Adhesive composition, adhesive, and adhesive sheet
A copolymerized pressure-sensitive adhesive composition with specific monomer ratios addresses the imbalance in adhesive and dielectric properties, providing superior performance for touch panels and image display devices.
Patent Information
- Application Number
- JP2020159912
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-24
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-09-24
AI Technical Summary
Existing pressure-sensitive adhesives used in touch panels fail to achieve a balance between excellent adhesive properties and low dielectric constant and loss tangent, particularly at higher frequency bands, necessitating further improvements.
A pressure-sensitive adhesive composition comprising a copolymer of methacrylic acid alkyl ester monomers with specific carbon atom ranges and a polar group-containing (meth)acrylic acid ester monomer, adjusted in weight ratios to enhance both adhesive properties and low dielectric performance.
The adhesive composition exhibits excellent adhesive properties and low dielectric constant and loss tangent, suitable for bonding optical members in touch panels and image display devices.
Smart Images

Figure 0007585685000001 
Figure 0007585685000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive composition, a pressure-sensitive adhesive and a pressure-sensitive adhesive sheet comprising such a pressure-sensitive adhesive composition, and more particularly to a pressure-sensitive adhesive composition having excellent adhesive properties and exhibiting a low dielectric constant and a low dielectric tangent, and a pressure-sensitive adhesive and a pressure-sensitive adhesive sheet using the same. [Background technology]
[0002] In recent years, touch panels that combine a display and a position input device have come into widespread use in mobile devices such as televisions, PC monitors, laptops, mobile phones, smartphones, and tablet terminals, and capacitive touch panels in particular are on the rise. A touch panel is typically composed of an organic electroluminescence (EL) or liquid crystal display, a transparent conductive film substrate (ITO substrate), and a protective film (glass), and a transparent adhesive sheet is used to bond these components together.
[0003] Adhesives for such transparent adhesive sheets are required to have not only adhesive properties such as adhesive strength, but also shock absorption properties to prevent damage to the display due to external impact, excellent optical properties (transparency), and a low dielectric constant to suppress malfunction of the touch panel caused by noise generated from the display component and other peripheral components.
[0004] Known examples of low dielectric constant pressure-sensitive adhesives include pressure-sensitive adhesives using a (meth)acrylic polymer obtained by polymerizing a monomer component containing as a main component an alkyl (meth)acrylate having a branched alkyl group having 10 to 18 carbon atoms at the end of the ester group (see, for example, Patent Document 1); pressure-sensitive adhesives using a copolymer of a monomer mixture (A) containing a monomer containing specific amounts of a methacrylic acid alkyl ester monomer having a long-chain alkyl group having 10 or more carbon atoms at the alkyl ester moiety and a methacrylic acid alkyl ester monomer having an alkyl group having 1 to 9 carbon atoms at the alkyl ester moiety (see, for example, Patent Document 2); and pressure-sensitive adhesive compositions containing a methacrylic polymer having a glass transition temperature (Tg) of 0° C. or lower, obtained by polymerizing a monomer component containing 40 to 99.5% by weight of a methacrylic acid alkyl ester having a C10 to C18 alkyl group at the side chain (see, for example, Patent Document 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-246477 A [Patent Document 2] JP 2015-40237 A [Patent Document 3] JP 2013-1761 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in recent years, as transmission signals have become increasingly frequent, adhesives are being required to have lower dielectric properties, particularly lower dielectric tangents, in the high frequency band than ever before. In this situation, although the techniques disclosed in Patent Documents 1 and 2 provide adhesives with low dielectric constants, they are still not sufficient in terms of low dielectric tangents, and further improvements are being required. In addition, the technology disclosed in the above Patent Document 3 has good low dielectric properties, but is not satisfactory in terms of adhesive properties as an adhesive, and does not sufficiently achieve both low dielectric properties and adhesive properties.
[0007] Under such circumstances, an object of the present invention is to provide a pressure-sensitive adhesive composition that has excellent adhesive properties, and also exhibits a low dielectric constant and a low dielectric loss tangent. [Means for solving the problem]
[0008] However, the present inventors have conducted extensive research in light of these circumstances and have found that, in an adhesive composition containing an acrylic resin, by using an acrylic resin obtained by copolymerizing, in a predetermined content ratio, an alkyl methacrylate ester monomer having an alkyl group with a large number of carbon atoms as a copolymerization component constituting the acrylic resin, and further comprising an alkyl methacrylate monomer having an alkyl group having a smaller number of carbon atoms than the number of carbon atoms in the acrylic group of the alkyl methacrylate monomer, and a polar group-containing (meth)acrylic ester monomer, the copolymerization components being included in the copolymerization components in the predetermined content ratio, an acrylic adhesive composition can be obtained which is capable of providing an adhesive having excellent adhesive properties and exhibiting a low dielectric constant and a low dielectric tangent, and thus completed the present invention.
[0009] That is, the gist of the present invention is a pressure-sensitive adhesive composition comprising an acrylic resin (A) which is a copolymer of a copolymerization component (a) containing a methacrylic acid alkyl ester monomer (a1) having an alkyl group with 10 to 36 carbon atoms, a methacrylic acid alkyl ester monomer (a2) having an alkyl group with 2 to 9 carbon atoms, and a polar group-containing (meth)acrylic acid ester monomer (a3), The present invention relates to a pressure-sensitive adhesive composition, in which, in the copolymerization component (a), the content ratio (a1 / a2) of the methacrylic acid alkyl ester monomer (a1) having an alkyl group with 10 to 36 carbon atoms and the methacrylic acid alkyl ester monomer (a2) having an alkyl group with 2 to 9 carbon atoms is 50 / 50 to 95 / 5 (weight ratio), and the content of the polar group-containing (meth)acrylic acid ester monomer (a3) is 0.01% by weight or more and less than 3% by weight relative to the copolymerization component (a).
[0010] Furthermore, the present invention also provides a pressure-sensitive adhesive comprising the above-mentioned pressure-sensitive adhesive composition, and a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer comprising such a pressure-sensitive adhesive. Effect of the Invention
[0011] The pressure-sensitive adhesive composition of the present invention is an adhesive composition comprising an acrylic resin (A) which is a copolymer of a copolymerization component (a) containing a methacrylic acid alkyl ester monomer (a1) having an alkyl group having 10 to 36 carbon atoms, a methacrylic acid alkyl ester monomer (a2) having an alkyl group having 2 to 9 carbon atoms, and a polar group-containing (meth)acrylic acid ester monomer (a3), wherein in the copolymerization component (a), the content ratio (a1 / a2) of the methacrylic acid alkyl ester monomer (a1) having an alkyl group having 10 to 36 carbon atoms and the methacrylic acid alkyl ester monomer (a2) having an alkyl group having 2 to 9 carbon atoms is 50 / 50 to 95 / 5 (weight ratio), and the content of the polar group-containing (meth)acrylic acid ester monomer (a3) is 0.01% by weight or more and less than 3% by weight based on the copolymerization component (a). Therefore, a pressure-sensitive adhesive obtained from such a pressure-sensitive adhesive composition has excellent adhesive properties and exhibits a low dielectric constant and a low dielectric tangent, and is particularly useful as a pressure-sensitive adhesive used for bonding optical components that constitute touch panels, image display devices, etc.
[0012] In general, in order to impart low dielectric properties (low dielectric constant and low dielectric tangent) to a pressure-sensitive adhesive composition using an acrylic resin, it is known that a large amount of alkyl (meth)acrylic acid ester monomers having an alkyl group with 10 or more carbon atoms are copolymerized in order to reduce the dipole moment of the molecule. However, acrylic resins copolymerized with copolymerization components having a large number of carbon atoms in the alkyl group tend to have poor adhesive properties such as adhesion and retention, especially at high temperatures, and in order to solve this problem, functional groups such as acids are generally introduced, but the introduction of highly polar functional groups tends to make it difficult to obtain a low dielectric tangent, making it difficult to achieve both adhesive properties and a low dielectric tangent. In contrast, the present invention has found that by adjusting the copolymerization ratio of methacrylic acid alkyl ester monomers having alkyl groups of a predetermined length and methacrylic acid alkyl ester monomers having alkyl groups of a predetermined length, and further polar group-containing (meth)acrylic acid ester monomers, the resins have excellent adhesive properties and low dielectric properties, especially low dielectric tangent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below, but these are merely examples of preferred embodiments. In the present invention, "(meth)acrylic" means acrylic or methacrylic, "(meth)acryloyl" means acryloyl or methacryloyl, and "(meth)acrylate" means acrylate or methacrylate, respectively, and "acrylic resin" means a resin obtained by polymerizing a monomer component containing at least one (meth)acrylic monomer. Furthermore, "sheet" conceptually includes a sheet, a film, and a tape.
[0014] The pressure-sensitive adhesive composition of the present invention contains an acrylic resin (A) which is a copolymer of a copolymerization component (a) containing a methacrylic acid alkyl ester monomer (a1) having an alkyl group with 10 to 36 carbon atoms (hereinafter sometimes simply referred to as "methacrylic acid alkyl ester monomer (a1)"), a methacrylic acid alkyl ester monomer (a2) having an alkyl group with 2 to 9 carbon atoms (hereinafter sometimes simply referred to as "methacrylic acid alkyl ester monomer (a2)"), and a polar group-containing (meth)acrylic acid ester monomer (a3). Each component will be described below.
[0015] [Methacrylic acid alkyl ester monomer (a1)] Examples of the methacrylic acid alkyl ester monomer (a1) include linear aliphatic methacrylates such as decyl methacrylate, lauryl methacrylate, tridecyl methacrylate, cetyl methacrylate, stearyl methacrylate, and myristyl methacrylate, and branched aliphatic methacrylates such as isodecyl methacrylate, isotridecyl methacrylate, isomyristyl methacrylate, isostearyl methacrylate, and isotetracosyl methacrylate. These may be used alone or in combination of two or more. Among them, lauryl methacrylate, tridecyl methacrylate, and stearyl methacrylate are preferred from the viewpoint of achieving both low dielectric properties and adhesive properties.
[0016] The content of the methacrylic acid alkyl ester monomer (a1) is usually 50 to 95% by weight, preferably 55 to 90% by weight, and particularly preferably 60 to 85% by weight, based on the copolymerization component (a). If the content is too low, the dielectric constant tends to be high and the thermal stability of the acrylic resin (A) tends to decrease, whereas if the content is too high, the adhesive properties tend to decrease.
[0017] In addition, the methacrylic acid alkyl ester monomer (a1) having an alkyl group with 10 to 36 carbon atoms used in the present invention preferably contains a methacrylic acid alkyl ester monomer (a1-1) having an alkyl group with 10 to 15 carbon atoms (hereinafter sometimes simply referred to as "methacrylic acid alkyl ester monomer (a1-1)") and a methacrylic acid alkyl ester monomer (a1-2) having an alkyl group with 16 to 36 carbon atoms (hereinafter sometimes simply referred to as "methacrylic acid alkyl ester monomer (a1-2)").
[0018] Examples of the methacrylic acid alkyl ester monomer (a1-1) include linear aliphatic methacrylates such as decyl methacrylate, lauryl methacrylate, and tridecyl methacrylate, and branched aliphatic methacrylates such as isodecyl methacrylate and isotridecyl methacrylate. These may be used alone or in combination of two or more. Among them, linear aliphatic methacrylates are preferred from the viewpoint of achieving both low dielectric properties and adhesive properties, and lauryl methacrylate and tridecyl methacrylate are more preferred.
[0019] The content of the methacrylic acid alkyl ester monomer (a1-1) is usually 30 to 85% by weight, preferably 40 to 80% by weight, and particularly preferably 45 to 75% by weight, based on the copolymerization component (a). If the content is too low, the dielectric constant tends to be high and the thermal stability of the acrylic resin (A) tends to decrease, whereas if the content is too high, the adhesive properties tend to decrease.
[0020] Examples of the methacrylic acid alkyl ester monomer (a1-2) include linear aliphatic methacrylates such as cetyl methacrylate, stearyl methacrylate, and myristyl methacrylate, and branched aliphatic methacrylates such as isomyristyl methacrylate, isostearyl methacrylate, and isotetracosyl methacrylate. These may be used alone or in combination of two or more. Among them, methacrylates having an alkyl group with 18 to 24 carbon atoms are preferred, and stearyl methacrylate is more preferred, from the viewpoint of easily increasing the monomer conversion when copolymerized and further achieving both low dielectric properties and adhesive properties.
[0021] The content of the methacrylic acid alkyl ester monomer (a1-2) is usually 1 to 50% by weight, preferably 5 to 40% by weight, and particularly preferably 10 to 30% by weight, based on the copolymerization component (a). If the content is too low, the relative dielectric constant tends to be high, whereas if the content is too high, the adhesive properties tend to be reduced.
[0022] In the copolymerization component (a), the content ratio (a1-1 / a1-2) of the methacrylic acid alkyl ester monomer (a1-1) and the methacrylic acid alkyl ester monomer (a1-2) is usually 1 / 99 to 99 / 1, preferably 30 / 70 to 95 / 5, and more preferably 55 / 45 to 90 / 10. When the content ratio of the methacrylic acid alkyl ester monomer (a1-1) and the methacrylic acid alkyl ester monomer (a1-2) is within the above range, the dielectric properties tend to be excellent.
[0023] [Methacrylic acid alkyl ester monomer (a2)] Examples of the methacrylic acid alkyl ester monomer (a2) include linear aliphatic methacrylates such as ethyl methacrylate, propyl methacrylate, and n-butyl acrylate, and branched aliphatic methacrylates such as iso-butyl methacrylate, tert-butyl methacrylate, and 2-ethylhexyl methacrylate. These may be used alone or in combination of two or more. Among them, ethyl methacrylate is preferred from the viewpoint of cohesive strength, and 2-ethylhexyl methacrylate is preferred from the viewpoint of cohesive strength and low dielectric properties.
[0024] The content of the methacrylic acid alkyl ester monomer (a2) is 1 to 50% by weight, preferably 5 to 40% by weight, and particularly preferably 10 to 35% by weight, based on the copolymerization component (a). If the content is too low, the adhesive strength tends to be insufficient, and if the content is too high, the adhesive properties and handling properties at high temperatures tend to decrease.
[0025] In the copolymerization component (a) used in the present invention, the content ratio (a1 / a2) of the methacrylic acid alkyl ester monomer (a1) and the methacrylic acid alkyl ester monomer (a2) is 50 / 50 to 95 / 5 by weight, preferably 55 / 45 to 93 / 7, and particularly preferably 60 / 40 to 90 / 10. When the content ratio (a1 / a2) is within the above range, the adhesive properties and low dielectric properties are excellent.
[0026] [Polar group-containing (meth)acrylic acid ester monomer (a3)] Examples of the polar group-containing (meth)acrylic acid ester monomer (a3) include hydroxyl group-containing (meth)acrylic acid ester monomer, carboxyl group-containing (meth)acrylic acid ester monomer, and amino group-containing (meth)acrylic acid ester monomer. These may be used alone or in combination of two or more. Among them, hydroxyl group-containing (meth)acrylic acid ester monomer is preferred in terms of excellent adhesive properties and reactivity with the crosslinking agent described below.
[0027] Examples of the hydroxyl group-containing (meth)acrylic acid ester monomer include hydroxyalkyl acrylates such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified monomers such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; oxyalkylene-modified monomers such as diethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate; and primary hydroxyl group-containing monomers such as 2-acryloyloxyethyl-2-hydroxyethyl phthalate, N-methylol (meth)acrylamide, and hydroxyethyl acrylamide; secondary hydroxyl group-containing monomers such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-chloro 2-hydroxypropyl (meth)acrylate; and tertiary hydroxyl group-containing monomers such as 2,2-dimethyl 2-hydroxyethyl (meth)acrylate. Among these, 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are preferred, and 4-hydroxybutyl acrylate is particularly preferred, in that they contain less impurities such as di(meth)acrylates and are easy to produce.
[0028] Examples of the carboxy group-containing (meth)acrylic acid ester monomer include (meth)acrylic acid and β-carboxyethyl acrylate.
[0029] Examples of the amino group-containing (meth)acrylic acid ester monomer include dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and quaternary products thereof.
[0030] The content of the polar group-containing (meth)acrylic acid ester monomer (a3) is from 0.01% by weight to less than 3% by weight based on the copolymerization component (a), preferably from 0.1% by weight to 2.5% by weight, more preferably from 0.2% by weight to 2% by weight, and particularly preferably from 0.5% by weight to 1.5% by weight. If the content is too low, the adhesive properties decrease, whereas if the content is too high, the dielectric tangent increases.
[0031] [(Meth)acrylic acid ester monomer (a4) containing an active energy ray-curable structural portion] The acrylic resin (A) used in the present invention preferably has an active energy ray crosslinkable structural site, which allows the acrylic resin (A) to be efficiently cured (crosslinked) and the cohesive strength to be increased. The active energy ray crosslinkable structural moiety is a structural moiety that can react with a part of the acrylic resin (A) or other curing components contained in the pressure-sensitive adhesive composition upon irradiation with active energy rays to form a crosslinked structure. In the present invention, the active energy ray crosslinkable structural portion is preferably a benzophenone-based crosslinked structure, which has high reactivity and is excellent in improving cohesive strength.
[0032] Therefore, in the present invention, it is preferable to further use an active energy ray-crosslinkable structural site-containing (meth)acrylic acid ester monomer (a4) as the copolymerization component (a) of the acrylic resin (A). The (meth)acrylic acid ester monomer (a4) having an active energy ray crosslinkable structure preferably contains a (meth)acrylic acid ester monomer having a benzophenone structure, since an efficient crosslinked structure can be formed by active energy rays such as ultraviolet rays and electron beams. For example, 4-(meth)acryloyloxybenzophenone can be mentioned.
[0033] The content of the (meth)acrylic acid ester monomer (a4) containing an active energy ray crosslinkable structure is preferably 0.01 to 5% by weight relative to the copolymerization component (a), and the content of the (meth)acrylic acid ester monomer having a benzophenone structure is preferably 0.01 to 5% by weight relative to the copolymerization component (a), particularly preferably 0.1 to 2% by weight, and more preferably 0.2 to 1% by weight. If the content is too small, the holding power when forming a crosslinked structure by active energy rays tends to decrease, and further, in order to prepare a processable adhesive sheet, a large amount of active energy rays is required when forming a crosslinked structure, and a large amount of energy is required when preparing the adhesive sheet, which tends to make efficient production difficult. In addition, if the content is too large, the cohesive force of the entire system increases too much, and the adhesive force tends to decrease.
[0034] Furthermore, when introducing an active energy ray-crosslinkable structural moiety into an acrylic resin, a hydroxyl group may be contained in the acrylic resin, and an ethylenically unsaturated group may be introduced as the active energy ray-crosslinkable structural moiety by reacting an ethylenically unsaturated group-containing isocyanate compound with the hydroxyl group.
[0035] [Ethylenically unsaturated monomers (a5)] In the present invention, the copolymerization component (a) may further contain other copolymerizable ethylenically unsaturated monomers (a5) as necessary. Other copolymerizable ethylenically unsaturated monomers (a5) include, for example, phenyl(meth)acrylate, benzyl(meth)acrylate, phenoxyethyl(meth)acrylate, phenyldiethylene glycol(meth)acrylate, 2-hydroxy-3-phenoxypropyl(meth)acrylate, phenoxypolyethylene glycol(meth)acrylate, phenoxypolyethylene glycol-polypropylene glycol-(meth)acrylate, orthophenylphenoxyethyl(meth)acrylate, nonylphenol ethyl Aromatic ring-containing monomers such as olefin oxide adduct (meth)acrylate; alicyclic ring-containing monomers such as cyclohexyl (meth)acrylate, cyclohexyloxyalkyl (meth)acrylate, tert-butylcyclohexyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-butoxydiethylene Ether chain-containing monomers such as ethylene glycol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, octoxypolyethylene glycol-polypropylene glycol mono(meth)acrylate, lauroxypolyethylene glycol mono(meth)acrylate, and stearoxypolyethylene glycol mono(meth)acrylate; carboxy group-containing monomers such as (meth)acrylic acid, acrylic acid dimers such as β-carboxyethyl acrylate, crotonic acid, maleic acid, maleic anhydride, fumaric acid, citraconic acid, glutaconic acid, itaconic acid, N-glycolic acid, and cinnamic acid; amide group-containing monomers such as (meth)acrylamide, N-(n-butoxyalkyl)(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, and N,N-dimethylaminoalkyl(meth)acrylamide;Other examples include acrylonitrile, methacrylonitrile, styrene, α-methylstyrene, vinyl acetate, vinyl propionate, vinyl stearate, vinyl chloride, vinylidene chloride, alkyl vinyl ether, vinyl toluene, vinyl pyridine, vinyl pyrrolidone, itaconic acid dialkyl ester, fumaric acid dialkyl ester, allyl alcohol, acrylic chloride, methyl vinyl ketone, N-acrylamidomethyltrimethylammonium chloride, allyltrimethylammonium chloride, dimethylallyl vinyl ketone, etc.; These may be used alone or in combination of two or more.
[0036] In addition, when the objective is to increase the molecular weight of the acrylic resin (A), a compound having two or more ethylenically unsaturated groups, such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, or divinylbenzene, can also be used in combination.
[0037] The content of the other copolymerizable ethylenically unsaturated monomer (a5) is usually 20% by weight or less, preferably 10% by weight or less, and more preferably 5% by weight or less, based on the copolymerization component (a). If the content is too high, the dielectric properties and adhesive strength tend to decrease.
[0038] The acrylic resin (A) used in the present invention can be produced by copolymerizing the above-mentioned methacrylic acid alkyl ester monomer (a1) having an alkyl group with 10 to 36 carbon atoms, the methacrylic acid alkyl ester monomer (a2) having an alkyl group with 2 to 9 carbon atoms, and the polar group-containing (meth)acrylic acid ester monomer (a3) as essential components, and further copolymerizing the copolymerization component (a) appropriately containing the above-mentioned optional polymerization components.
[0039] In the copolymerization component (a), from the viewpoint of low dielectric properties, particularly low dielectric tangent, the methacrylic acid alkyl ester monomer is preferably contained in an amount of 80 to 99% by weight, more preferably 90 to 99% by weight, and particularly preferably 95 to 99% by weight, based on the copolymerization component (a).
[0040] The average carbon number of the alkyl group of the methacrylic acid alkyl ester monomer contained in the copolymerization component (a) is preferably 10-15, and more preferably 11-14, from the viewpoint of low dielectric properties, particularly low dielectric tangent.
[0041] As the polymerization method for the acrylic resin (A), for example, a conventionally known polymerization method such as solution polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. can be used. In the present invention, however, production by solution polymerization is preferred in that the acrylic resin (A) can be safely and stably produced with any monomer composition. An example of a preferred method for producing the acrylic resin (A) used in the present invention will be described below.
[0042] First, the copolymerization components and a polymerization initiator are mixed or dropped into an organic solvent to carry out solution polymerization.
[0043] Examples of the organic solvent used in the polymerization reaction include aromatic hydrocarbons such as toluene and xylene, aliphatic hydrocarbons such as n-hexane, esters such as methyl acetate, ethyl acetate, and butyl acetate, aliphatic alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, and isopropyl alcohol, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, aliphatic ethers such as dimethyl ether and diethyl ether, aliphatic halogenated hydrocarbons such as methylene chloride and ethylene chloride, and cyclic ethers such as tetrahydrofuran. These may be used alone or in combination of two or more. Among these solvents, esters and ketones are preferred, and ethyl acetate and acetone are particularly preferred.
[0044] As the polymerization initiator used in the above polymerization reaction, azo-based polymerization initiators and peroxide-based polymerization initiators, which are ordinary radical polymerization initiators, can be used. Examples of the azo-based polymerization initiator include 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobisisobutyronitrile, (1-phenylethyl)azodiphenylmethane, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-cyclopropylpropionitrile), 2,2'-azobis(2-cyclopropylpropionitrile), 2,2'-azobis(2-methylbutyro ... Examples of the peroxide-based polymerization initiator include benzoyl peroxide, di-tert-butyl peroxide, cumene hydroperoxide, lauroyl peroxide, tert-butyl peroxypivalate, tert-hexyl peroxypivalate, tert-hexyl peroxyneodecanoate, diisopropyl peroxycarbonate, and diisobutyryl peroxide. These may be used alone or in combination of two or more. Among these, azo-based polymerization initiators are preferred, and more preferred are 2,2'-azobisisobutyronitrile and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile).
[0045] The amount of the polymerization initiator used is usually 0.001 to 10 parts by weight, preferably 0.1 to 8 parts by weight, particularly preferably 0.5 to 6 parts by weight, further preferably 1 to 4 parts by weight, particularly preferably 1.5 to 3 parts by weight, and most preferably 2 to 2.5 parts by weight, based on 100 parts by weight of the copolymerization component (a). If the amount of the polymerization initiator used is too small, the polymerization rate of the acrylic resin (A) tends to decrease, the amount of residual monomers tends to increase, and the weight average molecular weight of the acrylic resin (A) tends to increase, while if the amount used is too large, the acrylic resin (A) tends to gel.
[0046] The polymerization conditions for the solution polymerization may be any conventionally known polymerization conditions. For example, a copolymerization component containing a (meth)acrylic monomer and a polymerization initiator may be mixed or dropped into a solvent, and polymerization may be carried out under predetermined polymerization conditions.
[0047] The polymerization temperature in the above polymerization reaction is usually 40 to 120° C., but in the present invention, from the viewpoint of stable reaction, it is preferably 50 to 90° C. If the polymerization temperature is too high, the acrylic resin (A) tends to gel easily, whereas if the polymerization temperature is too low, the activity of the polymerization initiator decreases, so that the polymerization rate decreases and the amount of residual monomers tends to increase.
[0048] The polymerization time in the polymerization reaction is not particularly limited, but is preferably 0.5 hours or more, more preferably 1 hour or more, further preferably 2 hours or more, and particularly preferably 5 hours or more from the final addition of the polymerization initiator. The polymerization reaction is preferably carried out while refluxing the solvent in order to facilitate heat removal. In this manner, the acrylic resin (A) used in the present invention can be produced.
[0049] <Acrylic resin (A)> The acrylic resin (A) used in the present invention preferably has a weight-average molecular weight of 150,000 to 1,500,000, more preferably 200,000 to 1,000,000, particularly preferably 250,000 to 800,000, and especially preferably 300,000 to 600,000. If the weight-average molecular weight is too large, the viscosity becomes too high, and the coatability and handling properties tend to decrease, whereas if the weight-average molecular weight is too small, the cohesive force tends to decrease, and the adhesive properties tend to decrease. The weight average molecular weight of the acrylic resin (A) is the weight average molecular weight at the time of completion of production, that is, the weight average molecular weight of the acrylic resin (A) that has not been subjected to heating or the like after production.
[0050] The dispersity (weight average molecular weight / number average molecular weight) of the acrylic resin (A) is preferably 15 or less, more preferably 10 or less, particularly preferably 7 or less, and even more preferably 5 or less. If the dispersity is too high, the durability of the pressure-sensitive adhesive layer tends to decrease and foaming and the like tends to occur easily, and if the dispersity is too low, the handleability tends to decrease. The lower limit of the dispersity is usually 1.1 from the viewpoint of production limitations.
[0051] The weight-average molecular weights mentioned above are those calculated based on the molecular weight of standard polystyrene. The high-performance liquid chromatograph (Waters Japan, "Waters 2695 (main body)" and "Waters 2414 (detector)") was equipped with a Shodex GPC KF-806L column (exclusion limit molecular weight: 2 × 10 7 , Separation range: 100~2×10 7 The number average molecular weight can be measured using three tubes in series (theoretical plate number: 10,000 plates / tube, filler material: styrene-divinylbenzene copolymer, filler particle size: 10 μm), and the number average molecular weight can be measured using the same method. The degree of dispersion can be calculated from the weight average molecular weight and the number average molecular weight.
[0052] The acrylic resin (A) used in the present invention preferably has a glass transition temperature (Tg) of −100 to 50° C., particularly −50 to 20° C., and further preferably −15 to 5° C. If the glass transition temperature is too high, the adhesive strength tends to decrease with a decrease in step conformability and adhesion. If the glass transition temperature is too low, the adhesive properties at high temperatures tend to decrease.
[0053] The glass transition temperature (Tg) is determined by the following measurement method. The release sheet is peeled off from the adhesive sheet before irradiation with active energy rays, which will be described later, and multiple adhesive sheets are laminated to prepare an adhesive sheet with a thickness of about 650 μm in an uncrosslinked state. The dynamic viscoelasticity of the prepared sheet is measured under the following conditions, and the temperature at which the loss tangent (loss modulus G'' / storage modulus G'=tan δ) becomes maximum is read and regarded as the glass transition temperature (Tg) of the acrylic resin.
[0054] [Measurement conditions] Measuring equipment: DVA-225 (manufactured by IT Instrumentation and Control Co., Ltd.) Deformation mode: Shear Distortion: 0.1% Measurement temperature: -100~50℃ Measurement frequency: 1Hz
[0055] The pressure-sensitive adhesive composition of the present invention preferably contains the above-mentioned acrylic resin (A) in an amount of 90% by weight or more, more preferably 95 to 99.9% by weight, particularly preferably 98 to 99.9% by weight, and even more preferably 99 to 99.9% by weight, based on the total weight of the pressure-sensitive adhesive composition.
[0056] [Crosslinking agent] The pressure-sensitive adhesive composition of the present invention may further contain a crosslinking agent such as a monofunctional monomer or a polyfunctional monomer, which allows the cohesive strength of the entire pressure-sensitive adhesive layer to be adjusted and allows stable adhesive properties to be obtained.
[0057] The crosslinking agent is preferably a polyfunctional monomer containing two or more ethylenically unsaturated groups in one molecule, such as hexanediol di(meth)acrylate, butanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, isocyanuric acid ethylene oxide modified tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, urethane (meth)acrylate, and the like. The polyfunctional monomers can be used alone or in combination of two or more. Among them, alkyl(meth)acrylates containing two ethylenically unsaturated groups are preferred because they can achieve both adhesive properties and a low dielectric tangent, and 1,9-nonanediol di(meth)acrylate and 1,10-decanediol di(meth)acrylate are particularly preferred.
[0058] The content of the crosslinking agent is usually 10 parts by weight or less, preferably 0.01 to 8 parts by weight, and more preferably 0.1 to 6 parts by weight, based on 100 parts by weight of the acrylic resin (A). If the amount of the crosslinking agent is too much, the adhesive strength and the dielectric properties tend to decrease. If the amount is too little, the adhesive properties under high temperature conditions tend to decrease.
[0059] [Silane coupling agents] The pressure-sensitive adhesive composition of the present invention also preferably contains a silane coupling agent from the viewpoint of improving durability under high-temperature and high-humidity conditions.
[0060] The silane coupling agent can be any known one without any particular limitation, and examples thereof include epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, amino group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, and 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, (meth)acrylic group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane, and isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane. These may be used alone or in combination of two or more. Of these, 3-glycidoxypropyltrimethoxysilane is preferred.
[0061] The content of the silane coupling agent is usually 5 parts by weight or less, preferably 0.01 to 3 parts by weight, more preferably 0.05 to 2 parts by weight, based on 100 parts by weight of the acrylic resin (A). If the content of the silane coupling agent is too high, the adhesive properties and transparency tend to decrease due to bleeding out. If the content is too low, the durability under high temperature and high humidity conditions tends to decrease.
[0062] [Photopolymerization initiator] The pressure-sensitive adhesive composition of the present invention can be crosslinked (cured) to form a pressure-sensitive adhesive, and in order to efficiently carry out crosslinking, a photopolymerization initiator may be further blended. In particular, when the acrylic resin (A) does not have an active energy ray crosslinkable structural site, it is preferable to blend a photopolymerization initiator.
[0063] Such a photopolymerization initiator is not particularly limited as long as it generates radicals by the action of light, and examples thereof include acetophenone-based, benzoin-based, benzophenone-based, thioxanthone-based, and acylphosphine oxide-based photopolymerization initiators. However, it is preferable to use a hydrogen abstraction type benzophenone-based photopolymerization initiator because it can efficiently crosslink between molecules or within molecules.
[0064] Examples of the benzophenone-based photopolymerization initiator include benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, etc. These may be used alone or in combination of two or more kinds.
[0065] In addition, as an auxiliary for these photopolymerization initiators, it is possible to use in combination triethanolamine, triisopropanolamine, 4,4'-dimethylaminobenzophenone (Michler's ketone), 4,4'-diethylaminobenzophenone, 2-dimethylaminoethylbenzoic acid, ethyl 4-dimethylaminobenzoate, (n-butoxy)ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, 2-ethylhexyl 4-dimethylaminobenzoate, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, etc. These auxiliary agents may be used alone or in combination of two or more.
[0066] The amount of the photopolymerization initiator is preferably 0.01 to 10 parts by weight, more preferably 0.1 to 5 parts by weight, and even more preferably 0.5 to 2 parts by weight, based on 100 parts by weight of the acrylic resin (A). If the amount is too small, the curing speed tends to decrease or the curing tends to be insufficient, while if the amount is too large, the curability does not improve and the economic efficiency tends to decrease.
[0067] The pressure-sensitive adhesive composition of the present invention may further contain other pressure-sensitive adhesives or may contain conventionally known additives such as crosslinking accelerators, antistatic agents, tackifiers, and functional dyes, if necessary.
[0068] Thus, the pressure-sensitive adhesive composition of the present invention can be obtained by mixing the acrylic resin (A), if necessary, the crosslinking agent, the silane coupling agent, the photopolymerization initiator and other optional components. The mixing method is not particularly limited, and various methods can be adopted, such as a method of mixing each component at once, or a method of mixing the optional components and then mixing the remaining components at once or sequentially.
[0069] <Adhesive> As described above, the adhesive composition of the present invention becomes an adhesive by crosslinking (curing) the adhesive composition, or by irradiating the acrylic resin (A) with active energy ray crosslinkable structural moieties, forming at least one intramolecular and intermolecular crosslinking structure. The adhesive has excellent adhesive properties and exhibits low dielectric constant and low dielectric loss tangent, and is suitable for use in bonding optical members constituting touch panels, image display devices, etc.
[0070] The above-mentioned pressure-sensitive adhesive can be made into a pressure-sensitive adhesive sheet by providing a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive on a base sheet, and can be made into a double-sided pressure-sensitive adhesive sheet by providing the above-mentioned pressure-sensitive adhesive layer on a release sheet.
[0071] <Adhesive sheet> The pressure-sensitive adhesive sheet can be produced, for example, as follows. First, the pressure-sensitive adhesive composition of the present invention is applied directly onto a substrate sheet, either as is or after adjusting the concentration with an appropriate organic solvent. After that, the composition is dried, for example, by heating at 80 to 105°C for 0.5 to 10 minutes, and then attached to a substrate sheet or a release sheet. Then, the pressure-sensitive adhesive composition is crosslinked (cured) by irradiation with active energy rays, and further aged as necessary, to produce a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive. Alternatively, a substrate-less double-sided pressure-sensitive adhesive sheet can be produced by forming a pressure-sensitive adhesive layer on a release sheet instead of the above-mentioned base sheet, and then laminating a release sheet onto the opposite side of the pressure-sensitive adhesive layer. When the obtained pressure-sensitive adhesive sheet or double-sided pressure-sensitive adhesive sheet is used, the release sheet is peeled off from the pressure-sensitive adhesive layer.
[0072] Examples of the base sheet include polyester-based resins such as polyethylene naphthalate, polyethylene terephthalate, polybutylene terephthalate, and polyethylene terephthalate / isophthalate copolymer; polyolefin-based resins such as polyethylene, polypropylene, and polymethylpentene; polyethylene fluoride resins such as polyvinyl fluoride, polyvinylidene fluoride, and polyethylene fluoride; polyamides such as nylon 6 and nylon 6,6; vinyl polymers such as polyvinyl chloride, polyvinyl chloride / vinyl acetate copolymer, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, polyvinyl alcohol, and vinylon; cellulose-based resins such as cellulose triacetate and cellophane; acrylic resins such as polymethyl methacrylate, polyethyl methacrylate, polyethyl acrylate, and polybutyl acrylate; polystyrene; polycarbonate; polyarylate; and synthetic resin sheets such as polyimide; metal foils such as aluminum, copper, and iron; paper such as fine paper and glassine paper; and woven fabrics and nonwoven fabrics made of glass fiber, natural fibers, synthetic fibers, and the like. These substrate sheets can be used as a single layer or as a multi-layered body in which two or more types are laminated together. Among these, synthetic resin sheets are preferred from the viewpoint of weight reduction and the like.
[0073] Furthermore, as the release sheet, for example, various synthetic resin sheets, papers, woven fabrics, nonwoven fabrics, etc. exemplified as the base material sheets can be used which have been subjected to a release treatment. As the release sheet, it is preferable to use a silicone-based release sheet.
[0074] The method for applying the pressure-sensitive adhesive composition is not particularly limited as long as it is a common application method, and examples of the method include roll coating, die coating, gravure coating, comma coating, slot coating, and screen printing.
[0075] Examples of the active energy rays that can be used include light rays such as far ultraviolet rays, ultraviolet rays, near ultraviolet rays, and infrared rays, electromagnetic waves such as X-rays and gamma rays, as well as electron beams, proton beams, and neutron beams. Curing with ultraviolet rays is preferred in terms of curing speed, availability of irradiation equipment, cost, and the like.
[0076] The gel fraction of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet is preferably 10 to 100% by weight, more preferably 30 to 90% by weight, and even more preferably 50 to 80% by weight, from the viewpoints of durability and adhesive strength. If the gel fraction is too low, the cohesive strength decreases, and thus durability tends to decrease. However, if the gel fraction is too high, the cohesive strength increases, and thus adhesive strength tends to decrease.
[0077] The gel fraction can be adjusted to fall within the above range by, for example, adjusting the amount of active energy ray irradiation or the content of active energy ray crosslinkable structural moieties in the acrylic resin (A), or adjusting the types and amounts of crosslinking agents and photopolymerization initiators.
[0078] The gel fraction is a measure of the degree of crosslinking (degree of curing) and is calculated, for example, by the following method. That is, an adhesive sheet (without a release sheet) in which an adhesive layer is formed on a polymer sheet (e.g., a polyethylene terephthalate (PET) film, etc.) serving as a substrate is wrapped in a 200-mesh SUS wire net and immersed in toluene kept at 23°C for 24 hours, and the weight percentage of the insoluble adhesive component remaining in the wire net is taken as the gel fraction. However, the weight of the substrate is deducted.
[0079] The thickness of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet is usually preferably 50 to 3000 μm, more preferably 75 to 1000 μm, and particularly preferably 100 to 350 μm. If the pressure-sensitive adhesive layer is too thin, the impact absorption properties tend to decrease, whereas if it is too thick, the thickness of the entire optical component tends to increase, decreasing the practicality.
[0080] The thickness of the adhesive layer in the present invention is a value obtained by subtracting the measured thickness of the constituent members other than the adhesive layer from the measured thickness of the entire adhesive layer-containing laminate using a Mitutoyo Corporation "ID-C112B."
[0081] The pressure-sensitive adhesive layer preferably has a relative dielectric constant at 1 MHz of 3.0 or less, more preferably 2.7 or less, and even more preferably 2.5 or less. The lower limit of the relative dielectric constant is usually 1.0. If the dielectric constant at 1 MHz is too high, the capacitance between the electrodes on the touch panel will increase, which will tend to cause malfunctions, whereas if it is too low, the capacitance will decrease, which will tend to reduce detection sensitivity.
[0082] The pressure-sensitive adhesive layer preferably has a relative dielectric constant at 10 GHz of 3.0 or less, more preferably 2.8 or less, the lower limit of which is usually 1.0. If the relative dielectric constant at 10 GHz is too high, the transmission loss tends to increase in antennas, sensors, wiring, etc. that come into contact with the adhesive layer.
[0083] The pressure-sensitive adhesive layer preferably has a dielectric loss tangent at 10 GHz of 0.005 or less, particularly preferably 0.004 or less, and even more preferably 0.003 or less. If the dielectric loss tangent at 10 GHz is too high, the transmission loss tends to increase in antennas, sensors, wiring, etc. that come into contact with the adhesive layer.
[0084] The adhesive layer of the adhesive sheet of the present invention preferably has a haze value of 2% or less when the thickness of the adhesive layer is 175 μm, particularly preferably 0 to 1.5%, and further preferably 0 to 1%. If the haze value exceeds 2%, the adhesive layer tends to whiten and lose transparency.
[0085] In the present invention, the pressure-sensitive adhesive layer can be laminated on an optical member to obtain an optical member with a pressure-sensitive adhesive layer. Optical members can also be bonded to each other using the double-sided pressure-sensitive adhesive sheet.
[0086] Examples of the optical members include displays (organic EL, liquid crystal), transparent conductive film substrates (ITO substrates), protective films (glass), transparent antennas (films), transparent wiring, and the like that constitute touch panels and image display devices. EXAMPLES
[0087] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not exceed the gist of the invention. In the examples, "parts" and "%" refer to weight standards. The weight average molecular weight and glass transition temperature of the acrylic resin were measured according to the above-mentioned methods.
[0088] [Production Example 1: Production of acrylic resin [A-1]] In a 2 L flask equipped with a condenser, 27 parts of ethyl acetate (boiling point 77°C), 3 parts of acetone (boiling point 56°C) as a polymerization solvent, 0.02 parts of 2,2'-azobisisobutyronitrile (AIBN, half-life temperature 65°C) as a polymerization initiator, 20 parts of a premixed monomer solution (stearyl methacrylate (SMA: a1-2), 53.55 parts of a mixture of lauryl methacrylate and tridecyl methacrylate (SLMA: a1-1), 2-ethylhexyl methacrylate (2EHMA 40% of 100 parts of a mixture of 20 parts of ethyl methacrylate (EMA: a2), 5 parts of 4-hydroxybutyl acrylate (4HBA: a3), 1 part of 4-methacryloyloxybenzophenone (MBP: a4) was added and heated to reflux in a flask, and then 0.05 parts of 2,2'-azobis (2,4-dimethylvaleronitrile) (ADVN: 10-hour half-life temperature 52 ° C) as a polymerization initiator and the remaining 60% of the above-mentioned monomer solution were dropped over 2 hours. After another hour after the dropwise addition, a mixture of 10 parts of ethyl acetate and 0.2 parts of ADVN was dropped over 1 hour to react, and an acrylic resin [A-1] (weight average molecular weight: 420,000, dispersity: 4.20, solid concentration 57%, viscosity 5100 mPa · s (25 ° C), glass transition temperature -3 ° C) solution was obtained. The average number of carbon atoms in the alkyl group of the methacrylic acid alkyl ester monomer was 12.1.
[0089] [Production Examples 2 to 4, Comparative Production Examples 1 to 3] Acrylic resins [A-2] to [A-4] and [A'-1] to [A'-3] were produced in the same manner as in Production Example 1, except that the copolymerization components of the acrylic resins were as shown in Table 1.
[0090] [Table 1]
[0091] <Examples 1 to 4 and Comparative Examples 1 to 3> The adhesive composition made of the acrylic resin solution obtained above was adjusted to a solid content concentration of 45% with ethyl acetate, and the adhesive composition solution was applied to a polyester release sheet so that the thickness after drying would be about 75 μm, and dried at 100° C. for 5 minutes to form an adhesive composition layer. Two of the obtained adhesive composition layers were laminated, sandwiched between polyester release sheets, and exposed to UV light using a high-pressure mercury UV irradiation device with a peak irradiance of 150 mW / cm. 2 , Accumulative exposure: 1000mJ / cm 2 (500mJ / cm 2 A pressure-sensitive adhesive layer was formed by irradiating the sheet with ultraviolet light (×2 passes) to obtain a substrate-less double-sided pressure-sensitive adhesive sheet. In addition, the release sheet on one side was peeled off from the adhesive layer of the substrate-less double-sided adhesive film obtained above, and the film was pressed against an easy-adhesion treated polyethylene terephthalate (PET) sheet (thickness 125 μm) to obtain a PET sheet with an adhesive layer having a thickness of 150 μm.
[0092] The adhesive composition of Example 4 was prepared by blending 5 parts of 1,9-nonanediol diacrylate (1,9-NDA) as a crosslinking agent and 0.1 part of 3-glycidoxypropyltrimethoxysilane (KBM403) as a silane coupling agent with 100 parts of acrylic resin. The substrate-less double-sided PSA sheets or PSA-layered PET sheets obtained above were subjected to the following evaluations.
[0093] [Gel fraction] The above substrate-less double-sided adhesive sheet was cut to 40 mm x 40 mm, and then irradiated with a high-pressure mercury UV irradiator with a peak irradiance of 150 mW / cm 2 Accumulated exposure: 4000mJ / cm 2 (1000mJ / cm 2The sample was irradiated with ultraviolet light using a 100-μm UV lamp (×4 passes) and left to stand for 30 minutes under conditions of 23°C × 50% RH, after which one release sheet was peeled off and the adhesive layer side was attached to a 50 mm × 100 mm SUS mesh sheet (200 mesh). The other release sheet was then peeled off and the SUS mesh sheet was folded back from the center in the longitudinal direction to encase the sample. The sample was then immersed for 24 hours in a sealed container containing 250 g of toluene held at 23°C, and the gel fraction (%) was measured based on the change in weight.
[0094] [Dielectric properties (low frequency: 1MHz) [relative dielectric constant (ε')]] The above-mentioned substrate-less double-sided adhesive sheet was laminated until the thickness of the adhesive layer reached 600 μm, and then one of the release sheets was peeled off and the sheet was pressed against an untreated polyethylene terephthalate (PET) sheet (thickness 50 μm). Then, the other release sheet was peeled off and the sheet was pressed against the same untreated polyethylene terephthalate (PET) sheet as above, obtaining a PET sheet with an adhesive layer having a layer structure of "PET sheet / adhesive layer / PET sheet". The PET sheet with the adhesive layer is irradiated with a high-pressure mercury UV irradiator with a peak irradiance of 150 mW / cm 2 Accumulated exposure: 4000mJ / cm 2 (1000mJ / cm 2 × 4 passes), and then cut into a 70 mm × 70 mm specimen for dielectric constant measurement. The dielectric constant measurement test piece was measured by using a HP4284A precision LCR meter (Agilent) under an atmosphere of 23°C x 50% RH, with the test piece sandwiched between electrodes and an electric field applied at a frequency of 1 MHz. The impedance was measured, and the dielectric constant of the adhesive layer was calculated from the change in the electric capacitance between the electrodes. Then, the relative dielectric constant was calculated from the obtained dielectric constant, and evaluated according to the following criteria. (Evaluation Criteria) ○ The adhesive layer has a dielectric constant of 3.0 or less at 1 MHz. × The dielectric constant of the adhesive layer at 1 MHz is greater than 3.0
[0095] [Dielectric properties (high frequency: 10GHz) [relative dielectric constant (ε'), dielectric tangent (tanδ)]] The above-mentioned substrate-less double-sided adhesive sheet was laminated until the thickness of the adhesive layer reached 600 μm, and then one of the release sheets was peeled off and the sheet was pressed against an untreated polyethylene terephthalate (PET) sheet (thickness 50 μm). Then, the other release sheet was peeled off and the sheet was pressed against the same untreated polyethylene terephthalate (PET) sheet as above, to obtain a PET sheet with an adhesive layer having a configuration of "PET sheet / adhesive layer / PET sheet." The PET sheet with the adhesive layer is irradiated with a high-pressure mercury UV irradiator with a peak irradiance of 150 mW / cm 2 Accumulated exposure: 4000mJ / cm 2 (1000mJ / cm 2 × 4 passes), and then cut into a size of 2 mm × 80 mm to prepare a test piece for dielectric constant measurement. For the above-mentioned dielectric constant measurement test pieces, the dielectric constant (relative dielectric constant (ε'), dielectric tangent (tan δ)) of the adhesive layer at 10 GHz was calculated by the cavity resonator perturbation method using an E8361A PNA series network analyzer (manufactured by Agilent), and evaluated according to the following criteria.
[0096] (Evaluation criteria for relative dielectric constant (ε')) ○ The adhesive layer has a dielectric constant of 2.2 or less at 10 GHz. × The dielectric constant of the adhesive layer at 10 GHz is greater than 2.2 (Evaluation standard for dielectric tangent (tan δ)) ○ The dielectric tangent of the adhesive layer at 10 GHz is 0.005 or less × The dielectric tangent of the adhesive layer at 10 GHz is greater than 0.005
[0097] [180 degree peel strength at 23℃] The PET sheet with the adhesive layer was cut into a size of 25 mm wide x 100 mm long, and irradiated with a high-pressure mercury UV irradiation device with a peak irradiance of 150 mW / cm. 2 , Accumulative exposure: 4000mJ / cm 2 (1000mJ / cm 2After irradiating the sample with ultraviolet light (1.1 mm thickness, 300 mm × 4 passes), the release sheet was peeled off and the adhesive layer side was attached to alkali-free glass (Corning Incorporated's "Eagle XG", thickness 1.1 mm) under pressure with a 2 kg rubber roller going back and forth twice in an atmosphere of 23°C and 50% RH. The sample was left to stand for 30 minutes under the conditions of 23°C × 50% RH, and then the 180 degree peel strength (N / 25 mm) was measured at room temperature (23°C) and a peel speed of 300 mm / min.
[0098] [180 degree peel strength at 60℃] The PET sheet with the adhesive layer was cut into a size of 25 mm wide x 100 mm long, and irradiated with a high-pressure mercury UV irradiation device with a peak irradiance of 150 mW / cm. 2 , Accumulative exposure: 4000mJ / cm 2 (1000mJ / cm 2 After irradiating the sample with ultraviolet light (x4 passes), the release sheet was peeled off and the adhesive layer side was pressed and attached to alkali-free glass (Corning "Eagle XG", thickness 1.1 mm) using a 2 kg rubber roller in two passes at 23°C and 50% RH. The sample was then autoclaved (50°C, 0.5 MPa, 20 minutes) and allowed to stand for 60 minutes at 60°C. After that, the 180 degree peel strength (N / 25 mm) was measured at 60°C and a peel speed of 300 mm / min.
[0099] [80℃ holding power] The PET sheet with the adhesive layer was cut into a size of 25 mm x 50 mm and irradiated with a high-pressure mercury UV irradiation device with a peak irradiance of 150 mW / cm. 2 , Accumulative exposure: 4000mJ / cm 2 (1000mJ / cm 2 After irradiating the sample with ultraviolet light (1000 x 4 passes), the release sheet was peeled off and the sample was pressed and attached to a stainless steel plate (SUS304) by reciprocating a 2 kg roller (attached area 25 mm x 25 mm). The retention strength was measured for 24 hours at 80°C under a load of 1 kg using a creep tester (Tester Sangyo Co., Ltd., Retention Strength Tester BE-501 with High Temperature and Humidity Chamber). The evaluation criteria are as follows. (Evaluation Criteria) ◎ No misalignment ○ Misalignment is less than 0.1 mm △ Misalignment is 0.1 mm or more and less than 1.0 mm × Misalignment of 1.0 mm or more or falling
[0100] [50℃ constant load holding power] The PET sheet with the adhesive layer was cut into a size of 25 mm x 75 mm (adhesive layer part 25 mm x 50 mm + non-adhesive layer part 25 mm x 25 mm) and irradiated with a high-pressure mercury UV irradiation device with a peak irradiance of 150 mW / cm. 2 , Accumulative exposure: 4000mJ / cm 2 (1000mJ / cm 2 After irradiating the sheet with ultraviolet light (1 x 4 passes), the release sheet was peeled off and the sheet was pressed and attached to a stainless steel plate (SUS304) by reciprocating a 2 kg roller (attached area 25 mm x 50 mm) and left to stand for 20 minutes in a 50°C atmosphere. A 50 g weight was then hung from the end of the non-attached portion (area 25 mm x 25 mm) and a 50 g load was applied in a direction 90° to the plane of the stainless steel plate. The sheet was left to stand in this state for 60 minutes and the distance the PET sheet had peeled off was measured. The evaluation criteria are as follows: (Evaluation Criteria) ○ Peeling distance is less than 20 mm △ Peeling distance is 20mm or more and less than 50mm ×...Falling
[0101] [Optical properties of pressure-sensitive adhesive layer (transparency)] The PET sheet with the adhesive layer was cut into 25 mm x 25 mm pieces and irradiated with a high-pressure mercury UV irradiator with a peak irradiance of 150 mW / cm. 2 , Accumulative exposure: 4000mJ / cm 2 (1000mJ / cm 2 Then, the release sheet on one side was peeled off from the adhesive layer, and the adhesive layer side was attached to alkali-free glass (Corning's "Eagle XG", thickness 1.1 mm), and then autoclaved (50°C x 0.5 MPa x 20 minutes) to prepare a test piece with a structure of "alkali-free glass / adhesive layer / PET."
[0102] [Haze value] The haze value was measured using the obtained test piece. The haze value was calculated by measuring the diffuse transmittance and total light transmittance using a HAZE MATER NDH2000 (manufactured by Nippon Denshoku Industries Co., Ltd.) and substituting the obtained diffuse transmittance and total light transmittance values into the following formula. This machine complies with JIS K7361-1. Haze value (%) = (diffuse transmittance / total light transmittance) x 100
[0103] [Table 2]
[0104] The pressure-sensitive adhesive sheets obtained using the pressure-sensitive adhesive compositions of Examples 1 to 4 had a low dielectric constant and a low dielectric loss tangent in both the low-frequency and high-frequency ranges, and also had excellent, well-balanced adhesive properties. On the other hand, the pressure-sensitive adhesive sheet obtained using the pressure-sensitive adhesive composition of Comparative Example 1, which did not contain the methacrylic acid alkyl ester monomers (a1) and (a2) as copolymerization components of the acrylic resin, was inferior in adhesive properties and dielectric properties compared to Examples 1 to 4. Moreover, the pressure-sensitive adhesive sheets obtained using the pressure-sensitive adhesive compositions of Comparative Examples 2 and 3, which did not contain the methacrylic acid alkyl ester monomer (a2) as copolymerization components of the acrylic resin, were inferior in adhesive properties compared to Examples 1 to 4. [Industrial Applicability]
[0105] The adhesive obtained using the adhesive composition of the present invention has excellent adhesive properties and exhibits a low dielectric constant and a low dielectric tangent, and is particularly useful as an adhesive used for bonding optical members constituting touch panels, image display devices, etc., and for sealing organic EL displays, etc.
Claims
1. A pressure-sensitive adhesive composition comprising an acrylic resin (A) which is a copolymer of a copolymerization component (a) containing a methacrylic acid alkyl ester monomer (a1) having an alkyl group with 10 to 36 carbon atoms, a methacrylic acid alkyl ester monomer (a2) having an alkyl group with 2 to 9 carbon atoms, and a polar group-containing (meth)acrylic acid ester monomer (a3), the content of the methacrylic acid alkyl ester monomer (a1) having an alkyl group having 10 to 36 carbon atoms is 50 to 90% by weight based on the copolymerization component (a); the content of the methacrylic acid alkyl ester monomer (a2) having an alkyl group having 2 to 9 carbon atoms is 5 to 50% by weight based on the copolymerization component (a); In the copolymerization component (a), the content ratio (a1 / a2) of the methacrylic acid alkyl ester monomer (a1) having an alkyl group with 10 to 36 carbon atoms and the methacrylic acid alkyl ester monomer (a2) having an alkyl group with 2 to 9 carbon atoms is 55 / 45 to 95 / 5 (weight ratio), the (meth)acrylic acid alkyl ester monomer (a1) having an alkyl group having 10 to 36 carbon atoms contains a methacrylic acid alkyl ester monomer (a1-1) having an alkyl group having 10 to 15 carbon atoms and a methacrylic acid alkyl ester monomer (a1-2) having an alkyl group having 16 to 36 carbon atoms; the content of the methacrylic acid alkyl ester monomer (a1-2) having an alkyl group having 16 to 36 carbon atoms is 5 to 40% by weight based on the copolymerization component (a); A pressure-sensitive adhesive composition, characterized in that the content of the polar group-containing (meth)acrylic acid ester monomer (a3) is 0.01% by weight or more and less than 3% by weight based on the copolymerization component (a). 。
2. The pressure-sensitive adhesive composition according to claim 1, characterized in that the content of the methacrylic acid alkyl ester monomer in the copolymerization component (a) is 80 to 99 wt % relative to the copolymerization component (a), and the average carbon number of the alkyl group of the methacrylic acid alkyl ester monomer is 10 to 15.
3. 3. The pressure-sensitive adhesive composition according to claim 1, wherein the acrylic resin (A) has an active energy ray-crosslinkable structural moiety.
4. 4. The pressure-sensitive adhesive composition according to claim 3, wherein the active energy ray crosslinkable structural moiety is a benzophenone-based crosslinkable structure.
5. 5. The pressure-sensitive adhesive composition according to claim 1, wherein the acrylic resin (A) has a weight average molecular weight of 150,000 to 1,500,000.
6. A pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition according to any one of claims 1 to 5.
7. A pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition according to any one of claims 1 to 5 with active energy rays.
8. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer comprising the pressure-sensitive adhesive according to claim 6 or 7.
Citation Information
Patent Citations
Pressure-sensitive adhesive sheet for transfer use
JP1992239575A
Adhesive, adhesive layer, and adhesive sheet
JP2012246477A
Self-adhesive composition, self-adhesive layer, and self-adhesive sheet
JP2013001761A
Optical adhesive composition, optical adhesive sheet, image display device and input-output device
JP2015040237A
Adhesive composition for polarizing plates and polarizing plate having adhesive layer
WO2016072199A1