Positive electrode active material for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and method for producing positive electrode active material for non-aqueous electrolyte secondary battery
By optimizing the Ni and Nb content and distribution in the positive electrode active material, the reaction resistance of lithium transition metal compounds is reduced, enhancing the performance of non-aqueous electrolyte secondary batteries.
Patent Information
- Application Number
- JP2021528250
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-28
- Filing Date
- 2020-06-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-06-16
AI Technical Summary
Existing lithium transition metal compounds with a Ni ratio of 80 mol% or more and a Co ratio of 10 mol% or less exhibit high reaction resistance due to the formation of a NiO layer and electrolyte decomposition, which is not addressed by existing technologies.
A positive electrode active material with a Ni content of 80 mol% to 94 mol% and a controlled Nb content of 0.1 mol% to 0.6 mol%, distributed such that the ratio n1/(n1+n2) falls within 50% to 75%, is used, along with a specific manufacturing process involving mixing and sintering to optimize the distribution state of Nb.
The solution reduces reaction resistance and maintains high battery capacity by suppressing the formation of a NiO layer and electrolyte decomposition, resulting in a non-aqueous electrolyte secondary battery with improved performance.
Smart Images

Figure 0007584063000005 
Figure 0007584063000001 
Figure 0007584063000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a positive electrode active material for a non-aqueous electrolyte secondary battery, a non-aqueous electrolyte secondary battery, and a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery. [Background technology]
[0002] In recent years, non-aqueous electrolyte secondary batteries that include a positive electrode, a negative electrode, and a non-aqueous electrolyte and transfer lithium ions or the like between the positive electrode and the negative electrode to charge and discharge have been widely used as high-output, high-energy-density secondary batteries. From the viewpoints of lowering the resistance, increasing the capacity, and increasing the reliability of the battery, there is a demand for improving the characteristics of a positive electrode active material contained in the positive electrode of the battery.
[0003] For example, Patent Document 1 discloses a positive electrode active material for non-aqueous electrolyte secondary batteries that is a lithium nickel manganese composite oxide containing 2 mol % to 8 mol % of Nb, has a lithium niobium compound on the surfaces of the primary particles, and has a portion of Nb dissolved in the primary particles, thereby achieving high capacity and improved cycle characteristics and thermal stability. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2018 / 123951 Summary of the Invention
[0005] Incidentally, in the lithium transition metal compound contained in the positive electrode active material, it is possible to design it so that the Ni content is high to obtain a high battery capacity, while the Co content is low to reduce the manufacturing cost. However, in a lithium transition metal compound in which the Ni ratio is 80 mol % or more and the Co ratio is 10 mol % or less with respect to the total number of moles of metal elements excluding Li, the reaction resistance of the battery may become large. The technology of Patent Document 1 does not take into consideration the reaction resistance of the battery, and there is still room for improvement.
[0006] Therefore, an object of the present disclosure is to provide a positive electrode active material containing a lithium transition metal compound in which the ratio of Ni is 80 mol % or more and the ratio of Co is 10 mol % or less relative to the total number of moles of metal elements excluding Li, thereby reducing the reaction resistance of the battery.
[0007] A positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a lithium transition metal compound that contains Ni at a ratio of 80 mol % or more and 94 mol % or less with respect to the total number of moles of metal elements excluding Li, and Nb at a ratio of 0.1 mol % or more and 0.6 mol % or less with respect to the total number of moles of metal elements excluding Li, and a first sample solution in which 0.2 g of the lithium transition metal compound is added to an aqueous hydrochloric acid solution of 5 mL of pure water / 5 mL of 35% hydrochloric acid is dissolved under bumping for 120 minutes, and the first sample solution is filtered and collected. The method is characterized in that the amount of Nb n1 determined by inductively coupled plasma atomic emission spectrometry in the first filtrate obtained by filtering the first sample solution and immersing the filter used for filtering the first sample solution in 5 mL of 46% hydrofluoric acid / 5 mL of 63% nitric acid / hydrofluoric nitric acid to dissolve the second sample solution under bumping for 180 minutes, and then filtering the second sample solution to obtain a second filtrate, satisfies the condition of 50%≦n1 / (n1+n2)<75%, in terms of molar amount.
[0008] A nonaqueous electrolyte secondary battery according to one aspect of the present disclosure is characterized by including a positive electrode containing the above-described positive electrode active material, a negative electrode, and a nonaqueous electrolyte.
[0009] A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a mixing step of mixing a composite oxide containing at least Ni, a Li compound, and a Nb compound to obtain a mixture, and a firing step of firing the mixture in an oxygen atmosphere at a heating rate of 450° C. or more and 680° C. or less in a range of more than 3.5° C. / min to 5.5° C. / min and at a maximum temperature of 700° C. or more and 780° C. or less, and is characterized in that the holding time at the maximum temperature is 1 hour or more and 10 hours or less.
[0010] According to the positive electrode active material for a nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure, a nonaqueous electrolyte secondary battery having low reaction resistance can be provided. [Brief description of the drawings]
[0011] [Figure 1] 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The layered structure of the lithium transition metal compound includes a transition metal layer such as Ni, a Li layer, and an oxygen layer, and the Li ions present in the Li layer reversibly enter and exit the Li layer, which allows the charge and discharge reaction of the battery to proceed. In the lithium transition metal compound contained in the positive electrode active material, if the ratio of Ni to the total number of moles of metal elements excluding Li is 80 mol % or more and the ratio of Co is 10 mol % or less, the formation of a NiO layer on the surfaces of the primary and secondary particles of the lithium transition metal compound and the decomposition of the electrolyte are promoted, which may increase the reaction resistance of the battery.
[0013] As a result of intensive research, the inventors have found that the reaction resistance of a battery can be reduced by suppressing the Nb content to 0.6 mol% or less and adjusting the distribution state of Nb. It is presumed that the interface resistance can be reduced by having a predetermined amount of Nb compound present on the surfaces of the primary particles and secondary particles of the lithium ion transition metal compound, thereby reducing the reaction resistance of the battery.
[0014] An example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail below. A cylindrical battery in which a wound electrode body is housed in a cylindrical battery case will be exemplified below, but the electrode body is not limited to the wound type, and may be a laminate type in which a plurality of positive electrodes and a plurality of negative electrodes are alternately laminated one by one with a separator interposed therebetween. In addition, the battery case is not limited to a cylindrical shape, and may be, for example, a square shape, a coin shape, or the like, or may be a battery case made of a laminate sheet including a metal layer and a resin layer.
[0015] Fig. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery 10 according to an embodiment. As illustrated in Fig. 1, the nonaqueous electrolyte secondary battery 10 includes an electrode assembly 14, a nonaqueous electrolyte (not shown), and a battery case 15 that accommodates the electrode assembly 14 and the nonaqueous electrolyte. The electrode assembly 14 has a wound structure in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween. The battery case 15 includes a cylindrical outer can 16 with a bottom, and a sealing body 17 that closes the opening of the outer can 16.
[0016] The electrode body 14 is composed of a long positive electrode 11, a long negative electrode 12, two long separators 13, a positive electrode tab 20 joined to the positive electrode 11, and a negative electrode tab 21 joined to the negative electrode 12. The negative electrode 12 is formed to have a size slightly larger than the positive electrode 11 in order to prevent lithium deposition. That is, the negative electrode 12 is formed to be longer in the longitudinal direction and width direction (short direction) than the positive electrode 11. The two separators 13 are formed to have a size at least slightly larger than the positive electrode 11, and are arranged to sandwich the positive electrode 11, for example.
[0017] The nonaqueous electrolyte secondary battery 10 includes insulating plates 18, 19 disposed above and below the electrode body 14. In the example shown in Fig. 1, a positive electrode tab 20 attached to the positive electrode 11 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and a negative electrode tab 21 attached to the negative electrode 12 passes outside the insulating plate 19 and extends toward the bottom side of the outer can 16. The positive electrode tab 20 is connected to the lower surface of a bottom plate 23 of the sealing body 17 by welding or the like, and a cap 27 of the sealing body 17 electrically connected to the bottom plate 23 serves as a positive electrode terminal. The negative electrode tab 21 is connected to the inner bottom surface of the outer can 16 by welding or the like, and the outer can 16 serves as a negative electrode terminal.
[0018] The exterior can 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the exterior can 16 and the sealing body 17, and the internal space of the battery case 15 is sealed. The exterior can 16 has a grooved portion 22 that supports the sealing body 17 and is formed, for example, by pressing the side portion from the outside. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior can 16, and supports the sealing body 17 on its upper surface.
[0019] The sealing body 17 has a structure in which a bottom plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are laminated in this order from the electrode body 14 side. Each member constituting the sealing body 17 has, for example, a disk shape or a ring shape, and each member except the insulating member 25 is electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks so as to push the upper valve body 26 toward the cap 27, and the current path between the lower valve body 24 and the upper valve body 26 is interrupted. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0020] The positive electrode 11, negative electrode 12, separator 13 and nonaqueous electrolyte that constitute the nonaqueous electrolyte secondary battery 10 will be described in detail below, in particular the positive electrode active material contained in the positive electrode active material layer 31 that constitutes the positive electrode 11.
[0021] [Positive electrode] The positive electrode 11 has a positive electrode collector 30 and a positive electrode active material layer 31 formed on both sides of the positive electrode collector 30. For the positive electrode collector 30, a foil of a metal, such as aluminum or an aluminum alloy, that is stable in the potential range of the positive electrode 11, or a film having the metal disposed on the surface layer, can be used. The positive electrode active material layer 31 includes a positive electrode active material, a conductive material, and a binder. The thickness of the positive electrode active material layer 31 is, for example, 10 μm or more and 150 μm or less on one side of the positive electrode collector 30. The positive electrode 11 can be produced by applying a positive electrode slurry containing a positive electrode active material, a conductive material, a binder, and the like to the surface of the positive electrode collector 30, drying the coating, and then compressing it to form the positive electrode active material layer 31 on both sides of the positive electrode collector 30.
[0022] Examples of the conductive material contained in the positive electrode active material layer 31 include carbon materials such as carbon black, acetylene black, ketjen black, and graphite. Examples of the binder contained in the positive electrode active material layer 31 include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, and polyolefin. These resins may be used in combination with carboxymethylcellulose (CMC) or a salt thereof, polyethylene oxide (PEO), and the like.
[0023] The positive electrode active material includes a lithium transition metal compound containing 80 mol% to 94 mol% of Ni relative to the total number of moles of metal elements excluding Li, and 0.1 mol% to 0.6 mol% of Nb relative to the total number of moles of metal elements excluding Li. The lithium transition metal compound has a layered structure, and the layered structure includes a transition metal layer such as Ni, a Li layer, and an oxygen layer. Examples of the layered structure of the lithium transition metal compound include a layered structure belonging to the space group R-3m and a layered structure belonging to the space group C2 / m. Among these, a layered structure belonging to the space group R-3m is preferable in terms of high capacity and stability of the crystal structure.
[0024] Lithium transition metal compounds have the general formula Li a Ni x Co y M z Nb α O2 (0.95≦a≦1.10, 0.80≦x≦0.94, 0≦y≦0.02, 0.04≦z≦0.20, 0.001≦α≦0.006, x+y+z+α=1, M includes at least one element selected from Al, W, Mg, Ti, Mn, and Mo).
[0025] The ratio of Li to the total mole number of metal elements other than Li in the lithium transition metal compound satisfies 0.95≦a≦1.10, more preferably satisfies 0.95≦a≦1.05, and particularly preferably satisfies 0.97≦a≦1.03. When a is less than 0.95, the battery capacity may decrease compared to when a satisfies the above range. When a is 1.10 or more, compared to when a satisfies the above range, more Li compound is added, which may not be economical from the viewpoint of production cost.
[0026] x, which indicates the ratio of Ni to the total mole number of metal elements other than Li and Nb in the lithium transition metal compound, satisfies 0.80≦x≦0.94 in order to increase the capacity of the battery and to add other metal elements.
[0027] The ratio y of Co to the total number of moles of metal elements other than Li in the lithium transition metal compound satisfies 0≦y≦0.02. Co is an optional component. In addition, since Co is expensive, from the viewpoint of reducing the production cost, y≦0.02 is satisfied.
[0028] The ratio z of M (including at least one element selected from Al, Mn, Ti, Mo, W, and Mg) to the total mole number of metal elements other than Li in the lithium transition metal compound satisfies 0.04≦z≦0.20. M can be Al and Mn.
[0029] The ratio α of Nb to the total moles of metal elements other than Li in the lithium transition metal compound satisfies 0.001≦α≦0.006, and more preferably satisfies 0.001≦α≦0.003. Nb is an essential component. When α<0.001, it is difficult to obtain the effect of reducing the reaction resistance of the battery. On the other hand, when Nb>0.006, the initial battery capacity is low.
[0030] In addition, the reaction resistance of the battery can be reduced depending on the distribution state of Nb contained in the lithium transition metal compound. Specifically, the reaction resistance of the battery can be reduced by the presence of Nb compounds on the primary particle surface and the secondary particle surface of the lithium transition metal compound such that the index n1 / (n1+n2) calculated as follows satisfies the condition 50%≦n1 / (n1+n2)<75%. (1) 0.2 g of a lithium transition metal compound is added to an aqueous hydrochloric acid solution of 5 mL of pure water / 5 mL of 35% hydrochloric acid to prepare a first sample solution, which is dissolved under bumping for 120 minutes, and then the first sample solution is filtered. (2) The first sample solution is filtered, and the amount of Nb in the first filtrate, n1, is quantified by inductively coupled plasma atomic emission spectrometry. (3) The filter used to filter the first sample solution is immersed in 5 mL of 46% hydrofluoric acid / 5 mL of 63% nitric acid / hydrofluoric / nitric acid to dissolve the second sample solution under bumping for 180 minutes, and then the second sample solution is filtered. (4) The second sample solution is filtered, and the amount of Nb in the collected second filtrate, n2, is quantified by inductively coupled plasma atomic emission spectrometry. (5) From the n1 and n2 quantified above, calculate n1 / (n1+n2) in molar terms.
[0031] It is believed that n1 represents the amount of Nb contained in the crystal lattice of the lithium transition metal compound, particularly in the Li layer. It is also believed that n2 represents the amount of Nb present on the primary particle surface and secondary particle surface of the lithium transition metal compound. Therefore, n1 / (n1+n2) is an index that represents the approximate proportion of Nb contained in the crystal lattice of the lithium transition metal compound. It is presumed that the presence of Nb compounds on the primary particle surface and secondary particle surface of the lithium transition metal compound to an extent that satisfies the condition 50%≦n1 / (n1+n2)<75% can suppress the reaction resistance of the battery from increasing.
[0032] The content of elements constituting the lithium transition metal compound can be measured by an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), etc. For example, the content of Nb can be quantified by dissolving a sample solution of 0.2 g of the lithium transition metal compound in 5 mL of 46% hydrofluoric acid / 5 mL of 63% nitric acid under bumping for 180 minutes, filtering the sample solution, and subjecting the collected filtrate to inductively coupled plasma atomic emission spectroscopic analysis.
[0033] The content of the lithium transition metal compound in the positive electrode active material is preferably 90 mass% or more, and more preferably 99 mass% or more, relative to the total mass of the positive electrode active material, from the standpoint of, for example, improving the battery capacity and effectively suppressing deterioration of the charge-discharge cycle characteristics.
[0034] The positive electrode active material of the present embodiment may contain other lithium transition metal compounds in addition to the lithium transition metal compound of the present embodiment, such as lithium transition metal compounds having a Ni content of 0 mol % or more and less than 80 mol %.
[0035] Next, an example of a method for producing a lithium transition metal compound will be described.
[0036] The method for producing a lithium transition metal compound includes a mixing step of mixing a composite oxide containing at least Ni, a Li compound, and a Nb compound to obtain a mixture, and a firing step of firing the mixture in an oxygen atmosphere by heating a firing furnace at a temperature rise rate of more than 3.5°C / min to 5.5°C / min at 450°C or higher and 680°C or lower, and at a maximum temperature of 700°C or higher and 780°C or lower, the maximum temperature being held for 1 hour or higher and 10 hours or lower.
[0037] The composite oxide containing at least Ni may be any composite oxide in which the proportion of Ni in the composite oxide is 80 mol % or more and 94 mol % or less. x Co y M zIt is preferable to use a composite oxide represented by O2 (0.80≦x≦0.94, 0≦y≦0.02, 0.04≦z≦0.20, x+y+z=1, M includes at least one element selected from Al, W, Mg, Ti, Mn, and Mo). The method for producing the composite oxide is not particularly limited, but for example, an alkaline solution such as sodium hydroxide is dropped while stirring a solution of a metal salt containing Ni and other metal elements (Co, Al, Mn, etc.), and the pH is adjusted to the alkaline side (for example, 8.5 to 12.5), thereby precipitating (co-precipitating) a composite hydroxide containing Ni and other metal elements, and the composite hydroxide is calcined to obtain a composite oxide containing Ni and other metal elements. The calcination temperature is not particularly limited, but is, for example, in the range of 500°C to 600°C.
[0038] The mixing ratio of the composite oxide, the Li compound, and the Nb compound in the mixing step may be appropriately determined so that the respective elements in the Li transition metal oxide finally obtained are in the desired ratio. The molar ratio of Li to metal elements other than Li and Nb is 0.95 mol% or more and 1.10 mol% or less, more preferably 0.95 mol% or more and 1.05 mol% or less, and particularly preferably 0.97 mol% or more and 1.03 mol% or less. The molar ratio of Nb to metal elements other than Li and Nb is 0.001 mol% or more and 0.006 mol% or less, more preferably 0.0025 mol% or more and 0.005 mol% or less. Examples of Li compounds include Li2CO3, LiOH, Li2O3, Li2O, LiNO3, LiNO2, Li2SO4, LiOH·H2O, LiH, LiF, etc. Examples of Nb compounds include Nb2O5, Nb2O5·nH2O, LiNbO3, and NbCl5, with Nb2O5 being particularly preferred. In the mixing step, when mixing the composite oxide, Li compound, and Nb compound, other metal raw materials may be added as necessary. The other metal raw materials are oxides containing metal elements other than the metal elements constituting the composite oxide, Li, and Nb.
[0039] In the calcination step, the mixture obtained in the mixing step is calcined under an oxygen atmosphere to obtain the lithium transition metal compound according to the present embodiment. In the calcination step, the heating rate from 450°C to 680°C is in the range of more than 3.5°C / min to 5.5°C / min, and the maximum temperature is in the range of 700°C to 780°C. The heating rate from over 680°C to the maximum temperature is, for example, 0.5 to 2°C / min. The holding time of the maximum temperature is 1 hour to 10 hours. The calcination step is performed, for example, in a calcination furnace, and the maximum pressure applied in the calcination furnace during the calcination is preferably in the range of more than 0.55 kPa to 1.0 kPa in addition to the pressure outside the calcination furnace. In addition, the calcination step is preferably, for example, a two-stage calcination in terms of facilitating the adjustment of the distribution state of Nb. The calcination temperature in the first stage is preferably, for example, in the range of 450°C to 680°C. The second-stage firing temperature is preferably, for example, in the range of 700° C. to 780° C. The Nb distribution state of the finally obtained lithium transition metal compound is adjusted by controlling the heating rate, the maximum temperature reached, the maximum pressure in the firing furnace, and the like in the firing step.
[0040] [Negative electrode] The negative electrode 12 has a negative electrode current collector 40 and a negative electrode active material layer 41 formed on both sides of the negative electrode current collector 40. For the negative electrode current collector 40, a foil of a metal stable in the potential range of the negative electrode 12, such as copper or a copper alloy, or a film having the metal disposed on the surface layer can be used. The negative electrode active material layer 41 includes a negative electrode active material and a binder. The thickness of the negative electrode active material layer 41 is, for example, 10 μm or more and 150 μm or less on one side of the negative electrode current collector 40. The negative electrode 12 can be produced by applying a negative electrode slurry containing a negative electrode active material, a binder, and the like to the surface of the negative electrode current collector 40, drying the coating, and then rolling the coating to form the negative electrode active material layer 41 on both sides of the negative electrode current collector 40.
[0041] The negative electrode active material contained in the negative electrode active material layer 41 is not particularly limited as long as it can reversibly occlude and release lithium ions. Generally, carbon materials such as graphite are used. The graphite may be any of natural graphite such as flake graphite, massive graphite, and earthy graphite, artificial massive graphite, and artificial graphite such as graphitized mesophase carbon microbeads. Further, as the negative electrode active material, metals that alloy with Li such as Si and Sn, metal compounds containing Si, Sn, etc., lithium titanium composite oxides, etc. may be used. Further, those provided with a carbon coating may be used. For example, SiO x (0.5 ≦ x ≦ 1.6), or Li 2y SiO (2+y) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0 < y < 2), etc. may be used in combination with graphite.
[0042] As the binder contained in the negative electrode active material layer 41, similar to the case of the positive electrode 11, fluorine-containing resins such as PTFE and PVdF, PAN, polyimide, acrylic resin, polyolefin, etc. may be used, but preferably styrene-butadiene rubber (SBR) is used. Further, the negative electrode active material layer 41 may contain CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc.
[0043] [Separator] For the separator 13, for example, a porous sheet having ion permeability and insulation is used. Specific examples of the porous sheet include microporous thin films, woven fabrics, non-woven fabrics, etc. As the material of the separator, polyolefins such as polyethylene and polypropylene, cellulose, etc. are suitable. The separator 13 may have a single-layer structure or a laminated structure. Further, a resin layer with high heat resistance such as an aramid resin or a filler layer containing an inorganic compound filler may be provided on the surface of the separator 13.
[0044] [Non-aqueous electrolyte] The non-aqueous electrolyte includes, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. For example, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these can be used as the non-aqueous solvent. The non-aqueous solvent may contain a halogen-substituted product in which at least a part of the hydrogen of these solvents is substituted with a halogen atom such as fluorine. Examples of the halogen-substituted product include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylates such as methyl fluoropropionate (FMP).
[0045] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylates such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylates such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).
[0046] Examples of the above ethers include cyclic ethers such as 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, crown ether, etc., and chain ethers such as 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, etc.
[0047] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1 < x < 6, n is 1 or 2), LiB 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborane, lithium lower aliphatic carboxylate, borate salts such as Li2B4O7, Li(B(C2O4)F2), etc., LiN(SO2CF3)2, LiN(C1F 2l+1 SO2)(C m F 2m+1Examples of the lithium salt include imide salts such as LiPF6, LiPF2, and the like (wherein l and m are integers of 0 or more). The lithium salt may be used alone or in combination of two or more. Among these, LiPF6 is preferably used from the viewpoints of ion conductivity, electrochemical stability, and the like. The concentration of the lithium salt is, for example, 0.8 mol to 1.8 mol per 1 L of the non-aqueous solvent. Furthermore, vinylene carbonate or a propane sultone-based additive may be added. EXAMPLES
[0048] The present disclosure will be further described below with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0049] [Preparation of positive electrode active material] <Example 1-1> [Ni 0.90 Co 0.01 Al 0.05 Mn 0.04 The composite hydroxide represented by the formula ](OH)2 was calcined at 500°C for 2 hours to obtain the composite oxide (Ni 0.90 Co 0.01 Al 0.05 Mn 0.04 O2) was obtained. LiOH, the above composite oxide, and Nb2O5 were mixed so that the molar ratio of Li to the total amount of Ni, Co, Al, Mn, and Nb was 1.01:1 to obtain a mixture. The molar ratio of Nb to the total molar amount of metals other than Li was 0.0025. The mixture was heated to 680°C at a heating rate of 3.8°C / min in a temperature range of 450°C to 680°C inclusive, and then heated at a heating rate of 1°C / min and baked at a maximum temperature of 720°C for 5 hours, and then washed with water to remove impurities, thereby obtaining a lithium transition metal compound. The composition of the lithium transition metal compound obtained above was measured using an inductively coupled plasma emission spectrometer (manufactured by Seiko Instruments Inc., product name "SPS3100"), and the composition was found to be LiNi 0.90 Co 0.01 Al 0.05 Mn 0.04 Nb 0.0025 This was used as the positive electrode active material of Example 1-1.
[0050] <Example 1-2> A lithium transition metal compound was obtained in the same manner as in Example 1-1, except that the heating rate in the temperature range of 450° C. to 680° C. was changed to 5.5° C. / min. This was used as the positive electrode active material of Example 1-2.
[0051] <Example 1-3> A lithium transition metal compound was obtained in the same manner as in Example 1-1, except that Nb2O5 was mixed so that the molar ratio of Nb was 0.00125 relative to the total molar ratio of metals excluding Li. The composition of the obtained lithium transition metal compound was LiNi 0.90 Co 0.01 Al 0.05 Mn 0.04 Nb 0.00125 This was used as the positive electrode active material of Example 1-3.
[0052] <Comparative Example 1-1> A lithium transition metal compound was obtained in the same manner as in Example 1-1, except that the heating rate in the temperature range of 450° C. to 680° C. was changed to 3.2° C. / min. The composition of the obtained lithium transition metal compound was LiNi 0.90 Co 0.01 Al 0.05 Mn 0.04 Nb 0.0025 This was used as the positive electrode active material of Comparative Example 1-1.
[0053] <Comparative Example 1-2> A lithium transition metal compound was obtained in the same manner as in Example 1-1, except that the heating rate in the temperature range of 450° C. to 680° C. was changed to 1.2° C. / min. This was used as the positive electrode active material of Comparative Example 1-2.
[0054] <Comparative Example 1-3> A lithium transition metal compound was obtained in the same manner as in Example 1-1, except that Nb2O5 was mixed so that the molar ratio of Nb was 0.00125 relative to the total molar ratio of metals excluding Li, and the heating rate in the temperature range of 450°C to 680°C was changed to 1.2°C / min. The composition of the obtained lithium transition metal compound was LiNi0.90 Co 0.01 Al 0.05 Mn 0.04 Nb 0.00125 This was used as the positive electrode active material of Comparative Example 1-3.
[0055] <Comparative Example 1-4> A lithium transition metal compound was obtained in the same manner as in Example 1-1, except that a mixture was obtained without mixing Nb2O5. The composition of the obtained lithium transition metal compound was LiNi 0.90 Co 0.01 Al 0.05 Mn 0.04 This was used as the positive electrode active material of Comparative Example 1-4.
[0056] <Comparative Example 1-5> A lithium transition metal compound was obtained in the same manner as in Example 1-1, except that Nb2O5 was mixed so that the molar ratio of Nb was 0.00025 relative to the total molar ratio of metals excluding Li. The composition of the obtained lithium transition metal compound was LiNi 0.90 Co 0.01 Al 0.05 Mn 0.04 Nb 0.00025 This was used as the positive electrode active material of Comparative Example 1-5.
[0057] <Comparative Example 1-6> A lithium transition metal compound was obtained in the same manner as in Example 1-1, except that Nb2O5 was mixed so that the molar ratio of Nb was 0.0100 relative to the total molar ratio of metals excluding Li. The composition of the obtained lithium transition metal compound was LiNi 0.90 Co 0.01 Al 0.05 Mn 0.04 Nb 0.0098 This was used as the positive electrode active material of Comparative Example 1-6.
[0058] <Comparative Example 1-7> A lithium transition metal compound was obtained in the same manner as in Example 1, except that the heating rate in the temperature range of 450° C. or more and 680° C. or less was changed to 6.0° C. / min. This was used as the positive electrode active material of Comparative Example 7.
[0059] <Example 2> [Ni 0.85 Al 0.05 Mn 0.10 The composite hydroxide represented by the formula ](OH)2 was calcined at 500°C for 2 hours to obtain the composite oxide (Ni 0.85 Al 0.05 Mn 0.10 O2) was obtained. LiOH, the above composite oxide, and Nb2O5 were mixed so that the molar ratio of Li to Ni, Al, Mn, and Nb was 1.01:1 to obtain a mixture. The molar ratio of Nb to the total moles of metals excluding Li was 0.0025. The mixture was heated to 680°C at a heating rate of 3.8°C / min in a temperature range of 450°C to 680°C inclusive, and then heated at a heating rate of 1°C / min and baked at a maximum temperature of 750°C for 5 hours, and then washed with water to remove impurities, thereby obtaining a lithium transition metal compound. The composition of the lithium transition metal compound obtained above was measured using an inductively coupled plasma emission spectrometer (manufactured by Seiko Instruments Inc., product name "SPS3100"), and the composition was found to be LiNi 0.85 Al 0.05 Mn 0.10 Nb 0.0025 This was used as the positive electrode active material of Example 2.
[0060] <Comparative Example 2> A lithium transition metal compound was obtained in the same manner as in Example 2, except that the heating rate in the temperature range of 450° C. to 680° C. was changed to 1.2° C. / min. The composition of the obtained lithium transition metal compound was LiNi 0.85 Al 0.05 Mn 0.10 Nb 0.0025 This was used as the positive electrode active material of Comparative Example 2.
[0061] <Example 3> [Ni 0.93 Al 0.04 Mn 0.03 The composite hydroxide represented by the formula ](OH)2 was calcined at 500°C for 2 hours to obtain the composite oxide (Ni 0.93 Al 0.04 Mn0.03 O2) was obtained. LiOH, the above composite oxide, and Nb2O5 were mixed so that the molar ratio of Li to the total amount of Ni, Al, Mn, and Nb was 1.01:1 to obtain a mixture. The molar ratio of Nb to the total molar amount of metals other than Li was 0.0025. The mixture was heated to 680°C at a heating rate of 3.8°C / min in a temperature range of 450°C to 680°C inclusive, and then heated at a heating rate of 1°C / min and baked at a maximum temperature of 710°C for 5 hours, and then washed with water to remove impurities, thereby obtaining a lithium transition metal compound. The composition of the lithium transition metal compound obtained above was measured using an inductively coupled plasma emission spectrometer (manufactured by Seiko Instruments Inc., product name "SPS3100"), and the composition was found to be LiNi 0.93 Al 0.04 Mn 0.03 Nb 0.0025 This was used as the positive electrode active material of Example 3.
[0062] <Comparative Example 3> A lithium transition metal compound was obtained in the same manner as in Example 3, except that the heating rate in the temperature range of 450° C. to 680° C. was changed to 1.2° C. / min. The composition of the obtained lithium transition metal compound was LiNi 0.93 Al 0.04 Mn 0.03 Nb 0.0025 This was used as the positive electrode active material of Comparative Example 3.
[0063] The value of the index n1 / (n1+n2), which indicates the distribution state of Nb, was calculated for the lithium transition metal compounds (positive electrode active materials) of the examples and comparative examples under the conditions described above. Table 1 shows the values of n1, n2, and n1 / (n1+n2)×100(%).
[0064] [Table 1]
[0065] Test cells were prepared as follows using the lithium transition metal compounds (positive electrode active materials) of the Examples and Comparative Examples.
[0066] [Preparation of positive electrode] A positive electrode slurry was prepared by mixing 91 parts by mass of the positive electrode active material of Example 1, 7 parts by mass of acetylene black as a conductive material, and 2 parts by mass of polyvinylidene fluoride as a binder, and mixing this with N-methyl-2-pyrrolidone (NMP). Next, the slurry was applied to both sides of a positive electrode current collector made of aluminum foil with a thickness of 15 μm, and after drying the coating, the coating was rolled with a rolling roller to prepare a positive electrode in which a positive electrode active material layer was formed on both sides of the positive electrode current collector. The packing density of the positive electrode active material layer was 3.55 g / cm 3 Positive electrodes were produced in the same manner in the other examples and comparative examples.
[0067] [Preparation of negative electrode] As the negative electrode active material, 96 parts by mass of graphite and 4 parts by mass of SiO x (x=0.94) was used. 100 parts by mass of the negative electrode active material, 1 part by mass of SBR dispersion, and 1 part by mass of sodium salt of CMC were mixed, and this was mixed with water to prepare a negative electrode slurry. Next, the slurry was applied to both sides of a negative electrode current collector made of copper foil, and after drying the coating, the coating was rolled with a rolling roller to prepare a negative electrode in which a negative electrode active material layer was formed on both sides of the negative electrode current collector.
[0068] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF6) was dissolved in the mixed solvent to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0069] [Preparation of test cell] The positive electrode and the negative electrode of Example 1 were stacked so as to face each other with a separator interposed therebetween, and the stack was wound to prepare an electrode assembly. Next, the electrode assembly and the non-aqueous electrolyte were inserted into an aluminum exterior body to prepare a test cell. Test cells were prepared in the same manner in the other Examples and Comparative Examples.
[0070] [Initial battery capacity measurement] The test cell was charged at a constant current of 120 mA at a temperature of 25° C. until the cell voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current value reached 8 mA. The charge capacity at this time was taken as the battery capacity.
[0071] [Measurement of reaction resistance] After the battery capacity was measured, the test cell was again charged at a constant current of 120 mA under a temperature condition of 25° C. until the cell voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current value reached 8 mA. Next, the test cell was measured for AC impedance from 20 kHz to 0.01 Hz using an AC impedance measuring device, and a Cole-Cole plot was drawn from the measurement data, and the reaction resistance was calculated from the size of the arc between 10 Hz and 0.1 Hz.
[0072] The battery capacities and reaction resistances of the examples and comparative examples are shown in Tables 2 to 4. Table 2 shows the actual measured values of the battery capacities and reaction resistances of the test cells of Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-7.
[0073] Table 3 shows the measured values of the battery capacity of the test cells of Example 2 and Comparative Example 2. The reaction resistance of the test cell of Example 2 is shown relative to the reaction resistance of the test cell of Comparative Example 2, which is set as 100.
[0074] Table 4 shows the measured values of the battery capacity of the test cells of Example 3 and Comparative Example 3. The reaction resistance of the test cell of Example 3 is expressed relative to the reaction resistance of the test cell of Comparative Example 3, which is set as 100.
[0075] [Table 2]
[0076] [Table 3]
[0077] [Table 4]
[0078] In Table 2, Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-6, which satisfied the condition of 50%≦n1 / (n1+n2)<75%, had lower reaction resistance than Comparative Examples 1-1 to 1-6. It is also presumed that Comparative Example 1-6 had a too high Nb content and Comparative Example 1-7 had a too fast temperature rise rate, resulting in a low battery capacity.
[0079] Also in Tables 3 and 4, regardless of the Ni content, Examples 2 and 3 which satisfied the condition 50%≦n1 / (n1+n2)<75% had lower reaction resistance than Comparative Examples 2 and 3, respectively. [Explanation of symbols]
[0080] 10 Nonaqueous electrolyte secondary battery 11 Positive electrode 12 Negative electrode 13 Separator 14 Electrode body 15 Battery case 16 Outer can 17 Sealing body 18,19 Insulating plate 20 Positive tab 21 Negative electrode tab 22 Grooved part 23 Bottom plate 24 Lower valve body 25 Insulating materials 26 Upper valve 27 Cap 28 Gasket 30 Positive electrode current collector 31 Positive electrode active material layer 40 Negative electrode current collector 41 Negative electrode active material layer
Claims
1. A lithium transition metal compound containing Ni in a ratio of 80 mol % or more and 94 mol % or less based on the total number of moles of metal elements excluding Li, Co in a ratio of 10 mol % or less based on the total number of moles of metal elements excluding Li, and Nb in a ratio of 0.1 mol % or more and 0.6 mol % or less based on the total number of moles of metal elements excluding Li, A positive electrode active material for a nonaqueous electrolyte secondary battery, in which a first sample solution obtained by adding 0.2 g of the lithium transition metal compound to an aqueous hydrochloric acid solution of 5 mL of pure water / 5 mL of 35% hydrochloric acid is dissolved under bumping for 120 minutes, and then the first sample solution is filtered and collected to obtain a first filtrate, and an amount of Nb n1 determined by inductively coupled plasma atomic emission spectrometry in a first filtrate obtained by dissolving under bumping for 180 minutes a second sample solution obtained by immersing a filter used for filtering the first sample solution in 5 mL of 46% hydrofluoric acid / 5 mL of 63% nitric acid and fluoronitric acid, and then the second sample solution is filtered and collected, the amount of Nb n2 determined by inductively coupled plasma atomic emission spectrometry in a second filtrate obtained by dissolving under bumping for 180 minutes, and then the second sample solution is filtered and collected, satisfy the condition of 50%≦n1 / (n1+n2)<75%, in terms of molar amount.
2. The lithium transition metal compound has the general formula Li a Ni x Co y M z Nb α O 2 2. The positive electrode active material for a nonaqueous electrolyte secondary battery according to claim 1, wherein: (0.95≦a≦1.10, 0.80≦x≦0.94, 0≦y≦0.02, 0.04≦z≦0.20, 0.001≦α≦0.006, x+y+z+α=1, and M contains at least one element selected from Al, W, Mg, Ti, Mn, and Mo).
3. A non-aqueous electrolyte secondary battery comprising: a positive electrode containing the positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1; a negative electrode; and a non-aqueous electrolyte.
4. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, comprising a lithium transition metal compound containing Ni in a ratio of 80 mol % or more based on the total number of moles of metal elements excluding Li, Co in a ratio of 10 mol % or less based on the total number of moles of metal elements excluding Li, and Nb in a ratio of 0.1 mol % to 0.6 mol % based on the total number of moles of metal elements excluding Li, A mixing step of mixing a composite oxide containing at least Ni, a Li compound, and a Nb compound to obtain a mixture; The method includes a firing step of firing the mixture in an oxygen atmosphere at a heating rate of more than 3.5° C. / min and not more than 5.5° C. / min at 450° C. to 680° C., and at a maximum temperature of 700° C. to 780° C. in a firing furnace; The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, wherein the maximum temperature is maintained for a time period of 1 hour or more and 10 hours or less.
5. 5. The method for producing a positive electrode active material for a nonaqueous electrolyte secondary battery according to claim 4, wherein in the firing step, a maximum pressure applied inside the firing furnace is in a range of more than 0.55 kPa and not more than 1.0 kPa in addition to the pressure outside the firing furnace.
Citation Information
Patent Citations
Positive electrode active material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery employing the same
JP2009140787A
Nonaqueous electrolyte secondary battery
JP2011187435A
Method for manufacturing positive electrode active material for nonaqueous electrolyte secondary batteries, positive electrode active material for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery arranged by use thereof
JP2015122298A
Positive electrode active material for non-aqueous electrolyte secondary cell and method for manufacturing same, and non-aqueous electrolyte secondary cell
WO2018123951A1
Positive electrode active material for nonaqueous electrolyte secondary batteries, method for producing positive electrode active material for nonaqueous electrolyte secondary batteries, and method for evaluating lithium metal composite oxide powder
WO2019087558A1