Thermoplastic polyurethane elastic fiber and wound body thereof, gathers and sanitary materials containing said thermoplastic polyurethane elastic fiber, and method for producing said polyurethane elastic fiber

Incorporating specific solvents like DMAc, DMF, or NMP into thermoplastic polyurethane elastic fibers enhances recovery and unwinding properties, addressing the lack of these properties in existing fibers and improving manufacturing efficiency and fit in gathered materials.

JP7583939B2Active Publication Date: 2024-11-14ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023535252
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-07-13
Filing Date
2022-07-04
Publication Date
2024-11-14
Estimated Expiration
2042-07-04

AI Technical Summary

Technical Problem

Thermoplastic polyurethane elastic fibers produced by melt spinning lack both recovery and unwinding properties, which are essential for applications like innerwear and diapers to prevent yarn breakage during processing.

Method used

Incorporating specific amounts of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), or N-methylpyrrolidone (NMP) into the thermoplastic polyurethane elastic fibers, along with a polymer polyol, diisocyanate, and a low molecular weight diol, to enhance compatibility and reduce nozzle clogging.

Benefits of technology

The fibers exhibit improved recovery and unwinding properties, allowing for easier processing and higher yield in manufacturing, with reduced yarn breakage and improved fit in gathered materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583939000004
    Figure 0007583939000004
  • Figure 0007583939000001
    Figure 0007583939000001
  • Figure 0007583939000002
    Figure 0007583939000002
Patent Text Reader

Abstract

The present invention provides: a thermoplastic polyurethane elastic fiber which has both recoverability and unwindability; a wound body of this thermoplastic polyurethane elastic fiber; and a gather member and a sanitary material, each of which comprises this thermoplastic polyurethane elastic fiber. The present invention relates to: a thermoplastic polyurethane elastic fiber which is characterized by containing 0.05 ppm to 100 ppm of at least one substance that is selected from the group consisting of dimethyl acetamide (DMAc), dimethyl formamide (DMF), dimethyl sulfoxide (DMSO) and N-methyl pyrrolidone (NMP); a wound body of this thermoplastic polyurethane elastic fiber; gather and sanitary materials, each of which comprises this thermoplastic polyurethane elastic fiber; and a method for producing this thermoplastic polyurethane elastic fiber.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic polyurethane elastic fiber and a wound product thereof, gathers and sanitary materials containing the thermoplastic polyurethane elastic fiber, and a method for producing the polyurethane elastic fiber. [Background technology]

[0002] Polyurethane elastic fibers are used in innerwear, stockings, compression wear, diapers, etc. In the above-mentioned applications, the polyurethane elastic fibers are required to have recovery properties when stretched, and are also required to have good unwinding properties from a wound yarn so as to prevent yarn breakage during the processing steps in the manufacture of the above-mentioned applications. Patent Document 1 below discloses that polyurethane elastic fibers containing a lubricant and Guerbet alcohol promote the release of DMAc, which is used in the production of the polyurethane elastic fibers by a dry spinning method, from the polyurethane elastic fibers, and the remaining amount of DMAc is set to about 300 to 900 ppm, thereby improving the releasability. Furthermore, Patent Document 2 below discloses that an oil agent containing an amino-modified polyorganosiloxane resin improves the unwinding balance between the inner and outer layers of cheese when producing elastic fibers (particularly when produced by a melt spinning method). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-186704 A [Patent Document 2] JP 2003-49368 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, a thermoplastic polyurethane elastic fiber having good recovery and releasability produced by melt spinning has not yet been disclosed. In view of the problems of the prior art described above, an object of the present invention is to provide a thermoplastic polyurethane elastic fiber that combines recoverability and releasability, a wound yarn containing the same, gathers and sanitary materials containing the thermoplastic polyurethane elastic fiber, and a method for producing the polyurethane elastic fiber. [Means for solving the problem]

[0005] As a result of intensive research and repeated experiments to solve the above-mentioned problems, the inventors of the present application unexpectedly discovered that the above-mentioned problems can be solved by adding a specific amount of at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP) to the thermoplastic polyurethane elastic fiber, and thus completed the present invention.

[0006] That is, the present invention is as follows. [1] A thermoplastic polyurethane elastic fiber, characterized by containing at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP) in an amount of 0.05 ppm or more and 100 ppm or less. [2] The thermoplastic polyurethane elastic fiber according to [1], containing at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP) in an amount of 0.05 ppm or more and 10 ppm or less. [3] The thermoplastic polyurethane elastic fiber according to [2], containing at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP) in an amount of 0.05 ppm or more and 5 ppm or less. [4] The thermoplastic polyurethane elastic fiber according to any one of [1] to [3] above, which contains a thermoplastic polyurethane composed of a polymer polyol, a diisocyanate, and a low molecular weight diol. [5] The thermoplastic polyurethane elastic fiber according to [4], wherein the molecular weight of the low molecular weight diol is 60 or more and 120 or less. [6] The thermoplastic polyurethane elastic fiber according to any one of [1] to [5], wherein the thermoplastic polyurethane elastic fiber is a multifilament yarn, and the ratio of the maximum diameter to the minimum diameter of the constituent single yarns is 1.1 or more and 2.0 or less. [7] The thermoplastic polyurethane elastic fiber according to [6] above, having a single yarn fineness of 5 dtex or more and 40 dtex or less. [8] The thermoplastic polyurethane elastic fiber according to any one of [1] to [7] above, wherein the flow start temperature of the thermoplastic polyurethane elastic fiber measured with a flow tester is 150°C or higher and 220°C or lower. [9] The thermoplastic polyurethane elastic fiber according to any one of [1] to [8], wherein the ratio of the 100% elongation stress at 20°C to the 100% elongation stress at 80°C is 1.30 or more and 3.00 or less.

[10] The thermoplastic polyurethane elastic fiber according to any one of [1] to [9] above, which is substantially free of crosslinks containing allophanate bonds.

[11] The thermoplastic polyurethane elastic fiber according to any one of [1] to

[10] above, which is for use in sanitary materials.

[12] A wound body of the thermoplastic polyurethane elastic fiber according to any one of [1] to

[11] above.

[13] A gather comprising the thermoplastic polyurethane elastic fiber according to any one of [1] to

[11] above.

[14] A sanitary material comprising the thermoplastic polyurethane elastic fiber according to any one of [1] to

[11] above.

[15] A method for producing a thermoplastic polyurethane elastic fiber according to any one of [1] to

[11] above, the method comprising the step of melt spinning a polyurethane resin.

[16] The method for producing a thermoplastic polyurethane elastic fiber according to

[15] , wherein the polyurethane resin contains at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP).

[17] The method for producing a thermoplastic polyurethane elastic fiber according to

[16] , wherein the polyurethane resin contains at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP) in an amount of 0.05 ppm or more and 100 ppm or less.

[18] A method for producing a thermoplastic polyurethane elastic fiber according to the above item

[11] , comprising the step of melt spinning a polyurethane resin containing at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP) in an amount of 0.05 ppm or more and 100 ppm or less. Effect of the Invention

[0007] The thermoplastic polyurethane elastic fiber and the wound body thereof according to one embodiment of the present invention have the above-mentioned configuration, and thus are suitable for gathers, having both recovery and unwinding properties. In addition, the gathers and the sanitary material containing the same according to another embodiment of the present invention have high recovery properties, making them easy to put on and take off, have a good fit, and are unlikely to slip off. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a schematic diagram of an apparatus used for evaluating unwinding properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described in detail. The present invention is not limited to the following embodiment, and can be modified in various ways within the scope of the present invention.

[0010] [Thermoplastic polyurethane elastic fiber] The thermoplastic polyurethane elastic fiber of this embodiment is characterized by containing at least one selected from the group consisting of DMAc, DMF, DMSO, and NMP (hereinafter also referred to as "specific compound") in an amount of 0.05 ppm to 100 ppm. By containing the specific compound in an amount of 0.05 ppm to 100 ppm, the thermoplastic polyurethane elastic fiber of this embodiment has excellent recovery and releasability, and can suppress nozzle clogging caused by fine powder generated from nonwoven fabrics and absorbents adhering to the thermoplastic polyurethane elastic fiber during the diaper manufacturing process.

[0011] In the thermoplastic polyurethane elastic fiber of this embodiment, the reason why the recovery can be improved by including the specific compound in an amount of 0.05 ppm or more and 100 ppm or less is not yet clear, but the inventor presumes it as follows. By including the specific compound in the thermoplastic polyurethane elastic fiber in an amount of 0.05 ppm or more and 100 ppm or less, these compounds act as compatibilizers for the hard domains and soft domains of the thermoplastic polyurethane, and the hard domains are finely dispersed in the yarn, thereby exhibiting high recovery. In addition, the reason why the unwinding property can be improved is not yet clear, but the inventor presumes it as follows. By including the specific compound in the thermoplastic polyurethane elastic fiber in an amount of 0.05 ppm or more and 100 ppm or less, these compounds act as compatibilizers for the hard domains and soft domains of the thermoplastic polyurethane, and the soft domains are finely dispersed in the yarn, thereby reducing the contact area between the soft domains between the yarns, which is one of the causes of deterioration of unwinding property, and thus exhibiting high unwinding property. In addition, the reason why nozzle clogging can be suppressed is not yet clear, but the inventor presumes it as follows. By incorporating the specific compounds in the thermoplastic polyurethane elastic fiber at 0.05 ppm to 100 ppm, these compounds act as compatibilizers for the hard and soft domains of the thermoplastic polyurethane, causing the highly polar hard domains to be finely dispersed in the yarn, making it easier to release the electric charge accumulated in the thermoplastic polyurethane elastic fiber. This makes it possible to suppress nozzle clogging caused by the adhesion of fine powder generated from nonwoven fabrics and absorbents to the thermoplastic polyurethane elastic fiber during the diaper manufacturing process.

[0012] In the thermoplastic polyurethane elastic fiber of this embodiment, the content of the specific compound is preferably 0.05 ppm or more and 10 ppm or less, and more preferably 0.05 ppm or more and 5 ppm or less.

[0013] In the thermoplastic polyurethane elastic fiber of this embodiment, from the viewpoint of enhancing the effect of improving the releasability and recovery property by compatibilizing the hard domains and the soft domains, the specific compound contained in the thermoplastic polyurethane elastic fiber is preferably DMAc or DMF, and more preferably DMAc.

[0014] The thermoplastic polyurethane elastic fiber of the present embodiment includes a thermoplastic polyurethane. The thermoplastic polyurethane may have thermoplasticity, and is not particularly limited as long as it has a structure polymerized from, for example, diisocyanate, polymer polyol, low molecular weight diol, and low molecular weight diamine. The polymerization method is also not particularly limited. The thermoplastic polyurethane may be, for example, polyurethane polymerized from diisocyanate, polymer polyol, and low molecular weight diamine as a chain extender composed of an active hydrogen compound (hereinafter, also referred to as "polyurethane urea"), or polyurethane polymerized from diisocyanate, polymer polyol, and low molecular weight diol as a chain extender composed of an active hydrogen compound (hereinafter, also referred to as "polyurethane urethane"). Glycols and isocyanates having three or more functionalities may be used within a range that does not interfere with the desired effects of the present invention. In this specification, "thermoplastic" means that it has a reversible property that it can be melted by heating at a temperature below its decomposition temperature, shows plastic flow while in a molten state, and solidifies by cooling. In general, polyurethane resins begin to decompose at temperatures of 230°C or higher.

[0015] Examples of the polymer polyol include, but are not limited to, polyether-based diols, polyester-based diols, polycarbonate diols, etc. From the viewpoint of hydrolysis resistance, the polymer polyol is preferably a polyether-based polyol, and more preferably a polyether-based diol.

[0016] Examples of polyether polyols include polyethylene oxide, polyethylene glycol, polyethylene glycol derivatives, polypropylene glycol, polytetramethylene ether glycol, copolymer diols consisting of tetrahydrofuran (THF) and neopentyl glycol, and copolymer diols consisting of THF and 3-methyltetrahydrofuran. These polyether polyols may be used alone or in combination of two or more. The number average molecular weight of the polymer diol is preferably 1000 or more and 8000 or less. By using a polymer diol within this range, an elastic fiber excellent in elongation, stretch recovery, and heat resistance can be easily obtained. From the viewpoint of photoembrittlement, the polyether polyol is preferably polytetramethylene ether glycol, a copolymer diol which is a copolymer of tetrahydrofuran (THF) and neopentyl glycol, or a polyol obtained by blending these.

[0017] Examples of diisocyanates include aromatic diisocyanates, alicyclic diisocyanates, and aliphatic diisocyanates. Examples of aromatic diisocyanates include, but are not limited to, diphenylmethane diisocyanate (hereinafter also referred to as "MDI"), tolylene diisocyanate, 1,4-diisocyanate benzene, xylylene diisocyanate, 2,6-naphthalene diisocyanate, and the like. Examples of alicyclic diisocyanates and aliphatic diisocyanates include methylene bis(cyclohexyl isocyanate) (hereinafter also referred to as "H12MDI"), isophorone diisocyanate, methylcyclohexane 2,4-diisocyanate, methylcyclohexane 2,6-diisocyanate, cyclohexane 1,4-diisocyanate, hexahydroxylylene diisocyanate, hexahydrotolylene diisocyanate, and octahydro-1,5-naphthalene diisocyanate. These diisocyanates may be used alone or in combination of two or more. In particular, from the viewpoint of the stretch recovery of elastic fibers, the diisocyanate is preferably an aromatic diisocyanate, and more preferably MDI.

[0018] The chain extender made of an active hydrogen compound is preferably at least one selected from the group consisting of low molecular weight diamines and low molecular weight diols. The chain extender may be one having both a hydroxyl group and an amino group in the molecule, such as ethanolamine. From the viewpoint of obtaining a thermoplastic polyurethane suitable for melt spinning, the active hydrogen compound is preferably a low molecular weight diol.

[0019] Examples of low molecular weight diamines as chain extenders made of active hydrogen compounds include, but are not limited to, hydrazine, ethylenediamine, 1,2-propanediamine, 1,3-propanediamine, 2-methyl-1,5-pentanediamine, 1,2-diaminobutane, 1,3-diaminobutane, 1-amino-3,3,5-trimethyl-5-aminomethylcyclohexane, 2,2-dimethyl-1,3-diaminopropane, 1,3-diamino-2,2-dimethylbutane, 2,4-diamino-1-methylcyclohexane, 1,3-pentanediamine, 1,3-cyclohexanediamine, bis(4-aminophenyl)phosphine oxide, hexamethylenediamine, 1,3-cyclohexyldiamine, hexahydrometaphenylenediamine, 2-methylpentamethylenediamine, and bis(4-aminophenyl)phosphine oxide.

[0020] Examples of low molecular weight diols as chain extenders made of active hydrogen compounds include, but are not limited to, ethylene glycol, 1,3-propanediol, 1,4-butanediol, bishydroxyethoxybenzene, bishydroxyethylene terephthalate, 1-methyl-1,2-ethanediol, and 1,6-hexanediol. These low molecular weight diols may be used alone or in combination of two or more. From the viewpoint of improving the releasability and recovery of the elastic fiber and suppressing nozzle clogging in the diaper manufacturing process, the low molecular weight diol is preferably a diol having a molecular weight of 60 to 120, and more preferably 1,4-butanediol. In the thermoplastic polyurethane elastic fiber of this embodiment, by using a diol having a molecular weight of 60 to 120 as a chain extender, the hydrogen bonds of the hard segments are strengthened, and the releasability and recovery can be improved.

[0021] Thermoplastic polyurethane can be produced by a known polyurethane reaction technique, and may be produced by either a one-shot method or a prepolymer method. In the case of the prepolymer method, a polymer polyol and a diisocyanate are added to a reaction tank having a hot water jacket and a stirrer under nitrogen purging, preferably in a molar ratio of 1.0:1.8-3.0, more preferably 1.0:2.0-2.5, and a prepolymer reaction is carried out at a temperature of preferably 40°C or more and 100°C or less, more preferably 50°C or more and 80°C or less to obtain a prepolymer having isocyanate groups at both ends. Next, an active hydrogen compound is added to the prepolymer having isocyanate groups at both ends in an equivalent amount approximately equal to the number of functional groups of the isocyanate terminal group, and a chain extension reaction is carried out. The equivalent ratio is preferably 0.95 to 1.1, more preferably 0.99 to 1.05, relative to the isocyanate terminal group. Then, solid-phase polymerization is carried out to obtain a thermoplastic polyurethane of a predetermined molecular weight. As a method of chain extension reaction and solid-state polymerization, an active hydrogen compound may be added directly to a batch reaction vessel containing a prepolymer at preferably 40° C. to 100° C., and then discharged and solid-state polymerization may be carried out at preferably 60° C. to 200° C., more preferably 70° C. to 150° C., and pelletized to obtain a chip-like polymer. After uniformly mixing the prepolymer and the active hydrogen compound, a cylindrical pipe-shaped or twin-screw extruder may be used to set the cylinder temperature of the polymerization zone to preferably 160° C. to 240° C., and a polymer may be obtained continuously or semi-continuously, and then solid-state polymerization may be carried out at preferably 60° C. to 220° C., more preferably 70° C. to 150° C.

[0022] The weight average molecular weight (Mw) of the thermoplastic polyurethane elastic fiber of this embodiment, when measured by GPC using polystyrene as a standard, is preferably 80,000 or more and 800,000 or less, more preferably 80,000 or more and 500,000 or less, and even more preferably 100,000 or more and 300,000 or less.

[0023] The number average molecular weight (Mn) of the thermoplastic polyurethane elastic fiber of the present embodiment, when measured by GPC using polystyrene as a standard, is preferably 40,000 or more and 400,000 or less, more preferably 40,000 or more and 250,000 or less, and even more preferably 50,000 or more and 150,000 or less.

[0024] The polydispersity (Mw / Mn) of the thermoplastic polyurethane elastic fiber of the present embodiment, when measured by GPC using polystyrene as a standard, is preferably 1.8 to 3.5, more preferably 1.8 to 3, and even more preferably 18,000 to 2.5.

[0025] In the thermoplastic polyurethane elastic fiber of the present embodiment, if the ratio of the maximum value to the minimum value of the single yarn diameter constituting the multifilament is 1.1 or more and 2.0 or less, the effect of improving the recovery property and unwinding property is further enhanced, which is preferable. By making the ratio of the maximum value to the minimum value of the single yarn diameter 1.1 or more, the unwinding property can be improved, and this effect becomes more effective by making the ratio of the maximum value to the minimum value of the single yarn diameter 1.2 or more. By making the ratio of the single yarn diameter 1.1 or more in this way, it is considered that the contact area between the yarns is reduced by making the single yarn diameters vary appropriately, and the unwinding property can be improved. By making the ratio of the maximum value to the minimum value of the single yarn diameter 2.0 or less, the recovery property and unwinding property can be improved, and this effect becomes more effective by making the ratio of the maximum value to the minimum value of the single yarn diameter 1.8 or less. By making the ratio of the single yarn diameter 2.0 or less in this way, the variation in physical properties between the single yarns is reduced, and therefore the recovery property and unwinding property can be improved. The method of controlling the ratio of the maximum and minimum values ​​of the single yarn diameter is not particularly limited, but a method of aligning yarns discharged from two spinnerets with different numbers of holes to produce a thermoplastic polyurethane elastic fiber is preferably used. Specifically, a thermoplastic polyurethane resin melted in an extruder is discharged from two spinnerets with different numbers of holes so that the same weight is obtained, two yarns with the same fineness but different numbers of filaments are formed, and then aligned in a false twisting process to produce a single thermoplastic polyurethane elastic fiber. More specifically, for example, when a thermoplastic polyurethane resin is discharged from spinnerets with 40 and 20 holes, each with a weight that results in a yarn of 310 dtex, to form two yarns, and then aligned in a false twisting process, the thermoplastic polyurethane elastic fiber as a whole has a diameter of 620 dtex and a number of filaments of 60, but the single yarn from a spinneret with 20 holes has a diameter of about 1.5 times that of a single yarn from a spinneret with 40 holes, so that the ratio of the maximum and minimum values ​​of the single yarn diameter can be about 1.5.As other methods for controlling the ratio of the maximum and minimum single yarn diameters, there can be suitably used a method for appropriately shaking the yarn during spinning by adjusting the die temperature, the cold air length, cold air speed, and cold air temperature of the cold air chamber, a method for precisely controlling the temperature profile of the fiber during spinning by adjusting the focusing position and spinning speed, and a method for controlling the tension of the elastic fiber in the spinning tube by adjusting the speed of the godet roller during winding.

[0026] In the thermoplastic polyurethane elastic fiber of this embodiment, from the viewpoint of improving recovery and unwinding properties, the single yarn fineness is preferably 5 dtex to 40 dtex, more preferably 5 dtex to 20 dtex, and even more preferably 8 dtex to 20 dtex. By setting the single yarn fineness to 5 dtex to 40 dtex, it becomes easier to apply uniform tension to the single yarn during spinning, so that the variation in physical properties between single yarns is reduced, and recovery and unwinding properties can be improved. This effect becomes more effective by setting the single yarn fineness to 8 dtex to 20 dtex.

[0027] The fineness and number of filaments of the thermoplastic polyurethane elastic fiber of the present embodiment are not particularly limited as long as a thermoplastic polyurethane elastic fiber having physical properties suitable for gathers and sanitary materials can be obtained. The fineness is preferably 100 dtex or more and 2000 dtex or less, more preferably 300 dtex or more and 1500 dtex or less. The number of filaments is preferably 10 or more and 120 or less.

[0028] In this embodiment, the flow start temperature of the thermoplastic polyurethane elastic fiber measured by a flow tester is preferably 150°C or more, or 180°C or more, and is preferably 220°C or less, 200°C or less, or 180°C or less. By setting the flow start temperature to 150°C or more, the tackiness of the thermoplastic polyurethane elastic fiber can be suppressed, and sufficient unwinding property can be obtained without yarn breakage during processing. By setting the flow start temperature to 220°C or less, recovery property and unwinding property can be improved. The reason for this is not yet clear, but the inventor presumes it as follows. By setting the flow start temperature of the thermoplastic polyurethane elastic fiber to 220°C or less, the mobility of the hard segment and the soft segment is increased, and the hard domain and the soft domain are easily compatible with each other, so that the hard domain and the soft domain are finely dispersed in the yarn, and high recovery property and unwinding property are exhibited. The method for producing the thermoplastic polyurethane elastic fiber with the flow start temperature of 150°C or more and 220°C or more is not particularly limited, but there are, for example, a method of setting the weight average molecular weight of the polyurethane polymer within a certain range, a method of adjusting the hard segment content in the polymer, and the like. The number average molecular weight of the polyurethane polymer can be controlled within a certain range, for example, by adjusting the equivalent ratio of the active hydrogen compound added to the isocyanate terminal functional group of the prepolymer having isocyanate groups at both ends in the prepolymer method. In general, the number average molecular weight can be increased by bringing the equivalent ratio closer to 1 with respect to the isocyanate terminal group.

[0029] In the thermoplastic polyurethane elastic fiber of this embodiment, from the viewpoint of improving recovery and unwinding properties and suppressing nozzle clogging, the ratio of 100% elongation stress at 20°C to 100% elongation stress at 80°C (hereinafter also referred to as "elongation stress ratio") is preferably 1.30 to 3.00, more preferably 1.30 to 2.70, and most preferably 1.50 to 2.50. The reason why the unwinding properties and unwinding properties can be improved and nozzle clogging can be suppressed by setting the elongation stress ratio to 1.30 to 3.00 is not yet clear, but the inventors presume as follows. By setting the elongation stress ratio to 1.30 or more, the physical properties at room temperature when the yarn is released are not too low, so that the yarn is unwound with an appropriate tension and the unwinding properties can be improved. In addition, by making the ratio of elongation stress 1.30 or more, the physical properties at high temperature when the hot melt adhesive is applied can be reduced, the frictional resistance between the nozzle and the yarn is reduced, and the amount of charge on the yarn is reduced, so that paper powder, which causes nozzle clogging, is less likely to adhere to the yarn. In addition, by making the ratio of elongation stress 3.00 or less, the change in the chemical structure of the yarn during the elongation process can be reduced, and recovery can be improved. In particular, when the ratio of elongation stress is 1.50 or more and the content of the specific compound is 0.05 ppm or more and 5 ppm or less, nozzle clogging is significantly suppressed. Although there is no particular limitation on the method for producing a thermoplastic polyurethane elastic fiber having a ratio of elongation stress of 1.30 or more and 3.00 or less, a method of controlling the crystal structure of the hard domain of the thermoplastic polyurethane elastic fiber by controlling the cooling and heating profile in the melt spinning process can be exemplified. For example, a method of cooling the yarn discharged from the spinneret by applying cold air using a cooling chamber installed directly below the spinneret, and then reheating the yarn using a heating cylinder and winding it via a godet roll can be exemplified.

[0030] In the thermoplastic polyurethane elastic fiber of the present embodiment, from the viewpoint of improving the releasability and recovery, it is preferable that the fiber is substantially free of allophanate bonds in which urethane bonds are crosslinked by the reaction of isocyanate groups. Here, "substantially free of allophanate bonds" means that the fiber is determined to be "substantially free of crosslinks containing allophanate bonds" by the "method of determining the presence or absence of crosslinks containing allophanate bonds" described below. By substantially free of crosslinks containing allophanate bonds, it is possible to prevent the deterioration of releasability caused by crosslinking of urethane groups between single yarns by isocyanate groups generated by the decomposition of allophanate bonds with low thermal stability. Furthermore, by substantially free of crosslinks containing allophanate bonds, it is possible to prevent the decomposition of allophanate bonds with low thermal stability, and it is possible to prevent the deterioration of recovery. In addition to allophanate bonds, biuret bonds formed by the reaction of isocyanate groups are also exemplified as crosslinks formed by the reaction of isocyanate groups with urea bonds, but since the polyurethane elastic fiber of this embodiment has a small amount of urea bonds, the amount of biuret bonds that can be formed is also extremely small, and the influence of biuret bonds may be ignored. There are no particular limitations on the method for producing a thermoplastic polyurethane elastic fiber that is substantially free of crosslinks including allophanate bonds, but for example, a method for producing a thermoplastic polyurethane elastic fiber from a thermoplastic polyurethane polymerized by controlling the total number of moles of a chain extender consisting of a polymer polyol and an active hydrogen compound to be equal to or greater than the number of moles of isocyanate is preferably used.

[0031] The thermoplastic polyurethane elastic fiber of the present embodiment may contain polymers other than thermoplastic polyurethanes and additives, such as antioxidants, light fasteners, ultraviolet absorbers, gas discoloration inhibitors, dyes, activators, matting agents, lubricants, etc., to the extent that the desired effects of the present invention are not lost.

[0032] In the present embodiment, from the viewpoint of reeling property, processability, etc., a treatment agent such as an oil agent may be applied to the thermoplastic polyurethane elastic fiber. Examples of the treatment agent include, but are not limited to, silicone-based oils such as dimethyl silicone, mineral oils, and combinations thereof. The method of applying the treatment agent is not particularly limited, and examples thereof include a method of applying the treatment agent using an oiling roller or the like.

[0033] [Method of manufacturing thermoplastic polyurethane elastic fiber] The spinning method is not particularly limited as long as the desired physical properties can be obtained, but it is preferable to manufacture by melt spinning.Specific methods of melt spinning include, for example, a method of feeding thermoplastic polyurethane resin chips into an extruder, heating, and melt spinning, a method of melting thermoplastic polyurethane resin chips, mixing them with a polyisocyanate compound, and spinning them, and a method of adding a reaction product of a prepolymer with isocyanate groups at both ends and an active hydrogen compound to a prepolymer with isocyanate groups at both ends, and continuously spinning them without chipping.

[0034] The thermoplastic polyurethane fed into the extruder is metered by a metering pump and introduced into the spinning head. If necessary, foreign matter is removed by filtration using a wire mesh or glass beads in the spinning head, and the mixture is discharged from the spinneret, air-cooled in a cold air chamber, treated with a treatment agent, and wound up via a godet roll.

[0035] In the spinning process, the die temperature, cold air speed, cold air temperature, heating barrel temperature, focusing position, and spinning speed are adjusted to precisely control the temperature profile and spinning tension of the fiber. The die temperature is preferably 180°C to 220°C, more preferably 200°C to 210°C. A general melt spinning cooling method is used, such as a method in which cold air is applied perpendicularly to the running direction of the yarn from just below the spinneret, and the cold air speed is preferably 0.2m / s to 2.0m / s, more preferably 0.5m / s to 1.2m / s, and the cold air temperature is preferably 5°C to 20°C, more preferably 7°C to 15°C. As a method for focusing the multifilaments, a false twisting machine is installed between the spinneret and the godet roll, and the twist is propagated from the bottom depending on the strength of the twist, the filaments are focused with each other, and the height of the focusing point is controlled. The false twisting method can be selected from the usual methods, such as air false twisting using an air nozzle, or a ring false twisting machine in which the yarn is brought into contact with a rotating ring.

[0036] In the method for producing the thermoplastic polyurethane elastic fiber of the present embodiment, the method for incorporating the specific compound at 0.05 ppm or more and 100 ppm or less is not particularly limited, but examples thereof include a method of melt spinning a thermoplastic polyurethane resin containing a predetermined amount of the specific compound in advance, a method of adding a predetermined amount of the specific compound in an extruder, and a method of applying a treatment agent containing the specific compound to the yarn when winding it up. From the viewpoint of ease of controlling the content of the specific compound, the method of melt spinning a thermoplastic polyurethane resin containing the specific compound is preferred, and in this case, it is particularly preferred to use a thermoplastic polyurethane elastic resin containing the specific compound at 0.05 ppm or more and 100 ppm or less.

[0037] [Gathers, sanitary materials] Gathers and sanitary materials containing the thermoplastic polyurethane elastic fiber of this embodiment are also aspects of the present invention. Specific examples of sanitary materials include absorbent articles such as disposable paper diapers and sanitary products, masks, bandages, etc. In paper diapers, gathers in which elastic fibers are bonded to nonwoven fabrics via hot melt are used in the waist and leg areas, and the gathers of this embodiment are preferably used in such areas. Since the thermoplastic polyurethane elastic fiber of this embodiment has good unwinding properties, gathers and sanitary materials can be produced with a high yield in the processing step. In addition, since the thermoplastic polyurethane elastic fiber of this embodiment has high recovery properties, gathers and sanitary materials that are easy to put on and take off, have a good fit, and are not likely to slip off can be produced. EXAMPLES

[0038] The present invention will be specifically described with reference to the following examples and comparative examples, but the technical scope of the present invention is not limited to the following examples. The evaluation methods used in the examples and comparative examples are as follows.

[0039] (1) GC measurement (measurement of the content of specific compounds in yarn) 0.2 g of thermoplastic polyurethane elastic fiber is weighed out, immersed in 10 g of acetone, and extracted for 5 hours for analysis. The concentration of a specific compound can be calculated in weight percent by comparing with the area of ​​a calibration curve of the specific compound separately prepared using GC. GC device: Agilent Technologies 7890A Inlet temperature: 320℃ Column: DB-1MS (30m x 0.25mmφ), liquid phase thickness 0.25μm Column temperature: 40°C (hold time 5 min), 20°C / min heating, 320°C (hold for 11 min) MS instrument: Agilent Technologies 5975C MSD Ion source temperature: 230℃ Ionization method: Electron ionization method If the amount of thermoplastic polyurethane elastic fiber that can be collected is less than 0.2 g, the amount of acetone may be adjusted so that the concentration of the thermoplastic polyurethane elastic fiber becomes the same as in the above test.

[0040] (2) NMR measurement (qualitative analysis of low molecular weight diols) A certain amount of thermoplastic polyurethane elastic fiber was dried at 80°C for 5 hours under a vacuum of -0.1 MPa, and NMR was measured under the following conditions to qualitatively identify the low molecular weight diol (specify the type and molecular weight). [NMR measurement conditions] Measurement equipment: AVANCE NEO600 manufactured by Bruker Japan Measurement nuclei: 1 H Resonance frequency: 600MHz Number of times accumulated: 256 Measurement temperature: room temperature Solvent: Deuterated dimethylformamide Measured concentration: 0.5% by weight Chemical shift reference: dimethylformamide (8.0233 ppm)

[0041] (3) Measurement of the ratio of maximum to minimum single yarn diameter A 1m sample of thermoplastic polyurethane elastic fiber was taken, and the diameters of all single yarns were measured at five randomly selected cross sections, and the ratio of the maximum value to the minimum value was taken as the ratio of the maximum single yarn diameter to the minimum value. The diameters of each single yarn were measured by observing the cross section of the thermoplastic polyurethane elastic fiber using an electron microscope JSM-6510 manufactured by JEOL Ltd. In addition, when the cross section of a single yarn is not circular but has an irregular cross section such as an ellipse or a dumbbell shape, a circle with the smallest diameter that completely contains the cross section (hereinafter also referred to as the "minimum inclusive circle") was drawn, and the diameter of the minimum inclusive circle was taken as the single yarn diameter.

[0042] (4) Measurement of single yarn size The single yarn fineness of the thermoplastic polyurethane elastic fiber was measured and calculated by the following procedure. A sample was prepared by unwinding 0.5 m of the thermoplastic polyurethane elastic fiber from the thermoplastic polyurethane elastic fiber wound body in a relaxed state length (hereinafter also referred to as the "relaxed length"), and the weight (g) of the sample was measured. The fineness of the thermoplastic polyurethane elastic fiber in a relaxed state (relaxed fineness A (dtex)) was calculated using the following formula. The measurement was performed four times, and the average value was taken. The "relaxed state" refers to a state in which the yarn was left unwound from the cheese and left unloaded for at least two hours. Relaxed fineness A (dtex) = sample weight (g) x 10,000 / relaxed length (m) The number B of single yarns was measured by observing the cross section of the thermoplastic polyurethane elastic fiber using an electron microscope JSM-6510 manufactured by JEOL Ltd. The formula is as follows: Single yarn size (dtex) = A / B From this, the single filament fineness (dtex) of the thermoplastic polyurethane elastic fiber was calculated.

[0043] (5) Flow start temperature measurement of thermoplastic polyurethane elastic fiber The flow start temperature of the thermoplastic polyurethane elastic fiber is measured using a flow tester CFT-500D type (manufactured by Shimadzu Corporation). The thermoplastic polyurethane elastic fiber is not subjected to any pretreatment such as removing treatment agents such as oils, and 1.5 g of the fiber is sampled for each measurement to measure the flow start temperature. A die (nozzle) with a diameter of 0.5 mm and a thickness of 1.0 mm is used, and an extrusion load of 49 N is applied. After a preheating time of 240 seconds at an initial setting temperature of 120°C, the temperature is raised at a constant rate of 3°C / min to 250°C, and a curve of stroke length (mm) and temperature is obtained. As the temperature rises, the polymer in the toner is heated and the polymer begins to flow out of the die. The temperature at this time is the flow start temperature.

[0044] (6) Measurement of recovery of thermoplastic polyurethane elastic fiber Using a tensile testing machine (EZ-SX AUTOGRAPH manufactured by Shimadzu Corporation), in an atmosphere of 20°C and 65% RH, the thermoplastic polyurethane elastic fiber was set on the tensile testing machine with an initial length of 5 cm, and the elongation and recovery up to 200% at a speed of 1000% / min were repeated 3 times. The stress R (cN) at 90% elongation during the third elongation and the stress R' (cN) at 90% elongation during the third recovery were measured. · The following calculation formula: Recovery (%) = (R' / R) × 100 From this, the recovery (%) of the thermoplastic polyurethane elastic fiber was calculated.

[0045] (7) Method for determining the presence or absence of crosslinking containing allophanate bonds The polyurethane elastic fiber that dissolved in the following DMAc dissolution test and in which no allophanate bond could be confirmed by the following NMR measurement was determined as the one "substantially having no crosslinking containing allophanate bonds" in this specification. The polyurethane elastic fiber that did not dissolve in the following DMAc dissolution test or that dissolved in the following DMAc dissolution test but in which an allophanate bond could be confirmed by the following NMR measurement was determined as the one "having crosslinking containing allophanate bonds". <DMAc Dissolution Test> Precisely weigh 0.2 g of the polyurethane elastic fiber, immerse it in 10 g of DMAc, and stir at 20°C for 48 hours. After stirring, if no polymer lumps with a diameter of 1 mm or more can be visually confirmed, it was determined that it had dissolved in DMAc. <NMR Measurement (Qualitative Analysis of Allophanate Bonds)> A predetermined amount of the polyurethane elastic fiber dried under a vacuum of -0.1 MPa at 80°C for 5 hours and internal standard dimethyl sulfoxide were measured and NMR was measured under the following conditions. By this measurement, the ratio of allophanate bonds to urethane bonds was confirmed. The ratio of allophanate bonds to urethane bonds can be calculated by comparing the integral values of each hydrogen. When this ratio is less than 0.05%, it is defined that no allophanate group is contained. Generally, the hydrogen signal of allophanate bonds is often observed at 10.5 - 11.0 ppm, but this is not absolute. [NMR Measurement Conditions] Measuring device: JEOL ECS400 Measurement nuclei: 1 H Resonance frequency: 400MHz Number of times accumulated: 256 Measurement temperature: room temperature Solvent: Deuterated dimethylformamide Measured concentration: 1.5% by weight Chemical shift reference: dimethylformamide (8.0233 ppm)

[0046] (8) Measurement method of tensile stress ratio Using a tensile tester (Orientec Co., Ltd. RTG-1210 Tensilon) and a constant temperature and humidity tester, the elastic fiber is set in the tensile tester so that it has an initial length of 5 cm and an initial load of 0 cN without deflection under an atmosphere of 20°C and 65% RH and an atmosphere of 80°C, respectively, and is stretched to an elongation of 200% at an elongation rate of 500% / min, and the stress (cN) at 100% elongation is measured. Here, the stress at 100% elongation in a 20°C atmosphere is R, and the stress at 100% elongation in an 80°C atmosphere is R', and the following calculation formula is used: Ratio of extension stresses = R' / R The ratio of the elongation stress of the elastic fiber was calculated from the above. The tensile tests at 20°C and 80°C were carried out using separate samples.

[0047] (9) Gather manufacturing example Four thermoplastic polyurethane elastic fibers were arranged in parallel at intervals of 7 mm and stretched to 2.5 times their original length. A hot melt adhesive (765E manufactured by Henkel Japan Ltd.) melted at 150°C was continuously applied to the stretched thermoplastic polyurethane elastic fibers using a V-shaped slit so that the amount of adhesive applied per stretched thermoplastic polyurethane elastic fiber was 0.04 g / m. The thermoplastic polyurethane elastic fibers coated with the hot melt adhesive were then stretched to a width of 30 cm and a basis weight of 17 g / m. 2The fabric was sandwiched between two sheets of nonwoven fabric (Eltasguard, manufactured by Asahi Kasei Corporation) and then continuously pressed from above with a pair of rollers measuring 16 cm in outer diameter and 40 cm in width, one of which was pressed using an air cylinder (CQ2WB100-50DZ, manufactured by SMC Corporation) supplying 0.5 MPa of air pressure, to create gathers.

[0048] (10) Wearing comfort of gathers The gathers made in (9) were left in an unstretched state for one day to allow the stress of the elastic fibers to fully relax. After that, a 42 cm long ring was made from the relaxed gathers. Ten subjects with waist lengths of 75 cm to 80 cm wore this ring around their waists, and the degree of tightness was scored based on the number of subjects who judged it to be.

[0049] (11) Method for evaluating the reelability of thermoplastic polyurethane elastic fiber The elastic fiber was peeled off from the paper tube until the winding thickness was 1 cm, and the wound elastic fiber body was placed in the device shown in Figure 1, and the elastic fiber feed roll 2 was run at a speed of 50 m / min, the pre-draft roll 3 around which the elastic fiber was wound three times was run at a speed of 80 m / min, and the take-up roll 4 was run at a speed of 85 m / min. The behavior of the elastic fiber at the observation site 5 was visually observed for 3 minutes, and the yarn sway was evaluated according to the following evaluation criteria. In this evaluation, the smaller the yarn sway width, the smaller the frictional resistance during use of the yarn and the less likely it is to break the yarn. (Evaluation Criteria) 10: The thread sway width is between 0 mm and 1 mm. 9: The thread sway width is 1mm or more and less than 2mm. 8: The thread sway width is 2mm or more and less than 3mm. 7: The thread sway width is 3mm or more and less than 4mm. 6: The thread sway width is 4mm or more and less than 5mm. 5: The thread sway width is 5 mm or more and less than 6 mm. 4: The thread sway width is 6 mm or more and less than 7 mm. 3: The thread sway width is 7 mm or more and less than 8 mm. 2: The thread sway width is 8 mm or more and less than 9 mm. 1: The thread break width is 9 mm or more or there is a thread break. In addition, when the yarn sway width fluctuated between the two evaluation criteria in the 3-minute visual observation, the evaluation result was given a range, for example, "3 to 4."

[0050] (12) Method for evaluating nozzle clogging resistance Gathers were produced for 10 hours in the same manner as in (9), except that 10 polyurethane elastic fibers were arranged in parallel with each other at intervals of 7 mm and stretched to three times their original length, and the number of nozzles that had no dirt on the surface was recorded as a score.

[0051] [Example 1] 2400g of polytetramethylene ether diol having a number average molecular weight of 1800 and 750.75g of 4,4'-diphenylmethane diisocyanate were reacted under stirring in a dry nitrogen atmosphere at 60°C for 3 hours to obtain a polyurethane prepolymer capped with an isocyanate terminal. 150.95g of 1,4-butanediol was added to this polyurethane prepolymer and stirred for 15 minutes to obtain a polyurethane with a viscosity of 2000 poise (30°C). Thereafter, the polyurethane was poured onto a Teflon (registered trademark) tray, and annealed in the tray in a hot air oven at 110° C. for 19 hours to obtain a thermoplastic polyurethane resin.

[0052] The thermoplastic polyurethane resin thus obtained was pulverized into powder of about 3 mm using a UG-280 pulverizer manufactured by Horai Co., Ltd. The pulverized chips were dried in a dehumidifying dryer under a temperature condition of 110 ° C to a moisture content of 100 ppm, and then the thermoplastic polyurethane resin powder and DMAc were charged into the hopper so that the DMAc content of the thermoplastic polyurethane elastic fiber was 1 ppm, and melted in the extruder. After measuring and pressurizing with a gear pump installed in the head and filtering with a filter, the material was discharged at a discharge rate of 620 dtex from a nozzle with a diameter of 0.23 mm and 60 holes at a die temperature of 210 ° C. Thereafter, in order to adjust the ratio of the maximum and minimum values ​​of the single yarn diameter, cold air was blown from a cold air chamber in which the cold air length and cold air speed were appropriately adjusted, and the yarn was melt-spun by applying it perpendicularly to the fiber to moderately shake the yarn. The multifilaments were then passed through a heating cylinder, 50 cm long and with a central temperature of 130°C, placed directly below the cooling chamber, and twisted using a ring-type false twisting machine, and wound around a paper tube while being treated with a treatment agent mainly composed of polydimethylsiloxane and mineral oil, to obtain a wound thermoplastic polyurethane elastic fiber body of 620 dtex / 60 filaments. The thermoplastic polyurethane elastic fiber had a DMAc content of 1 ppm, a maximum / minimum ratio of single yarn diameter of 1.5, and an outflow start temperature of 160°C.

[0053] [Examples 2 to 6] Except for increasing or decreasing the amount of DMAc put into the hopper, a thermoplastic polyurethane elastic fiber of 620 dtex / 60 filaments was obtained in the same manner as in Example 1. The DMAc content of this thermoplastic polyurethane elastic fiber was 0.05 ppm to 100 ppm, the ratio of the maximum value to the minimum value of the single yarn diameter was 1.5, and the outflow start temperature was 159 to 161°C.

[0054] [Examples 7 to 11] A thermoplastic polyurethane elastic fiber of 620 dtex / 60 filaments was obtained in the same manner as in Example 1, except that the low molecular weight diol used to polymerize the thermoplastic polyurethane resin was changed from 1,4-butanediol to an equimolar amount of ethylene glycol (Example 7), 1,3-propanediol (Example 8), 1,3-butanediol (Example 9), 1,6-hexanediol (Example 10), or 1,8-octanediol (Example 11).

[0055] [Examples 12 to 16] A thermoplastic polyurethane elastic fiber of 620 dtex / 60 filaments was obtained in the same manner as in Example 1, except that the length and speed of cold air blown from the cold air chamber were increased or decreased.

[0056] [Examples 17 to 24] Thermoplastic polyurethane elastic fibers of 310 to 930 dtex and 14 to 120 filaments were obtained in the same manner as in Example 1, except that melt spinning was performed by increasing or decreasing the number of holes in the nozzle and the discharge amount.

[0057] [Examples 25 to 29] A thermoplastic polyurethane elastic fiber of 620 dtex / 60 filaments was obtained in the same manner as in Example 1, except that a thermoplastic polyurethane resin polymerized by increasing or decreasing the amount of 1,4-butanediol used to polymerize the thermoplastic polyurethane resin was used.

[0058] [Examples 30 to 32] Thermoplastic polyurethane elastic fibers of 620 dtex / 60 filaments were obtained in the same manner as in Example 1, except that the compound put into the hopper was changed from DMAc to DMF (Example 30), DMSO (Example 31), or NMP (Example 32).

[0059] [Examples 33 to 38] A thermoplastic polyurethane elastic fiber of 620 dtex / 60 filaments was obtained in the same manner as in Example 1, except that the central temperature of the concentric circle of the heating barrel was changed.

[0060] [Example 39] A thermoplastic polyurethane elastic fiber of 620 dtex / 60 filaments was obtained in the same manner as in Example 1, except that a thermoplastic polyurethane resin polymerized by increasing the amount of 4,4'-diphenylmethane diisocyanate used for polymerizing the thermoplastic polyurethane resin was used. Allophanate bonds were confirmed in this thermoplastic polyurethane elastic fiber by NMR measurement.

[0061] [Comparative Example 1] A thermoplastic polyurethane elastic fiber of 620 dtex / 60 filaments was obtained in the same manner as in Example 1, except that no DMAc was added to the hopper.

[0062] [Comparative Example 2] A thermoplastic polyurethane elastic fiber of 620 dtex / 60 filaments was obtained in the same manner as in Example 1, except that the amount of DMAc put into the hopper was adjusted so that the DMAc content of the thermoplastic polyurethane elastic fiber was 200 ppm. The production conditions, and the measurement results of the properties of the obtained thermoplastic polyurethane elastic fibers and gathers in the above-mentioned respective examples and comparative examples are shown in the following Tables 1 to 3.

[0063] [Table 1]

[0064] [Table 2]

[0065] [Table 3] [Industrial Applicability]

[0066] The thermoplastic polyurethane elastic fiber according to the present invention can be suitably used in the production of innerwear, stockings, compression wear, diapers, and the like. In particular, in the process of producing gathers, the fiber has good unwinding properties, can reduce the occurrence of thread breakage, and can produce gathers with excellent fitting properties. [Explanation of symbols]

[0067] 1. Elastic fiber winding 2. Delivery roll 3 Pre-draft roll 4 Take-up roll 5 Observation area 6 Ceramic Hook Guide 7. Bearing free roller

Claims

1. A thermoplastic polyurethane elastic fiber, characterized by containing at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP) in an amount of 0.05 ppm or more and 100 ppm or less.

2. The thermoplastic polyurethane elastic fiber according to claim 1, which contains at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP) in an amount of 0.05 ppm or more and 10 ppm or less.

3. The thermoplastic polyurethane elastic fiber according to claim 2, containing at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP) in an amount of 0.05 ppm or more and 5 ppm or less.

4. The thermoplastic polyurethane elastic fiber according to any one of claims 1 to 3, comprising a thermoplastic polyurethane composed of a polymer polyol, a diisocyanate, and a low molecular weight diol.

5. The thermoplastic polyurethane elastic fiber according to claim 4 , wherein the molecular weight of the low molecular weight diol is 60 or more and 120 or less.

6. The thermoplastic polyurethane elastic fiber according to any one of claims 1 to 3, wherein the thermoplastic polyurethane elastic fiber is a multifilament yarn, and the ratio of the maximum diameter to the minimum diameter of the constituent single yarns is 1.1 or more and 2.0 or less.

7. The thermoplastic polyurethane elastic fiber according to claim 6, having a single yarn fineness of 5 dtex or more and 40 dtex or less.

8. The thermoplastic polyurethane elastic fiber according to any one of claims 1 to 3, wherein the flow start temperature of the thermoplastic polyurethane elastic fiber as measured by a flow tester is 150°C or higher and 220°C or lower.

9. The thermoplastic polyurethane elastic fiber according to any one of claims 1 to 3, wherein the ratio of the 100% elongation stress at 20°C to the 100% elongation stress at 80°C is 1.30 or more and 3.00 or less.

10. The thermoplastic polyurethane elastic fiber according to any one of claims 1 to 3, which is substantially free of crosslinks containing allophanate bonds.

11. The thermoplastic polyurethane elastic fiber according to any one of claims 1 to 3, which is for use in sanitary materials.

12. A wound body of the thermoplastic polyurethane elastic fiber according to any one of claims 1 to 3.

13. A gather comprising the thermoplastic polyurethane elastic fiber according to any one of claims 1 to 3.

14. A sanitary material comprising the thermoplastic polyurethane elastic fiber according to any one of claims 1 to 3.

15. A method for producing a thermoplastic polyurethane elastic fiber according to any one of claims 1 to 3, comprising the step of melt spinning a polyurethane resin.

16. The method for producing thermoplastic polyurethane elastic fibers according to claim 15, wherein the polyurethane resin contains at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP).

17. The method for producing thermoplastic polyurethane elastic fibers according to claim 16, wherein the polyurethane resin contains at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP) in an amount of 0.05 ppm or more and 100 ppm or less.

18. 12. A method for producing a thermoplastic polyurethane elastic fiber according to claim 11, comprising the step of melt spinning a polyurethane resin containing 0.05 ppm or more and 100 ppm or less of at least one selected from the group consisting of dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), and N-methylpyrrolidone (NMP).

Citation Information

Patent Citations

  • Finish for elastic fiber

    JP2003049368A

  • Polyurethane elastic fiber

    JP2015224399A

  • Treatment agent for elastic fiber, elastic fiber and method for producing elastic fiber and polyurethane-based elastic fiber

    JP2017186704A

  • Urethane resin solution, process for production thereof, and process for production of urethane resin

    WO2006043568A1

  • Polyurethane elastic fiber and wound body thereof

    WO2019103013A1