Highly moisture-absorbent and flexible laminate
A laminate structure with a base, gas barrier, and moisture-absorbing layers addresses moisture and bending resistance issues, enhancing packaging materials for metal products and medicines with improved moisture absorption and flexibility.
Patent Information
- Application Number
- JP2020155989
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-17
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-09-17
AI Technical Summary
Existing packaging materials for metal products and medicines lack sufficient moisture resistance, flexibility, and bending resistance, leading to issues such as moisture absorption causing rust and deterioration, and insufficient moisture resistance after opening.
A laminate structure comprising a base material layer, a gas barrier layer, and a moisture-absorbing sealant layer, with specific resin compositions and moisture absorbents like calcium oxide and hydrophilic zeolite, ensuring high moisture absorption and bending resistance.
The laminate provides excellent moisture absorption, bending resistance, and heat sealability, reducing pinhole formation and improving packaging integrity.
Smart Images

Figure 0007585676000004 
Figure 0007585676000001 
Figure 0007585676000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a highly moisture-absorbing and flex-resistant laminate that has excellent moisture absorption, flex resistance and impact resistance, and is flexible and highly adhesive, and to a highly moisture-absorbing and flex-resistant packaging material and a highly moisture-absorbing and flex-resistant packaging body made from the highly moisture-absorbing and flex-resistant laminate. [Background technology]
[0002] Packaging materials are known that are intended for the transport or long-term storage of contents such as metal products and chemicals made of metal materials or parts using metal, particularly medical instruments and pharmaceuticals, and that are capable of maintaining the quality and functionality of the contents, have a simple layer structure, and are manufactured through a simple manufacturing process. These products employ methods to prevent moisture from reaching the contents or to apply anti-rust treatments to prevent the contents from deteriorating in quality or rusting due to moisture absorption. For example, Patent Documents 1 to 3 propose packaging laminates in which a resin contains a highly volatile anti-rust agent that volatilizes at room temperature and exerts an anti-rust effect, with the aim of preventing rusting of metal product contents. However, packaging materials that do not use volatile rust inhibitors are desired because they require a tightly sealed exterior, and there are concerns that vaporized rust inhibitors may have effects other than the rust-preventing effect, such as deterioration of the contents or functional impairment if they come into contact with the contents, and their removal is also troublesome and limited in scope. PTP packaging and blister packaging are widely used for packaging food and medicine, but traditionally many of them have insufficient moisture-proofing, and to compensate for this, aluminum foil pillow bags are used as outer bags and a desiccant is also included. However, with this method, the moisture-proofing is insufficient after the outer bag is opened, and there are many accidents where the desiccant is accidentally ingested. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-254350 A [Patent Document 2] JP 2007-308726 A [Patent Document 3] JP 2010-052751 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention aims to solve the above problems and to provide a highly moisture-absorbent, flex-resistant laminate that is easy to work with during laminate production, has a small total number of constituent layers, is thin and flexible, has high heat sealability, is highly hygroscopic, and produces little pinholes under bending load, as well as a highly moisture-absorbent, flex-resistant packaging material and a highly moisture-absorbent, flex-resistant packaging body made from the highly moisture-absorbent, flex-resistant laminate. [Means for solving the problem]
[0005] As a result of various studies, the present inventors have found that a highly moisture-absorbing and flexible laminate having at least one moisture-absorbing layer and two heat seal layers, in which the moisture-absorbing layer contains a specific resin and a moisture absorbent, can achieve the above-mentioned objective.
[0006] The present invention is characterized in the following points. 1. A highly moisture-absorbing and flexible laminate having a structure in which at least a base layer, a gas barrier layer, and a moisture-absorbing sealant layer are laminated in this order, the base layer is a layer made of a resin film, the gas barrier layer is a layer containing a metal or a metal oxide, The moisture absorbing sealant layer has at least one moisture absorbing layer and two heat seal layers. , The moisture absorbing layer contains a polyethylene resin, a moisture absorbing agent, and a flexible resin and / or an adhesive reinforcing resin, The flexible resin contains a polyethylene-based elastomer and / or a polyethylene-based plastomer, The adhesive reinforcing resin contains a functional group-containing modified polyolefin, the heat seal layer contains linear low density polyethylene and does not contain the moisture absorbent, and is a layer on both surfaces of the highly water absorbent flex-resistant film; A highly moisture-absorbent and flexible laminate, wherein the linear low-density polyethylene contained in each of the two heat seal layers or in the moisture-absorbent layer is the same or different. 2. The content of the flexible resin in the moisture absorption layer is 2% by mass or more and 20% by mass or less; 2. The highly moisture-absorbing and flexible laminate according to 1 above, wherein the content of the moisture absorbent in the moisture absorbing layer is 25% by mass or more and 65% by mass or less. 3. The polyethylene elastomer has a density of 0.86 g / cm 3 More than 0.935g / cm 3 3. The highly moisture-absorbing and flexible laminate according to 1 or 2 above, characterized in that: 4. The polyethylene plastomer has a density of 0.86 g / cm 3 More than 0.935g / cm 3 4. The highly moisture-absorbing and flex-resistant laminate according to any one of the above 1 to 3, characterized in that: 5. The highly moisture-absorbing and flexible laminate according to any one of the above items 1 to 4, wherein the adhesive reinforcing resin is maleic anhydride-modified polyethylene. 6. The highly moisture-absorbing and flexible laminate according to any one of 1 to 5 above, wherein the moisture absorbent is a metal oxide. 7. The highly moisture-absorbing and flexible laminate according to any one of 1 to 6 above, wherein the metal oxide is one or more selected from the group consisting of calcium oxide, magnesium oxide, barium oxide, and hydrophilic zeolite. 8. The amount of moisture absorbed at 23℃ 50% RH for 14 days is 6g / m 2 More than 10g / m 2 8. The highly moisture-absorbing and flex-resistant laminate according to any one of the above 1 to 7, characterized in that: 9. The highly moisture-absorbing and flexible laminate according to any one of 1 to 8 above, wherein the moisture-absorbing sealant layer is a layer made of a moisture-absorbing sealant film. 10. A highly moisture-absorbing and flexible packaging material produced using the highly moisture-absorbing and flexible laminate described in any one of 1 to 9 above. 11. A highly moisture-absorbent, flexible packaging product packaged with the highly moisture-absorbent, flexible packaging material described in 10 above. Effect of the Invention
[0007] According to the present invention, it is possible to obtain a highly moisture-absorbent, flex-resistant film which has excellent workability during laminate production, a small total number of constituent layers, is thin and flexible, has high heat sealability, is highly hygroscopic, and generates little pinholes under bending load, as well as a highly moisture-absorbent, flex-resistant packaging material and a highly moisture-absorbent, flex-resistant package made from the highly moisture-absorbent, flex-resistant film. [Brief description of the drawings]
[0008] [Figure 1] 1 is a schematic cross-sectional view showing an example of a layer structure of a highly moisture-absorbing and flexible laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The highly moisture-absorbent, flex-resistant laminate of the present invention, and the highly moisture-absorbent, flex-resistant packaging material and highly moisture-absorbent, flex-resistant packaging product produced from the highly moisture-absorbent, flex-resistant laminate will be described in detail below with reference to the drawings.
[0010] In the present invention, the total number of constituent layers refers to the detailed number of layers constituting the laminate, such as the inorganic vapor deposition layer, the crack resistance imparting adhesive layer, the inorganic vapor deposition layer supporting layer, the substrate layer, the sealant layer, and the adhesive layer. This refers to the number of layers, including special coating layers such as vapor deposition layers and anchor coat layers in each layer. For example, a PET film layer with an aluminum vapor deposition layer is counted as two layers. The laminate according to the present invention and the packaging material and packaging bag made of the laminate will now be described. The resin names used in the present invention are those commonly used in the industry. Furthermore, the present invention is not limited to the specific examples listed below. In the present invention, films and sheets are collectively referred to as films.
[0011] <Highly moisture-absorbent and flexible laminate> The highly moisture-absorbing and flex-resistant laminate of the present invention has a configuration in which at least a substrate layer, a gas barrier layer, and a moisture-absorbing sealant layer are laminated in this order. The layers may be laminated with an adhesive layer between them. The highly moisture-absorbing and flexible laminate may have one base layer or two or more gas barrier layers. The moisture absorbing sealant layer is a surface layer on one side of the highly moisture absorbing and flexible laminate.
[0012] The moisture absorption of the highly moisture-absorbent and flexible laminate of the present invention is, for example, 6 g / m2 of moisture absorption amount at 23°C and 50% RH for 14 days. 2 More than 10g / m 2 It is preferable that:
[0013] <Base material layer> The substrate layer may be a known resin film, paper material, or the like, and may be composed of a single layer or a multilayer structure including two or more layers having the same or different compositions.
[0014] The thickness of the substrate layer varies depending on the material, but in the case of a resin film, it is preferably 5 μm or more and 50 μm or less, and more preferably 10 μm or more and 30 μm or less. The resin film used for the base layer may be a film of a thermoplastic resin, and is preferably a thermoplastic resin that has excellent chemical and physical strength, can withstand the conditions for forming a vapor deposition film of a metal or metal oxide, and can well retain the properties of the vapor deposition film of the metal oxide without impairing the properties.
[0015] Examples of such resins include polyolefin resins such as polyethylene resins and polypropylene resins, cyclic polyolefin resins, polystyrene resins, acrylonitrile-styrene copolymers (AS resins), acrylonitrile-butadiene-styrene copolymers (ABS resins), poly(meth)acrylic resins, polycarbonate resins, polyester resins such as polyethylene terephthalate and polyethylene naphthalate, polyamide resins such as various nylons, polyurethane resins, acetal resins, and cellulose resins. In the present invention, the resin is preferably a polyester resin, a polyamide resin, or a polyolefin resin, and in particular, polyethylene terephthalate (PET), nylon, or polypropylene (PP).
[0016] In the present invention, the thermoplastic resin used in the substrate layer can be formed into a film by various known and used film-forming methods. For example, a method of forming a film using one type of resin by a film forming method such as extrusion, cast molding, T-die method, cutting method, inflation method, etc., a method of forming a multilayer film by co-extrusion using two or more types of resins, a method of mixing two or more types of resins before film formation and forming a film by the above-mentioned film forming method, etc. can be mentioned. Furthermore, a film can be uniaxially or biaxially stretched using a tenter system, tubular system, etc.
[0017] Alternatively, one or more resins may be coated on another resin film by applying and drying, or a molten resin may be laminated by a T-die method or the like. In the present invention, the resin film is preferably a polyester film, and more preferably a biaxially oriented PET film, a biaxially oriented nylon film, or a biaxially oriented PP film or sheet.
[0018] In addition, when forming the resin film, various plastic compounding agents and additives can be added to the resin film for the purpose of improving or modifying, for example, the processability, heat resistance, weather resistance, mechanical properties, dimensional stability, oxidation resistance, slipperiness, release properties, flame retardancy, mold resistance, electrical properties, strength, etc. of the film. The amount of these additives can range from a very small amount to several tens of percent and can be added at any amount depending on the purpose. In the above, examples of common additives that can be used include lubricants, crosslinking agents, antioxidants, ultraviolet absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, modifying resins, and the like.
[0019] <Gas barrier layer> The gas barrier layer is a layer that suppresses the permeation of gas through the highly moisture-absorbing and flexible laminate. The gas barrier layer is a layer containing a metal, a metal oxide or a gas barrier resin. Specifically, the gas barrier layer may be made of one or more materials selected from the group consisting of a gas barrier resin film, a metal foil, a resin film with a vapor-deposited layer of a metal or metal oxide, and a gas barrier resin coating film.
[0020] The gas barrier resin film may be a known resin film having gas barrier properties. For example, the gas barrier film may be a resin film made of a resin such as PET, polybutylene terephthalate, polyethylene naphthalate, polyamide, polyimide, polyvinyl alcohol, or an ethylene-vinyl alcohol copolymer.
[0021] The metal foil is preferably an aluminum foil having a thickness of 3 μm or more and 15 μm or less.
[0022] The resin film with a metal or metal oxide vapor-deposited layer is preferably one in which an aluminum vapor-deposited film, a silica vapor-deposited film, or an aluminum oxide vapor-deposited film is formed on at least one surface of the above-mentioned base resin film. Commercially available resin films with an aluminum oxide vapor-deposited film include alumina-vapor-deposited IB-PET-PIR (thickness 12 μm) and silica-vapor-deposited IB-ON-UB (thickness 15 μm) manufactured by Dai Nippon Printing Co., Ltd., which are PET films with alumina vapor-deposited on one surface by the PVD method.
[0023] As the gas barrier resin coating film, a coating film containing a sol-gel hydrolysis polycondensate formed from a metal alkoxide and a water-soluble polymer is preferred.
[0024] The metal foil for the gas barrier layer, or the resin film with the metal or metal oxide vapor-deposited layer can be bonded to other layers using a dry lamination adhesive. Alternatively, by using a resin film for the base layer as the resin film of the resin film with a metal or metal oxide vapor-deposited layer, lamination onto the base layer can be omitted.
[0025] <Moisture-absorbing sealant layer> The moisture-absorbing sealant layer has at least one moisture-absorbing layer and two heat-sealing layers, and has a layer structure in which the moisture-absorbing layer is sandwiched between the two heat-sealing layers. One heat seal layer is laminated on the substrate layer side of the highly moisture-absorbing and flex-resistant laminate, and the other heat seal layer is laminated on the opposite side, that is, on the outermost surface of the highly moisture-absorbing and flex-resistant laminate. The layers may be laminated with an adhesive layer between them. The moisture absorbing layer contains a polyethylene resin, a flexible resin, an adhesive reinforcing resin, and a moisture absorbing agent. The flexible resin may be a polyethylene elastomer and / or a polyethylene plastomer, and the adhesive reinforcing resin preferably contains a functional group-containing modified polyolefin. The heat seal layer is a layer containing a polyethylene resin, and preferably does not contain a moisture absorbent in order to have good heat sealability. Here, the polyethylene resins contained in each of the two heat seal layers or the moisture absorbing layer may be the same or different. The polyethylene resin is preferably LLDPE and / or LDPE, more preferably LLDPE.
[0026] The content of the flexible resin in the moisture absorbing layer is preferably 2% by mass or more and 20% by mass or less, and more preferably 5% by mass or more and 15% by mass or less. If it is less than the above range, the bending resistance and impact resistance of the highly moisture absorbing and flexible resistant laminate may be insufficient, and if it is more than the above range, the rigidity of the moisture absorbing layer and / or the entire highly moisture absorbing and flexible resistant laminate may be too low, which may cause the laminate to lack suitability as a packaging material.
[0027] The content of the adhesive reinforcing resin in the moisture absorbing layer is preferably 2% by mass or more and 20% by mass or less, more preferably 5% by mass or more and 15% by mass or less. If it is less than the above range, the adhesive strength at the interface of the moisture absorbing layer, and the heat sealability, flex resistance, and impact resistance of the highly moisture absorbing and flexible laminate may be insufficient, while if it is more than the above range, the adhesive strength at the interface of the moisture absorbing layer, and the heat sealability, flex resistance, and impact resistance of the highly moisture absorbing and flexible laminate are not significantly improved.
[0028] The content of the moisture absorbent in the moisture absorbing layer is preferably 0.5% by mass or more and 70% by mass or less, and more preferably 20% by mass or more and 55% by mass or less. If it is less than the above range, the moisture absorption may be insufficient, and if it is more than the above range, the film formability and the interfacial adhesive strength may decrease, or the flex resistance may be insufficient.
[0029] The thickness of the moisture-absorbing sealant layer is not particularly limited, but is preferably 20 μm to 200 μm, more preferably 30 μm to 150 μm, and more preferably 30 μm to 100 μm. If it is thinner than the above range, the heat sealability and moisture absorption properties may be insufficient, and if it is thicker than the above range, the rigidity of the highly moisture-absorbing and bending-resistant laminate becomes too strong, and it is likely to be inferior in suitability as a packaging material.
[0030] The thickness of the moisture-absorbing layer is not particularly limited, but is preferably 10 μm to 100 μm, more preferably 15 μm to 75 μm, and even more preferably 15 μm to 50 μm. If the thickness is thinner than the above range, the moisture absorption of the highly moisture-absorbing and flexible laminate may be insufficient, and if the thickness is thicker than the above range, the moisture absorption is not improved significantly, and the rigidity of the highly moisture-absorbing and flexible laminate may become too strong, which may result in poor suitability as a packaging material.
[0031] The thickness of the heat seal layer is not particularly limited, but is preferably 5 μm to 50 μm, more preferably 7 μm to 40 μm, and more preferably 10 μm to 30 μm. If it is thinner than the above range, the heat sealability of the highly moisture-absorbing and flexible laminate may be insufficient, and if it is thicker than the above range, the rigidity of the highly moisture-absorbing and flexible laminate may be too high, making it less suitable as a packaging material.
[0032] The moisture-absorbing sealant layer can be formed from a moisture-absorbing sealant film having a layer structure similar to that of the moisture-absorbing sealant layer. The moisture-absorbing sealant film has excellent bending resistance and impact resistance. The flex resistance of the moisture-absorbing sealant film can be evaluated by the number of pinholes generated after flexing. The flex resistance of the highly moisture-absorbing and flex-resistant laminate can be evaluated by, for example, the following method according to ASTM F392: It is preferable that the number of pinholes generated after 1000 flexes in a Gelbo flex test is 0 or more and 7 or less. The impact resistance of the moisture-absorbing sealant film is preferably such that the impact strength is 1.5 J or more and 3 J or less in an impact destruction test in accordance with ASTM D3420, the standard test method for pendulum impact resistance of plastic films.
[0033] <Moisture absorption layer> The moisture absorbing layer is a layer that is responsible for the moisture absorbing property in the highly moisture absorbing and flexible laminate, and is a layer that contains a moisture absorbent, a thermoplastic resin as a binder resin, and an adhesive reinforcing resin. The moisture absorbing layer may be one layer in the highly moisture absorbing and flexible laminate, or it may be two or more layers having the same or different compositions. The binder resin contained in the moisture absorbing layer is preferably a thermoplastic resin having excellent bending resistance, affinity suitable for dispersing the moisture absorbent, and excellent film forming properties, and more preferably a thermoplastic resin having excellent heat sealing properties.
[0034] Such a thermoplastic resin preferably contains a polyethylene resin, more preferably contains linear low density polyethylene (hereinafter referred to as LLDPE) and a flexible resin. A combination of a polyethylene resin, particularly LLDPE, and a flexible resin has a synergistic effect, and has high flexibility and affinity with a moisture absorbent, making it an excellent binder resin for the moisture absorption layer of a highly moisture-absorbing and flexible laminate. The adhesive reinforcing resin contained in the moisture-absorbing layer reinforces the interlayer adhesive strength at the interface where the moisture-absorbing layers contact and the heat seal strength of the highly moisture-absorbing and flexible laminate.
[0035] In the moisture absorbing layer, various kinds of thermoplastic resins can be used in combination within the range that does not significantly adversely affect the bending resistance, moisture absorption property, heat sealability, film formability, and the like.
[0036] <Heat seal layer> The heat seal layer is preferably a surface layer on both sides of the moisture absorbing sealant layer, and preferably contains a thermoplastic resin having excellent film-forming and heat sealability. Such a thermoplastic resin is preferably a polyethylene-based resin, and more preferably contains LLDPE. The content of LLDPE in the heat seal layer is preferably 75% by mass or more and 100% by mass or less, and more preferably 65% by mass or more and 95% by mass or less.
[0037] In the heat seal layer, various kinds of thermoplastic resins can be used in combination within the range that does not significantly adversely affect the heat sealability, film formability, and the like.
[0038] <Adhesive layer> There are no particular limitations on the adhesive used in the adhesive layer, and adhesives for DL (dry lamination), adhesives for EC (extrusion coating), adhesives for non-solvent lamination, any anchor coating agent, and the like can be used. The adhesive may be of any of the following types: heat-curable, ultraviolet-curable, and electron-beam-curable types; and may be in any form, such as aqueous, solution, emulsion, and dispersion types. The adhesive may be in any form, such as film / sheet, powder, and solid. The adhesive mechanism may be any of the following types: chemical reaction, solvent volatilization, thermal melting, and thermal pressure.
[0039] Components that form such an adhesive layer include polyvinyl acetate adhesives such as polyvinyl acetate and vinyl acetate-ethylene copolymers, polyacrylic acid adhesives made of copolymers of polyacrylic acid and polystyrene, polyester, polyvinyl acetate, etc., cyanoacrylate adhesives, monosodium acrylate adhesives such as ethylene and vinyl acetate, ethyl acrylate, acrylic acid, methacrylic acid, etc. Examples of suitable adhesives include ethylene copolymer-based adhesives consisting of copolymers with ethylene mers, cellulose-based adhesives, polyurethane-based adhesives, polyester-based adhesives, polyamide-based adhesives, polyimide-based adhesives, polyolefin-based adhesives such as LDPE, amino resin-based adhesives consisting of urea resin or melamine resin, phenol resin-based adhesives, epoxy-based adhesives, reactive (meth)acrylic-based adhesives, elastomer-based adhesives consisting of chloroprene rubber, nitrile rubber, styrene-butadiene rubber, etc., silicone-based adhesives, and inorganic adhesives consisting of alkali metal silicates, low-melting point glass, etc.
[0040] <About each ingredient> [Moisture absorbent] The moisture absorbent contained in the highly moisture-absorbing and flexible laminate of the present invention is preferably a metal oxide. The metal oxide is preferably one or more selected from the group consisting of calcium oxide, magnesium oxide, barium oxide, and hydrophilic zeolite.
[0041] The moisture absorbent may have any external shape, such as a spherical shape, a rod shape, an elliptical shape, or the like, and may be in any form, such as a powder shape, a lump shape, or a granular shape. From the viewpoints of uniform dispersibility, kneading characteristics, film-forming properties, and the like, when dispersed in a resin, a powder shape is preferred.
[0042] In the present invention, the average particle diameter of the moisture absorbent can be appropriately selected from any average particle diameter depending on the application, but the average particle diameter is preferably 0.01 μm or more and 15 μm or less, and more preferably 1 μm or more and 12 μm or less. Here, the average particle diameter is a value measured by a dynamic light scattering method. If the average particle size is smaller than the above range, the hydrophilic zeolite tends to aggregate and the dispersibility tends to decrease.If the average particle size is larger than the above range, the film-forming property of the layer containing the hydrophilic zeolite tends to be poor, so it tends to be difficult to add a large amount of hydrophilic zeolite, and the surface area is also reduced, so there is a possibility that a sufficient moisture absorption effect cannot be obtained.
[0043] (hydrophilic zeolite) In the present invention, the hydrophilic zeolite used as the moisture absorbent preferably contains one or more types selected from the group consisting of A-type zeolite, CHA-type zeolite, and MFI-type zeolite. Here, the A-type zeolite preferably has a pore diameter of 0.3 to 0.5 nm, the CHA-type zeolite preferably has a pore diameter of about 0.38 nm, and the MFI-type zeolite preferably has a pore diameter of about 0.55 nm and / or a specific surface area of 300 to 400 m. 2 / g is preferred. In addition to water, the above zeolites can absorb gases with molecular sizes according to their pore sizes and gases in amounts according to their specific surface areas. For example, CHA-type zeolites are excellent at adsorbing lower hydrocarbons and carbon dioxide, while MFI-type zeolites are excellent at adsorbing carbon dioxide, lower hydrocarbons, lower aldehydes, lower organic acids, and lower alcohols. On the other hand, the above-mentioned zeolites have low affinity for organic gases having low polarity, and are inferior in their ability to adsorb such gases.
[0044] (How to Disperse Moisture Absorbent) The moisture absorbent is preferably incorporated via a master batch in which the moisture absorbent is melt-blended with a thermoplastic resin. Specifically, it is preferable to prepare a master batch by melt blending a moisture absorbent into a thermoplastic resin at a relatively high concentration, and then dry blending the master batch with components such as a binder resin to obtain a moisture absorbent concentration. The moisture absorbent and thermoplastic resin to be melt blended may be one type or two or more types. One master batch may contain one or more kinds of moisture absorbents.
[0045] The content of the moisture absorbent in the master batch is preferably 10% by mass or more and 90% by mass or less, and more preferably 30% by mass or more and 70% by mass or less. Within the above range, it is easy to contain a necessary and sufficient amount of the moisture absorbent in a dispersed state. The above thermoplastic resin may be the same as or different from the thermoplastic resin contained as the binder resin in the moisture absorbing layer.
[0046] <Thermoplastic resin> The thermoplastic resins used in combination as binder resins in the moisture absorption layer and the heat seal layer, and the thermoplastic resins used in the master batch may be the same thermoplastic resin for each layer, or different thermoplastic resins may be used depending on the required performance.
[0047] Specific examples of thermoplastic resins include polyolefin resins, polyester resins, polyamide resins, polyaramid resins, polycarbonate resins, polyacetal resins, fluorine resins, ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers (EVOH), polyvinyl alcohol, polyacrylonitrile, etc. These resins may be used alone or in combination of two or more. Among these resins, polyolefin resins are preferred from the viewpoint of film-forming properties.
[0048] Specific examples of polyolefin resins include polyethylene resins, polypropylene resins, unsaturated carboxylic acid modified resins of polyolefin resins, cyclic polyolefin resins, cyclic olefin copolymers, methylpentene polymers, etc. As unsaturated carboxylic acids, it is preferable to use acrylic acid, methacrylic acid, maleic anhydride, fumaric acid, etc. These polyolefin resins may be used alone or in combination of two or more, or in a multilayer structure containing different types of resins. These copolymerized unsaturated carboxylic acids may be used alone or in combination of two or more. Among these polyolefin resins, polyethylene resins are preferred from the viewpoint of film-forming properties.
[0049] <Heat sealable resin> The heat-sealable resin that can be used in the highly moisture-absorbing and flexible laminate of the present invention is not particularly limited, and any known heat-sealable resin can be used as long as it is a thermoplastic resin that can be melted and fused by heat. Specific examples of heat-sealable resins include polyethylene, very low density polyethylene (hereinafter referred to as VLDPE), low density polyethylene (hereinafter referred to as LDPE), medium density polyethylene (hereinafter referred to as MDPE), high density polyethylene (hereinafter referred to as HDPE), LLDPE, metallocene polyethylene, polypropylene, ethylene-vinyl acetate copolymer, ionomer resin, ethylene-ethyl (meth)acrylate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-propylene copolymer, methylpentene polymer, polyolefin resins obtained by modifying polyolefin resins such as polyethylene or polypropylene with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic anhydride, fumaric acid, and the like, terpolymer resins of ethylene-(meth)acrylic acid ester-unsaturated carboxylic acid, cyclic polyolefin resins, cyclic olefin copolymers, polyethylene terephthalate (PET), polyacrylonitrile (PAN), and the like.
[0050] Among these, polyolefin-based resins are preferred, and among polyolefin-based resins, polyethylene-based resins are more preferred, and among polyethylene-based resins, LDPE and LLDPE are further preferred, with LLDPE being particularly preferred. In the highly moisture-absorbing and flexible film of the present invention, it is preferable to select the resin from those used as binder resins.
[0051] <Polyethylene resin> Specific examples of polyethylene resins include HDPE, MDPE, LDPE, LLDPE, very low density polyethylene (hereinafter referred to as VLDPE), metallocene polyethylene, polypropylene, ethylene-vinyl acetate copolymer, ethylene-ethyl (meth)acrylate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-propylene copolymer, methylpentene polymer, unsaturated carboxylic acid modified resin of polyethylene polyolefin resin, etc. As the unsaturated carboxylic acid, it is preferable to use acrylic acid, methacrylic acid, maleic anhydride, fumaric acid, etc.
[0052] Among the above polyethylene resins, LDPE, LLDPE and VLDPE are more preferred, and VLDPE is even more preferred. These polyethylene resins may be used alone or in combination of two or more.
[0053] [Polyethylene elastomer] The polyethylene elastomer in the present invention is a copolymer having a hard segment and a soft segment derived from an ethylene monomer and another monomer, and is classified into a random copolymer type and a block copolymer type depending on the arrangement of the repeating units derived from each monomer. These may be used alone or in combination of two or more types. In general, the random copolymer type is relatively softer and has a lower melting point (softening point) than the block copolymer type. Specific examples of polyethylene-based elastomers include ethylene-propylene block copolymers, ethylene / butene random copolymers, ethylene / octene block copolymers, and copolymers of ethylene and various cyclic olefins. The random copolymerization type polyethylene elastomer is an ethylene copolymer in which repeating units derived from each monomer are arranged randomly. For example, the main chain structure of a random copolymer consisting of monomer A and monomer B is represented by -ABAABABBAB- or the like. A block copolymer type polyethylene elastomer is an ethylene copolymer in which several consecutive repeating units derived from one type of monomer form a block, and then several consecutive repeating units derived from another type of monomer form a block. For example, the main chain structure of a block copolymer consisting of monomer A and monomer B is represented by -AAAABBBBBAAA-, etc. A polyethylene elastomer has extremely high elasticity at room temperature like rubber, and has a lower density, a lower elastic modulus, and a lower softening point than ordinary polyethylene resins. The polyethylene elastomer in the present invention has a density of 0.86 g / cm 3 More than 0.935g / cm 3 It is preferable that the content is 0.88 g / cm or less. 3 More than 0.915g / cm 3 It is more preferable that:
[0054] [Polyethylene plastomer] A plastomer is a polymeric compound that exhibits plasticity at room temperature, like plastic. The polyethylene plastomer in the present invention is a polyethylene whose main chain is mainly composed of ethylene monomer units, but due to the influence of the side chains and a narrow molecular weight distribution, it exhibits elasticity and thermoplasticity at the same time. Polyethylene plastomers have both plastic and elastic properties, and are superior in flexibility, transparency, low-temperature sealing properties, and impact resistance to ordinary polyethylene resins. The polyethylene plastomer used in the highly moisture-absorbing and flexible laminate of the present invention has a density of 0.86 g / cm 3 More than 0.935g / cm 3 Preferably, it is 0.88g / c or less. m 3 More than 0.915g / cm 3 It is more preferable that:
[0055] <Adhesive reinforced resin> The adhesive-strengthening resin is a resin that strengthens adhesiveness, and can improve the interfacial adhesion strength around the layers contained in the highly moisture-absorbing and flexible laminate, and the heat seal strength of the highly moisture-absorbing and flexible laminate. In the present invention, the adhesive reinforcing resin preferably contains a functional group-containing modified polyolefin. Since the moisture-absorbing layer containing the adhesive-reinforcing resin contains LLDPE and a flexible resin, the main skeleton of the adhesive-reinforcing resin is preferably a polyolefin-based skeleton that has high affinity with these resins, and is preferably modified to contain functional groups in order to enhance adhesion. The functional group-containing modified polyolefin is more preferably maleic anhydride modified polyethylene. When the main skeleton of the polyethylene-based resin and flexible resin contained in the moisture-absorbing layer is polyethylene-based, it is preferable that the main skeleton of the adhesive reinforcing resin contained in the same moisture-absorbing layer is also polyethylene-based, as this will have higher affinity.In order to have high adhesion, it is preferable for the resin to have a highly polar functional group, and a polyethylene-based resin modified with maleic anhydride is more preferable.
[0056] [Method for producing highly moisture-absorbent and flexible laminate] The preparation method described below is an example and is not intended to limit the present invention. The film formation and lamination of each layer constituting the highly moisture-absorbing and flexible laminate is not particularly limited, and any known or commonly used film formation and lamination method can be applied. For example, any method such as wet lamination, dry lamination, solventless dry lamination, extrusion lamination, T-die coextrusion molding, coextrusion lamination, inflation method, etc. can be used. The obtained highly moisture-absorbing and flexible laminate can be subjected to secondary processing for the purpose of imparting surface functions such as chemical functions, electrical functions, magnetic functions, mechanical functions, friction / wear / lubrication functions, optical functions, thermal functions, and biocompatibility. The moisture-absorbing sealant layer may be laminated with other layers after the moisture-absorbing sealant film is produced, or may be laminated on other layers such as a gas barrier substrate layer by extrusion coating or co-extrusion. Even in the case of the extrusion coating method, lamination may be performed via an adhesive layer as necessary.
[0057] Examples of secondary processing include embossing, painting, adhesives, printing, metallizing (plating, etc.), machining, surface treatment (antistatic treatment, corona discharge treatment, plasma treatment, photochromic treatment, physical vapor deposition, chemical vapor deposition, coating, etc.), and the like.
[0058] Below, an example is described of the production of a highly moisture-absorbing and flexible laminate (highly moisture-absorbing and flexible laminate packaging material) having a layer structure of, for example, substrate layer / adhesive layer / gas barrier layer / adhesive layer / moisture-absorbing sealant layer [adhesive reinforcement layer / moisture-absorbing layer / heat seal layer].
[0059] (Preparation of moisture-absorbing sealant film) A resin composition for the adhesion reinforcing layer, a resin composition for the moisture absorbing layer, and a resin composition for the heat seal layer are each prepared, and a moisture absorbing sealant film having the following layer structure is obtained by an inflation method. Layer structure: Adhesive reinforcement layer / moisture absorption layer / heat seal layer
[0060] (Preparation of highly moisture-absorbent and flexible laminate) Next, the moisture-absorbing sealant film for the moisture-absorbing sealant layer obtained above, the base film for the base layer, and the aluminum foil for the gas barrier layer were dry-laminated in this order via the DL adhesive for the adhesive layer (coating amount: 3.5 g / m 2 , drying temperature: 70° C.) to obtain a highly moisture-absorbing and flexible laminate having the above layer structure.
[0061] ≪High moisture absorption bending resistant packaging material≫ The highly moisture-absorbing and flex-resistant packaging material of the present invention is a packaging material prepared using the highly moisture-absorbing and flex-resistant laminate of the present invention, and may be the same as the highly moisture-absorbing and flex-resistant laminate, or may further include various functional layers, printed layers, etc., as necessary. The highly moisture-absorbing and flexible packaging material of the present invention can also be subjected to lamination (dry lamination or extrusion lamination), bag making, and other post-treatments.
[0062] ≪High moisture absorption bending resistant packaging≫ The highly moisture-absorbent and flexible packaging body of the present invention is a packaging body packaged with the highly moisture-absorbent and flexible packaging material of the present invention. The highly moisture-absorbent, flex-resistant packaging body of the present invention can be produced in various shapes by, for example, using the highly moisture-absorbent, flex-resistant packaging material of the present invention and folding it in half, or by preparing two sheets of highly moisture-absorbent, flex-resistant packaging material, overlapping them with their heat-sealed layers facing each other, and then heat-sealing the peripheral edges using a heat seal type, such as a side seal type, two-sided seal type, three-sided seal type, four-sided seal type, envelope seal type, grommet seal type (pillow seal type), pleated seal type, flat bottom seal type, square bottom seal type, gusset type, or other heat seal type. In the above, the heat sealing can be performed by a known method such as bar sealing, rotary roll sealing, belt sealing, impulse sealing, high frequency sealing, ultrasonic sealing, etc. EXAMPLES
[0063] Details of the raw materials used in the examples are as follows. [Base material layer] PET film 1: E5100 manufactured by Toyobo Co., Ltd., 12 μm thick. [AL layer] Aluminum foil 1: Manufactured by Toyo Aluminum Co., Ltd. Thickness: 7 μm. [Adhesive layer] DL Adhesive 1: ADOLOCK RU77T / H7 manufactured by Rock Paint Co., Ltd. Polyester adhesive. [Moisture absorbent] Metal oxide 1: Calcium oxide F-Lime 1300-K manufactured by Calfine Co., Ltd. Average particle size: 4.3 μm. Metal oxide 2: Kyowamag 30 magnesium oxide manufactured by Kyowa Chemical Industry Co., Ltd. Average particle size: 3.16 μm. Metal oxide 3: Hydrophilic zeolite 4A manufactured by Tomoe Engineering Co., Ltd. Average particle size: 10 μm.
[0064] [Thermoplastic resin] LLDPE1: Prime Polymer LLDPE, Evolu SP1540. Density 0.913g / cm 3 , MFR3.8g / 10min.
[0065] [Flexible resin] Elastomer 1: Polyethylene elastomer, Toughmer A8050S, manufactured by Mitsui Chemicals, Inc. Density: 0.885g / cm 3 , MFR3.6g / 10min. Elastomer 2: Polyethylene elastomer manufactured by The Dow Chemical Company, Ltd. INFUSE9107. Density 0.866g / cm 3 , MFR1g / 10min. Plastomer 1: Polyethylene plastomer manufactured by Japan Polyethylene Co., Ltd., Kernel KS340T. Density: 0.880g / cm 3 , MFR3.5g / 10min. Plastomer 2: Polyethylene plastomer manufactured by Japan Polyethylene Co., Ltd., Kernel KF282, density 0.915g / cm 3 , MFR2.2g / 10min.
[0066] [Adhesive reinforced resin] Adhesive reinforcement resin 1: Admer NF557, maleic anhydride modified polyethylene manufactured by Mitsui Chemicals, Inc. Density 0.903g / cm 3 , MFR1.7g / 10min. Adhesive reinforcement resin 2: Dow Chemical Co., maleic anhydride modified polyethylene. Amplify TY1052H. Density 0.87g / cm 3 , MFR1.25g / 10min.
[0067] [Preparation of master batch] The masterbatch used in the gas adsorption layer was prepared as follows.
[0068] (Preparation of Masterbatch 1) LLDPE 1 and metal oxide 1 were melt-blended in the following ratio to obtain master batch 1 (MB1). LLDPE1 30 parts by mass Metal oxide 1 70 parts by mass
[0069] [Adjustment of Masterbatches 2 to 4] According to the formulation in Table 1, the raw materials were melt-blended in the same manner as for Masterbatch 1 to obtain Masterbatches 2 to 4 (MB2 to 4).
[0070] [Table 1]
[0071] [Example 1]
[0072] (Preparation of moisture absorbing layer resin composition) The moisture-absorbing layer resin composition used in the moisture-absorbing layer was prepared as follows.
[0073] MB1, LLDPE1, elastomer1, and adhesive reinforcing resin1 were dry blended in the following ratio to obtain a moisture absorbing layer resin composition. MB1 72 parts by mass LLDPE1 25 parts by mass Adhesive reinforced resin 1 3 parts by mass
[0074] (Preparation and evaluation of moisture-absorbing sealant film) The moisture absorbing layer resin composition obtained above and LLDPE1 were formed into a film and laminated by co-extrusion to obtain a highly moisture absorbing and flexible laminate (40 μm thick) having the following layer structure, and various evaluations were then carried out. Layer structure: heat seal layer 1 / moisture absorption layer / heat seal layer 2=LLDPE1 (10 μm thick) / moisture absorption layer resin composition 1 (20 μm thick) / LLDPE1 (10 μm thick)
[0075] (Preparation and evaluation of highly moisture-absorbent and flexible laminates) Next, the moisture-absorbing sealant film obtained above, PET film 1, and aluminum foil 1 were dry-laminated with DL adhesive 1 (coating amount: 3.5 g / m 2 , drying temperature: 70° C.) to obtain a highly moisture-absorbing and flexible laminate having the following layer structure. Composition of highly moisture-absorbent, flexible laminate: Base layer / adhesive layer / gas barrier layer / adhesive layer / moisture-absorbing sealant layer [heat seal layer 1 / moisture-absorbing layer / heat seal layer 2] = PET film 1 (12 μm) / DL adhesive 1 (3.5 g / m 2 ) / aluminum foil 1 (7 μm) / DL adhesive 1 (3.5 g / m 2 ) / [LLDPE1(10μm) / moisture absorption layer resin composition(20μm) / LLDPE1(10μm)] The obtained highly moisture-absorbing and flexible laminate was used to evaluate the heat sealability and the moisture absorption amount. The evaluation results are shown in Table 2.
[0076] [Examples 2 to 15, Comparative Examples 1 to 7] Using the materials shown in Table 2, the moisture absorbing layer resin composition, the moisture absorbing sealant film, and the highly moisture absorbing and flexible laminate were prepared in the same manner as in Example 1, and were similarly evaluated.
[0077] <Evaluation method> [Film forming property] The appearance of the highly moisture-absorbing and flexible laminate was observed and evaluated sensorily according to the following criteria. ○: Film formation is possible without wrinkles or bumps. ×: Numerous wrinkles and bumps were generated, making film formation difficult.
[0078] [Heat sealability] The highly moisture-absorbent and flexible laminate was cut into 100 mm x 100 mm pieces, and the heat-sealed layers were overlapped. Using a heat seal tester (TP-701-A manufactured by Tester Sangyo Co., Ltd.), an area of 10 mm x 100 mm was heat-sealed under the following conditions to prepare a test piece for peel strength in which the ends were not heat-sealed or bonded, and the ends were split into two. This test piece was cut into a strip of 15 mm width, and each bifurcated end was attached to a tensile tester to measure the peel strength (N / 15 mm) under the conditions below, and the pass / fail judgment was made according to the pass / fail judgment criteria below. Heat sealing conditions Temperature: 160℃ Pressure: 1kgf / cm 2 Time: 1 second Test conditions Test speed: 300mm / min Load range: 50N Pass / Fail Criteria ○: 30N / 15mm or more, passed. ×: Less than 30N / 15mm, failing.
[0079] [Moisture absorption amount] The highly moisture-absorbent and flexible laminate was cut into a size of 100 mm x 100 mm, and the weight was measured in an environment of 23°C and 50% RH, and the amount of moisture absorption was calculated using the following formula. Moisture absorption (g / m 2 ) = [wet weight after 2 weeks (g) - initial dry weight (g)] / 0.01(m 2 )
[0080] <Summary of results> The highly moisture-absorbing and flexible laminates of all the Examples exhibited good film-forming properties, heat seal strength and moisture absorption properties. However, Comparative Examples 1 to 4, which did not contain a flexible resin and / or an adhesive reinforcing resin or contained too little of them, showed poor heat sealability, Comparative Example 5, which contained too little moisture absorbent, showed insufficient moisture absorption, and Comparative Example 6, which contained too much moisture absorbent, showed insufficient film-forming properties. Comparative Example 7, in which the content of the flexible resin and / or the adhesive enhancing resin was too high, showed poor film-forming properties.
[0081] [Table 2]
[0082] [Table 3] [Explanation of symbols]
[0083] 1. Highly moisture-absorbent and flexible laminate 2. Heat-sealable moisture-absorbing packaging materials 3 Base material layer 4 Adhesive layer 5 Gas barrier layer 6 Moisture-absorbing sealant layer 6a Heat seal layer 6b Moisture absorption layer 6c Moisture absorbent
Claims
1. A highly moisture-absorbent and flexible laminate having a structure in which at least a base layer, a gas barrier layer, and a moisture-absorbent sealant layer are laminated in this order, the base layer is a layer made of a resin film, the gas barrier layer is a layer containing a metal or a metal oxide, The moisture absorbing sealant layer has at least one moisture absorbing layer and two heat seal layers, The moisture-absorbing layer contains a linear low-density polyethylene, a moisture absorbent, and a flexible resin and / or an adhesive reinforcing resin, The flexible resin contains a polyethylene-based elastomer and / or a polyethylene-based plastomer, The adhesive reinforcing resin contains maleic anhydride modified polyethylene, The content of the flexible resin and / or the adhesive reinforcing resin in the moisture absorbing layer is 2% by mass or more and 20% by mass or less, The content of the moisture absorbent in the moisture absorbing layer is 25% by mass or more and 65% by mass or less, the heat seal layer contains linear low density polyethylene, does not contain the moisture absorbent, and is a layer on both surfaces of the moisture absorbent sealant layer; The highly moisture-absorbent, flex-resistant laminate has a flex resistance characterized in that the number of pinholes generated after 1,000 flexes in a Gelbo flex test in accordance with ASTM F392 is 0 or more and 7 or less.
2. The polyethylene elastomer has a density of 0.86 g / cm 3 Above, 0.935g / cm 3 2. The highly moisture-absorbing and flexible laminate according to claim 1, wherein:
3. The polyethylene plastomer has a density of 0.86 g / cm 3 Above, 0.935g / cm 3 2. The highly moisture-absorbing and flexible laminate according to claim 1, wherein:
4. 4. The highly moisture-absorbing and flexible laminate according to claim 1, wherein the moisture absorbent is a metal oxide.
5. 5. The highly moisture-absorbing and flexible laminate according to claim 4, wherein the metal oxide is one or more selected from the group consisting of calcium oxide, magnesium oxide, barium oxide, and hydrophilic zeolite.
6. Moisture absorption amount for 14 days at 23°C and 50% RH is 6g / m 2 Above, 10g / m 2 The highly moisture-absorbing and flexible laminate according to any one of claims 1 to 5, characterized in that:
7. 7. The highly moisture-absorbing and flexible laminate according to claim 1, wherein the moisture-absorbing sealant layer is a layer made of a moisture-absorbing sealant film.
8. A highly moisture-absorbent and flexible packaging material produced using the highly moisture-absorbent and flexible laminate according to any one of claims 1 to 7.
9. A highly moisture-absorbent and flexible packaging product, which is packaged with the highly moisture-absorbent and flexible packaging material according to claim 8.
Citation Information
Patent Citations
Resin composition having moisture-absorbing function and indicator function and laminate and package each using the same
JP2004331855A
Moisture content regulated wrapper bag and moisture amount adjusted wrapper packaged with this bag
JP2006103761A
Corrosion inhibitor composition for metal, resin composition comprising the same and molding thereof
JP2007308726A
Rust-proof packaging material
JP2010052751A
Multilayer film containing desiccant and electronic device having the film
JP2010201630A