Polymer membrane, composite membrane, electrolyte membrane for battery, electrode composite, and method for producing polymer membrane
A polymer membrane with aramid polymers and ionic liquids addresses the limitations of existing membranes by providing high ionic conductivity, dendrite resistance, and antistatic properties, suitable for batteries with aqueous electrolytes, enhancing battery performance and safety.
Patent Information
- Application Number
- JP2021044294
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-03-18
AI Technical Summary
Existing polymer membranes for batteries lack sufficient ionic conductivity, dendrite resistance, liquid separation properties, and antistatic properties, particularly when used with aqueous electrolytes, and often require additional components like polyether polymer electrolytes.
A polymer membrane composed of aramid polymers and ionic liquids, with specific conductivity and resistivity values, designed to prevent water permeation and maintain structural integrity, achieving high ionic conductivity and antistatic properties without pores, and incorporating ionic liquids to enhance conductivity and resistance.
The membrane exhibits excellent ionic conductivity, dendrite resistance, and antistatic properties, suitable for use with aqueous electrolytes, ensuring high ion permeability and preventing short circuits while maintaining mechanical strength and preventing foreign matter adhesion.
Smart Images

Figure 0007585904000001 
Figure 0007585904000002 
Figure 0007585904000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymer membrane having excellent ion conductivity, as well as good dendrite resistance, liquid separation properties and antistatic properties. [Background technology]
[0002] In order to reduce the weight of batteries and increase their energy, active research is being conducted on metallic Li anodes, all-solid-state batteries, and air batteries. In particular, the evolution of the cathode into an air cathode that uses air as an energy source is attracting attention because it would enable overwhelming weight reduction compared to current oxides. However, many issues remain to be addressed in the design of anodes, separators, electrolytes, etc. before they can be put to practical use.
[0003] The separator must have ionic conductivity and productivity. In addition, dendrite resistance and liquid separation properties are also required for stable operation of the air battery. Battery performance can be improved by selecting electrolytes that match the positive and negative electrodes, but when using different electrolytes, particularly when using a nonaqueous electrolyte system and an aqueous electrolyte system, the separator must have liquid separation properties to prevent the electrolytes from mixing. So far, there has been little research into separators that can achieve both of these properties.
[0004] Generally, in batteries, separators made of porous membranes or nonwoven fabrics with through holes of tens of nm to several μm in diameter are used to enable ion conduction between the positive and negative electrodes while preventing short circuits due to contact between the positive and negative electrodes. However, when separators with holes are used, there is an issue of dendrite growth. Solid electrolytes can be cited as a solution to this issue, and are broadly divided into inorganic and organic types. Organic types are further divided into polymer gel electrolytes and polymer solid electrolytes (intrinsic polymer electrolytes).
[0005] Inorganic solid electrolytes are composed of anionic lattice sites and metal ions, and many inorganic solid electrolytes with practical ionic conductivity have been reported (for example, Patent Document 1). Among organic electrolytes, the application of polymer gel electrolytes, in which the electrolyte solution is semi-solidified with a polymer, to batteries began with a report by Feuillade et al. in 1975 (Non-Patent Document 1). Since then, various reports have been made up to now (for example, Patent Document 2), and they have been put to practical use as lithium polymer batteries. Research on polymer solid electrolytes began with a paper by Wright published in 1973 (Non-Patent Document 2), and many achievements have been reported to date, mainly on polyether-based electrolytes (for example, Patent Document 3). However, further improvements are required for practical use and high performance, such as poor contact with electrodes, inability to be made into a thin film by itself, and low ionic conductivity.
[0006] As described above in the prior art documents, when a polymer that has strength when made into a membrane is used, high ionic conductivity cannot be expected, and therefore Patent Document 4 and Patent Document 5 attempt to improve these problems.
[0007] Patent Document 4 discloses an ion-conductive film using aromatic polyamide that has strength when made into a film, in which a swollen gel is obtained by using a rigid polymer that is not permeable to electrolyte solution after being made into a film, and replacing the electrolyte solution with a solvent-containing (or washing water-containing) solution in the film manufacturing process. Meanwhile, Patent Document 5 discloses a composite membrane in which the pores of an aromatic polyamide porous membrane are filled with a polymer solid electrolyte. This membrane is intended to improve upon the issues of porous membranes, such as short circuits and vulnerability to deformation, and the issues of polymer solid electrolytes, such as low strength. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2014-13772 A [Patent Document 2] JP 2008-159496 A [Patent Document 3] JP 2007-103145 A [Patent Document 4] International Publication No. 95 / 31499 [Patent Document 5] Japanese Patent Application Publication No. 9-302115 [Non-patent literature]
[0009] [Non-Patent Document 1] G. Feuillade, Ph. Perche, J. Appl. Electrochem., 5, 63 (1975). [Non-Patent Document 2] PVWright,Br.Polm.J.,7.319(1975). Summary of the Invention [Problem to be solved by the invention]
[0010] However, the films described in Patent Documents 4 and 5 need to be used in combination with a polyether polymer electrolyte, and therefore liquid separation is not possible, and it is considered difficult to apply them to batteries that use aqueous electrolytes. In addition, there is room for improvement in ion conductivity.
[0011] In view of the above circumstances, an object of the present invention is to provide a polymer membrane having excellent ion conductivity, as well as good dendrite resistance, liquid separation properties and antistatic properties. [Means for solving the problem]
[0012] In order to solve the above problems, the present invention has the following features. (1) Ionic conductivity at 25°C is 1.0×10 -6 S / cm or more, surface resistivity is 10 14 Ω / cm 2 The following further features that water does not pass through when one side is in contact with water for 15 minutes. , containing aramid polymer Polymer membrane. (2) The polymer membrane according to (1), comprising a polymer and an ionic liquid. (3) The polymer membrane according to (1) or (2), characterized in that the thickness increase ratio after immersion in an electrolyte for 8 hours is 1 or less. (4) The polymer membrane according to any one of (1) to (3), characterized in that the air permeability is 10,000 S or more. (5) The polymer film according to any one of (1) to (4), which exhibits a weight loss rate of 5% or more when heated from 140° C. to 300° C. and held at 300° C. for 2 hours. ( 6 )(1)~( 5 2. A composite film comprising the polymer film according to claim 1, formed on a substrate having holes. ( 7 )(1)~( 5 9. An electrolyte membrane for a battery comprising the polymer membrane according to any one of (1) to (7) above or the composite membrane according to (8). ( 8 )(1)~( 5 2. An electrode composite comprising the polymer film according to claim 1, formed on a battery electrode. ( 9 ) The polymer (1) to ( 5 ) A method for producing a polymer membrane. Effect of the Invention
[0013] According to the present invention, it is possible to provide a polymer membrane having excellent ion conductivity, as well as good dendrite resistance, liquid separation properties and antistatic properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be described in detail below.
[0015] The present invention is a method for producing a ferroelectric material having an ionic conductivity of 1.0×10 at 25° C. -6 S / cm or more, surface resistivity is 10 14 Ω / cm 2 The following further relates to a polymer membrane that is characterized in that water does not permeate when one side of the membrane is in contact with water for 15 minutes. In order to realize the effects of the present invention, the above characteristics must be satisfied simultaneously.
[0016] The ionic conductivity of the polymer membrane of the present invention at 25° C. is 1.0×10 -6 S / cm or more. 1.0×10 -5 S / cm or more, and 1.0×10 -4 More preferably, it is 5.0×10 S / cm or more. -4 It is more preferable that the ionic conductivity of the polymer membrane of the present invention is 1.0×10 S / cm or more. The ionic conductivity of the polymer membrane of the present invention is determined by the above-mentioned ionic conductivity value. By setting the ionic conductivity of the membrane within the above-mentioned range, when it is used as an electrolyte membrane for a battery, high ion permeability and excellent output characteristics and cycle characteristics can be obtained. Ionic conductivity is 1.0×10 -6 If it is less than S / cm, when used as an electrolyte membrane for a battery, the ion permeability is low, the output characteristics are reduced, and the capacity is significantly deteriorated after repeated use.
[0017] In order to realize the excellent antistatic properties of the present invention, the surface resistivity of the polymer film is 10 14 Ω / cm 2 It must be less than 1.0×10 13 Ω / cm 2 It is preferable that the value is less than 1.0×10 11 Ω / cm 2 More preferably, the surface resistivity is 1×10 14 Ω / cm 2 If it exceeds this value, static electricity is likely to be generated, foreign matter will adhere to the surface of the film, causing defects due to the foreign matter, and wrinkles and misalignment when wound into a roll. By making the surface resistivity within the range of the present invention, it is possible to impart antistatic properties to the polymer film, and to solve problems of quality degradation due to foreign matter adhesion and productivity problems such as reduced winding properties.
[0018] When one side of the polymer membrane of the present invention is in contact with water for 15 minutes, it is necessary that water does not permeate. The water does not permeate in the present invention means that after contacting one side of the polymer membrane with a basic aqueous solution by the method described below and 15 minutes have passed, the pH test paper on the side not in contact with water does not turn blue. If the pH test paper turns blue, it can be determined that water has permeated the film, and it is difficult to apply the film to a battery using an aqueous electrolyte. In order to realize the liquid separation property of the present invention, it is preferable that the polymer membrane does not contain a water-soluble polymer.
[0019] In order to realize the effects of the present invention, it is preferable that the polymer membrane contains a polymer and an ionic liquid. By introducing an ionic liquid into the polymer, it is possible to simultaneously impart ionic conductivity and antistatic properties to a substantially non-porous polymer membrane. Up until now, many methods have been considered for improving dendrite resistance by using a polymer membrane without through-holes, but the ionic conductivity is significantly lower than that of a porous membrane, and improvement is required for practical use. By using an ionic liquid, high ionic conductivity can be expressed even without a pore structure, and both dendrite resistance and ionic conductivity can be achieved. This is thought to be because the ionic liquid penetrates between the polymer chains, reducing the resistance of the entire membrane and dramatically improving ionic conductivity.
[0020] The polymer that can be used in the present invention is not particularly specified, but in order to realize liquid separation, it is preferable to use a polymer that is not water-soluble. A polymer that has affinity with ionic liquid is preferable, and a polymer that can maintain the strength of the film even if it contains ionic liquid is particularly preferable. As a polymer that satisfies these characteristics, a polymer having an aromatic ring on the main chain can be suitably used, and examples thereof include aromatic polyamide (aramid), aromatic polyimide, aromatic polyamideimide, aromatic polyether ketone, aromatic polyether ether ketone, aromatic polyarylate, aromatic polysulfone, aromatic polyether sulfone, aromatic polyether imide, and aromatic polycarbonate. In addition, a blend of multiple polymers may be used. Among them, aromatic polyamide (including aromatic polyamic acid, which is a precursor of aromatic polyimide), aromatic polyimide, or aromatic polyamideimide is particularly preferable because it is easy to maintain high strength when thinned. The content of the polymer in the film is not particularly specified, but it is preferably 10 to 95 wt% (mass%) of the entire film, more preferably 25 to 85 wt%, and even more preferably 40 to 85 wt%.
[0021] As a polymer that can be suitably used in the present invention, it is preferable that the polymer constituting the membrane contains a polymer having a structure represented by any one of the following chemical formulas (1) to (3). Examples of aromatic polyamides include those having a repeating unit represented by the following chemical formula (1), aromatic polyimides include those having a repeating unit represented by the following chemical formula (2), and aromatic polyamideimides include those having a repeating unit represented by the following chemical formula (3). Chemical formula (1):
[0022] [ka]
[0023] Chemical formula (2):
[0024] [ka]
[0025] Chemical formula (3):
[0026] [ka]
[0027] Here, Ar1 and Ar2 in the chemical formulas (1) to (3) are aromatic groups, and each may be a single group or a multi-component copolymer with multiple groups. In addition, the bonds constituting the main chain on the aromatic ring may be either meta-oriented or para-oriented. Furthermore, some of the hydrogen atoms on the aromatic ring may be substituted with any group.
[0028] In the present invention, when an aromatic polyamide, aromatic polyimide, or aromatic polyamideimide is used, it is preferable that the main chain or side chain has an ether bond or a thioether bond (in the main chain or on the side chain). The unshared electron pair of the ether bond or the thioether bond accelerates the movement of ions required for the operation of the battery, and when used in combination with an ionic liquid, the ion conductivity can be further improved.
[0029] The ionic liquid in the present invention refers to an ionic salt that is a liquid at room temperature among compounds composed only of ions (Chemical Industry 2004 VOL.55 NO.11). The type of ionic liquid in the present invention is not limited, and a commercially available product may be used, and excellent effects can be confirmed even if one that can be prepared at low cost by a neutralization method is used.
[0030] Ionic liquids are composed of cations and anions, and various properties can be imparted by changing the combination of cations and anions. There are no particular limitations on the cations and anions of the ionic liquid in the present invention.
[0031] Examples of cations include, but are not limited to, those with nitrogen as the ion center, those with phosphorus as the ion center, those with sulfur as the ion center, those having nitrogen and sulfur as the ion center, and those with a metal element as the ion center.
[0032] Examples of cations with nitrogen as the ion center include, but are not limited to, dialkylammonium ions such as dioctylammonium ion and bis(2-ethylhexyl)ammonium ion, trialkylammonium ions such as trioctylammonium ion, dimethylmyristylammonium ion, dimethylpalmitylammonium ion, dimethylstearylammonium ion, dimethylbehenylammonium ion, and dilaurylmethylammonium ion, and diarylammonium and triarylammonium ions such as dibenzylammonium ion and tribenzylammonium ion. In the ionic liquid of the present invention, from the viewpoint of being able to be prepared at low cost by a neutralization method, the structure of the cation is preferably a protonated nitrogen-containing compound, and among the nitrogen-containing compounds, those having a structure in which a tertiary amine is protonated are particularly preferred. In addition, these cations may have a substituent represented by an alkyl group at any position, and the number of the substituents may be multiple.
[0033] Cations having phosphorus as the ion center are generally called phosphonium cations, and specific examples thereof include tetrabutylphosphonium, tetrahexylphosphonium, trihexyltetradecylphosphonium, triphenylmethylphosphonium, (2-cyanoethyl)triethylphosphonium, (3-chloropropyl)trioctylphosphonium, tributyl(4-vinylbenzyl)phosphonium, triisobutylmethylphosphonium, triethylmethylphosphonium, tributylmethylphosphonium, tributylhexadecylphosphonium, 3-(triphenylphosphonio)propane-1-sulfonic acid, and the like, but are not limited thereto.
[0034] Cations with sulfur as the ionic center are generally called sulfonium cations, and specific examples thereof include, but are not limited to, triethylsulfonium, tributylsulfonium, 1-ethyltetrahydrothiophenium, and 1-butyltetrahydrothiophenium.
[0035] Examples of cations having a metal element as the ion center include, but are not limited to, lithium ion, sodium ion, potassium ion, rubidium ion, and cesium ion.
[0036] The anion of the ionic liquid of the present invention may be selected from, but is not limited to, a carboxylate ion, an organic phosphate ion, a sulfonate ion, etc. Among these, an aromatic carboxylate ion is preferred.
[0037] Specific examples of carboxylate ions include formate, acetate, propionate, and butyrate. Examples of aromatic carboxylate ions include benzoate, salicylate, p-methylbenzoate, and p-nitrobenzoate. Examples of organic phosphate ions include dibutyl phosphate, diethyl phosphate, and dimethyl phosphate. Specific examples of sulfonate ions include methanesulfonate and p-toluenesulfonate, but are not limited to these.
[0038] The ionic liquid of the present invention is most preferably an ionic salt in which the cation is a structure obtained by protonating a nitrogen-containing compound and the anion is a structure obtained by deprotonating an aromatic carboxylic acid. By combining a cation and an anion, the ionic liquid can be synthesized at low cost using the neutralization method described below, and further good ionic conductivity and antistatic properties can be achieved.
[0039] The ionic liquid of the present invention can be synthesized by adopting a general method for synthesizing ionic salts. Examples of ammonium salts include a method (anion exchange method) in which an ammonium salt obtained by reacting an amine with an alkyl halide compound or the like is subjected to anion exchange using a metal salt and purified to obtain the desired ammonium salt, and a method (neutralization method) in which an amine is directly reacted with an acid to obtain the desired ammonium salt by neutralization, but are not limited thereto.
[0040] In the ionic liquid of the present invention, since no by-products are generated and it can be used without purification, it is preferable to synthesize it using a neutralization method. It is particularly preferable that the molar ratio of the raw materials, amine and acid, is 1:1. By making the molar ratio 1:1, no unreacted raw materials remain, so that subsequent purification is not necessary. A reaction solvent may be used as necessary, but since it is necessary to remove the solvent after the reaction, it is preferable to carry out the reaction without a solvent.
[0041] Specific examples of ionic liquids include trioctylammonium salicylate, dioctylammonium benzoate, dioctylammonium = 4-methylbenzoate, dioctylammonium = 4-nitrobenzoate, dioctylammonium salicylate, bis(2-ethylhexyl)ammonium benzoate, bis(2-ethylhexyl)ammonium = 4-methylbenzoate, bis(2-ethylhexyl)ammonium = 4-nitrobenzoate, bis(2-ethylhexyl)ammonium salicylate, trioctylammonium benzoate, trioctylammonium = 4-methylbenzoate, trioctylammonium = 4-nitrobenzoate, dimethylmyristylammonium benzoate, dimethylmyristylammonium = 4-methylbenzoate, dimethylmyristylammonium = 4-nitrobenzoate, dimethylmyristylsalicylate, dimethylpalmitylammonium benzoate, dimethylpalmitylammonium = 4-methylbenzoate, dimethylpalmitylammonium = 4-nitrobenzoate, dimethylmyristylsalicylate, dimethylpalmitylammonium benzoate, dimethylpalmitylammonium = 4-methylbenzoate, dimethylpalmitylammonium = 4-nitrobenzoate, dimethylpalmit ...nitrobenzoate, dimethylpalmitylsalicylate, ammonium benzoate, dimethylstearyl ammonium benzoate, dimethylstearyl ammonium 4-methyl benzoate, dimethylstearyl ammonium 4-nitro benzoate, dimethylstearyl salicylate, dimethylbehenyl ammonium benzoate, dimethylbehenyl ammonium 4-methyl benzoate, dimethylbehenyl ammonium 4-nitro benzoate, dimethylbehenyl salicylate, dilauryl methyl ammonium benzoate, dilauryl methyl ammonium 4-methyl benzoate, dilauryl methyl ammonium ammonium 4-nitro benzoate, dilauryl methyl ammonium salicylate, dibenzyl ammonium benzoate, dibenzyl ammonium 4-methyl benzoate, dibenzyl ammonium 4-nitro benzoate, dibenzyl ammonium salicylate, tribenzyl ammonium benzoate, tribenzyl ammonium 4-methyl benzoate, tribenzyl ammonium 4-nitro benzoate, tribenzyl ammonium salicylate, and the like, but are not limited thereto.
[0042] The content of the ionic liquid of the present invention is not particularly limited, but is preferably 5 to 90 wt% of the entire membrane. More preferably, it is 15 to 75 wt%. Still more preferably, it is 15 to 60 wt%. By setting the content of the ionic liquid within the above range, the membrane has sufficient strength and excellent ionic conductivity and antistatic properties can be obtained.
[0043] The confirmation of each component and its content in the polymer membrane of the present invention is not limited to a specific method, but may be performed by proton nuclear magnetic resonance spectroscopy ( 1 H-NMR and Fourier transform infrared spectroscopy (FT-IR) can be used. If necessary, multiple techniques can be used together to confirm the structure.
[0044] The thickness increase ratio of the polymer membrane of the present invention after immersion in the electrolyte for 8 hours is preferably 1 or less. More preferably 0.8 or less, and even more preferably 0.5 or less. Since the electrolyte molecules are small, it is expected that the thickness will increase as they penetrate into the polymer molecular chain, but it is preferable to keep the thickness increase ratio within the above range in order to maintain liquid separation. This thickness increase ratio is also an index of the swelling property of the polymer membrane, and even if a polymer having high swelling property is contained, the thickness increase ratio of the obtained polymer membrane is preferably within the above range, and it is particularly preferable that the polymer membrane does not contain a polymer having high swelling property.
[0045] The polymer membrane of the present invention preferably has an air permeability of 10,000 S or more. In this specification, air permeability is the time required for 100 mL of air to pass through the membrane, and the higher the air permeability value, the more difficult it is for the gas to pass through. Air permeability is also an index of the amount of voids in the membrane, and in the past, high ionic conductivity was achieved by making the membrane porous, but the air permeability value was low, so the dendrite resistance of the present invention could not be achieved and the liquid separation property was also reduced. In the present invention, by applying an ionic liquid to a non-porous polymer membrane, it was possible to impart dendrite resistance and liquid separation property while simultaneously achieving both high ionic conductivity and antistatic properties.
[0046] The weight loss rate of the polymer film of the present invention when heated from 140°C to 300°C and held at 300°C for 2 hours is evaluated by the method described below. The weight loss rate is preferably 5% or more, and more preferably 10% or more. It is preferable that this weight loss is not due to decomposition of the polymer, but is due to the ionic liquid. Therefore, it is preferable that the polymer contains a polymer that does not undergo weight loss due to thermal decomposition under the above temperature conditions.
[0047] The thickness of the polymer membrane of the present invention is preferably 0.05 to 30 μm, more preferably 0.10 to 20 μm, and even more preferably 0.20 to 10 μm. By setting the thickness within the above range, the strength of the polymer membrane is sufficient, and there is no increase in resistance due to the membrane thickness, so that the polymer membrane can be suitably used for various applications (for example, as an electrolyte membrane for batteries). The thickness of the polymer membrane of the present invention can be controlled by various conditions such as the concentration of the membrane-forming solution, the viscosity of the membrane-forming solution, additives in the membrane-forming solution, the casting thickness, the heat treatment temperature, and the stretching conditions.
[0048] Next, the method for producing the polymer membrane of the present invention will be described below.
[0049] Methods for obtaining polymers that can be used in the polymer film of the present invention will be described using aromatic polyamides, aromatic polyimides, or their precursors, polyamic acids, as examples, but the polymers that can be used and the polymerization methods thereof are not limited to these.
[0050] Various methods are available for obtaining aromatic polyamides. For example, when using low-temperature solution polymerization with acid dichloride and diamine as raw materials, they are synthesized in aprotic organic polar solvents such as N-methylpyrrolidone, N,N-dimethylacetamide, dimethylformamide, and dimethylsulfoxide. In the case of solution polymerization, in order to obtain a polymer with a high molecular weight, it is preferable to set the water content of the solvent used for polymerization to 500 ppm or less (based on mass, the same applies below), more preferably 200 ppm or less. Furthermore, a metal salt may be added to promote dissolution of the polymer. As the metal salt, a halide of an alkali metal or alkaline earth metal that dissolves in an aprotic organic polar solvent is preferable, and examples of the metal salt include lithium chloride, lithium bromide, sodium chloride, sodium bromide, potassium chloride, and potassium bromide. When the acid dichloride and diamine are used in equal amounts, a polymer with an ultra-high molecular weight may be produced, so it is preferable to adjust the molar ratio so that one is 95.0 to 100.0 mol% of the other. In addition, the polymerization reaction of aromatic polyamide is accompanied by heat generation, and if the temperature of the polymerization system rises, a side reaction may occur and the degree of polymerization may not rise sufficiently, so it is preferable to cool the temperature of the solution during polymerization to 40° C. or less. Furthermore, when acid dichloride and diamine are used as raw materials, hydrogen chloride is by-produced in the polymerization reaction, and in order to neutralize this, it is recommended to use an inorganic neutralizing agent such as lithium carbonate, calcium carbonate, calcium hydroxide, or an organic neutralizing agent such as ethylene oxide, propylene oxide, ammonia, triethylamine, triethanolamine, diethanolamine, etc.
[0051] On the other hand, when the aromatic polyimide or its precursor polyamic acid that can be used in the present invention is polymerized using, for example, tetracarboxylic anhydride and aromatic diamine as raw materials, a method of synthesis by solution polymerization in an aprotic organic polar solvent such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, dimethylformamide, dimethylsulfoxide, etc. can be adopted. Since an ultra-high molecular weight polymer may be generated when the raw materials tetracarboxylic anhydride and aromatic diamine are used in equal amounts, it is preferable to adjust the molar ratio so that one is 90.0 to 99.5 mol% of the other. In addition, the polymerization reaction is accompanied by heat generation, and if the temperature of the polymerization system rises, precipitation may occur due to the imidization reaction, so it is preferable to keep the temperature of the solution during polymerization at 70°C or less. As a method of imidizing the aromatic polyamic acid synthesized in this way to obtain an aromatic polyimide, heat treatment, chemical treatment, or a combination thereof is used. The heat treatment method is generally a method of imidizing polyamic acid by heating it at about 100 to 500°C. On the other hand, chemical treatments include a method using a tertiary amine such as triethylamine as a catalyst and a dehydrating agent such as an aliphatic acid anhydride or an aromatic acid anhydride, or a method using an imidizing agent such as pyridine.
[0052] The viscosity η of the aromatic polyamide and aromatic polyimide or the polyamic acid precursor thereof is preferably 0.5 to 7.0 dl / g. By setting the viscosity within the above range, there is no decrease in mechanical properties due to a decrease in the bonding strength between polymer molecular chains, and the strength of the polymer film is sufficient even when an ionic liquid is added, and excellent ionic conductivity is also obtained.
[0053] Next, the membrane-forming stock solution used in the process for producing the polymer membrane of the present invention (hereinafter, referred to as membrane-forming stock solution) will be described.
[0054] The polymer solution after polymerization may be used as it is for the membrane forming stock solution, or the polymer may be isolated once and then redissolved in an inorganic solvent such as the above-mentioned aprotic organic polar solvent or sulfuric acid. The method for isolating the polymer is not particularly limited, but examples include a method in which the polymer solution after polymerization is poured into a large amount of water to extract the solvent and neutralization salt into the water, and only the precipitated polymer is separated and then dried. In addition, a metal salt may be added as a dissolution aid during redissolution. As the metal salt, an alkali metal or alkaline earth metal halide that dissolves in an aprotic organic polar solvent is preferable, and examples thereof include lithium chloride, lithium bromide, sodium chloride, sodium bromide, potassium chloride, and potassium bromide.
[0055] In order to achieve the effects of the present invention, it is necessary to add an ionic liquid to the polymer in the manufacturing process. The timing of adding the ionic liquid is not limited, and it may be added in any of the polymer polymerization process, the film-forming solution preparation process, and the film-forming process, but it is preferable to add it in the film-forming solution preparation process because it can be uniformly dispersed with the polymer. It can also be added in multiple processes, or it can be added in multiple batches in the same process.
[0056] The concentration of the polymer in the film-forming solution is preferably 3 to 30 wt%, more preferably 5 to 20 wt%. Inorganic particles or organic particles may be added to the film-forming solution for the purpose of improving the strength, heat resistance, and ion permeability of the resulting polymer film, reducing the static friction coefficient, etc. Examples of inorganic particles include wet and dry silica, colloidal silica, aluminum silicate, titanium oxide, calcium carbonate, calcium phosphate, barium sulfate, alumina, aluminum hydroxide, magnesium hydroxide, magnesium carbonate, zinc carbonate, titanium oxide, zinc oxide (zinc oxide), antimony oxide, cerium oxide, zirconium oxide, tin oxide, lanthanum oxide, magnesium oxide, barium carbonate, zinc carbonate, basic lead carbonate (lead white), barium sulfate, calcium sulfate, lead sulfate, zinc sulfide, mica, titanium mica, talc, clay, kaolin, lithium fluoride, and calcium fluoride. Examples of organic particles include particles obtained by crosslinking a polymer compound using a crosslinking agent. Examples of such crosslinked particles include crosslinked particles of polymethoxysilane-based compounds, crosslinked particles of polystyrene-based compounds, crosslinked particles of acrylic compounds, crosslinked particles of polyurethane-based compounds, crosslinked particles of polyester-based compounds, crosslinked particles of fluorine-based compounds, or mixtures thereof. In order to achieve the liquid separation properties of the present invention, it is preferable not to add water-soluble particles.
[0057] Next, a method for forming the polymer membrane of the present invention will be described. The membrane forming solution prepared as above can be used to form a membrane by a so-called solution membrane forming method. The solution membrane forming method includes a dry-wet method, a dry method, a wet method, etc., and any method may be used to form a membrane, but here, the dry-wet method will be described as an example. The polymer membrane of the present invention may be formed directly on a substrate or an electrode having pores to form a laminated composite, but here, a method for forming a polymer membrane as a single polymer membrane will be described.
[0058] When a film is formed by a dry-wet method, the film forming solution is extruded from a die onto a support such as a glass plate, a drum, an endless belt, or a film to form a film, and then the film is dried until it has self-supporting properties. The drying conditions can be, for example, within a range of 50 to 220°C and 60 min. However, when a polyamic acid polymer is used to obtain a film made of polyamic acid without imidization, the drying temperature is preferably 50 to 150°C. More preferably, it is 50 to 120°C. The film that has completed the dry process is peeled off from the support and introduced into a wet process, where it is subjected to desalting, desolvation, and the like, and further stretched, dried, and heat treated. The stretching ratio is preferably within a range of 0.8 to 8.0 in area ratio (area ratio is defined as the value obtained by dividing the area of the film after stretching by the area of the film before stretching. 1 or less means relaxation), and more preferably 1.0 to 5.0. The heat treatment is carried out at a temperature of 80° C. to 500° C., preferably 100° C. to 300° C., for a period of several seconds to several tens of minutes. However, when a polyamic acid polymer is used and a film made of polyamic acid is to be obtained without imidization, the heat treatment temperature is preferably 80° C. to 150° C. More preferably, the heat treatment temperature is 80° C. to 120° C. under reduced pressure.
[0059] The polymer membrane obtained by the above manufacturing method may be subjected to a doping treatment in order to develop high ion conductivity. The doping treatment is a treatment performed to realize higher ion conductivity and reduce the initial irreversible capacity by doping the membrane with ions to be conducted in advance. As a method of doping treatment, for example, a method of inserting metal ions from the metal foil into the membrane by creating a potential difference while contacting a metal foil (lithium metal foil in the case of a lithium ion battery) suitable for the metal ion species to be made conductive with an ion permeable membrane is mentioned. Specifically, the treatment can be performed by preparing a laminate of metal foil / ion permeable membrane / Al foil and connecting the metal foil and Al foil with a lead. At this time, annealing may be performed at 40 to 100°C. In addition, when applied to a liquid battery, in addition to the method using the above-mentioned metal foil, the doping effect can also be obtained by immersing the ion permeable membrane in an electrolyte solution in which an electrolyte containing metal ions is dissolved, and annealing at 40 to 100°C for about 10 min to 24 h. The doping treatment may be performed before the ion-permeable membrane is incorporated into a battery, or may be performed by charging and discharging or annealing the completed battery after the membrane is incorporated into the battery. When the doping treatment is performed, an improvement in ion conductivity is expected, but the doping treatment process itself may be difficult. Since the polymer membrane of the present invention contains an ionic liquid, high ion conductivity can be achieved without performing the doping treatment.
[0060] The polymer membrane of the present invention may be used alone as a battery electrolyte membrane (or separator), or may be laminated with a substrate having pores. Examples of substrates having pores include polymer porous membranes and nonwoven fabrics that are generally used as separators. As a lamination method, the substrate having pores and the polymer membrane of the present invention may be laminated in order when assembling a battery, or the polymer membrane of the present invention may be formed in advance on a substrate having pores to form an integrated composite ion-permeable membrane. The polymer membrane of the present invention may also be formed by directly applying the polymer membrane to a battery electrode to form an integrated electrode / ion-permeable membrane composite.
[0061] The polymer membrane of the present invention has excellent antistatic properties, and can solve problems of quality deterioration due to adhesion of foreign matter, and productivity problems such as reduced winding properties. Furthermore, even if it contains an ionic liquid, it has excellent strength, and although it has substantially no pores, it exhibits ion permeability. Therefore, it can be suitably used as an electrolyte membrane for batteries. When used as an electrolyte membrane for batteries, it may be used as a separator disposed between positive and negative electrodes together with an electrolyte solution, or it may be used as a solid electrolyte membrane. When a sample of a polymer membrane is taken out from a battery used together with an electrolyte solution and evaluated, it is preferable to evaluate the sample from which the electrolyte solution has been removed in advance. As a method for removing the electrolyte solution, a method can be mentioned in which the sample taken out from the battery is fixed to a fixed length and width using a metal frame or the like, the electrolyte solution in the sample is thoroughly washed out in a water bath or the like to replace it with water, and then it is dried in a vacuum oven at 60 to 120 ° C. for about 1 to 12 hours.
[0062] When the polymer membrane of the present invention is used as an electrolyte membrane for a battery, excellent properties can be obtained in terms of suppressing short circuits caused by dendrites, etc. In addition, it is expected to prevent deterioration due to dissolution of the active material into the electrolyte, and to reduce the size and capacity of the battery by reducing the thickness.
[0063] Examples of batteries to which the polymer membrane of the present invention can be applied include, but are not limited to, air batteries, lithium ion secondary batteries (including lithium sulfur batteries and lithium metal batteries), sodium ion secondary batteries, and multivalent ion secondary batteries such as magnesium and calcium. When applied to the lithium-sulfur battery, it is expected to suppress the elution of polysulfide ions, which are the reduction products of sulfur, and improve the Coulomb efficiency and cycle characteristics. When applied to a lithium metal battery, it is expected to suppress the growth of dendritic metal from the metal negative electrode. Furthermore, since it has liquid separation properties, it can be used in batteries with two or more types of electrolytes, and can also be suitably used in batteries with aqueous electrolytes.
[0064] The battery using the polymer membrane of the present invention as an electrolyte can be suitably used as a power source for small electronic devices, transportation such as electric vehicles (EVs), hybrid vehicles (HEVs), and plug-in hybrid vehicles (PHEVs), and large industrial equipment such as industrial cranes. It can also be suitably used as a power storage device for leveling power in solar cells, wind power generation devices, and the like, and for smart grids. It can also be suitably used as a battery used in special environments such as space. EXAMPLES
[0065] The present invention will be described in more detail below with reference to examples. The physical properties of the examples were measured by the following methods.
[0066] (1) Ionic conductivity (unit: S / cm) After immersing the polymer film in the electrolyte (1M LiTFSI ethylene carbonate (EC) / diethyl carbonate (DEC) = 1 / 1, manufactured by Mitsui Chemicals) for 8 hours, it was placed on a SUS304 electrode so as to cover the electrode part, and after dripping the electrolyte, it was sandwiched with another SUS electrode to produce an electrode / polymer film / electrode laminate. The laminate was fixed with a silicon plate to prevent it from shifting, and an evaluation cell was produced.
[0067] The AC impedance of the prepared cell was measured at 25°C using an electrochemical tester (Biologic, model number: SP-150) under conditions of an amplitude of 10 mV and a frequency of 1 MHz to 10 mHz, and the resistance value was read from a graph plotted on a complex plane and substituted into the following formula to calculate the ionic conductivity. The measurement was performed five times, and the calculated average value was taken as the ionic conductivity. σ=d1 / AR σ: Ionic conductivity (S / cm) d1: Thickness of polymer film (cm) (before immersion in electrolyte) A: Electrode area (cm 2 ) R: Resistance value (Ω) (2) Surface resistivity (unit: Ω / cm 2 ) The polymer film was left to stand at a temperature of 23°C and a relative humidity of 65% for 24 hours to condition the humidity, and then measured under the same conditions using a high resistivity meter (manufactured by Mitsubishi Chemical Corporation, model number: MCP-HT450) at an applied voltage of 10V-1000V. When evaluating a composite film in which a polymer film is formed and integrated on a substrate, the surface of the polymer film was measured. Five measurements were taken, and the average value was regarded as the surface resistivity. The antistatic properties were evaluated according to the following criteria. 1.0×10 11 Ω / cm 2 Below:◎ 1.0×10 11 Ω / cm 2 Exceeds 1.0×10 13 Ω / cm 2 Below: 1.0×10 13 Ω / cm 2 Exceeds 1.0×10 14 Ω / cm 2 Below:△ 1.0×10 14 Ω / cm 2 Exceeds: ×.
[0068] (3) Thickness increase ratio The polymer film was immersed in an electrolyte (1M LiTFSI EC / DEC = 1 / 1, manufactured by Mitsui Chemicals) for 8 hours, and the polymer film thickness before and after immersion was measured using a high-precision digital length measuring device (manufactured by Mitutoyo Corporation, model number: VL-50) and calculated by substituting the results into the following formula. The measurement was performed five times, and the calculated average value was used as the increase ratio. Thickness increase ratio = (d2-d1) / d1 d1: Thickness of polymer film (cm) (before immersion in electrolyte) d2: Thickness of the polymer film (cm) (after immersion in the electrolyte).
[0069] (4) Air permeability (unit: S) The air permeability of the polymer membrane was measured using an air permeability measurement controller (manufactured by Asahi Seiko Co., Ltd., model number: EG01). Since the upper limit of the device is 99999S, when the upper limit is reached, it is determined that there is practically no air permeability and is recorded as no air permeability.
[0070] (5) Weight reduction rate (unit: %) Measurements were performed using a thermogravimetric analyzer (Shimadzu Corporation, model number: TGA-50) under the following conditions: nitrogen flow 20 mL / min, heating rate 5°C / min, heating from room temperature to 300°C, and holding at 300°C for 2 hours. The weight at 140°C and the weight at the end of the measurement (after holding at 300°C for 2 hours) were confirmed, and the weight loss rate was calculated by substituting the following formula. Weight reduction rate=(M1-M2)×100 / M1 M1: Weight at 140℃ (mg) M2: Weight at the end of the measurement (mg).
[0071] (6) Viscosity (unit: dl / g) The polymer was dissolved at a concentration of 0.5 g / dl in N-methylpyrrolidone (NMP) containing 2.5 wt% lithium bromide (LiBr), and the flow time was measured at 30° C. using an Ubbelohde viscometer. The flow time of a blank LiBr 2.5 wt% / NMP in which no polymer was dissolved was also measured in the same manner, and the viscosity η (dl / g) was calculated using the following formula.
[0072] η=[ln(t / t0)] / 0.5 t0: Blank flow time (S) t: sample flow time (S).
[0073] (7)NMR The solution of ionic liquid dissolved in chloroform-d (CDCl3, Fujifilm Wako Pure Chemical Industries, Ltd.) 1 H-NMR was measured using an NMR measuring device (manufactured by JEOL, model number: GSX-400). Each peak was assigned and the ionic liquid structure was analyzed.
[0074] (8) Dendrite resistance The dendrite resistance against metallic Li was evaluated. In metallic Li negative electrodes, Li ions in the electrolyte are precipitated on the metal surface during charging, and are dissolved during discharging. Li dendrites are formed when the reaction on the metallic Li surface is uneven, and Li deposition proceeds quickly in areas with low resistance. When dendrites penetrate the polymer film, tears occur in the polymer film. In the present invention, the dendrite resistance of the polymer film was evaluated by the following method.
[0075] First, the polymer film was immersed in an electrolyte (1M LiTFSI EC / DEC=1 / 1, manufactured by Mitsui Chemicals) for 8 hours. After that, a laminate was formed in an argon atmosphere glove box using a cell (manufactured by Hosen Co., Ltd.) so that it had a negative electrode (Li (manufactured by Honjo Metals Co., Ltd.)) / polymer film after electrolyte impregnation / positive electrode (NCM523 (manufactured by Hachiyama Co., Ltd.)), and the electrolyte was poured into the cell and sealed to prepare an evaluation cell. Using the above evaluation cell, constant current charging was performed at 0.05C to 4.15V and constant voltage charging at 4.15V in a charge / discharge device (manufactured by Hokuto Denko Co., Ltd.), for a total of 48 hours of charging. After 48 hours of charging, the polymer film was removed from the evaluation cell and its condition was observed, and the dendrite resistance was evaluated according to the following criteria. No polymer film rupture: 〇 Polymer film broken: × The breakage in the present invention is judged as follows. When a visible breakage can be confirmed, it is judged that a breakage has occurred. Even when there is no visible breakage, if water drips from the opposite side (the side not in contact with pure water) immediately after one side of the polymer is brought into contact with pure water, it is judged that a break has occurred. When there is no visible breakage and water does not drip from the opposite side immediately after one side is brought into contact with pure water, it is judged that no breakage has occurred.
[0076] (9)Liquid separation property An aqueous solution was prepared using sodium hydroxide (NaOH) (Kanto Chemical) so that its concentration was 0.1 mol / L. When this aqueous solution was brought into contact with pH test paper (pH range 1-11, Toyo Roshi Co., Ltd.), the test paper turned blue. Two dried 20 mL glass sample bottles (As One Co., Ltd.) were prepared, one of which was filled with 1 g of the above NaOH aqueous solution (hereinafter referred to as bottle 1), and the other was left empty (hereinafter referred to as bottle 2). A polymer film was attached to the mouth of bottle 1 so that there were no gaps, and then a pH test paper (pH range 1-11, Toyo Roshi Co., Ltd.) was placed on top of the polymer film, and bottle 2 was placed on top of the pH test paper, with the mouths of bottle 1 and bottle 2 overlapping and connected with parafilm. After that, the order was bottle 2 / pH test paper / polymer film / bottle 1 from the bottom, and one side of the polymer film was brought into contact with water for 15 minutes, and the color of the pH test paper was confirmed. Using unused pH test paper as a comparison, the liquid separation property was evaluated according to the following criteria. No change in test paper color (test paper is yellow): Yes Test paper color change (test paper is blue): × The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. It is not something that should be done.
[0077] (Reference Example 1) Polymer solution P-1 4,4'-diaminodiphenyl ether (manufactured by Tokyo Chemical Industry Co., Ltd.) was dissolved as a diamine in dehydrated NMP (manufactured by Mitsubishi Chemical Co., Ltd.) under a nitrogen stream and cooled to 30°C or less. 2-chloroterephthaloyl chloride (manufactured by Nippon Light Metal Co., Ltd.) equivalent to 99 mol% of the total amount of diamine was added thereto over 30 min while keeping the inside of the system under a nitrogen stream and 30°C or less, and after the entire amount was added, the mixture was stirred for about 2 h to polymerize aromatic polyamide (P-1). The obtained polymerization solution was neutralized with 97 mol% lithium carbonate (manufactured by Honjo Chemical Co., Ltd.) and 6 mol% diethanolamine (manufactured by Tokyo Chemical Industry Co., Ltd.) with respect to the total amount of acid chloride to obtain polymer solution P-1. The viscosity η of the obtained polymer was 2.5 dl / g.
[0078] (Reference Example 2) Polymer solution P-2 Except for changing the diamine 4,4'-diaminodiphenyl ether to 1,4-bis(4-aminophenoxy)benzene (Tokyo Chemical Industry Co., Ltd.), a polymer solution P-2 was obtained in the same manner as in Reference Example 1. The viscosity η of the obtained polymer was 2.5 dl / g.
[0079] (Reference Example 3) Polymer solution P-3 Except for changing the diamine 4,4'-diaminodiphenyl ether to 4,4'-thiodianylene (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), a polymer solution P-3 was obtained in the same manner as in Reference Example 1. The viscosity η of the obtained polymer was 1.6 dl / g.
[0080] (Reference Example 4) Polymer solution P-4 Except for changing 2-chloroterephthaloyl chloride to 2-phenoxyterephthaloyl chloride (manufactured by Ihara Nikkei Chemical Industry Co., Ltd.), a polymer solution P-4 was obtained in the same manner as in Reference Example 1. The viscosity η of the obtained polymer was 1.5 dl / g.
[0081] (Reference Example 5) Ionic Liquid I-1 Trioctylamine (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) and salicylic acid (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) were weighed out so that the molar ratio was 1:1, and charged into a reaction vessel. The contents were stirred and mixed at room temperature for 1 hour to obtain trioctylammonium salicylate (ionic liquid I-1) (light yellow liquid). 1 H-NMR measurement confirmed that it had the structure of chemical formula (4). Chemical formula (4):
[0082] [ka]
[0083] (Reference Example 6) Ionic Liquid I-2 Trioctylamine (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) and methanesulfonic acid (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) were weighed out so that the molar ratio was 1:1, and charged into a reaction vessel. The contents were stirred and mixed at room temperature for 1 hour to obtain trioctylammonium methanesulfonate (ionic liquid I-2) (light yellow liquid). 1 H-NMR measurement confirmed that the structure was that of chemical formula (5). Chemical formula (5):
[0084] [ka]
[0085] Example 1 The ionic liquid I-1 obtained in Reference Example 5 (ionic liquid addition amount: 20 wt% relative to the polymer) was added to the polymer solution P-1 obtained in Reference Example 1, and the mixture was stirred and degassed using a mixer (manufactured by THINKY, model number: AR-250) to obtain a uniform, transparent solution. The obtained uniform mixed solution of the polymer and the ionic liquid was applied in the form of a film on a glass plate as a support, and dried at a hot air temperature of 60°C until the polymer film had self-supporting properties, and then the polymer film was peeled off from the support. Next, the solvent and neutralized salt were extracted by introducing the mixture into a water bath at 25°C. Next, the water on the surface of the obtained water-containing polymer film was wiped off, and then the mixture was subjected to heat treatment for 1 min in a tenter chamber at a temperature of 130°C to obtain a polymer film with a thickness of 5 μm. The evaluation results of the obtained polymer film are shown in Table 1. The ionic conductivity of the polymer film of Example 1 was 1.6 × 10 -5 S / cm, and the dendrite resistance, liquid separation property and antistatic property were good.
[0086] (Examples 2 to 5) A polymer membrane was obtained in the same manner as in Example 1, except that the amount of ionic liquid I-1 added was changed as shown in Table 1.
[0087] (Examples 6 to 8) A polymer membrane was obtained in the same manner as in Example 1, except that the type of polymer solution was changed as shown in Table 1.
[0088] Example 9 A polymer membrane was obtained in the same manner as in Example 1, except that the type of ionic liquid was changed to I-2.
[0089] Example 10 A polymer membrane was obtained in the same manner as in Example 1, except that the type of ionic liquid was changed to IL-M51 (referred to as I-3) manufactured by Koei Chemical Industry Co., Ltd.
[0090] Example 11 The ionic liquid I-1 obtained in Reference Example 5 (ionic liquid addition amount: 50 wt% based on the polymer) was added to the polymer solution P-1 obtained in Reference Example 1, and the mixture was stirred and degassed using a mixer (manufactured by THINKY, model number: AR-250) to obtain a uniform, transparent solution. The obtained uniform mixed solution of the polymer and the ionic liquid was applied in the form of a film on a polyethylene (PE) separator (manufactured by Toray Industries, Inc.) having a thickness of 12 μm, and introduced into a water bath at 25° C. to extract the solvent and neutralized salts. Subsequently, the mixture was subjected to a heat treatment for 5 minutes in a tenter chamber at a temperature of 65° C., and a polymer film having a thickness of 16 μm was obtained. The evaluation results of the obtained polymer film are shown in Table 1.
[0091] Comparative Example 1 A polymer membrane was obtained by forming a membrane using only the polymer solution P-1 without adding the ionic liquid I-1 in the same manner as in Example 1. The ionic conductivity was significantly lower than in Example 1, and the antistatic properties were unacceptable.
[0092] Comparative Example 2 Polyethylene oxide E-45 (referred to as P-5) (manufactured by Meisei Chemical Industry Co., Ltd.) was dissolved in acetonitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) at 60°C to obtain a solution with a concentration of 10 wt%, and then ionic liquid I-1 (amount of ionic liquid added: 20 wt% relative to the polymer) was added. The obtained solution was applied in the form of a film on a stainless steel (SUS316) plate, which was a support, and dried in a hot air oven at 80°C until the film had self-supporting properties, and then the film was peeled off from the support. Next, the peeled film was fixed to a metal frame and subjected to heat treatment for 12 hours in a vacuum oven at a temperature of 100°C to obtain a sample with a thickness of 5 μm. The evaluation results of the obtained sample are shown in Table 1. When the liquid separation property was evaluated, the polymer film broke and the liquid separation property was unacceptable.
[0093] Comparative Example 3 The polyethylene (PE) separator of Example 11 (manufactured by Toray Industries, Inc.) was evaluated, and the results are shown in Table 1. The dendrite resistance and antistatic properties were unacceptable.
[0094] [Table 1]
Claims
1. Ionic conductivity at 25°C is 1.0 x 10 -6 S / cm or more, surface resistivity is 10 14 Ω / cm 2 Further, a polymer membrane containing an aramid polymer, which is characterized in that water does not permeate when one side of the polymer membrane is in contact with water for 15 minutes, is described below.
2. 2. The polymer membrane of claim 1, comprising a polymer and an ionic liquid.
3. 3. The polymer membrane according to claim 1, wherein the thickness increase ratio after immersion in an electrolyte for 8 hours is 1 or less.
4. 4. The polymer membrane according to claim 1, wherein the air permeability is 10,000 S or more.
5. 5. The polymer film according to claim 1, wherein the weight loss rate is 5% or more when the polymer film is heated from 140° C. to 300° C. and held at 300° C. for 2 hours.
6. A composite membrane comprising a polymer membrane according to any one of claims 1 to 5 formed on a substrate having voids.
7. 8. An electrolyte membrane for a battery, comprising the polymer membrane according to claim 1 or the composite membrane according to claim 7.
8. 6. An electrode composite comprising the polymer film according to claim 1 formed on a battery electrode.
9. The method for producing a polymer membrane according to any one of claims 1 to 5, further comprising adding an ionic liquid to the polymer.
Citation Information
Patent Citations
Composite membrane of polymer electrolyte and its production
JP1997302115A
Polyelectrolyte, electrolyte film using the same and electrochemical element
JP2007103145A
Gel electrolyte, lithium-ion secondary battery, and manufacturing method of gel electrolyte
JP2008159496A
Sulfide-based solid electrolyte for lithium ion secondary battery
JP2014013772A
Polymer membrane
JP2015149223A