Membrane electrode assembly, solid oxide fuel cell, and electrochemical device
A membrane electrode assembly with a proton conductor electrolyte and specific lanthanum strontium cobalt iron composite oxide air electrode addresses high manufacturing costs and reliability issues in solid oxide fuel cells by enhancing power generation efficiency and water vapor resistance at lower operating temperatures.
Patent Information
- Application Number
- JP2021515860
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-28
- Filing Date
- 2020-03-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-03-09
AI Technical Summary
Existing solid oxide fuel cells using stabilized zirconia as a solid electrolyte face high manufacturing costs and reliability issues due to high operating temperatures, which lead to increased energy requirements and longer startup times, along with potential electrode peeling and cracking from thermal expansion differences.
The use of a membrane electrode assembly with an electrolyte membrane containing a proton conductor, such as BaZr1-x1M1x1O3-γ, BaCe1-x2M2x2O3-γ, or BaZr1-x3-y3Ce3x3O3-γ, and an air electrode composed of lanthanum strontium cobalt iron composite oxide with a specific molar ratio of cobalt to iron between 0.35 and 0.6, reduces ohmic resistance and enhances water vapor resistance stability at operating temperatures of 600°C or lower.
This configuration improves power generation efficiency and maintains high water vapor resistance stability, reducing reaction resistance and operational costs while preventing electrode decomposition under humid conditions.
Smart Images

Figure 0007584062000002 
Figure 0007584062000003 
Figure 0007584062000004
Abstract
Description
Technical Field
[0001] The present disclosure relates to a membrane electrode assembly, a solid oxide fuel cell, and an electrochemical device.
Background Art
[0002] As an electrochemical device including a membrane electrode assembly including an electrolyte membrane made of a solid oxide and an electrode, for example, a solid oxide fuel cell, a water electrolysis cell, and a steam electrolysis cell are known. As the solid electrolyte of the electrochemical device, an oxide ion (O 2- ) conductor typified by stabilized zirconia is widely used. The oxide ion conductor has a lower ionic conductivity at lower temperatures. For this reason, for example, the operating temperature of a solid oxide fuel cell using stabilized zirconia as the solid electrolyte is desirably 700° C. or higher. The operating temperature is particularly desirably in the range of 700° C. or higher and 1000° C. or lower.
[0003] By the way, in a solid oxide fuel cell using stabilized zirconia as the solid electrolyte, a lanthanum strontium cobalt iron composite oxide is used as the most common air electrode material. This is represented by the composition formula of La 1-m Sr m Co n Fe 1-n O 3-δ (0 < m < 1, 0 < n < 1, δ represents the amount of oxygen deficiency, 0 ≦ δ ≦ 0.5), and La with m = 0.4 and n = 0.2 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ is preferred. This is because when operating at 700° C. or higher, the reaction resistance of the electrode reaction (O2 + 4e - →2O 2- ) at the air electrode is small, the power generation efficiency is increased, the material is relatively stable even at high temperatures, and the difference in thermal expansion coefficient from the solid electrolyte is small, so that peeling of the electrode during temperature increase and decrease during startup and shutdown can be suppressed.
[0004] However, when the operating temperature of an electrochemical device is as high as 700°C or higher, there is a problem of increased manufacturing costs. In other words, when the operating temperature is as high as 700°C or higher, it is necessary to cover the outer periphery of the electrochemical device with a thick, high-performance insulating material. As a result, manufacturing costs increase. Furthermore, expensive special heat-resistant metals are required as components of a system including this electrochemical device, so the manufacturing costs of the entire system also increase.
[0005] In addition, when the system is started and stopped, differences in thermal expansion of the components can easily cause cracks, reducing the reliability of the system. Other issues include longer start-up times and an increase in the amount of energy required for start-up.
[0006] Therefore, lowering the operating temperature of electrochemical devices such as solid oxide fuel cells that use a solid electrolyte made of solid oxide is one of the major goals for their practical application.Solid oxide fuel cells that use a proton conductor as the solid electrolyte and can operate at temperatures below 600°C, especially between 350°C and 600°C, have attracted attention.
[0007] In solid oxide fuel cells that use a proton conductor as the solid electrolyte, the reaction (O2 + 4H + +4e - →2H2O), water vapor is generated. Therefore, the effect of water vapor at the air electrode must be taken into consideration.
[0008] For example, Non-Patent Document 1 mentions the stability of lanthanum strontium cobalt iron composite oxide or lanthanum strontium cobalt composite oxide used as an air electrode material against water vapor in the air. In other words, it is shown that the presence of water vapor in the air causes decomposition of lanthanum strontium cobalt iron composite oxide and lanthanum strontium cobalt oxide. In particular, in the case of lanthanum strontium cobalt oxide containing a large amount of Co, the decrease in water vapor resistance stability is remarkable. [Prior art documents] [Non-patent literature]
[0009] [Non-Patent Document 1] I.Kivi et. al., “Influence of humidified synthetic air feeding conditions on the stoichiometry of (La1-xSrx)yCoO3-δ and La0.6Sr0.4Co0.2Fe0.8O3-δ cathodes under applied potential measured by electrochemical in situ high-temperature XRD method” J Solid State Electrochem, 2017, 21, 361-369 Summary of the Invention [Problem to be solved by the invention]
[0010] However, in the past, in a membrane electrode assembly including an electrolyte membrane using a solid electrolyte having proton conductivity and an electrode, the reaction efficiency and water vapor resistance stability at operating temperatures of 600°C or lower have not been sufficiently studied.
[0011] Therefore, the present disclosure provides a membrane electrode assembly, a solid oxide fuel cell, and an electrochemical device that have high reaction efficiency and water vapor resistance stability at operating temperatures of 600° C. or less. [Means for solving the problem]
[0012] One embodiment of the membrane electrode assembly of the present disclosure includes an electrolyte membrane containing an oxide having proton conductivity, and an electrode provided on the electrolyte membrane and containing a lanthanum strontium cobalt iron composite oxide, wherein the ratio of the number of moles of cobalt to the sum of the number of moles of cobalt and the number of moles of iron in the electrode is a value in the range of 0.35 or more and 0.6 or less.
[0013] One aspect of the solid oxide fuel cell of the present disclosure has a membrane electrode assembly including an electrolyte membrane containing an oxide having proton conductivity, and an electrode provided on the electrolyte membrane and containing a lanthanum strontium cobalt iron composite oxide, in which the ratio of the number of moles of cobalt to the sum of the number of moles of cobalt and the number of moles of iron in the electrode is a value in the range of 0.35 to 0.6.
[0014] One embodiment of the electrochemical device of the present disclosure has a membrane electrode assembly including an electrolyte membrane containing an oxide having proton conductivity, and an electrode provided on the electrolyte membrane and containing a lanthanum strontium cobalt iron composite oxide, in which the ratio of the number of moles of cobalt to the sum of the number of moles of cobalt and the number of moles of iron in the electrode is a value in the range of 0.35 to 0.6. Effect of the Invention
[0015] The present disclosure is configured as described above, and has the effect of providing high reaction efficiency and water vapor resistance stability at operating temperatures of 600° C. or lower. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic configuration of a membrane electrode assembly included in an electrochemical device according to a first embodiment of the present disclosure. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a schematic configuration of a membrane electrode assembly included in an electrochemical device according to a second embodiment of the present disclosure. [Diagram 3] FIG. 3 is a graph showing the results of measurement by X-ray diffraction method for the LSCFs according to Examples 2 and 3 and the LSCFs according to Comparative Examples 1 to 4 of the present disclosure. [Figure 4] FIG. 4 is a diagram showing an example of an AC impedance measurement result in an embodiment of the present disclosure by a Cole-Cole plot. [Diagram 5] FIG. 5 is a graph showing the relationship between the molar ratio of Co to the sum of the moles of Co and Fe and the reaction resistance for the air electrodes according to Examples 1 to 3 and Comparative Examples 1 to 4 of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] (How one embodiment of the present disclosure was achieved) When a membrane electrode assembly using stabilized zirconia as an electrolyte membrane is used at an operating temperature of 600°C, the ohmic resistance of the electrolyte membrane becomes large. As a result, for example, in a solid oxide fuel cell having this membrane electrode assembly, the power generation efficiency decreases. This is because the activation energy of oxide ion conduction in stabilized zirconia is large, and the oxide ion conductivity decreases significantly at temperatures below 600°C.
[0018] In addition, in solid oxide fuel cells with membrane electrode assemblies that use stabilized zirconia as an electrolyte membrane, La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ (δ is the amount of oxygen vacancy. 0≦δ≦0.5) When operating at 600°C, the reaction resistance is greater than when operating at 700°C, leading to a decrease in power generation efficiency.
[0019] In order to obtain good power generation efficiency, the reaction resistance generated at the air electrode must be less than 1.0 V and the current density must be less than 0.2 A / cm in an open circuit state where no current is applied to a solid oxide fuel cell. 2 The voltage actually obtained during operation is 0.7 V or more, and the ohmic resistance of the electrolyte is 0.1 Ω cm 2 When set to 1.4Ωcm 2 It needs to be smaller.
[0020] Therefore, it has been proposed to use proton conductors as materials for electrolyte membranes that can reduce ohmic resistance at operating temperatures of 600°C or less. Among these proton conductors, barium zirconate oxides, barium cerate oxides, and barium zirconate cerate oxides are known to exhibit high proton conductivity. For example, BaZr 0.8 Y 0.2O3 or BaZr 0.8 Yb 0.2 O3 is 1.0×10 at 600℃. -2 It has high proton conductivity of over S / cm.
[0021] In a membrane electrode assembly that uses a proton conductor as the electrolyte membrane, the water vapor resistance of the electrode is important. For example, when a solid oxide fuel cell is constructed using a membrane electrode assembly that uses a proton conductor as the electrolyte membrane, the air electrode is charged with (O2 + 4H + +4e - Water vapor is generated by the reaction of O2 + 4H2O. For example, if the air utilization rate during power generation in a solid oxide fuel cell is 30%, the water vapor concentration in the air at the outlet of the solid oxide fuel cell is approximately 12%. In addition, the water vapor concentration may be even higher in localized electrode reactions. For example, oxygen in the air (volume fraction 21%) reacts with oxygen in the air to produce O2 + 4H2O. + 4e - →If all of the 2H2O reacts to become water vapor, the volume fraction of water vapor in the outlet air may be approximately 35%. Thus, in a membrane electrode assembly that uses a proton conductor as the electrolyte membrane, the electrodes are exposed to air with a high water vapor concentration. Therefore, in the case of electrode materials with low water vapor resistance, there is a concern that the electrodes may decompose.
[0022] Here, in Non-Patent Document 1, (La 0.6 Sr 0.4 ) x Chief of Staff 3-δ (0.99≦x≦1.01, 0≦δ≦0.5) and La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δIt discloses the effect of compositions used in air electrode materials on humidified air, such as a temperature range of 0≦δ≦0.5. In other words, Non-Patent Document 1 reports on the effect of water vapor on air electrode materials, assuming the water vapor concentration in normal air. However, Non-Patent Document 1 does not suggest the effect on electrode materials under operating conditions (e.g., 600°C and high water vapor concentration (e.g., the volume fraction of water vapor in air is 35%)) of a membrane electrode assembly using a proton conductor as an electrolyte membrane.
[0023] Therefore, the present inventors have conducted extensive research into a membrane electrode assembly that can achieve both high reaction efficiency and water vapor resistance stability at operating temperatures of 600°C or less. Note that water vapor resistance stability refers to the property of not changing the composition even under highly humidified conditions. In other words, under highly humidified conditions at 600°C or less, decomposition products may be generated in the electrode (hereinafter, sometimes referred to as the "air electrode") due to a reaction between a substance contained in the electrode and water. As a result, the composition of the electrode may change.
[0024] Specifically, we investigated a membrane electrode assembly that includes an electrolyte membrane using a proton conductor and an electrode that can reduce reaction resistance while maintaining high water vapor stability. We then clarified the molar ratio of cobalt (Co) to the sum of the moles of cobalt (Co) and the moles of iron (Fe) in a lanthanum strontium cobalt iron composite oxide that can form an electrode that can reduce reaction resistance while maintaining high water vapor stability at operating temperatures of 600°C or less.
[0025] The above-mentioned findings of the present inventors have not been disclosed so far, and show a membrane electrode assembly, a solid oxide fuel cell, and an electrochemical device having a novel configuration. Specifically, the present disclosure provides the following aspects.
[0026] A membrane electrode assembly according to a first aspect of the present disclosure includes an electrolyte membrane containing an oxide having proton conductivity, and an electrode provided on the electrolyte membrane and containing a lanthanum strontium cobalt iron composite oxide, wherein a ratio of the number of moles of cobalt to the sum of the number of moles of cobalt and the number of moles of iron in the electrode is a value in the range of 0.35 or more and 0.6 or less.
[0027] According to the above configuration, the ratio of the number of moles of cobalt to the sum of the number of moles of cobalt and the number of moles of iron in the electrode is a value in the range of 0.35 to 0.6, so that at the operating temperature of a solid electrolyte fuel cell using a proton conductor as the solid electrolyte, for example, at 600°C or lower, it is possible to improve reaction efficiency (i.e., power generation efficiency) by reducing reaction resistance, and to have high water vapor resistance stability.
[0028] A membrane electrode assembly according to a second aspect of the present disclosure is the membrane electrode assembly of the first aspect described above, wherein the electrolyte membrane and the electrodes are disposed in contact with each other.
[0029] According to the above configuration, the electrolyte membrane and the electrodes are arranged in contact with each other, and therefore the reaction resistance can be reduced, and the reaction efficiency can be improved.
[0030] A membrane electrode assembly according to a third aspect of the present disclosure is the membrane electrode assembly according to the first or second aspect described above, wherein the electrolyte membrane is BaZr 1-x1 M1 x1 O 3-γ , BaCe 1-x2 M2 x2 O 3-γ , and BaZr 1-x3-y3 Ce x3 M3 y3 O 3-γcomprising at least one compound selected from the group consisting of, M1, M2, and M3 are each independently at least one element selected from the group consisting of La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Y, Sc, Mn, Fe, Co, Ni, Al, Ga, In, and Lu, such that x1 satisfies 0 < x1 < 1, x2 satisfies 0 < x2 < 1, x3 satisfies 0 < x3 < 1, and y3 satisfies 0 < y3 < 1. Also, γ is the amount of oxygen deficiency and 0 < γ ≤ 0.5.
[0031] According to the above configuration, since the electrolyte membrane exhibits high proton conductivity, the ohmic resistance of the membrane electrode assembly can be reduced even in a temperature range where the operating temperature is 600 °C or lower. Therefore, when the membrane electrode assembly is used as a solid oxide fuel cell, the power generation efficiency can be improved even in a temperature range where the operating temperature is 600 °C or lower.
[0032] The membrane electrode assembly according to the fourth aspect of the present disclosure is, in the third aspect described above, the electrolyte membrane is BaZr 1-x1 Yb x1 O 3-γ and may be a compound represented by.
[0033] According to the above configuration, the electrolyte membrane can have high proton conductivity and high durability against carbon dioxide gas. Therefore, when the membrane electrode assembly is used as a solid oxide fuel cell, the power generation efficiency can be improved and the stability against carbon dioxide gas can be improved even in a temperature range where the operating temperature is 600 °C or lower.
[0034] The membrane electrode assembly according to the fifth aspect of the present disclosure is, in any one of the first to fourth aspects described above, the electrode may be an air electrode.
[0035] According to the above-mentioned configuration, when the electrode reaction proceeds as the air electrode in the membrane electrode assembly, the reaction resistance can be reduced, and at the same time, high water vapor resistance stability can be achieved even if the air electrode is exposed to a high water vapor concentration during the electrode reaction. That is, high reaction efficiency and water vapor resistance stability can be achieved at an operating temperature of 600°C or less.
[0036] A solid oxide fuel cell according to a sixth aspect of the present disclosure has an electrolyte membrane containing an oxide having proton conductivity, and an electrode provided on the electrolyte membrane and containing a lanthanum strontium cobalt iron composite oxide, and has a membrane electrode assembly in which the ratio of the number of moles of cobalt to the sum of the number of moles of cobalt and the number of moles of iron in the electrode is a value in the range of 0.35 or more and 0.6 or less.
[0037] According to the above configuration, the solid oxide fuel cell can have high power generation efficiency and water vapor resistance stability at an operating temperature of 600° C. or less.
[0038] An electrochemical device according to a seventh aspect of the present disclosure has an electrolyte membrane including an oxide having proton conductivity, and an electrode including a lanthanum strontium cobalt iron composite oxide provided on the electrolyte membrane, the electrode having a membrane electrode assembly in which the ratio of the number of moles of cobalt to the sum of the number of moles of cobalt and the number of moles of iron in the electrode is a value in the range of 0.35 or more and 0.6 or less.
[0039] According to the above configuration, the electrochemical device can have high reaction efficiency and water vapor resistance stability at an operating temperature of 600° C. or less.
[0040] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.
[0041] The embodiments described below are all comprehensive or specific examples. The numerical values, shapes, materials, components, arrangement positions and connection forms of the components shown in the following embodiments are merely examples and are not intended to limit the present disclosure. Furthermore, among the components in the following embodiments, components that are not described in the independent claims are described as optional components.
[0042] In addition, each figure is a schematic diagram and is not necessarily illustrated precisely. Therefore, for example, the scales in each figure do not necessarily match. In addition, in each figure, substantially the same configurations are given the same reference numerals, and duplicated explanations are omitted or simplified.
[0043] In this specification, terms indicating the relationship between elements, such as "parallel," terms indicating the shape of elements, such as "rectangle," and numerical ranges are not expressions that only express a strict meaning, but are expressions that include a substantially equivalent range, for example, a difference of about several percent. Note that the "thickness direction" in this specification is the direction in which the electrodes and the electrolyte membrane are stacked.
[0044] (First embodiment) [Configuration of membrane electrode assembly] Fig. 1 is a cross-sectional view that shows a schematic configuration of a membrane electrode assembly 10 included in an electrochemical device according to a first embodiment of the present disclosure. Fig. 1 shows a cross section of the membrane-like membrane electrode assembly 10 cut in its thickness direction. As shown in Fig. 1, the membrane electrode assembly 10 includes an electrolyte membrane 11 that includes a solid electrolyte that is an oxide having proton conductivity, and an air electrode 12 that is provided on the electrolyte membrane 11. That is, the membrane electrode assembly 10 has a laminated structure in which the electrolyte membrane 11 and the air electrode 12 are arranged in contact with each other.
[0045] Examples of electrochemical devices including the membrane electrode assembly 10 include solid oxide fuel cells, water electrolysis cells, water vapor electrolysis cells, and electrochemical reactors.
[0046] [Electrolyte membrane] As described above, the electrolyte membrane 11 contains a solid electrolyte having proton conductivity. The solid electrolyte can be represented by any one of the following composition formulas (1) to (3). BaZr 1-x1 M1 x1 O 3-γ (1) BaCe 1-x2 M2 x2 O 3-γ (2) BaZr 1-x3-y3 Ce x3 M3 y3 O 3-γ (3) Here, M1, M2, and M3 are each independently at least one element selected from the group consisting of La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Y, Sc, Mn, Fe, Co, Ni, Al, Ga, In, and Lu. These M1, M2, and M3 may be referred to as dopants. In addition, x1, x2, x3, and y3 each satisfy the following conditions (a) to (d).
[0047] 0 <x1<1 ···(a) 0 <x2<1 ···(b) 0 <x3<1 ···(c) 0 <y3<1 ···(d) 0<γ≦0.5 (e) Among the above solid electrolytes, BaZr 1-x1 M1 x1 O 3-γ The compound of composition formula (1) represented by the following formula (hereinafter, sometimes referred to as "BZM") has high stability against carbon dioxide gas.
[0048] In the composition formulas (1) to (3), γ is a value corresponding to the amount of oxygen vacancies in the composition, and varies depending on the oxidation number of the dopant and the mixing ratios x1, x2, x3, and y3. O from H2O corresponding to the amount of oxygen vacancies γ can be inserted at the oxygen vacancy sites, and γ can be as small as 0. The range of values that γ can take is 0<γ≦0.5.
[0049] In the compositional formulas (1) to (3), as the values of x1, x2, x3, and y3 increase, the performance of the solid electrolyte, that is, the proton conductivity, tends to improve. Also, as the values of x1, x2, x3, and y3 decrease, the crystal structure of the solid electrolyte tends to be stable.
[0050] For example, in the compositional formula (3), the greater the value of x3, the better the performance, but the stability against carbon dioxide gas decreases.
[0051] Regarding the compositional formulas (1) and (2), when x1 and x2 have the same value, generally, the performance of the compositional formula (2) is better. However, the stability against carbon dioxide gas decreases.
[0052] From the perspective of achieving both improved performance of the solid electrolyte (improvement of proton conductivity) and improved structural stability, in the compositional formulas (1) to (3), it is preferable to satisfy 0.05 < x1 < 0.3, 0.05 < x2 < 0.3, and 0.05 < x3 < 0.3 respectively. Preferably, it is more preferable to satisfy 0.1 ≤ x1 ≤ 0.2, 0.1 ≤ x2 ≤ 0.2, and 0.1 ≤ x3 ≤ 0.2 respectively. Even more preferably, it is more preferable to satisfy x1 = 0.2, x2 = 0.2, and x3 = 0.2 respectively. In the compositional formula (1), M1 may be at least one element selected from the group consisting of Y, Tm, Yb, and Lu from the perspective of proton conductivity. From the perspective of proton conductivity and the difficulty of generating impurities when mixed and calcined with a compound containing Ni, in the compositional formula (1), M1 may be at least one element of Lu and Yb. That is, the solid electrolyte represented by the compositional formula (1) is, for example, BaZr where M1 is Yb and x = 0.2 0.8 Yb 0.2 O 3-γ It may also be. When the solid electrolyte is BaZr 0.8 Yb 0.2 O 3-γ a membrane electrode assembly 10 with improved power generation efficiency and durability can be obtained. Also, for the BZM of the compositional formula (1), for example, when the element M is Yb and the molar ratio of Zr to Yb is 8:2, it has a proton conductivity of approximately 0.011 S / cm at 600°C.
[0053] In order to reduce the ohmic resistance (that is, IR resistance) of the electrolyte membrane 11, the electrolyte membrane 11 may be made as thin as possible.
[0054] [Air pole] The air electrode 12 is made of a mixed oxide ion and electronic conductor material. The mixed oxide ion and electronic conductor material is a lanthanum strontium cobalt iron composite oxide (hereinafter sometimes referred to as "LSCF"), and the ratio of the number of moles of Co to the sum of the number of moles of Co and the number of moles of Fe is a value in the range of 0.4 to 0.6. The air electrode 12 may be made of only LSCF, or may be made of a combination of LSCF and another mixed oxide ion and electronic conductor material. Furthermore, for example, the air electrode 12 may contain a material (hereinafter referred to as electrolyte material) that constitutes the solid electrolyte of the electrolyte membrane 11, such as BZM.
[0055] When the air electrode 12 is used as an air electrode of a solid oxide fuel cell, for example, a reaction occurs in which oxygen in the gas phase is electrochemically reduced. For this reason, the air electrode 12 may be a porous body in order to secure a diffusion path for oxygen and promote the reaction. For example, the air electrode 12 may be a porous body having a porosity of 20 to 50 volume % as measured by the Archimedes method or mercury intrusion method.
[0056] LSCF can be expressed by the following composition formula (4). La 1-m Sr m Co n Fe 1-n O 3-δ (4) In composition formula (4), n is a value in the range of 0.4≦n≦0.6. For this reason, for example, in the operating temperature range of a solid oxide fuel cell having proton conductivity (i.e., a temperature range of 600° C. or less) and under highly humidified conditions where the volume fraction of water vapor in the air is about 35%, it is possible to prevent the generation of decomposition products (e.g., oxides of Co) at the air electrode 12 due to reaction with water. In addition, it is possible to reduce the reaction resistance of the electrode reaction at the air electrode 12, thereby improving power generation efficiency.
[0057] In the composition formula (4), m is preferably a value in the range of 0≦m≦0.5, and m is particularly preferably 0.4. In the composition formula (4), δ represents the amount of oxygen vacancy. δ can vary in the range of 0 to 0.5 depending on the molar ratio of Sr (i.e., the value of m), the molar ratio of Co (i.e., the value of n), and the oxidation numbers of Co and Fe.
[0058] The membrane electrode assembly 10 according to the first embodiment, which includes the above-mentioned electrolyte membrane 11 and air electrode 12, has a laminated structure in which the air electrode 12 is disposed on one main surface of the electrolyte membrane 11, as shown in FIG.
[0059] Therefore, the membrane electrode assembly 10 can reduce reaction resistance and improve the reaction efficiency of the electrochemical device. In particular, since the air electrode 12 exhibits high water vapor resistance and low reaction resistance, the membrane electrode assembly 10 can achieve both high reaction efficiency and water vapor resistance.
[0060] Second embodiment A membrane electrode assembly 100 included in an electrochemical device according to a second embodiment of the present disclosure will be described below with reference to Fig. 2. In the description of the second embodiment, differences from the first embodiment will be mainly described, and the same or corresponding components will be denoted by the same reference symbols throughout all the drawings, and descriptions thereof may be omitted.
[0061] FIG. 2 is a cross-sectional view showing a schematic configuration of a membrane electrode assembly 100 included in an electrochemical device according to a second embodiment of the present disclosure. FIG. 2 shows a cross section of the membrane electrode assembly 100 cut in the thickness direction. As shown in FIG. 2, the membrane electrode assembly 100 according to the second embodiment further includes a fuel electrode 13 in addition to the configuration of the membrane electrode assembly 10 according to the first embodiment. That is, in the membrane electrode assembly 10, the air electrode 12 is disposed on one main surface side of the electrolyte membrane 11, and the fuel electrode 13 is disposed on the other main surface side. In other words, in the electrochemical device, the air electrode 12, the electrolyte membrane 11, and the fuel electrode 13 are laminated in this order.
[0062] The membrane electrode assembly 100 according to the second embodiment has the same configuration as the membrane electrode assembly 10 according to the first embodiment, except that it further includes a fuel electrode 13. For this reason, the same members as those in the membrane electrode assembly 10 are denoted by the same reference numerals, and detailed descriptions thereof will be omitted.
[0063] 2, the membrane electrode assembly 100 has a structure in which the electrolyte membrane 11 is laminated on the fuel electrode 13, and the air electrode 12 is laminated on the electrolyte membrane 11, but is not limited to this. For example, another layer made of an ion-conductive material different from that of the electrolyte membrane 11 may be formed between the fuel electrode 13 and the electrolyte membrane 11.
[0064] [Fuel electrode] The fuel electrode 13 is an electrode where electrochemical oxidation occurs, and is, for example, an electrode made of a cermet of Ni and an electrolyte material.
[0065] When the fuel electrode 13 is used as a fuel electrode of a solid oxide fuel cell, for example, a reaction occurs in the fuel electrode 13 to oxidize hydrogen in the gas phase to protons. For this reason, the fuel electrode 13 may be formed as a bond between Ni, which has electronic conductivity and hydrogen oxidation activity, and an electrolyte material having proton conductivity, in order to promote the oxidation reaction from hydrogen to protons. Furthermore, the fuel electrode 13 may be a porous body in order to ensure a diffusion path for gas (e.g., hydrogen). For example, the fuel electrode 13 may be a porous body having a porosity of 20 to 50 volume % as measured by the Archimedes method or mercury intrusion method.
[0066] Furthermore, when the electrochemical device including the membrane electrode assembly 100 is a solid oxide fuel cell, electricity is generated by supplying air to the side of the electrolyte membrane 11 where the air electrode 12 is provided, and supplying a gas containing hydrogen (i.e., fuel) to the side where the fuel electrode 13 is provided. Therefore, when the electrochemical device including the membrane electrode assembly 100 is a solid oxide fuel cell, the electrolyte membrane 11 needs to be gas-tight.
[0067] As described above, the membrane electrode assembly 100 according to the second embodiment has a configuration in which the air electrode 12, the electrolyte membrane 11, and the fuel electrode 13 are laminated in this order. Therefore, like the membrane electrode assembly 10 according to the first embodiment, the membrane electrode assembly 100 according to the second embodiment can reduce reaction resistance and improve the reaction efficiency of the electrochemical device. In particular, since the air electrode 12 exhibits high water vapor resistance and low reaction resistance, the membrane electrode assembly 10 can achieve both high reaction efficiency and water vapor resistance.
[0068] Therefore, when an electrochemical device including the membrane electrode assembly 100 is a solid oxide fuel cell, the solid oxide fuel cell can reduce reaction resistance to improve power generation efficiency and achieve high water vapor resistance stability.
[0069] When the electrochemical device including the membrane electrode assembly 100 is a steam electrolysis cell, the steam electrolysis cell can reduce reaction resistance to improve electrolysis efficiency and achieve high stability against steam.
[0070] When the membrane electrode assembly 100 according to the second embodiment is used in a solid oxide fuel cell, it can be configured as, for example, a fuel cell system as follows: That is, the fuel cell system includes a raw material supply path (not shown) for supplying raw material, a reformer (not shown) for reforming the raw material flowing through the raw material supply path to generate a hydrogen-containing gas, and an air supply path (not shown) for supplying air (i.e., an oxidizing gas).
[0071] In a fuel cell system, a raw material such as a hydrocarbon gas is supplied to a reformer from the outside through a raw material supply path. The reformer reforms the supplied raw material to generate a hydrogen-containing gas. The hydrogen-containing gas generated in the reformer is supplied to the fuel electrode 13 of a solid oxide fuel cell including a membrane electrode assembly 100. Alternatively, the system may be configured not to include a reformer, and the hydrogen-containing gas may be supplied directly to the fuel electrode 13 from the outside through the raw material supply path.
[0072] Meanwhile, an oxidant gas is supplied from the outside through an air supply passage to the air electrode 12 of the solid oxide fuel cell (membrane electrode assembly 100). The solid oxide fuel cell (membrane electrode assembly 100) generates electricity by an electrochemical reaction between hydrogen in the hydrogen-containing gas supplied in this manner and oxygen in the oxidant gas.
[0073] (Example) Examples (Examples 1 and 2) of the present disclosure will be described below. Note that Examples 1 and 2 of the present disclosure are examples of the membrane electrode assembly 10 according to the first embodiment and the membrane electrode assembly 100 according to the second embodiment of the present disclosure, and the configurations of the membrane electrode assembly 10 according to the first embodiment and the membrane electrode assembly 100 according to the second embodiment of the present disclosure are not limited to the configurations of these examples.
[0074] First, an air electrode according to Example 1 represented by composition formula (5), an air electrode according to Example 2 represented by composition formula (6), and an air electrode according to Example 3 represented by composition formula (7) were prepared.
[0075] In each of the air electrodes according to Examples 1, 2, and 3, the ratio of the number of moles of Co to the sum of the number of moles of Co and the number of moles of Fe is in the range of 0.35 or more and 0.6 or less. La 0.6 Sr 0.4 Co 0.35 Fe 0.65 O 3-δ (5) La 0.6 Sr 0.4 Co 0.4 Fe 0.6 O 3-δ (6) La 0.6 Sr 0.4 Co 0.6 Fe 0.4 O 3-δ (7) Furthermore, an air electrode according to Comparative Example 1 represented by the following composition formula (8), an air electrode according to Comparative Example 2 represented by the composition formula (9), an air electrode according to Comparative Example 3 represented by the composition formula (10), and an air electrode according to Comparative Example 4 represented by the composition formula (11) were each prepared. La0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ (8) La 0.6 Sr 0.4 Co 0.3 Fe 0.7 O 3-δ (9) La 0.6 Sr 0.4 Co 0.8 Fe 0.2 O 3-δ (10) La 0.6 Sr 0.4 Chief of Staff 3-δ (11) In each of the air electrodes according to Comparative Example 1 to Comparative Example 4, the ratio of the number of moles of Co to the sum of the number of moles of Co and the number of moles of Fe is smaller than 0.35 or larger than 0.6. In the composition formula described above, δ represents the amount of oxygen vacancy. The value of δ satisfies 0≦δ≦0.5.
[0076] (Method of manufacturing air electrode material) Next, a method for producing LSCF (LSC in Comparative Example 4) which is the air electrode material in Examples 1 to 3 and Comparative Examples 1 to 4 will be described.
[0077] [Production method of the cathode material of Example 1] The cathode material (LSCF) of Example 1 was prepared by the citrate complex method using La(NO3)3·6H2O, Sr(NO3)2, Co(NO3)2·6H2O, and Fe(NO3)3·9H2O (each manufactured by Kanto Chemical) as starting materials.
[0078] Specifically, 23.27g of La(NO3)3·6H2O powder, 7.58g of Sr(NO3)2 powder, 9.12g of Co(NO3)2·6H2O powder, and 23.52g of Fe(NO3)3·9H2O powder were weighed out. Each weighed powder was dissolved in distilled water, and 34.42g of citric acid monohydrate (Kanto Chemical) and 26.17g of ethylenediaminetetraacetic acid (EDTA) (Kanto Chemical) were added. Then, the pH was adjusted to 7 using ammonia water (28wt%) (Kanto Chemical). After the pH adjustment, the solvent was removed at 90℃ on a hot stirrer. Then, it was heated to about 300℃, and finally sintered at 1200℃ in an air atmosphere to obtain LSCF powder.
[0079] [Production method of the air electrode material according to the second embodiment] The cathode material (LSCF) of Example 2 was produced in the same manner as the cathode material of Example 1, except that the amounts of the starting powders and the amounts of citric acid monohydrate and ethylenediaminetetraacetic acid (EDTA) added to the distilled water in which the powders were dissolved were different.
[0080] In the cathode material of Example 2, the amounts of the powders used as starting materials were 23.25 g of La(NO3)3·6H2O powder, 7.58 g of Sr(NO3)2 powder, 10.42 g of Co(NO3)2·6H2O powder, and 21.69 g of Fe(NO3)3·9H2O powder (each manufactured by Kanto Chemical Co., Ltd.), 34.39 g of citric acid monohydrate (manufactured by Kanto Chemical Co., Ltd.), and 26.16 g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical Co., Ltd.).
[0081] [Production method of the air electrode material according to the third embodiment] The cathode material (LSCF) of Example 3 was prepared in the same manner as the cathode material of Example 1, except that the amounts of the starting powders and the amounts of citric acid monohydrate and ethylenediaminetetraacetic acid (EDTA) added to the distilled water in which the powders were dissolved were different.
[0082] In the cathode material of Example 3, the amounts of the powders used as starting materials were 23.19 g of La(NO3)3·6H2O powder, 7.55 g of Sr(NO3)2 powder, 15.58 g of Co(NO3)2·6H2O powder, and 14.42 g of Fe(NO3)3·9H2O powder (each manufactured by Kanto Chemical Co., Ltd.), 34.30 g of citric acid monohydrate (manufactured by Kanto Chemical Co., Ltd.), and 26.08 g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical Co., Ltd.).
[0083] [Production method of air electrode material of Comparative Example 1] The cathode material (LSCF) of Comparative Example 1 was prepared in the same manner as the cathode material of Example 1, except that the amounts of the starting powders and the amounts of citric acid monohydrate and ethylenediaminetetraacetic acid (EDTA) added to the distilled water in which the powders were dissolved were different.
[0084] In the cathode material of Comparative Example 1, the amounts of the powders used as starting materials were 23.32 g of La(NO3)3·6H2O powder, 7.60 g of Sr(NO3)2 powder, 5.22 g of Co(NO3)2·6H2O powder, and 29.00 g of Fe(NO3)3·9H2O powder (each manufactured by Kanto Chemical Co., Ltd.), 34.49 g of citric acid monohydrate (manufactured by Kanto Chemical Co., Ltd.), and 26.19 g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical Co., Ltd.).
[0085] [Production method of air electrode material of Comparative Example 2] The cathode material (LSCF) of Comparative Example 2 was prepared in the same manner as the cathode material of Example 1, except that the amounts of the starting powders and the amounts of citric acid monohydrate and ethylenediaminetetraacetic acid (EDTA) added to the distilled water in which the powders were dissolved were different.
[0086] In the cathode material of Comparative Example 2, the amounts of the powders used as starting materials were 23.28 g of La(NO3)3·6H2O powder, 7.59 g of Sr(NO3)2 powder, 7.82 g of Co(NO3)2·6H2O powder, and 25.34 g of Fe(NO3)3·9H2O powder (each manufactured by Kanto Chemical Co., Ltd.), 34.44 g of citric acid monohydrate (manufactured by Kanto Chemical Co., Ltd.), and 26.19 g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical Co., Ltd.).
[0087] [Production method of air electrode material of Comparative Example 3] The air electrode material (LSCF) of Comparative Example 3 was prepared in the same manner as the air electrode material of Example 1, except that the amounts of the starting powders and the amounts of citric acid monohydrate and ethylenediaminetetraacetic acid (EDTA) added to the distilled water in which the powders were dissolved were different.
[0088] In the cathode material of Comparative Example 3, the amounts of the powders used as starting materials were 23.12 g of La(NO3)3·6H2O powder, 7.53 g of Sr(NO3)2 powder, 20.72 g of Co(NO3)2·6H2O powder, and 7.19 g of Fe(NO3)3·9H2O powder (each manufactured by Kanto Chemical Co., Ltd.), 34.20 g of citric acid monohydrate (manufactured by Kanto Chemical Co., Ltd.), and 26.01 g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical Co., Ltd.).
[0089] [Production method of air electrode material of Comparative Example 4] The cathode material (LSC) of Comparative Example 4 was prepared in the same manner as the cathode material of Example 1, except that the amounts of the starting powders and the amounts of citric acid monohydrate and ethylenediaminetetraacetic acid (EDTA) added to the distilled water in which the powders were dissolved were different.
[0090] In the cathode material of Comparative Example 4, the amounts of the powders used as starting materials were 23.06 g of La(NO3)3·6H2O powder, 7.51 g of Sr(NO3)2 powder, and 25.83 g of Co(NO3)2·6H2O powder (each manufactured by Kanto Chemical Co., Ltd.), 34.11 g of citric acid monohydrate (manufactured by Kanto Chemical Co., Ltd.), and 25.94 g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical Co., Ltd.).
[0091] [Water vapor resistance test of air electrode] A water vapor resistance test was carried out on the LSCFs according to Examples 1 to 3 and the LSCFs according to Comparative Examples 1 to 4 obtained by the above-mentioned production methods as follows.
[0092] First, the powders of the LSCF according to Examples 1 to 3 and the LSCF according to Comparative Examples 1 to 4 obtained by the above-mentioned "Manufacturing method of air electrode material" were filled into a depression (1 mm thick, 1 cm diameter) of a quartz dish. Then, the surface of the LSCF powder was smoothed using a glass squeegee. After that, analysis was performed using the measurement results by X-ray diffraction method at room temperature, and the results were used as a reference before the test (i.e., before the water vapor resistance test). A Rigaku Smart Lab was used to perform the measurement by X-ray diffraction method. The X-rays irradiated to the sample were CuKα characteristic X-rays (wavelength 1.5418 Å).
[0093] Next, powders of the LSCF according to Examples 1 to 3 and the LSCF according to Comparative Examples 1 to 4 were placed in a quartz tube having a gas flow path installed in a tubular furnace. The tubular furnace was heated so that the temperature in the vicinity of the LSCF powder reached 600°C. Thereafter, a humidified gas containing 40% water vapor by volume fraction, obtained by bubbling synthetic air, was circulated through the gas flow path at 160cc / min. Note that the volume fraction of water vapor is determined by the oxygen in the air (volume fraction 21%) being O2+4H + +4e - →The ratio is set to be slightly higher than the water vapor fraction (approximately 35%) when all of the 2H2O reacts to become water vapor.
[0094] After 1000 hours, the LSCF powder was measured by X-ray diffraction at room temperature. In this way, the measurement results after the water vapor resistance test (i.e., the measurement results after the test) were obtained. The measurement results after the test obtained were compared with the standard before the test. If a peak not attributable to LSCF was detected in this comparison, it was determined that decomposition products of LSCF were generated. The presence or absence of decomposition products after 1000 hours for the LSCFs according to Examples 1 to 3 and the LSCFs according to Comparative Examples 1 to 4 is shown in Table 1 below and FIG. 3. FIG. 3 is a graph showing the measurement results by X-ray diffraction for the LSCFs according to Examples 2 and 3 of the present disclosure and the LSCFs according to Comparative Examples 1 to 4.
[0095] [Table 1] No peaks indicating decomposition products other than LSCF were detected when the ratio of the number of moles of cobalt (Co) to the sum of the number of moles of cobalt (Co) and the number of moles of iron (Fe) was 0.2, 0.3, 0.4, or 0.6. On the other hand, when the ratio of the number of moles of cobalt (Co) to the sum of the number of moles of cobalt (Co) and the number of moles of iron (Fe) was 0.8 and 1.0, a peak of cobalt oxide (Co3O4) was detected (see the arrow in Figure 3).
[0096] These results show that alloys with a Co ratio of 0.6 or less to the sum of Co and Fe have high stability against water vapor at 600°C. On the other hand, alloys with a Co ratio of 0.8 or 1.0 to the sum of Co and Fe are unstable against water vapor at 600°C.
[0097] (Method of manufacturing membrane electrode assembly) The membrane electrode assemblies using the LSCFs according to Examples 1 to 3 and Comparative Examples 1 to 4 were manufactured by the following manufacturing method. The membrane electrode assemblies used here were configured such that an air electrode was disposed on one main surface side of an electrolyte membrane, and a fuel electrode was disposed on the other main surface side. The electrolyte membranes of the membrane electrode assemblies using the LSCFs according to Examples 1 to 3 and Comparative Examples 1 to 4 were all made of the same electrolyte material, and a representative composition of the electrolyte material was BaZr 0.8 Yb 0.2 O 2.9 (hereinafter, BZYb). The fuel electrodes of the membrane electrode assemblies using the LSCF according to Examples 1 to 3 and Comparative Examples 1 to 4 were all the same, and were made of a compound using BZYb and NiO.
[0098] [Method of manufacturing electrolyte material] First, a method for producing a BZYb green sheet material, which is an electrolyte material constituting an electrolyte membrane, will be described.
[0099] BZYb was prepared by the citrate complex method using powders of Ba(NO3)2 (Kanto Chemical) and ZrO(NO3)2·2H2O (Kanto Chemical), and powder of Yb(NO3)3·xH2O (Kojundo Chemical) as starting materials.
[0100] (Preparation of electrolyte powder) First, the electrolyte powder is explained. First, BZYb was prepared by dissolving 42.43 g of Ba(NO3)2 powder and 34.71 g of ZrO(NO3)2·2H2O powder in distilled water. In addition, 180 g of Yb(NO3)3·xH2O powder was dissolved in 300 mL of distilled water to obtain Yb. 3+ 187 mL of an aqueous solution with an ion concentration of 0.87 mol / L was added, and the resulting aqueous solution was stirred. 3+ The ion concentration was calculated from the results of inductively coupled plasma atomic emission spectrometry (ICP-AES). The analysis device used was an iCAP7400 Duo manufactured by Thermo Fisher Scientific.
[0101] Next, 1.5 equivalents of citric acid monohydrate (Kanto Chemical) and 1.5 equivalents of ethylenediaminetetraacetic acid (EDTA) (Kanto Chemical) were added to the aqueous solution relative to the metal cations contained in the aqueous solution, and the aqueous solution was then stirred at 90°C.
[0102] Subsequently, the aqueous solution was adjusted to pH 7 using ammonia water (28% (weight ratio)) (Kanto Chemical Co., Ltd.). After the pH adjustment, the solution was heated to 95° C. to 240° C. using a hot stirrer to remove the solvent, and a solid was obtained.
[0103] The obtained solid was crushed in a mortar and then degreased at about 400°C. After degreasing, the obtained powder was press-molded into a cylindrical shape and calcined at 900°C for 10 hours in an air atmosphere. After calcination, the coarsely crushed powder was placed in a plastic container together with zirconia balls, and ethanol was added and crushed in a ball mill for more than 4 days. After crushing in the ball mill, the solvent was removed by lamp drying. This resulted in the production of a powder of the electrolyte material.
[0104] (Preparation of electrolyte powder for green sheets and preparation of green sheets) The above-mentioned operation of "(Preparation of electrolyte powder)" was repeated several times. In this way, about 200 g of electrolyte powder for green sheet was obtained. A green sheet was prepared using the obtained electrolyte material powder. Specifically, this electrolyte material powder was kneaded with polyvinyl butyral as a resin, butyl benzyl phthalate as a plasticizer, and butyl acetate and 1-butanol as a solvent. In this way, a kneaded material was obtained. The obtained kneaded material was processed by a tape casting method. In this way, an electrolyte green sheet was obtained.
[0105] [Method of manufacturing fuel electrode material] Next, a method for producing the fuel electrode material using BZYb and NiO will be described.
[0106] The electrolyte material powder obtained by the above-mentioned "Method for producing electrolyte material" and NiO powder (manufactured by Sumitomo Metal Mining Co., Ltd.) were weighed out so that the weight ratio was NiO:BZYb=80:20 (that is, the volume ratio of Ni to BZYb was 69:31). Then, a green sheet was produced using the weighed electrolyte material powder and NiO powder. Specifically, the electrolyte material powder, NiO powder, polyvinyl butyral as a resin, butyl benzyl phthalate as a plasticizer, and butyl acetate and 1-butanol as a solvent were kneaded together. In this way, a kneaded material was obtained. The kneaded material obtained was processed by a tape casting method. In this way, a green sheet of the fuel electrode was obtained.
[0107] [Method of manufacturing laminate] First, a method for manufacturing a laminate of an anode and an electrolyte membrane will be described. The green sheet of the anode obtained by the above-mentioned "method for manufacturing an anode material" was cut to a predetermined size so that it would become a 20 mm x 20 mm square (with the four corners chamfered at 3 mm) after firing, assuming a linear shrinkage rate of 22%, and multiple sheets were laminated. The green sheet of the anode cut to a predetermined size and laminated was then stacked on top of the green sheet of the electrolyte obtained by the "method for manufacturing an electrolyte material", and a pressure of 50 MPa was applied by hot pressing to obtain a laminate.
[0108] The resulting laminate was sintered at 1475°C for 2 hours, and a half cell measuring 20mm x 20mm square (with 3mm chamfered corners) was fabricated from the laminate of the fuel electrode and electrolyte membrane. The BZYb that constitutes the electrolyte membrane was confirmed to be a single phase by X-ray diffraction. A Rigaku Smart Lab was used for the measurements. The X-rays irradiated to the sample were CuKα characteristic X-rays (wavelength 1.5418 Å).
[0109] Next, a method for forming an air electrode on an electrolyte membrane will be described. The powder of each of the air electrode materials according to Examples 1 to 3 and Comparative Examples 1 to 4 obtained by the above-mentioned "Production method of air electrode material" was mixed with a vehicle of a mixture of alcohol and ether in a predetermined weight ratio, and kneaded in a rotation-revolution mixer to prepare a paste of each of the air electrode materials. The powder of each of the air electrode materials according to Examples 1 to 3 and Comparative Examples 1 to 4 was mixed with the vehicle in a weight ratio of 3:2.
[0110] Each of the pastes of the air electrode material according to Examples 1 to 3 and Comparative Examples 1 to 4 was screen-printed onto the electrolyte membrane of the half-cell to form an air electrode having a diameter of 10 mm. Then, the resulting membrane electrode assemblies were fired at 950°C for 2 hours in an air atmosphere to obtain the membrane electrode assemblies according to Examples 1 to 3 and Comparative Examples 1 to 4. The thicknesses of the electrolyte membrane, air electrode, and fuel electrode of the obtained membrane electrode assemblies according to Examples 1 to 3 and Comparative Examples 1 to 4 were 13 μm, 10 μm, and 0.6 mm, respectively.
[0111] (Measurement of reaction resistance of membrane electrode assembly) Subsequently, the reaction resistance of the membrane / electrode assemblies according to Examples 1 to 3 and Comparative Examples 1 to 4 was measured. The measurement was carried out by AC impedance measurement using a four-terminal method as follows.
[0112] An Ag mesh for current collection was attached using Ag paste to the surfaces of the fuel electrode and the air electrode of each of the membrane electrode assemblies according to Examples 1 to 3 and Comparative Examples 1 to 4. In addition, two Pt wires were attached to each of the fuel electrode side and the air electrode side of the Ag mesh as external output terminals for four-terminal measurement.
[0113] First, the membrane electrode assembly was heated to 700°C, and humidified air containing 3% water vapor was supplied to the air electrode side, and humidified hydrogen containing 3% water vapor was supplied to the fuel electrode side. By holding the two in this state for more than four hours, the NiO in the mixture of NiO and BZYb at the fuel electrode was reduced to Ni.
[0114] Resistance measurements were performed after the reduction operation of the membrane electrode assembly, under conditions where humidified air containing 3% water vapor (volume ratio) was supplied to the air electrode side, and humidified hydrogen containing 3% water vapor to the fuel electrode side at 600°C. AC impedance measurements were performed using a Solartron ModuLab XM, applying an AC voltage with an amplitude of 10 mV and changing the frequency from 100 kHz to 0.01 Hz to the terminal voltage at an external current of 0 A.
[0115] FIG. 4 is a diagram showing an example of the AC impedance measurement result in the embodiment of the present disclosure by a Cole-Cole plot. FIG. 4 shows a schematic breakdown of the resistance components by the AC impedance measurement. As shown in FIG. 4, the AC impedance measurement result can be illustrated by a Cole-Cole plot in which the real component Z' of the impedance Z (=Z'+jZ'') is plotted on the horizontal axis and the imaginary component Z'' is plotted on the vertical axis. In the Cole-Cole plot, for an arc drawn in the frequency range of about 10 kHz to 0.01 Hz, the length of the chord formed by the arc and the real axis (Z'), that is, the length of the two intersections where the arc cuts the real axis, is the reaction resistance. The reaction resistance results obtained by the measurement are shown in Table 1 above.
[0116] The relationship between the molar ratio of Co to the sum of the moles of Co and Fe and the reaction resistance is shown in Figure 5. Figure 5 is a graph showing the relationship between the molar ratio of Co to the sum of the moles of Co and Fe and the reaction resistance for the air electrodes according to Examples 1 to 3 and Comparative Examples 1 to 4 of the present disclosure. In Figure 5, the vertical axis represents the reaction resistance (unit: Ωcm 2 ) and the horizontal axis indicates the ratio of Co to the sum of the moles of Co and Fe in the air electrode.
[0117] As shown in Table 1 and FIG. 5, in the air electrode material (LSCF) in which the molar ratio of Co to the sum of the moles of Co and Fe is 0.35 or more (air electrodes according to Examples 1 and 2 and the air electrode according to Comparative Example 3), the reaction resistance was 1.4 Ωcm 2For this reason, when the membrane electrode assembly is used in a solid oxide fuel cell, the voltage will not fall below 0.7 V, which is set as the minimum voltage that can actually be obtained during the operation of the solid oxide fuel cell.
[0118] On the other hand, for the air electrode material (LSCF) in which the molar ratio of Co to the sum of the moles of Co and Fe was 0.2 and 0.3 (air electrodes according to Comparative Examples 1 and 2), the reaction resistance was 2.1 cm 2 , 1.8cm 2 These tend to be significantly larger than those of the air electrodes according to Examples 1 and 2, respectively, and the reaction resistance was 1.4 Ωcm 2 The value exceeded that.
[0119] From the above results, it was revealed that the reaction resistance of the membrane electrode assembly can be reduced when the molar ratio of Co to the sum of the moles of Co and Fe in the air electrode material (LSCF) is 0.35 or more. Therefore, it was clarified that high power generation efficiency can be achieved when a membrane electrode assembly in which the molar ratio of Co to the sum of the moles of Co and Fe in the air electrode material (LSCF) is 0.35 or more is used in a solid oxide fuel cell.
[0120] Regarding the above-mentioned water vapor resistance stability, as shown in Table 1, it was confirmed that a membrane electrode assembly in which the molar ratio of Co to the sum of the moles of Co and Fe in the air electrode material (LSCF) is 0.6 or less has high water vapor resistance stability.
[0121] From the above, it was found that a membrane electrode assembly in which the molar ratio of Co to the sum of the moles of Co and Fe in the air electrode material (LSCF) is 0.35 or more and 0.6 or less can achieve both high reaction efficiency and high water vapor resistance. [Industrial Applicability]
[0122] The membrane electrode assembly according to the present disclosure can be used in electrochemical devices such as solid oxide fuel cells, water electrolysis cells, and steam electrolysis cells. [Explanation of symbols]
[0123] 10 Membrane electrode assembly 11 Electrolyte membrane 12 Air electrode 13 Fuel electrode 100 Membrane electrode assembly
Claims
1. an electrolyte membrane containing an oxide having proton conductivity; A membrane electrode assembly comprising: an electrode provided on the electrolyte membrane and containing a lanthanum strontium cobalt iron composite oxide, the lanthanum strontium cobalt iron composite oxide being represented by the following composition formula: La 1-m Sr m Con Fe 1-n O 3- δ (0.35≦n≦0.6, 0≦m≦0.5, 0≦δ≦0.5)
2. The electrolyte membrane and the electrodes are arranged in contact with each other. The membrane electrode assembly according to claim 1 .
3. The electrolyte membrane is BaZr 1-x1 M1 x1 O 3-γ , BaCe 1-x2 M2 x2 O 3-γ , and BaZr 1-x3-y3 C.E. x3 M3 y3 O 3-γ At least one compound selected from the group consisting of M1, M2, and M3 are each independently at least one element selected from the group consisting of La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Y, Sc, Mn, Fe, Co, Ni, Al, Ga, In, and Lu; x1 satisfies 0<x1<1, x2 satisfies 0<x2<1, x3 satisfies 0<x3<1, y3 satisfies 0<y3<1, and γ satisfies 0<γ≦0.5 The membrane electrode assembly according to claim 1 or 2.
4. The electrolyte membrane is BaZr 1-x1 Yb x1 O 3-γ The membrane electrode assembly according to claim 3 , wherein the compound is represented by the formula:
5. The electrode is an air electrode. The membrane electrode assembly according to claim 1 .
6. The membrane electrode assembly according to any one of claims 1 to 5, Solid oxide fuel cell.
7. The membrane electrode assembly according to any one of claims 1 to 5, Electrochemical devices.
Citation Information
Patent Citations
Electrode forming method
JP1989014872A
Ceramic powder, its sintered compact and air electrode for solid oxide type fuel cell using the same
JP2009035447A
Fuel cell
JP2015149245A
Fuel cell system