Electrical contact material and its manufacturing method, circuit breaker and electromagnetic switch
By integrating FeO particles into Ag-SnO2 electrical contact materials and controlling oxygen partial pressure during heat treatment, the material's sulfidation resistance and contact resistance are enhanced, addressing the sulfidation issues of Ag-SnO2 materials.
Patent Information
- Application Number
- JP2023525273
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-03
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-06-03
AI Technical Summary
Existing Ag-SnO2 electrical contact materials suffer from sulfidation resistance issues, leading to increased contact resistance in environments containing sulfur dioxide, despite techniques that suppress contact resistance during arcing.
Incorporating FeO particles into the Ag-SnO2 sintered body, which act as reducing agents to stabilize the contact resistance by reducing SnO2 to Sn and forming an Ag-Sn alloy, while maintaining a controlled oxygen partial pressure during heat treatment to ensure FeO and SnO2 coexistence.
The resulting electrical contact material exhibits improved sulfidation resistance and suppressed contact resistance increase due to arcing, maintaining stable performance in sulfur dioxide-containing environments.
Smart Images

Figure 0007584646000001 
Figure 0007584646000002 
Figure 0007584646000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an electrical contact material used for contacts in control devices, a method for producing the same, a circuit breaker, and an electromagnetic switch. [Background technology]
[0002] Ag-CdO (cadmium oxide), Ag-SnO2 (tin oxide), Ag-ZnO (zinc oxide), etc., which are mixtures of Ag (silver), a conductive component that does not oxidize easily in the air, and metal oxide, an arc-resistant component, have been used as electrical contact materials for control devices such as air circuit breakers, electromagnetic switches, and relays. Unlike electrical contact materials made of pure metals such as Ag-Ni (nickel), these materials have the advantage of being highly resistant to welding and arcing, and are therefore often used in products with a rated current of 50A or more. In recent years, the use of Ag-CdO-based electrical contact materials, which contain cadmium, has decreased in consideration of their impact on the environment and human body, and instead, cadmium-free Ag-SnO2-based electrical contact materials have become widely used.
[0003] The manufacturing methods of Ag-SnO2-based electrical contact materials are roughly divided into powder metallurgy and internal oxidation. In the powder metallurgy method, Ag powder and SnO2 powder are mixed, the mixed powder is put into a mold, and then molded under appropriate pressure, and the molded powder is then sintered to manufacture Ag-SnO2-based electrical contact materials. Powder metallurgy is also called powder sintering. In the internal oxidation method, an Ag-Sn alloy ingot is produced and then divided into fine chips. The divided fine chips are heated and pressurized in an oxidation furnace to thermally oxidize them. At temperatures above 200°C, Ag does not oxidize, and only the other added metals oxidize. Here, Sn oxidizes to become SnO2. However, if only Sn is mixed with Ag, oxidation does not progress to the inside of the fine chips, so low-melting point metals such as In (indium) and Bi (bismuth) are often mixed as auxiliary agents. When In is added as an auxiliary agent, the resulting electrical contact material is Ag-SnO2-In2O3. This internal oxidation method is further classified into post-oxidation and pre-oxidation methods depending on the manufacturing process steps. In the post-oxidation method, the fine chips are miniaturized to the actual shape of the contacts, which are several millimeters in size, and after thermal oxidation, the electrical contact material is used as is as the contact. In the pre-oxidation method, fine chips, which are several millimeters to a dozen millimeters in size, are oxidized, solidified to form a billet, and thin wires are produced by finely mixing the materials by hot extrusion, and the wires are formed into the shape of the contacts in a molding machine.
[0004] SnO2 has a higher decomposition temperature than CdO and ZnO, and therefore has the advantage of being more resistant to wear than other oxide-based electrical contact materials. However, it also has the disadvantage of remaining on the contact surface and increasing the contact resistance. When an arc is broken, the contact surface melts and part of it evaporates, and the remaining molten part resolidifies. During manufacturing, SnO2 was uniformly distributed within the contact, but Ag evaporated more, and as a result, more SnO2 remained on the contact surface, increasing the contact resistance. In actual contacts, the concentration of SnO2 is determined in consideration of the contact resistance, adhesion resistance, ease of manufacturing, etc., in light of the current-carrying conditions of the product to which it is applied. The concentration of SnO2 is generally used in the range of 5wt% to 20wt%.
[0005] For this reason, a method has been proposed for suppressing the increase in contact resistance of Ag-SnO2-In2O3-based electrical contact materials. Patent Document 1 proposes an electrical contact material in which the iron-based metal Co (cobalt) is added to an Ag-SnO2-based electrical contact material. In Patent Document 1, when manufacturing an electrical contact material using an internal oxidation method, not only Sn but also Co is added to Ag. This allows the Co oxide to form a conjugate with SnO2, resulting in a contact with stable contact resistance. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 60-36636 Summary of the Invention [Problem to be solved by the invention]
[0007] Incidentally, Ag in Ag-SnO2-based electrical contact materials is resistant to oxidation, but is susceptible to sulfurization. Therefore, in an environment where the air contains a small amount of sulfur dioxide (SO2), the material discolors and the contact resistance increases. The technology described in Patent Document 1 can suppress the increase in contact resistance caused by arcing during interruption, but does not disclose the sulfurization resistance of Ag. Therefore, there is a demand for a technology that improves the sulfurization resistance of Ag while suppressing the increase in contact resistance.
[0008] The present disclosure has been made in view of the above, and has an object to provide an electrical contact material that can improve sulfidation resistance compared to conventional materials while suppressing an increase in contact resistance of the contacts due to arcing during interruption. [Means for solving the problem]
[0009] In order to solve the above problems and achieve the object, the electrical contact material according to the present disclosure comprises: An electrical contact material used for contacts of a control device, comprising:It is characterized in that Fe oxide particles, mainly composed of FeO, are contained in the Ag-SnO2 sintered body containing Ag particles and SnO2 particles. Effect of the Invention
[0010] The electrical contact material according to the present disclosure has the effect of suppressing an increase in the contact resistance of the contacts due to arcing during interruption, while improving sulfurization resistance compared to conventional materials. [Brief description of the drawings]
[0011] [Figure 1] Ellingham diagram showing the standard Gibbs energies of formation for Fe and Sn oxides at various temperatures [Diagram 2] Diagram showing the oxidation states of Fe and Sn [Diagram 3] FIG. 1 is a diagram showing an example of a method for controlling oxygen partial pressure in a method for producing an electrical contact material according to the first embodiment. [Figure 4] FIG. 1 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in a method for producing an electrical contact material according to the first embodiment. [Diagram 5] FIG. 3 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the first embodiment. [Figure 6] FIG. 3 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the first embodiment. [Figure 7] FIG. 3 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the first embodiment. [Figure 8] FIG. 1 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in a method for producing an electrical contact material according to the first embodiment. [Figure 9] FIG. 3 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the first embodiment. [Figure 10] FIG. 3 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the first embodiment. [Figure 11]FIG. 3 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the first embodiment. [Figure 12] FIG. 1 is a perspective view showing an example of a configuration of a two-layer molded body. [Figure 13] FIG. 1 is a schematic diagram showing an example of the configuration of a heat treatment device used in a method for producing an electrical contact material according to a first embodiment; [Figure 14] FIG. 1 is a front view showing a schematic example of a configuration of a circuit breaker using an electrical contact material according to a first embodiment; [Figure 15] FIG. 15 is a cross-sectional view showing a schematic example of a circuit breaker using the electrical contact material according to the first embodiment, taken along the line XV-XV of FIG. [Figure 16] FIG. 1 is a cross-sectional view showing an example of the configuration of an electromagnetic switch using the electrical contact material according to embodiment 1. [Figure 17] FIG. 11 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the second embodiment. [Figure 18] FIG. 11 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the second embodiment. [Figure 19] FIG. 11 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the second embodiment. [Figure 20] FIG. 11 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the second embodiment. [Figure 21] FIG. 11 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the second embodiment. [Figure 22] FIG. 11 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the second embodiment. [Figure 23] FIG. 11 is a cross-sectional view showing a schematic example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the second embodiment. [Figure 24] FIG. 1 shows the measurement results of a shielding test of shields using the electrical contact materials produced in Examples 1 to 3 and Comparative Examples 1 to 7. [Diagram 25]A graph showing the resistance increase rate and contact erosion amount in the interruption test of Examples 1 to 3 normalized by the ratio of FeO to SnO2 added, based on Comparative Example 1, which does not contain FeO. [Figure 26] FIG. 13 is a diagram showing an example of a cross-sectional SEM observation result of the electrical contact material of Example 3. [Figure 27] FIG. 1 shows the results of measuring the Sn content in Ag near the contact surface after interruption tests of shields using the electrical contact materials produced in Examples 1 to 3 and Comparative Examples 1 to 7. [Figure 28] FIG. 1 shows the measurement results of a shielding test of shields using electrical contact materials produced in Examples 4 to 6 and Comparative Examples 8 to 11. [Figure 29] FIG. 1 shows the results of measuring the Sn content in Ag near the contact surface after interruption tests of shields using the electrical contact materials produced in Examples 4 to 6 and Comparative Examples 8 to 11. [Diagram 30] FIG. 1 shows the results of environmental testing of shields using electrical contact materials manufactured in Examples 1 to 3 and Comparative Examples 1 and 5 to 7. [Diagram 31] FIG. 1 shows the results of environmental testing of shields using electrical contact materials produced in Examples 4 to 6 and Comparative Examples 8 to 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An electrical contact material, a manufacturing method thereof, a circuit breaker, and an electromagnetic switch according to embodiments of the present disclosure will be described in detail below with reference to the drawings.
[0013] Embodiment 1 The electrical contact material according to the first embodiment contains Fe (iron) oxide particles mainly composed of FeO (iron (II) oxide) which has a reducing effect on SnO2, in an Ag-SnO2 sintered body containing Ag particles and SnO2 particles. That is, in the electrical contact material according to the first embodiment, SnO2 particles and FeO particles coexist in a sintered body of Ag particles. By forming contacts of control devices such as air circuit breakers, electromagnetic switches, and relays with this electrical contact material, the temperature of the contact surface rises sharply when an arc is generated, and the FeO particles near the surface act as an oxidizing agent by the heat, reducing some of the SnO2 particles, and the FeO particles themselves are oxidized to become Fe3O4 particles. Metal Sn reduced from the SnO2 particles is dissolved in the Ag particles. Since some of the SnO2 particles are no longer oxides, the increase in contact resistance on the contact surface is mitigated. At the same time, the reduced Sn dissolves in the Ag particles, forming an Ag-Sn alloy, which is an alloy of Sn and Ag. By adding a few wt% of Sn to Ag, the sulfurization resistance is improved, and the sulfurization resistance of the outermost surface of the contact is improved.
[0014] It is theoretically impossible to manufacture the electrical contact material according to the first embodiment by the internal oxidation method or the powder sintering method, and therefore, controlling the atmosphere during the heat treatment is important. The manufacturing method of the electrical contact material according to the first embodiment will be described below.
[0015] Figure 1 is an Ellingham diagram showing the standard Gibbs energy of formation at each temperature for oxides of Fe and Sn. In this diagram, the horizontal axis shows temperature [℃], the vertical axis on the left shows the Gibbs energy of formation [kcal], and the vertical axis on the right shows the partial pressure of oxygen [atm]. The Ellingham diagram plots the standard Gibbs energy of formation at each temperature for oxides of Fe and Sn. The Ellingham diagram shows what kind of reducing agent should be used at what temperature to reduce a metal oxide to a metal. In addition, for example, for a substance in which two metal materials are mixed, it shows how the reaction will occur, that is, which metal oxidizes or reduces the other metal. In the Ellingham diagram, among the graphs of oxides of multiple metals, the graph shown at the bottom is the more stable oxide. For example, between the reaction system of Fe → FeO and the reaction system of Sn → SnO2, the reaction system of Fe → FeO is located lower. For example, when a mixture of metallic Fe and SnO2 is heated in a state such as the inside of an electrical contact material that is blocked off from the outside air, the metallic Fe removes oxygen from the SnO2 and is oxidized, while the SnO2 is reduced back to metallic Sn.
[0016] In the normal internal oxidation method, oxidation is performed at a pressure of several atmospheres, so the heat treatment atmosphere is 1 atm, which is the top value on the right vertical axis of the graph, and all Sn becomes SnO2 and all Fe becomes Fe2O3 and stabilizes. For this reason, it is impossible to achieve both SnO2 and a state such as FeO, which has a reducing effect.
[0017] What is of interest here is the point in the Ellingham diagram where the reaction system Sn → SnO2 and the reaction system FeO → Fe3O4 are very close to each other. In one example, in the temperature range around 500°C, the reaction system Sn → SnO2 and the reaction system FeO → Fe3O4 become very close to each other.
[0018] Even with the powder sintering method, when manufacturing an Ag-oxide electrical contact material, it is necessary to heat the powder molded body of the material at a temperature of 700°C or higher and 900°C or lower. As explained in Figure 1, the Fe → FeO reaction system has a low Gibbs energy of formation, so the reduction effect of SnO2 is greater than that of the FeO → Fe3O4 reaction system. However, for example, if Ag powder, SnO2 powder, and Fe powder are mixed, molded, and heated in a normal Ar (argon) atmosphere, the Fe reduces the SnO2 at the time of this heat treatment, and it will no longer be an Ag-SnO2 electrical contact material.
[0019] Figure 2 shows the oxidation states of Fe and Sn. In Figure 2, the horizontal axis shows the oxygen partial pressure [atm] under 1 atmosphere, and the vertical axis shows the temperature [℃]. In Figure 2, a graph showing the oxidation state of Sn is superimposed on a graph showing each oxidation state of Fe at a combination of oxygen partial pressure and temperature. It can be seen that the oxygen partial pressure range in which FeO is stable is quite narrow. From Figure 2, it can be seen that when heated in the oxygen partial pressure range in which the state of Fe can be maintained, all of the SnO2 is reduced to Sn. In addition, in the oxygen concentration range in which Fe3O4 or Fe2O3 exists stably, SnO2 can maintain its state even if the temperature is raised, but since Fe2O3 has no reducing properties in the first place, even if it is incorporated into an electrical contact material, the reduction effect of SnO2 cannot be expected.
[0020] Fig. 3 is a diagram showing an example of a method for controlling the oxygen partial pressure in the manufacturing method of the electrical contact material according to the first embodiment. Fig. 3 is a diagram in which the path of controlling the oxygen partial pressure in the manufacturing method of the electrical contact material according to the first embodiment is drawn into the graph shown in Fig. 2. The dashed arrow shows the path of controlling the oxygen partial pressure. The path of controlling the oxygen partial pressure passes through the region R where SnO2 and FeO coexist. In other words, when manufacturing the electrical contact material, it is possible to manufacture an electrical contact material in which SnO2 and FeO coexist by increasing the temperature of the furnace and sintering while controlling the oxygen partial pressure as shown by the dashed line in Fig. 3.
[0021] Therefore, a specific manufacturing method of the electrical contact material according to the first embodiment will be described below. In one example, the raw materials of the electrical contact material are Ag powder, SnO2 powder, and FeO powder, which is an Fe oxide powder. In light of the current-carrying conditions of the product to which it is applied, the concentration of SnO2 in the electrical contact material is determined in consideration of the contact resistance, adhesion resistance, ease of manufacture, and the like. The concentration of SnO2 is generally used in the range of 5 wt% to 20 wt%. Here, an example is taken in which the Ag powder is 83 wt%, and the total of the SnO2 powder and the FeO powder is 17 wt%. The average particle size of the Ag powder can be 5 μm, and the average particle size of the SnO2 powder and the FeO powder can be 1 μm.
[0022] First, a combination of SnO2 powder and FeO powder is mixed for 15 minutes using a dry mixer. Then, Ag powder is added to the mixed powder and mixed for another 15 minutes. This forms a mixed powder of SnO2 powder, FeO powder and Ag powder. The process of forming the mixed powder corresponds to the mixing process.
[0023] Next, the mixed powder and Ag powder are placed in a metal mold in that order to simultaneously mold two layers. This forms a two-layer molded body having a contact layer made of the mixed powder and an Ag layer made of Ag powder. When brazing the circuit breaker electrode to the copper base, if the Ag contact contains oxides, brazing properties will be poor, so an Ag layer that does not contain oxides is molded. The process of forming the two-layer molded body corresponds to the molding process.
[0024] 4 to 11 are cross-sectional views showing an example of a method for forming a two-layer molded body in the method for producing an electrical contact material according to the first embodiment. As shown in FIG. 4, a space 15 for putting powder is formed by a die 11 of a cylindrical mold 10 and a lower punch 12 inserted into a through hole provided in the die 11. The diameter of the cylindrical mold 10 is Φ15 mm, for example. As shown in FIG. 5, a mixed powder 1 of raw material is put into the die 11. As shown in FIG. 6, an abrasive plate 16 scrapes off the excess mixed powder 1 present above the upper surface of the die 11. Thereafter, as shown in FIG. 7, the lower punch 12 is lowered by a predetermined distance to form a gap 15a in the die 11. Next, as shown in FIG. 8, Ag powder 2 is put into the gap 15a formed in the die 11. At this time, the mixed powder 1 put into the die 11 is weighed so that the thickness of the contact layer of the completed contact is 1.5 mm, and the Ag powder 2 spread on the mixed powder 1 is weighed so that the thickness is 1 / 10 of the contact layer. As shown in FIG. 9, the excess Ag powder 2 present above the upper surface of the die 11 is scraped off by a scraping plate 16. Thereafter, as shown in FIG. 10, an upper punch 13 is attached. Then, as shown in FIG. 11, the die 11 is turned upside down and molded at a predetermined molding pressure. In one example, the molding pressure is 640 MPa. As a result, a two-layer molded body is formed.
[0025] Fig. 12 is a perspective view showing an example of the configuration of a two-layer molded body. As shown in Fig. 12, the two-layer molded body 30 has a cylindrical shape and has a contact layer 31 formed by the mixed powder 1 and an Ag layer 32 formed by the Ag powder 2 on one end surface of the contact layer 31.
[0026] After the two-layer molded body 30 is formed, a heat treatment is performed while controlling the oxygen partial pressure. Fig. 13 is a diagram showing a schematic example of a configuration of a heat treatment apparatus used in the manufacturing method of an electrical contact material according to embodiment 1. The heat treatment apparatus 50 includes a horizontal annular furnace 51, a heater 52, a temperature controller 53, an extremely low oxygen partial pressure control device 54, an Ar gas cylinder 55, a pipe 56, a gas pipe 57, and a valve 58.
[0027] The furnace tube of the horizontal annular furnace 51 is made of alumina, for example. The heater 52 is provided at the center of the horizontal annular furnace 51 in the extending direction, and the upper part can be opened and closed. The temperature controller 53 is connected to the heater 52 and controls the heater 52 so that the temperature inside the horizontal annular furnace 51 in which the heater 52 is provided is set to a predetermined temperature. The horizontal annular furnace 51 and the extremely low oxygen partial pressure control device 54 are connected by a gas pipe 57 so as to form a circulation path in which the oxygen-containing gas from the extremely low oxygen partial pressure control device 54 returns to the extremely low oxygen partial pressure control device 54 via the horizontal annular furnace 51. The Ar gas cylinder 55 is connected to the extremely low oxygen partial pressure control device 54 via a pipe 56. A valve 58 is provided on the gas pipe 57.
[0028] In the heat treatment apparatus 50 having such a configuration, Ar gas supplied from an Ar gas cylinder 55 is introduced into a horizontal annular furnace 51 via an extremely low oxygen partial pressure control device 54. The Ar gas introduced into the horizontal annular furnace 51 is returned again to the extremely low oxygen partial pressure control device 54 via a gas pipe 57 from the opposite end.
[0029] The two-layer molded body 30 is placed on an alumina plate with the Ag layer 32 facing down, and the alumina plate on which the two-layer molded body 30 is placed is inserted into a horizontal annular furnace 51 of a heat treatment device 50. Next, a valve 58 at the end of the horizontal annular furnace 51 is opened, and the gas in the gas pipe 57 and the horizontal annular furnace 51 is replaced with Ar gas. Thereafter, the internal atmosphere is adjusted to 1 atm with Ar gas, and the extremely low oxygen partial pressure control device 54 is operated to reflux the Ar gas until the internal oxygen partial pressure reaches 1×10 -27 Wait until the oxygen partial pressure becomes extremely low, about 1×10 atm. After the oxygen partial pressure becomes stable, the temperature of the horizontal tube furnace 51 is increased to 500°C at a heating rate of 5°C / min. Then, the oxygen partial pressure is controlled in accordance with the oxygen partial pressure control path shown in FIG. 3 so as not to reduce SnO2, i.e., at 550°C, 1×10 -24 atm, and 1×10 -23 atm, and 1×10 -21The temperature and oxygen partial pressure in the furnace are controlled so that the oxygen partial pressure is 7.3×10 atm. That is, the temperature of the horizontal annular furnace 51 is gradually increased while taking care that the oxygen partial pressure falls within the region R shown in FIG. 3 where SnO2 and FeO coexist. This is equivalent to heat treating the two-layer molded body 30 under oxygen partial pressure and temperature conditions that maintain the form of FeO without reducing SnO2. Then, at 900°C, 7.3×10 -15 After reaching atm, sintering is carried out in this state for 2 hours.
[0030] After sintering, the furnace temperature was gradually lowered while paying attention to the oxygen partial pressure as in the case of the temperature rise, and the sintering temperature was increased to 1×10 at 500°C as in the case of the temperature rise. -27 Then, the power supply to the heater 52 of the horizontal circular furnace 51 is stopped, and after waiting for the temperature to drop to 400° C., the top of the heater 52 is opened, and 1×10 -27 The furnace core tube of the horizontal annular furnace 51 is cooled while maintaining the low oxygen partial pressure of atm. Then, after waiting until the actual temperature of the furnace core tube becomes 50°C or less, the extremely low oxygen partial pressure control device 54 is stopped, the Ar gas in the horizontal annular furnace 51 is exhausted, and the two-layer molded body 30 is taken out. The process of heat-treating the two-layer molded body 30 by controlling the oxygen partial pressure and temperature so that SnO2 and FeO coexist corresponds to the heat treatment process.
[0031] The electrical contact material constituting the contact layer 31 of the two-layer molded body 30 thus manufactured is in a state in which SnO2 and FeO coexist. As described above, when manufactured by a method such as powder sintering, SnO2 and FeO do not coexist, and SnO2 is reduced to Sn. In other words, a state in which SnO2 and FeO contained in Ag coexist cannot be obtained by a normal method.
[0032] The two-layer molded body 30 taken out of the horizontal annular furnace 51 is processed by a wire-type electric discharge machine into the shape of contacts of control devices such as air circuit breakers, electromagnetic switches, and relays. Here, the case of processing into the shape of contacts for circuit breakers will be described. Circuit breaker contacts include movable contacts and fixed contacts. In one example, the movable contacts are processed by a wire-type electric discharge machine into 4×6 mm and the fixed contacts into 5×5 mm. Next, the processed contacts are welded to the copper electrodes of the circuit breaker by resistance heating using a silver solder material. An example of the silver solder material is BAg-7 (Ag-Cu(copper)-Zn(zinc)-Sn system). BAg-7 is a silver solder specified in Z 3261:1998 of the Japanese Industrial Standards (JIS). JIS Z 3261:1998 corresponds to the international standard 3677:1992 (MOD) established by the International Organization for Standardization (ISO). The reason for using an automatic welding machine capable of rapid heating and rapid cooling is to suppress the reaction between SnO2 and FeO inside the contacts caused by the temperature rise of the contacts during welding. After that, the brazed contacts are assembled into a circuit breaker.
[0033] Next, a circuit breaker and an electromagnetic switch using the electrical contact material according to the first embodiment will be described. FIG. 14 is a front view showing a schematic example of the configuration of a circuit breaker using the electrical contact material according to the first embodiment. FIG. 15 is a cross-sectional view showing a schematic example of the configuration of a circuit breaker using the electrical contact material according to the first embodiment, taken along the line XV-XV of FIG. 14. In FIG. 14 and FIG. 15, in a plane in which the fixed contactor 71 is arranged, the extension direction of the fixed contactor 71 is defined as the X-axis direction, and the direction perpendicular to the X-axis direction is defined as the Y-axis direction. The direction perpendicular to the X-axis direction and the Y-axis direction is defined as the Z-axis direction.
[0034] The circuit breaker 70 includes a fixed contact 71 extending in the X-axis direction, a movable contact 73 movable in the ZX-plane direction, and an arc-extinguishing insulating material molded body 75. The fixed contact 71 has a fixed contact 72 at one end in the extension direction of the fixed contact 71 on a surface facing the movable contact 73. The movable contact 73 has a movable contact 74. The movable contact 74 is provided at a position corresponding to the fixed contact 72 on a surface facing the fixed contact 71. The above-mentioned electrical contact material is used for the fixed contact 72 and the movable contact 74. In a state where the movable contact 74 is in contact with the fixed contact 72, the movable contact 73 has a shape extending in the X-axis direction. In one example, the movable contact 73 is fixed to be rotatable in the ZX-plane direction at an end opposite to the end where the movable contact 74 of the movable contact 73 is provided.
[0035] The arc-extinguishing insulating material molded body 75 is disposed at a position exposed to an arc generated between the movable contact 74 and the fixed contact 72 when the movable contact 74 and the fixed contact 72 are separated. In the example of Fig. 14 and Fig. 15, the arc-extinguishing insulating material molded body 75 is disposed on both sides of the fixed contact 71 and the movable contact 73 in the Y-axis direction. This configuration of the circuit breaker 70 can mitigate the increase in contact resistance caused by the deposition of SnO2 on the contact surface and the sulfurization of Ag.
[0036] 16 is a cross-sectional view showing an example of the configuration of an electromagnetic switch using the electrical contact material according to embodiment 1. An electromagnetic switch 90 includes a mounting base 91a made of an insulating material, and a fixed core 92 made of laminated silicon steel plates fixed to the mounting base 91a.
[0037] The electromagnetic switch 90 includes a base 91b also made of an insulating material, a fixed contact 93 attached to the base 91b, a movable core 94, an operation coil 95, and a crossbar 96. The movable core 94 is an iron core made of laminated silicon steel plates like the fixed core 92, and both iron cores are arranged facing each other. When excited, the operation coil 95 generates a driving force that attracts the fixed core 92 and the movable core 94 against a tripping spring 97. The crossbar 96 is made of an insulating material and has a square window 98. The crossbar 96 holds the movable core 94 at its lower end.
[0038] The electromagnetic switch 90 includes a movable contact 99, a pressure spring 100, a terminal screw 101, and an arc cover 102. The movable contact 99 is inserted into a square window 98 of the crossbar 96 and is held by the pressure spring 100. The fixed contact 93 is provided opposite the movable contact 99, and when the two contact each other, a current flows. A movable contact 103 is joined to the movable contact 99, and a fixed contact 104 is joined to the fixed contact 93. The above-mentioned electrical contact material is used for the movable contact 103 and the fixed contact 104. The terminal screw 101 is used to connect the electromagnetic switch 90 to an external circuit. The arc cover 102 is provided with an arc extinguishing chamber 102a. In the electromagnetic switch 90, an arc 107 is generated between the movable contact 103 and the fixed contact 104. This configuration of the electromagnetic switch 90 can mitigate the increase in contact resistance caused by the deposition of SnO2 on the contact surfaces and the sulfurization of Ag.
[0039] The electrical contact material of the first embodiment is made by mixing Fe oxide particles, mainly composed of FeO, which has a reducing effect on SnO2, into the Ag-SnO2 sintered body. This makes it possible to reduce the oxide SnO2 by heating only using FeO, utilizing the difference in oxidation potential between FeO and SnO2, and suppress the increase in contact resistance of the contact. In addition, when the contact is subjected to heat from an arc, the FeO particles act as an oxidizing agent, reducing a portion of the SnO2 particles, and suppressing the deposition of SnO2 on the surface. This makes it possible to alleviate the increase in contact resistance due to the deposition of SnO2 on the contact surface. Furthermore, when the contact is subjected to heat from an arc, the FeO particles act as an oxidizing agent, reducing a portion of the SnO2 particles, and further includes a component in which the reduced Sn and Ag particles are alloyed. This configuration makes it possible to alleviate the increase in contact resistance due to the sulfurization of Ag on the contact surface.
[0040] Also, by performing heat treatment according to the combination of temperature and oxygen partial pressure conditions that allow FeO and SnO2 to coexist, it is possible to manufacture an electrical contact material without oxidizing FeO and reducing SnO2. That is, it is possible to manufacture a contact in which SnO2 and FeO coexist. As a result, it is possible to obtain an electrical contact material that can suppress an increase in contact resistance of the contact due to arcing during interruption, while improving sulfurization resistance compared to conventional contact materials. That is, by forming a contact made of an electrical contact material containing FeO particles and SnO2 particles in an extremely low oxygen atmosphere, it is possible to suppress an increase in the resistance of the contact during a current test and improve sulfurization resistance.
[0041] Embodiment 2 In the first embodiment, a method for producing an electrical contact material was described in which Fe oxide particles mainly composed of FeO, which has a reducing effect on SnO2, are mixed into Ag-SnO2 using Ag powder, SnO2 powder, and FeO powder. In the second embodiment, a method for producing an electrical contact material was described in which Fe oxide particles mainly composed of FeO are mixed into Ag-SnO2 sintered body using Ag powder, SnO2 powder, and Fe oxide powder, Fe3O4 powder or Fe2O3 powder.
[0042] The raw materials of the electrical contact material are, for example, Ag powder, SnO2 powder, and Fe3O4 powder. Here, an example is taken in which the Ag powder is 87 wt%, and the total of the SnO2 powder and the Fe3O4 powder is 13 wt%. The average particle size of the Ag powder can be 5 μm, and the average particle size of the SnO2 powder and the Fe3O4 powder can be 1 μm.
[0043] First, a combination of SnO2 powder and Fe3O4 powder is mixed for 15 minutes using a dry mixer. Then, Ag powder is added to the mixed powder and mixed for another 15 minutes. This results in a mixed powder of SnO2 powder, Fe3O4 powder, and Ag powder.
[0044] Next, the mixed powder is placed in a cylindrical mold 10 with a diameter of 15 mm, weighed so that the thickness of the target contact point is 1.5 mm when the density is 100%, and molded lightly with a predetermined molding pressure so that the powder does not crumble. In one example, the molding pressure is 400 MPa. This forms a molded body.
[0045] Next, the molded body is placed on an alumina plate, and the alumina plate on which the molded body is placed is inserted into a horizontal annular furnace 51 made of alumina of a heat treatment device 50. The heat treatment device used in the second embodiment has a similar configuration to the heat treatment device 50 shown in FIG. 13 of the first embodiment, but the configuration of the heater 52 is different. In the heat treatment device used in the second embodiment, the heating area is divided into three in the longitudinal direction of the horizontal annular furnace 51, and a heater 52 capable of separately controlling each heating area is used. The molded body that serves as the contact point is placed in the central heating area. In addition, oxygen getter materials are placed in the heating areas on both sides. An example of the oxygen getter material is a metal Al (aluminum) foil piece cut into about 1 cm square. Here, the heat treatment in the heat treatment device 50 will be described using the symbols in FIG. 13 of the first embodiment.
[0046] Thereafter, the valve 58 at the end of the horizontal annular furnace 51 is opened, and the gas in the gas pipe 57 and the horizontal annular furnace 51 is replaced with Ar gas. Next, the internal atmosphere is adjusted to 1 atm with Ar gas, and the extremely low oxygen partial pressure control device 54 is operated to reflux the Ar gas, and the internal oxygen partial pressure becomes 1×10 -27 The oxygen partial pressure is then waited until it becomes extremely low, around 1000 atm. After the oxygen partial pressure has stabilized, the temperature of the horizontal annular furnace 51 is increased to 500°C at a heating rate of 5°C / min to start the first sintering. When the temperature exceeds 500°C in this extremely low oxygen region, Fe3O4 begins to be reduced to FeO, causing the oxygen partial pressure to fluctuate in the increasing direction. For this reason, the heater 52 in the central heating area is controlled to gradually increase the furnace temperature after waiting for the oxygen partial pressure to sufficiently settle. The heaters 52 in the heating areas on both sides are maintained at 500°C. At this time, the controlled oxygen partial pressure is also increased little by little at the same time as the temperature is increased. In order to prevent SnO2 from being reduced, that is, the central heating area is heated to 1×10 -24 atm, and 1×10 -23atm, and 1×10 -21 The temperature and oxygen partial pressure in the furnace are controlled so that the oxygen partial pressure is within the region R in FIG. 3, where SnO2 and FeO coexist. The temperature of the horizontal circular furnace 51 is gradually increased. Then, at 750° C., the oxygen partial pressure is 1.5×10 -18 After the oxygen partial pressure reaches 1 atm, the mixture is sintered for 48 hours while maintaining this condition.
[0047] In the first sintering, the sintering temperature is set to be 200°C or more lower than the melting point of Ag in order to prevent liquid phase sintering. In the second embodiment, the density of the original molded body is lowered so that the O2 gas separated from Fe3O4 during the temperature rise can easily escape from the molded body. If the sintering temperature is raised to near the melting point of Ag, the hollow parts in the molded body will be surrounded by molten Ag and become closed pores, forming low-density contacts. For this reason, sintering is performed at a temperature at which liquid phase sintering does not occur.
[0048] After sintering, the furnace temperature was gradually lowered while paying attention to the oxygen partial pressure as in the case of the temperature rise, and the sintering temperature was increased to 1×10 at 500°C as in the case of the temperature rise. -27 The oxygen partial pressure is then reduced to 1×10 atm. Then, the power to the three heaters 52 of the horizontal tube furnace 51 is stopped, and after waiting for the temperature to drop to 400° C., the top of the heaters 52 is opened, and 1×10 -27 The furnace tube of the horizontal circular furnace 51 is cooled while maintaining the low oxygen partial pressure of atm. Then, after waiting until the actual temperature of the furnace tube drops to 50° C. or less, the extremely low oxygen partial pressure control device 54 is stopped, the Ar gas in the furnace is exhausted, and the molded body is removed.
[0049] Thereafter, a two-layer molded body 30 is formed by adding an Ag layer to one surface of the molded body taken out. FIG. 17 to FIG. 23 are cross-sectional views that show an example of a method for forming a two-layer molded body in the manufacturing method of an electrical contact material according to the second embodiment. As shown in FIG. 17, a space 15b for putting a molded body 31a is formed by a die 11 of a cylindrical mold 10 and a lower punch 12 inserted into a through hole provided in the die 11. As shown in FIG. 18, the molded body 31a is inserted into the die 11. Next, as shown in FIG. 19 and FIG. 20, Ag powder 2 is put on the molded body 31a in the die 11. At this time, the Ag powder 2 put into the die 11 is weighed so as to be 1 / 10 of the intended thickness of the molded body 31a. Thereafter, as shown in FIG. 21, the excess of the Ag powder 2 present above the upper surface of the die 11 is scraped off by a scraping plate 16. Next, as shown in Fig. 22, an upper punch 13 is attached. Then, as shown in Fig. 23, the die 11 is turned upside down and molded at a predetermined molding pressure. In one example, the molding pressure is 640 MPa. This results in the formation of a two-layer molded body. The two-layer molded body has a contact layer and an Ag layer, and the contact layer is made of a sintered body that has been sintered once.
[0050] Next, the two-layer molded body 30 is placed on an alumina plate with the Ag layer facing down, and the alumina plate on which the two-layer molded body is placed is inserted into a horizontal annular furnace 51 of a heat treatment device 50. Here again, a heat treatment device 50 is used in which the heating area is divided into three and the heating areas can be temperature-controlled separately. The two-layer molded body that serves as the contact point is placed in the central heating area. In addition, oxygen getter materials are placed in the heating areas on both sides. An example of the oxygen getter material is a metal Al foil piece cut into a size of about 1 cm square.
[0051] Thereafter, the valve 58 at the end of the horizontal annular furnace 51 is opened, and the gas in the gas pipe 57 and the horizontal annular furnace 51 is replaced with Ar gas. Next, the internal atmosphere is adjusted to 1 atm with Ar gas, and the extremely low oxygen partial pressure control device 54 is operated to reflux the Ar gas, and the internal oxygen partial pressure becomes 1×10 -27Wait until the oxygen partial pressure becomes extremely low, about 1000 atm. After the oxygen partial pressure becomes stable, the temperature of the horizontal circular furnace 51 is raised to 500°C at a heating rate of 5°C / min to start the second sintering. After that, in order to prevent SnO2 from being reduced, that is, at 550°C, 1×10 -24 atm, and 1×10 -23 atm, and 1×10 -21 The temperature and oxygen partial pressure inside the furnace are controlled so that the oxygen partial pressure is 7.3×10 atm. That is, the temperature of the horizontal annular furnace 51 is gradually increased while taking care that the oxygen partial pressure falls within the region R shown in FIG. 3 where SnO2 and FeO coexist. In the first sintering, the temperature is not raised above 750°C, so the temperature is gradually increased while taking care of the oxygen partial pressure value, and each time the oxygen partial pressure increases, the temperature is waited for to return to the set value before increasing the temperature again. Then, at 900°C, 7.3×10 -15 After reaching atm, sintering is carried out in this state for 2 hours.
[0052] After sintering, the furnace temperature was gradually lowered while paying attention to the oxygen partial pressure as in the case of the temperature rise, and the sintering temperature was increased to 1×10 at 500°C as in the case of the temperature rise. -27 The oxygen partial pressure is then reduced to 1×10 atm. Then, the power to the three heaters 52 of the horizontal circular furnace 51 is stopped, the top of the heaters 52 is opened, and 1×10 -27 The furnace tube of the horizontal annular furnace 51 is cooled while maintaining the low oxygen partial pressure of atm. Then, after waiting until the actual temperature of the furnace tube becomes 50°C or less, the extremely low oxygen partial pressure control device 54 is stopped, the Ar gas in the furnace is exhausted, and the two-layer molded body is taken out. As described above, in the first and second sintering, while maintaining SnO2, heat treatment is performed under oxygen partial pressure and temperature conditions that reduce Fe3O4 or Fe2O3 to FeO, and a molded body containing SnO2 and FeO is formed. In other words, a two-layer molded body is manufactured that includes a contact layer made of an electrical contact material in which SnO2 particles and FeO particles coexist.
[0053] The two-layer molded body removed from the horizontal annular furnace 51 is machined by a wire-type electric discharge machine into the shape of contacts for control devices such as air circuit breakers, electromagnetic switches, and relays. Here, the molded body is machined into the shape of contacts for circuit breakers. Circuit breaker contacts include movable contacts and fixed contacts, and in one example, the movable contacts are machined by the wire-type electric discharge machine to be 4 x 6 mm and the fixed contacts are machined to be 5 x 5 mm. Next, the machined contacts are welded to the copper electrodes of the circuit breaker by resistance heating using silver solder BAg-7. The brazed contacts are then assembled into a circuit breaker.
[0054] In the above description, the Fe3O4 powder having an average particle size of 1 μm is used as the raw material powder. However, Fe2O3 powder having an average particle size of 1 μm may be used instead of the Fe3O4 powder.
[0055] In the second embodiment, a molded body containing Fe3O4 or Fe2O3 and SnO2 is reduced to FeO in an oxygen partial pressure region where SnO2 is not reduced, and finally an electrical contact material in which SnO2 and FeO coexist is obtained. This makes it possible to obtain an electrical contact material that can improve sulfurization resistance compared to conventional contact materials while suppressing an increase in contact resistance of the contact due to arcing during interruption. By forming a contact containing FeO and SnO2 in an extremely low oxygen atmosphere, it is possible to suppress an increase in contact resistance during a current test and to improve sulfurization resistance. In addition, by performing a heat treatment under oxygen partial pressure and temperature conditions that reduce Fe3O4 or Fe2O3 to FeO while maintaining SnO2, and forming a molded body containing SnO2 and FeO, it is possible to mitigate an increase in contact resistance due to the volume of SnO2 on the contact surface. EXAMPLES
[0056] (Method of manufacturing electrical contact materials) [Example 1] Ag powder with an average particle size of 5 μm, SnO2 powder with an average particle size of 1 μm, and FeO powder with an average particle size of 1 μm are prepared as raw materials for the electrical contact material, and the electrical contact material is manufactured by the method described in the first embodiment. In the first embodiment, the Ag powder is 83 wt%, the SnO2 powder is 13.1 wt%, and the FeO powder is 3.9 wt%. Also, by the method described in the first embodiment, a movable contact with a size of 4×6 mm and a fixed contact with a size of 5×5 mm are processed from the electrical contact material, and a shield is assembled.
[0057] [Example 2] Example 2 is similar to Example 1, except that the Ag powder is 83 wt%, the SnO2 powder is 10.63 wt%, and the FeO powder is 6.37 wt%.
[0058] [Example 3] Example 3 is similar to Example 1, except that the Ag powder is 83 wt%, the SnO2 powder is 8.5 wt%, and the FeO powder is 8.5 wt%.
[0059] [Comparative Example 1] As raw materials for the electrical contact material, Ag powder with an average particle size of 5 μm and SnO2 powder with an average particle size of 1 μm are prepared. In Comparative Example 1, the Ag powder and the SnO2 powder are 83 wt% and 17 wt%, respectively. In Comparative Example 1, the Ag powder and the SnO2 powder are mixed for 30 minutes, and then the two-layer molded body 30 is formed by the method described in the first embodiment, and the two-layer molded body 30 is sintered in Ar gas at 900° C. for 2 hours to produce the electrical contact material. That is, sintering is performed without controlling the oxygen partial pressure as in the first embodiment. Also, by the method described in the first embodiment, a movable contact with a size of 4×6 mm and a fixed contact with a size of 5×5 mm are processed from the electrical contact material to assemble a shield.
[0060] [Comparative Example 2] Comparative Example 2 is the same as Comparative Example 1, except that FeO powder is added as a raw material for the electrical contact material. In Comparative Example 2, the Ag powder is 83 wt%, the SnO2 powder is 13.1 wt%, and the FeO powder is 3.9 wt%.
[0061] [Comparative Example 3] Comparative Example 3 is similar to Comparative Example 2, except that the Ag powder is 83 wt%, the SnO2 powder is 10.63 wt%, and the FeO powder is 6.37 wt%.
[0062] [Comparative Example 4] Comparative Example 4 is similar to Comparative Example 2, except that the Ag powder is 83 wt%, the SnO2 powder is 8.5 wt%, and the FeO powder is 8.5 wt%.
[0063] [Comparative Example 5] Comparative Example 5 is similar to Comparative Example 2, except that the FeO powder of Comparative Example 2 is replaced with Fe3O4 powder having an average particle size of 1 μm.
[0064] [Comparative Example 6] Comparative Example 6 is similar to Comparative Example 3, except that the FeO powder of Comparative Example 3 is replaced with Fe3O4 powder.
[0065] [Comparative Example 7] Comparative Example 7 is similar to Comparative Example 4, except that the FeO powder of Comparative Example 4 is replaced with Fe3O4 powder.
[0066] [Example 4] As raw materials for the electrical contact material, Ag powder with an average particle size of 5 μm, SnO2 powder with an average particle size of 1 μm, and Fe3O4 powder with an average particle size of 1 μm are prepared, and the electrical contact material is manufactured by the method described in the second embodiment. In the fourth embodiment, the Ag powder is 87 wt%, the SnO2 powder is 10 wt%, and the Fe3O4 powder is 3 wt%. Also, by the method described in the second embodiment, a movable contact with a size of 4×6 mm and a fixed contact with a size of 5×5 mm are processed from the electrical contact material, and a shield is assembled.
[0067] [Example 5] Example 5 is similar to Example 4, except that the Ag powder is 87 wt%, the SnO2 powder is 8.13 wt%, and the Fe3O4 powder is 4.88 wt%.
[0068] [Example 6] Example 6 is similar to Example 5, except that the Fe3O4 powder in Example 5 is replaced with Fe2O3 powder having an average particle size of 1 μm.
[0069] [Comparative Example 8] In Comparative Example 8, the Ag powder is 87 wt% and the SnO2 powder is 13 wt%. After mixing the Ag powder and the SnO2 powder for 30 minutes, the two-layer molded body 30 is formed by the method described in the first embodiment, and the two-layer molded body 30 is sintered once in Ar gas at 900°C for two hours. In other words, one sintering is performed instead of two sinterings in which the oxygen partial pressure is controlled as in the second embodiment. Also, by the method described in the second embodiment, a movable contact having a size of 4 x 6 mm and a fixed contact having a size of 5 x 5 mm are processed from the electrical contact material, and a shield is assembled.
[0070] [Comparative Example 9] In Comparative Example 9, the Ag powder was 87 wt%, the SnO2 powder was 10 wt%, and the Fe3O4 powder was 3 wt%, and the two-layer molded body 30 was formed by the method described in the first embodiment, which is the same as Comparative Example 8.
[0071] [Comparative Example 10] Comparative Example 10 is similar to Comparative Example 9, except that the Ag powder is 87 wt%, the SnO2 powder is 8.13 wt%, and the Fe3O4 powder is 4.88 wt%.
[0072] [Comparative Example 11] Comparative Example 11 is similar to Comparative Example 9, except that the Ag powder is 87 wt%, the SnO2 powder is 6.5 wt%, and the Fe3O4 powder is 6.5 wt%.
[0073] (Shielding test) [Examples 1 to 3, Comparative Examples 1 to 7] The assembled circuit breaker is subjected to an interruption test under the conditions of AC 300V and 5kA. In order to reduce the individual differences in the circuit breaker's mechanical parts, the contacts are energized from the closed state, i.e., the closed state, and the contacts are opened by the action of the overcurrent detection tripping device inside the circuit breaker. In addition, the phase of the test current is controlled in accordance with the timing of the start of closing, so that the opening starts at the point of maximum current. The test is performed three times under the same conditions. The amount of contact wear due to the interruption test is calculated from the remaining area before and after the interruption test. In addition, the resistance between the circuit breaker's terminals before and after the interruption test is measured. The amount of contact wear is measured by observing the cross-section of the contacts before and after the interruption test using a scanning electron microscope (SEM). The results of these measurements are then averaged. In the following, the cross-sectional observation using SEM is referred to as cross-sectional SEM. Furthermore, elemental analysis is performed on Ag near the surface of the circuit breaker contacts after the interruption test. Elemental analysis is performed on 10 arbitrary points within a range of 100 μm deep from the surface of the contacts, and the average value is calculated.
[0074] FIG. 24 is a diagram showing the measurement results of the shielding test of the shields using the electrical contact materials manufactured in Examples 1 to 3 and Comparative Examples 1 to 7. FIG. 24 shows the results when the number of tests n is 3. FIG. 24 also shows the ratio of the raw material powders and the sintering atmosphere of the electrical contact materials in Examples 1 to 3 and Comparative Examples 1 to 7. In the sintering atmosphere, "Ar (extremely low oxygen)" indicates that sintering is performed while controlling the oxygen partial pressure and temperature so that SnO2 and FeO coexist. Also, "Ar" indicates that sintering is performed without controlling the oxygen partial pressure and temperature.
[0075] The inter-terminal resistance increases when a current is passed through the electrical contact material produced under any of the conditions, but the resistance increase rate is clearly lower in Examples 1 to 3 than in Comparative Example 1, which did not contain Fe oxide mainly composed of FeO. It is confirmed that, among the contacts obtained by heat treatment under extremely low oxygen partial pressure, those with a higher FeO content have a smaller resistance increase rate, but the amount of wear of the contacts tends to increase.
[0076] Comparative Examples 2 to 4 use the same raw materials as Examples 1 to 3, but the heat treatment atmosphere is different. In other words, since the heat treatment is not performed to control the oxygen partial pressure so that SnO2 and FeO coexist, FeO reduces SnO2 during the heat treatment, and the terminal resistance tends to be larger than Examples 1 to 3 from the beginning. In addition, Comparative Examples 2 to 4 do not show the effect of suppressing the increase in terminal resistance. Comparative Examples 5 to 7, which use Fe3O4 powder instead of FeO powder as the raw material powder, are similar to Comparative Examples 2 to 4. The amount of wear of the contacts is larger in Comparative Examples 2 to 4 than in Examples 1 to 3. This is thought to be because FeO reduces SnO2 during the heat treatment, which reduces the arc-proof component SnO2, and the wear of the contacts increases during the interruption test.
[0077] FIG. 25 is a diagram in which the resistance rise rate and the contact erosion amount in the interruption test of Examples 1 to 3 at the ratio of the amount of FeO added to SnO2 are standardized with Comparative Example 1 not containing FeO as a reference. In this figure, the horizontal axis indicates the ratio of the amount of FeO added to SnO2, and the vertical axis indicates the change amount when the contact not containing FeO is set to 1. This figure also shows the average value. From this figure, the change amount of the resistance rise decreases up to the ratio of the amount of FeO added to SnO2 of 0.6, and when it exceeds 0.6, the change amount of the resistance rise becomes almost the same. Also, the change amount of the contact erosion amount increases as the ratio of the amount of FeO added to SnO2 increases. From this, when the ratio of the amount of FeO added to SnO2 is 0.6 times, a contact with a good balance between the effect of suppressing the resistance rise and the effect of suppressing the amount of contact erosion is possible.
[0078] Fig. 26 is a diagram showing an example of a cross-sectional SEM observation result of the electrical contact material of Example 3. Fig. 26 shows the electrical contact material before the shielding test. In this figure, the black parts are FeO, the gray parts are SnO2, and the whitest parts are Ag. It can be seen that SnO2 and FeO are present along the grain boundaries of Ag. Such characteristics are also observed in other Examples.
[0079] In addition, when the vicinity of the contact surface after the interruption test is observed by cross-sectional SEM, segregation of melted and resolidified Ag and oxides progresses. FIG. 27 is a diagram showing the measurement results of the Sn content in Ag near the contact surface after the interruption test of the shield using the electrical contact material manufactured in Examples 1 to 3 and Comparative Examples 1 to 7. FIG. 27 shows the results when the number n of the locations where elemental analysis was performed is 10. FIG. 27 also shows the ratio of the raw material powder of the electrical contact material in Examples 1 to 3 and Comparative Examples 1 to 7. From FIG. 27, it was confirmed that Sn was contained in the Ag of the samples in Examples 1 to 3 and Comparative Examples 2 to 4. In Comparative Examples 2 to 4, it is considered that Sn was diffused in the Ag before the interruption test. In addition, Sn was not contained in the Ag of the samples in Comparative Examples 1, 5 to 7.
[0080] [Examples 4 to 6, Comparative Examples 8 to 11] The assembled circuit breaker is subjected to an interruption test under the conditions of AC300V and 3.5kA. When checking the wear amount of the contacts with a cross-sectional SEM, if the wear amount is small, the measurement error becomes large, so the interruption test is performed twice for each contact. As in Examples 1 to 3 and Comparative Examples 1 to 7, in order to reduce the individual differences in the mechanical parts of the circuit breaker, the contacts are energized from a closed state, i.e., a closed state, and the contacts are opened by the action of a tripping device for detecting overcurrent inside the circuit breaker. In addition, the phase of the test current is controlled in accordance with the timing of the start of closing, so that the opening starts at the point of maximum current. The test is performed three times under the same conditions. The amount of wear of the contacts due to the interruption test is calculated from the remaining area observed using a cross-sectional SEM before and after the interruption test. In addition, the resistance between the terminals of the circuit breaker is measured before and after the interruption test. The results of these measurements are then averaged. Furthermore, elemental analysis is performed on Ag near the surface of the circuit breaker contacts after the interruption test. Elemental analysis is performed on 10 arbitrary points within a depth range of 100 μm from the surface of the contacts, and the average value is calculated.
[0081] FIG. 28 is a diagram showing the measurement results of the shielding test of the shields using the electrical contact materials manufactured in Examples 4 to 6 and Comparative Examples 8 to 11. FIG. 28 shows the results when the number of tests n is 3. FIG. 28 also shows the ratio of the raw material powders and the sintering atmosphere of the electrical contact materials in Examples 4 to 6 and Comparative Examples 8 to 11. In the sintering atmosphere, "Ar (extremely low oxygen), sintered twice" indicates that sintering is performed twice while controlling the oxygen partial pressure and temperature so that SnO2 and FeO coexist as described in the second embodiment. Also, "Ar" indicates that sintering is performed without controlling the oxygen partial pressure and temperature.
[0082] The inter-terminal resistance increases with current flow in all electrical contact materials manufactured under all conditions, but the resistance increase rate is clearly lower in Examples 4 to 6 compared to Comparative Example 8. Among contacts obtained by heat treatment under extremely low oxygen partial pressure, those with a higher Fe3O4 content tend to have a smaller resistance increase rate. Contacts using Fe2O3 powder as the raw material also tend to have a smaller resistance increase rate. Example 5, which uses Fe3O4 powder as the raw material, and Example 6, which uses Fe2O3 powder as the raw material, have the same effect. On the other hand, the difference in the amount of contact erosion was small even when the Fe3O4 content increased. This may be due to the low test current.
[0083] Comparative Examples 9 and 10 use the same raw materials as Examples 4 and 5, respectively, but the heat treatment atmosphere is different, but the effect of suppressing the increase in resistance between terminals is not observed. Also, in Comparative Example 11, the Fe3O4 content is further reduced compared to Comparative Example 10, but the effect of suppressing the increase in resistance between terminals is not observed.
[0084] In addition, when the vicinity of the contact surface after the interruption test is observed by cross-sectional SEM, segregation of melted and resolidified Ag and oxides progresses. FIG. 29 is a diagram showing the measurement result of the Sn content in Ag near the contact surface after the interruption test of the shield using the electrical contact material manufactured in Examples 4 to 6 and Comparative Examples 8 to 11. FIG. 29 shows the result when the number n of the points where the elemental analysis was performed is 10. FIG. 29 also shows the ratio of the raw material powder and the sintering atmosphere of the electrical contact material in Examples 4 to 6 and Comparative Examples 8 to 11. From FIG. 29, it is confirmed that the Ag of the samples of Examples 4 to 6 contains Sn. However, it is confirmed that the Ag of the samples of Comparative Examples 8 to 11 does not contain Sn.
[0085] (Environmental test for sulfur resistance) [Examples 1 to 6, Comparative Examples 1, 5 to 11] For each of the cases of Examples 1 to 3 and Comparative Examples 1 and 5 to 7 in which the interruption test was performed and the inter-terminal resistance was measured, the circuit breaker was placed in an H2S (hydrogen sulfide) gas test tank for 4 days at a temperature of 25°C, humidity of 75%, and concentration of 10 ppm. The inter-terminal resistance after removing the circuit breaker was measured, and the rate of increase in resistance compared to before it was placed in the test tank was confirmed.
[0086] Fig. 30 shows the measurement results of the environmental test of the shields using the electrical contact materials manufactured in Examples 1 to 3 and Comparative Examples 1, 5 to 7. Fig. 30 shows the results when the number of tests n is 3. Fig. 30 also shows the ratio of the raw material powder and the sintering atmosphere of the electrical contact materials in Examples 1 to 3 and Comparative Examples 1, 5 to 7. An increase in contact resistance due to sulfurization of the Ag contact was observed under all conditions, but it was confirmed that the rate of increase was particularly low for the electrical contact materials manufactured in Examples 1 to 3.
[0087] FIG. 31 shows the measurement results of the environmental test of the shield using the electrical contact materials manufactured in Examples 4 to 6 and Comparative Examples 8 to 11. FIG. 31 shows the results when the number of tests n is 3. FIG. 31 also shows the ratio of the raw material powder and the sintering atmosphere of the electrical contact materials in Examples 4 to 6 and Comparative Examples 8 to 11. Although the increase in contact resistance due to sulfurization of the Ag contact was observed under all conditions, it is confirmed that the increase rate is particularly low for the electrical contact materials manufactured in Examples 4 to 6. Moreover, the effect of sulfurization resistance is the same in Example 5, which uses Fe3O4 powder as the raw material, and Example 6, which uses Fe2O3 powder as the raw material.
[0088] From the above, by forming a contact containing FeO and SnO2 in an extremely low oxygen atmosphere, it is possible to suppress the increase in contact resistance during an electric current test and to improve sulfurization resistance. In addition, by reducing a contact containing Fe3O4 or Fe2O3 and SnO2 from Fe3O4 or Fe2O3 to FeO in an oxygen partial pressure region where SnO2 is not reduced, and finally forming a contact where SnO2 and FeO coexist, it is also possible to suppress the increase in contact resistance during an electric current test and to improve sulfurization resistance.
[0089] The configurations shown in the above embodiments are merely examples, and may be combined with other known technologies, or the embodiments may be combined with each other. Also, parts of the configurations may be omitted or modified without departing from the spirit of the invention. [Explanation of symbols]
[0090] 1 mixed powder, 2 Ag powder, 10 cylindrical mold, 11 die, 12 lower punch, 13 upper punch, 15,15b space, 15a gap, 16 scraping plate, 30 two-layer molded body, 31 contact layer, 31a molded body, 32 Ag layer, 50 heat treatment device, 51 horizontal circular furnace, 52 heater, 53 temperature controller, 54 extremely low oxygen partial pressure control device, 55 Ar gas cylinder, 56 piping, 57 gas piping, 58 valve, 70 circuit breaker, 71,93 fixed contact, 72,104 fixed contact, 73,99 moving contact, 74,103 moving contact, 90 electromagnetic switch.
Claims
1. An electrical contact material used for contacts of a control device, comprising: Ag particles and SnO 2 Ag—SnO particles 2 An electrical contact material comprising a sintered body containing Fe oxide particles mainly composed of FeO.
2. The SnO 2 2. The electrical contact material according to claim 1, wherein the ratio of the amount of FeO added to the amount of particles is 0.6 times.
3. When exposed to heat from an arc, the FeO acts as an oxidizer, and the SnO 2 Part of the particles is reduced to SnO 2 3. The electrical contact material according to claim 1, wherein the electrical contact material inhibits deposition of the above-mentioned on the surface of the electrical contact.
4. When exposed to heat from an arc, the FeO acts as an oxidizer, and the SnO 2 4. The electrical contact material according to claim 1, further comprising a component obtained by reducing a portion of the particles and alloying the reduced Sn with the Ag particles.
5. A circuit breaker comprising a contact made of the electrical contact material according to any one of claims 1 to 4.
6. 5. An electromagnetic switch comprising a contact made of the electrical contact material according to claim 1.
7. A method for producing an electrical contact material used for contacts of a control device, comprising the steps of: SnO 2 a mixing step of mixing the powder, the Fe oxide powder and the Ag powder to form a mixed powder; a molding step of molding the mixed powder to form a molded body; SnO 2 a heat treatment step of heat treating the molded body by controlling the oxygen partial pressure and temperature so that FeO and FeO coexist; A method for producing an electrical contact material, comprising:
8. The Fe oxide powder is FeO powder, In the heat treatment step, SnO 2 8. The method for producing an electrical contact material according to claim 7, further comprising heat-treating the molded body under oxygen partial pressure and temperature conditions that maintain the form of FeO without reducing FeO.
9. The Fe oxide powder is Fe 3 O 4 Powder or Fe 2 O 3 It is a powder, In the heat treatment step, SnO 2 While maintaining 3 O 4 Or Fe 2 O 3 Heat treatment is performed under oxygen partial pressure and temperature conditions that reduce SnO to FeO. 2 and FeO.
Citation Information
Patent Citations
Method for manufacturing sliver oxidized tin contactor materials
CN1925078A
Electrical contact point material consisting of silver-tin oxide alloy
JP1985036636A
Silver-iron oxide sintered electrical contact material
JP1989055345A
Optical information recording and reproducing device
JP1997050646A
POWDER FOR Ag / SnO2 ELECTRIC CONTACT, Ag / SnO2 ELECTRIC CONTACT MATERIAL AND MANUFACTURING METHOD THEREFOR
JP2015196902A