Gas barrier laminate, coating liquid for producing the same, packaging material, package, and packaged article

A coating liquid with specific components forms a gas barrier laminate that addresses peeling issues in high humidity and temperature conditions, ensuring durable and effective gas barrier performance.

JP7585630B2Active Publication Date: 2024-11-19TOPPAN HOLDINGS INC
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020105783
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-19
Publication Date
2024-11-19
Estimated Expiration
2040-06-19

AI Technical Summary

Technical Problem

Existing gas barrier laminates face issues with peeling between the gas barrier coating layer and adjacent layers, such as adhesive or sealant layers, in high temperature and high humidity environments, and require multiple steps or high-temperature heat treatments, limiting their application and durability.

Method used

A coating liquid comprising a carboxyl group-containing polymer, polyvalent metal-containing particles, surfactant, organic solvent, and silicon-containing compounds, with specific mass ratios and water content, is used to form a gas barrier laminate that prevents peeling and maintains integrity under harsh conditions.

Benefits of technology

The laminate exhibits excellent gas barrier properties and adhesion in high humidity and temperature environments, maintaining integrity and preventing peeling, even after heat sterilization processes like boiling or retorting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585630000001
    Figure 0007585630000001
Patent Text Reader

Abstract

To provide a gas barrier laminate capable of preventing peeling between a gas barrier coat layer and a layer adjacent thereto from occurring.SOLUTION: A coating liquid for manufacturing a gas barrier laminate includes: a carboxyl group containing polymer (A); polyvalent metal containing particles (B); a surfactant (C); an organic solvent (D); and at least one kind of silicon containing compounds (E) selected from a group consisting of a silane coupling agent represented by the general formula (1), a silane coupling agent represented by the general formula (2), these hydrolysates and these condensates. The mass ratio of the silicon containing compound (E) to the carboxyl group containing polymer (A) is 0.5% or more. Si(OR1)3Z1...(1) and Si(R2)(OR3)2Z2...(2), (where, R1 and R3 are a 1-6C alkyl group, R2 is a methyl group, and Z1 and Z2 are a group including an epoxy group.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas barrier laminate. [Background technology]

[0002] Food, medicine, cosmetics, agricultural chemicals, industrial products, and other items may deteriorate in quality due to oxygen when stored for a long period of time. For this reason, films and sheets with oxygen gas barrier properties are used as packaging materials for these items.

[0003] Conventionally, such packaging materials have often been used that have aluminum foil as a gas barrier layer. However, when using packaging materials that contain aluminum foil, the contents cannot be visually confirmed, and metal detectors cannot be used. Therefore, there has been a demand for development of packaging materials that have excellent gas barrier properties and are transparent, particularly in the food and pharmaceutical fields.

[0004] In response to such demands, gas barrier laminates have been used in which a layer made of polyvinylidene chloride (PVDC) is provided on a substrate by applying a coating liquid containing PVDC. The layer made of PVDC is transparent and has gas barrier properties.

[0005] However, there are concerns that PVDC generates dioxins when incinerated. Therefore, there has been a demand to switch from PVDC to non-chlorine-based materials. In response to this demand, for example, the use of polyvinyl alcohol (PVA)-based polymers instead of PVDC has been proposed.

[0006] A layer made of a PVA-based polymer is densified by hydrogen bonds of hydroxyl groups, and exhibits high gas barrier properties in a low humidity atmosphere. However, a layer made of a PVA-based polymer has a problem that hydrogen bonds are loosened by moisture absorption in a high humidity atmosphere, and gas barrier properties are significantly reduced. Therefore, gas barrier laminates using a layer made of a PVA-based polymer as a gas barrier layer often cannot be used as packaging materials for foods containing a lot of moisture, and their applications have been limited to packaging materials for dry foods, etc.

[0007] In order to further improve the gas barrier property, it has been proposed to add an inorganic layered compound to a PVA-based polymer (see Patent Document 1). However, even if an inorganic layered compound is added, the water resistance of the PVA-based polymer itself is not improved, and the problem of reduced gas barrier property in a high humidity atmosphere still remains.

[0008] In order to improve the gas barrier property under a high humidity atmosphere, it has been proposed to produce a gas barrier laminate by applying a coating liquid containing a PVA-based polymer and a polymer capable of forming a crosslinked structure with the PVA-based polymer to a substrate and then heat treating the substrate (see Patent Documents 2 to 6).

[0009] However, in order to obtain sufficient gas barrier properties using these techniques, it is necessary to perform a heat treatment after application of the coating liquid at a high temperature, for example, 150°C or higher, to form a crosslinked structure. Such a heat treatment can cause severe deterioration of the substrate depending on the substrate material, for example, when the substrate material is a polyolefin such as polypropylene (OPP) or polyethylene (PE). Therefore, there is a demand for a gas barrier laminate that can be produced under milder conditions.

[0010] As a method for forming a gas barrier layer, a method has been proposed in which a layer containing a polycarboxylic acid polymer such as polyacrylic acid is formed and the polycarboxylic acid polymer is ionically crosslinked with polyvalent metal ions (see Patent Documents 7 and 8).

[0011] This method does not require the high-temperature heat treatment performed in the methods described in Patent Documents 2 to 6. Therefore, polyolefin can be used as the substrate. In addition, the obtained gas barrier layer has excellent gas barrier properties even in a high humidity atmosphere. Therefore, the gas barrier laminate including this gas barrier layer can be used in applications where heat sterilization treatment such as boiling or retorting is performed.

[0012] However, when a polycarboxylic acid polymer and a polyvalent metal compound are allowed to coexist in a coating liquid, the polycarboxylic acid polymer and the polyvalent metal compound react with each other in the coating liquid, and precipitation is likely to occur. If precipitation occurs in the liquid, a uniform film cannot be formed. Therefore, in this method, when forming a gas barrier layer, a layer containing a polycarboxylic acid polymer and a layer containing a polyvalent metal compound are formed separately, or an aqueous solution of a polyvalent metal salt is brought into contact with the layer containing a polycarboxylic acid polymer. Therefore, this method has a problem in that more steps are required.

[0013] It has been proposed to set the water content of a coating liquid containing a polycarboxylic acid polymer, polyvalent metal compound particles, a surfactant, and an organic solvent to 1000 ppm or less (see Patent Document 9). In this coating liquid, the water content is 1000 ppm or less, so that the reaction between the polycarboxylic acid polymer and the polyvalent metal compound is suppressed. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] Japanese Patent Application Publication No. 6-093133 [Patent Document 2] JP 2000-289154 A [Patent Document 3] JP 2000-336195 A [Patent Document 4] JP 2001-323204 A [Patent Document 5] JP 2002-020677 A [Patent Document 6] JP 2002-241671 A [Patent Document 7] International Publication No. 2003 / 091317 [Patent Document 8] International Publication No. 2005 / 053954 [Patent Document 9] JP 2005-126528 A Summary of the Invention [Problem to be solved by the invention]

[0015] Patent Document 9 describes that the coating liquid disclosed therein can form a film with excellent gas barrier properties even under high-humidity conditions. However, in a more severe high-temperature and high-humidity environment, a laminate formed by applying this coating liquid may experience peeling between the gas barrier coat layer applied with the coating liquid and an adjacent layer, such as an adhesive layer or a sealant layer, resulting in a decrease in gas barrier properties.

[0016] The present invention aims to provide a gas barrier laminate in which peeling is unlikely to occur between a gas barrier coating layer and an adjacent layer, such as an adhesive layer or a sealant layer, in a high-temperature and high-humidity environment. [Means for solving the problem]

[0017] According to a first aspect of the present invention, there is provided a composition comprising a carboxy group-containing polymer (A), a polyvalent metal-containing particle (B), a surfactant (C), an organic solvent (D), and at least one silicon-containing compound (E) selected from the group consisting of a silane coupling agent represented by the following general formula (1), a silane coupling agent represented by the following general formula (2), their hydrolysates, and their condensates, wherein the mass ratio of the silicon-containing compound (E) to the carboxy group-containing polymer (A) (wherein the mass of the silicon-containing compound (E) is calculated as the mass of the silane coupling agent) is 0.5% or more. The moisture content is 50,000 ppm or less by mass fraction. The present invention provides a coating liquid for producing a gas barrier laminate.

[0018] Si(OR1)3Z1 …(1) Si(R2)(OR3)2Z2 …(2) (In general formula (1), R1 may be the same or different and is an alkyl group having 1 to 6 carbon atoms, and Z1 is a group containing an epoxy group; in general formula (2), R2 is a methyl group, R3 may be the same or different and is an alkyl group having 1 to 6 carbon atoms, and Z2 is a group containing an epoxy group.) According to a second aspect of the present invention, there is provided the coating liquid according to the first aspect, wherein the mass ratio is 20% or less.

[0019] According to a third aspect of the present invention, there is provided a coating liquid according to the first or second aspect, in which a ratio of the product (Bt) of the number of moles and the valence of the polyvalent metal contained in the polyvalent metal-containing particles (B) to the number of moles (At) of carboxy groups contained in the carboxy group-containing polymer (A) is 0.6 or more.

[0020] According to a fourth aspect of the present invention, there is provided the coating liquid according to any one of the first to third aspects, wherein the carboxyl group-containing polymer (A) is a homopolymer of a carboxyl group-containing unsaturated monomer, a copolymer of two or more kinds of carboxyl group-containing unsaturated monomers, a copolymer of a carboxyl group-containing unsaturated monomer and another polymerizable monomer, a carboxyl group-containing polysaccharide, or a mixture of two or more of these.

[0021] According to a fifth aspect of the present invention, there is provided the coating liquid according to any one of the first to fourth aspects, wherein the carboxyl group-containing unsaturated monomer constituting the carboxyl group-containing polymer (A) is at least one α,β-monoethylenically unsaturated carboxylic acid selected from the group consisting of acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid, and fumaric acid.

[0022] According to a sixth aspect of the present invention, there is provided the coating liquid according to any one of the first to fifth aspects, wherein the polyvalent metal-containing particles (B) have an average particle size within the range of 10 nm to 10 μm.

[0023] According to a seventh aspect of the present invention, there is provided the coating liquid according to any one of the first to sixth aspects, wherein the polyvalent metal of the polyvalent metal-containing particles (B) is a divalent metal.

[0024] According to an eighth aspect of the present invention, there is provided a method for producing a gas barrier laminate, the method comprising forming a coating layer from the coating liquid according to any one of the first to seventh aspects.

[0025] According to a ninth aspect of the present invention, there is provided a gas barrier laminate obtained by the production method according to the eighth aspect.

[0026] According to a tenth aspect of the present invention, there is provided a packaging material including the gas barrier laminate according to the ninth aspect.

[0027] According to an eleventh aspect of the present invention there is provided a package comprising the packaging material according to the ninth aspect.

[0028] According to a twelfth aspect of the present invention, there is provided a packaged article including a package according to the eleventh aspect and contents contained in the package. Effect of the Invention

[0029] According to the present invention, it is possible to provide a gas barrier laminate in which peeling is unlikely to occur between a gas barrier coating layer and an adjacent layer, for example, either an adhesive layer or a sealant layer, in a high-temperature and high-humidity environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following describes embodiments of the present invention, which are specific embodiments of any of the above aspects.

[0031] <Coating solution for manufacturing gas barrier laminate> The coating liquid for producing a gas barrier laminate according to an embodiment of the present invention (hereinafter, also simply referred to as the coating liquid) contains a carboxy group-containing polymer (A), polyvalent metal-containing particles (B), a surfactant (C), an organic solvent (D), and at least one silicon-containing compound (E) selected from the group consisting of a silane coupling agent represented by the following general formula (1), a silane coupling agent represented by the following general formula (2), their hydrolysates, and their condensates, and is characterized in that the mass ratio of the silicon-containing compound (E) to the carboxy group-containing polymer (A) is 0.5% or more. Si(OR1)3Z1 …(1) Si(R2)(OR3)2Z2 …(2) Here, the mass of the silicon-containing compound (E) is the mass calculated based on the silane coupling agent. In addition, in the general formula (1), R1 is an alkyl group having 1 to 6 carbon atoms, which may be the same or different, and Z1 is a group containing an epoxy group. In the general formula (2), R2 is a methyl group, R3 is an alkyl group having 1 to 6 carbon atoms, which may be the same or different, and Z2 is a group containing an epoxy group.

[0032] [Carboxy Group-Containing Polymer (A)] The carboxyl group-containing polymer used in the coating liquid is a polymer having two or more carboxyl groups in the molecule, and is sometimes called a "polycarboxylic acid polymer." Representative examples of the carboxyl group-containing polymer include a homopolymer of a carboxyl group-containing unsaturated monomer, a copolymer of two or more kinds of carboxyl group-containing unsaturated monomers, a copolymer of a carboxyl group-containing unsaturated monomer and another polymerizable monomer, and a polysaccharide containing a carboxyl group in the molecule (also called a "carboxyl group-containing polysaccharide" or an "acidic polysaccharide").

[0033] The carboxy group includes not only a free carboxy group but also an acid anhydride group (specifically, a dicarboxylic acid anhydride group). The acid anhydride group may be partially ring-opened to form a carboxy group. A part of the carboxy group may be neutralized with an alkali. In this case, the degree of neutralization is preferably 20% or less.

[0034] Here, the "degree of neutralization" is a value obtained by the following method. That is, the carboxyl groups can be partially neutralized by adding an alkali (F) to the carboxyl group-containing polymer (A). In this case, the ratio of the number of moles (Ft) of the alkali (F) to the number of moles (At) of the carboxyl groups contained in the carboxyl group-containing polymer (A) is the degree of neutralization.

[0035] In addition, a graft polymer obtained by graft polymerizing a carboxyl-containing unsaturated monomer onto a polymer not containing a carboxyl group, such as polyolefin, can also be used as the carboxyl-containing polymer. A polymer obtained by hydrolyzing a polymer having a hydrolyzable ester group, such as an alkoxycarbonyl group (e.g., a methoxycarbonyl group), to convert it into a carboxyl group can also be used.

[0036] The carboxyl group-containing unsaturated monomer is preferably an α,β-monoethylenically unsaturated carboxylic acid. Therefore, the carboxyl group-containing polymer includes a homopolymer of an α,β-monoethylenically unsaturated carboxylic acid, a copolymer of two or more kinds of α,β-monoethylenically unsaturated carboxylic acids, and a copolymer of an α,β-monoethylenically unsaturated carboxylic acid and another polymerizable monomer. The other polymerizable monomer is typically an ethylenically unsaturated monomer.

[0037] Examples of α,β-monoethylenically unsaturated carboxylic acids include unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid; unsaturated dicarboxylic anhydrides such as maleic anhydride and itaconic anhydride; and mixtures of two or more of these. Among these, at least one α,β-monoethylenically unsaturated carboxylic acid selected from the group consisting of acrylic acid, methacrylic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid is preferred, and at least one α,β-monoethylenically unsaturated carboxylic acid selected from the group consisting of acrylic acid, methacrylic acid, and maleic acid is more preferred.

[0038] Other polymerizable monomers copolymerizable with α,β-monoethylenically unsaturated carboxylic acid, particularly ethylenically unsaturated monomers, include, for example, ethylene; α-olefins such as propylene, 1-butene, 1-pentene, 1-hexene, and 1-octene; saturated carboxylic acid vinyl esters such as vinyl acetate; acrylic acid alkyl esters such as methyl acrylate and ethyl acrylate; methacrylic acid alkyl esters such as methyl methacrylate and ethyl methacrylate; chlorine-containing vinyl monomers such as vinyl chloride and vinylidene chloride; fluorine-containing vinyl monomers such as vinyl fluoride and vinylidene fluoride; unsaturated nitriles such as acrylonitrile and methacrylonitrile; aromatic vinyl monomers such as styrene and α-methylstyrene; and itaconic acid alkyl esters. These ethylenically unsaturated monomers can be used alone or in combination of two or more. In addition, when the carboxy group-containing polymer is a copolymer of an α,β-monoethylenically unsaturated carboxylic acid and a saturated carboxylic acid vinyl ester such as vinyl acetate, a copolymer obtained by saponifying this copolymer to convert the saturated carboxylic acid vinyl ester units into vinyl alcohol units can also be used.

[0039] Examples of the carboxyl group-containing polysaccharides include acidic polysaccharides having a carboxyl group in the molecule, such as alginic acid, carboxymethylcellulose, and pectin. These acidic polysaccharides can be used alone or in combination of two or more. The acidic polysaccharides can also be used in combination with a (co)polymer of an α,β-monoethylenically unsaturated carboxylic acid.

[0040] When the carboxy group-containing polymer is a copolymer of an α,β-monoethylenically unsaturated carboxylic acid and another ethylenically unsaturated monomer, from the viewpoints of the gas barrier properties, hot water resistance, and water vapor resistance of the resulting film, the proportion of the number of moles of the α,β-monoethylenically unsaturated carboxylic acid monomer to the total number of moles of those monomers in the copolymer is preferably 60 mol % or more, more preferably 80 mol % or more, and particularly preferably 90 mol % or more.

[0041] The carboxyl group-containing polymer is preferably a homopolymer or copolymer obtained by polymerization of only α,β-monoethylenically unsaturated carboxylic acid, in that it is easy to obtain a film having excellent gas barrier properties, moisture resistance, water resistance, hot water resistance, and water vapor resistance, and also excellent gas barrier properties under high humidity conditions. When the carboxyl group-containing polymer is a (co)polymer consisting of only α,β-monoethylenically unsaturated carboxylic acid, its preferred specific examples are homopolymers, copolymers, and mixtures of two or more thereof obtained by polymerization of at least one α,β-monoethylenically unsaturated carboxylic acid selected from the group consisting of acrylic acid, methacrylic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid. Among these, homopolymers and copolymers of at least one α,β-monoethylenically unsaturated carboxylic acid selected from the group consisting of acrylic acid, methacrylic acid, and maleic acid are more preferred.

[0042] As the carboxyl group-containing polymer, polyacrylic acid, polymethacrylic acid, polymaleic acid, and a mixture of two or more of them are particularly preferred. As the acidic polysaccharide, alginic acid is preferred. Among these, polyacrylic acid is particularly preferred because it is relatively easy to obtain and a film having excellent physical properties can be easily obtained.

[0043] The number average molecular weight of the carboxy group-containing polymer is not particularly limited, but from the viewpoint of film formability and film physical properties, the number average molecular weight is preferably in the range of 2,000 to 10,000,000, more preferably in the range of 5,000 to 1,000,000, and even more preferably in the range of 10,000 to 500,000.

[0044] Here, the "number average molecular weight" is a value obtained by measurement using gel permeation chromatography (GPC). In GPC measurement, the number average molecular weight of a polymer is generally measured in terms of standard polystyrene.

[0045] [Polyvalent metal-containing particles (B)] The polyvalent metal-containing particles used in the coating liquid are particles containing one or more polyvalent metals whose metal ions have a valence of 2 or more. The polyvalent metal-containing particles may be particles made of a polyvalent metal whose metal ions have a valence of 2 or more, particles made of a compound of a polyvalent metal whose metal ions have a valence of 2 or more, or a mixture thereof.

[0046] Specific examples of polyvalent metals include, but are not limited to, metals in Group 2A of the short periodic table, such as beryllium, magnesium, and calcium; transition metals, such as titanium, zirconium, chromium, manganese, iron, cobalt, nickel, copper, and zinc; and aluminum.

[0047] The polyvalent metal is preferably a divalent metal, and the polyvalent metal preferably forms a compound.

[0048] Specific examples of polyvalent metal compounds include, but are not limited to, oxides, hydroxides, carbonates, organic acid salts, and inorganic acid salts of polyvalent metals. Examples of organic acid salts include, but are not limited to, acetates, oxalates, citrates, lactates, phosphates, phosphites, hypophosphites, stearates, and monoethylenically unsaturated carboxylates. Examples of inorganic acid salts include, but are not limited to, chlorides, sulfates, and nitrates. Alkyl alkoxides of polyvalent metals can also be used as polyvalent metal compounds. These polyvalent metal compounds can be used alone or in combination of two or more.

[0049] Among the polyvalent metal compounds, from the viewpoints of dispersion stability of the coating liquid and the gas barrier properties of the laminate formed from the coating liquid, compounds of beryllium, magnesium, calcium, copper, cobalt, nickel, zinc, aluminum, and zirconium are preferred, and compounds of divalent metals such as beryllium, magnesium, calcium, copper, zinc, cobalt, and nickel are more preferred.

[0050] Preferred divalent metal compounds include, but are not limited to, oxides such as zinc oxide, magnesium oxide, copper oxide, nickel oxide, and cobalt oxide; carbonates such as calcium carbonate; organic acid salts such as calcium lactate, zinc lactate, and calcium acrylate; and alkoxides such as magnesium methoxide.

[0051] The polyvalent metal or polyvalent metal compound is used as particles, and the particle shape is maintained even in the coating liquid. From the viewpoint of the dispersion stability of the coating liquid and the gas barrier property of the laminate formed from the coating liquid, the average particle diameter of the polyvalent metal-containing particles is preferably within the range of 10 nm to 10 μm (or 10,000 nm), more preferably within the range of 12 nm to 1 μm (or 1,000 nm), even more preferably within the range of 15 nm to 500 nm, and particularly preferably within the range of 15 nm to 50 nm.

[0052] If the average particle size of the polyvalent metal-containing particles in the coating liquid is too large, the uniformity of the film thickness of the resulting coating layer, the flatness of the surface, and the ionic crosslinking reactivity with the carboxyl group-containing polymer are likely to be insufficient. If the average particle size of the polyvalent metal-containing particles is too small, the ionic crosslinking reaction with the carboxyl group-containing polymer may proceed early. In addition, it is difficult to uniformly disperse ultrafine particles with a particle size of less than 10 nm in the coating liquid.

[0053] The average particle size of the polyvalent metal-containing particles can be measured by measuring and counting using a scanning electron microscope or a transmission electron microscope when the sample is a dry solid. The average particle size of the polyvalent metal-containing particles in the coating liquid can be measured by a light scattering method (Reference: "Fine Particle Engineering System", Vol. I, pp. 362-365, Fuji Techno System (2001)).

[0054] The polyvalent metal-containing particles in the coating liquid exist as primary particles, secondary particles, or a mixture of these, but in many cases, judging from the average particle size, it is assumed that they exist as secondary particles.

[0055] [Surfactant (C)] In the above coating liquid, a surfactant is used to enhance the dispersibility of the polyvalent metal-containing particles. A surfactant is a compound having both a hydrophilic group and a lipophilic group in the molecule. The surfactant includes anionic, cationic, and amphoteric ionic surfactants, as well as nonionic surfactants. Any surfactant may be used in the above coating liquid.

[0056] Anionic surfactants include, for example, carboxylic acid type, sulfonic acid type, sulfate type, and phosphate type. Examples of carboxylic acid type anionic surfactants include aliphatic monocarboxylates, polyoxyethylene alkyl ether carboxylates, N-acylsarcosinates, and N-acylglutamates. Examples of sulfonic acid type anionic surfactants include dialkyl sulfosuccinates, alkanesulfonates, alpha olefin sulfonates, linear alkylbenzene sulfonates, alkyl (branched) benzene sulfonates, naphthalene sulfonate-formaldehyde condensates, alkyl naphthalene sulfonates, and N-methyl-N-acyltaurates. Examples of sulfate type anionic surfactants include alkyl sulfates, polyoxyethylene alkyl ether sulfates, and oil sulfates. Examples of phosphate type anionic surfactants include alkyl phosphates, polyoxyethylene alkyl ether phosphates, and polyoxyethylene alkyl phenyl ether phosphates.

[0057] Cationic surfactants include, for example, alkylamine salt type and quaternary ammonium salt type. Cationic surfactants of alkylamine salt type include, for example, monoalkylamine salt, dialkylamine salt, and trialkylamine salt. Cationic surfactants of quaternary ammonium salt type include, for example, alkyltrimethylammonium halide (chloride, bromide, or iodide) salt and alkylbenzalkonium chloride.

[0058] Examples of amphoteric surfactants include carboxybetaine type, 2-alkylimidazoline derivative type, glycine type, and amine oxide type. Examples of carboxybetaine type amphoteric surfactants include alkylbetaine and fatty acid amidopropyl betaine. Examples of 2-alkylimidazoline derivative type amphoteric surfactants include 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine. Examples of glycine type amphoteric surfactants include alkyl or dialkyl diethylenetriaminoacetic acid. Examples of amine oxide type amphoteric surfactants include alkylamine oxide.

[0059] Examples of nonionic surfactants include ester type, ether type, ester ether type, and alkanolamide type. Examples of ester type nonionic surfactants include glycerin fatty acid ester, sorbitan fatty acid ester, and sucrose fatty acid ester. Examples of ether type nonionic surfactants include polyoxyethylene alkyl ether, polyoxyethylene alkyl phenyl ether, and polyoxyethylene polyoxypropylene glycol. Examples of ester ether type nonionic surfactants include fatty acid polyethylene glycol and fatty acid polyoxyethylene sorbitan. Examples of alkanolamide type nonionic surfactants include fatty acid alkanolamide.

[0060] Surfactants having a polymeric backbone, such as styrene-acrylic acid copolymers, can also be used.

[0061] Among these surfactants, anionic surfactants such as phosphate esters, and surfactants having a polymer skeleton such as styrene-acrylic acid copolymers are preferred.

[0062] [Organic solvent (D)] In the coating liquid, an organic solvent is used as a solvent or dispersion medium. As the organic solvent, a polar organic solvent capable of dissolving a carboxyl group-containing polymer is generally used, but an organic solvent having no polar group (heteroatom or atomic group having a heteroatom) may be used in combination with the polar organic solvent.

[0063] Examples of organic solvents that can be preferably used include alcohols such as methanol, ethanol, isopropanol, n-propanol, and n-butanol; and polar organic solvents such as dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, tetramethylurea, hexamethylphosphoric triamide, and γ-butyrolactone.

[0064] In addition to the above polar organic solvents, hydrocarbons such as benzene, toluene, xylene, hexane, heptane, and octane, ketones such as acetone and methyl ethyl ketone, halogenated hydrocarbons such as dichloromethane, esters such as methyl acetate, and ethers such as diethyl ether can be used as appropriate. Hydrocarbons such as benzene that do not have a polar group are generally used in combination with a polar organic solvent.

[0065] The coating liquid may contain only an organic solvent as a solvent or dispersion medium, but may further contain water. By containing water, the solubility of the carboxyl group-containing polymer can be improved, and the coating property and workability of the coating liquid can be improved. The water content of this coating liquid may be 100 ppm or more, 1,000 ppm or more, 1,500 ppm or more, or 2,000 ppm or more by mass fraction.

[0066] The water content of this coating liquid is preferably 50,000 ppm or less, more preferably 10,000 ppm or less, and even more preferably 5,000 ppm or less, in terms of mass fraction.

[0067] [Silicon-containing compounds (E)] In order to increase the peel strength, the coating liquid contains a silicon-containing compound, which is at least one compound selected from the group consisting of a silane coupling agent represented by the following general formula (1), a silane coupling agent represented by the following general formula (2), their hydrolysates, and their condensates. Si(OR1)3Z1 …(1) Si(R2)(OR3)2Z2 …(2) Here, the mass of the silicon-containing compound (E) is the mass calculated based on the silane coupling agent. In addition, in the general formula (1), R1 is an alkyl group having 1 to 6 carbon atoms, which may be the same or different, and Z1 is a group containing an epoxy group. In the general formula (2), R2 is a methyl group, R3 is an alkyl group having 1 to 6 carbon atoms, which may be the same or different, and Z2 is a group containing an epoxy group.

[0068] Silane coupling agents easily undergo hydrolysis, and also easily undergo condensation reaction in the presence of acid or alkali.Therefore, in the above coating liquid, the silicon-containing compound (E) rarely exists only in the form of the silane coupling agent represented by general formula (1) or (2), only in the form of its hydrolyzate, or only in the form of its condensate.That is, in the above coating liquid, the silicon-containing compound (E) is usually mixed as a mixture of at least one of the silane coupling agent represented by general formula (1) and the silane coupling agent represented by general formula (2), its hydrolyzate, and its condensate.

[0069] Each of R1 and R3 may be an alkyl group having 1 to 6 carbon atoms, and is preferably a methyl group or an ethyl group. Each of Z1 and Z2 may be a group containing an epoxy group.

[0070] Specific examples of the silane coupling agent represented by general formula (1) or (2) include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane, and 3-glycidoxypropylmethyldimethoxysilane and 3-glycidoxypropyltrimethoxysilane are preferred. As the silane coupling agent, one type may be used, or two or more types may be used.

[0071] The hydrolysate of the silane coupling agent represented by the general formula (1) or (2) may be a partial hydrolysate, a complete hydrolysate, or a mixture thereof.

[0072] The condensate contained in the coating liquid as at least a part of the silicon-containing compound (E) is at least two of the following: a hydrolysis condensate of a silane coupling agent represented by general formula (1), a hydrolysis condensate of a silane coupling agent represented by general formula (2), and a condensate of a hydrolysis product of a silane coupling agent represented by general formula (1) and a hydrolysis product of a silane coupling agent represented by general formula (2). These hydrolysis condensates are generated by the following reaction. That is, first, the silane coupling agent is hydrolyzed. As a result, one or more of the alkoxy groups contained in the molecule of the silane coupling agent are replaced by hydroxyl groups, and the silane coupling agent becomes a hydrolyzate. Then, these hydrolyzates are condensed to form a compound in which a silicon atom (Si) is bonded via oxygen. This condensation is repeated to obtain a hydrolysis condensate.

[0073] 〔composition〕 The above coating liquid contains a carboxy group-containing polymer (A), polyvalent metal-containing particles (B), a surfactant (C), an organic solvent (D) and a silicon-containing compound (E), and is a dispersion in which the polyvalent metal-containing particles are dispersed.

[0074] The ratio (hereinafter also referred to as equivalent ratio) of the product (Bt) of the number of moles of the polyvalent metal contained in the polyvalent metal-containing particle (B) and the valence to the number of moles (At) of the carboxyl group contained in the carboxyl group-containing polymer (A) is preferably 0.6 or more. This ratio is more preferably 0.8 or more, and particularly preferably 1.0 or more. The upper limit of this ratio is usually 10.0, preferably 2.0. If this ratio is too small, the properties such as gas barrier property, hot water resistance, and water vapor resistance of the laminate formed with the coating layer from the coating liquid are reduced.

[0075] The above-mentioned equivalent ratio can be determined, for example, as follows: An example will be described in which the carboxyl group-containing polymer is polyacrylic acid and the polyvalent metal compound is magnesium oxide.

[0076] Polyacrylic acid has a molecular weight of 72 per monomer unit, and has one carboxy group per monomer molecule. Therefore, the amount of carboxy groups in 100 g of polyacrylic acid is 1.39 moles. The above-mentioned equivalent ratio of 1.0 in a coating liquid containing 100 g of polyacrylic acid means that the coating liquid contains magnesium oxide in an amount that neutralizes 1.39 moles of carboxy groups. Therefore, in order to make the above-mentioned equivalent ratio in a coating liquid containing 100 g of polyacrylic acid 0.6, it is sufficient to add magnesium oxide in an amount that neutralizes 0.834 moles of carboxy groups to the coating liquid. Here, the valence of magnesium is divalent, and the molecular weight of magnesium oxide is 40. Therefore, in order to make the above-mentioned equivalent ratio in a coating liquid containing 100 g of polyacrylic acid 0.6, it is sufficient to add 16.68 g (0.417 moles) of magnesium oxide to the coating liquid.

[0077] The organic solvent is used in an amount sufficient to uniformly dissolve the carboxyl group-containing polymer and uniformly disperse the polyvalent metal-containing particles. Therefore, the organic solvent used is one that dissolves the carboxyl group-containing polymer but does not substantially dissolve the polyvalent metal compound and can disperse it in the form of particles.

[0078] The surfactant is used in an amount sufficient to stably disperse the polyvalent metal-containing particles. The concentration of the surfactant in the coating liquid is usually within the range of 0.0001 to 70% by mass, preferably 0.001 to 60% by weight, and more preferably 0.1 to 50% by mass.

[0079] If a surfactant is not added, it is difficult to disperse the polyvalent metal-containing particles in the coating solution so that their average particle size is sufficiently small, and as a result, it is difficult to obtain a coating solution in which the polyvalent metal-containing particles are uniformly dispersed, and it is difficult to form a coating film with a uniform thickness when applied to a substrate.

[0080] The mass ratio of the silicon-containing compound to the carboxyl group-containing polymer (wherein the mass of the silicon-containing compound is the mass of the silane coupling agent) is preferably 0.5% or more, more preferably 1.0% or more, even more preferably 1.5% or more, and particularly preferably 2.0% or more.

[0081] If the amount of silicon-containing compound added is too small, the peel strength of the gas barrier laminate formed by the coating liquid described above, for example, the laminate formed by forming a coating film of the coating liquid on a support, drying the coating film, and then laminating an adhesive layer and a sealant layer in order on the gas barrier layer, is reduced.Therefore, careful handling is required to prevent interlayer peeling, which leads to a decrease in productivity.

[0082] The mass ratio of the silicon-containing compound to the carboxyl group-containing polymer is preferably 20% or less, more preferably 15% or less, even more preferably 12% or less, and particularly preferably 7% or less.

[0083] Silicon-containing compounds do not have gas barrier properties, and therefore, if the amount of silicon-containing compound added is too large, the gas barrier properties of the laminate formed from the coating liquid are reduced.

[0084] [Method of producing coating liquid] To produce the coating liquid, first, the carboxyl group-containing polymer (A) is uniformly dissolved in the organic solvent (D), and then the silicon-containing compound (E) is added thereto to prepare a carboxyl group-containing polymer solution.

[0085] On the other hand, the polyvalent metal-containing particles (B), the surfactant (C), and the organic solvent (D) are mixed and, if necessary, a dispersion is prepared by carrying out a dispersion treatment. The dispersion treatment is carried out so that the average particle diameter of the polyvalent metal-containing particles (B) becomes a predetermined value. If the average particle diameter of the polyvalent metal-containing particles (B) in the mixed liquid before the dispersion treatment is 10 μm or less, the dispersion treatment may not be carried out, but even in that case, it is preferable to carry out the dispersion treatment. By carrying out the dispersion treatment, the aggregation of the polyvalent metal-containing particles (B) is dissolved, the coating liquid is stabilized, and the transparency of the gas barrier laminate obtained by applying the coating liquid is increased. Furthermore, when the coating liquid is applied and the coating film is dried, the crosslinking between the carboxyl group-containing polymer and the polyvalent metal ions is easily promoted, and a gas barrier laminate having good gas barrier properties is easily obtained.

[0086] Dispersion methods include those using a high-speed stirrer, homogenizer, ball mill, or bead mill. In particular, dispersion using a ball mill or bead mill can achieve high efficiency, and therefore a coating liquid with a stable dispersion state can be obtained in a relatively short time. In this case, the diameter of the balls or beads is preferably small, preferably 0.1 to 1 mm.

[0087] The coating liquid can be prepared by mixing the carboxyl group-containing polymer solution prepared as above with the dispersion of polyvalent metal-containing particles. The silicon-containing compound (E) may be omitted from the carboxyl group-containing polymer solution. In this case, the silicon-containing compound (E) is mixed together, for example, when the carboxyl group-containing polymer solution and the dispersion of polyvalent metal-containing particles are mixed.

[0088] The total concentration of the components other than the organic solvent in the above coating liquid is preferably within the range of 0.1 to 60% by mass, more preferably 0.5 to 25% by mass, and particularly preferably 1 to 20% by mass, in order to obtain a coating film or coat layer of a desired thickness with high workability.

[0089] The above coating liquid may contain various additives, such as other polymers, thickeners, stabilizers, UV absorbers, antiblocking agents, softeners, inorganic layered compounds (e.g., montmorillonite), and colorants (dyes, pigments), as necessary.

[0090] <Gas barrier laminate> The gas barrier laminate according to an embodiment of the present invention comprises a substrate and a gas barrier layer provided on at least one surface of the substrate, and is characterized in that the gas barrier layer includes a coating layer formed from the above-mentioned coating liquid.

[0091] [Base material] There are no particular limitations on the substrate in the gas barrier laminate, and various types of substrates can be used.

[0092] The material constituting the substrate is not particularly limited, and various types of materials can be used, such as plastic or paper.

[0093] The substrate may be a single layer made of a single material, or may be a multi-layer made of multiple materials, such as a substrate in which a plastic film is laminated to paper.

[0094] Of the above materials, plastics are preferred as the material for the substrate, since they can be molded into various shapes and can be given gas barrier properties to further expand the range of applications.

[0095] Examples of plastics include, but are not limited to, polyolefin resins such as polyethylene and polypropylene; polyester resins such as polyethylene terephthalate, polyethylene-2,6-naphthalate, polybutylene terephthalate, and copolymers thereof; polyamide resins such as nylon-6, nylon-66, nylon-12, metaxylylene adipamide, and copolymers thereof; styrene resins such as polystyrene, styrene-butadiene copolymer, and styrene-butadiene-acrylonitrile copolymer; poly(meth)acrylic acid esters; polyacrylonitrile; polyvinyl acetate; ethylene-vinyl acetate copolymer; ethylene-vinyl alcohol copolymer; polycarbonate; polyarylate; regenerated cellulose; polyimide; polyetherimide; polysulfone; polyethersulfone; polyetherketone; and ionomer resins.

[0096] When the gas barrier laminate is used as a food packaging material, the substrate is preferably made of polyethylene, polypropylene, polyethylene terephthalate, nylon-6 or nylon-66.

[0097] As the plastic constituting the substrate, one type may be used alone, or two or more types may be blended and used.

[0098] The plastic may contain additives. The additives may be appropriately selected from known additives such as pigments, antioxidants, antistatic agents, ultraviolet absorbers, and lubricants depending on the application. The additives may be used alone or in combination of two or more.

[0099] The form of the substrate is not particularly limited, and examples thereof include a film, a sheet, a cup, a tray, a tube, and a bottle. Among these, a film is preferable.

[0100] When the substrate is a film, the film may be a stretched film or an unstretched film.

[0101] There are no particular limitations on the thickness of the film, but from the viewpoint of the mechanical strength and processability of the resulting gas barrier laminate, it is preferably in the range of 1 to 200 μm, and more preferably in the range of 5 to 100 μm.

[0102] The surface of the substrate may be subjected to plasma treatment, corona treatment, ozone treatment, flame treatment, or radical activation treatment using ultraviolet (UV) or electron beams, etc., so that the coating liquid can be applied without being repelled by the substrate. The treatment method is appropriately selected depending on the type of substrate.

[0103] [Coat layer] The coating layer is formed from the above coating liquid, specifically, by applying the above coating liquid onto a substrate and drying the coating film. As described above, this coating layer contains a carboxyl group-containing polymer ionically cross-linked with polyvalent metal ions, and exhibits excellent gas barrier properties even in a high humidity atmosphere.

[0104] The coating layer may be provided on one surface or on both surfaces of the substrate. The coating layer may be provided directly on the surface of the substrate, or may be provided on the surface of one or more other layers (for example, an anchor coating layer) provided on the substrate. The method for forming the coating layer will be described in detail later.

[0105] The thickness of the coating layer is not particularly limited, but from the viewpoints of formability and handling during formation of the gas barrier laminate, it is preferably in the range of 0.01 to 100 μm, more preferably in the range of 0.1 to 10 μm, and even more preferably in the range of 0.1 to 0.5 μm.

[0106] [Other layers] The gas barrier laminate may further include one or more layers other than the substrate and the coating layer, if necessary.

[0107] For example, the gas barrier layer of the gas barrier laminate may consist of only a coating layer, or may further include one or more other layers in addition to the coating layer. For example, a layer made of an inorganic compound such as aluminum oxide, silicon oxide, and aluminum may be formed on the surface of a substrate by a sputtering method, an ion plating method, or the like.

[0108] The gas barrier laminate may further include an anchor coat layer between the substrate and the coat layer for the purposes of increasing the adhesion between the substrate and the coat layer and enabling the coating liquid to be applied to the substrate without being repelled by the substrate.

[0109] The anchor coat layer can be formed by a conventional method using a known anchor coat agent.

[0110] Examples of the anchor coating agent include those containing resins such as polyurethane resin, acrylic resin, melamine resin, polyester resin, phenol resin, amino resin, and fluororesin.

[0111] In addition to the resin, the anchor coating agent may further contain an isocyanate compound for the purpose of improving adhesion and hot water resistance. The isocyanate compound may be any compound having one or more isocyanate groups in the molecule, and examples thereof include hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, and tolylene diisocyanate.

[0112] The anchor coating agent may further contain a liquid medium for dissolving or dispersing the resin and the isocyanate compound. The thickness of the anchor coat layer is not particularly limited.

[0113] The gas barrier laminate may, as necessary, further comprise another layer laminated via an adhesive onto the coating layer provided on the substrate, or onto a surface of the substrate on which no coating layer is provided, or may further comprise another layer formed by extrusion lamination of an adhesive resin.

[0114] The other layers to be laminated can be appropriately selected according to the purpose of imparting strength, sealing properties, easy opening when sealed, design, light blocking properties, moisture resistance, etc., and are not particularly limited, but examples thereof include those made of the same material as the plastics described above for the substrate. In addition, paper, aluminum foil, etc. may be used.

[0115] The thickness of the other layer to be laminated is preferably in the range of 1 to 1000 μm, more preferably in the range of 5 to 500 μm, even more preferably in the range of 5 to 200 μm, and particularly preferably in the range of 5 to 150 μm. The other layer to be laminated may be one type or two or more types.

[0116] The gas barrier laminate may further include a printed layer, if necessary. The printed layer may be formed on a coating layer provided on a substrate, or may be formed on a surface of a substrate on which no coating layer is provided. In addition, when another layer is laminated, the printed layer may be formed on the other layer to be laminated.

[0117] [Method for producing gas barrier laminate] The gas barrier laminate can be produced by a production method including a step of forming a coating layer by applying the above-mentioned coating liquid to a substrate and drying the coating film. This production method can further include a step of laminating another layer and a step of forming a print layer, etc., before and / or after the step of forming the coating layer, as necessary.

[0118] The method for applying the coating liquid is not particularly limited, but examples thereof include methods using an air knife coater, a direct gravure coater, a gravure offset coater, an arc gravure coater, a reverse roll coater such as a top feed reverse coater, a bottom feed reverse coater, or a nozzle feed reverse coater, a five-roll coater, a lip coater, a bar coater, a bar reverse coater, or a die coater.

[0119] The method for drying the coating film is not particularly limited, but examples thereof include a method of natural drying, a method of drying in an oven set at a predetermined temperature, and a method using a dryer attached to a coater, such as an arch dryer, a floating dryer, a drum dryer, or an infrared dryer.

[0120] Drying conditions can be appropriately selected depending on the drying method, etc. For example, in a method of drying in an oven, the drying temperature is preferably within the range of 40 to 150° C., more preferably within the range of 45 to 150° C., and particularly preferably within the range of 50 to 140° C. The drying time varies depending on the drying temperature, but is preferably within the range of 0.5 seconds to 10 minutes, more preferably within the range of 1 second to 5 minutes, and particularly preferably within the range of 1 second to 1 minute.

[0121] It is presumed that during or after drying, the carboxyl group-containing polymer contained in the coating film reacts with the polyvalent metal-containing particles to introduce an ionic crosslinking structure. In order to fully advance the ionic crosslinking reaction, it is preferable to age the dried film for about 1 second to 10 days in an atmosphere with a relative humidity of preferably 20% or more, more preferably 40 to 100%, and at a temperature of preferably 5 to 200°C, more preferably 20 to 150°C.

[0122] The gas barrier laminate thus obtained is ionically crosslinked, and therefore has excellent moisture resistance, water resistance, hot water resistance, and water vapor resistance. This gas barrier laminate has excellent gas barrier properties not only under low humidity conditions but also under high humidity conditions. This gas barrier laminate preferably has an oxygen transmission rate of 1,000 cm, measured at 30°C and a relative humidity of 70% according to JIS K-7126 B method (constant pressure method) and the method described in ASTM D3985. 3 / (m 2 ·day·MPa) or less, more preferably 500cm 3 / (m 2·day·MPa) or less, particularly preferably 100 cm 3 / (m 2 The lower the oxygen permeability, the better. There is no particular lower limit for the oxygen permeability, but it is usually 0.1 cm 3 / (m 2 ·day·MPa) or more.

[0123] <Packaging materials, packages and packaged articles> A packaging material according to an embodiment of the present invention includes the gas barrier laminate described above. This packaging material is used, for example, in the production of a package for packaging an article.

[0124] A package according to an embodiment of the present invention includes the above-described packaging material. This package may be made of the above-mentioned packaging material, or may include the above-mentioned packaging material and other members. In the former case, the package may be, for example, the above-mentioned packaging material formed into a bag shape. In the latter case, the package may be, for example, a container including the above-mentioned packaging material as a lid and a cylindrical container body with a bottom.

[0125] In this package, the packaging material may be a molded product. As described above, this molded product may be a container such as a bag, or a part of a container such as a lid. Specific examples of the package or a part thereof include a bag, a spouted pouch, a laminated tube, an infusion bag, a container lid, and a paper container.

[0126] There is no particular limitation on the application of this packaging material, and this packaging material can be used to package various items.

[0127] A packaging article according to an embodiment of the present invention includes the above-described package and contents contained therein.

[0128] As described above, the gas barrier laminate has excellent gas barrier properties. Therefore, the packaging material and package containing this gas barrier laminate are preferably used as packaging materials and packages for items that are easily deteriorated by the influence of oxygen and water vapor, and particularly as packaging materials and packages for food. These packaging materials and packages are also preferably used as packaging materials and packages for packaging chemicals such as agricultural chemicals and medicines, medical equipment, machine parts, and industrial materials such as precision materials.

[0129] The gas barrier laminate does not deteriorate in gas barrier properties or interlayer adhesion when subjected to heat sterilization such as boiling or retort treatment, and tends to improve the gas barrier properties or interlayer adhesion. Therefore, the packaging material and the packaging body may be a packaging material for heat sterilization and a packaging body for heat sterilization, respectively.

[0130] The packaging material for heat sterilization and the package for heat sterilization are used for packaging articles that are to be subjected to a heat sterilization treatment after packaging. Examples of products that are subjected to heat sterilization treatment after packaging include food products such as curry, stew, soup, sauce, and processed meat products.

[0131] Examples of the heat sterilization treatment include boiling and retort treatment. Boiling is a moist heat sterilization process for preserving food and the like. In boiling, a packaged article in which the contents such as food are packaged in the above-mentioned package is usually subjected to moist heat sterilization at atmospheric pressure at a temperature of 60 to 100°C for 10 to 120 minutes, although this depends on the contents. Boiling is usually performed using a hot water bath. There are two types of boiling: a batch type in which the packaged article is immersed in a hot water bath at a constant temperature and removed after a certain time, and a continuous type in which the packaged article is sterilized by passing it through a hot water bath in a tunnel style.

[0132] Retort processing is a process for sterilizing microorganisms such as mold, yeast, and bacteria by pressurizing and heating in order to generally preserve food, etc. In retort processing, a packaged article in which food is packaged in the above-mentioned package is usually subjected to pressurized sterilization and heating treatment at a pressure of 0.15 to 0.3 MPa and a temperature of 105 to 140° C. for 10 to 120 minutes. Retort devices include a steam type that uses heated steam and a hot water type that uses pressurized superheated water, and they are used appropriately depending on the sterilization conditions of the food, etc., that is the content. EXAMPLES

[0133] Specific examples of the present invention are described below. (Example 1) The carboxyl group-containing polymer (A) was dissolved in 2-propanol by heating. Polyacrylic acid (Jurymer (registered trademark) AC-10LP, number average molecular weight 50,000, manufactured by Toa Gosei Co., Ltd.) was used as the carboxyl group-containing polymer (A). In this manner, a polyacrylic acid solution containing polyacrylic acid at a concentration of 10% by mass was prepared.

[0134] 1.8 g of polyether phosphate (Disparlon (registered trademark) DA-325, manufactured by Kusumoto Chemical Industries Co., Ltd., solid content 100% by mass) was dissolved in 26.2 g of 2-propanol. Next, 12 g of zinc oxide (FINEX (registered trademark)-30, manufactured by Sakai Chemical Industry Co., Ltd.) having an average primary particle diameter of 35 nm was added to this and stirred. The obtained liquid was dispersed in a planetary ball mill (P-7, manufactured by Fritsch Co., Ltd.) for 1 hour. Zirconia beads with a diameter of 0.2 mm were used for this dispersion treatment. The beads were then sieved out of this liquid to obtain a dispersion containing zinc oxide at a concentration of 30% by mass.

[0135] Next, 30.64 g of the polyacrylic acid solution, 5.79 g of the zinc oxide dispersion, 0.08 g of a silicon-containing compound (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd., functional group: epoxy group), and 23.57 g of 2-propanol were mixed to prepare coating liquid 1. In this coating liquid 1, the mass ratio of the silicon-containing compound to the carboxyl group-containing polymer was 2.5%.

[0136] This coating liquid 1 was applied to one side of a biaxially stretched polyethylene terephthalate film (Lumirror (registered trademark) P60, manufactured by Toray Film Processing Co., Ltd., thickness 12 μm) using a bar coater (ROD No. 8, manufactured by Yasuda Seiki Seisakusho Co., Ltd., wet film thickness 20 μm). This coating film was dried in an oven at 50° C. for 1 minute to form a coating layer. In this manner, laminate 1 was obtained.

[0137] Next, an unstretched polypropylene film (ZK93-FM, 60 μm thick, manufactured by Toray Film Processing Co., Ltd.) was dry laminated onto the surface of the coating layer side of the laminate 1 via a two-component polyurethane adhesive (Takelac A-525 / Takenate A-52, manufactured by Mitsui Chemicals, Inc.), and aging was performed at 40°C for 3 days to obtain laminate film 1.

[0138] (Example 2) Coating liquid 2 was prepared in the same manner as described above for coating liquid 1, except that the blend amounts were 30.64 g of polyacrylic acid solution, 5.79 g of zinc oxide dispersion, 0.15 g of silicon-containing compound (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd., functional group: epoxy group), and 23.43 g of 2-propanol. In this coating liquid 2, the mass ratio of the silicon-containing compound to the carboxyl group-containing polymer was 5.0%. Except that this coating liquid 2 was used instead of coating liquid 1, laminate 2 was obtained in the same manner as described above for laminate 1. Except that this laminate 2 was used instead of laminate 1, laminate film 2 was obtained in the same manner as in Example 1.

[0139] (Example 3) Coating liquid 3 was prepared in the same manner as described above for coating liquid 1, except that the blend amounts were 30.64 g of polyacrylic acid solution, 5.79 g of zinc oxide dispersion, 0.31 g of silicon-containing compound (KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd., functional group: epoxy group), and 23.26 g of 2-propanol. In this coating liquid 3, the mass ratio of the silicon-containing compound to the carboxyl group-containing polymer was 10.0%. Except that this coating liquid 3 was used instead of coating liquid 1, laminate 3 was obtained in the same manner as described above for laminate 1. Except that this laminate 3 was used instead of laminate 1, laminate film 3 was obtained in the same manner as in Example 1.

[0140] (Example 4) Coating liquid 4 was prepared in the same manner as described above for coating liquid 1, except that the blend amounts were 30.64 g of polyacrylic acid solution, 5.79 g of zinc oxide dispersion, 0 g of silicon-containing compound, and 23.57 g of 2-propanol. In this coating liquid 4, the mass ratio of the silicon-containing compound to the carboxyl group-containing polymer was 0%. Except that this coating liquid 4 was used instead of coating liquid 1, laminate 4 was obtained in the same manner as described above for laminate 1. Except that this laminate 4 was used instead of laminate 1, laminate film 4 was obtained in the same manner as in Example 1.

[0141] (Example 5) Coating liquid 5 was prepared in the same manner as described above for coating liquid 1, except that KBM-603 (manufactured by Shin-Etsu Chemical Co., Ltd., functional group: amino group) was used as the silicon-containing compound instead of KBM-403 (manufactured by Shin-Etsu Chemical Co., Ltd., functional group: epoxy group). In this coating liquid 5, the mass ratio of the silicon-containing compound to the carboxyl group-containing polymer was 2.5%.

[0142] In this example, immediately after the addition of the silicon-containing compound (functional group: amino group), aggregation occurred in the coating liquid 5. Therefore, film formation using this was impossible, and no laminate or laminate film was formed.

[0143] 〔evaluation〕 (1) Peel strength of laminate film Two pieces of film measuring 20 cm x 15 cm were cut out from each of the obtained laminate films, and these were overlapped with the unstretched polypropylene film sides facing each other, and three sides were sealed to prepare a pouch. 200 mL of water was poured into this pouch, and the remaining side was sealed.

[0144] The obtained water-filled pouch was subjected to a retort treatment at 121° C. for 30 minutes using a retort treatment machine (RCS-60 manufactured by Hisaka Works, Ltd.).

[0145] After the retort treatment, the water was removed and each of the laminate films 1 to 4 was cut into a 15 mm wide strip, and the peel strength was measured at a speed of 300 mm / min with a T-shaped peel angle using a Tensilon universal material testing machine (RTC-1250, manufactured by Orientec Co., Ltd.). The results are shown in Table 1. If the peel strength between the layers is strong and exceeds the breaking strength of the substrate, the substrate will break during the peel strength evaluation. Substrates that broke during the evaluation are indicated as "broken" in the table.

[0146] (2) Oxygen permeability of laminated film Two pieces of film measuring 20 cm x 15 cm were cut out from each of the obtained laminate films, and these were overlapped with the unstretched polypropylene film sides facing each other, and three sides were sealed to prepare a pouch. 200 mL of water was poured into this pouch, and the remaining side was sealed.

[0147] The obtained water-filled pouch was subjected to a retort treatment at 121° C. for 30 minutes using a retort treatment machine (RCS-60 manufactured by Hisaka Works, Ltd.).

[0148] After the retort treatment, the water was removed, and the oxygen permeability of each of the laminate films 1 to 4 was measured by the following procedure.

[0149] That is, the oxygen permeability of each laminate was measured under conditions of a temperature of 30° C. and a relative humidity of 70% using an oxygen permeability tester OXTRAN (registered trademark) 2 / 20 manufactured by Modern Control Co., Ltd. The measurement method was in accordance with JIS K-7126 B method (constant pressure method) and ASTM D3985, and the measurement value is in the unit of cm 3 / (m 2 The results are shown in Table 1.

[0150] [Table 1]

[0151] As shown in Table 1, laminate films 1 and 2 were excellent in both peel strength and gas barrier properties. In contrast, laminate film 4 had low peel strength because it was formed using coating liquid 4 that did not contain a silicon-containing compound. In addition, as described above, coating liquid 5 coagulated immediately after the silicon-containing compound (functional group: amino group) was added, making it impossible to form a film using this coating liquid. The invention as originally claimed is set forth below. [1] A coating liquid for producing a gas barrier laminate, comprising: a carboxy group-containing polymer (A), polyvalent metal-containing particles (B), a surfactant (C), an organic solvent (D), and at least one silicon-containing compound (E) selected from the group consisting of a silane coupling agent represented by the following general formula (1), a silane coupling agent represented by the following general formula (2), their hydrolysates, and their condensates, wherein the mass ratio of the silicon-containing compound (E) to the carboxy group-containing polymer (A) (wherein the mass of the silicon-containing compound (E) is calculated as the mass of the silane coupling agent) is 0.5% or more, and the water content is 50,000 ppm or less in terms of mass fraction. Si(OR1) 3 Z1 …(1) Si(R2)(OR3) 2 Z2 …(2) (In general formula (1), R1 may be the same or different and is an alkyl group having 1 to 6 carbon atoms, and Z1 is a group containing an epoxy group; in general formula (2), R2 is a methyl group, R3 may be the same or different and is an alkyl group having 1 to 6 carbon atoms, and Z2 is a group containing an epoxy group.) [2] Item 2. The coating liquid according to item 1, wherein the mass ratio is 20% or less. [3] 3. The coating liquid according to item 1 or 2, wherein a ratio of a product (Bt) of the number of moles and a valence of a polyvalent metal contained in the polyvalent metal-containing particle (B) to a number of moles (At) of a carboxy group contained in the carboxy group-containing polymer (A) is 0.6 or more. [4] 4. The coating liquid according to any one of Items 1 to 3, wherein the carboxyl group-containing polymer (A) is a homopolymer of a carboxyl group-containing unsaturated monomer, a copolymer of two or more kinds of carboxyl group-containing unsaturated monomers, a copolymer of a carboxyl group-containing unsaturated monomer and another polymerizable monomer, a carboxyl group-containing polysaccharide, or a mixture of two or more kinds thereof. [5] 5. The coating liquid according to any one of items 1 to 4, wherein the carboxyl group-containing unsaturated monomer constituting the carboxyl group-containing polymer (A) is at least one α,β-monoethylenically unsaturated carboxylic acid selected from the group consisting of acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid, and fumaric acid. [6] 6. The coating liquid according to any one of items 1 to 5, wherein the polyvalent metal-containing particles (B) have an average particle size within a range of 10 nm to 10 μm. [7] 7. The coating liquid according to any one of Items 1 to 6, wherein the polyvalent metal of the polyvalent metal-containing particles (B) is a divalent metal. [8] Item 8. A method for producing a gas barrier laminate, comprising forming a coating layer from the coating liquid according to any one of Items 1 to 7. [9] Item 9. A gas barrier laminate obtained by the production method according to item 8.

[10] Item 10. A packaging material comprising the gas barrier laminate according to item 9.

[11] Item 11. A package comprising the packaging material according to item 10.

[12] Item 12. A packaged article comprising the package according to item 11 and contents contained in the package.

Claims

1. 1. A coating liquid for producing a gas barrier laminate comprising: a carboxy group-containing polymer (A); polyvalent metal-containing particles (B); a surfactant (C); an organic solvent (D); and at least one silicon-containing compound (E) selected from the group consisting of a silane coupling agent represented by the following general formula (1), a silane coupling agent represented by the following general formula (2), a hydrolysate thereof, and a condensate thereof, wherein the mass ratio of the silicon-containing compound (E) to the carboxy group-containing polymer (A) (wherein the mass of the silicon-containing compound (E) is calculated as the mass of the silane coupling agent) is 0.5% or more, and the water content is 50,000 ppm or less in terms of mass fraction. Si (OR1) 3 Z1 …(1) Si(R2)(OR3) 2 Z2 …(2) (In general formula (1), R1 may be the same or different and is an alkyl group having 1 to 6 carbon atoms, and Z1 is a group containing an epoxy group; in general formula (2), R2 is a methyl group, R3 may be the same or different and is an alkyl group having 1 to 6 carbon atoms, and Z2 is a group containing an epoxy group.)

2. The coating liquid according to claim 1 , wherein the mass ratio is 20% or less.

3. 3. The coating liquid according to claim 1, wherein a ratio of a product (Bt) of the number of moles and a valence of the polyvalent metal contained in the polyvalent metal-containing particles (B) to a number of moles (At) of carboxy groups contained in the carboxy group-containing polymer (A) is 0.6 or more.

4. 4. The coating liquid according to claim 1, wherein the carboxyl group-containing polymer (A) is a homopolymer of a carboxyl group-containing unsaturated monomer, a copolymer of two or more kinds of carboxyl group-containing unsaturated monomers, a copolymer of a carboxyl group-containing unsaturated monomer and another polymerizable monomer, a carboxyl group-containing polysaccharide, or a mixture of two or more kinds thereof.

5. The coating liquid according to any one of claims 1 to 4, wherein the carboxyl group-containing unsaturated monomer constituting the carboxyl group-containing polymer (A) is at least one α,β-monoethylenically unsaturated carboxylic acid selected from the group consisting of acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid, and fumaric acid.

6. 6. The coating liquid according to claim 1, wherein the polyvalent metal-containing particles (B) have an average particle size in the range of 10 nm to 10 μm.

7. 7. The coating liquid according to claim 1, wherein the polyvalent metal of the polyvalent metal-containing particles (B) is a divalent metal.

8. A method for producing a gas barrier laminate, comprising forming a coating layer from the coating liquid according to claim 1 .

9. A gas barrier laminate obtained by the method according to claim 8.

10. A packaging material comprising the gas barrier laminate according to claim 9.

11. A package comprising the packaging material of claim 10.

12. A packaged article comprising the package according to claim 11 and contents contained in the package.

Citation Information

Patent Citations

  • Gas-barrier resin composition and film

    JP1994093133A

  • Film with gas barrier property and manufacture thereof

    JP2000289154A

  • Gas barrier film and its production

    JP2000336195A

  • Coating agent having gas barrierness and film

    JP2001323204A

  • Gas barrier coating agent, gas barrier film prepared therefrom, and method for preparing same

    JP2002020677A