Fiber board, manufacturing method of fiber board, and molded body

By integrating bent fibers and a bending process, the method addresses the challenge of unpredictable thickness changes in fiber boards, achieving controlled thickness adjustment and varied thickness in molded articles.

JP7585963B2Active Publication Date: 2024-11-19TOYOTA BOSHOKU KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021084924
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-19
Publication Date
2024-11-19
Estimated Expiration
2041-05-19

AI Technical Summary

Technical Problem

Existing fiber boards experience unpredictable thickness increases due to the springback effect during shaping, making it difficult to control the final thickness accurately.

Method used

Incorporating bent fibers with an average length of 70-140 mm into the fiber board composition, and utilizing a bending process during manufacturing to enhance the springback effect for controlled thickness adjustment.

Benefits of technology

The method allows for precise control of the fiber board thickness by leveraging the springback effect, enabling the formation of regions with varying thicknesses in molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585963000003
    Figure 0007585963000003
  • Figure 0007585963000004
    Figure 0007585963000004
  • Figure 0007585963000005
    Figure 0007585963000005
Patent Text Reader

Abstract

To provide a fiber board capable of controlling a board thickness utilizing a springback action, a manufacturing method of the fiber board, and a molded body.SOLUTION: A fiber board 10 includes vegetable fibers 11 and a binder resin 12 for binding the vegetable fibers 11. The vegetable fiber 11 includes a fiber 13 having a bent shape. An average fiber length of the fibers 13 having the bent shape is over 70 mm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fiber board containing plant fibers and a binder resin that binds the plant fibers, a method for producing the fiber board, and a molded product. [Background technology]

[0002] Fiber boards in which plant fibers such as kenaf fibers are bound with binder resins are lightweight and highly rigid, and in recent years, their use as materials for vehicle interiors and the like has expanded. Fiber boards are produced by laminating webs in which plant fibers and thermoplastic resin fibers that serve as binder resins are mixed to obtain a mat, compressing the mat to obtain a preboard, and then hot pressing the preboard to form it into the desired shape. Patent Document 1 is known as a technology related to such fiber boards. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-076589 A Summary of the Invention [Problem to be solved by the invention]

[0004] Usually, when a fiberboard is applied to a product that requires a certain thickness, a preboard that is made thicker than the required thickness is used to control the thickness of the fiberboard. Incidentally, when fiberboard is shaped from a preboard, the solidified binder resin melts and the constraint on the plant fibers is loosened, so that the plant fibers are forced to straighten, which may cause a springback effect. This springback effect increases the thickness of the fiberboard after shaping compared to the thickness of the preboard before shaping. For this reason, control of the board thickness using the springback effect has been considered, but this is not practical because the increase in board thickness due to the springback effect is very small.

[0005] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a fiber board whose thickness can be controlled by utilizing the springback effect, a manufacturing method for the fiber board, and a molded body obtained by shaping the fiber board. [Means for solving the problem]

[0006] In order to solve the above problems, the present invention is presented below. The fiber board according to claim 1 is a fiber board containing plant fibers and a binder resin that binds the plant fibers, The present invention is characterized in that the plant fibers include fibers having a bent shape. The invention described in claim 2 is characterized in that in the invention described in claim 1, the vegetable fibers have an average fiber length of 70 mm or more and 140 mm or less. The method for producing a fiber board according to claim 3 is the method for producing a fiber board according to claim 1 or 2, A first step of laminating webs of mixed fibers of plant fibers and resin fibers serving as a binder resin to obtain a mat; A second step of hot pressing the mat to obtain the fiber board, The first step includes a step of making the plant fibers contain fibers having a bent shape. The method for producing a fiber board according to claim 4 is the method for producing a fiber board according to claim 1 or 2, A first step of laminating webs of mixed fibers of plant fibers and resin fibers serving as a binder resin to obtain a mat; A second step of hot pressing the mat to obtain the fiber board, The second step includes a folding step of folding the plant fibers. The invention described in claim 5 is characterized in that in the invention described in claim 4, the folding step compresses the mat in a direction perpendicular to or intersecting with the lamination direction of the web. The invention described in claim 6 is the invention described in claim 4, wherein the folding step uses a press platen having an uneven press surface to compress the mat. The molded article according to the seventh aspect of the present invention is obtained by shaping the fiber board according to the first or second aspect of the present invention. Effect of the Invention

[0007] According to the fiber board of the present invention, a fiber board can be obtained in which the board thickness can be controlled by utilizing the spring back effect. According to the method for producing a fiber board of the present invention, it is possible to produce a fiber board whose board thickness can be controlled by utilizing the spring back effect. According to the molded article of the present invention, the thickness can be controlled by utilizing the spring back effect of the fiber board. [Brief description of the drawings]

[0008] The present invention will be further described in the following detailed description by way of non-limiting examples of exemplary embodiments according to the invention and with reference to the several drawings mentioned, in which like reference numerals refer to like parts throughout the several views of the drawings. [Figure 1] FIG. 1 is a cross-sectional view showing a fiber board of the present invention. [Diagram 2] FIG. 2 is an explanatory diagram showing the first step in the method for producing a fiber board of the present invention. [Diagram 3] FIG. 2 is a cross-sectional view showing a mat for manufacturing a fiberboard. [Figure 4] FIG. 4 is an explanatory diagram showing a second step in the method for producing a fiber board of the present invention. [Diagram 5] FIG. 2 is an explanatory diagram showing the production of a fiber board from the mat. [Figure 6] FIG. 11 is a cross-sectional view showing another form of mat for producing a fiberboard. [Figure 7] FIG. 2 is an explanatory diagram showing a folding step in the manufacturing method of the fiber board of the present invention. [Figure 8]FIG. 2 is an explanatory diagram showing a folding step in the manufacturing method of the fiber board of the present invention. [Figure 9] 1 is a graph showing the relationship between fiber length and swelling amount in an example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in detail below. The matters shown herein are illustrative and are intended to exemplify the embodiments of the present invention, and are described for the purpose of providing what is believed to be the most effective and easily understandable explanation of the principles and conceptual features of the present invention. In this respect, it is not intended to show structural details of the present invention beyond the extent necessary for a fundamental understanding of the present invention, and the description in conjunction with the drawings will make it clear to those skilled in the art how some forms of the present invention can be actually embodied.

[0010] [1] Fiberboard The fiber board (10) of the present invention is a fiber board (10) containing vegetable fibers (11) and a binder resin (12) that binds the vegetable fibers (11), The plant fibers (11) include bent fibers (13), and the bent fibers (13) have an average fiber length of more than 70 mm (see FIG. 1).

[0011] That is, as shown in FIG. 1, a fiber board 10 of the present invention contains vegetable fibers 11 and a binder resin 12 that binds the vegetable fibers 11 together. In this fiber board 10, the vegetable fibers 11 contain fibers 13 having a bent shape (hereinafter, also referred to as "bent fibers 13"). The bent fibers 13 have an average fiber length of more than 70 mm.

[0012] (1) Plant Fiber The plant fibers 11 are fibers extracted from a plant body (trunk, stem, branch, leaf, root, etc.), and include leaf vein plant fibers, bast plant fibers, woody plant fibers, and the like. The plant body from which the plant fiber is derived is not particularly limited. Examples of the plant body include kenaf, hemp, jute, ramie, flax, Manila hemp, sisal, gampi, mitsumata, kozo, kapok, banana, pineapple, coconut, corn, sugarcane, bagasse, palm, papyrus, reed, esparto, sabai grass, wheat, rice, bamboo, various coniferous trees (such as cedar and cypress), broadleaf trees, and cotton. These plant bodies may be used alone or in combination of two or more kinds. As the plant body from which the plant fibers are derived, among the above-mentioned plants, bast plants, i.e., kenaf, hemp, jute, ramie, and flax, are preferred, and among these, kenaf is particularly preferred, and kenaf fiber harvested from the bast of kenaf is particularly preferred. In particular, kenaf fibers harvested from the bast of kenaf are less likely to break or break when bent, and can be suitably used to form the bent fibers 13.

[0013] The average fiber diameter of the plant fibers is not particularly limited. For example, the average fiber diameter can be 1 to 2500 μm. The average fiber diameter is preferably 10 to 2000 μm, more preferably 100 to 1750 μm, and even more preferably 200 to 1500 μm. The average fiber diameter is an average value of the fiber diameters at the center in the longitudinal direction of a total of 200 single fibers used in the measurement of the average fiber length, measured using an optical microscope.

[0014] In the following description, in order to distinguish between the bent fiber 13 and normal plant fibers other than the bent fiber 13, the plant fiber 11 will be referred to as "normal fiber" when describing the normal plant fiber.

[0015] The average fiber length of the normal fiber is not particularly limited. For example, the average fiber length can be 10 mm or more and 200 mm or less. The average fiber length is preferably 20 mm or more and 170 mm or less, more preferably 25 mm or more and 150 mm or less, and even more preferably 30 mm or more and 90 mm or less. The average fiber length of the plant fiber 11 is usually the same in the molded product obtained by shaping the fiber board 10. The average fiber length is measured in accordance with JIS L1015 by randomly selecting one plant fiber at a time using the direct method, stretching it straight without stretching it, and measuring the fiber length on a measuring scale.The average fiber length is the average value measured for a total of 200 fibers.

[0016] (2) Bent Fiber The plant fibers 11 include bent fibers 13. The bent fibers 13 are fibers formed by bending the above-mentioned plant fibers at one or more points on the fibers. Since the folded fibers 13 are folded at one or more points, the folded portions function like springs, and exert a stronger force to straighten the shape than normal fibers. Therefore, by including the folded fibers 13 as the vegetable fibers 11, the fiber board 10 can generate a springback effect more favorably than one that includes only normal fibers. The shape of the folded fiber 13 is not particularly limited. For example, the shape may be a broken line shape, a zigzag shape, a parabolic shape, or the like.

[0017] The average fiber length of the folded fibers 13 is longer than that of the normal fibers, and the lower limit of the average fiber length is more than 70 mm. In this case, the springback effect can be suitably generated in the fiber board 10. The lower limit of the average fiber length is preferably 80 mm or more, more preferably 100 mm or more. The upper limit of the average fiber length of the folded fibers 13 may be less than 140 mm. In this case, a mat for obtaining the fiber board 10 can be suitably produced. The upper limit of the average fiber length is preferably 130 mm or less, more preferably 120 mm or less. The average fiber length is an average value of values ​​measured in the same manner as for the above-mentioned normal fibers.

[0018] The folded fibers 13 may be included in the fiber board 10 as the vegetable fibers 11 together with the normal fibers, or all of the vegetable fibers 11 may be included in the fiber board 10 as the folded fibers 13. Specifically, the proportion of the bent fibers 13 contained in the plant fibers 11 can be 30% by mass or more and 100% by mass or less, assuming that the total amount of the plant fibers 11 contained in the fiber board 10 is 100% by mass. The lower limit of the proportion is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. The upper limit of the proportion can further be 95% by mass or less, particularly 90% by mass or less, and especially 85% by mass or less.

[0019] (3) Binder resin The binder resin 12 binds the plant fibers 11 together. There are no limitations on the type of the binder resin 12, and various thermoplastic resins can be used. Specific examples of the thermoplastic resin include polyolefin resin, polyester resin, polystyrene resin, acrylic resin, polyamide resin, polycarbonate resin, polyacetal resin, ABS resin, etc. These may be used alone or in combination of two or more.

[0020] Examples of the polyester resin include polylactic acid, aliphatic polyester resin, and aromatic polyester resin. Examples of the aliphatic polyester resin include polycaprolactone and polybutylene succinate. Examples of the aromatic polyester resin include polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of the acrylic resin include various resins obtained using methacrylate, acrylate, and the like.

[0021] Of the above-mentioned thermoplastic resins, the binder resin 12 of the present invention is preferably a polyolefin resin. Examples of olefin monomers constituting the polyolefin resin include ethylene, propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, etc. These may be used alone or in combination of two or more. That is, examples of polyolefin resins include polyethylene resins such as ethylene homopolymers, ethylene-1-butene copolymers, ethylene-1-hexene copolymers, and ethylene-4-methyl-1-pentene copolymers. These polyethylene resins are resins in which 50% or more of the total number of structural units are derived from ethylene. In addition, polypropylene resins such as propylene homopolymers, propylene-ethylene copolymers (propylene-ethylene random copolymers, etc.), and propylene-1-butene copolymers are also included. These polypropylene resins are resins in which 50% or more of the total number of structural units are derived from propylene.

[0022] The binder resin 12 may be only an unmodified thermoplastic resin, but may also contain a thermoplastic resin modified by introducing a polar group. A modified thermoplastic resin (hereinafter simply referred to as a "modified thermoplastic resin") is a resin in which the above-mentioned various thermoplastic resins form the main chain and a modifying group is introduced into the main chain. The type of the modifying group is not limited, but a polar group is preferred. Examples of polar groups include carboxylic anhydride groups (-CO-O-OC-), carboxylic acid groups (-COOH), carbonyl groups (-CO-), hydroxyl groups (-OH), amino groups (-NH2), nitro groups (-NO2), and nitrile groups (-CN). These may be used alone or in combination of two or more. Among these, at least one of a carboxylic acid anhydride group, a carboxylic acid group, and a carbonyl group is preferred, and a carboxylic acid anhydride group or a carboxylic acid group is particularly preferred.

[0023] When the thermoplastic resin includes a non-modified thermoplastic resin and a modified thermoplastic resin, the main chains of these resins may be different from each other, but are preferably the same. That is, when the unmodified thermoplastic resin is a polyolefin resin (unmodified polyolefin resin), the modified thermoplastic resin is preferably a modified polyolefin resin. When the thermoplastic resin contains an unmodified thermoplastic resin and a modified thermoplastic resin, the proportion of the modified thermoplastic resin is preferably 1 to 12 mass%, more preferably 2 to 9 mass%, even more preferably 3 to 7 mass%, and particularly preferably 4 to 6 mass%, with the total of the unmodified thermoplastic resin and the modified thermoplastic resin being 100 mass%.

[0024] (4) Additives The fiber board 10 can be made of only plant fibers 11 and binder resin 12, but can contain additives such as a plasticizer (for the thermoplastic resin that becomes the binder resin 12), antioxidants, flame retardants, lubricants, anti-fungal agents, antibacterial agents, fillers, and colorants, if necessary. When the fiber board 10 contains an additive, the content of the additive is usually 0.1 to 10 parts by mass, assuming that the total mass of the plant fibers 11 and the binder resin 12 is 100 parts by mass.

[0025] (5) Specifications, composition, uses, etc. of fiberboard The thickness of the fiber board 10 is not particularly limited and can be appropriately set depending on the application, etc. Usually, the thickness can be 0.5 to 200 mm, particularly 0.5 to 80 mm, and if the fiber board 10 has a thickness of 0.5 to 200 mm, it has sufficient strength, etc. for many applications and can be used as a lightweight member. The basis weight of the fiber board 10 is not particularly limited, and is, for example, 200 to 3000 g / m 2 This basis weight can be further set to 400 to 2500 g / m 2 and more preferably 600 to 2000 g / m 2 and more preferably 800 to 1800 g / m 2 It is preferable that:

[0026] There is no particular limitation on the ratio of the plant fibers 11 and the binder resin 12 contained in the fiber board 10. For example, when the total of the plant fibers 11 and the binder resin 12 is 100 mass%, the ratio of the plant fibers can be 10 mass% or more and 90 mass% or less. The proportion of plant fibers is preferably 15% by mass or more and 85% by mass or less, more preferably 15% by mass or more and 85% by mass or less, even more preferably 20% by mass or more and 80% by mass or less, even more preferably 25% by mass or more and 75% by mass or less, particularly preferably 30% by mass or more and 70% by mass or less, more particularly preferably 35% by mass or more and 65% by mass or less, and particularly preferably 40% by mass or more and 60% by mass or less.

[0027] The fiber board 10 contains the plant fibers 11 and the folded fibers 13, and a strong force acts on the folded fibers 13 to straighten them. When the fiber board 10 is heated to soften the binder resin 12, a springback effect occurs and the fiber board 10 expands in the thickness direction due to the force acting on the plant fibers 11 to straighten them. As shown in FIG. 1, a fiber board 10A in which a springback effect has been generated has an increased board thickness compared to a fiber board 10 before the springback effect has been generated. Specifically, if the thickness of the fiber board 10 before the springback effect is Tp and the thickness of the fiber board 10A after the springback effect is Tb, the increase in thickness due to the springback effect, that is, the amount of expansion (Tb-Tp) can be 0.1 mm to 0.45 mm. This expansion amount is preferably 0.18 mm to 0.45 mm, more preferably 0.35 mm to 0.45 mm.

[0028] [2] Molded body The molded article of the present invention is characterized in that it is obtained by shaping the above-mentioned fiber board (10). That is, the fiber board 10 is shaped into a molded body. During shaping, the fiber board 10 is heated to a temperature at which the binder resin 12 is softened and molded. During this heating, the constraint on the plant fibers 11 by the binder resin 12 is loosened, and a force acts on the plant fibers 11 to straighten them, generating a springback effect.

[0029] The thickness of the molded body during shaping can be freely controlled within the above-mentioned range of the expansion amount of the fiber board 10. In other words, when the thickness of the molded body is T1 (mm) and the thickness of the fiber board 10 is T2 (mm), T1 can be controlled within the range of T2+0.1 mm≦T1≦T2+0.45 mm. Therefore, the molded body can be freely formed into regions of different thicknesses. The heating temperature of the fiber board 10 during shaping is not particularly limited as long as it can generate a springback effect, and can be set appropriately depending on the type of thermoplastic resin used in the binder resin 12. For example, the heating temperature can be 150° C. or higher and 250° C. or lower. This heating temperature is preferably 160° C. or higher and 240° C. or lower, more preferably 170° C. or higher and 235° C. or lower, and even more preferably 170° C. or higher and 210° C. or lower.

[0030] The use of the molded article is not particularly limited, but is preferably used as an interior material for automobiles, railroad cars, ships, airplanes, and the like. Among these, automotive interior materials include instrument panels, center clusters, door trims, quarter trims, roof linings, pillar garnishes, deck trims, tonneau boards, package trays, dashboards, console boxes, kicking plates, switch bases, seat back boards, arm rests, sun visors, and air filter boxes. Furthermore, the molded article is also suitable for use as interior materials and structural materials for buildings and furniture, etc. That is, the molded article can be used as door covering materials, door structural materials, covering materials and structural materials for various furniture (desks, chairs, shelves, chests, etc.), etc. In addition, it can also be used as various containers (trays, etc.), protective materials, partition members, etc.

[0031] [3] Fiberboard manufacturing method 1 The method for producing a fiber board of the present invention comprises the steps of: A bending process of bending at least a portion of the plant fibers to include fibers having a bent shape in the plant fibers; A first step of laminating a web of mixed fibers of vegetable fibers containing bent fibers and resin fibers serving as a binder resin to obtain a mat; A second step of hot pressing the mat to obtain the fiber board, The first step is characterized by including a step of adding folded fibers to the plant fibers.

[0032] That is, the method for producing the fiber board 10 includes a folding step, a first step, and a second step. The folding step is a step of folding at least a part of the plant fibers 11 so that the plant fibers 11 include folded fibers 13. The first step is a step of laminating a web 101 in which plant fibers 11 and resin fibers 121 that become a binder resin 12 are mixed, as shown in Fig. 2, to obtain a mat 102, as shown in Fig. 3. This first step includes a step of making the plant fibers 11 contain folded fibers 13. The second step is a step of hot pressing the mat 102 to obtain the fiber board 10, as shown in FIGS.

[0033] The resin fibers 121 used in the manufacturing method of the fiber board are fibers obtained by melt spinning the thermoplastic resins listed above as the binder resins 12, or the like. There is no particular limitation on the average fiber length of the resin fibers 121. For example, the average fiber length can be 10 to 200 mm (further, 20 to 170 mm, particularly 25 to 150 mm, and especially 30 to 90 mm). The average fiber length is the average value of the measurements taken for a total of 200 single fibers in accordance with JIS L1015, which were taken at random using the direct method, straightened without being stretched, and their fiber length was measured on a flat surface.

[0034] There is no particular limitation on the fineness of the resin fibers 121. For example, the fineness can be 1 to 100 dtex (further, 2 to 50 dtex, particularly 3 to 25 dtex, and especially 5 to 15 dtex). The fineness is calculated by randomly selecting one single fiber, stretching it straight without stretching it, measuring the fiber length on a measuring scale, and measuring the mass when the total length reached 10 m. This process was repeated five times and is the average value.

[0035] (1)Bending process In the folding process, the plant fibers may be folded to form the folded fibers 13 in any manner, but examples of the method include crushing a mass of plant fibers before they are opened with a press machine, compressing the plant fibers with a press platen having an uneven press surface, or folding the plant fibers manually. The vegetable fibers to be used may have an average fiber length of more than 70 mm. The average fiber length is preferably more than 70 mm and less than 140 mm, more preferably 80 mm or more and 130 mm or less, and even more preferably 100 mm or more and 120 mm or less.

[0036] (2) First step The first step may be carried out in any manner, but for example, it can be carried out using a card device 31 and a cross layer device 32 as shown in FIG. The carding device 31 is a device for obtaining the web 101, and has a blender 311 that blends plant fibers and resin fibers, a tank 312 that stores the blended plant fibers and resin fibers, and a carding machine 313 that blends the resin fibers and plant fibers. The cross layer device 32 is a device for obtaining the mat 102, and has a swinging conveyor 321 that swings in the horizontal direction.

[0037] Specifically, in the first step, in the carding device 31, the plant fibers 11 and the resin fibers 121 are blended in the blender 311, and the resin fibers 121 and the plant fibers 11 stored in the tank 312 are sent to the carding machine 313, where they are blended to produce the web 101. The manufactured web 101 is sent to the cross layer device 32, and when it is sent out from the oscillating conveyor 321, the oscillating conveyor 321 oscillates, so that the webs 101 are stacked in order from bottom to top. Then, the webs 101 are stacked with the stacking direction being the upward direction, and the mat 102 is manufactured.

[0038] In the carding device 31 described above, the vegetable fibers 11 and the resin fibers 121 are respectively stored in hoppers (not shown), and are respectively discharged from the hoppers and supplied to the blender 311 . The folded fibers 13 obtained before the first step in the above-mentioned folding process are fed into a hopper for vegetable fibers 11, and are mixed with resin fibers 121 by a carding device 31. In this case, only the folded fibers 13 can be fed into the hopper for vegetable fibers 11, or the folded fibers 13 can be mixed with normal fibers and fed.

[0039] (3)Second process The second step may be carried out in any manner, but may be carried out, for example, using a hot press device 34 and a cold press device 35 . The hot press device 34 is a device for heating and compressing the mat 102 obtained in the first step, and has a pair of upper and lower platens 341 incorporating heating means such as a heater. The cold press device 35 is a device for obtaining the fiberboard 10 by further compressing the mat 102 that has been heated and compressed by the hot press device 34 , and has a pair of upper and lower platens 351 .

[0040] Specifically, in the second step, the mat 102 is first sent to the hot press device 34, placed between a pair of platens 341, and compressed while being heated between the pair of platens 341. Thereafter, the mat 102 is transferred to the cold press device 35 , placed between a pair of platens 351 , and cooled while being further compressed between the pair of platens 351 , to obtain the fiber board 10 . As shown in FIG. 5, in the mat 102, the resin fibers 121 are melted in the heat press device 34, and the plant fibers 11 are bonded together. Furthermore, in the cold press device 35, the mat 102 is subjected to compressive stress on the plant fibers 11 including the folded fibers 13, and in this state, the plant fibers 11 are restrained by the binder resin 12, thereby producing the fiber board 10. That is, in the fiber board 10, the plant fibers 11 including the folded fibers 13 are bound in a compressed state by the binder resin 12. For this reason, when the fiber board 10 is heated during shaping or the like, the binder resin 12 melts and the binding of the plant fibers 11 is loosened, the folded fibers 13 contained in the plant fibers 11, coupled with the fact that they are released from the compressed state, are strongly forced to become linear, and the springback effect is favorably generated.

[0041] The second step may have an intertwining means such as a needle punch mechanism. The intertwining means intertwines the webs 101 constituting the mat 102, making it easier to transport the mat 102 to the second step.

[0042] [4] Fiberboard manufacturing method 2 The method for producing a fiber board of the present invention comprises the steps of: A first step of laminating webs of mixed fibers of plant fibers and resin fibers serving as a binder resin to obtain a mat; A second step of hot pressing the mat to obtain the fiber board, The second step is characterized by including a folding step of folding the vegetable fibers.

[0043] That is, the method for producing the fiber board 10 includes a first step and a second step. The first step is a step of laminating webs 101 in which plant fibers 11 and resin fibers 121 that will become binder resin 12 are mixed to obtain a mat 102 as shown in FIG. The second step is a step of hot pressing the mat 102 to obtain the fiber board 10. This second step includes a folding step of folding the plant fibers 11. The folding process can be carried out by compressing the mat 102 in a direction perpendicular or intersecting the lamination direction of the web 101 as shown in FIG. 7, or by compressing the mat 102 using a press platen 371 having an uneven press surface as shown in FIG. 8, or the like.

[0044] The resin fibers 121 may be those described in the above [3] Fiber board manufacturing method 1, and detailed description thereof will be omitted. In addition, the fiber board manufacturing method 2 differs from the fiber board manufacturing method 1 described above [3] in that the folding step is included in the second step, whereas in the fiber board manufacturing method 1 described above [3] the folding step is included in the second step. In all other respects, the fiber board manufacturing method 2 is substantially similar to the fiber board manufacturing method 1. Therefore, the following description will focus on the folding process, and detailed description of the points that are substantially similar to those in [3] Fiber board manufacturing method 1 will be omitted. The mat 102 obtained in the first step of the fiber board manufacturing method 2 is constructed by stacking the webs 101 with the stacking direction facing upward, as shown in Figure 6, and contains plant fibers 11 and resin fibers 121, but the plant fibers 11 do not contain bent fibers 13.

[0045] (1) Bending process (second process) The folding step included in the second step may be performed in any manner, but may be performed, for example, by using a press device 36 as shown in FIG. The press device 36 is a device for compressing the mat 102 obtained in the first step in a direction perpendicular or intersecting the lamination direction of the web 101 to fold the vegetable fibers, and has a pair of upper and lower base plates 361. Specifically, in the folding process, the mat 102 is sent to the press device 36. At this time, the mat 102 is placed in a horizontally laid state between a pair of upper and lower surface plates 361. That is, by laying the mat 102 on its side, the lamination direction of the web 101 changes from the upward direction to the horizontal direction, and the lamination direction becomes perpendicular to the compression direction (vertical direction) by the surface plate 361. Then, the plant fibers 11 in the mat 102 are compressed and bent vertically between the pair of upper and lower surface plates 361, as the extension direction becomes vertical (approximately vertical), and the bent fibers 13 are formed (see FIG. 7).

[0046] After the folding process, as described in the above [3] Fiberboard Manufacturing Method 1 (3) Step 2, the mat 102 is first sent to the hot press device 34, where it is compressed while being heated, and then sent to the cold press device 35, where it is further compressed and cooled, to obtain the fiber board 10.

[0047] The folding step can also be carried out using a heat press device 37 as shown in FIG. The hot press device 37 is a device for heating and compressing the mat 102 obtained in the first step, and has a pair of upper and lower press platens 371 equipped with a heating means such as a heater. The press platens 371 have an uneven press surface that is pressed against the mat 102.

[0048] Specifically, in the folding process, the mat 102 is sent to the heating press device 37, placed between a pair of press platens 371, and compressed while being heated between the pair of press platens 371. At this time, the plant fibers 11 in the mat 102 are folded by being pressed against the uneven press surface, and folded fibers 13 are formed (see FIG. 8). After the folding process, the mat 102 is sent to a cold press device 35, where it is placed between a pair of platens 351 and cooled while being further compressed between the pair of platens 351, thereby obtaining the fiber board 10. EXAMPLES

[0049] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.

[0050] [Plant fiber] Kenaf fiber was used as the plant fiber, which is obtained by defibrating the bast extracted from kenaf. Kenaf fibers having different average fiber lengths were used in Examples 1 to 6 and Comparative Examples 1 to 10. The average fiber lengths of the kenaf fibers in each example are shown below. In addition, in Examples 1 to 6 and Comparative Examples 1 and 2, all of the kenaf fibers used were folded fibers (folded fibers). In addition, in Comparative Examples 3 to 10, all of the kenaf fibers used were unbent fibers (normal fibers). Average Fiber Length Example 1: 80 mm Example 2: 90 mm Example 3: 100 mm Example 4: 110 mm Example 5: 120 mm Example 6: 130 mm Comparative example 1; 70mm Comparative example 2; 140mm Comparative example 3; 70mm Comparative example 4; 80mm Comparative example 5; 90mm Comparative Example 6: 100 mm Comparative example 7; 110mm Comparative example 8; 120mm Comparative example 9; 130mm Comparative example 10; 140mm

[0051] [Binder resin] The resin fibers used as the binder resin were obtained by melt spinning polypropylene resin, had a melting point of 170°C, and a fineness of 6.6 dtex. These resin fibers were cut to an average fiber length of 50 mm.

[0052] [Fabric board production] The kenaf fibers of Examples 1 to 6 and Comparative Examples 1 to 10 and the above-mentioned resin fibers were mixed using a carding device 31 shown in FIG. 2 to obtain a web, and then this web was laminated using a cross-layer device shown in FIG. 2 to obtain a mat (first step). Next, a portion of the mat was cut out to a size of 30 cm x 30 cm (width x length), and heated to 200°C (heating time 40 seconds) using the heat press device 34 shown in Figure 4 while applying a press pressure of 22.2 kgf / cm. 2 After hot pressing under the condition of 25° C., the mixture was subjected to a press pressure of 7.0 kgf / cm using the cold press device 35 shown in FIG. 2 Then, the mixture was cold pressed to obtain a fiberboard. This fiber board had a width x length of 30 cm x 30 cm and a thickness (Tp) of 2.5 mm.

[0053] [Measurement of swelling amount] The fiber board obtained as described above was heated to 200° C. to cause the springback effect of the kenaf fibers to occur and expand, and then allowed to stand and cool naturally to room temperature (25° C.). The average thickness (Tb) after the heating test was measured for each of the fiber boards in Examples 1 to 6 and Comparative Examples 1 to 10. The average thickness (Tb) was the average value of thickness measurements taken at 10 points on the fiber board at intervals of 5 mm or more. The difference in thickness (Tb-Tp) of the fiber board before and after the heating test was calculated, and this difference was taken as the swelling amount (mm) of each of the fiber boards of Examples 1-6 and Comparative Examples 1-10. The results are shown in Tables 1 and 2 and in FIG. FIG. 9 is a graph showing the relationship between the swelling amount (mm) shown in Tables 1 and 2 and the average fiber length of the plant fibers (kenaf fibers). In addition, in Tables 1 and 2, in Comparative Example 2 and Comparative Example 10, in which the average fiber length of the kenaf fiber was 140 mm, a mat could not be formed during the production of the fiber board, so the swelling amount (mm) was recorded as 0 mm.

[0054] [Table 1]

[0055] [Table 2]

[0056] [Consideration] As shown in Tables 1 and 2 and the graph in Figure 9, Examples 1 to 6, which used folded fibers (folded fibers), had a clearly increased amount of expansion (mm) when compared with Comparative Examples 4 to 9, which used unfolded fibers (folded fibers) with the same average fiber length. On the other hand, in Comparative Example 1, the amount of expansion (mm) was 0.1 mm, which was unchanged from Comparative Example 3, which had the same average fiber length of 70 mm. From the above results, it was found that when the average fiber length of the plant fiber (kenaf fiber) is more than 70 mm and folded fiber is used for the plant fiber (kenaf fiber), the amount of expansion (mm) of the fiber board due to the springback effect increases.

[0057] The above description is merely illustrative and should not be construed as limiting the present invention. Although the present invention has been described with reference to exemplary embodiments, it is understood that the words used in describing and illustrating the present invention are explanatory and exemplary, rather than limiting. As detailed herein, changes may be made within the scope of the appended claims without departing from the scope or spirit of the present invention in its aspects. Although the detailed description of the present invention has referred to specific structures, materials and embodiments, it is not intended that the present invention be limited to the disclosures herein, but rather that the present invention extends to all functionally equivalent structures, methods and uses within the scope of the appended claims. [Industrial Applicability]

[0058] The fiber board of the present invention can be used in a wide range of product fields such as vehicles and building materials, and is particularly useful as an interior material for vehicles. For example, it can be suitably used for various interior materials such as floor trim, roof trim, and door trim. [Explanation of symbols]

[0059] 10; fiberboard, 101; web, 102; mat, 11;Plant fiber, 12; binder resin, 121; resin fiber, 13;Bent fiber, 31; carding device; 311; blender; 312; tank; 313; carding machine; 32; cross layer device, 321; rocking conveyor, 34; Heating press device, 341; Platen, 35; cold press equipment, 351; surface plate, 36; Press equipment, 361; Surface plate, 37;heated press apparatus, 371;press platen.

Claims

1. A method for producing a fiber board comprising: plant fibers; and a binder resin that binds the plant fibers; wherein the plant fibers include fibers having a bent shape; and wherein the average fiber length of the bent fibers is more than 70 mm, A first step of laminating webs of mixed fibers of plant fibers and resin fibers serving as a binder resin to obtain a mat; A second step of hot pressing the mat to obtain the fiber board, The method for producing a fiber board, wherein the second step includes a folding step of folding the plant fibers.

2. The method for producing a fiber board according to claim 1 , wherein the folding step compresses the mat in a direction perpendicular to or intersecting a lamination direction of the web.

3. The method for producing a fiber board according to claim 1 , wherein the folding step uses a press platen having an uneven press surface to compress the mat.

Citation Information

Patent Citations

  • Fiberboard and manufacture thereof

    JP1999019907A

  • Method for manufacturing molding molded by bending decoration laminating board

    JP2002307411A

  • Fiber board and method for producing the same

    JP2013036140A

  • Fiber board

    JP2014076589A

  • Method for manufacturing crimped fiber, method for manufacturing fiber formed body, and apparatus for manufacturing crimped fiber

    JP2020204109A