Separator for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
The separator with dot-shaped filler particle aggregates addresses heat and resistance issues in non-aqueous electrolyte secondary batteries by transforming to a liquid phase during nail penetration, forming a film to suppress heat and maintain low resistance.
Patent Information
- Application Number
- JP2021566842
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-24
- Filing Date
- 2020-10-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-10-15
AI Technical Summary
Existing non-aqueous electrolyte secondary batteries face challenges in suppressing heat generation and resistance during nail penetration tests, which simulate internal short circuits, without compromising lithium ion mobility during normal use.
A separator for non-aqueous electrolyte secondary batteries featuring a porous base material with dot-shaped aggregates of filler particles made from compounds like phosphorus, silicon, boron, nitrogen, potassium, or sodium, which transform to a liquid phase or decompose thermally at specific temperatures, forming a film to suppress short-circuit current and inhibit lithium ion movement during normal use.
The solution effectively suppresses heat generation during nail penetration tests while maintaining low battery resistance by allowing smooth lithium ion transport, thus enhancing safety and performance.
Smart Images

Figure 0007584105000003 
Figure 0007584105000004 
Figure 0007584105000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a separator for a nonaqueous electrolyte secondary battery and a nonaqueous electrolyte secondary battery. [Background technology]
[0002] 2. Description of the Related Art In recent years, non-aqueous electrolyte secondary batteries, which perform charging and discharging by transferring lithium ions between a positive electrode and a negative electrode, have been widely used as high-output, high-energy density secondary batteries.
[0003] Incidentally, a nail penetration test is a safety evaluation test for checking the resistance of a battery to an internal short circuit. The nail penetration test is a test in which, for example, a nail is penetrated into a battery to simulate an internal short circuit, and the degree of heat generation is examined to check the safety of the battery. In order to ensure the safety of the battery, it is important to suppress the heat generation of the battery when the battery is penetrated by the nail.
[0004] For example, Patent Document 1 discloses that a separator with excellent safety can be provided by providing a porous layer containing inorganic particles and a basic phosphate in a separator disposed between a positive electrode and a negative electrode. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6347580 [Patent Document 2] Patent No. 6016757 Summary of the Invention
[0006] A separator for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a separator substrate and an aggregate of filler particles present in a dot pattern on a surface of the separator substrate, the filler particles being compound particles containing at least one of phosphorus, silicon, boron, nitrogen, potassium, sodium, and bromine, and having a transformation point in the range of 180°C to 1000°C where the filler particles transform from a solid phase to a liquid phase or thermally decompose.
[0007] A nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, the separator being a separator for nonaqueous electrolyte secondary batteries.
[0008] According to the present disclosure, it is possible to suppress heat generation in a battery during a nail penetration test while suppressing an increase in battery resistance. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a separator according to the present embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.
[0011] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a separator according to this embodiment. The separator 60 shown in FIG. 1 is a separator for a non-aqueous electrolyte secondary battery. The separator 60 shown in FIG. 1 includes a separator substrate 63 having a porous substrate 62 and a heat-resistant layer 64 formed on the porous substrate 62. The separator 60 shown in FIG. 1 also includes aggregates 66 of filler particles present in a dot shape on the surface of the heat-resistant layer 64. However, the heat-resistant layer 64 is not essential, and the separator substrate 63 may be the porous substrate 62. In this case, the aggregates 66 are present in a dot shape on the surface of the porous substrate 62, which is the separator substrate 63. The aggregates 66 may be disposed on one surface of the separator substrate 63, or on both surfaces. In any case, the surface structure of the separator 60 according to this embodiment is a sea-island structure having a sea region on the surface of the separator substrate and an island region of the aggregates 66. The aggregates 66 are a collection of a plurality of filler particles.
[0012] The filler particles constituting the aggregate 66 are compound particles containing at least one of phosphorus, silicon, boron, nitrogen, potassium, sodium, and bromine, and have a transformation point in the range of 180°C to 1000°C at which they transform from a solid phase to a liquid phase or decompose thermally.
[0013] By using the separator for a non-aqueous electrolyte secondary battery according to this embodiment, the rise in the battery temperature during the nail penetration test is suppressed. The mechanism is not fully clear, but the following is presumed. Due to the heat generated by the battery during the nail penetration test, that is, the heat generated by the battery when a nail is pierced into the battery to simulate an internal short circuit, the filler particles constituting the aggregate 66 transform from a solid phase to a liquid phase and flow on the surface of the separator substrate 63, or extend on the surface of the separator substrate 63 by thermal decomposition, and become a coating covering the surface of the separator substrate 63. Since the coating functions as a resistance component, the amount of short-circuit current flowing between the positive and negative electrodes through the nail is suppressed, and as a result, the rise in the battery temperature during the nail penetration test is also suppressed. The formation of the coating after the transformation of the filler particles into a liquid phase depends on the type of filler particles, but is due to, for example, a temperature rise above the melting point of the filler material, a heat fusion reaction, a dehydration condensation reaction, a thermal polymerization reaction, or the like.
[0014] In addition, the separator for a non-aqueous electrolyte secondary battery according to this embodiment suppresses an increase in battery resistance. During normal use when the battery is not generating abnormal heat, the aggregates 66 of the filler particles are made of a material with low lithium ion conductivity, and if they are present in a layered form, they will inhibit the movement of lithium ions, causing an increase in battery resistance. However, since the aggregates 66 are dot-shaped in this embodiment, there are gaps between the aggregates 66, and ions such as lithium ions can easily pass through the gaps. Therefore, when the battery is charged and discharged, lithium ions move more smoothly between the positive and negative electrodes than when the entire surface of the separator substrate 63 is covered without gaps with a coating layer of filler particles, and it is considered that an increase in battery resistance is suppressed.
[0015] The constituent materials of the separator 60 will be described in further detail below.
[0016] The filler particles are not particularly limited as long as they are compound particles containing at least one of phosphorus, silicon, boron, nitrogen, potassium, sodium, and bromine, and have a transformation point of 180°C to 1000°C at which they transform from a solid phase to a liquid phase or are thermally decomposed. Examples of the filler particles include compounds having a transformation point of 180°C to 1000°C at which they transform from a solid phase to a liquid phase or are thermally decomposed, such as phosphoric acid compounds, silicic acid compounds, boric acid compounds, melamine salt compounds, potassium salt compounds, and sodium salt compounds. Examples of the phosphoric acid compounds include metal salts of phosphoric acid such as lithium phosphoric acid salt, sodium phosphoric acid salt, potassium phosphoric acid salt, calcium phosphoric acid salt, magnesium phosphoric acid salt, and aluminum phosphate, condensed phosphates such as ammonium polyphosphate, sodium tripolyphosphate, and melamine polyphosphate, and phosphoric acid esters such as trimethyl phosphate and triphenyl phosphate. Examples of the boric acid compound include metal borate salts such as sodium borate, potassium borate, calcium borate, magnesium borate, aluminum borate, and melamine borate, borate esters such as trimethyl borate, boron oxides, and condensed borates. Examples of the silicic acid compound include metal silicates such as sodium silicate, potassium silicate, calcium silicate, magnesium silicate, barium silicate, and manganese silicate. Examples of the melamine salt compound include melamine cyanurate, melamine pyrophosphate, ethylene dimelamine, trimethylene dimelamine, tetramethylene dimelamine, hexamethylene dimelamine, and 1,3-hexylene dimelamine. Examples of the potassium salt compound include potassium pyrosulfate (K 2 S 2 O 7 ), potassium citrate monohydrate (C 6 H 5 K 3 O 7 H 2Examples of the sodium salt compound include sodium carbonate. Among these, melamine polyphosphate, ammonium polyphosphate, sodium tripolyphosphate, sodium silicate, sodium borate, potassium citrate monohydrate, lithium metaphosphate, potassium dihydrogen phosphate, melamine cyanurate, potassium pyrosulfate, boron oxide, ethylene-1,2-bis(pentabromophenyl), ethylenebistetrabromophthalimide, potassium carbonate, and sodium carbonate are preferred.
[0017] The transformation point of the filler particles may be in the range of 180°C to 1000°C so that the filler particles appropriately transform from a solid phase to a liquid phase or thermally decompose due to heat generation in the battery during a nail penetration test, but is preferably in the range of 180°C to 900°C, and more preferably in the range of 180°C to 600°C.
[0018] The coverage of the aggregates 66 with respect to the surface of the separator substrate 63 is preferably 90% or less, more preferably 65% or less, in order to suppress an increase in battery resistance. Also, in order to suppress an increase in battery temperature in a nail penetration test, the coverage is preferably 20% or more, more preferably 30% or more. The coverage of the aggregates 66 is calculated as follows.
[0019] The coverage rate is obtained by performing elemental mapping of the separator surface by SEM-EDX (Energy Dispersive X-ray spectrometry) etc. For example, the coverage rate is obtained by distinguishing the island regions of the aggregates 66 from the sea regions of the separator substrate surface by elemental mapping, and calculating the ratio of the area of the island regions to the total area of the island regions and the sea regions.
[0020] The average particle size of the filler particles is preferably 0.1 μm to 5 μm, and more preferably 0.2 μm to 1 μm. When the average particle size of the filler particles satisfies the above range, the filler particles are transformed from a solid phase to a liquid phase more quickly due to heat generation of the battery during the nail penetration test, compared to when the average particle size of the filler particles does not satisfy the above range, and therefore the rise in battery temperature during the nail penetration test can be effectively suppressed.
[0021] The aggregate 66 may contain a binder in addition to the filler particles. By including a binder, the adhesiveness between the filler particles and between the filler particles and the separator substrate 63 can be improved. Examples of the binder include polyvinylidene fluoride (PVdF), ethylene dimethacrylate, allyl methacrylate, t-dodecyl mercaptan, α-methylstyrene dimer, and methacrylic acid. Note that polyvinylidene fluoride (PVdF), ethylene dimethacrylate, allyl methacrylate, t-dodecyl mercaptan, α-methylstyrene dimer, and methacrylic acid can bond the electrodes and the separator by applying pressure and / or heat to the aggregate 66. The aggregate 66 may also contain compound particles other than the filler particles. Examples of compound particles other than the filler particles include inorganic particles such as alumina, boehmite, and titania.
[0022] The porous substrate 62 is, for example, a porous sheet such as a microporous thin film, a woven fabric, or a nonwoven fabric having ion permeability and insulation properties. Examples of materials constituting the porous substrate 62 include polyolefins such as polyethylene, polypropylene, copolymers of polyethylene and α-olefin, acrylic resins, polystyrene, polyester, and cellulose. The porous substrate 62 may have a single-layer structure or a laminated structure. The thickness of the porous substrate 62 is not particularly limited, but is, for example, in the range of 3 μm to 20 μm.
[0023] The porosity of the porous substrate 62 is preferably, for example, 30% or more and 70% or less in terms of ensuring ion permeability, etc. The porosity of the porous substrate 62 is measured by the following method. (1) The substrate is punched out at 10 locations to form circles with a diameter of 2 cm, and the thickness (h) and mass (w) of the center of each punched piece of substrate are measured. (2) From the thickness h and mass w, the volume V and mass W of the 10 pieces are calculated, and the porosity ε is calculated using the following formula.
[0024] Porosity ε(%)=((ρV-W) / (ρV))×100 ρ: Density of the material that constitutes the base material The average pore size of the porous substrate 62 is, for example, 0.02 μm to 0.5 μm, preferably 0.03 μm to 0.3 μm. The average pore size of the porous substrate 62 is measured using a Perm Porometer (manufactured by Seika Sangyo Co., Ltd.) capable of measuring pore size by the bubble point method (JIS K3832, ASTM F316-86). The maximum pore size of the substrate 24 is, for example, 0.05 μm to 1 μm, preferably 0.05 μm to 0.5 μm.
[0025] The heat-resistant layer 64 is composed of inorganic particles such as alumina, boehmite, and titania. By providing the heat-resistant layer 64, it is possible to improve the heat resistance of the separator 60. The heat-resistant layer 64 may contain, for example, a binder. By containing a binder, it is possible to ensure adhesion between the porous substrate 62 and the heat-resistant layer 64. The binder is not particularly limited, and examples thereof include polyvinylidene fluoride (PVdF), methacrylic acid, and the like.
[0026] The thickness of the heat-resistant layer 64 is not particularly limited, but is, for example, in the range of 1 μm to 10 μm. The heat-resistant layer 64 may be provided on one surface of the porous substrate 62, or on both surfaces.
[0027] An example of a method for producing the separator 60 will be described. A filler slurry containing filler particles, a binder, a solvent, etc. is prepared. The prepared filler slurry is then sprayed, dropped or applied onto the surface of the separator substrate 63, and then dried to form aggregates 66 of filler particles present in the form of dots on the surface of the separator substrate 63. Examples of the solvent contained in the slurry include water and N-methyl-2-pyrrolidone (NMP).
[0028] The dot-shaped aggregate can be produced, for example, by a gravure coater method using a dot-shaped plate, or a spray coating method using a mask on which a dot-shaped through pattern is formed.
[0029] An example of the nonaqueous electrolyte secondary battery according to this embodiment will be described below.
[0030] FIG. 2 is a schematic cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment. The nonaqueous electrolyte secondary battery 10 shown in FIG. 2 includes a wound electrode body 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 therebetween, a nonaqueous electrolyte, insulating plates 18 and 19 respectively arranged above and below the electrode body 14, and a battery case 15 for accommodating the above-mentioned members. The battery case 15 is composed of a bottomed cylindrical case body 16 and a sealing body 17 for closing an opening of the case body 16. Note that, instead of the wound electrode body 14, an electrode body of another form may be applied, such as a laminated electrode body formed by alternately stacking positive and negative electrodes with a separator interposed therebetween. In addition, examples of the battery case 15 include a cylindrical, square, coin-shaped, button-shaped, or other metal case, and a resin case formed by laminating a resin sheet (so-called laminate type).
[0031] The case body 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has a protruding portion 22 that supports the sealing body 17, for example, a part of the side surface of the case body 16 protruding inward. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the case body 16, and supports the sealing body 17 on its upper surface.
[0032] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are laminated in this order from the electrode body 14 side. Each member constituting the sealing body 17 has, for example, a disk shape or a ring shape, and each member except the insulating member 25 is electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between each of their peripheral edges. When the internal pressure of the secondary battery 10 increases due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 24 deforms and breaks so as to push the upper valve body 26 toward the cap 27, and the current path between the lower valve body 24 and the upper valve body 26 is interrupted. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0033] 2, a positive electrode lead 20 attached to the positive electrode 11 extends through a through hole in an insulating plate 18 toward the sealing body 17, and a negative electrode lead 21 attached to the negative electrode 12 extends through the outside of an insulating plate 19 toward the bottom side of a case body 16. The positive electrode lead 20 is connected to the underside of a filter 23, which is the bottom plate of the sealing body 17, by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the filter 23, serves as a positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the case body 16 by welding or the like, and the case body 16 serves as a negative electrode terminal.
[0034] The positive electrode 11 has, for example, a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector. The positive electrode current collector can be, for example, a foil of a metal such as aluminum that is stable in the potential range of the positive electrode, or a film having the metal disposed on the surface layer. The positive electrode active material layer preferably contains a positive electrode active material, and also contains a conductive material and a binder.
[0035] Examples of the positive electrode active material include lithium transition metal composite oxides. Specifically, lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium nickel manganese composite oxide, lithium nickel cobalt composite oxide, etc. can be used. These lithium transition metal composite oxides may contain Al, Ti, Zr, Nb, B, W, Mg, Mo, etc.
[0036] As the conductive material, carbon powder such as carbon black, acetylene black, ketjen black, graphite, etc. may be used alone or in combination of two or more kinds.
[0037] Examples of the binder include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide-based resins, acrylic-based resins, polyolefin-based resins, etc. These may be used alone or in combination of two or more kinds.
[0038] The negative electrode 12 has, for example, a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector. For the negative electrode current collector, for example, a foil of a metal such as copper that is stable in the potential range of the negative electrode, or a film having such a metal disposed on the surface layer, can be used. In addition, the negative electrode active material layer preferably contains a negative electrode active material and also contains a binder, etc.
[0039] As the negative electrode active material, a carbon material capable of absorbing and releasing lithium ions can be used, and in addition to graphite, non-graphitizable carbon, graphitizable carbon, fibrous carbon, coke, carbon black, etc. Furthermore, as a non-carbon-based material, silicon, tin, and alloys and oxides mainly containing these can be used.
[0040] Examples of the binder include fluorine-based resin, PAN, polyimide-based resin, acrylic resin, polyolefin-based resin, styrene-butadiene rubber (SBR), nitrile-butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more kinds.
[0041] The separator 13 is the separator 60 described above.
[0042] The non-aqueous electrolyte includes a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixtures of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen of these solvents is replaced with a halogen atom such as fluorine. The electrolyte salt may include, for example, LiPF 6 Lithium salts such as
[0043] Next, an embodiment will be described.
[0044] <Example> <Example 1> [Preparation of positive electrode] LiNi 0.82 Co 0.15 Al 0.03 O 2 100 parts by weight of the positive electrode active material represented by the formula (I) was mixed with 1 part by weight of acetylene black (AB) and 1 part by weight of polyvinylidene fluoride (PVdF), and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode mixture slurry. Next, the positive electrode mixture slurry was applied to both sides of a positive electrode current collector made of aluminum foil and dried. This was cut into a predetermined electrode size and rolled using a roller to form a positive electrode active material layer on both sides of the positive electrode current collector.
[0045] [Preparation of negative electrode] 100 parts by weight of graphite powder, 1 part by weight of carboxymethyl cellulose (CMC), and 1 part by weight of styrene-butadiene rubber (SBR) were mixed, and an appropriate amount of water was added to prepare a negative electrode composite slurry. Next, the negative electrode composite slurry was applied to both sides of a negative electrode current collector made of copper foil and dried. This was cut into a predetermined electrode size and rolled using a roller to form a negative electrode active material layer on both sides of the negative electrode current collector.
[0046] [Making the separator] A filler slurry was prepared by mixing 80 parts by weight of melamine polyphosphate particles, 20 parts by weight of polyvinylidene fluoride (PVdF), and N-methyl-2-pyrrolidone (NMP) to a solid content ratio of 40% by weight. The slurry was applied in a dot pattern using a gravure coater on one side of a single-layer polyethylene porous substrate having a thickness of 12 μm, and dried at 60° C. This was the separator of Example 1.
[0047] When the surface of the separator in Example 1 was observed by SEM-EDX, it was confirmed that the aggregates of the melamine polyphosphate particles were in the form of round dots having a diameter of 300 μm, and the coverage rate of the aggregates of the melamine polyphosphate particles was 30%.
[0048] [Preparation of non-aqueous electrolyte] Lithium hexafluorophosphate (LiPF 6 ) was dissolved in water to a concentration of 1 mol / L to prepare a non-aqueous electrolyte.
[0049] [Preparation of non-aqueous electrolyte secondary battery] (1) A positive electrode lead was attached to the positive electrode current collector, and a negative electrode lead was attached to the negative electrode current collector. The separator was then disposed between the positive electrode and the negative electrode such that the aggregate of filler particles faced the positive electrode, and these were then wound to prepare a wound electrode body. (2) Insulating plates were placed above and below the electrode body, the negative electrode lead was welded to the case body, and the positive electrode lead was welded to the sealing member, and the electrode body was housed within the case body. (3) After the non-aqueous electrolyte was injected into the case body under reduced pressure, the open end of the case body was sealed with a sealing member via a gasket, completing the non-aqueous electrolyte secondary battery.
[0050] <Example 2> A separator was produced in the same manner as in Example 1, except that the gravure mesh roll pattern of the gravure coater was changed, and this was used as the separator of Example 2. When the surface of the separator of Example 2 was observed by SEM-EDX, it was confirmed that the aggregates of the melamine polyphosphate particles were in the form of dots, and the coverage rate of the aggregates of the melamine polyphosphate particles was 90%.
[0051] <Example 3> Except for changing polyvinylidene fluoride to butyl acrylate in the preparation of the filler slurry, the procedure was the same as in Example 1, and this was used to prepare a separator of Example 3. When the surface of the separator of Example 3 was observed by SEM-EDX, it was confirmed that the aggregates of the melamine polyphosphate particles were in the form of dots, and the coverage rate of the aggregates of the melamine polyphosphate particles was 30%.
[0052] <Examples 4 to 8> In preparing the filler slurry, the melamine polyphosphate particles were replaced with ammonium polyphosphate particles in Example 4, sodium tripolyphosphate particles in Example 5, and sodium silicate (Na 2 SiO 3 In Example 7, sodium borate (Na 2 B 4 O 7 In Example 8, potassium citrate monohydrate (C 6 H 5 K 3 O 7 H 2 Except for replacing the filler particles with the O) particles, separators were produced in the same manner as in Example 1. When the surfaces of the separators in Examples 4 to 8 were observed by SEM-EDX, it was confirmed that the aggregates of the filler particles were in a dot shape in all cases, and the coverage rate of the aggregates of the filler particles was 30%.
[0053] <Comparative Example 1> A nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example 1, except that no filler slurry was used.
[0054] <Comparative Example 2> A separator was produced in the same manner as in Example 1, except that the pattern of the gravure mesh roll of the gravure coater was changed, and this was used as a separator of Comparative Example 2. When the surface of the separator of Comparative Example 2 was observed by SEM-EDX, the aggregate of the filler particles covered the entire surface, and the coverage rate was 100%.
[0055] [Nail penetration test] For the nonaqueous electrolyte secondary batteries of Examples 1 to 8 and Comparative Examples 1 and 2, a nail penetration test was carried out according to the following procedure. (1) In an environment of 25°C, the battery was charged at a constant current of 600 mA until the battery voltage reached 4.2 V, and then continued to be charged at a constant voltage until the current value reached 90 mA. (2) In an environment of 25°C, the tip of a round nail with a diameter of 2.7 mm was brought into contact with the center of the side of the battery charged in (1), and the round nail was thrust into the battery in the stacking direction of the electrode body at a speed of 1 mm / sec. Immediately after detecting a drop in the battery voltage due to an internal short circuit, thrusting of the round nail was stopped. (3) The battery surface temperature was measured one minute after the battery started to short circuit with the round nail. The measured temperatures are shown in Table 1 as the temperatures after the nail penetration test.
[0056] [Battery resistance] The battery resistance of the nonaqueous electrolyte secondary batteries of Examples 1 to 8 and Comparative Examples 1 and 2 was measured as follows. In a temperature environment of 25°C, the nonaqueous electrolyte secondary battery was charged at a constant current of 0.3C until the battery voltage reached 4.2V, then charged at a constant voltage until the current value reached 0.05C, and then discharged at a constant current of 0.3C to set the SOC to 50%. Next, the voltage values were obtained when discharge currents of 0A, 0.1A, 0.5A, and 1.0A were applied for 10 seconds. DC-IR was calculated from the absolute value of the slope when the voltage value after 10 seconds for each discharge current value was linearly approximated by the least squares method, and this value was summarized in Table 1 as the battery resistance.
[0057] [Table 1]
[0058] As shown in Table 1, in all of Examples 1 to 8 in which aggregates of filler particles were present in a dot pattern on the surface of the polyethylene porous substrate, the battery temperature after the nail penetration test was lower than in Comparative Example 1 in which no filler particles were present on the surface of the polyethylene porous substrate. Here, when the coverage rate of the aggregates of filler particles was taken as 100%, as in Comparative Example 2, the battery resistance increased significantly compared to Comparative Example 1. However, in Examples 1 to 8, the increase in battery resistance was suppressed more than in Comparative Example 2. That is, in Examples 1 to 8, it was possible to suppress the heat generation of the battery in the nail penetration test while suppressing the increase in battery resistance.
[0059] <Examples 9 to 18> In preparing the filler slurry, melamine polyphosphate particles were used in Example 9, and lithium metaphosphate (LiPO 3 ) n In Example 10, potassium dihydrogen phosphate (KH 2 PO 4 ) particles, in Example 11 melamine cyanurate, and in Example 12 potassium pyrosulfate (K 2 S 2 O 7 In Example 13, instead of the boron oxide (B 2 O 3 ) particles, in Example 14, ethylene-1,2-bis(pentabromophenyl) particles, in Example 15, ethylenebistetrabromophthalimide particles, and in Example 16, potassium carbonate (K 2 CO 3 In Example 17, sodium carbonate (Na 2 CO 3 Separators were produced in the same manner as in Example 1, except that in Example 18, a mixture of 80 parts by weight of melamine polyphosphate particles and 20 parts by weight of alumina particles was used instead of the filler particles in Example 9. When the separator surfaces of Examples 9 to 18 were observed by SEM-EDX, it was confirmed that the aggregates of the filler particles were in a dot shape in all cases, and the coverage rate of the aggregates of the filler particles was 30%.
[0060] The coverage of the aggregates of the filler particles in Examples 9 to 18 is summarized in Table 2. In addition, the nonaqueous electrolyte secondary batteries of Examples 9 to 18 were subjected to the above-mentioned nail penetration test and battery resistance measurement.
[0061] [Table 2]
[0062] In all of Examples 9 to 18, the battery temperature after the nail penetration test was lower than in Comparative Example 1 in which no filler particles were present on the surface of the polyethylene porous substrate. In addition, the battery resistance was higher than in Comparative Example 1, but was comparable to that of Example 2. In other words, it can be said that Examples 9 to 18 were also able to suppress the heat generation of the battery during the nail penetration test while suppressing the increase in battery resistance. [Explanation of symbols]
[0063] 10 Nonaqueous electrolyte secondary battery 11 Positive electrode 12 Negative electrode 13 Separator 14 Electrode body 15 Battery case 16 Case body 17 Sealing body 18,19 Insulating plate 20 Positive lead 21 Negative lead 22 Overhang 23 Filters 24 Lower valve body 25 Insulating materials 26 Upper valve 27 Cap 28 Gasket 60 Separator 62 Porous substrate 64 Heat-resistant layer 66 Aggregate
Claims
1. A separator substrate and an aggregate of filler particles present in a dot shape on a surface of the separator substrate, the filler particles include compound particles containing at least one of silicon, boron, nitrogen, potassium, and bromine, and at least one of melamine polyphosphate, ammonium polyphosphate, sodium tripolyphosphate, lithium metaphosphate, and sodium carbonate, and the solid-to-liquid phase transformation point or thermal decomposition point is in the range of 180°C to 1000°C.
2. 2. The separator for a non-aqueous electrolyte secondary battery according to claim 1, wherein the coverage of the surface of the separator substrate with the assembly is 90% or less.
3. 3. The separator for a non-aqueous electrolyte secondary battery according to claim 1, wherein the coverage of the surface of the separator substrate with the assembly is 30% or more.
4. The separator for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 3, wherein the filler particles include at least one of the melamine polyphosphate, the ammonium polyphosphate, the sodium tripolyphosphate, the lithium metaphosphate, a silicate compound, a boric acid compound, a melamine salt compound, a potassium salt compound, the sodium carbonate, and an aromatic bromine compound.
5. 5. The separator for a non-aqueous electrolyte secondary battery according to claim 4, wherein the filler particles include at least one of the melamine polyphosphate, the ammonium polyphosphate, the sodium tripolyphosphate, sodium silicate, sodium borate, potassium citrate monohydrate, the lithium metaphosphate, potassium phosphate, melamine cyanurate, potassium pyrosulfate, boron oxide, ethylene-1,2-bis(pentabromophenyl), ethylenebistetrabromophthalimide, potassium carbonate, and the sodium carbonate.
6. The separator for a nonaqueous electrolyte secondary battery according to any one of claims 1 to 5, wherein the assembly includes a binder, and the binder includes at least one of polyvinylidene fluoride, ethylene dimethacrylate, allyl methacrylate, t-dodecyl mercaptan, α-methylstyrene dimer, and methacrylic acid.
7. 7. The separator for a non-aqueous electrolyte secondary battery according to claim 1, wherein the aggregate contains inorganic particles, and the inorganic particles contain at least one of alumina, boehmite, and titania.
8. The separator for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 7, wherein the separator substrate has a porous substrate and a heat-resistant layer provided on the porous substrate, the heat-resistant layer contains inorganic particles, and the inorganic particles contain at least one of alumina, boehmite, and titania.
9. A battery comprising a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode; The separator is the separator for non-aqueous electrolyte secondary batteries according to any one of claims 1 to 8.
Citation Information
Patent Citations
Electrochemical apparatus, isolation membrane used therein and preparation method of the isolation membrane
CN104979516A
Lithium ion battery and membrane thereof
CN107039624A
Document transmission system
JP1985016757A
Holding valve
JP1988047580A
Separator for power storage device
JP2016072120A