Polyolefin microporous membrane, laminate, and battery
A polyolefin microporous membrane with controlled molecular weight distribution and peak widths, combined with specific stretching and heat treatment, addresses the balance of shutdown and meltdown temperatures, enhancing safety and output in high-energy density batteries.
Patent Information
- Application Number
- JP2020545384
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-22
- Filing Date
- 2020-08-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-08-19
AI Technical Summary
Existing microporous polyolefin membranes for battery separators face challenges in achieving a balance between low shutdown temperature, high meltdown temperature, and high strength, particularly in high-energy density and high-capacity batteries, due to issues with molecular weight distribution, crystal orientation, and material composition.
A polyolefin microporous membrane composed of polyethylene and polypropylene with controlled molecular weight distribution and peak widths, combined with specific stretching and heat treatment, to achieve a shutdown temperature of 135°C or less and a meltdown temperature of 160°C or higher, while maintaining high strength and porosity.
The membrane provides enhanced safety and output characteristics, suitable for high-energy density and high-capacity batteries by ensuring rapid shutdown and high meltdown temperatures, with improved mechanical strength and porosity.
Smart Images

Figure 0007585789000001 
Figure 0007585789000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyolefin microporous membrane that is excellent in safety and output characteristics when used as a battery separator, a laminate, and a battery using the same. [Background technology]
[0002] Polyolefin microporous membranes are used as filters, fuel cell separators, capacitor separators, etc. In particular, they are suitably used as separators for lithium-ion batteries, which are widely used in notebook personal computers, mobile phones, digital cameras, etc. The reason for this is that polyolefin microporous membranes have excellent membrane mechanical strength and shutdown properties. In particular, in recent years, development of lithium-ion secondary batteries has been progressing with the aim of achieving higher energy density, higher capacity, and higher output, mainly for in-vehicle use, and this has led to even higher safety requirements for separators.
[0003] In order to prevent accidents such as fire when the inside of the battery is overheated in an overcharged state, the separator must have a function (shutdown function) of melting to clog the pores and cut off the current, and it is preferable that the temperature at which this shutdown function occurs (shutdown temperature) is low. In addition, the temperature inside the battery continues to rise momentarily even after shutdown. Therefore, at temperatures above the shutdown temperature, the shape of the separator itself must be maintained and short circuits of the electrodes must be prevented, and it is preferable that the separator's rupture temperature (meltdown temperature) is high. Therefore, it is necessary to achieve both low shutdown and high meltdown, and it can be said that the greater the temperature difference between the shutdown temperature and the meltdown temperature, the higher the safety. One method of lowering the shutdown temperature is to lower the melting point of the raw material by reducing the molecular weight of the material that constitutes the separator, and one method of raising the meltdown temperature is to add a polyolefin with a high melting point such as polypropylene. In addition, with regard to the shutdown function, it is necessary for safety to quickly cut off the current, and the shutdown speed is also an important characteristic.
[0004] On the other hand, as the capacity of batteries increases, the thickness of separators tends to become thinner, and in order to prevent short circuits caused by foreign objects inside the battery or during winding, there is a demand for stronger separators. In general, methods for increasing the strength of separators include controlling the crystal orientation of polyolefins by stretching at a high ratio, and increasing the molecular weight of raw materials. However, when the crystals are highly oriented, the melting point and the shutdown temperature also increase, so there is a trade-off between increasing the strength and lowering the shutdown temperature.
[0005] Patent Document 1 provides a polyolefin microporous membrane that has a low heat shrinkage rate, excellent resistance to membrane rupture, and small variation in membrane thickness by using polyethylene with a high concentration of terminal vinyl groups in combination with polypropylene. In Patent Document 2, meltdown properties are improved by adding a high molecular weight polypropylene.
[0006] Patent Document 3 proposes a separator with excellent safety by adding high molecular weight polypropylene to improve meltdown characteristics and increase the temperature difference between the shutdown temperature and the meltdown temperature. In addition, by using ultra-high molecular weight polyethylene in combination, a low heat shrinkage rate at high temperatures is achieved, and in Example 17, a film with a thin thickness of 3.2 μm but a high strength of 200 gf puncture strength is obtained. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2007 / 051416 [Patent Document 2] Japanese Patent Publication No. 2005-200578 [Patent Document 3] International Publication No. 2015 / 166878 Summary of the Invention [Problem to be solved by the invention]
[0008] However, Patent Document 1 does not focus on the melting point and shutdown properties of the polyethylene used, and the shutdown temperature of the obtained film exceeds 135°C. Furthermore, as a method for lowering the shutdown temperature, the polyolefin microporous membrane is characterized by containing a certain amount or more of a component with a molecular weight of 1000 or less, and the molecular weight distribution of the polyolefin microporous membrane is very broad. When the molecular weight distribution is broad like this, the melting point peak becomes broad, and the shutdown speed becomes slow.
[0009] The polyolefin microporous membrane described in Patent Document 2 is composed mainly of linear polyethylene and has highly oriented crystals through stretching, so its shutdown temperature exceeds 135°C and there is room for improvement in terms of safety.
[0010] The separator described in Patent Document 3 is stretched at a high ratio in order to achieve high strength, and the shutdown temperature is as high as 138°C, with a relatively small temperature difference from the meltdown temperature. Furthermore, since linear high-density polyethylene is used, it is believed that high-melting point components are generated as the crystal orientation progresses due to stretching. In such a case, although shutdown starts at a low temperature, it is believed that it takes time for shutdown to be completed due to the presence of high-melting point components.
[0011] As described above, there is room for improvement in the development of safe separators that meet the diversifying customer needs associated with higher energy density, higher capacity, and higher output without compromising battery performance.
[0012] An object of the present invention is to solve the above-mentioned problems, that is, to provide a microporous polyolefin membrane which is excellent in safety and output characteristics when used as a battery separator. [Means for solving the problem]
[0013] In order to solve the above problems and achieve the object, the present invention has the following configuration. [1] A microporous polyolefin film comprising a polyethylene resin and a polyolefin other than polyethylene (B), which has peaks below 150°C and above 150°C in a differential scanning calorimeter (DSC), the half-width of the peak below 150°C being 10°C or less, and has a 10μm converted pin puncture strength of 2.0N or more. [2] The polyolefin microporous membrane according to [1], further having a peak at 135°C or lower in DSC. [3] The polyolefin microporous membrane according to [1] or [2], which is a single layer. [4] The microporous polyolefin film according to any one of [1] to [3], wherein the content of the polyolefin other than polyethylene (B) is 10% by mass or more. [5] The microporous polyolefin film according to any one of [1] to [4], wherein the polyolefin other than polyethylene (B) is a polypropylene-based resin. [6] The microporous polyolefin membrane according to any one of [1] to [5], which has a shutdown temperature of 135° C. or lower. [7] The microporous polyolefin film according to any one of [1] to [6], which has a meltdown temperature of 160°C or higher. [8] The microporous polyolefin film according to any one of [1] to [7], which has a thickness of 10 μm or less. [9] The microporous polyolefin film according to any one of [1] to [8], which has a peak at 120° C. or higher in a differential scanning calorimeter (DSC).
[10] A laminate comprising a coating layer provided on at least one surface of the polyolefin microporous membrane according to any one of [1] to [9].
[11] A battery using the polyolefin microporous membrane according to any one of [1] to [9] or the laminate according to
[10] . Effect of the Invention
[0014] The polyolefin microporous membrane of the present invention has high strength and low shutdown and high meltdown properties when used as a battery separator, and has high safety and excellent output characteristics. Therefore, it can be suitably used as a battery separator or laminate for batteries and secondary batteries that require high energy density, high capacity, and high output, such as for electric vehicles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The polyolefin microporous membrane according to an embodiment of the present invention contains a polyethylene resin and a polyolefin (B) other than polyethylene, In DSC, it has peaks below 150°C and above 150°C, and the half width of the peak at less than 150°C is 10°C or less; The 10μm conversion puncture strength is 2.0N or more.
[0016] A polyolefin microporous membrane according to an embodiment of the present invention (hereinafter sometimes simply referred to as "microporous membrane") has a characteristic that, when heated with a differential scanning calorimeter (DSC) according to JIS K7121, it has peaks below 150°C and above 150°C. Here, having a peak means that the results obtained by DSC have a maximum value when the horizontal axis is temperature and the vertical axis is heat flow, and the polyolefin microporous membrane according to an embodiment of the present invention is characterized in that the maximum temperatures are below 150°C and above 150°C.
[0017] The peak temperature of less than 150°C is preferably 140°C or lower, more preferably 135°C or lower. The lower limit is 120°C or higher, preferably 123°C or higher. If it is higher than the above range, it is not preferable because the shutdown becomes high temperature when used as a battery separator. If the maximum temperature of the peak of less than 150°C is lower than the above range, it is not preferable because the shrinkage rate at high temperatures increases and the electrodes come into contact with each other in the battery, causing a short circuit.
[0018] Furthermore, the polyolefin microporous membrane according to the embodiment of the present invention needs to have a half-value width of the peak below 150°C of 10°C or less, preferably 10.0°C or less, more preferably 9.5°C or less, still more preferably 9.3°C or less, particularly preferably 9.1°C or less, and most preferably 9.0°C or less. The smaller the half-value width, the easier it is for the resin to melt all at once when the temperature reaches a certain level when the polyolefin microporous membrane is used as a separator of a battery. Therefore, the shutdown speed increases, leading to an improvement in the safety of the battery. Thus, a smaller half-value width is preferable. The half-value width of the peak mentioned here means the value of T2 - T1 when the temperatures corresponding to 0.5 times the maximum heat generation amount Q in the region below 150°C are T1 and T2 (T1 < T2), respectively. Since there are two or more maximum values in the region below 150°C, when there are three or more temperatures corresponding to Q 1 / 2 the half-value width is calculated with the minimum temperature of the corresponding temperatures as T1 and the maximum temperature as T2. To make the half-value width within the above range, it is preferable that the raw material composition of the film is within the range described later, and the stretching conditions and heat fixation conditions during film formation are within the range described later. 1 / 2
[0019] Generally, as a method for lowering the above shutdown temperature, it has been achieved by adding a low melting point polymer that melts at a low temperature as a raw material. However, since the low melting point polymer has low crystallinity, pore formation during the stretching process is insufficient, the porosity of the resulting porous film decreases, and the strength also tends to decrease. It has been difficult to achieve both the output characteristics and safety of the battery. Furthermore, in order to increase the strength, a method of high magnification stretching can be mentioned. However, due to the orientation of the crystals of polyolefin other than the low melting point polymer that is the main component and the progress of high melting point formation due to the increase in magnification, the shutdown temperature rises, and it has been difficult to achieve both high strength and low shutdown temperature. Furthermore, by performing high magnification stretching, the crystal orientation of polyolefin progresses and high melting point components are generated. Therefore, particularly on the high temperature side of the peak of the DSC chart, it becomes broad, and generally, the half-value width becomes wide, leading to a decrease in the shutdown speed.
[0020] The thickness of the polyolefin microporous membrane according to the embodiment of the present invention is not particularly limited and is appropriately adjusted depending on the application, but a thin membrane is preferable for increasing the capacity of the battery. The lower limit is preferably 2 μm or more, more preferably 3 μm or more. The upper limit is preferably 15 μm or less, more preferably 12 μm or less, even more preferably 10 μm or less, and particularly preferably 8 μm or less. If the membrane thickness exceeds 15 μm, sufficient output characteristics and energy density may not be obtained when used as a separator for future high-capacity batteries. From the above viewpoint, the thinner the membrane, the better, but the lower limit of the membrane is about 2 μm because safety may decrease or handling may become difficult. The membrane thickness can be adjusted by the extruder discharge amount, membrane production speed, stretching ratio, stretching temperature, etc. within a range that does not deteriorate other physical properties.
[0021] The porosity of the polyolefin microporous membrane according to the embodiment of the present invention is preferably 30% or more, more preferably 35% or more, and even more preferably 40% or more. The upper limit is preferably 70% or less, more preferably 65% or less, and even more preferably 60% or less. If the porosity is lower than the above range, when used as a battery separator, the ion permeability is insufficient and the output characteristics of the battery are reduced, so it is preferably 30% or more. If it is higher than the above range, the strength is reduced and short circuits due to foreign matter during winding or in the battery are likely to occur, so it is preferably 70% or less. In order to set the porosity in the above range, it is preferable that the raw material composition of the film is within the range described below, and that the stretching conditions and heat setting conditions during film production are within the range described below.
[0022] The polyolefin microporous membrane according to the embodiment of the present invention must have a puncture strength of 2.0N or more, preferably 2.5N or more, more preferably 2.8N or more, even more preferably 3.0N or more, even more preferably 3.3N or more, particularly preferably 3.5N or more, and most preferably 3.8N or more. If the puncture strength is less than 2.0N, a short circuit may occur during winding or due to foreign matter in the battery, and the safety of the battery may be reduced. From the viewpoint of battery safety, if the puncture strength is 2.0N or more, the strength can be increased. However, there are many cases where there is a trade-off between increasing the puncture strength and lowering the shutdown temperature, and the upper limit is 15N. In order to set the puncture strength in the above range, it is preferable that the raw material composition of the film is within the range described below, and the stretching conditions during film formation are within the range described below. In general, it is possible to increase the strength by increasing the stretching ratio.
[0023] The polyolefin microporous membrane according to the embodiment of the present invention has an air resistance of 100 sec / 100 cm when converted into a membrane thickness of 10 μm. 3 More than 2000 seconds / 100cm 3 It is preferably 100 seconds / 100 cm or less. 3 More than 600 seconds / 100cm 3 Less than 100 seconds / 100 cm, more preferably 3 More than 400 seconds / 100cm 3 Below 140 seconds / 100 cm, most preferably 3 More than 400 seconds / 100cm 3 Air resistance is 100 sec / 100 cm or less. 3 If the film has an air permeability of less than 2000 sec / 100 cm, the strength of the film may be reduced and handling may be impaired when the film is used as a thin separator, or micro-short circuits may be easily caused by dendrites when the film is used as a separator for high-power batteries. 3When the film is used as a battery separator, if the film exceeds the above range, the ion permeability becomes insufficient, and the output characteristics of the battery may be deteriorated. In order to set the air permeability resistance in the above range, it is preferable that the raw material composition of the film is within the range described later, and the stretching conditions during film formation are within the range described later.
[0024] The polyolefin microporous membrane according to the embodiment of the present invention has a tensile strength in the longitudinal direction of the film of M MD , tensile strength in the transverse direction is M TD Then, M MD and M. TD are preferably 80 MPa or more. The tensile strength is more preferably 90 MPa or more, even more preferably 100 MPa or more, most preferably 110 MPa or more, and particularly preferably 150 MPa or more. If the tensile strength is less than 90 MPa, when the thin film is wound, short circuiting due to foreign matter in the battery or the like may occur easily, and the safety of the battery may be reduced. From the viewpoint of improving safety, a higher tensile strength is preferable, but there is often a trade-off between lowering the shutdown temperature and improving the tensile strength, and the upper limit is about 200 MPa. In order to set the tensile strength within the above range, it is preferable to set the raw material composition of the film within the range described later and the stretching conditions during film formation within the range described later, so that the tensile strength falls within the above range, and the increase in the peak temperature and the half-width in DSC can be suppressed.
[0025] In the embodiment of the present invention, the direction parallel to the film production direction is referred to as the film production direction or longitudinal direction or MD direction, and the direction perpendicular to the film production direction within the film plane is referred to as the width direction or TD direction.
[0026] The tensile elongation in the MD direction (tensile elongation at break) and the tensile elongation in the TD direction of the polyolefin microporous membrane are not particularly limited, but are, for example, from 40% to 300%, preferably from 50% to 200%, more preferably from 60% to 200%, and even more preferably from 70% to 150%. When the tensile elongation in the MD direction is within the above range, deformation is unlikely to occur even when high tension is applied during coating, and wrinkles are unlikely to occur, so that coating defects are suppressed and the flatness of the coating surface is good, which is preferable.
[0027] The tensile elongation in the TD direction of the polyolefin microporous membrane (tensile elongation at break) is preferably 60% or more, more preferably 70% or more. When the tensile elongation in the TD direction is in the above range, the membrane has excellent impact resistance that can be evaluated by an impact test or the like, and when the polyolefin microporous membrane is used as a separator, the separator can follow the unevenness of the electrodes, deformation of the battery, internal stress caused by heat generation of the battery, and the like, which is preferable.
[0028] The MD tensile elongation and the TD tensile elongation are values measured by a method in accordance with ASTM D882.
[0029] The polyolefin microporous membrane according to the embodiment of the present invention preferably has a shutdown temperature of 135°C or less. More preferably, it is 133°C or less, even more preferably, it is 130°C or less, and most preferably, it is 128°C or less. If the shutdown temperature is 135°C or less, safety is improved when the membrane is used as a battery separator for secondary batteries that require high energy density, high capacity, and high output, such as electric vehicles. From the viewpoint of safety, a low shutdown temperature is preferable, but if the shutdown temperature is 80°C or less, the pores will close even under normal use conditions, and the battery characteristics will deteriorate, so the lower limit of the shutdown temperature is about 80°C. In order to set the shutdown temperature in the above range, it is preferable that the raw material composition of the film is in the range described below, and the stretch ratio during film formation is 25 to 100 times, and the heat setting temperature is in the range of 70 to 135°C.
[0030] In an embodiment of the present invention, a specific polyethylene-based resin described below is used as a raw material, the raw material composition is within the range described below, and the stretching conditions and heat setting conditions during film production are within the ranges described below, thereby achieving both high strength and low shutdown temperature without decreasing the shutdown speed.
[0031] The polyolefin microporous membrane according to the embodiment of the present invention preferably has a meltdown temperature of 160°C or higher. More preferably, it is 162°C or higher, even more preferably, it is 165°C or higher, and most preferably, it is 168°C or higher. If the meltdown temperature is 160°C or higher, safety is improved when the membrane is used as a battery separator for secondary batteries that require high energy density, high capacity, and high output, such as electric vehicles. From the viewpoint of safety, it is preferable that the meltdown temperature is high, but from the viewpoint of balance with other properties, the upper limit is about 250°C. In order to set the meltdown temperature in the above range, it is preferable that the raw material composition of the film is within the range described later, and that the stretching conditions and heat setting conditions during film formation are within the range described later.
[0032] The polyolefin microporous membrane in the embodiment of the present invention is preferably a single layer. The single layer here refers to a structure in which layers with different compositions, raw materials used, and physical properties are not arranged in the thickness direction of the polyolefin microporous membrane. If it is a single layer, it is preferable that the manufacturing process is simpler than a laminate in which two or more layers with different compositions, raw materials used, and physical properties are arranged in the thickness direction of the polyolefin microporous membrane, and it is also possible to make the membrane thinner.
[0033] Usually, in order to achieve both the shutdown property and the meltdown property, a method of laminating a layer that lowers the shutdown temperature and a layer that raises the meltdown temperature has been common. However, in the thin microporous membranes that will be required in the future, lamination may result in the thickness of each layer being too thin, making it difficult to express the properties of each layer, or causing large thickness unevenness and lamination unevenness, resulting in large variations in physical properties. On the other hand, in order to achieve both the shutdown property and the meltdown property in a single-layer microporous membrane, it is necessary to uniformly knead raw materials with different properties, but uniform kneading is difficult with conventional technology, and furthermore, the unevenness of kneading becomes more pronounced in thin films, so it has been difficult to obtain a single-layer microporous membrane that is thin and has both excellent shutdown property and meltdown property.
[0034] The polyolefin microporous membrane according to the embodiment of the present invention preferably has an average pore size of 50 nm or less. More preferably, it is 40 nm or less, even more preferably, it is 30 nm or less, and most preferably, it is 25 nm or less. The above preferred ranges are preferable because they improve resistance to dendrites and prevent internal short circuits. From the above viewpoints, the smaller the average pore size, the better, but if it is too small, the ion permeability becomes insufficient and the output characteristics of the battery may decrease, so the lower limit is about 10 nm. To make the average pore size within the above range, it is preferable to use at least a high molecular weight material and a polyolefin (B) described later as raw materials for the film, and to set the stretching ratio during film formation to a range of 25 to 100 times.
[0035] The polyolefin microporous membrane according to the embodiment of the present invention preferably has a ratio of average pore size to maximum pore size (average pore size / maximum pore size) of 0.7 to 1.0. More preferably, it is 0.72 to 1.0, even more preferably 0.75 to 1.0, and most preferably 0.8 to 1.0. When the (average pore size / maximum pore size) is 0.7 or more, the pore size uniformity is high, so that even when used as a thin-film separator for high-power batteries, micro-short circuit caused by dendrites can be suppressed. The upper limit is 1.0 based on the measurement principle. In order to set the (average pore size / maximum pore size) in the above range, it is preferable that the raw material composition of the film is within the range described below, and the stretching conditions during film formation are within the range described below.
[0036] Next, raw materials for the polyolefin microporous membrane according to the embodiment of the present invention will be described, but are not necessarily limited thereto.
[0037] The microporous polyolefin membrane according to the embodiment of the present invention is a film mainly composed of a polyolefin resin. Here, in the present invention, the term "main component" means that the proportion of a specific component in the total components is 50% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and most preferably 99% by mass or more.
[0038] The polyolefin resin used in the embodiment of the present invention may be a polyolefin composition. Examples of the polyolefin resin include polyethylene-based resins and polypropylene-based resins, and two or more of these may be blended together.
[0039] The polyolefin microporous membrane according to the embodiment of the present invention is preferably composed mainly of a polyethylene-based resin. The polyethylene-based resin referred to here includes not only ethylene homopolymers but also copolymers of other monomers.
[0040] The microporous polyolefin membrane according to an embodiment of the present invention contains a polyethylene resin and a polyolefin other than polyethylene (B). First, the polyethylene resin will be described.
[0041] As described above, the polyethylene-based resin includes not only ethylene homopolymers but also copolymers of other monomers, and various polyethylenes can be used, such as ultra-high molecular weight polyethylene, high density polyethylene, medium density polyethylene, and low density polyethylene.
[0042] As for copolymerization of other monomers, it is preferable to use a copolymer containing other α-olefins in order to lower the melting point and crystallinity of the raw material. Examples of α-olefins include propylene, butene-1, hexene-1, pentene-1, 4-methylpentene-1, octene, vinyl acetate, methyl methacrylate, and styrene. As a copolymer containing α-olefins (ethylene-α-olefin copolymers), it is preferable to use a copolymer containing hexene-1, and more preferably, an ethylene-1-hexene copolymer is used as the main component. In addition, the α-olefin is preferably C 13 This can be confirmed by measuring with -NMR.
[0043] Polyethylene resins have excellent melt extrusion properties and uniform stretching properties, so they are used as high-density polyethylene (density 0.920 g / cm 3 More than 0.970g / cm 3 It is preferable to use polyethylene (hereinafter referred to as polyethylene) as the main component.
[0044] High density polyethylene includes linear high density polyethylene and branched high density polyethylene, and it is particularly preferable to include branched high density polyethylene (branched HDPE). Branched high density polyethylene is more preferable because it is difficult for in-plane crystal orientation to proceed, changes in the crystal structure can be suppressed, and the shutdown temperature can be reduced. Furthermore, even if the stretching ratio is increased, crystal orientation does not proceed easily, and the generation of high melting point components can be suppressed, so it is also possible to suppress an increase in the half-width of the peak in DSC. As a result, it is possible to achieve high strength and thin film by high-ratio stretching while maintaining the shutdown speed.
[0045] The melting point of the high-density polyethylene is preferably 130° C. or higher and 135° C. or lower. If the melting point is 130° C. or higher, a decrease in porosity can be suppressed, and if the melting point is 135° C. or lower, an increase in shutdown temperature can be suppressed.
[0046] That is, in the embodiment of the present invention, the polyolefin resin or the polyolefin resin used for the purpose of lowering the shutdown temperature is particularly preferably in the form of a polyolefin resin having a Mw of 1.0×10 5 ~1.0×10 6 It is also preferable that the polyethylene has a melting point of 130 to 135° C., and that the polyethylene accounts for 50% by mass or more when the entire polyolefin resin is taken as 100% by mass.
[0047] Furthermore, adding low-molecular-weight polyethylene such as low-density polyethylene, linear low-density polyethylene, ethylene-α-olefin copolymer produced with a single-site catalyst, or low-molecular-weight polyethylene with a weight-average molecular weight of 1,000 to 100,000 to a polyethylene resin provides a shutdown function at low temperatures, improving the properties of the battery separator. However, if the content of the above-mentioned low-molecular-weight polyethylene in a polyethylene resin is high, the porosity of the microporous membrane decreases during the membrane production process. Therefore, the content of low-molecular-weight polyethylene should be such that the density of the ethylene-α-olefin copolymer is 0.94 g / cm or less. 3 It is preferable to adjust the density so that it exceeds 100%, and it is more preferable to adjust the density by adding a branched high-density polyethylene having a long-chain branched component.
[0048] From the above viewpoints, the molecular weight distribution of the polymer constituting the polyolefin microporous membrane according to the embodiment of the present invention is preferably such that the amount of components having a molecular weight of less than 40,000 is less than 20%, more preferably such that the amount of components having a molecular weight of less than 20,000 is less than 20%, and even more preferably such that the amount of components having a molecular weight of less than 10,000 is less than 20%.
[0049] In addition, the polyolefin microporous membrane according to the embodiment of the present invention contains a polyolefin (B) other than polyethylene in order to improve meltdown properties. The polyolefin (B) is not particularly limited, and polypropylene resins, polymethylpentene resins, polybutene resins, polyacetal resins, styrene resins, polyphenylene ether resins, etc. can be used, but polypropylene resins are preferred from the viewpoint of kneadability and electrical stability when used as a separator. As for the type of polypropylene resin, in addition to propylene homopolymers, block copolymers and random copolymers can also be used. The block copolymers and random copolymers can contain copolymer components with other α-ethylenes other than propylene, and the other α-ethylenes are preferably ethylene.
[0050] The upper limit of the content of polyolefin (B) in the polyolefin microporous membrane is preferably 40% by mass or less, more preferably 35% by mass or less, based on the total mass of the polyolefin microporous membrane. The lower limit of the content of polyolefin (B) is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, particularly preferably 20% by mass or more, and most preferably 22% by mass or more. If the content of polyolefin (B) is 40% by mass or less, the pore size of the microporous membrane becomes large, sufficient permeability is obtained, the strength is excellent, and the rise in the shutdown temperature can be suppressed. If the content of polyolefin (B) is 5% by mass or more, it has a co-continuous structure with the polyolefin resin, which is the main component, and the effect of improving the meltdown temperature by polyolefin (B) is easily expressed.
[0051] The melting point of the polyolefin (B) to be added is preferably 150° C. or higher, more preferably 155° C. or higher, and further preferably 160° C. or higher.
[0052] Furthermore, the molecular weight of the polyolefin (B) is 5.0×10 5 More preferably, it is 10×10 or more. 5More preferably, it is 15×10 5 The upper limit of the weight average molecular weight is 10 × 10 6 It is preferable that the value is equal to or less than 8.0×10 6 It is preferable that the value is equal to or less than 5.0×10 6 or less, and most preferably 3.0×10 6 When the molecular weight is within the above range, the strength of the obtained polyolefin microporous film is sufficient and the meltdown temperature can be increased, which is preferable.
[0053] As described below, the microporous polyolefin membrane according to the embodiment of the present invention is preferably produced using a polyolefin resin solution prepared by dissolving the polyolefin resin used in the embodiment of the present invention in a plasticizer by heating.
[0054] The polyolefin resin contained in the polyolefin resin solution, high-density polyethylene, has a weight-average molecular weight (Mw) of 1.0×10 4 Above 1.0×10 6 It is preferable that the value is less than 5.0×10 4 More than 3.5×10 5 More preferably, it is 1.0×10 5 More than 2.5 x 10 5 More preferably, it is 1.0×10 5 Above 2.0×10 5 It is particularly preferable that the weight average molecular weight is within the above range. When the weight average molecular weight is within the above range, excessive in-plane crystal orientation is unlikely to occur during film formation, and the change in the crystal structure of the polyolefin microporous membrane is easily controlled within an appropriate range, so that the shutdown property can be improved and deterioration of permeability can be suppressed. In addition, this is preferable because it leads to an increase in the strength of the polyolefin microporous membrane.
[0055] The polyolefin other than polyethylene contained in the polyolefin resin solution has a weight average molecular weight of 5.0 × 10 5 More preferably, it is 10×10 or more. 5 More preferably, it is 15×105 The upper limit of the weight average molecular weight is 10 × 10 6 It is preferable that the value is equal to or less than 8.0×10 6 It is preferable that the value is equal to or less than 5.0×10 6 or less, and most preferably 3.0×10 6 The molecular weight is 5.0×10 5 When the thickness is 10×10 or more, the strength of the resulting polyolefin microporous membrane is sufficient, which is preferable. 6 It is preferable to use the raw materials described below, since the viscosity does not become too high during melt-kneading in the production process and the raw materials can be kneaded uniformly.
[0056] The melting point of the polyolefin other than polyethylene is preferably 150° C. or higher, more preferably 155° C. or higher, and further preferably 160° C. or higher. This range is preferable because it allows the meltdown temperature to be high.
[0057] The blending ratio of polyolefin resin and plasticizer is 100% by mass, and the content of polyolefin resin may be appropriately selected within a range that does not impair molding processability, but is 10 to 50% by mass. If the polyolefin resin is less than 10% by mass (if the plasticizer is 90% by mass or more), swelling and necking are large at the outlet of the die when molding into a sheet, and the moldability of the sheet deteriorates and the film formability decreases. On the other hand, if the polyolefin resin exceeds 50% by mass (if the plasticizer is 50% by mass or less), shrinkage in the film thickness direction increases and molding processability also decreases.
[0058] In addition, the polyolefin microporous membrane according to the embodiment of the present invention may contain various additives such as antioxidants, heat stabilizers, antistatic agents, ultraviolet absorbers, antiblocking agents, and fillers, within the scope of the present invention. In particular, it is preferable to add an antioxidant for the purpose of suppressing oxidative deterioration due to thermal history of polyethylene resin. As the antioxidant, it is preferable to use one or more selected from, for example, 2,6-di-t-butyl-p-cresol (BHT: molecular weight 220.4), 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene (e.g., BASF's "Irganox" (registered trademark) 1330: molecular weight 775.2), tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane (e.g., BASF's "Irganox" (registered trademark) 1010: molecular weight 1177.7), etc. Appropriate selection of the type and amount of antioxidant and heat stabilizer is important for adjusting or enhancing the properties of the microporous membrane.
[0059] The polyolefin microporous membrane according to the embodiment of the present invention is obtained by biaxially stretching the above-mentioned raw material. As the biaxial stretching method, any of the inflation method, simultaneous biaxial stretching method, and sequential biaxial stretching method can be used, among which, it is preferable to adopt the simultaneous biaxial stretching method or the sequential biaxial stretching method in terms of film formation stability, thickness uniformity, and control of high rigidity and dimensional stability of the film.
[0060] Next, a method for producing a polyolefin microporous membrane according to an embodiment of the present invention will be described, but is not necessarily limited thereto. The method for producing a polyolefin microporous membrane according to an embodiment of the present invention comprises the following steps (a) to (e). (a) A polyolefin solution is prepared by kneading and dissolving polymer materials including a polyolefin alone, a polyolefin mixture, a polyolefin solvent (plasticizer) mixture, additives, and a polyolefin mixture. (b) The melt is extruded, formed into a sheet, and cooled to solidify. (c) The obtained sheet is stretched by a roll method or a tenter method. (d) The plasticizer is then extracted from the resulting stretched film and the film is dried. (e) This is followed by heat treatment / re-stretching / heat setting.
[0061] Each step will be described below.
[0062] (a) Preparation of polyolefin resin solution The polyolefin resin used in the embodiment of the present invention is heated and dissolved in a plasticizer to prepare a polyolefin resin solution. The plasticizer is not particularly limited as long as it is a solvent that can sufficiently dissolve the polyolefin resin, but in order to enable relatively high-magnification stretching, it is preferable that the solvent is liquid at room temperature. Examples of the solvent include aliphatic, cycloaliphatic, or aromatic hydrocarbons such as nonane, decane, decalin, paraxylene, undecane, dodecane, and liquid paraffin, and mineral oil fractions having boiling points corresponding thereto, as well as phthalic acid esters that are liquid at room temperature, such as dibutyl phthalate and dioctyl phthalate. In order to obtain a gel-like sheet with a stable content of liquid solvent, it is preferable to use a non-volatile liquid solvent such as liquid paraffin. A solvent that is miscible with the polyolefin resin in the melt-kneaded state but is solid at room temperature may be mixed with the liquid solvent. Examples of such solid solvents include stearyl alcohol, ceryl alcohol, and paraffin wax. However, if only a solid solvent is used, there is a risk of uneven stretching and the like occurring.
[0063] The viscosity of the liquid solvent is preferably 20 to 200 cSt at 40°C. If the viscosity at 40°C is 20 cSt or more, the sheet extruded from the die of the polyolefin resin solution is less likely to become non-uniform. On the other hand, if the viscosity is 200 cSt or less, the liquid solvent is easily removed. The viscosity of the liquid solvent is measured at 40°C using an Ubbelohde viscometer.
[0064] When two or more types of polyethylene are blended into the polyethylene resin used in the embodiment of the present invention, the weight average molecular weight is preferably 1.0×10 6 Above 4.0×10 6It is preferable to use ultra-high molecular weight polyethylene having a molecular weight of less than 1000 nm. By containing ultra-high molecular weight polyethylene, it is possible to make the pores finer and to improve heat resistance, and furthermore, it is possible to improve strength and elongation. The ultra-high molecular weight polyethylene may be not only an ethylene homopolymer, but also a copolymer containing a small amount of other α-olefin. The other α-olefins other than ethylene may be the same as those described above.
[0065] Furthermore, since the molecular weight of the main raw material or the raw material used for lowering the shutdown temperature is relatively small, when the raw material is molded into a sheet, there is a tendency for swelling and necking to be large at the outlet of the die, which deteriorates the moldability of the sheet. Adding ultra-high molecular weight polyethylene as a secondary material increases the viscosity and strength of the sheet and increases the process stability, so it is preferable to add ultra-high molecular weight polyethylene. However, if the proportion of ultra-high molecular weight polyethylene is 50% by mass or more, the extrusion load increases and the extrusion moldability decreases, so the amount of ultra-high molecular weight polyethylene added is preferably less than 50% by mass of the total amount of polyolefin resin.
[0066] (b) Formation of an extrudate and formation of a gel-like sheet The homogeneous melt kneading of the polyolefin resin solution is not particularly limited, but when a high-concentration polyolefin resin solution is to be prepared, it is preferable to carry out the melt kneading in a twin-screw extruder. If necessary, various additives such as an antioxidant may be added within a range that does not impair the effects of the present invention. In particular, it is preferable to add an antioxidant to prevent oxidation of the polyolefin resin.
[0067] Since the polyolefin microporous membrane according to the embodiment of the present invention is a single-layer microporous membrane containing a polyethylene resin and a polyolefin (B) other than polyethylene, it is necessary to uniformly knead and extrude a plurality of raw materials with different melting points. If the kneading state is not uniform, the strength and meltdown temperature of the microporous membrane may decrease, or the pore size may vary widely. In order to knead uniformly, it is preferable to set the melting point of the raw material with the lowest melting point among the polyethylene resin and polyolefin (B) used in the first half of the extruder to Tm1+30°C or less, and to mix the raw materials uniformly before they melt. Next, in the second half of the extruder, the polyolefin resin solution is mixed uniformly at a temperature at which the polyethylene resin and polyolefin (B) are completely melted. The melt kneading temperature is preferably (Tm2-10°C) to (Tm2+120°C), where Tm2 is the melting point of the raw material with the highest melting point among the polyethylene resin and polyolefin (B) used. More preferably, it is (Tm2+20°C) to (Tm2+100°C). Here, the melting point refers to a value measured by DSC based on JIS K7121 (1987) (hereinafter the same). For example, when a polyethylene resin and a polypropylene resin are used, the melt kneading temperature is preferably 160°C or less in the first half of the extruder and 150 to 280°C in the second half.
[0068] From the viewpoint of suppressing deterioration of the resin, the melt-kneading temperature is preferably low, but if the temperature is lower than the above-mentioned temperature, unmelted material may be generated in the extrudate extruded from the die, which may cause film breakage in the subsequent stretching process, and if the temperature is higher than the above-mentioned temperature, the thermal decomposition of the polyolefin resin becomes intense, and the physical properties of the obtained microporous film, such as strength and porosity, may be inferior. In addition, the decomposition product may precipitate on the chill roll or the roll in the stretching process, and adhere to the sheet, leading to deterioration of the appearance. Therefore, it is preferable to knead within the above-mentioned range.
[0069] Next, the obtained extrudate is cooled to obtain a gel-like sheet, and the microphase of the polyolefin resin separated by the solvent can be fixed by cooling. In the cooling step, it is preferable to cool to 10 to 50°C. This is because it is preferable to set the final cooling temperature below the crystallization end temperature, and by making the high-order structure finer, it becomes easier to perform uniform stretching in the subsequent stretching. Therefore, it is preferable to cool at a rate of 30°C / min or more at least until the temperature is below the gelation temperature. If the cooling rate is less than 30°C / min, the crystallization degree increases and it is difficult to obtain a gel-like sheet suitable for stretching. In general, if the cooling rate is slow, relatively large crystals are formed, so the high-order structure of the gel-like sheet becomes coarse, and the gel structure that forms it also becomes large. On the other hand, if the cooling rate is fast, relatively small crystals are formed, so the high-order structure of the gel-like sheet becomes dense, leading to high strength and uniform pore size.
[0070] The cooling method may be a method of directly contacting the material with cold air, cooling water or other cooling medium, a method of contacting the material with a roll cooled with a cooling medium, or a method using a casting drum or the like.
[0071] In addition, the polyolefin microporous membrane according to the embodiment of the present invention is preferably a single layer from the viewpoint of process simplification and thinning, but is not limited to a single layer and may be a laminate. There is no particular limit to the number of layers, and it may be a two-layer laminate or a three-layer laminate or more. As described above, the laminated portion may contain desired resins in addition to polyethylene to the extent that the effect of the present invention is not impaired. As a method for making the polyolefin microporous membrane into a laminate, a conventional method can be used, but for example, there is a method of forming a laminate by preparing desired resins as needed, separately feeding these resins to an extruder and melting them at a desired temperature, joining them in a polymer tube or die, and extruding them from a slit-shaped die to the desired thickness.
[0072] (c) Stretching process The obtained gel-like sheet (including laminated sheet) is stretched. Examples of the stretching method include uniaxial stretching in the sheet conveying direction (MD direction) by a roll stretching machine, uniaxial stretching in the sheet width direction (TD direction) by a tenter, sequential biaxial stretching by a combination of a roll stretching machine and a tenter or a tenter and a tenter, and simultaneous biaxial stretching by a simultaneous biaxial tenter. The stretching ratio varies depending on the thickness of the gel-like sheet from the viewpoint of uniformity of the film thickness, but it is preferable to stretch 5 times or more in any direction. The area ratio is preferably 25 times or more, more preferably 36 times or more, even more preferably 49 times or more, and most preferably 64 times or more. If the area ratio is less than 25 times, the stretching is insufficient, the uniformity of the film is easily impaired, and a microporous film with excellent strength is not obtained. The area ratio is preferably 100 times or less. Increasing the area ratio makes the microporous membrane more susceptible to breakage during production, reducing productivity, while increasing the crystallinity due to increased orientation improves the melting point and strength of the microporous membrane. However, increasing the crystallinity means decreasing the amorphous portion, which increases the melting point and shutdown temperature of the film.
[0073] The stretching temperature is preferably set to the melting point of the gel-like sheet + 10°C or less, and more preferably in the range of (crystal dispersion temperature Tcd of polyolefin resin) to (melting point of gel-like sheet + 5°C). Specifically, since the polyethylene composition has a crystal dispersion temperature of about 90 to 100°C, the stretching temperature is preferably 90 to 125°C, more preferably 90 to 120°C. The crystal dispersion temperature Tcd is determined from the temperature characteristics of dynamic viscoelasticity measured according to ASTM D 4065. Alternatively, it may be determined from NMR. If it is less than 90°C, the opening of holes becomes insufficient due to low-temperature stretching, making it difficult to obtain a uniform film thickness, and the porosity is also low. If it is higher than 125°C, the sheet melts and the holes are easily blocked.
[0074] The stretching as described above causes the higher-order structure formed in the gel sheet to cleave, the crystal phase to become finer, and a large number of fibrils to be formed. The fibrils form a network structure that is irregularly connected three-dimensionally. The stretching improves the mechanical strength and expands the pores, making it suitable for battery separators. In addition, by stretching before removing the plasticizer, the polyolefin resin is in a sufficiently plasticized and softened state, so that the higher-order structure can be smoothly cleaved and the crystal phase can be uniformly refined. In addition, because the stretching is easy, distortion during stretching is less likely to remain, and the thermal shrinkage rate can be reduced compared to the case of stretching after removing the plasticizer.
[0075] (d) Plasticizer extraction (washing) and drying process Next, the plasticizer (solvent) remaining in the gel-like sheet is removed using a cleaning solvent. Since the polyolefin resin phase and the solvent phase are separated, a microporous membrane is obtained by removing the solvent. Examples of cleaning solvents include saturated hydrocarbons such as pentane, hexane, and heptane, chlorinated hydrocarbons such as methylene chloride and carbon tetrachloride, ethers such as diethyl ether and dioxane, ketones such as methyl ethyl ketone, and chain fluorocarbons such as trifluoroethane. These cleaning solvents have low surface tension (for example, 24 mN / m or less at 25°C). By using a cleaning solvent with low surface tension, shrinkage due to the surface tension of the gas-liquid interface during drying after cleaning is suppressed in the network structure that forms micropores, and a microporous membrane with good porosity and permeability is obtained. These cleaning solvents are appropriately selected according to the plasticizer and used alone or in combination.
[0076] The washing method can be a method of immersing the gel-like sheet in a washing solvent and extracting it, a method of showering the washing solvent on the gel-like sheet, or a combination of these methods. The amount of washing solvent used varies depending on the washing method, but is generally preferably 300 parts by mass or more per 100 parts by mass of the gel-like sheet. The washing temperature may be 15 to 30°C, and is heated to 80°C or less as necessary. At this time, the longer the time that the gel-like sheet is immersed in the washing solvent, the better, from the viewpoint of enhancing the washing effect of the solvent, preventing the physical properties of the resulting polyolefin microporous membrane from becoming non-uniform in the TD direction and / or MD direction, and improving the mechanical and electrical properties of the polyolefin microporous membrane. The washing as described above is preferably performed until the residual solvent in the washed gel-like sheet, i.e., the polyolefin microporous membrane, is less than 1% by mass.
[0077] Thereafter, the solvent in the polyolefin microporous membrane is dried and removed in a drying step. The drying method is not particularly limited, and a method using a metal heating roll or a method using hot air can be selected. The drying temperature is preferably 40 to 100°C, more preferably 40 to 80°C. If the drying is insufficient, the porosity of the polyolefin microporous membrane decreases in the subsequent heat fixation, and the permeability deteriorates.
[0078] (e) Heat treatment / re-stretching / heat setting process The dried polyolefin microporous membrane may be stretched (restretched) at least uniaxially. The restretching may be performed by a tenter method or the like while heating the microporous membrane, similar to the above-mentioned stretching. The restretching may be uniaxial or biaxial. In the case of multistage stretching, simultaneous biaxial and / or sequential stretching may be combined.
[0079] The re-stretching temperature is preferably equal to or lower than the melting point of the polyolefin composition, more preferably within the range of (Tcd-20°C) to the melting point. Specifically, the temperature is preferably 70 to 135°C, more preferably 110 to 132°C, and most preferably 120 to 130°C.
[0080] In the case of uniaxial stretching, the re-stretching ratio is preferably 1.01 to 1.6 times, particularly in the TD direction, preferably 1.1 to 1.6 times, more preferably 1.2 to 1.4 times. In the case of biaxial stretching, it is preferably 1.01 to 1.6 times in both the MD and TD directions. The re-stretching ratios may be different between the MD and TD directions. By stretching within the above range, the porosity and permeability can be increased, but if stretching is performed at a ratio of 1.6 or more, orientation proceeds, the melting point of the film increases, and the shutdown temperature increases. From the viewpoint of heat shrinkage and wrinkles and sagging, the relaxation rate from the maximum re-stretching ratio is preferably 0.9 or less, and more preferably 0.8 or less.
[0081] Regardless of whether re-stretching is performed or not, it is preferable to perform heat setting with the film width fixed constant. By performing heat setting, the strain stress caused by stretching can be alleviated, and the DSC peak half width becomes sharp. The heat setting temperature is preferably 70 to 135°C, more preferably 110 to 132°C, and most preferably 115 to 130°C. The heat setting time is not particularly limited, but is 1 second to 15 minutes. Within this range, it is possible to sufficiently alleviate the strain stress while suppressing pore clogging due to melting of the polyolefin resin.
[0082] (f) Other processes Furthermore, depending on other applications, the microporous membrane may be subjected to a hydrophilization treatment. The hydrophilization treatment may be performed by monomer grafting, surfactant treatment, corona discharge, or the like. The monomer grafting is preferably performed after the crosslinking treatment. The polyolefin microporous membrane is preferably subjected to a crosslinking treatment by irradiation with ionizing radiation such as α-rays, β-rays, γ-rays, or electron beams. In the case of electron beam irradiation, the electron beam dose is preferably 0.1 to 100 Mrad, and the acceleration voltage is preferably 100 to 300 kV. The crosslinking treatment increases the meltdown temperature of the polyolefin microporous membrane.
[0083] In the case of surfactant treatment, any of nonionic surfactants, cationic surfactants, anionic surfactants, and amphoteric surfactants can be used, but nonionic surfactants are preferred. The multi-layer, microporous membrane is immersed in a solution prepared by dissolving the surfactant in water or a lower alcohol such as methanol, ethanol, or isopropyl alcohol, or the solution is applied to the multi-layer, microporous membrane by a doctor blade method.
[0084] The polyolefin microporous membrane may be subjected to a surface coating of a fluorine-based resin porous body such as polyvinylidene fluoride or polytetrafluoroethylene, a porous body such as polyimide or polyphenylene sulfide, or an inorganic coating such as ceramic, for the purpose of improving the meltdown property or heat resistance when used as a battery separator.
[0085] The polyolefin microporous membrane according to the embodiment of the present invention is also preferably a laminate having a coating layer provided on at least one surface.
[0086] The polyolefin microporous membrane obtained as described above can be used for various applications such as filters, fuel cell separators, and condenser separators. In particular, when used as a battery separator, it not only has low shutdown properties and high meltdown properties but also has high strength despite being a thin film, thereby achieving both high safety functions and output properties. Therefore, it can be preferably used as a battery separator for secondary batteries that require high energy density, high capacity, and high output, such as for electric vehicles.
[0087] The present invention also relates to a battery using the microporous polyolefin membrane or laminate according to an embodiment of the present invention. EXAMPLES
[0088] The present invention will be described in detail below with reference to examples. The properties were measured and evaluated by the following methods.
[0089] 1. Measurement of molecular weight distribution of polyolefin The molecular weight distribution of polyolefin (weight average molecular weight, molecular weight distribution, content of specific components, etc.) was measured by high-temperature gel permeation chromatography (GPC) under the following measurement conditions. Equipment: High temperature GPC equipment (Equipment No. HT-GPC, manufactured by Polymer Laboratories, PL-220) Detector: Differential refractive index detector RI Guard column: Shodex G-HT Column: Shodex HT806M (2 columns) (φ7.8mm×30cm, Showa Denko) Solvent: 1,2,4-trichlorobenzene (TCB, Wako Pure Chemical Industries, Ltd.) (0.1% BHT added) Flow rate: 1.0mL / min Column temperature: 145℃ Sample preparation: 5 mL of the measurement solvent was added to 5 mg of sample, and the mixture was heated and stirred at 160 to 170°C for about 30 minutes, after which the resulting solution was filtered through a metal filter (pore size 0.5 um). Injection volume: 0.200mL Standard sample: Monodisperse polystyrene (manufactured by Tosoh) (PS) Data processing: TRC GPC data processing system
[0090] The obtained Mw and Mn were then converted into polyethylene (PE) values using the following conversion formula: Mw (PE equivalent) = Mw (PS equivalent measurement value) x 0.468 Mn (PE conversion) = Mn (PS conversion measurement value) x 0.468
[0091] 2. Film Thickness The thickness of the polyolefin microporous membrane was measured at five points within a 50 mm x 50 mm area using a contact thickness gauge, Litematic VL-50 (10.5 mmφ ultrahard spherical probe, measuring load 0.01 N) manufactured by Mitutoyo Corporation, and the average value was recorded as the thickness (μm).
[0092] 3.Air resistance For a polyolefin microporous membrane with a thickness of T1 (μm), the air permeability (sec / 100 cm) was measured in an atmosphere of 25°C using an Oken air permeability meter (manufactured by Asahi Seiko Co., Ltd., EGO-1T) in accordance with JIS P-8117. 3 The air permeability (converted to 10 μm) (sec / 100 cm) when the membrane thickness was 10 μm was also measured using the following formula: 3 ) was calculated. Formula: Air permeability (10μm conversion) (sec / 100cm 3 ) = Air permeability (sec / 100cm 3 )×10(μm) / polyolefin microporous membrane thickness(μm)
[0093] 4.Piercing strength The puncture strength was measured in accordance with JIS Z 1707 (2019), except that the test speed was 2 mm / sec. Using a force gauge (IMADA Co., Ltd., DS2-20N), the maximum load (N) was measured when a polyolefin microporous membrane was punctured in an atmosphere of 25°C with a 1.0 mm diameter needle with a spherical tip (radius of curvature R: 0.5 mm), and the puncture strength when the membrane was 10 μm thick was calculated using the following formula. Formula: Puncture strength (10 μm equivalent) (N) = Maximum load (N) × 10 (μm) / Polyolefin microporous membrane thickness (μm)
[0094] 5.Porosity (%) A sample of 50 mm × 50 mm square was cut from the polyolefin microporous membrane, and its volume (cm) at room temperature (25°C) was measured. 3 ) and mass (g). These values and the film density (g / cm 3 ) The porosity of the polyolefin microporous membrane was calculated from the following formula. Porosity (%) = (volume-mass / film density) / volume x 100
[0095] The film density is 0.99 g / cm 3 The calculations were performed assuming a constant value of
[0096] 6. Tensile strength, tensile elongation Tensile strength M MD and tensile strength M TDThe tensile elongation in the MD direction and the tensile elongation in the TD direction were measured at a speed of 100 mm / min using a rectangular test piece having a width of 30 mm in accordance with ASTM D882.
[0097] 7.Shutdown Temperature The polyolefin microporous membrane was heated at a heating rate of 5°C / min while measuring the air permeability resistance with an air permeability meter (EGO-1T, manufactured by Asahi Seiko Co., Ltd.). 5 seconds / 100cm 3 The temperature at which air reached was determined and taken as the shutdown temperature (°C).
[0098] The measurement cell was composed of an aluminum block and had a structure in which a thermocouple was placed directly under the polyolefin microporous membrane. The sample was cut into a 5 cm x 5 cm square and heated while being fixed with an O-ring around the periphery.
[0099] 8. Meltdown Temperature A 50 mm square microporous membrane was sandwiched between a pair of metal block frames with a 12 mm diameter hole, and a 10 mm diameter tungsten carbide ball was placed on the microporous membrane. The microporous membrane was placed so that it had a flat surface in the horizontal direction. The temperature was started at 30°C and increased at a rate of 5°C / min. The temperature at which the microporous membrane was ruptured by the ball was measured and was taken as the meltdown temperature (MD temperature).
[0100] 9.DSC measurement The melting point and half-width are determined by differential scanning calorimetry (DSC). This DSC was performed using a TA Instruments MDSC2920 or Q1000Tzero-DSC, and the temperature was raised from 30°C to 230°C at a rate of 10°C / min based on JIS K7121, and the temperature at the maximum value of the melting peak (peak temperature) obtained was evaluated. The peak temperature in the range below 150°C was designated as P1, and the peak temperature at 150°C or higher was designated as P2.
[0101] The half-width is 0.5 times the maximum heat generation amount Q in the region below 150°C. 1 / 2The value of T2 - T1 was calculated when the temperatures were T1 and T2 (T1 < T2), respectively. In the region below 150°C, when there are two or more maximum values and there are three or more temperatures at which Q 1 / 2 is obtained, the half-width is calculated with the minimum temperature of the corresponding temperatures as T1 and the maximum temperature as T2.
[0102] 10. Maximum pore diameter and average pore diameter Using a palm porometer (manufactured by PMI, CFP-1500A), the maximum pore diameter and average pore diameter were measured in the order of Dry-up and Wet-up. For Wet-up, pressure was applied to a porous polyolefin film sufficiently immersed in Galwick (trade name) manufactured by PMI with a surface tension of 1.59×10 -2 N / m, and the pore diameter converted from the pressure at which air began to penetrate was defined as the maximum pore diameter.
[0103] Regarding the average diameter, the pore diameter was converted from the pressure at the point where the curve showing half the slope of the pressure-flow rate curve in the Dry-up measurement intersects the curve of the Wet-up measurement. The conversion between pressure and pore diameter used the following formula. d = C·γ / P
[0104] In the above formula, "d (μm)" is the pore diameter of the porous polyolefin film, "γ (mN / m)" is the surface tension of the liquid, "P (Pa)" is the pressure, and "C" is a constant determined by the wetting tension of the immersion liquid, contact angle, etc.
[0105] Hereinafter, examples will be shown for specific description, but the present invention is not limited by these examples at all.
[0106] [Example 1] 54.6 parts by mass of branched high-density polyethylene (branched HDPE) (weight average molecular weight (Mw) 1.8×10 5 , melting point 133°C), 23.4 parts by mass of ultra-high molecular weight polyethylene (UHPE) (Mw 2.0×10 6 , melting point 133°C), and polypropylene (PP) (Mw 1.1×10 6A polyolefin composition was obtained by mixing 22.0 parts by mass of 1,2-di-t-butyl-p-cresol and 22.0 parts by mass of 1,2-di-t-butyl-p-cresol (melting point 165°C). 71.5% by mass of liquid paraffin was added to 28.5% by mass of the polyolefin composition, and 0.5% by mass of 2,6-di-t-butyl-p-cresol and 0.7% by mass of tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane were added as antioxidants based on the mass of the polyolefin in the mixture and mixed to prepare a polyethylene resin solution.
[0107] The obtained polyethylene resin solution was charged into a twin-screw extruder and kneaded at 150°C in the first half of the extruder and 180°C in the second half. The mixture was then fed into a T-die and extruded into a sheet. The extrudate was then cooled with a cooling roll controlled at 15°C to form a gel-like sheet.
[0108] The obtained gel-like sheet was stretched 7 times in the longitudinal direction at 115°C with the four sides held with clips using a film stretcher, and then stretched 7 times in the width direction (sequential stretching (area magnification 49 times)). The sheet width was then fixed in the film stretcher, and the sheet was held at a temperature of 115°C for 10 seconds and then removed.
[0109] The stretched gel-like sheet was then fixed on a metal frame and immersed in a methylene chloride bath in a cleaning tank to remove the liquid paraffin, followed by drying to obtain a microporous polyolefin membrane.
[0110] Finally, the polyolefin microporous membrane fixed on the metal frame was placed in a hot air oven and heat-set at 120°C for 10 minutes.
[0111] Table 1 shows the raw material properties of the polyolefin microporous membrane, the membrane production conditions, and the evaluation results of the microporous membrane.
[0112] [Example 2] A microporous polyolefin membrane was obtained in the same manner as in Example 1, except that the branched HDPE was 59.5 parts by mass, the UHPE was 25.5 parts by mass, and the PP was 15.0 parts by mass.
[0113] [Example 3] A polyolefin microporous membrane was obtained in the same manner as in Example 1, except that no UHPE was used, 60 mass% liquid paraffin was added to 40 mass% of a polyolefin composition consisting of 80.0 parts by mass of branched HDPE and 20.0 parts by mass of PP, and the mixture was simultaneously biaxially stretched and the heat setting temperature was 125°C.
[0114] [Example 4] A microporous polyolefin membrane was obtained in the same manner as in Example 3, except that the stretching ratio was 10 times in the longitudinal direction and 10 times in the transverse direction.
[0115] [Example 5] A polyolefin microporous membrane was obtained in the same manner as in Example 1, except that the stretching method was simultaneous biaxial stretching at a stretching ratio of 5 times in the longitudinal direction and 5 times in the transverse direction.
[0116] [Example 6] A microporous polyolefin membrane was obtained in the same manner as in Example 1, except that the branched HDPE was 62.5 parts by mass, the UHPE was 30.0 parts by mass, and the PP was 7.5 parts by mass.
[0117] [Example 7] Branched high density polyethylene (branched HDPE) (weight average molecular weight (Mw) 9.0 x 10 4 , melting point 131°C) 20.0 parts by mass, ultra-high molecular weight polyethylene (UHPE) (Mw1.0×10 6 , melting point 136°C) 70.0 parts by mass, polypropylene (PP) (Mw 1.1 × 10 6 A polyolefin composition was obtained by mixing 10.0 parts by mass of 1,2-di-t-butyl-p-cresol and 10.0 parts by mass of 1,2-di-t-butyl-p-cresol (melting point 165°C). 77% by mass of liquid paraffin was added to 23% by mass of the polyolefin composition, and 0.5% by mass of 2,6-di-t-butyl-p-cresol and 0.7% by mass of tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane were added as antioxidants based on the mass of the polyolefin in the mixture and mixed to prepare a polyethylene resin solution.
[0118] The obtained polyethylene resin solution was charged into a twin-screw extruder and kneaded at 180°C, fed into a T-die, and extruded into a sheet. The extrudate was then cooled with a cooling roll controlled at 15°C to form a gel-like sheet.
[0119] The obtained gel-like sheet was stretched 5 times in the longitudinal direction at 115°C with the four sides held with clips using a film stretcher, and then stretched 5 times in the width direction (simultaneous stretching (area magnification 25 times)). The sheet width was fixed in the film stretcher and held at a temperature of 115°C for 10 seconds, and then removed.
[0120] The stretched gel-like sheet was then fixed on a metal frame and immersed in a methylene chloride bath in a cleaning tank to remove the liquid paraffin, followed by drying to obtain a microporous polyolefin membrane. Finally, the polyolefin microporous membrane fixed on the metal frame was placed in a hot air oven and heat-set at 130°C for 10 minutes.
[0121] [Example 8] A microporous polyolefin membrane was obtained in the same manner as in Example 7, except that the branched HDPE was 20.0 parts by mass, the UHPE was 75.0 parts by mass, and the PP was 5.0 parts by mass.
[0122] [Comparative Example 1] Instead of branched HDPE, linear HDPE (Mw3.0×10 5 A microporous polyolefin membrane was obtained in the same manner as in Example 1, except that a polyolefin copolymer having a melting point of 136°C was used and the temperature of the twin-screw extruder was kept constant at 180°C.
[0123] [Comparative Example 2] A microporous polyolefin membrane was obtained in the same manner as in Comparative Example 1, except that the stretching method was simultaneous biaxial stretching at a stretching ratio of 5 times in the longitudinal direction and 5 times in the transverse direction.
[0124] [Comparative Example 3] A polyolefin microporous membrane was obtained in the same manner as in Example 3, except that no PP was used, 75.0 mass% liquid paraffin was added to 25 mass% polyolefin composition consisting of 40.0 parts by mass of branched HDPE and 60.0 parts by mass of UHPE, the stretching temperature was 110°C, and the heat setting temperature was 115°C.
[0125] [Comparative Example 4] Instead of branched HDPE, linear HDPE (Mw3.0×10 5 A microporous polyolefin membrane was obtained in the same manner as in Example 6, except that a polyolefin copolymer (melting point 136°C) was used, the temperature of the twin-screw extruder was constant at 180°C, and the heat setting temperature was 120°C.
[0126] [Comparative Example 5] A polyolefin microporous membrane was obtained in the same manner as in Comparative Example 2, except that 70% by mass of liquid paraffin was added to 30.0% by mass of a polyolefin composition consisting of 80.0 parts by mass of linear HDPE and 20.0 parts by mass of PP, the stretching ratio was 8 times in the longitudinal direction and 8 times in the transverse direction, and the heat setting temperature was 125°C.
[0127] The evaluation results of the obtained microporous polyolefin membrane are shown in Tables 1 and 2.
[0128] In addition, "Linear HDPE" in Tables 1 and 2 refers to linear high-density polyethylene.
[0129] [Table 1]
[0130] [Table 2] [Industrial Applicability]
[0131] The polyolefin microporous membrane of the present invention has high strength and low shutdown and high meltdown properties when used as a battery separator, and has high safety and excellent output characteristics. Therefore, it can be suitably used as a battery separator or laminate for batteries and secondary batteries that require high energy density, high capacity, and high output, such as for electric vehicles.
[0132] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made therein without departing from the spirit and scope of the invention.
[0133] This application is based on a Japanese patent application (Patent Application No. 2019-152105) filed on August 22, 2019, the contents of which are incorporated herein by reference.
Claims
1. The composition comprises a polyethylene resin and a polyolefin other than polyethylene (B), In a differential scanning calorimeter (DSC), it has peaks below 150° C. and above 150° C., The polyolefin microporous film has a half-width of a peak at less than 150°C of 10°C or less, a 10 μm converted pin puncture strength of 2.0 N or more, and a meltdown temperature of 162°C or more.
2. The microporous polyolefin membrane according to claim 1, which further has a peak at 135° C. or lower in DSC.
3. The microporous polyolefin membrane according to claim 1 or 2, which is a single layer.
4. The microporous polyolefin membrane according to any one of claims 1 to 3, wherein the content of the polyolefin other than polyethylene (B) is 10 mass% or more.
5. The microporous polyolefin membrane according to any one of claims 1 to 4, wherein the polyolefin other than polyethylene (B) is a polypropylene-based resin.
6. The microporous polyolefin membrane according to any one of claims 1 to 5, having a shutdown temperature of 135°C or lower.
7. The microporous polyolefin membrane according to any one of claims 1 to 6, having a membrane thickness of 10 µm or less.
8. The microporous polyolefin membrane according to any one of claims 1 to 7, which has a peak at 120°C or higher in a differential scanning calorimeter (DSC).
9. A laminate comprising the polyolefin microporous membrane according to any one of claims 1 to 8 and a coating layer provided on at least one surface of the membrane.
10. A battery using the polyolefin microporous membrane according to any one of claims 1 to 8 or the laminate according to claim 9.
Citation Information
Patent Citations
Polyolefin fine porous film and method of manufacturing the same
JP2002194132A
Polyolefin fine porous membrane and method for producing the same and use
JP2004196871A
Microporous polyolefin film
JP2005200578A
Polyolefin multilayer microporous membrane, method for producing the same, separator for batteries, and battery
JP2010537845A
Heat-resistance improved polyolefin microporous membrane and production method therefor
JP2013057045A