Optical film manufacturing method
By heating and solvent-contacting crystalline resin films within a specific temperature range and stretching, the method effectively addresses the challenge of changing birefringence in optical films, ensuring high quality and efficiency.
Patent Information
- Application Number
- JP2021013201
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-01-29
Smart Images

Figure 0007585829000002 
Figure 0007585829000003 
Figure 0007585829000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an optical film. [Background technology]
[0002] It has been known that crystalline resins are molded into films for use in various applications. In addition, it is known that in the process of producing such films, the raw film is stretched and then brought into contact with a hydrocarbon solvent, thereby improving the dimensional stability of the finished film when heated (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-026909 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present inventors have conducted various studies on changing the physical properties of a crystalline resin by contacting it with a solvent, and have found that the birefringence in the thickness direction of the film can be changed by contacting it with the solvent, and that as a result, a film useful as an optical film can be produced that has special optical properties that cannot be produced by a normal production method such as simply stretching a resin for optical films that has a normal positive intrinsic birefringence.
[0005] However, when the birefringence in the thickness direction is changed by contacting a crystalline resin with a solvent, it is necessary to contact the crystalline resin with the solvent sufficiently to obtain a desired change in the birefringence. On the other hand, from the viewpoint of production efficiency, it is required that the time for such contact is short. In order to meet such a requirement, the present inventors have considered performing the contact step with the solvent at an elevated temperature. However, when the solvent temperature is elevated, undesirable phenomena such as the film easily becoming cloudy occur, and an optical film of good quality cannot be obtained.
[0006] Therefore, an object of the present invention is to provide a method for producing an optical film, which can easily achieve a change in birefringence in the thickness direction and suppresses undesirable phenomena such as clouding of the film. [Means for solving the problem]
[0007] The present inventors have conducted research to solve the above problems. As a result, the present inventors have found that the above problems can be solved by heating the film, not the solvent, and setting the temperature within a specific range in the solvent contact step. Based on this finding, the present inventors have completed the present invention. That is, the present invention includes the following.
[0008] [1] A step (I) of preparing a film (pA) having a layer made of a crystalline resin (a) having a glass transition temperature TgR (°C); A step (II) of heating the film (pA); and (III) contacting at least one side of the film (pA) with a solvent while the temperature Tf of the film (pA) is in a state in which the temperature Tf is equal to or higher than (TgR-50)°C and equal to or lower than (TgR-20)°C, thereby changing the birefringence in the thickness direction of the film (pA) to obtain a film (qA). [2] The method for producing an optical film according to [1], wherein the step (II) includes heating the film (pA) in an oven. [3] The method for producing an optical film according to [1] or [2], wherein the step (II) includes transporting the film (pA) in a state of contact with a heated roll. [4] The method for producing an optical film according to any one of [1] to [3], further comprising a step (IV) of stretching the film (qA). [5] The method for producing an optical film according to any one of [1] to [4], wherein the optical film has an Nz coefficient greater than 0 and less than 1. [6] The method for producing an optical film according to any one of [1] to [5], wherein the optical film is a single-layer film. [7] The method for producing an optical film according to any one of [1] to [6], wherein the crystalline resin (a) has a positive intrinsic birefringence value. [8] The method for producing an optical film according to any one of [1] to [7], wherein the crystalline resin (a) contains an alicyclic structure-containing polymer. Effect of the Invention
[0009] According to the present invention, there is provided a method for producing an optical film, which can easily achieve a change in birefringence in the thickness direction and suppresses undesirable phenomena such as clouding of the film. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a side view that shows an outline of an example of a production apparatus for carrying out the production method of the present invention and an operation for carrying out the production method of the present invention using the same. [Diagram 2] FIG. 2 is a partial side view that illustrates an example of a heating method different from that shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0012] In the following description, the in-plane retardation Re of a layered structure such as a film is a value expressed by Re = (nx - ny) x d unless otherwise specified. The retardation Rth in the thickness direction of a layered structure is a value expressed by Rth = [{(nx + ny) / 2} - nz] x d unless otherwise specified. The Nz coefficient of a layered structure is a value expressed by (nx - nz) / (nx - ny) unless otherwise specified.
[0013] nx, ny, and nz are the principal refractive indices of the layered structure. That is, nx represents the refractive index in a direction perpendicular to the thickness direction of the layered structure (in-plane direction) and giving the maximum refractive index. ny represents the refractive index in the in-plane direction of the layered structure and perpendicular to the direction of nx. nz represents the refractive index in the thickness direction of the layered structure. d represents the thickness of the layered structure. The measurement wavelength is 590 nm unless otherwise specified.
[0014] In the following description, unless otherwise specified, a material with positive intrinsic birefringence means a material whose refractive index in the stretching direction is greater than that in the direction perpendicular thereto. Also, a material with negative intrinsic birefringence means a material whose refractive index in the stretching direction is smaller than that in the direction perpendicular thereto. The value of intrinsic birefringence can be calculated from the dielectric constant distribution.
[0015] In the following description, the slow axis of a layered structure is an in-plane slow axis unless otherwise specified.
[0016] In the following description, a "long" film refers to a film having a length of 5 times or more, preferably 10 times or more, the width, specifically a film having a length that can be wound into a roll for storage or transportation. There is no particular upper limit on the length, but it is usually 100,000 times or less the width.
[0017] [Optical film manufacturing method: Overview] The method for producing an optical film of the present invention includes the following steps (I) to (III): The method for producing an optical film of the present invention may further include the following step (IV). Step (I): A step of preparing a film (pA) having a layer made of a crystalline resin (a). Step (II): Heating the film (pA). Step (III): A step of contacting at least one side of the film (pA) with a solvent while the temperature Tf of the film (pA) is within a specific range of values, thereby changing the birefringence in the thickness direction of the film (pA) to produce a film (qA). Step (IV): A step of stretching the film (qA).
[0018] [Process (I)] In step (I), a film (pA) having a layer made of a crystalline resin (a) is prepared. The film (pA) may be prepared by simply purchasing a commercially available product, or may be prepared by forming the film (pA) using the crystalline resin (a) as a material.
[0019] The film (pA) may have a layer other than the layer made of the crystalline resin (a), but may be a film made of only the crystalline resin (a). When the film (pA) has a layer other than the layer made of the crystalline resin (a), at least one of the front surface and the back surface of the film (pA) is a layer made of the crystalline resin (a). The film (pA) may have two or more layers made of the crystalline resin (a), but is usually a single-layer film made of only one layer made of the crystalline resin (a). Therefore, the optical film obtained by the manufacturing method of the present invention may also have a layer other than the layer made of the crystalline resin (a), but may be a film made of only the crystalline resin (a), or may have two or more layers made of the crystalline resin (a), but is usually a single-layer film made of only one layer made of the crystalline resin (a).
[0020] In the manufacturing method of the present invention, when the film (pA) is formed as a long film in step (I), the film (pA) can be transported in the longitudinal direction in the manufacturing line, and the subsequent steps can be performed continuously. By carrying out the manufacturing method in this manner, efficient manufacturing can be performed. However, the manufacturing method of the present invention is not limited to this. For example, after the film (pA) is formed as a long film in step (I), the film (pA) can be cut into a sheet-like film having a rectangular shape or the like, and the film can be sequentially subjected to the subsequent steps to carry out the manufacturing method.
[0021] When the step (I) is carried out by forming the film (pA) using the crystalline resin (a) as a material, the film can be formed by various known film forming methods. In particular, it is preferable to form the film by melt extrusion from the viewpoint of production efficiency. The film forming conditions can be appropriately adjusted according to the properties of the crystalline resin (a). The thickness of the film (pA) formed in the step (I) is not particularly limited, and can be appropriately adjusted so that the thickness of the optical film as a product is a desired value. The film (pA) may be a film having optical anisotropy, but even if it does not have optical anisotropy, the optical film of the present invention can be easily produced by subjecting it to the subsequent steps.
[0022] FIG. 1 is a side view showing an example of a manufacturing apparatus for carrying out the manufacturing method of the present invention and an example of an operation for carrying out the manufacturing method of the present invention using the same. FIG. 1 shows an example in which a resin (a) is melt-extruded to form a long film (pA) 12, which is transported in the direction of arrow A1 in a manufacturing line, and the subsequent steps are continuously carried out. In FIG. 1, the manufacturing apparatus 10 includes, in order from the upstream of the transport path of the manufacturing line, a melt-extrusion molding apparatus 110, an oven 120 as a heating device, a solvent tank 130, and a stretching device 140. The manufacturing apparatus 10 also includes a measuring device 190 for measuring the temperature of the film 11 immediately before entering the solvent tank 130.
[0023] In the example of Fig. 1, the melt extrusion molding apparatus 110 includes a die 111 and a cast roll 112. A heated and melted resin (a) 11 is extruded from the die 111 into the shape of a film, which is cast onto the cast roll 112 and cooled to form a film (pA) 12.
[0024] [Resin (a)] Resin (a) may be a crystalline polymer, i.e., a resin containing a polymer having crystallinity. A polymer having crystallinity refers to a polymer having a melting point Tm. In other words, a polymer having crystallinity refers to a polymer whose melting point can be observed by a differential scanning calorimeter (DSC). The crystalline resin is preferably a thermoplastic resin.
[0025] The crystalline polymer preferably has a positive intrinsic birefringence. By using a crystalline polymer having a positive intrinsic birefringence, the resin (a) can be a resin having a positive intrinsic birefringence value. In this case, an optical film having a particularly useful property regarding the Nz coefficient can be particularly easily produced.
[0026] The crystalline polymer may be, for example, polyester such as polyethylene terephthalate (PET) or polyethylene naphthalate (PEN); polyolefin such as polyethylene (PE) or polypropylene (PP); and is not particularly limited, but preferably contains an alicyclic structure. By using a crystalline polymer containing an alicyclic structure, the mechanical properties, heat resistance, transparency, low moisture absorption, dimensional stability, and light weight of the obtained optical film can be improved. The polymer containing an alicyclic structure refers to a polymer having an alicyclic structure in the molecule. Such a polymer containing an alicyclic structure may be, for example, a polymer obtained by a polymerization reaction using a cyclic olefin as a monomer, or a hydrogenated product thereof.
[0027] Examples of the alicyclic structure include a cycloalkane structure and a cycloalkene structure. Among these, the cycloalkane structure is preferred because it is easy to obtain an optical film having excellent properties such as thermal stability. The number of carbon atoms contained in one alicyclic structure is preferably 4 or more, more preferably 5 or more, and preferably 30 or less, more preferably 20 or less, and particularly preferably 15 or less. When the number of carbon atoms contained in one alicyclic structure is within the above range, mechanical strength, heat resistance, and moldability are highly balanced.
[0028] In the crystalline polymer containing an alicyclic structure, the ratio of the structural unit having an alicyclic structure to all structural units is preferably 30% by weight or more, more preferably 50% by weight or more, and particularly preferably 70% by weight or more. By increasing the ratio of the structural unit having an alicyclic structure as described above, heat resistance can be improved. The ratio of the structural unit having an alicyclic structure to all structural units can be 100% by weight or less. In addition, in the crystalline polymer containing an alicyclic structure, the remainder other than the structural unit having an alicyclic structure is not particularly limited and can be appropriately selected according to the purpose of use.
[0029] Examples of the crystalline polymer containing an alicyclic structure include the following polymers (α) to (δ). Among these, polymer (β) is preferred because it is easy to obtain an optical film having excellent heat resistance. Polymer (α): A ring-opening polymer of a cyclic olefin monomer, which has crystallinity. Polymer (β): A hydrogenated product of polymer (α) and has crystallinity. Polymer (γ): An addition polymer of a cyclic olefin monomer, which has crystallinity. Polymer (δ): A hydrogenated polymer (γ) having crystallinity.
[0030] Specifically, the crystalline polymer containing an alicyclic structure is preferably a dicyclopentadiene ring-opening polymer having crystallinity, and a dicyclopentadiene ring-opening polymer hydrogenation product having crystallinity. Among them, a dicyclopentadiene ring-opening polymer hydrogenation product having crystallinity is particularly preferred. Here, the dicyclopentadiene ring-opening polymer refers to a polymer in which the ratio of dicyclopentadiene-derived structural units to all structural units is usually 50% by weight or more, preferably 70% by weight or more, more preferably 90% by weight or more, and even more preferably 100% by weight.
[0031] The hydrogenated ring-opening polymer of dicyclopentadiene preferably has a high ratio of racemo dyads. Specifically, the ratio of racemo dyads in the repeating units of the hydrogenated ring-opening polymer of dicyclopentadiene is preferably 51% or more, more preferably 70% or more, and particularly preferably 85% or more. A high ratio of racemo dyads indicates high syndiotactic stereoregularity. Therefore, the higher the ratio of racemo dyads, the higher the melting point of the hydrogenated ring-opening polymer of dicyclopentadiene tends to be. The ratio of racemo-dyads is described in the Examples below. 13 It can be determined based on C-NMR spectrum analysis.
[0032] As the polymer (α) to polymer (δ), polymers obtained by the production method disclosed in WO 2018 / 062067 can be used.
[0033] The melting point Tm of the crystalline polymer is preferably 200° C. or higher, more preferably 230° C. or higher, and preferably 290° C. or lower. By using a crystalline polymer having such a melting point Tm, an optical film having an even better balance between moldability and heat resistance can be obtained.
[0034] A crystalline polymer has a glass transition temperature, and the crystalline resin (a) containing the crystalline polymer as a main component has the glass transition temperature TgR. Although TgR is not particularly limited, it is usually 85°C or higher and usually 170°C or lower.
[0035] The glass transition temperature TgR and melting point Tm can be measured by the following method. First, the sample is melted by heating, and the melted sample is quenched with dry ice. Then, the glass transition temperature Tg and melting point Tm of this sample can be measured using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min (heating mode).
[0036] The weight average molecular weight (Mw) of the crystalline polymer is preferably 1,000 or more, more preferably 2,000 or more, and is preferably 1,000,000 or less, more preferably 500,000 or less. A crystalline polymer having such a weight average molecular weight has an excellent balance between moldability and heat resistance.
[0037] The molecular weight distribution (Mw / Mn) of the crystalline polymer is preferably 1.0 or more, more preferably 1.5 or more, and is preferably 4.0 or less, more preferably 3.5 or less. Here, Mn represents the number average molecular weight. A crystalline polymer having such a molecular weight distribution has excellent moldability.
[0038] The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the polymer can be measured in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran as a developing solvent.
[0039] The crystalline polymer may be used alone or in combination of two or more kinds in any ratio.
[0040] The proportion of the crystalline polymer in the crystalline resin (a) is preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 90% by weight or more. When the proportion of the crystalline polymer is equal to or more than the lower limit, the birefringence expression and heat resistance of the obtained optical film can be improved. The upper limit of the proportion of the crystalline polymer can be 100% by weight or less.
[0041] The crystalline resin (a) may contain optional components in addition to the crystalline polymer. Examples of the optional components include antioxidants such as phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants; light stabilizers such as hindered amine-based light stabilizers; waxes such as petroleum wax, Fischer-Tropsch wax, and polyalkylene wax; nucleating agents such as sorbitol-based compounds, metal salts of organic phosphoric acids, metal salts of organic carboxylic acids, kaolin, and talc; diaminostilbene derivatives, coumarin derivatives, and azole-based derivatives (e.g., benzoxazole derivatives, benzotriazole derivatives, and benzimide derivatives); and the like. Examples of the optional components include fluorescent brighteners such as benzothiazole derivatives, carbazole derivatives, pyridine derivatives, naphthalic acid derivatives, and imidazolone derivatives; ultraviolet absorbers such as benzophenone-based ultraviolet absorbers, salicylic acid-based ultraviolet absorbers, and benzotriazole-based ultraviolet absorbers; inorganic fillers such as talc, silica, calcium carbonate, and glass fibers; colorants; flame retardants; flame retardant assistants; antistatic agents; plasticizers; near-infrared absorbers; lubricants; fillers; and any polymer other than a crystalline polymer, such as a soft polymer. One type of optional component may be used alone, or two or more types may be used in combination at any ratio.
[0042] [Steps (II) and (III)] In step (II), the film (pA) is heated. In the example of FIG. 1, the film (pA) 12 passes through an oven 120 provided in the transport path and is heated in the oven 120. However, the heating mode in the manufacturing method of the present invention is not limited to this, and other heating methods may be adopted. For example, as shown in FIG. 2, the film (pA) 12 may be transported in contact with a heating roll 220, and the heat of the heating roll 220 may be transferred to the film (pA) 12 to perform step (II). In addition, when the film (pA) is formed into a sheet-like shape before step (II), step (II) may be performed by leaving the film (pA) in an oven.
[0043] In step (III) following step (II), the film (pA) is brought into contact with a solvent while its temperature Tf is in a specific range. The temperature is (TgR-50)°C or higher, preferably (TgR-45)°C or higher, more preferably (TgR-40)°C or higher, and is (TgR-20)°C or lower, preferably (TgR-22)°C or lower, more preferably (TgR-25)°C or lower. The present inventors have found that by setting the temperature Tf within this range, it is possible to sufficiently change the birefringence in the thickness direction while suppressing undesirable phenomena such as the film easily becoming cloudy.
[0044] In the example of FIG. 1, the temperature of the film (pA) 12 at a position measured by the measuring device 190 just before the film (pA) 12 leaves the oven 120 and enters the solvent bath 130 is measured as the temperature Tf. The temperature condition of the step (III) can be achieved by adjusting the operating conditions so that the temperature Tf at this time is within the above-mentioned specific range. Therefore, for example, in the example of FIG. 1, if the oven 120 and the solvent bath 130 are far apart from each other and the film 12 may be cooled between leaving the oven 120 and entering the solvent bath 130, the film temperature at the outlet of the oven 120 can be set to a temperature higher than the desired Tf value. After the film (pA) 12 enters the solvent bath 130, the film (pA) 12 may be cooled by the solvent and may decrease in temperature, but regardless of the degree of the temperature decrease, the temperature condition of the step (III) can be achieved by having the temperature Tf of the film (pA) 12 just before the film (pA) 12 enters the solvent bath 130 be within the above-mentioned specific range.
[0045] The solvent used in step (III) may be appropriately selected from those that can penetrate into the crystalline resin (a) without dissolving the resin. An organic solvent is usually used as the solvent. Examples of the organic solvent include hydrocarbon solvents such as toluene, limonene, and decalin; and carbon disulfide. The type of solvent may be one type or two or more types.
[0046] In the example of Fig. 1, the contact in step (III) is performed by an immersion method in which the film (pA) is immersed in a solvent, but the contact in step (III) is not limited to this and can be achieved by any operation. Other examples of the contact operation include a spray method in which the solvent is sprayed on the surface of the film (pA), and a coating method in which the solvent is applied to the surface of the film (pA). From the viewpoint of easily performing continuous contact, the immersion method is preferred.
[0047] When the film (pA) is contacted with the solvent by the immersion method, the contact time is preferably 0.5 seconds or more, more preferably 1.0 seconds or more, particularly preferably 5.0 seconds or more, and preferably 120 seconds or less, more preferably 80 seconds or less, particularly preferably 60 seconds or less. When the contact time is equal to or more than the lower limit, the birefringence of the film (pA) can be effectively adjusted by contact with the solvent. On the other hand, even if the contact time is extended, the adjustment amount of the birefringence tends not to change significantly. Therefore, when the contact time is equal to or less than the upper limit, the productivity can be increased without impairing the quality of the film.
[0048] The temperature of the solvent during contact in step (III) is arbitrary within a range in which the solvent can maintain a liquid state, and can therefore be set within a range from the melting point to the boiling point of the solvent. However, from the viewpoint of more effectively suppressing the clouding of the film, it is preferable that the temperature is lower than a certain level, while from the viewpoint of efficiently adjusting the birefringence, it is preferable that the temperature is higher than a certain level. Specifically, the temperature Ts of the solvent is preferably lower than Tf, and the difference therebetween (Tf-Ts) is preferably 30°C or higher, more preferably 33°C or higher, while preferably 50°C or lower, more preferably 47°C or lower. By adjusting the temperature Ts of the solvent within such a range, it is possible to achieve suppression of clouding and efficient production.
[0049] As a result of contact with the solvent in step (III), the film (pA) becomes the film (qA). The film (qA) may have a changed thickness and a changed birefringence in the thickness direction compared to the film (pA). Such a change caused by contact with the solvent is difficult to obtain by a normal retardation film manufacturing method, such as simply stretching a resin for an optical film. Therefore, as a result of such a change, the optical film of the present invention can be easily manufactured.
[0050] When the film (qA) obtained as a result of the step (III) has an Nz coefficient greater than 0 and less than 1, it can be used as an optical film that can be used as a three-dimensional retardation film. However, in many cases, the film (qA) may have an Nz coefficient less than 0. In that case, the optical film can be easily manufactured by carrying out the step (IV).
[0051] [Step (IV)] In step (IV), the film (qA) obtained in step (III) is stretched. By stretching the film (qA), the refractive index in the thickness direction of the film (qA) is changed, and the Nz coefficient can be easily adjusted to a desired value greater than 0. Since the film (qA) has been subjected to step (III), as a result of step (IV), an optical film having optical properties that are difficult to obtain by a typical method for producing a retardation film, such as simply stretching a resin for an optical film, can be easily obtained.
[0052] The stretching in step (IV) may be simple uniaxial stretching. The Nz coefficient can be easily adjusted by such simple uniaxial stretching. There is no limitation on the stretching direction in step (IV), and examples of the stretching direction include the longitudinal direction, the width direction, and the oblique direction. Here, the oblique direction refers to a direction perpendicular to the thickness direction, and an angle between the width direction and the direction is neither 0° nor 90° (i.e., an angle between the width direction and the direction is more than 0° and less than 90°).
[0053] When a film having optical properties capable of functioning as a three-dimensional retardation film is to be produced by a production method not involving step (III), it is usually necessary to perform multiple complicated stretching steps and to incorporate a material having a negative inherent birefringence value into the material constituting the film. The implementation of these steps is highly disadvantageous in terms of production efficiency. In contrast, the production method of the present invention is advantageous in terms of production efficiency, since an optical film capable of functioning as a three-dimensional retardation film can be obtained by a relatively easy process.
[0054] The stretching ratio is preferably 1.1 times or more, more preferably 1.2 times or more, and preferably 5.0 times or less, more preferably 2.0 times or less, even more preferably 1.9 times or less, and particularly preferably 1.8 times or less. It is desirable to set the specific stretching ratio appropriately depending on factors such as the optical properties, thickness, and strength of the optical film to be produced. When the stretching ratio is equal to or more than the lower limit, the birefringence can be significantly changed by stretching. When the stretching ratio is equal to or less than the upper limit, good optical properties such as easy and good control of the direction of the slow axis can be realized. Also, breakage of the film can be effectively suppressed.
[0055] The stretching temperature is preferably (TgR+5)°C or higher, more preferably (TgR+10)°C or higher, and preferably (TgR+100)°C or lower, more preferably (TgR+90)°C or lower. When the stretching temperature is equal to or higher than the lower limit, the film can be sufficiently softened to perform uniform stretching. When the stretching temperature is equal to or lower than the upper limit, the film can be prevented from hardening due to the progress of crystallization of the crystalline polymer, so that the stretching can be performed smoothly and a large birefringence can be developed by stretching. Furthermore, the haze of the obtained optical film can usually be reduced to increase the transparency.
[0056] Since the birefringence of the film can be changed by the step (IV), the Nz coefficient can be adjusted. Thus, a film having desired optical properties can be obtained by the stretching in the step (IV). The obtained film can be used as it is as an optical film product. Alternatively, the obtained film can be further subjected to optional processing to be made into a product. Examples of optional processing include adjustment of birefringence by heat treatment while maintaining the stretched dimensions or relaxation treatment by shrinking the stretched dimensions.
[0057] [Other steps] The method for producing an optical film of the present invention may further include any step in combination with the above-mentioned steps. For example, after step (III), it may include a step of removing the solvent attached to the film (III). Examples of the method for removing the solvent include drying and wiping.
[0058] In the step (I), the film (pA) is prepared as a long film, and when the subsequent steps are performed in a production line while the film is in a long state, a long film can be obtained as an optical film. The long optical film can be wound into a roll as necessary to form a film roll. In addition, it can be cut into a desired shape as necessary.
[0059] [Optical Film] The optical film obtained by the production method of the present invention will now be described. The Nz coefficient of the optical film is preferably greater than 0, more preferably greater than 0.2, and more preferably less than 1, more preferably less than 0.8. A film having such an Nz coefficient is called a three-dimensional retardation film. When the three-dimensional retardation film is provided in a display device such as a liquid crystal display device, it can exhibit an effect of reducing the coloring of the display surface when viewed from an inclined direction.
[0060] The in-plane retardation Re of the optical film can be adjusted to a value suitable for the application of the optical film. In one example, the preferred range of the in-plane retardation Re(590) at a wavelength of 590 nm is 137.5 nm or a value close thereto, specifically, preferably 127.5 to 147.5 nm, more preferably 130.5 to 144.5 nm. By setting the value of Re(590) within this range, the optical film can be used as a λ / 4 wave plate. In another example, the preferred range of Re(590) is 275 nm or a value close thereto, specifically, preferably 265 to 285 nm, more preferably 268 to 282 nm. By setting the value of Re(590) within this range, the optical film can be used as a λ / 2 wave plate.
[0061] The degree of crystallinity of the crystalline polymer contained in the crystalline resin (a) when the optical film is produced by the production method of the present invention is not particularly limited, but is usually high to a certain degree. The specific range of the degree of crystallinity is preferably 10% or more, more preferably 15% or more, and particularly preferably 30% or more. The crystallinity of a crystalline polymer can be measured by X-ray diffraction.
[0062] Generally, optical films used in devices such as display devices need to be thick enough to exhibit optical properties, but are also required to be thin in order to make the device thinner. The thickness of the optical film obtained by the manufacturing method of the present invention is not particularly limited, but it is possible to obtain a film that satisfies the desired optical properties even if it is thin. Specifically, the thickness of the optical film is preferably 150 μm or less, more preferably 120 μm or less, and even more preferably 100 μm or less. The lower limit of the thickness of the optical film is not particularly limited, but can be, for example, 20 μm or more.
[0063] In the optical film obtained by the manufacturing method of the present invention, the resin (a) may contain an organic solvent. This organic solvent is usually the organic solvent used in step (III) of the manufacturing method of the present invention that is incorporated into the film. The resin (a) before being subjected to step (III) may or may not contain an organic solvent. Usually, the resin (a) after being subjected to step (III) contains a larger amount of organic solvent than the resin (a) before being subjected to step (III).
[0064] The organic solvent taken into the film in step (III) may penetrate into the polymer. Therefore, even if drying is performed at a temperature higher than the boiling point of the organic solvent, it is difficult to completely remove the solvent. Therefore, the optical film obtained by the manufacturing method of the present invention usually contains an organic solvent.
[0065] The ratio of the organic solvent contained in the optical film obtained by the manufacturing method of the present invention (solvent content) to 100% by weight is preferably 10% by weight or less, more preferably 5% by weight or less, and particularly preferably 0.1% by weight or less. The lower limit of the solvent content is not particularly limited, but may be 0.001% by weight or more, or 0.01% by weight or more. The content of the solvent in the film may be measured by thermogravimetric analysis.
[0066] The optical film obtained by the manufacturing method of the present invention can be processed into a desired shape such as a rectangle as necessary and used as a component of an optical device such as a display device. When the optical film is used as a component of a display device, the display quality, such as the viewing angle, contrast, and image quality, of an image displayed on the display device can be improved. EXAMPLES
[0067] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below, and can be modified and carried out as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto. In the following description, the units "%" and "parts" are by weight unless otherwise specified. Furthermore, the operations described below were carried out at room temperature and pressure unless otherwise specified.
[0068] [Evaluation method] (Method of measuring weight average molecular weight Mw and number average molecular weight Mn of polymer) The weight average molecular weight Mw and number average molecular weight Mn of the polymer were measured as polystyrene equivalent values using a gel permeation chromatography (GPC) system (Tosoh Corporation, "HLC-8320"). In the measurement, an H-type column (Tosoh Corporation) was used as the column, and tetrahydrofuran was used as the solvent. The temperature during the measurement was 40°C.
[0069] (Method of measuring hydrogenation rate of polymer) The hydrogenation rate of the polymer is 4 as a solvent at 145°C,1 Measured by H-NMR measurement.
[0070] (Method of measuring glass transition temperature Tg and melting point Tm) The glass transition temperature Tg and melting point Tm of the polymer were measured as follows. First, the polymer was melted by heating, and the melted polymer was quenched with dry ice. Then, the glass transition temperature Tg and melting point Tm of the polymer were measured using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min (heating mode) using the polymer as a test specimen.
[0071] (Method for measuring the ratio of racemo-dyads in polymers) The ratio of racemo-dyads in the polymer was determined as follows. 4 The inverse-gated decoupling method was applied to the polymer at 200°C using 13 C-NMR measurements were performed. 13 The results of C-NMR measurement showed that o-dichlorobenzene-d 4 Using the peak at 127.5 ppm as the reference shift, the signal at 43.35 ppm from the meso-dyad and the signal at 43.43 ppm from the racemo-dyad were identified. The ratio of the racemo-dyads in the polymer was calculated based on the intensity ratio of these signals.
[0072] (Thickness measurement) The thickness of the film was measured using a contact thickness meter (manufactured by MITUTOYO, Code No. 543-390).
[0073] (Refractive Index) The refractive index of the film was measured using a phase difference meter (AxoScan OPMF-1 manufactured by AXOMETRICS) at a wavelength of 590 nm.
[0074] (Measurement of crystallinity) The crystallinity of the film was confirmed by X-ray diffraction in accordance with JIS K 0131. Specifically, the diffracted X-ray intensity from the crystallized portion was determined using a wide-angle X-ray diffractometer (Rigaku Corporation, "RINT 2000"), and the crystallinity was calculated from the ratio to the total diffracted X-ray intensity according to the following formula (i). Xc=K·Ic / It Equation (i) In the above formula (i), Xc represents the crystallinity of the test sample, Ic represents the diffracted X-ray intensity from the crystallized portion, It represents the total diffracted X-ray intensity, and K represents a correction term.
[0075] [Production Example 1: Crystalline resin (a)] A metallic pressure reactor was thoroughly dried and then purged with nitrogen. 154.5 parts of cyclohexane, 42.8 parts of a 70% cyclohexane solution of dicyclopentadiene (endo isomer content of 99% or more) (30 parts as dicyclopentadiene), and 1.9 parts of 1-hexene were placed in the metallic pressure reactor and heated to 53°C.
[0076] 0.014 parts of tetrachlorotungsten phenylimide (tetrahydrofuran) complex was dissolved in 0.70 parts of toluene to prepare a solution. 0.061 parts of a 19% diethylaluminum ethoxide / n-hexane solution was added to this solution and stirred for 10 minutes to prepare a catalyst solution. This catalyst solution was added to the mixture in the pressure-resistant reactor to start the ring-opening polymerization reaction. After that, the reaction was continued for 4 hours while maintaining the temperature at 53°C to obtain a solution of a ring-opened polymer of dicyclopentadiene. The number-average molecular weight (Mn) and weight-average molecular weight (Mw) of the obtained ring-opened polymer of dicyclopentadiene were 8,750 and 28,100, respectively, and the molecular weight distribution (Mw / Mn) calculated from these was 3.21.
[0077] To 200 parts of the obtained solution of the ring-opening polymer of dicyclopentadiene, 0.037 parts of 1,2-ethanediol was added as a terminator, heated to 60°C, and stirred for 1 hour to terminate the polymerization reaction. One part of a hydrotalcite-like compound (Kyowa Chemical Industry Co., Ltd.'s "Kyoward (registered trademark) 2000") was added, heated to 60°C, and stirred for 1 hour. Thereafter, 0.4 parts of a filter aid (Showa Chemical Industry Co., Ltd.'s "Radiolight (registered trademark) #1500") was added, and the adsorbent and the solution were filtered using a PP pleated cartridge filter (ADVANTEC Toyo Co., Ltd.'s "TCP-HX").
[0078] 100 parts of cyclohexane was added to 200 parts of the filtered ring-opening polymer solution (polymer amount 30 parts), and 0.0043 parts of chlorohydridocarbonyltris(triphenylphosphine)ruthenium was added, and hydrogenation reaction was carried out at 180°C and hydrogen pressure of 6 MPa for 4 hours. As a result, a reaction liquid containing a hydrogenated product of the ring-opening polymer of dicyclopentadiene was obtained. The reaction liquid was a slurry solution in which the hydrogenated product was precipitated.
[0079] The hydrogenated product and the solution contained in the reaction solution were separated using a centrifuge and dried under reduced pressure at 60°C for 24 hours to obtain 28.5 parts of a hydrogenated product of a crystalline ring-opening polymer of dicyclopentadiene. The hydrogenation rate of this hydrogenated product was 99% or more, the glass transition temperature (Tg) was 93°C, the melting point (Tm) was 262°C, and the ratio of racemo-dyads was 89%.
[0080] 100 parts of the obtained hydrogenated ring-opening polymer of dicyclopentadiene was mixed with 1.1 parts of an antioxidant (tetrakis [methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl) propionate] methane; "Irganox (registered trademark) 1010" manufactured by BASF Japan Ltd.), and then the mixture was put into a twin-screw extruder (product name "TEM-37B", manufactured by Toshiba Machine Co., Ltd.) equipped with four die holes having an inner diameter of 3 mm. The mixture of the hydrogenated ring-opening polymer of dicyclopentadiene and the antioxidant was molded into a strand shape by hot melt extrusion molding, and then chopped with a strand cutter to obtain pellets of crystalline resin (a). The operating conditions of the twin-screw extruder were as follows. Barrel temperature setting: 270~280℃ Die temperature setting = 250℃ Screw speed: 145 rpm
[0081] Example 1 (1-1. Process (I)) The crystalline resin (a) produced in Production Example 1 was molded using a hot melt extrusion film molding machine equipped with a T-die (Optical Control Systems' "Measuring Extruder Type Me-20 / 2800V3") and wound on a roll at a speed of 1 m / min to obtain a long film (pA). The thickness of the film (pA) was 39 μm and the width was approximately 120 mm. The operating conditions of the film molding machine were as follows. Barrel temperature setting: 280℃~300℃ Die temperature = 270℃ Screw speed = 30 rpm Cast roll temperature = 80℃
[0082] The principal refractive indices (nx(pA), ny(pA), and nz(pA)) of the obtained film (pA) were measured.
[0083] (1-2. Process (II)) The film (pA) obtained in (1-1) was cut into a rectangular film of 100 mm x 100 mm. Each side of the rectangular film was parallel or perpendicular to the longitudinal direction of the long film (pA). The rectangular film was left to stand in an oven heated to 120°C and then removed. The temperature Tf of the rectangular film just before being subjected to the next step (III) was measured with an infrared thermometer and found to be 60°C.
[0084] (1-3. Process (III)) The bath was filled with toluene as the treatment solvent, the temperature of which, Ts, was kept at 25°C. The rectangular film whose temperature had been measured in step (II) was immediately immersed in toluene for 5 seconds. After the immersion time had elapsed, the rectangular film was taken out of the toluene and its surface was wiped with gauze to obtain a film (qA). The principal refractive indices (nx(qA), ny(qA), and nz(qA)) of the obtained film (qA) were measured.
[0085] (1-4. Process (IV)) A stretching device ("SDR-562Z" manufactured by Etoh Corporation) was prepared. This stretching device was equipped with clips capable of gripping the ends of a rectangular resin film, and an oven. A total of 24 clips were provided, five per side of the resin film and one at each vertex of the resin film, and the resin film could be stretched by moving these clips. In addition, two ovens were provided, and each could be set to a stretching temperature and a heat treatment temperature. Furthermore, in the stretching device, the resin film could be transferred from one oven to the other while still being gripped by the clips.
[0086] The film (qA) obtained in (1-3) was attached to the stretching device and treated at a preheating temperature of 110°C for 10 seconds. Thereafter, the film (qA) was stretched at a stretching temperature of 130°C with a longitudinal stretching ratio of 1, a transverse stretching ratio of 1.7, and a stretching speed of 1.5 / 10 seconds to obtain a film (rA). The "longitudinal stretching ratio" refers to the stretching ratio in the direction corresponding to the longitudinal direction of the long film (pA), and the "transverse stretching ratio" refers to the stretching ratio in the direction corresponding to the width direction of the long film (pA).
[0087] The principal refractive indices (nx(rA), ny(rA), and nz(rA)) of the obtained film (rA) were measured to determine the Nz coefficient Nz(rA). The crystallinity of the film (rA) was also measured. Furthermore, the appearance of the film (rA) was visually evaluated, and it was found to have a good transparent film appearance without any cloudiness.
[0088] Example 2 Except for the following changes, films (film (pA), film (qA) and film (rA)) were obtained and evaluated in the same manner as in Example 1. The heating conditions in (1-2) were changed. The temperature Tf of the rectangular film was 70° C. immediately before immersion in step (III) in (1-3). The appearance of the film (rA) was evaluated by visual inspection, and it was found to have a good transparent film appearance without any cloudiness, similar to Example 1.
[0089] Comparative Example 1 A film was obtained and evaluated in the same manner as in Example 1, except for the following changes. The temperature Ts of toluene in (1-3) was changed to 50°C. The heating conditions in (1-2) were changed. The temperature Tf of the rectangular film immediately before immersion in step (III) in (1-3) was 25°C.
[0090] In this comparative example, the films (qA) and (rA) became cloudy, and therefore it was not possible to measure their principal refractive indices.
[0091] Comparative Example 2 A film was obtained and evaluated in the same manner as in Example 1, except for the following changes. The heating conditions in (1-2) were changed. The temperature Tf of the rectangular film immediately before immersion in step (III) in (1-3) was 25°C. The appearance of the film (rA) was evaluated by visual inspection, and it was found to have a good transparent film appearance without any cloudiness, similar to Example 1.
[0092] Comparative Example 3 A film was obtained and evaluated in the same manner as in Example 1, except for the following changes. The heating conditions in (1-2) were changed. The temperature Tf of the rectangular film was 80° C. immediately before immersion in step (III) in (1-3).
[0093] In this comparative example, the films (qA) and (rA) became cloudy, and therefore it was not possible to measure their principal refractive indices.
[0094] The outline and results of the examples and comparative examples are shown in Table 1.
[0095] [Table 1]
[0096] *NA: The refractive index could not be measured due to white turbidity.
[0097] As is clear from the results of the Examples and Comparative Examples, in the production in the Examples which satisfy the heating and solvent contact conditions of the present invention, it is possible to easily achieve a change in birefringence in the thickness direction of the film, and production can be carried out in which undesirable phenomena such as clouding of the film are suppressed. [Explanation of symbols]
[0098] 10: Manufacturing equipment 11: Heat-melted resin (a) 12: Film (pA) 110: Melt extrusion molding device 111: Die 112: Cast roll 120: Oven 130: Solvent tank 140: Stretching device 190: Measuring equipment 220: Heating roll A1: Arrow
Claims
1. A step (I) of preparing a film (pA) having a layer made of a crystalline resin (a) having a glass transition temperature TgR (°C); A step (II) of heating the film (pA); a step of contacting at least one side of the film (pA) with a solvent while the temperature Tf of the film (pA) is in a state in which ... and a step (IV) of stretching the film (qA).
2. A step (I) of preparing a film (pA) having a layer made of a crystalline resin (a) having a glass transition temperature TgR (°C); A step (II) of heating the film (pA); a step (III) of contacting at least one side of the film (pA) with a solvent while the temperature Tf of the film (pA) is in a state in which ... The method for producing an optical film, wherein the optical film has an Nz coefficient greater than 0 and less than 1.
3. The method for producing an optical film according to claim 1 or 2, wherein the step (II) comprises heating the film (pA) in an oven.
4. The method for producing an optical film according to any one of claims 1 to 3, wherein the step (II) comprises transporting the film (pA) in a state of contact with a heated roll.
5. The method for producing an optical film according to any one of claims 1 to 4, wherein the optical film is a single-layer film.
6. The method for producing an optical film according to any one of claims 1 to 5, wherein the crystalline resin (a) has a positive intrinsic birefringence value.
7. The method for producing an optical film according to any one of claims 1 to 6, wherein the crystalline resin (a) contains an alicyclic structure-containing polymer.
Citation Information
Patent Citations
Method for producing birefringent film and liquid crystal display device using the same
JP1993346507A
Optical compensation film and its manufacturing method
JP2009145662A
Method of manufacturing multilayer optical film, multilayer optical film and use thereof
JP2009251011A
Method for producing resin film, resin film, and optical film
JP2016026909A
Liquid crystal alignment film and production method of the same
JP2018189724A