a size d of the electrical connection member 810 to a size D of the current collector layer 710 in the first direction is in a range of 1:2 to 5. The width size (d) of the electrical connection member of the electrode is relatively small, which has the advantages of a simple welding process, a small volume, and convenient assembly.

[0086] In some embodiments, Fig. 11 shows a top view of one electrode. As shown in Fig. 11, the direction perpendicular to the protruding direction of the electrical connection member 810 is defined as a first direction, and the ratio d of the size d of the electrical connection member 810 to the size D of the current collector layer 710 in the first direction is d:D=1:1. The width size (d) of the electrical connection member of the electrode is relatively large, which can reduce the internal resistance of the electrical connection member 810, further reduce Joule heat, and lower the electrode temperature.

[0087] In some embodiments, Fig. 12 shows a cross-sectional view of an electrode according to some embodiments, as shown in Fig. 12, the electrode includes a current collector layer 710, the current collector layer 710 has a porous structure 715, the current collector layer is gas permeable, the electrode further includes a first active material layer 721 and a second active material layer 722, the first active material layer 721 and the second active material layer 722 are respectively laminated on both sides of the current collector layer 710, and the first active material layer 721 and the second active material layer 722 are located outside the pores of the porous structure 715. The current collector layer 710 includes a porous matrix 711 and a conductive layer 712, and the conductive layer 712 covers at least a part of the surface of the porous matrix 711.

[0088] 12, the electrode further includes an electrical connection member 810 (e.g., a tab), which is attached to and electrically connected to the current collector layer 710. For example, the electrical connection member 810 is attached to the current collector layer 710 by a transfer welding process, and the electrical connection member 810 is electrically connected to the current collector layer 710 via a connection region 815.

[0089] In some embodiments, the surface of the current collector layer includes an active material region and a support region, the active material layer is laminated on the active material region of the current collector layer, and the electrode further includes a support layer, the support layer is laminated on the support region of the surface, as shown in Figure 12. In some embodiments, the material of the support layer includes ceramic (e.g., a coating layer containing ceramic particles).

[0090] In this solution, the supporting layer has the role of structural reinforcement, and such a design can improve the structural strength and structural stability of the electrode.

[0091] In one embodiment, Figures 13 and 14 each show a top view of one electrode. To allow for observation of each layer of the electrode from the top, in Figures 13 and 14, a portion of the surface of the porous matrix 711 is not covered by the conductive layer 712, and a portion of the surface of the current collector layer 710 is not covered by the first active material layer 721. It should be understood that, unless otherwise stated, these uncovered areas are depicted in this manner for ease of observation.

[0092] 13, a direction perpendicular to the protruding direction of the electrical connection member 810 is defined as a first direction, and a ratio d:D of a size d of the electrical connection member 810 to a size D of the current collector layer 710 in the first direction is in a range of 1:2 to 5. The electrode has the advantages that the width size (d) of the electrical connection member is relatively small, the welding process is simple, the volume is small, and the assembly is convenient.

[0093] 14, the direction perpendicular to the protruding direction of the electrical connection member 810 is defined as the first direction, and the ratio of the size d of the electrical connection member 810 to the size D of the current collector layer 710 in the first direction is d:D=1:1. In this electrode, the width size (d) of the electrical connection member is relatively large, the electrical conductivity of the electrical connection member 810 is high, the internal resistance is low, and the Joule heat of the electrical connection member is low, resulting in a low electrode temperature.

[0094] In some embodiments, the active material layer comprises an electrochemically active material, optionally selected from a lithium ion battery positive electrode active material or a lithium ion battery negative electrode active material, optionally selected from a lithium-ion battery positive electrode active material having an olivine structure, a lithium transition metal oxide, or a combination thereof, and optionally selected from an artificial graphite, a natural graphite, a soft carbon, a hard carbon, a silicon-based material, a tin-based material, a lithium titanate, a lithium metal, or a combination thereof. In this solution, the electrodes according to the present disclosure can be used in combination with a variety of electrochemically active materials.

[0095] In some embodiments, a method for producing an electrode is provided, the method comprising: providing a current collector layer having a porous structure and being gas permeable; providing an active material layer; and depositing the active material layer on at least a portion of a surface of the current collector layer such that the active material layer is disposed outside the pores of the porous structure, the electrode resulting from the method having improved gas permeability.

[0096] In some embodiments, a method of manufacturing an electrode includes the steps of manufacturing a current collector layer, the steps including providing a porous matrix and depositing a conductive layer on at least a portion of a surface of the porous matrix, optionally the deposition being selected from electroplating, electroless plating, vapor deposition, magnetron sputtering, or a combination thereof, and the resulting electrode has improved gas permeability.

[0097] In some embodiments, the electrical conductivity of the porous matrix is ​​less than the electrical conductivity of the conductive layer, such that the electrode obtained by the method has improved electrical conductivity.

[0098] In some embodiments, the density of the porous matrix is ​​less than the density of the conductive layer, resulting in an electrode having a low density.

[0099] In some embodiments, a battery is provided that includes an electrode according to any of the preceding embodiments or an electrode produced by a method according to any of the preceding embodiments.

[0100] In some embodiments, there is provided an electrical device including a battery according to any of the above embodiments for supplying electrical energy.

[0101] The following describes the technical solution of the present application in more detail with reference to the following examples.

[0102] Example 1

[0103] Hereinafter, an electrode and its manufacturing method will be described with reference to FIG. 9 and FIG. 10. In one embodiment, the electrode was manufactured by the following method. That is, first, a porous matrix 711, specifically a porous polypropylene (PP) film, was provided. Then, an edge region 713 was divided on the surface of the edge of the porous matrix 711. Then, a conductive layer 712 (Al plating layer or Cu plating layer) was coated on the area other than the edge region 713. The Al plating layer may be coated on the surface of the porous polypropylene (PP) film by a method such as vapor deposition or chemical vapor deposition (CVD). The Cu plating layer may be coated on the surface of the porous polypropylene (PP) film by a method such as magnetron sputtering or electroless plating. A current collector layer 710 was obtained. The conductive layer formed one layer of conductive network on the surface of the porous polypropylene film. The current collector layer 710 had a porosity of 35%, a thickness in the range of 30 μm, and a tortuosity of 1.75. Electrical connection member 810 (made of copper foil / aluminum foil) was attached onto current collector layer 710 using a conductive adhesive or roll welding, and the ratio of width d of electrical connection member 810 to length D of the sheet was 1:5. A first active material layer 721 (active material film) and a second active material layer 722 (active material film) that had been manufactured in advance were coated onto the active material region of current collector layer 710, and the first active material layer 721 and the second active material layer 722 were fixed to the active material region of current collector layer 710 using a conductive adhesive in combination with a method of rolling along the edges.

[0104] The positive and negative electrodes were prepared respectively by the above-mentioned methods, and the positive and negative electrodes and the separator were wound into a cylindrical bare battery cell, and the cell was packaged into a battery.

[0105] Example 2

[0106] Another electrode and its manufacturing method will be described below with reference to Figures 9 and 11. The difference from Example 1 was that the ratio of the width d of the electrical connection member 810 to the length D of the sheet was 1:1.

[0107] The positive and negative electrodes were prepared respectively by the above-mentioned methods, and the positive and negative electrodes and the separator were wound into a cylindrical bare battery cell, and the cell was packaged into a battery.

[0108] Example 3

[0109] Hereinafter, one electrode and its manufacturing method will be described with reference to FIG. 12 and FIG. 13. In one embodiment, first, a porous matrix 711, specifically a porous polypropylene (PP) film, was provided. Then, a conductive layer 712 (Al plating layer or Cu plating layer) was coated on the surface of the porous matrix 711. The Al plating layer may be coated on the surface of the porous polypropylene (PP) film by using a method such as vapor deposition or chemical vapor deposition (CVD). The Cu plating layer was coated on the surface of the porous polypropylene (PP) film by using a method such as magnetron sputtering or electroless plating. A current collector layer 710 was obtained. The conductive layer formed one layer of conductive network on the surface of the porous polypropylene film. The current collector layer 710 had a porosity of 35%, a thickness of 30 μm, and a tortuosity of 1.69. An active material region and a support region were divided on the current collector layer 710. The support region was coated with a support layer 730 by coating. The components of the support layer 730 were 99 wt% boehmite and 1 wt% PVDF. An electrical connection member 810 (made of copper foil / aluminum foil) was attached to the current collector layer 710 using a conductive adhesive or roll welding, and the ratio of the width d of the electrical connection member 810 to the length D of the sheet was 1:5. A first active material layer 721 (active material film) and a second active material layer 722 (active material film) that were previously manufactured were coated on the active material area of ​​the current collector layer 710, and the first active material layer 721 and the second active material layer 722 were fixed to the active material area of ​​the current collector layer 710 using a conductive adhesive in combination with a method of rolling along the edges.

[0110] The positive and negative electrodes were prepared respectively by the above-mentioned methods, and the positive and negative electrodes and the separator were wound into a cylindrical bare battery cell, and the cell was packaged into a battery.

[0111] Example 4

[0112] Another electrode and its manufacturing method will be described below with reference to Figures 12 and 14. The difference from Example 3 was that the ratio of the width d of the electrical connection member 810 to the length D of the sheet was 1:1.

[0113] The positive and negative electrodes were prepared respectively by the above-mentioned methods, and the positive and negative electrodes and the separator were wound into a cylindrical bare battery cell, and the cell was packaged into a battery.

[0114] As can be seen from the tests, compared to the batteries using metal foil current collectors without a porous structure, the batteries of Examples 1 to 4 showed the following significantly improved performance:

[0115] (1) The sheets (especially those located inside the cell) were permeated with the electrolyte earlier.

[0116] (2) The sheets (especially those located inside the cells) were more susceptible to the emission of by-reaction gases.

[0117] (3) Cell space utilization has improved.

[0118] (4) Cell manufacturability has improved.

[0119] Finally, the above-mentioned embodiments are merely for illustrating the technical solution of the present application, and are not intended to limit it. Although the present application has been described in detail with reference to the above-mentioned embodiments, those skilled in the art can still understand that modifications to the invention described in the above-mentioned embodiments or replacement of some or all of the technical features with equivalents are still possible, and such modifications or replacements do not deviate from the essence of the corresponding invention from the scope of the technical solution of each embodiment of the present application, and all should be included within the scope of the claims and the description of the present application. In particular, the technical features described in each embodiment can be combined in any manner as long as there is no structural contradiction. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions within the scope of the claims. [Explanation of symbols]

[0120] The symbols in the specific embodiment are as follows: 1000 vehicles 100 batteries 200 Controller 300 Motor 10. Chassis 11 First Part 12 Second Part 20 Battery Cells 21 cases 22 Electrode Assembly 221 First Sheet 222 Second Sheet 223 Separator 224 Two flat surfaces 23 Adapter 24 Cover Plate Assembly 241 Cover Plate 242 First electrode terminal 243 Second electrode terminal 710 Current collector layer 711 Porous Matrix 712 Conductive layer 713 Edge Area 715 Porous structure 721 First active material layer 722 Second active material layer 730 Support layer 810 Electrical connection parts 815 Connection Area

Claims

1. A current collector layer having a porous structure and being gas permeable; and an active material layer that is laminated on at least a portion of a surface of the current collector layer and disposed outside the pores of the porous structure, An electrode, characterized in that the current collector layer includes a porous matrix and a conductive layer covering at least a portion of a surface of the porous matrix, at least one side of the porous matrix includes at least one edge region, and an area other than the edge region is covered by the conductive layer.

2. The electrode according to claim 1 , wherein the material of the current collector layer includes a conductive material.

3. 3. The electrode according to claim 1, wherein the electrical conductivity of the conductive layer is greater than the electrical conductivity of the porous matrix.

4. 4. The electrode according to claim 1, wherein the density of the porous matrix is ​​less than the density of the conductive layer.

5. 5. The electrode according to claim 1, wherein the material of the porous matrix comprises a polymer.

6. The electrode described in Claim 5, characterized in that the polymer is selected from one or more of polyamides, polyimides, polyesters, polyolefins, polyalkynes, siloxane polymers, polyethers, polyalcohols, polysulfones, polysaccharide polymers, amino acid polymers, polysulfur nitrides, aromatic ring polymers, aromatic heterocyclic polymers, epoxy resins, phenolic resins, derivatives thereof, cross-linked products thereof, and copolymers thereof, or a combination thereof.

7. 7. The electrode according to claim 1, wherein the material of the conductive layer includes a metal.

8. The electrode of claim 7, wherein the metal is selected from aluminum, copper, nickel, iron, titanium, silver, nickel or an alloy of any one of them.

9. 9. The electrode according to claim 1, wherein the current collector layer has a porosity of 20% or more.

10. 10. The electrode according to claim 1, wherein the current collector layer has a thickness of 4 μm or more.

11. The gas permeability of the current collector layer is 1000 to 5000 cm 3 / m 2 11. The electrode according to claim 1, characterized in that the resistance is 0.1 MPa for 24 h.

12. 12. The electrode according to claim 1, further comprising an electrical connection member attached to and electrically connected to the current collector layer.

13. the surface of the current collector layer includes an active material region and a support region, the active material layer is laminated on an active material region of the current collector layer, The electrode according to any one of claims 1 to 12, further comprising a support layer, the support layer being laminated to a support area of ​​the surface.

14. The electrode according to any one of claims 1 to 13, characterized in that the active material layer comprises an electrochemically active material.

15. providing a current collector layer having a porous structure, being gas permeable, and including a porous matrix and a conductive layer covering at least a part of a surface of the porous matrix, at least one surface of the porous matrix including at least one edge region, and an area other than the edge region being covered by the conductive layer; Providing an active material layer; and laminating the active material layer on at least a portion of a surface of the current collector layer so that the active material layer is disposed outside the pores of the porous structure.

16. Providing a porous matrix; depositing a conductive layer on at least a portion of a surface of the porous matrix; 16. The method of claim 15, comprising the step of fabricating a current collector layer comprising:

17. the electrical conductivity of the porous matrix is ​​less than the electrical conductivity of the conductive layer; and The density of the porous matrix is ​​less than the density of the conductive layer.

17. The method according to claim 16, characterized in that:

18. A battery comprising the electrode according to any one of claims 1 to 14.

19. 20. An electrical device comprising the battery of claim 18 for supplying electrical energy.

Citation Information

Patent Citations

  • Winding type secondary battery and collector therefor

    JP2000090936A

  • Electrode for nonaqueous electrolyte secondary battery and method for manufacturing the same

    JP2001118566A

  • Electrode structural body for lithium secondary battery, and lithium secondary battery

    JP2005100804A

  • Nonaqueous electrolyte secondary battery

    JP2012248282A